Matrix resins for the production of fiber composites.

JP2023554454A5Inactive Publication Date: 2024-11-14EVONIK OPERATIONS GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023537082
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-12-17
Filing Date
2021-12-13
Publication Date
2024-11-14
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing bio-based matrix resins for fiber composites, such as methacrylated vanillin and cardanol mixtures, suffer from storage instability, crystallization issues, and inadequate mechanical properties, making them unsuitable for typical fiber composite processing.

Method used

A composition comprising aldehydes, phenolic compounds, and amines with (meth)acrylate groups, which upon curing forms a thermosetting resin suitable for fiber composites, offering storage stability, low viscosity, and excellent mechanical properties without brittleness.

Benefits of technology

The resin exhibits a long pot life, suitable for common manufacturing processes, and produces fiber composites with superior mechanical properties, including high glass transition temperature and flexural modulus, suitable for various industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000017_0000
    Figure 00000017_0000
Patent Text Reader

Abstract

The subject of the present invention is a composition comprising: at least one aldehyde (A); at least one phenolic compound (B); and at least one amine (C) having at least two amino groups selected from the group consisting of primary and secondary amino groups, at least one of which has at least one (meth)acrylate group; a fiber-reinforced composition comprising such a composition; a process for curing the fiber-reinforced composition; and a fiber composite material or a thermoset resin obtainable by such a process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a matrix resin for manufacturing fiber composite materials.

[0002] Fiber composite materials reinforced with glass fibers or carbon fibers for higher-value applications are mainly manufactured based on thermosetting resin systems. The unsaturated polyester resin occupies the largest proportion quantitatively, followed by epoxy resin and vinyl ester resin in that order. Here, usually, fiber composite materials based on epoxy resin exhibit the best mechanical properties, and members based on unsaturated polyester resin are the most inferior. However, unsaturated polyester resin is less expensive than epoxy resin and is crosslinked by peroxide, so it is easy to use. Vinyl ester resin is a compromise in terms of performance, ease of use, and cost.

[0003] All of these thermosetting resin systems are based on petroleum-based raw materials. Moreover, polyester resin and vinyl ester resin contain a large amount of styrene and cannot be said to be substances without problems in terms of labor hygiene.

[0004] Therefore, a bio-based matrix resin that is easy to use, has good mechanical properties, and is cost-effective has been sought for many years. However, the resin systems used so far do not meet these requirements. For example, polyfurfuryl alcohol is mentioned here. Polyfurfuryl alcohol crosslinks under water elimination and rapidly increases in viscosity. Low-viscosity polyfurfuryl alcohol resins that can be used in infusion generally contain a large amount of water. When this resin is cured, bubbles are generated. Also, the corresponding thermosetting resin or fiber composite material is very porous.

[0005] Bio-based reactive materials have long been known in both the field of epoxide chemistry (e.g., epoxidized soybean oil and epoxidized cashew nut shell oil) and polyester chemistry (e.g., cardanol, rosin resin, and unsaturated oleic acid derived from cashew nut shell oil). Because these polymers have poor mechanical properties in their pure form, they are often used only as compounding agents.

[0006] Vanillin is currently produced industrially and very cheaply from lignin, a waste product of the paper industry. By 2014, production of vanillin had already exceeded 17,000 tons. Vanillin is known to be used as a flavoring in the food industry and is non-toxic. Methacrylated vanillin is also known. In addition to its production, its use in composites or 3D printing has been described, for example, in Stanzione III et al., “Vanillin-based resin for use in composite applications”, Green Chem., 2012, 14, 2346-2352, or in Bassett et al., “Vanillin-Based Resin for Additive Manufacturing”, ACS Sustainable Chem. Eng. 2020, 8, 5626-5635.

[0007] However, in the field of fiber composite materials, two problems arise when using methacrylated vanillin. Firstly, because methacrylated vanillin is a solid, it cannot be used directly in the processing of general fiber composites. While methacrylated vanillin does dissolve in acrylate monomers commonly used as reactive diluents, such as 1,6-hexanediol diacrylate (HDDA), when this solution is mixed with the curing agent and accelerator required for use, the methacrylated vanillin crystallizes again, rendering it unusable. Secondly, cured methacrylated vanillin is very brittle, making it unsuitable as a matrix resin for fiber composite materials.

[0008] From prior art, for example, a mixture of methacrylated vanillin and acrylated epoxidized soybean oil is known from Zhang, C. et al. “Biorenewable Polymers based on acrylated epoxidized soybean oil and methacrylated vanillin”, Materials Today Communications 5 (2015) 18-22. However, the mechanical properties of the cured mixture are not sufficient for the manufacture of fiber composite components.

[0009] Experiments conducted by the inventors revealed that, as previously mentioned, a mixture of methacrylated vanillin and cardanol, often used in the field of polyester chemistry, lacks storage stability. Similarly, methacrylated vanillin also crystallizes.

[0010] Experiments conducted by the inventors further revealed that while a mixture of methacrylated vanillin, cardanol, and an acrylate monomer, such as HDDA, does indeed exhibit better storage stability as a reactive diluent, it also spontaneously crystallizes when mixed with a curing agent or accelerator, rendering it unusable.

[0011] Therefore, the object of the present invention was to overcome at least one of the above-mentioned drawbacks.

[0012] Surprisingly, this challenge is... - At least one aldehyde (A), - At least one phenolic compound (B), - At least one amine (C) having at least two amino groups selected from the group consisting of primary and secondary amino groups, and A composition comprising, It was found that at least one of these compounds could be resolved by a composition having at least one (meth)acrylate group.

[0013] This composition is advantageous as a resin, or resin system, that yields a thermosetting resin (a so-called thermosetting resin system) upon curing. This resin exhibits a property profile that is highly advantageous for the manufacture of composite materials, particularly fiber composite materials. This resin has storage stability, low viscosity, and can be mixed without problems with conventional curing agents and accelerators for further use. After the addition of curing agents and accelerators, this resin has a sufficiently long pot life (working time) of approximately 4 hours, which is very important in practice. This resin can be pre-cured at a moderate temperature of 40°C to 100°C, for example, 60°C. After post-curing at a temperature above 100°C to 200°C, for example, 140°C, this resin exhibits very good mechanical properties and is not brittle. Therefore, it is highly suitable for the manufacture of thermosetting resins and fiber composite materials.

[0014] Therefore, the first subject of the present invention is - At least one aldehyde (A), - At least one phenolic compound (B), - At least one amine (C) having at least two amino groups selected from the group consisting of primary and secondary amino groups, and A composition comprising, At least one of these compounds is a composition having at least one (meth)acrylate group.

[0015] Further subject matter of the present invention is - A fibrous material comprising at least one fibrous material, preferably composed of one or more renewable raw materials, - Composition according to the present invention and It is a fiber-reinforced composition containing [the specified ingredient].

[0016] Further subject matter of the present invention is a method for curing a composition or fiber-reinforced composition according to the present invention, wherein the curing is carried out by radical and non-radical curing mechanisms, and the curing is advantageously (i) A step of performing thermal pre-curing and / or photochemical pre-curing with chemical light, particularly UV light, at a temperature of 40°C to 100°C, especially for a period of 1 to 8 hours, (ii) A step of performing thermal post-curing at a temperature of over 100°C to 200°C, particularly for a period of 1 to 8 hours. The method is characterized by including [a certain element].

[0017] A further subject of the present invention is a fiber composite material or thermosetting resin that can be obtained by the method according to the present invention.

[0018] The advantageous configurations of the present invention are defined in the dependent claims, embodiments, and detailed description of the invention. Furthermore, it is explicitly noted that the disclosure of the subject matter of the present invention encompasses all combinations of the preceding and subsequent descriptions of the invention and the individual features of the claims. In particular, one embodiment of the subject matter of the present invention also corresponds to another embodiment of the subject matter of the present invention with necessary modifications.

[0019] The subject matter of the present invention and its preferred embodiments are described below illustratively, but the invention is not intended to be limited to these exemplary embodiments. Where ranges, general formulas, or compound classes are shown below, these include not only the corresponding ranges or groups of compounds explicitly mentioned, but also all subranges and subcompound groups obtained by selecting individual values ​​(ranges) or compounds. Where any document is referenced herein, its entirety constitutes the disclosure of the present invention.

[0020] Wherever measurements, parameters, or material properties are shown below, unless otherwise specified, these are measurements taken at 25°C, preferably at standard pressure. Standard pressure is understood to be 101325 Pa.

[0021] The term "(meth)acryl" represents "methacryl" and / or "acryl". Therefore, the term "(meth)acrylate group" represents a methacrylate group and / or an acrylate group. Here, the methacrylate group is understood to be a methacrylic acid ester group, and the acrylate group is understood to be an acrylic acid ester group.

[0022] As already explained above, the composition according to the invention - at least one aldehyde (A), - at least one phenolic compound (B), - at least one amine (C) having at least two amino groups selected from the group consisting of primary amino groups and secondary amino groups and wherein at least one of these compounds has at least one (meth)acrylate group.

[0023] (Meth)acrylate groups are necessary for the radical curing mechanism. Furthermore, aldehyde (A), phenolic compound (B) and amine (C) are necessary for a non-radical curing mechanism which proceeds by the Betti reaction / Mannich reaction, although not bound by theory.

[0024] It is preferred that at least one of compounds (A), (C) and (B) is produced from renewable raw materials or is a renewable raw material. It is particularly preferred that at least one aldehyde (A) and phenolic compound (B) are produced from renewable raw materials and / or are renewable raw materials. Depending on the composition of the mixture, it is possible to achieve, for example, a weight fraction of 75 to 96% of bio-based raw materials relative to the total weight of the composition.

[0025] It is preferable that at least one or all of the aldehydes (A) have at least one (meth)acrylate group. Furthermore, it is preferable that at least one or all of the aldehydes (A) are aromatic. Therefore, it is equally preferable that at least one or all of the aldehydes (A) are aromatic and have at least one (meth)acrylate group. It is even more preferable that at least one of the aldehydes (A) is (meth)acrylic vanillin (vanillin (meth)acrylate). It is particularly preferable that (meth)acrylic vanillin (vanillin (meth)acrylate) is used exclusively as the aldehyde (A). The terms "(meth)acrylic vanillin" and "vanillin (meth)acrylate" are used synonymously in this invention. "(meth)acrylic vanillin" or "vanillin (meth)acrylate" refers to 4-(meth)acryloxy-3-methoxybenzaldehyde, which is the (meth)acrylic acid ester of 4-hydroxy-3-methoxybenzaldehyde (vanillin). Methacrylic vanillin (vanillin methacrylate, 4-methacryloxy-3-methoxybenzaldehyde) is represented by formula (I): [ka] It has a structure based on the following.

[0026] Accordingly, acrylic vanillin (vanillin acrylate, 4-acrylooxy-3-methoxybenzaldehyde) is given by formula (II): [ka] It has a structure represented by the following:

[0027] It is particularly preferable that at least one aldehyde (A) is methacrylated vanillin (vanillin methacrylate, 4-methacryloxy-3-methoxybenzaldehyde) or contains the same. This compound is available, for example, from Evonik under the name Visiomer® VALMA.

[0028] The composition according to the present invention further comprises at least one phenolic compound (B). Here, a phenolic compound is understood to be a compound having one or more hydroxyl groups on one or more aromatic systems, also called aromatic ring systems. Thus, these hydroxyl groups are each bonded to one carbon atom that is part of the aromatic system. The simplest example of a phenolic compound is phenol (hydroxybenzene).

[0029] It is preferable that at least one or all of the phenolic compounds (B) are ethylenically unsaturated compounds. Here, an ethylenically unsaturated compound is understood to be a compound containing at least one C=C double bond that is not part of an aromatic system. Therefore, it is preferable that the phenolic compound (B) contains at least one C=C double bond that is not part of an aromatic system. Although not bound by theory, C=C double bonds are thought to be at least partially involved in the radical hardening mechanism.

[0030] It is particularly preferable that at least one or all of the phenolic compounds (B) are cardanol. Cardanol is a phenolic compound obtained by decarboxylation of anacardic acid. Anacardic acid is the main component of cashew nut shell liquid or cashew nut shell oil, which are by-products of cashew nut processing. In this invention, anacardic acid is understood to be the compound of formula (III), and cardanol is understood to be the compound of formula (IV). [ka] [ka] Here, R is either a saturated or unsaturated hydrocarbon group, independently of each other.

[0031] The anacardic acid in cashew nut shell oil, and the cardanol obtained therefrom, generally have a hydrocarbon group R with 15 carbon atoms, where the degree of saturation can vary. Cardanol obtained from cashew nut shell oil contains approximately 41% triunsaturated cardanol, approximately 34% monounsaturated cardanol, approximately 22% diunsaturated cardanol, and approximately 2% saturated cardanol, each expressed as a weight percentage of the total weight of cardanol.

[0032] Therefore, it is preferable that the group R of formula (III) or (IV) is a hydrocarbon group having 15 carbon atoms. It is even more preferable that the group R of formula (III) or (IV) has 0, 1, 2, or 3 C=C double bonds.

[0033] Therefore, it is particularly preferable that the groups R in formulas (III) and (IV) are each groups having 15 carbon atoms independently of each other, and that they have 0, 1, 2, or 3 C=C double bonds.

[0034] Since the C=C double bond is radically polymerizable, it is even more preferable that each of the groups R independently has at least one C=C double bond.

[0035] Therefore, each group R is a group having at least one C=C double bond and / or 15 carbon atoms, and it is particularly preferable that each group R has at least one C=C double bond and 15 carbon atoms.

[0036] The group of anacardic acids is given that name, and anacardic acid, the main component of anacardic acids in cashew nut shell oil, is, for example, formula (V) [ka] The group R is present, where the dashed line represents a covalent bond with the benzene ring. Therefore, it is preferable that the R in formulas (III) and (IV) is the group of formula (V). Equally preferred is the group R derived from the group of formula (V) (in form) by hydrogenation / saturation of one, two, or all three C=C double bonds.

[0037] Cardanol is commercially available. Particularly preferred is formula (VI) [where R = -C7H]. 14 Cardanol NX-2026 (Cardolite) is a divalent unsaturated cardanol with the formula -CH=CH-CH2-CH=CH-C3H7. In equations (III) and (IV), R = -C7H 14 -CH=CH-CH2-CH=CH-C3H7 is preferable.

[0038] The composition according to the present invention further comprises at least one amine (C) having at least two amino groups selected from the group consisting of primary amino groups and secondary amino groups. Primary or secondary amino groups are required for the Mannich reaction or the Betty reaction. In contrast, tertiary amino groups cannot be reacted in the Mannich reaction or the Betty reaction.

[0039] The compositions according to the present invention preferably comprise at least one amine (C) having at least two primary amino groups.

[0040] It is even more preferable that the amine (C) is aromatic. An aromatic amine is an amine that has one or more amino groups bonded to each carbon atom that is part of an aromatic system. The simplest example of an aromatic amine is aniline (phenylamine, aminobenzene).

[0041] It is even more preferable that amine (C) is a dianiline. Dianiline is understood to be a compound having two aminophenyl groups, particularly two 4-aminophenyl groups. Here, according to the present invention, the amino group is selected from the group of primary amino groups and secondary amino groups. Therefore, amine (C) is particularly preferably a dianiline having a primary amino group.

[0042] At least one amine (C) is selected from the group consisting of substituted or unsubstituted 4,4'-isopropylidenedianilines, substituted or unsubstituted 4,4'-methylenedianilines, and substituted or unsubstituted 4,4'-sulfonyldianilines, and more preferably, is selected from the group consisting of 4,4'-methylenebis(2,6-diethylaniline), 4,4'-methylenebis(2,6-diisopropylaniline), and 4,4'-diaminodiphenylsulfone. It is particularly preferred that at least one amine (C) is 4,4'-diaminodiphenylsulfone.

[0043] Dianilines are commercially available. For example, 4,4'-methylenebis(2,6-diethylaniline) is commercially available under the name Lonzacure® M-DEA (Lonza), 4,4'-methylenebis(2,6-diisopropylaniline) under the name Lonzacure® M-DIPA (Lonza), and 4,4'-diaminodiphenylsulfone under the name Aradur® 976-1 (Huntsman).

[0044] It is preferable that the composition according to the present invention further comprises at least one (meth)acrylate(D). Here, (meth)acrylate is understood to be a compound having one or more (meth)acrylate groups, i.e., one or more methacrylic acid ester groups and / or acrylic acid ester groups. (Meth)acrylate(D) acts as a reactive diluent and / or crosslinking agent. As a reactive diluent, (meth)acrylate(D) may have one or more (meth)acrylate groups. As a crosslinking agent, (meth)acrylate(D) must have at least two (meth)acrylate groups. Therefore, when (meth)acrylate(D) is used as both a reactive diluent and a crosslinking agent, it is necessary that (meth)acrylate(D) has at least two (meth)acrylate groups. Therefore, it is preferable that at least one or all of the (meth)acrylate(D) have at least two (meth)acrylate groups. It is more preferable that at least one or all of the (meth)acrylate(D) have 2 to 6 (meth)acrylate groups. Advantageously, the (meth)acrylate(D) consists only of the elements carbon, hydrogen, oxygen, and nitrogen, and in particular, only of the elements carbon, hydrogen, and oxygen. Preferred (meth)acrylate(D) are described in European Coatings Tech Files, Patrick Gloeckner et al. “Strahlenhaertung: Beschichtungen und Druckfarben”, 2008, Vincentz Network, Hannover, Germany.

[0045] Advantageously, at least one (meth)acrylate (D) is selected from the group consisting of trimethylolpropane triacrylate (TMPTA), tripropylene glycol diacrylate (TPGDA), dipropylene glycol diacrylate (DPGDA), isobornyl acrylate (IBOA), lauryl acrylate, dodecyl acrylate, 1,6-hexanediol diacrylate (HDDA), tridecyl acrylate, pentaerythritol triacrylate, polyethylene glycol diacrylate, and ethoxylated and / or propoxylated derivatives thereof.

[0046] It is equally preferable that at least one (meth)acrylate (D) is selected from the group consisting of (meth)acrylic acid esters of vanillyl alcohol (4-hydroxy-3-methoxybenzyl alcohol), guaiacol, and creosol, as described, for example, Holmberg, AL et al., “Softwood Lignin-Based Methacrylate Polymers with Tunable Thermal and Viscoelastic Properties”, Macromolecules 2016, 49, 1286-1295. Similar to (meth)acrylic vanillin, these compounds are compounds produced from lignin, a renewable raw material.

[0047] Suitable (meth)acrylate (D) products include Ebecryl® TMPTA (Allnex SA, Germany), Ebecryl® OTA480 (propoxylated glyceryl triacrylate, Allnex SA, Germany), Ebecryl® TPGDA (Allnex SA, Germany), Ebecryl® DPGDA (Allnex SA, Germany), Ebecryl® 892 (Allnex SA, Germany), Ebecryl® 11 (polyethylene glycol diacrylate, Allnex SA, Germany), Ebecryl® 45 (Allnex SA, Germany), PETIA (a mixture of pentaerythritol triacrylate and tetraacrylate, Allnex SA, Germany), and Ebecryl® 150 (bisphenol A-based diacrylate, Allnex SA, Germany). SA, Germany), Ebecryl® 605 (mixture of 80% bisphenol A diepoxyacrylate and 20% TPGDA, Allnex SA, Germany), Ebecryl® 40 (ethoxylated and propoxylated pentaerythritol tetraacrylate, Allnex SA, Germany), Laromer® TMPTA (BASF, Germany), Miramer® M200 (HDDA, Rahn AG, Germany), Miramer® M220 (TPGDA, Rahn AG, Germany), Miramer® 3130 (ethoxylated trimethylolpropane triacrylate, Rahn AG, Germany), SR 415 (ethoxylated trimethylolpropane triacrylate, Sartomer, France), SR It is marketed under the names 489 (tridecyl acrylate, Sartomer, France) and Sarbio® 5101 (dodecyl acrylate, Arkema, France).

[0048] Suitable (meth)acrylate (D) is also commercially available from Evonik Operations GmbH (Germany) under the VISIOMER® product line. Preferred compounds include glycerin formal methacrylate (VISIOMER® GLYFOMA), diurethane dimethacrylate (VISIOMER® HEMA TMDI), butyl diglycol methacrylate (VISIOMER® BDGMA), polyethylene glycol 200 dimethacrylate (VISIOMER® PEG200DMA), trimethylolpropane methacrylate (VISIOMER® TMPTMA), tetrahydrofurfuryl methacrylate (VISIOMER® THFMA), isobornyl methacrylate (VISIOMER® Terra IBOMA), isobornyl acrylate (VISIOMER® IBOA), methacrylate of fatty alcohols having an average of 13.0 carbon atoms (VISIOMER® Terra C13-MA), or methacrylate of fatty alcohols having an average of 17.4 carbon atoms (VISIOMER® Terra This is C17.4-MA).

[0049] Particularly preferred, the composition comprises at least one (meth)acrylate (D) selected from the group of diol and triol-based bifunctional and trifunctional acrylates, particularly 1,6-hexanediol diacrylate (HDDA).

[0050] Preferably, the composition according to the present invention further comprises at least one initiator (E).

[0051] The initiator (E) of the composition according to the present invention is a compound that forms a radical when exposed to an external trigger. This trigger may be chemical light, preferably UV light and / or visible light, or heat. Thus, the initiator (E) may be an initiator for photochemical radical curing or polymerization (photoinitiator) and / or an initiator for thermal radical curing or polymerization (thermal initiator).

[0052] Advantageously, as thermal initiators, organic peroxides are used, such as 2,5-bis(tert-butylperoxy)-2,5-dimethylhexane (e.g., LUPEROX 101®) from Arkema (France), dilauroyl peroxide (e.g., LUPEROX LP®), dibenzoyl peroxide (e.g., LUPEROX A98®), and bis(tert-butyldioxyisopropyl)benzene (e.g., VulCUP R®), or Peroxan BP-Pulver 50 W from Pergan GmbH (Germany), i.e., a powder containing about 40-50% by weight of dibenzoyl peroxide and about 40-50% by weight of dicyclohexyl phthalate. Preferred thermal initiators include ketone peroxides such as methyl ethyl ketone peroxide, diacyl peroxides such as benzoyl peroxide, hydroperoxides such as cumene hydroperoxide, as well as peroxyketals, dialkyl peroxides, peroxydicarbonates and peroxyesters, and inorganic peroxides, such as peroxodisulfates including sodium persulfate (Na2S2O8), potassium persulfate (K2S2O8) and ammonium persulfate ((NH4)2S2O8), and even azobisisobutyronitrile (AIBN).

[0053] Suitable photoinitiators include all photoinitiators known to those skilled in the art, including Norrish type I and Norrish type II photoinitiators. These include commonly used UV photoinitiators such as acetophenones (e.g., diethoxyacetophenone) and phosphine oxides (e.g., diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (PPO), and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide). Particularly preferred are Norrish type I photoinitiators such as benzophenone, benzoin, α-hydroxyalkylphenone, acylphosphine oxides, or their derivatives. Suitable photoinitiators are described, for example, in “A Compilation of Photoinitiators Commercially available for UV today” (K. Dietliker, SITA Technology Ltd., London 2002).

[0054] Preferably, the composition according to the present invention further comprises at least one accelerator (F).

[0055] If the composition contains a thermal initiator, it is preferable that it contains an accelerator (F) that promotes the radical thermal curing. Examples of such accelerators include organic acid metal salts such as cobalt naphthenate, and tertiary aromatic amines, preferably tertiary aromatic amines such as N,N-dimethylaniline, N,N-diethylaniline, and N,N-dimethylparatoluidine.

[0056] If the composition contains a photoinitiator, it is preferable that it contains an accelerator (F) that promotes the photochemical radical curing. Such accelerators are also called photosensitizers. Examples include amines such as n-butylamine, triethylamine, N-methyldiethanolamine, piperidine, N,N-dimethylaniline, and triethylenetetramine; sulfur compounds such as S-benzylisothiuronium-p-toluenesulfinate; phosphorus compounds such as N,N-dimethyl-p-aminobenzonitrile; and sodium diethylthiophosphate.

[0057] The composition according to the present invention is particularly preferably to contain, as an accelerator (F), at least one tertiary amine, preferably at least one tertiary aromatic amine, in particular N,N-diethylaniline. N,N-diethylaniline is commercially available as a solution, for example, from Pergan GmbH (Germany) under the name PERGAQUICK A3X. Here, the solution contains about 5-10% by weight of N,N-diethylaniline and about 80-90% by weight of 1-isopropyl-2,2-dimethyltrimethylenediisobutyrate.

[0058] Preferably, the composition according to the present invention further comprises at least one further additive (G). Advantageously, additive (G) is a substance capable of modifying the properties of the uncured or cured composition as desired. This may be, for example, a dye, pigment, rheology modifier, or impact modifier, or a nanoscale filler processable by infusion or injection molding. Examples include acrylate-functionalized acrylonitrile-butadiene copolymers, such as Hypro® VTBNX 1300x43 from Huntsman, Tegomer® M-Si 2650 from Evonik Operations, nanosilica, and nanoaluminates.

[0059] Each composition according to the present invention, in relation to the total weight of the composition, - One or more aldehydes (A) making up 60% to 90% in total, preferably 65% ​​to 85%, and especially 70% to 80% by weight, - One or more phenolic compounds (B) in total weight proportions of 1% to 25%, preferably 3% to 20%, and especially 5% to 15%, - One or more amines (C) in total weight proportions of 1% to 20%, preferably 2% to 10%, and especially 3% to 5%, - One or more (meth)acrylate (D) in a total weight of 1% to 25%, favorably 3% to 20%, especially 5% to 15%. - One or more initiators (E) in total weight proportions of 0.1% to 5%, preferably 0.2% to 4%, and especially 0.3% to 1%, - One or more accelerators (F) in total weight proportions of 0% to 10%, preferably 0.01% to 5%, and especially 0.02% to 2%, - One or more additives (G) in total weight proportions of 0% to 10%, preferably 0.01% to 5%, and especially 0.02% to 2%. It is preferable that it contains or consists of the following components.

[0060] The essential or optional components of the composition according to the present invention, namely aldehydes (A), phenolic compounds (B), amines (C), (meth)acrylates (D), initiators (E), accelerators (F), and additives (G), are all distinct from one another. If a compound belongs in principle to two or more of the aforementioned groups (A), (B), (C), (D), (E), (F), and (G), it shall be assigned to the group that is listed first in the above order, unless there is an explicit deviation from this rule. For example, if a compound belongs to any of groups (B), (D), and (G), it shall be assigned to the group that is listed first, i.e., (B) in this example. Therefore, no single compound can be assigned to more than one of the groups (A), (B), (C), (D), (E), (F), and (G).

[0061] The compositions according to the present invention can be used in electronics as potting compounds or in stereolithography (SLA). However, the compositions according to the present invention are particularly suitable for the manufacture of fiber-reinforced compositions and, by extension, fiber composite materials produced therefrom.

[0062] Therefore, a further subject of the present invention is, - A fibrous material comprising at least one fibrous material, preferably composed of one or more renewable raw materials, - Composition according to the present invention and It is a fiber-reinforced composition containing [the specified ingredient].

[0063] The fibrous material is preferably a monofilament, a fiber bundle containing a monofilament, or a yarn containing a monofilament or fiber bundle. More preferably, the fibrous material is a product such as a laid web and fabric containing a monofilament, fiber bundle, or yarn. A laid web containing a fiber bundle is particularly preferred. In the case of fabrics, these are preferably linen fabrics. A preferred laid web is constructed in layers, and these layers may be oriented in the same direction (uniaxial) or in different directions (multiaxial). An advantage of the laid web is that the fibers or fiber bundles of the layers are not bent by the braiding operation. As a result, a higher force absorption capacity can be obtained. The fibrous material is advantageously a glass fiber material, a mineral fiber material, a natural fiber material, and / or a polymer fiber material, preferably a natural fiber material, especially a natural fiber. More preferably, the fibrous material is a laid web composed of a glass fiber material, a mineral fiber material, a natural fiber material, and / or a polymer fiber material, especially a laid web composed of a natural fiber. The fibrous material is preferably a prepared material, either as a purified material or already coated, and preferably a purified fibrous material is used. Purification is preferably material-dependent, and a preferred purification method is heat treatment, particularly preferably irradiation using an IR emitter. The heat treatment can optionally be carried out under a protective gas. During this purification step, water, which is almost always present in natural fibers, is removed, in particular, as it can be an obstacle during subsequent processing to obtain a fibrous composite. It is preferable that the fibrous material is selected from the group consisting of flax fibers, hemp fibers, jute fibers, kenaf fibers, ramie fibers, sisal fibers, and wood fibers. The fibers can be modified as desired by ultrasonic decomposition so that they are given reproducible technical properties by a standardizable processing process.

[0064] The compositions and fiber-reinforced compositions according to the present invention are curable by a specific method. Here, the curing of these compositions can be carried out by either a radical curing mechanism or a non-radical curing mechanism.

[0065] Therefore, a further subject of the present invention is a method for curing a composition or fiber-reinforced composition according to the present invention, wherein the curing is carried out by radical and non-radical curing mechanisms, and the curing is advantageously (i) A step of performing thermal pre-curing and / or photochemical pre-curing with chemical light, particularly UV light, at a temperature of 40°C to 100°C, especially for a period of 1 to 8 hours, (ii) A step of performing thermal post-curing at a temperature of over 100°C to 200°C, particularly for a period of 1 to 8 hours. The method is characterized by including [a certain element].

[0066] The advantage here is that pre-curing is carried out by a radical curing mechanism, and post-curing is carried out by a non-radical curing mechanism.

[0067] During the radical curing mechanism, radical polymerization of (meth)acrylate groups and optionally ethylenically unsaturated double bonds occurs. Radical polymerization can be induced thermally or photochemically. In this case, thermal pre-curing is used particularly in the manufacture of fiber composite materials, while photochemical pre-curing is used in the field of stereolithography.

[0068] While not bound by theory, the non-radical hardening mechanism can be considered a generalized Betti reaction, which can be viewed as a special case of the Mannich reaction. The Betti reaction is described, for example, in Cardellicchio et al. “The Betti base: the awakening of a sleeping beauty”, Tetrahedron: Asymmetry Volume 21, Issue 5, 30 March 2010, Pages 507-517. https: / / en.wikipedia.org / wiki / Betti_reaction and https: / / de.wikipedia.org / wiki / Betti-Reaktion (See also). In this case, the aldehyde (A), phenolic compound (B), and amine (C) are thought to react with each other via the Betti reaction. This reaction is schematically shown in Figure 1.

[0069] Particularly preferably, thermal post-curing (ii) is carried out at a temperature of 140°C to 150°C.

[0070] The compositions according to the present invention are advantageously stable, low-viscosity resins that can be used in the general manufacturing processes of fiber composite materials. Therefore, the methods according to the present invention are preferably injection molding or infusion methods (e.g., VARI; vacuum infusion). These methods are known to those skilled in the art.

[0071] The method according to the present invention makes it possible to manufacture thermosetting resins or fiber composite materials having outstanding mechanical properties.

[0072] Therefore, a further subject of the present invention is a fiber composite material or thermosetting resin that can be obtained by the method according to the present invention.

[0073] The fiber composite material and thermosetting resin according to the present invention are used as components or molded components (for example, as pure resin sheets, as fiber composite components, etc.) in aircraft construction, rail vehicle construction, automobile manufacturing, shipbuilding, machinery construction, plant construction, civil engineering and construction, and in the manufacture of rotor blades for wind power plants.

[0074] It is assumed that those skilled in the art will be able to make the most of the above description without further detail. Therefore, preferred embodiments and examples should be interpreted as merely descriptive disclosures and not as limiting disclosures in any way.

[0075] The subject matter of the present invention will be explained in detail with reference to Figures 1 and 2, but the subject matter of the present invention is not limited to these. [Brief explanation of the drawing]

[0076] [Figure 1]This diagram schematically illustrates the formation of a Betti base / Mannich base (4) and the elimination of water through the condensation reaction (Betti reaction / Mannich reaction) of a phenolic compound (1), an aldehyde (2), and an amine (3). [Figure 2] This figure shows the differential scanning calorimetry (DSC) results of the compositions according to the present invention described in the examples. Two peaks were observed: one representing radical pre-curing and the other representing non-radical post-curing.

[0077] Examples General methods: Glass transformation temperature / glass transition temperature (Tg): The glass transformation temperature / glass transition temperature (Tg) is measured by dynamic viscoelasticity measurement (DMA) in accordance with the standard ISO 6721-11:2019-06.

[0078] Modulus of elasticity (E): The modulus of elasticity (E) is measured by dynamic viscoelasticity measurement (DMA) in accordance with the standard ISO 6721-4:2019-05.

[0079] Impact strength: Impact strength will be measured in accordance with the standard ISO 179-1:2010-11.

[0080] viscosity: Viscosity is measured in accordance with the standard DIN EN ISO 3219:1994-10.

[0081] Bending strength: The bending strength is measured by a three-point bending test in accordance with the standard ISO 178:2019-04.

[0082] Flexural modulus: The flexural modulus is measured by a three-point bending test in accordance with the standard ISO 178:2019-04.

[0083] Differential scanning calorimetry (DSC): Differential scanning calorimetry (DSC) will be performed in accordance with DIN EN ISO 11357-1:2017-02, DIN EN ISO 11357-2:2020-08, and DIN EN ISO 11357-4:2014-10.

[0084] Raw materials / materials: [Table 1]

[0085] Resin and fiber composite materials: a) Manufacturing of resins Using a Speedmixer, a mixture was first prepared from 76 parts by weight of Visiomer® VALMA, 10 parts by weight of Cardanol NX-2026, 10 parts by weight of HDDA, and 4 parts by weight of Aradur® 976-1. This mixture was then heat-treated at 60°C for 2 hours. A clear liquid product with a viscosity of 260 mPas (measured at 25°C) was obtained. This product was storage stable. The product remained clear even after storage for several months and could be used further without problems by the infusion method.

[0086] b) Curing and mechanical properties of the resin Product a) 100 parts by weight were mixed with 2 parts by weight of Peroxan BP Pulver 50W and 0.5 parts by weight of Pergaquick A3X under inert gas (N2). The pot life of this mixture was approximately 4 hours at 60°C. This mixture was pre-cured at 60°C for 6 hours, and then post-cured at 140°C for 2 hours. The cured product had a glass transformation temperature Tg of approximately 120°C, an elastic modulus of 1.8 GPa, and an elasticity of 1.5 kJ / m 2 It possesses the following impact strength. Two peaks were observed in DSC: one representing radical pre-curing and the other representing non-radical post-curing.

[0087] For comparison: Similarly cured vinyl ester resins typically have a glass transformation temperature of approximately 130°C and an elastic modulus of approximately 3 GPa. Furthermore, vinyl ester resins are very brittle. Standard epoxy resins such as DGEBA (e.g., Araldite® LY 556 from Huntsman) cured with anhydrous resin (e.g., Albidur® HE 600) have a Tg of 130°C and an elastic modulus of 2.8 GPa. It should be noted that the structure of the cured resin according to the present invention differs from that of both epoxy resins and vinyl ester resins, particularly due to a different curing mechanism. Therefore, different mechanical properties are expected.

[0088] c) Manufacturing and mechanical properties of fiber composite materials Product a) 100 parts by weight were mixed with 2 parts by weight of Peroxan BP Pulver 50W and 0.5 parts by weight of Pergaquick A3X under inert gas (N2). The resulting mixture was then treated by vacuum infusion (VARI). As a fibrous material, a ±45° structure (Bcomp / ampliTex® 5008 from Switzerland) and a basis weight of 350 g / m² were used. 2 Four layers of a laid web of biaxial flax fibers are used. The resulting fiber-reinforced resin is pre-cured at 60°C for 4 hours under vacuum, and then post-cured in an oven at 140°C for 6 hours. The weight percentage of renewable raw materials in the resulting fiber composite sheet is 93% of the total weight of the fiber composite material. This fiber composite sheet has a glass transformation temperature of approximately 120°C, a flexural strength of 137 MPa, and a flexural modulus of 9.8 GPa.

[0089] For comparison: A fiber composite sheet manufactured under equivalent conditions using the same textile laid web (same manufacturing batch), cured with a standard epoxy resin (Huntsman LY 556) and amine (Evonik Ancamine® 2167), at 80°C for 2 hours and then at 150°C for 4 hours, has a Tg of 108°C, a flexural strength of 160 MPa, and a flexural modulus of 9.4 GPa. For jute-reinforced members based on unsaturated polyester resin, the literature states a flexural strength of 80 MPa and a flexural modulus of 4.8 GPa.

[0090] Substitution of vanillin methacrylate in an equimolar mixture of vanillin and acrylic acid Similar to the method described in a), a mixture of 52 parts by weight of vanillin, 24 parts by weight of acrylic acid, 10 parts by weight of Cardanol NX-2026, 10 parts by weight of HDDA, and 4 parts by weight of Aradur® 976-1 was first prepared in a Speedmixer, and this composition was then heat-treated at 60°C for 2 hours. The vanillin could not be completely dissolved. Therefore, a clear solution could not be obtained. The resulting composition was a suspension. This composition was not suitable for use in the infusion method because the solid components of the composition could not flow through the fabric without being held by the fabric. Furthermore, after storage at room temperature for 4 hours, some of the undissolved vanillin settled at the bottom of the storage container.

[0091] Furthermore, we attempted to cure the resulting mixture according to the method described in b). No curing was observed at 60°C. At 140°C, intense smoke was produced, which is likely due to the leaching and decomposition of acrylic acid. Ultimately, we obtained a carbonized and crumbling solid that was completely unusable.

Claims

1. at least one aldehyde (A), at least one phenolic compound (B), at least one amine (C) having at least two amino groups selected from the group consisting of primary and secondary amino groups; A composition comprising: A composition, wherein at least one of said compounds has at least one (meth)acrylate group.

2. 2. The composition of claim 1, wherein at least one of the compounds (A), (C) and (B) is produced or is a renewable source.

3. The composition of claim 1 , wherein the at least one aldehyde (A) has at least one (meth)acrylate group.

4. The composition of claim 1 , wherein at least one aldehyde (A) is aromatic.

5. 2. The composition of claim 1, wherein the at least one aldehyde (A) is methacrylated vanillin.

6. The composition of claim 1 , wherein the at least one phenolic compound (B) is an ethylenically unsaturated compound.

7. The composition of claim 1 , wherein the at least one phenolic compound (B) is cardanol.

8. The composition of claim 1 , wherein at least one amine (C) is aromatic.

9. The composition of claim 1 , wherein the composition further comprises at least one (meth)acrylate (D).

10. The composition, at least one initiator (E), optionally at least one accelerator (F), optionally with at least one further additive substance (G); The composition of claim 1 further comprising:

11. The composition comprises, each based on the total weight of the composition: one or more aldehydes (A), in a total proportion by weight ranging from 60% to 90%, one or more phenolic compounds (B) in a total proportion by weight ranging from 1% to 25%, one or more amines (C), in a total proportion by weight ranging from 1% to 20%, one or more (meth)acrylates (D) in a total proportion by weight ranging from 1% to 25%, one or more initiators (E), in a total proportion by weight ranging from 0.1% to 5%, one or more accelerators (F), in a total proportion by weight ranging from 0% to 10%, - one or more additive substances (G) in a total proportion by weight between 0% and 10%; 2. The composition of claim 1, comprising or consisting of the components:

12. at least one textile material, - a composition according to claim 1; 1. A fiber reinforced composition comprising:

13. 13. A method for curing the composition of claim 1 or the fiber reinforced composition of claim 12, characterized in that the curing is carried out by radical and non-radical curing mechanisms.

14. The method of claim 13, wherein the method is an injection molding method or an infusion method.

15. A fibre composite material or a thermoset material obtainable by the process according to claim 13.