Wear-resistant coatings produced from at least two different AlCr-based targets

JP2023554012A5Active Publication Date: 2024-11-12OERLIKON SURFACE SOLUTIONS AG PFAFFIKON
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023535915
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-12-14
Filing Date
2021-12-14
Publication Date
2024-11-12
Estimated Expiration
2041-12-14

AI Technical Summary

Technical Problem

Existing coatings for cutting tools, such as end mills, fail to provide sufficient wear resistance, especially in wet machining conditions, leading to abrasive wear, crater wear, and thermal crack formation, which reduces tool performance and life.

Method used

A multilayer coating system comprising a base coat, intervening layers of A and B, and a top coat, where A and B layers differ in chemical composition and thickness, with A layers having higher dopant concentrations, is applied using a reactive cathodic arc PVD method to enhance wear resistance and thermal stability.

Benefits of technology

The multilayer coating significantly increases tool life by reducing abrasive wear, crater wear, and thermal crack formation, while maintaining effective heat transfer, resulting in improved cutting performance and longevity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

A coating system (210) deposited on a surface of a substrate (201), comprising a primer coating (212) and an intervening coating (216) deposited as a multilayer film (216) consisting of multiple A layers and multiple B layers alternately deposited on one another to form an A / B / A / B / A... structure, wherein the A layers comprise aluminum chromium and optionally one or more dopant elements, and the B layers comprise aluminum chromium nitride and one or more dopant elements.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to an AlCrN-based coating that exhibits excellent wear resistance in machining operations such as milling (both roughening and finishing). The present invention further relates to a method for applying a coating system (hereinafter also referred to as a coating scheme).

[0002] More specifically, the present invention relates to a coated article by a coating scheme comprising AlCrN-based layers that can be deposited at various thicknesses such that at least some of the AlCrN-based layers in the coating scheme can be nanolayers.

[0003] Exemplary coated articles in this context include, but are not limited to, cutting tools such as end mills, forming tools, and wear components. [Background technology]

[0004] technical level Anders et al., in International Publication No. 2016 / 102170, proposed a coating system to reduce crater wear of cutting tools during machining operations, which is expected to be particularly beneficial in dry machining operations such as hobbing.

[0005] The coated articles and coating methods described by Eriksson et al. in International Publication No. 2016 / 102170 have already yielded favorable results. However, there is a need to meet the steadily increasing demand. Therefore, despite the advantages achieved by the above-mentioned coatings and other currently available coatings, there is still a need for new coatings that exhibit a combination of improved properties, such as significant abrasion resistance, thermal insulation properties, and improved resistance to crack initiation and propagation.

[0006] In particular, in the case of a coated end mill, for the purpose of referring to an example of a coated article, a coated end mill typically includes a substrate having a coating scheme (also referred to as a coating system) thereon. The coated end mill is useful for removing material in a chip-forming material removal operation. Depending on the workpiece material, machining process, and cutting parameters, at the interface between the end mill and the chip, there can be a significant amount of wear, particularly polishing, and both the formation and propagation of cracks (particularly in wet machining) and / or heat transfer (particularly in dry machining). Thus, both wear, particularly abrasive wear, and the formation and propagation of cracks (particularly in wet machining) and / or heat transfer to the interface between the substrate and the coating scheme and the substrate at the cutting tool interface (i.e., the coating-substrate interface) (particularly in cyclic machining) can be detrimental to the performance of the end mill.

[0007] The coating scheme typically affects the degree of wear, crack formation and propagation, and heat transfer from the end mill chip interface to the substrate and the coating-substrate interface. The physicochemical properties of the coating scheme strongly influence the degree of all wear, crack formation and propagation, and such heat transfer. SUMMARY OF THE INVENTION PROBLEMS TO BE SOLVED BY THE INVENTION

[0008] OBJECT OF THE PRESENT INVENTION The main object of the present invention is to provide a coating solution that overcomes the drawbacks of coatings according to the prior art.

[0009] In particular, the present invention should provide a new coating system that exhibits enhanced properties suitable for meeting the increasing demand in various machining operations such as both milling operations (roughening and finishing).

[0010] More specifically, the present invention should provide a coating scheme that enables significantly higher wear resistance compared to the state of the art by simultaneously reducing abrasive wear, crater wear, and the formation and propagation of thermal cracks, thereby significantly increasing the cutting performance and lifespan of cutting tools used in machining operations, particularly milling. Furthermore, an object of the present invention is to provide a method for applying the coating scheme according to the present invention, which should be applicable to the coating of cutting tools. [Means for solving the problem]

[0011] Description of the present invention The object of the present invention is achieved by providing the coating system described in independent claim 1, and by providing the method according to independent claim 20.

[0012] According to a first aspect of the present invention, a coating system deposited on the surface of a substrate comprises an undercoat film and an interlayer film deposited as a multilayer film consisting of a plurality of A layers and a plurality of B layers deposited alternately to form an A / B / A / B / A... structure, wherein the A layers comprise aluminum chromium and optionally one or more dopant elements, the B layers comprise aluminum chromium nitride and one or more dopant elements, the undercoat film is deposited on the surface of the substrate to be coated, or in either case, on a surface closer to the substrate than the interlayer film, the interlayer film is deposited between the undercoat film and the topcoat film, the topcoat film is deposited further from the substrate than the interlayer film, and the A layers comprise aluminum (Al), chromium (Cr), and nitrogen (N), or aluminum (Al), chromium (Cr), nitrogen (N), boron (B), yttrium (Y), tantalum (Ta), silicon (Si), tungsten (W), titanium (Ti), calcium (Ca), magnesium (Mg), The first layer contains one or more dopant elements selected from iron (Fe), cobalt (Co), zinc (Zn), and niobium (Nb), and the second layer contains aluminum (Al), chromium (Cr), nitrogen (N), and one or more dopant elements selected from boron (B), yttrium (Y), tantalum (Ta), silicon (Si), tungsten (W), titanium (Ti), calcium (Ca), magnesium (Mg), iron (Fe), cobalt (Co), zinc (Zn), and niobium (Nb). A coating system is disclosed in which layer A has a different chemical composition from layer B, and at least one chemical element is present in layer B but not in layer A, or present in layer B but not in layer A, or if both layers A and B contain the same chemical element, the concentration of the chemical element in layer B is different from the concentration of the chemical element in layer A, and the concentration of one or more dopants in layer B is higher than the concentration of one or more dopant elements in layer A, if present.

[0013] In another example of the first embodiment, the topcoat film may be deposited as the outermost layer of the coating system.

[0014] In another example of the first embodiment, the individual thicknesses of layer A may be greater than the individual thicknesses of layer B.

[0015] In another example of the first embodiment, the ratio of the individual thicknesses of layer A to the individual thicknesses of layer B may be in the range of 1% to 600%, preferably 50% to 400% greater.

[0016] In another example of the first embodiment, the thickness of the undercoat film may be between 65% and 97% of the total thickness of the coating system.

[0017] In another example of the first embodiment, the thickness of the topcoat film may be between 3% and 35% of the total thickness of the coating system.

[0018] In another example of the first embodiment, the thickness of the topcoat film may be thinner than the thickness of the undercoat film. In another example of the first embodiment, the topcoat film or at least a portion of the topcoat film, or at least some of the A layers and / or at least some of the B layers, if present, may be included in the topcoat film, and / or the intervening film or at least a portion of the intervening film, or at least some of the A layers and / or at least some of the B layers, may be included in the intervening film, in addition to nitrogen (N), oxygen (O), and / or carbon (C).

[0019] In another example of the first embodiment, the atomic percentage concentration of carbon and / or oxygen in one coating layer or film forming a coating system may be between 3 at.% and 38 at.% when considering only the concentrations of N, C, and O (meaning that the sum of the concentrations of N, C, and O in each coating layer or film can be considered to be 100 at.%).

[0020] In another example of the first embodiment, the atomic percentage concentration of the dopant element in layer B, and, if layer A contains the dopant element, the atomic percentage concentration of the dopant element in layer A, may also vary along the total thickness of the intervening coating film of the coating system, and the range of variation may preferably be between 0.1% and 600%, based on the lowest concentration of each dopant element in the intervening coating film.

[0021] In another example of the first embodiment, the intervening coating may include different film portions, i varying from i=1 to i=n, ​​where i and n are natural numbers, i.e., including portions, the number of film portions being at least 1, i.e., n≧1, preferably more than 1, i.e., n≧2, each of the intervening film portions may include a lower and an upper portion, each of the portions being formed by one or more double layers b, each of the double layers b may be formed by one layer A and one layer B, and all A layers within the thickness extension of the intervening coating contain the same chemical elements Although they may appear to be the same concentration, all B layers within the extension of the interlayer coating thickness may contain the same chemical elements, but not necessarily at the same concentration, and at least two interlayer coating portions deposited on each other, e.g., 216.1 and 216.2, may differ in at least one of the following physicochemical properties: main crystal orientation, crystal size and / or crystal size distribution—all calculated from the peak intensity and sub-peak area and full width at half maximum from the X-ray diffraction pattern—mechanical properties such as hardness, elasticity and modulus of elasticity, and chemical composition.

[0022] In another example of the first embodiment, at least two sub-substrates belonging to each of two continuously deposited interlayer film portions may exhibit different intrinsic stresses, such that 216.i is closer to the substrate than 216.i+1, and the sub-substrate closer to the substrate may exhibit a lower intrinsic stress than the other sub-substrates.

[0023] In another example of the first embodiment, the undercoat may contain the same elements as layer A. In another example of the first embodiment, the topcoat film is 1) The same chemical elements as layer B (in this case, the topcoat film may be manufactured using the same target used for depositing layer B, and may preferably be deposited as a single layer), or 2) The same chemical element of layer A and the same chemical element of layer B (in this case, the top coating can be manufactured as a multi-layer by using the same targets as those used for the deposition of layers A and B in the intermediate coating respectively, but the top coating can have a different ratio of thicknesses of different layers A and B and a different chemical composition compared to the intermediate coating, and the thickness of each layer A with respect to the thickness of each layer B in the top coating (220) can be either lower or equal or higher, but A 層_厚さ_220中 / B 層_厚さ_220中 > 0, then A 層_厚さ_216中 / B 層_厚さ_216中 > A 層_厚さ_220中 / B 層_厚さ_220中 can include any of).

[0024] In another example of the first aspect, the concentration of the dopant element in the undercoat (if present) and in the top coat may vary along the total thickness of the undercoat.

[0025] In another example of the first aspect, the concentration of the dopant element may vary along the total thickness of the top coat of the coating system.

[0026] In another example of the first aspect, the range of variation is between 0.1% and 600% respectively based on the minimum concentration of each dopant element in the undercoat or the top coat.

[0027] According to a second aspect of the present invention, a method for manufacturing a coating system according to the first aspect is disclosed, the coating system is manufactured using the reactive cathode arc PVD method, and for the deposition of layer A, one or more A ソース - targets are used, and for the deposition of layer B, one or more B ソース - targets are used, at least nitrogen gas is used as the reactive gas, and the A ソース - target contains Al and Cr, and optionally one or more dopant elements selected from B, Y, Ta, Si, W, Ti, Ca, Mg, Fe, Co, Zn and Nb, and layer B ソース- The target comprises Al and Cr, and one or more dopant elements selected from B, Y, Ta, Si, W, Ti, Ca, Mg, Fe, Co, Zn and Nb, A ソース -Target and B ソース - If both targets contain one or more dopant elements, they must have at least one dopant element different from each other, and during the deposition of the coating system, the following parameters apply: At least one of the gas pressure, temperature, bias voltage, source current, magnetic field shape and / or strength, and reactive gas, The following physicochemical properties of the coating: The main crystal orientation, crystal size and / or crystal size distribution—all calculated from the peak intensity, sub-peak area and full width at half maximum from the X-ray diffraction pattern—are varied to alter mechanical properties such as hardness and modulus of elasticity, and at least one of the chemical composition. [Brief explanation of the drawing]

[0028] [Modes for carrying out the invention]

[0029] Detailed explanation To better illustrate the present invention, Figures 1 to 8 are used.

[0030] Figure 1 is used to schematically illustrate, in particular, preferred embodiments of the coating system (also called the coating scheme) of the present invention. Figure 1 includes Figures 1a, 1b, 1c, and 1d(a) and (b).

[0031] A schematic representation of a basic embodiment of the coating system according to the present invention is shown in Figure 1a. The coating system 210 (or coating scheme 210) of the present invention comprises at least three coating films: an undercoat film 212 (the undercoat film may also be called an undercoat layer), an intervening coating film 216, and a topcoat film 220 (the topcoat film may also be called a topcoat layer).

[0032] The undercoat film 212 is deposited on the surface of the substrate 201 to be coated, or in either case (if other layers are deposited between the substrate 201 and the undercoat film 212), it is deposited on the surface closer to the substrate 201 than the intervening coating film 216.

[0033] The intervening coating 216 is deposited between the undercoat coating 212 and the topcoat coating 220. The topcoat film 220 is deposited further away from the substrate 201 than the intervening film 216.

[0034] Preferably, the topcoat film 220 is deposited as the outermost layer of the coating system 210.

[0035] The intervening coating 216 is deposited as a multilayer film containing multiple Type A layers (hereinafter also referred to as A layers) and multiple Type B layers (hereinafter also referred to as B layers).

[0036] Layers A and B are deposited alternately, forming the sequence A / B / A / B / A...

[0037] Layer A contains aluminum (Al), chromium (Cr), and nitrogen (N), or aluminum (Al), chromium (Cr), nitrogen (N) and one or more dopant elements selected from boron (B), yttrium (Y), tantalum (Ta), silicon (Si), tungsten (W), titanium (Ti), calcium (Ca), magnesium (Mg), iron (Fe), cobalt (Co), zinc (Zn), and niobium (Nb). In other words, Layer A contains Al, Cr, and N, and optionally further contains one or more of the above-mentioned dopant elements.

[0038] The B layer contains aluminum (Al), chromium (Cr), nitrogen (N), and one or more dopant elements selected from boron (B), yttrium (Y), tantalum (Ta), silicon (Si), tungsten (W), titanium (Ti), calcium (Ca), magnesium (Mg), iron (Fe), cobalt (Co), zinc (Zn), and niobium (Nb). In other words, the B layer contains Al, Cr, N, and one or more of the aforementioned dopant elements.

[0039] According to a preferred embodiment, the chemical elements contained in layer B differ from those contained in layer A by at least one chemical element, meaning that if both the type A layer and the type B layer contain one or more dopants, then at least one of the dopants present in layer B is not present in layer A, or at least one of the dopants present in layer A is not present in layer B, and the concentration of one or more dopants in the type B layer (also referred to as layer B in the context of this invention) is higher than the concentration of one or more dopants in the type A layer (also referred to as layer A in the context of this invention).

[0040] In a more preferred embodiment, the chemical elements contained in layer B may be the same chemical elements contained in layer A, but in this case, both layer B and layer A contain one or more dopants, the chemical composition of layer A differs from that of layer B in terms of the concentration of chemical elements, and the concentration of one or more dopant elements in layer B is higher than the concentration of one or more dopant elements in layer A.

[0041] According to a preferred embodiment of the method of the present invention, A used to manufacture layer A ソース - The target chemical elemental composition is B used to manufacture the B layer. ソース - The target's chemical composition differs from that of at least one chemical element, i.e., B ソース - At least one chemical element contained in the target is A ソース - Not included in the target, or A ソース - At least one chemical element contained in the target is B ソース - Not included in the target, B ソース- The concentration of one or more dopants in the target is A ソース - Higher than the concentration of one or more dopants in the target.

[0042] According to a more preferred embodiment of the method according to the present invention, A is used to manufacture layer A. ソース - The target chemical elemental composition is B used to manufacture the B layer. ソース - The target has a different chemical composition and concentration of chemical elements, that is, B ソース - The chemical element contained in the target is A ソース -If the chemical elements contained in the target are the same, then both types of targets contain one or more dopant elements, A ソース - The chemical element concentration of the chemical element in the target is B ソース - Unlike the concentration of chemical elements in the target, B ソース - The concentration of one or more dopants in the target is A ソース - Higher than the concentration of one or more dopants in the target.

[0043] The intervening coating 216 consists of one or more film portions 216.i, as schematically shown in Figure 1b, where i varies from i=1 to i=n, ​​and i and n are natural numbers, with n≧1, preferably n≧2.

[0044] These intervening coating portions do not necessarily need to be of the same thickness. In all of these film portions, preferably all A layers are the same target (A in the context of the present invention). ソース -Manufactured by using (also called a target), preferably all B layers are the same target (B in the context of this invention). ソース - Manufactured by using (also called a target)

[0045] These interposed coating portions differ in at least one of the following physicochemical properties: main crystal orientation, crystal size and / or crystal size distribution (all calculated from peak intensity and sub-peak area and full width at half maximum from X-ray diffraction patterns), mechanical properties (e.g., hardness, modulus of elasticity), and chemical composition.

[0046] Differences in the physicochemical properties described above between different film portions 216.1 to 216.n (which means differences between different interlayer film portions 216.i) are preferably brought about by changing one or more process parameters selected from pressure, temperature, bias voltage, bias current, source current, magnetic field shape, magnetic field strength, reactive gas flow, reactive gas partial pressure, and the type of reactive gas introduced into the coating chamber during the coating deposition process.

[0047] However, regardless of the changes in process parameters due to the deposition of the intervening coating 216, all intervening film portions 216.i use the same target A for the deposition of layers A and B, respectively. ソース -Target and same B ソース - It is preferable that the entire intervening coating 216 is manufactured by using a target, which means i=1 to i=n.

[0048] According to a preferred embodiment of the present invention, the coating system is designed to have an intervening coating 216 comprising different film portions 216.i in which i varies from i=1 to i=n, ​​as schematically shown in Figure 1b, where i and n are natural numbers, i.e., comprising portions 216.1 to 216.n, the number of intervening film portions 216.i is at least 1, i.e., n≧1, preferably more than 1, i.e., n≧2, and each of the intervening film portions 216.i is as shown in Figure 1b and As schematically shown in Figure 1c, the portion includes the lower 216.i. lower and the upper 216.i. upper, and each portion is formed by one or more double layers b, each of which is formed by one layer A and one layer B, as schematically shown in Figure 1d, and all A layers within the thickness extension of the intervening coating 216 contain the same chemical elements but do not necessarily have to be at the same concentration, and all B layers within the thickness extension of the intervening coating 216 contain the same chemical elements but do not necessarily have to be at the same concentration.

[0049] Preferably, at least two interlayer film portions deposited on each other, for example 216.1 and 216.2, differ in at least one of the following: main crystal orientation, crystal size and / or crystal size distribution (both calculated from peak intensity and sub-peak area and full width at half maximum from the X-ray diffraction pattern), mechanical properties such as hardness and elastic modulus, and / or physicochemical properties of chemical composition.

[0050] According to a preferred embodiment of the present invention, at least one upper 216.i. deposited beneath each lower 216.i. exhibits a different intrinsic stress than the respective lower. This feature is preferably characterized by a value U during deposition beneath the lower 216.i., as schematically shown in Figure 1c. i By applying a constant bias voltage having the value U during deposition on the upper 216.i. i From value U i+1 It is generated by applying a variable bias voltage that changes up to, where preferably U i and U i+1 This is the negative bias voltage, and the absolute value of U i+1 U in absolute value iHigher than |U i+1 |>|U i Preferably, at least two sub-stresses belonging to each of two consecutive deposited interlayer film portions (e.g., 216.1.sub-stress included in 216.1 and 216.2.sub-stress included in 216.2, where 216.1 is closer to the substrate than 216.2) exhibit different intrinsic stresses, and preferably, the sub-stress closer to the substrate (e.g., 216.1.sub-stress) exhibits a lower intrinsic stress than the other sub-stress (e.g., 216.2.sub-stress). This feature is preferably characterized by a value U during deposition of sub-stress 216.i.sub-stress, as schematically shown in Figure 1c. i By applying a constant negative bias voltage having the value U during deposition on the lower 216.i+1. i+1 It is generated by applying different constant negative bias voltages having the absolute value of the bias voltage U i+1 This is the absolute value of the bias voltage U i Higher than U i+1 >U i For example, by applying a first constant negative bias voltage U1 for deposition at 216.1. bottom and a second constant negative bias voltage U2 for deposition at 216.2. bottom, it is achieved that 216.1. bottom is closer to the substrate than 216.2. bottom, U1 is lower in absolute value than U2, i.e., |U1| < |U2|, and the intrinsic stress at 216.2. bottom is higher than the intrinsic stress at 216.1. bottom. In this context, the intrinsic stress is preferably compressive stress.

[0051] As schematically shown in Figure 1d, layers A and B, which exist as a double layer b at the lower and upper parts respectively, are preferably deposited as nanolayers.

[0052] The thickness of the upper 216.i. is less than the thickness of the corresponding lower 216.i. below which the upper 216.i. is deposited, i.e., thickness 216.i. below > thickness 216.i. above.

[0053] The intervening coating 216 may also include an uppermost layer 216_TP, as schematically shown in Figure 1b.

[0054] Preferably, a negative bias voltage is applied during the deposition of the interleaving coating 216, and preferably, the value of the negative bias voltage is increased (in absolute value) from a lower bias voltage U1 used at the start of deposition of the interleaving coating 216 to a higher bias voltage Un used at the end of deposition of the interleaving coating 216. Preferably, this bias voltage fluctuation is carried out such that the bias voltage is kept as constant as possible at a value Ui during deposition under each lower 216.i., and gradually increases from Ui to a higher value Ui+1 during deposition on each upper 216.i.

[0055] According to the present invention, as schematically shown in Figure 1d, the individual thicknesses of layer A are greater than the individual thicknesses of layer B.

[0056] The ratio of the individual layer thicknesses of layer A to the individual layer thicknesses of layer B is in a large range between 50% and 400%.

[0057] The thickness of the undercoat film 212 is preferably between 65% and 97% of the total thickness of the coating system 210.

[0058] The thickness of the topcoat film 220 is preferably between 3% and 35% of the total thickness of the coating system 210.

[0059] The thickness of the topcoat film is preferably 220, which is thinner than the thickness of the undercoat film 212.

[0060] According to a preferred embodiment of the present invention, - Topcoat film 220 and / or intervening film 216, -At least a portion of the topcoat film 220 (i.e., a portion of the topcoat film 220 that extends along the thickness of the topcoat film 220 without including a complete extension, or the entire topcoat film 220 along that thickness) and / or at least a portion of the intervening coating film 216, In addition to nitrogen (N), it contains oxygen (O) and / or carbon (C), In this way - Topcoat film 220 and / or intervening film 216, - At least a portion of the topcoat film 220 and / or at least a portion of the intervening film 216, This may include not only metal nitrides, but also metal oxynitrides, metal carbonitrides, or metal carboxynitrides.

[0061] The atomic percentage concentration of carbon and / or oxygen in one coating layer or film forming the coating system 210 is preferably between 3 at.% and 38 at.% when considering only the concentrations of N, C, and O (meaning that the sum of the concentrations of N, C, and O in each coating layer or film can be considered to be 100 at.%).

[0062] The ratio of the atomic percentage concentration of aluminum to chromium (Al / Cr) preferably changes along the total thickness of the coating system. In this case, the range of variation of the Al / Cr concentration ratio is preferably between 69 / 31 and 79 / 21.

[0063] The atomic percentage concentration of the dopant element in layer B, and, if layer A contains a dopant element, the atomic percentage concentration of the dopant element in layer A, is between 0.1 at.% and 20 at.% when considering the concentrations of all elements (meaning when the sum of the concentrations of all elements in each layer B or A is considered to be 100 at.%), preferably between 0.5 at.% and 15 at.%.

[0064] When both layer B and layer A contain dopant elements, the atomic percentage concentration of the dopant elements in layer A preferably changes along the total thickness of the intervening coating film of the coating system. The range of variation is preferably between 0.1% and 600%, based on the lowest concentration of each dopant element in the intervening coating film.

[0065] The undercoat film 212 preferably contains the same elements as layer A. The topcoat film 220 is, - Preferably, the same chemical elements as layer B (meaning that the topcoat film 220 can be deposited as a single layer), or - Preferably, it contains either the chemical elements of layer A and the chemical elements of layer B (this means that the topcoat 220 is produced by using the same target used for depositing the interleaved coating 216, but can be deposited as a multilayer having multilayer periodicity, with different thickness ratios of layer A and B and different chemical compositions compared to the interleaved coating 216). The thickness of layer A to the thickness of layer B in the topcoat 220 may be lower, equal, or higher, but in the last case, it must be lower than in part 216, i.e., A 層_厚さ_220中 / B 層_厚さ_220中 If >0, A 層_厚さ_216中 / B 層_厚さ_216中 >A 層_厚さ_220中 / B 層_厚さ_220中 That is the case.

[0066] All layers A are the same A ソース -Manufactured from the target, all B layers are the same B ソース -Although manufactured from a target, this does not mean that all A layers have the same chemical composition, nor does it mean that all B layers have the same chemical composition along the thickness of the coating film, or along the portion of the coating film containing these A and B layers, because process parameters can be changed, and therefore the concentrations of chemical elements in each A and B layer can also be changed due to the influence of different process parameters used during coating deposition.

[0067] Similarly, even though a single coating film is manufactured from the same one or more targets, this does not mean that the chemical composition of this coating film is the same along its thickness, due to the influence of the process parameters used during coating deposition, as already mentioned above.

[0068] When dopant elements are present in the undercoat 212 and / or the topcoat 220, their concentration preferably varies along the total thickness of the undercoat 212 and / or the total thickness of the topcoat 220 of the coating system 210. The range of variation is preferably between 0.1% and 600%, respectively, based on the lowest concentration of the dopant element in the undercoat or topcoat.

[0069] The coating system of the present invention (also referred to as the coating scheme already described above) has the following challenging requirements, as described above: -Reduction of abrasive wear, -Reduction of crater wear, - Reduction / suppression of thermal crack formation and propagation, - Enables heat transfer from the end mill tip interface to the substrate and the coating-substrate interface. The present invention includes a layer configuration, particularly one adjusted by the present method, which makes it possible to satisfy the conditions simultaneously.

[0070] To illustrate the remarkable advantages that can be obtained by using the coating system according to the present invention, several examples are described below. These examples should not be understood as limitations of the present invention, but merely as examples. [Examples]

[0071] Process parameters used for deposition in several embodiments of the coating system 210 of the present invention: ○ Pressure range: 0.1 Pa to 9 Pa (N2 partial pressure control) ○ Substrate temperature range: 200℃~600℃ ○ Bias voltage range: +20V to -300V ○ Source current range: 50A~200A For deposition in the embodiment of the invention, coating parameters were selected from the above range and modified as needed to achieve various properties.

[0072] The elements nitrogen, carbon, and oxygen were provided into the coating chamber for the formation of the coating system 210 by using their respective reactive gases, such as N2 gas for nitrogen, O2 gas for oxygen, and C2H2 or CH4 for carbon.

[0073] To provide Al, Cr, and dopant elements, a solid target was used as a cathode for evaporation, and thus as a material source for forming a coating system.

[0074] The target preferably acted as the cathode of an arc evaporator used as an arc PVD source.

[0075] This means the process is reactive: Reactive cathode PVD coating process.

[0076] During the entire coating process for the deposition of coating scheme 210, at least two mutually distinct targets (mutually distinct targets meaning that one target is different from the other) were used. These targets differed from each other in at least one of the following aspects: 1) The concentration of Al in the total Al+Cr content (meaning Al / (Al+Cr) in at.% units), and / or 2) Total concentration of all dopants relative to total metal concentration and / or 3) The concentration of one dopant relative to the total dopant concentration and / or total elemental concentration.

[0077] In this example, an AlCr metal target is used as the Al and Cr source, and the AlCr metal target has a minimum Al concentration of 68% relative to Al and Cr (Al / (Al+Cr) at %).

[0078] All dopants (metallic or metalloid dopants) were supplied directly as dopants in the AlCr target.

[0079] In the following embodiment, the AlCr target is A ソース -Use as a target, and the AlCrB target is B ソース -Although used as targets, these embodiments should not be understood as limiting the invention, but merely as examples. [Examples]

[0080] Cutting test results: Milling of hardened steel (steel grade 1.2344) under wet conditions to achieve a surface roughening of 38 HRC and a finish of 45 HRC. The 38 HRC surface roughening test is referred to as Test Example 1.

[0081] The 45HRC finishing test is called Test Example 2. Test Example 1 includes testing of coated cutting end mills labeled as follows: -Technological level = benchmark coating in the commercial market - Exemplary coatings 1, 2, and 3 of the present invention are given in this invention.

[0082] Test parameters for 38HRC surface roughening: Here, the performance of surface roughening using an end mill is tested. The workpiece material is 38HRC hardened steel (1.2344). The tool is a carbide end mill with 4 teeth and a diameter of 10 mm. The cutting parameters are as follows: cutting speed Vc = 175 m / min; feed rate f = 0.05 mm / tooth; cutting depth ap = 5.0 mm; cut width ae = 4 mm; external cooling: wet; and wear criterion: VBmax = 120 μm. Figure 1 shows the tool life (%) comparing the state of the art and three inventive embodiments. The differences in wear progression after the test period are shown in Figure 2 for the state of the art and one inventive embodiment. Figure 2 shows one of four representative main cutting edges.

[0083] Figure 2 shows a comparison of the tool life of coated carbide end mills in a wet milling cutting test applied to 38HRC hardened steel (steel grade 1.2344) for three exemplary inventions (Invention Examples 1, 2, and 3) of wear-resistant coating schemes tested against the state of technology as a market benchmark. It can be seen that the coatings of the present invention have a significant increase in tool life of up to 220% compared to the state of technology as a market benchmark.

[0084] Figure 3 shows the wear and wear progression of a coated carbide end mill in Test Example 1, given as a representative example of one tool per variant selected from the tools tested, and depicts a wet milling test of 38HRC hardened steel (steel grade 1.2344) with the wear-resistant coating scheme of Invention Example 1 tested against the state of art as a benchmark. It can be seen that the state of art coating shows much higher wear, particularly initiation wear, and much faster wear progression in both the present invention and the coating of the present invention compared to the state of art coating. Thus, the state of art coating failed prematurely, as shown by the tool life test of Example 1 in Figure 2. In contrast, the present invention coating of Example 1 has very low initiation wear and uniform wear progression with no chipping until the end of tool life, defined by maximum wear (VBmax).

[0085] Test Example 2 includes testing of coated cutting end mills labeled as follows: -Technological level = benchmark coating in the commercial market - Exemplary coatings 1, 2, and 4 of the present invention are given in this invention.

[0086] Test parameters for 45HRC finish: Here, the performance of finishing using an end mill is tested. The workpiece material is 45HRC hardened steel (1.2344). The tool is a carbide end mill with four teeth and a diameter of 10 mm. The cutting parameters are as follows: cutting speed Vc = 150 m / min; feed rate f = 0.1 mm / tooth; cutting depth ap = 5.0 mm; cut width ae = 0.5 mm; external cooling: wet; and wear criterion: VBmax = 140 μm. Figure 3 shows the tool life (%) comparing the state of the art and three inventive embodiments (1, 2, and 4). The differences in wear progression after the test period are shown in Figure 5 for the state of the art and one inventive embodiment (4). Figure 5 shows one of the four main cutting edges as a representative example.

[0087] Figure 4 shows a comparison of the tool life of coated carbide end mills in a wet milling cutting test applied to 45HRC hardened steel (steel grade 1.2344) for three exemplary inventions (Invention Examples 1, 2, and 4) of wear-resistant coating schemes tested against the state of technology as a market benchmark. It can be seen that the coatings of the present invention have a significant increase in tool life of up to 200% compared to the state of technology as a market benchmark.

[0088] Figure 5 shows the wear and wear progression of a coated carbide end mill in Test Example 2, given as a representative example of one tool per variant selected from the tools tested, and depicts a wet milling test of 45HRC hardened steel (steel grade 1.2344) with the wear-resistant coating scheme of Invention Example 2 tested against the state of art as a benchmark. It can be seen that the state of art coating shows much higher wear, particularly initiation wear, and much faster wear progression in both the present invention and the coating of the present invention compared to the state of art coating. Thus, the state of art coating failed prematurely, as shown by the tool life test of Example 2 in Figure 4. In contrast, the coating of the present invention in Example 2 has very low initiation wear and uniform wear progression with no chipping until the end of tool life, defined by maximum wear (VBmax).

[0089] Table 1 shows the properties of a state-of-the-art coating and the coating of the present invention. These properties include hardness (H), elastic modulus (E), ratio H / E, and ratio H 3 / E 2 and compressive stress. The properties of the coatings of the present invention shown in Table 1 are that these coatings of the present invention have an increase in E, a decrease in H value, a slight decrease in the H / E ratio, and H 3 / E 2 These exhibit a common characteristic of a significant decrease in the ratio and an increase in compressive stress. Furthermore, the remarkably high compressive stress is maintained at a level beneficial for wear resistance without causing breakage between the substrate and the coating. All of these, combined with specialized chemistry including alloying and doping, and combined with a dedicated new structure, simultaneously enable reduced abrasive wear, reduced crater wear, reduced / suppression of thermal crack formation and propagation, and the ability to transfer heat from the end mill tip interface to the substrate and the coating-substrate interface of the present invention.

[0090] Table 1 shows the properties (hardness, elastic modulus, their ratio, and compressive stress) of examples of coatings of the present invention and those of the state of technology.

[0091] [Table 1]

Claims

1. Undercoat coating (212) and A / B / A / B / A a coating system (210) deposited on the surface of a substrate (201) comprising a multilayer (216) of A layers and B layers alternately deposited on one another forming a structure, the A layers comprising aluminum chromium and optionally one or more dopant elements, the B layers comprising aluminum chromium nitride and one or more dopant elements, - said undercoat coating (212) is deposited on the surface of said substrate (201) to be coated or, in any case, on a surface closer to said substrate (201) than said intermediate coating (216); - said intermediate coating (216) is deposited between said base coat (212) and top coat (220); - said topcoat (220) is deposited further from said substrate (201) than said intermediate coating (216); - said layer A is Aluminum (Al), Chromium (Cr) and Nitrogen (N), or - aluminum (Al), chromium (Cr), nitrogen (N) and one or more dopant elements selected from boron (B), yttrium (Y), tantalum (Ta), silicon (Si), tungsten (W), titanium (Ti), calcium (Ca), magnesium (Mg), iron (Fe), cobalt (Co), zinc (Zn) and niobium (Nb); the B layer comprises aluminum (Al), chromium (Cr), nitrogen (N) and one or more dopant elements selected from boron (B), yttrium (Y), tantalum (Ta), silicon (Si), tungsten (W), titanium (Ti), calcium (Ca), magnesium (Mg), iron (Fe), cobalt (Co), zinc (Zn) and niobium (Nb); Where: - said A layer differs from said B layer at least in its chemical composition, at least one chemical element is present in the B layer but not in the A layer, or is present in the A layer but not in the B layer, or - if both layers A and B contain the same chemical element, the concentration of said chemical element in said layer B is different from the concentration of said chemical element in said layer A, and - a coating system (210), characterized in that said concentration of said one or more dopants in said B layer, if present, is higher than said concentration of said one or more dopant elements in said A layer.

2. The coating system of claim 1 , wherein the topcoat (220) is deposited as an outermost layer of the coating system.

3. 3. The coating system according to claim 1, wherein the individual layer thicknesses of the A layers are greater than the individual layer thicknesses of the B layers.

4. 4. The coating system according to claim 1, wherein the individual layer thicknesses of the A layers are greater than the individual layer thicknesses of the B layers, and the ratio of the individual layer thicknesses of the A layers to the individual layer thicknesses of the B layers is in the range of between 1% and 600%, preferably 50% to 400%.

5. The coating system according to any one of claims 1 to 4, characterized in that the thickness of the undercoat (212) is between 65% and 97% of the total thickness of the coating system.

6. A coating system according to any one of claims 1 to 5, characterized in that the thickness of the topcoat is between 3% and 35% of the total thickness of the coating system.

7. The coating system according to any one of claims 1 to 6, characterized in that the layer thickness of the topcoat coating is thinner than the layer thickness of the undercoat coating.

8. said topcoat (220) or at least a part of said topcoat (220), or, if present, at least some of said A layers and / or at least some of said B layers comprised in said topcoat (220), and / or said intermediate coating (216) or at least a part of said intermediate coating (216), or at least some of said A layers and / or at least some of said B layers contained in said intermediate coating (216), 8. Coating system according to claim 1, characterized in that in addition to nitrogen (N) it also contains oxygen (O) and / or carbon (C).

9. 9. Coating system according to claim 8, characterized in that the concentration in atomic percentage of carbon and / or oxygen in one coating layer or one film forming said coating system is between 3 at. % and 38 at. %, when only the concentrations of N, C and O are taken into account, which means when the sum of the concentrations of N, C and O in said respective coating layer or film is considered as 100 at. %.

10. 10. A coating system according to any of claims 1 to 9, characterized in that the ratio of concentrations in atomic percentage of aluminium to chromium (Al / Cr) varies along the total thickness of the coating system, the range of variation of the Al / Cr concentration ratio being preferably between 69 / 31 and 79 / 21.

11. 11. Coating system according to any of claims 1 to 10, characterized in that the concentration in atomic percentage of the dopant element in the B layer and, if the A layer comprises a dopant element, also in the A layer, is between 0.1 at. % and 20 at. %, preferably between 0.5 at. % and 15 at. %, when taking into account the concentrations of all elements (which means when the sum of the concentrations of all elements of the respective B or A layer is taken as 100 at. %).

12. 12. A coating system according to any of claims 1 to 11, characterized in that the concentration in atomic percentage of the dopant element in the B layer, and, if the A layer comprises a dopant element, also the concentration in atomic percentage of the dopant element in the A layer, varies along the total thickness of the intervening coatings of the coating system, the range of variation being preferably between 0.1% and 600% based on the minimum concentration of the respective dopant element in the intervening coating.

13. said intermediate coating (216) comprises different film portions (216.i), i varying from i=1 to i=n, ​​where i and n are natural numbers, i.e. portions (216.1 to 216.n), the number of said film portions (216.i) being at least 1, i.e. n≧1, preferably more than 1, i.e. n≧2, each of said intermediate film portions (216.i) comprising a lower portion (216.i. below) and an upper portion (216.i. above), each of said portions being formed by one or more bilayers b, each of said bilayers b being formed by one layer A and one layer B, all A layers within said thickness extension of said intermediate coating (216) comprising the same chemical elements, but not necessarily in the same concentration, and all B layers within said thickness extension of said intermediate coating (216) comprising the same chemical elements, but not necessarily in the same concentration, 13. A coating system according to any of claims 1 to 12, wherein at least two intervening film parts, e.g. 216.1 and 216.2, deposited on one another, are characterized by differing in at least one of the following physicochemical properties: predominant crystal orientation, crystal size and / or crystal size distribution - in each case calculated from peak intensities and areas under the peaks and full width at half maximum from an X-ray diffraction diagram - mechanical properties such as hardness, elasticity and modulus, chemical composition.

14. The coating system according to claim 13, characterized in that at least two lower parts (216.i. lower part included in 216.i, 216.i+1. lower part included in 216.i+1) belonging to two successively deposited intervening film parts respectively exhibit different inherent stresses, 216.i is closer to the substrate than 216.i+1, and the lower part (216.i. lower part) closer to the substrate exhibits lower inherent stress than the other lower part (216.i+1. lower part).

15. A coating system according to any one of claims 1 to 14, characterized in that the undercoat (212) contains the same elements as the layer A.

16. The topcoat coating film (220) 3) the same chemical elements as layer B (in this case, the overcoat (220) is produced by using the same target as used for the deposition of layer B, and is preferably deposited as a single layer); or 4) the same chemical elements of the layer A and the same chemical elements of the layer B, in which the topcoat (220) is produced as a multilayer by using the same targets as used for the deposition of the layers A and B in the intermediate coating (216), respectively, but the topcoat (220) has a different layer A to layer B thickness ratio and a different chemical composition compared to the intermediate coating (216), and the thickness of the individual layer A relative to the thickness of the individual layer B in the topcoat (220) is either lower, equal or higher, but if A_thickness_220 / B_thickness_220>0 then A_thickness_216 / B_thickness_216>A_thickness_220 / B_thickness_220.

17. 17. A coating system according to any of claims 1 to 16, characterized in that the concentration of the dopant element in the basecoat (if present) as well as in the topcoat varies along the total thickness of the basecoat.

18. 18. The coating system of any of claims 1 to 17, characterized in that the concentration of the dopant element varies along the total thickness of the topcoat of the coating system.

19. 19. A coating system according to any of the preceding claims 16 to 18, characterized in that the range of variation is between 0.1% and 600% based on the lowest concentration of the respective dopant element in the basecoat or topcoat coating, respectively.

20. A method for producing a coating system according to any one of the preceding claims 1 to 19, said coating system being produced using a reactive cathodic arc PVD method, comprising the steps of: ソース - a target is used, for the deposition of the B layer, one or more B ソース - A target is used, and at least nitrogen gas is used as a reactive gas, ソース The target comprises Al and Cr and, optionally, one or more dopant elements selected from B, Y, Ta, Si, W, Ti, Ca, Mg, Fe, Co, Zn and Nb, ソース The target comprises Al and Cr and one or more dopant elements selected from B, Y, Ta, Si, W, Ti, Ca, Mg, Fe, Co, Zn and Nb, ソース - target and B ソース - if the targets both contain one or more dopant elements, they differ from each other by at least one dopant element, and during the deposition of the coating system, the following parameters are controlled: At least one of the gas pressure, temperature, bias voltage, source current, magnetic field shape and / or strength, and reactive gases; The following physicochemical properties of said coating: is altered to change at least one of the predominant crystal orientation, the crystal size and / or the crystal size distribution - all calculated from the peak intensities and areas under the peaks and the full width at half maximum from the X-ray diffraction diagram -, the mechanical properties such as hardness and elastic modulus, and the chemical composition.