Copper foil capable of preventing tear or wrinkle defect, electrode comprising the same, secondary battery comprising the same, and method for manufacturing the same

JP2024094274A5Active Publication Date: 2024-10-15SK NEXILIS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023214072
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-10-05
Filing Date
2023-12-19
Publication Date
2024-10-15
Estimated Expiration
2043-12-19

AI Technical Summary

Technical Problem

The challenge of manufacturing thin copper foils for secondary batteries is the occurrence of wrinkles and ruptures due to curling, which affects the efficiency and capacity of the batteries, and existing technologies struggle to maintain stability and high capacity while preventing these defects.

Method used

A copper foil with specific stress coefficient ranges (2.8 to 3.2, 2.5 to 3.0, and 3.5 to 4.5) is developed, along with a manufacturing process that includes precise control of electrolytic conditions and a protective layer to enhance strength and stability, minimizing curling and defects.

Benefits of technology

The solution results in a high-strength copper foil that prevents wrinkles and ruptures, improving the productivity and performance of secondary batteries by maintaining capacity and efficiency during charging and discharging cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide a copper foil capable of preventing tear or wrinkle defects therein.SOLUTION: There are provided: a copper foil that includes a copper film including 99.9 wt.% or more of copper, the copper foil having a first stress factor of 2.8 to 3.2, a second stress factor of 2.5 to 3.0, and a third stress factor of 3.5 to 4.5; and a method for manufacturing the copper foil. The first stress factor is calculated by Equation 1 below. [Equation 1] first stress factor=A / A'+B / B'+C / C' The second stress factor is calculated by Equation 2 below. [Equation 2] second stress factor=A / B+A' / B' The third stress factor is calculated by Equation 3 below. [Equation 3] third stress factor=A / C+A' / C' In the Equations, A is stress at 50% elongation in a MD direction, A' is stress at 50% elongation in a TD direction, B is stress at 10% elongation in the MD direction, B' is stress at 10% elongation in the TD direction, C is stress at 5% elongation in the MD direction, and C' is stress at 5% elongation in the TD direction.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a copper foil capable of preventing rupture or wrinkle defects, an electrode including the same, a secondary battery including the same, and a method for manufacturing the same. [Background technology]

[0002] Secondary batteries are a type of energy conversion device that converts electrical energy into chemical energy, stores it, and then converts the chemical energy back into electrical energy when electricity is needed to generate electricity, and are used as the energy source for portable home appliances such as mobile phones and laptops, as well as electric vehicles. Secondary batteries are also called rechargeable batteries because they can be recharged.

[0003] Secondary batteries, which have economic and environmental advantages over disposable primary batteries, include lead-acid batteries, nickel-cadmium secondary batteries, nickel-hydrogen secondary batteries, and lithium secondary batteries.

[0004] In particular, lithium secondary batteries can store a relatively large amount of energy compared to other secondary batteries in terms of their size and weight. Therefore, lithium secondary batteries are preferred in the field of information and communication devices where portability and mobility are important, and their range of application is expanding as energy storage devices for hybrid and electric vehicles.

[0005] Lithium secondary batteries are used repeatedly, with charging and discharging being one cycle. When a device is operated with a fully charged lithium secondary battery, the lithium ion secondary battery must have a high charge / discharge capacity in order to increase the operating time of the device. Therefore, there is a continuous demand for research to satisfy the ever-increasing expectations (needs) of consumers regarding the charge / discharge capacity of lithium secondary batteries.

[0006] Such secondary batteries include a negative electrode current collector made of copper foil, and among copper foils, electrolytic copper foil is widely used as the negative electrode current collector of secondary batteries. As the demand for secondary batteries increases, the demand for high-capacity, high-efficiency, and high-quality secondary batteries also increases, and thus electrolytic copper foil capable of improving the characteristics of secondary batteries is required. In particular, electrolytic copper foil capable of ensuring high capacity, stable capacity maintenance, and performance of secondary batteries is required.

[0007] Meanwhile, the thinner the copper foil, the more the amount of active material that can be contained in the same space and the more the number of current collectors can be increased, which can increase the capacity of a secondary battery. However, the thinner the copper foil, the more curling occurs, and defects such as copper foil rupture or wrinkles due to edge curling during winding of the copper foil occur, making it difficult to manufacture a very thin film type copper foil. Therefore, in order to manufacture a copper foil with a very thin thickness, it is necessary to prevent the copper foil from curling. Summary of the Invention [Problem to be solved by the invention]

[0008] Therefore, the present invention relates to a copper foil capable of preventing problems caused by the limitations and shortcomings of the related art, an electrode including the same, a secondary battery including the same, and a method for manufacturing the same.

[0009] An embodiment of the present invention provides a copper foil that does not wrinkle or burst by having a first stress coefficient value in the range of 2.8 to 3.2.

[0010] An embodiment of the present invention provides a copper foil that does not wrinkle or burst by having a second stress coefficient value in the range of 2.5 to 3.0.

[0011] One embodiment of the present invention provides a copper foil that does not wrinkle or burst by having a third stress coefficient value in the range of 3.5 to 4.5.

[0012] Another embodiment of the present invention provides a secondary battery electrode including such a copper foil, and a secondary battery including such a secondary battery electrode.

[0013] Yet another embodiment of the present invention provides a method for manufacturing a copper foil that is free from curling, wrinkling, or bursting.

[0014] In addition to the above-mentioned aspects of the present invention, other features and advantages of the present invention will be described below or will be clearly understood by those having ordinary skill in the art to which the present invention pertains from such description. [Means for solving the problem]

[0015] One embodiment of the present invention provides a copper foil comprising: a copper film containing 99.9% by weight or more of copper; and having a first stress coefficient in a range of 2.8 to 3.2, a second stress coefficient in a range of 2.5 to 3.0, and a third stress coefficient in a range of 3.5 to 4.5. In this case, the first stress coefficient is calculated by the following formula 1, [Formula 1] first stress coefficient = A / A' + B / B' + C / C', the second stress coefficient is calculated by the following formula 2, [Formula 2] second stress coefficient = A / B + A' / B', the third stress coefficient is calculated by the following formula 3, [Formula 3] third stress coefficient = A / C + A' / C', A in the formula 1 is the stress at 50% elongation in the MD direction, A' in the formula 1 is the stress at 50% elongation in the TD direction, B in the formula 1 is the stress at 10% elongation in the MD direction, B' in the formula 1 is the stress at 10% elongation in the TD direction, C in the formula 1 is the stress at 5% elongation in the MD direction, and C' in the formula 1 is the stress at 5% elongation in the TD direction. Effect of the Invention

[0016] According to the present invention, it is possible to produce a high-strength copper foil that can prevent wrinkles or ruptures during the copper foil manufacturing process, and by using such a high-strength copper foil to manufacture intermediate parts and final products such as flexible printed circuit boards (FPCBs) and secondary batteries, it is possible to improve the productivity of the intermediate parts as well as the final products. [Brief description of the drawings]

[0017] [Figure 1] FIG. 2 is a cross-sectional view of a copper foil according to an embodiment of the present invention. [Diagram 2] FIG. 4 is a cross-sectional view of a copper foil according to another embodiment of the present invention. [Diagram 3] FIG. 4 is a cross-sectional view of an electrode for a secondary battery according to still another embodiment of the present invention. [Figure 4] FIG. 4 is a cross-sectional view of an electrode for a secondary battery according to still another embodiment of the present invention. [Diagram 5] 4 is a schematic cross-sectional view of a secondary battery according to yet another embodiment of the present invention. [Figure 6] 2 is a copper foil manufacturing apparatus according to still another embodiment of the present invention. [Figure 7] FIG. 2 is a schematic diagram for explaining md and td of a copper foil according to still another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, the embodiments of the present invention will be described in detail with reference to the accompanying drawings. However, the embodiments described below are merely presented for illustrative purposes to facilitate a clear understanding of the present invention, and do not limit the scope of the present invention.

[0019] The shapes, sizes, ratios, angles, numbers, etc. disclosed in the drawings for explaining the embodiments of the present invention are merely examples, and the present invention is not limited to the matters shown in the drawings. The same components may be designated by the same reference numerals throughout the specification. In the description of the present invention, if it is determined that a detailed description of related known technology may unnecessarily obscure the gist of the present invention, the detailed description will be omitted.

[0020] When the terms "including," "having," "consisting of," etc. are used in this specification, other parts may be added unless the expression "only" is used. When an element is expressed in the singular, it includes the plural unless otherwise expressly stated. In addition, in interpreting an element, it is interpreted as including a margin of error even if there is no other express description.

[0021] In describing a positional relationship, for example, when the positional relationship between two parts is described using "above", "at the top", "below", "beside", etc., one or more other parts may be located between the two parts as long as the expressions "immediately" or "directly" are not used.

[0022] Spatially relative terms such as "below," "beneath," "lower," "above," "upper," and the like, may be used to easily describe the relationship of one element or component to another element or component as illustrated in the drawings. Spatially relative terms should be understood to include different orientations of elements in use or operation in addition to the orientation illustrated in the drawings. For example, if an element illustrated in the drawings is turned over, an element described as "below" or "beneath" another element may be placed "above" the other element. Thus, the exemplary term "below" can include both an orientation of below and above. Similarly, the exemplary terms "on" or "up" can include both an orientation of above and below.

[0023] In the case of explaining a temporal relationship, for example, when the temporal sequence is explained using "after", "following", "next to", "before", etc., it can also include cases where the events are not consecutive, since the expressions "immediately" or "directly" are not used.

[0024] Although the terms "first", "second" and the like are used to describe various components, these components are not limited by these terms. These terms are used merely to distinguish one component from another. Therefore, the first component referred to below may be the second component within the technical concept of the present invention.

[0025] The term "at least one" should be understood to include all combinations that can be presented from one or more of the associated items. For example, "at least one of the first item, the second item, and the third item" may mean not only the first item, the second item, or the third item, respectively, but also all combinations of items that can be presented from two or more of the first item, the second item, and the third item.

[0026] The respective features of the various embodiments of the present invention may be partially or fully combined or combined with each other, and various technical interlocking and driving mechanisms may be possible, and each embodiment may be implemented independently of each other, or may be implemented together in a related relationship.

[0027] FIG. 1 is a cross-sectional view of a copper foil 110 according to one embodiment of the present invention.

[0028] 1, the copper foil 110 of the present invention includes a copper film (111) containing 99.9% by weight or more of copper and a protective layer 112 on the copper film 111. In the copper foil 110 shown in FIG. 1, the protective layer 112 is formed on one side of the copper film 111, but the embodiment of the present invention is not limited thereto. Referring to FIG. 2, the protective layer 112 may be formed on both sides of the copper film 111.

[0029] The copper film 111 may be formed on the rotating cathode drum through electroplating, and has a shiny surface that is in direct contact with the rotating cathode drum during the electroplating process, and an opposite matte surface.

[0030] The protective layer 112 is formed by electrodepositing an anticorrosion material on the copper film 111. The anticorrosion material may include at least one of a chromium compound, a silane compound, and a nitrogen compound. The protective layer 112 prevents oxidation and corrosion of the copper film 111 and improves heat resistance, thereby extending the life of the copper foil 110 itself as well as the life of the final product including the copper foil 110.

[0031] According to an embodiment of the present invention, the copper foil 110 has a first stress coefficient value in the range of 2.8 to 3.2. The first stress coefficient value can be obtained by measuring and calculating A, A', B, B', C, and C', respectively, and calculating the measured values ​​of A, A', B, B', C, and C' according to the following Equation 1.

[0032] [Formula 1]

[0033] First stress coefficient = A / A' + B / B' + C / C'

[0034] A in the formula 1 means the stress when the copper foil 110 is elongated by 50% in the MD direction, A' in the formula 1 means the stress when the copper foil 110 is elongated by 50% in the TD direction, B in the formula 1 means the stress when the copper foil 110 is elongated by 10% in the MD direction, B' in the formula 1 means the stress when the copper foil 110 is elongated by 10% in the TD direction, C in the formula 1 means the stress when the copper foil 110 is elongated by 5% in the MD direction, and C' in the formula 1 means the stress when the copper foil 110 is elongated by 5% in the TD direction. Here, A, A', B, B', C and C' are measured using a universal tensile testing machine (UTM).

[0035] 7, there are MD (machine direction) and TD (transverse direction), and the surface characteristics of the machine direction and transverse direction are different from each other. The copper foil 110 according to an embodiment of the present invention is characterized by minimizing the difference between the surface characteristics of the machine direction (MD) and transverse direction (TD).

[0036] According to one embodiment of the present invention, the copper foil 110 may have a first stress coefficient value of 2.8 or greater.

[0037] If the first stress coefficient value of the copper foil 110 is less than 2.8, the difference in stress between the MD and TD may be large when the copper foil 110 is stretched. As a result, wrinkles or ruptures may occur during the manufacturing process of the copper foil 110, and pinholes or curls may occur on the surface of the copper foil 110. This may result in a decrease in workability and an increase in the defective rate of secondary batteries.

[0038] Therefore, in order to prevent the copper foil 110 from wrinkling or bursting during the manufacturing process, the first stress coefficient value of the copper foil 110 needs to be 2.8 or more.

[0039] According to one embodiment of the present invention, the copper foil 110 may have a second stress coefficient value of 2.5 or greater.

[0040] The second stress coefficient value can be obtained by measuring and calculating A, A', B and B', respectively, and calculating the measured values ​​of A, A', B and B' according to the following formula 2.

[0041] [Formula 2]

[0042] Second stress coefficient = A / B + A' / B'

[0043] If the second stress coefficient value of the copper foil 110 is less than 2.5, a stress difference may occur between the MD direction and the TD direction when the copper foil 110 is stretched by 10% and 50%. As a result, wrinkles or ruptures may occur during the manufacturing process of the copper foil 110, and pinholes or curls may occur on the surface of the copper foil 110. This may result in a decrease in the charge / discharge efficiency of the negative electrode material, a decrease in workability, and an increase in the defective rate of secondary batteries.

[0044] Therefore, in order to prevent the copper foil 110 from wrinkling or bursting during the manufacturing process, the second stress coefficient value of the copper foil 110 needs to be 2.5 or more.

[0045] According to one embodiment of the present invention, the copper foil 110 may have a third stress coefficient of 3.5 or greater.

[0046] The third stress coefficient value can be obtained by measuring and calculating A, A', C and C', respectively, and calculating the measured values ​​of A, A', C and C' according to the following formula 3.

[0047] [Formula 3]

[0048] Third stress coefficient = A / C + A' / C'

[0049] If the third stress coefficient value of the copper foil 110 is less than 3.5, a stress difference may occur between the MD direction and the TD direction when the copper foil 110 is stretched by 5% and 10%. As a result, wrinkles or ruptures may occur during the manufacturing process of the copper foil 110, and pinholes or curls may occur on the surface of the copper foil 110. This may result in a decrease in the charge / discharge efficiency of the negative electrode material, a decrease in workability, and an increase in the defective rate of secondary batteries.

[0050] Therefore, in order to prevent the copper foil 110 from wrinkling or bursting during the manufacturing process, the third stress coefficient value of the copper foil 110 needs to be 3.5 or more.

[0051] The copper foil 110 according to an embodiment of the present invention has a thickness of 4 to 35 μm. When the copper foil 110 is used as a current collector of an electrode in a secondary battery, the thinner the thickness of the copper foil 110, the more current collectors can be accommodated in the same space, which is advantageous for increasing the capacity of the secondary battery. However, manufacturing a copper foil 110 having a thickness of less than 4 μm causes a decrease in workability.

[0052] On the other hand, when a secondary battery is manufactured using a copper foil 110 having a thickness exceeding 35 μm, it becomes difficult to realize a high capacity due to the thick copper foil 110 .

[0053] The copper foil 110 according to the embodiment of the present invention has a thickness of 45 kg / mm 2 In order to prevent the copper foil 110 from wrinkling and bursting, the copper foil 110 of the present invention has a tensile strength of 45 kg / mm 2 The copper foil 110 has a high tensile strength of 45 kg / mm 2If it is less than this, folding of the copper foil 110 between two adjacent rolls may occur during the roll-to-roll manufacturing process, or wrinkles may occur at the left and right ends of the copper foil 110 during the roll-to-roll manufacturing process.

[0054] The copper foil 110 according to an embodiment of the present invention may have an elongation rate of 3 to 13%.

[0055] If the elongation rate of the copper foil 110 is less than 3%, when the copper foil 110 is used as a current collector of a secondary battery, the copper foil 110 does not elongate sufficiently to accommodate the large volume expansion of the high capacity active material, and there is a high risk of the copper foil 110 bursting.

[0056] On the other hand, if the elongation rate of the copper foil 110 exceeds 13%, the copper foil 110 may easily elongate during the process of manufacturing an electrode for a secondary battery, causing deformation of the electrode.

[0057] According to an embodiment of the present invention, the copper foil 110 may have a 10-point average roughness (Rz) of 0.7 to 0.9 μm.

[0058] As the secondary battery is repeatedly charged and discharged, the active material layer alternately contracts and expands, which induces separation between the active material layer and the copper foil 110, reducing the charge and discharge efficiency of the secondary battery. Therefore, in order for the secondary electrode to ensure a certain level of capacity retention and lifespan (i.e., to prevent a decrease in the charge and discharge efficiency of the secondary battery), the copper foil 110 must have excellent coating properties for the active material, so that the adhesive strength between the copper foil 110 and the active material layer must be high.

[0059] Specifically, the smaller the ten-point average roughness (Rz) of the copper foil 110, the more the charge / discharge efficiency of a secondary battery including the copper foil 110 tends to decrease. Therefore, according to one embodiment of the present invention, the copper foil 110 has a ten-point average roughness (Rz) of 0.7 to 0.9 μm.

[0060] If the ten-point average roughness (Rz) of the copper foil 110 is less than 0.7, the active material is easily detached from the copper foil 110 due to the relatively small surface area of ​​the copper foil 110, resulting in a rapid decrease in the lifespan of the secondary battery due to repeated charging and discharging.

[0061] On the other hand, if the 10-point average roughness (Rz) of the copper foil 110 exceeds 0.9, the contact uniformity between the copper foil 110 and the active material layer does not reach a certain level, resulting in the existence of numerous spaces between the copper foil 110 and the active material layer (i.e., the coating itself is not partially completed), which results in a rapid decrease in the lifespan of the secondary battery due to repeated charging and discharging.

[0062] In the following, the electrode 100 including the copper foil 110 of the present invention and the secondary battery including this electrode 100 will be specifically described.

[0063] FIG. 3 is a cross-sectional view of an electrode for a secondary battery according to one embodiment of the present invention.

[0064] As illustrated in FIG. 3, a secondary battery electrode 100 according to an embodiment of the present invention includes a copper foil 110 and an active material layer 120 according to any one of the above-described embodiments of the present invention.

[0065] 3 illustrates a configuration in which the active material layer 120 is formed on one side of the copper foil 110. However, the embodiment of the present invention is not limited thereto, and referring to FIG. 4, the active material layer 120 may be formed on both sides of the copper foil 110.

[0066] In lithium secondary batteries, aluminum foil is generally used as a positive electrode current collector combined with a positive electrode active material, and copper foil 110 is generally used as a negative electrode current collector combined with a negative electrode active material.

[0067] According to an embodiment of the present invention, the secondary battery electrode 100 is a negative electrode, the copper foil 110 is used as a negative electrode current collector, and the active material layer 120 includes a negative electrode active material.

[0068] In order to ensure a high capacity of the secondary battery, the active material layer 120 of the present invention may be formed of a composite of carbon and metal, for example, the metal may include at least one of Si, Ge, Sn, Li, Zn, Mg, Cd, Ce, Ni, and Fe, preferably Si and / or Sn.

[0069] FIG. 5 is a schematic cross-sectional view of a secondary battery according to an embodiment of the present invention.

[0070] 5, the secondary battery includes a cathode 370, an anode 340, an electrolyte 350 disposed between the cathode 370 and the anode 340 to provide an environment in which ions can move, and a separator 360 to electrically insulate the cathode 370 and the anode 340. Here, the ions that move between the cathode 370 and the anode 340 are, for example, lithium ions. The separator 360 separates the cathode 370 and the anode 340 to prevent charges generated at one electrode from moving to another electrode through the inside of the secondary battery 105 and being wasted. Referring to FIG. 5, the separator 360 is disposed in the electrolyte 350.

[0071] The positive electrode 370 includes a positive electrode current collector 371 and a positive electrode active material layer 372, and the positive electrode current collector 371 may be aluminum foil.

[0072] The negative electrode 340 includes a negative electrode current collector 341 and a negative electrode active material layer 342 , and the negative electrode current collector 341 may be made of copper foil 110 .

[0073] According to an embodiment of the present invention, the copper foil 110 shown in FIG. 1 or 2 may be used as the negative electrode current collector 341. Also, the secondary battery electrode 100 shown in FIG. 3 or 4 may be used as the negative electrode 340 of the secondary battery shown in FIG. 5.

[0074] Hereinafter, the method for producing the copper foil 110 of the present invention will be described in detail with reference to FIG.

[0075] The method for manufacturing the copper foil 110 of the present invention includes the steps of forming a copper film 111 and forming a protective layer 112 on the copper film 111 .

[0076] The method of the present invention includes a step of forming a copper film 111 on a rotating cathode drum 40 by passing an electric current through an anode plate 30 and a rotating cathode drum 40 that are spaced apart from each other in an electrolyte 20 in an electrolytic cell 10 .

[0077] As illustrated in FIG. 6, the anode plate 30 can include first and second anode plates 31, 32 that are electrically insulated from one another.

[0078] The copper film 111 formation step can be carried out by forming a seed layer by passing an electric current between the first anode plate 31 and the rotating cathode drum 40, and then growing the seed layer by passing an electric current between the second anode plate 32 and the rotating cathode drum 40.

[0079] The current density provided by the first and second anode plates 31, 32, respectively, may be 30-130 ASD.

[0080] When the current density provided by each of the first and second anode plates 31, 32 is less than 30 ASD, the surface roughness of the copper foil 110 is low, so that the adhesion between the copper foil 110 and the active material layer 120 may be insufficient.

[0081] On the other hand, if the current density provided by each of the first and second anode plates 31 and 32 exceeds 130ASD, the surface of the copper foil 110 is rough, so that the coating of the active material may not be performed smoothly.

[0082] The surface characteristics of the copper film 111 may vary depending on the degree of buffing or polishing of the surface of the rotating cathode drum 40. For example, the surface of the rotating cathode drum 40 may be polished with an abrasive brush having a grit size of #800 to #3000.

[0083] In the process of forming the copper film 111, the electrolyte 20 is maintained at a temperature of 48 to 60° C. More specifically, the temperature of the electrolyte 20 may be maintained at 50° C. or higher. At this time, the physical, chemical, and electrical properties of the copper film 111 may be controlled by adjusting the composition of the electrolyte 20.

[0084] According to one embodiment of the present invention, the electrolyte 20 contains 70-100 g / L of copper ions, 70-150 g / L of sulfuric acid, 15-25 ppm of chlorine (Cl), 15-150 ppm of nickel (Ni), 1-20 ppm of lead ions (Pb 2+ ), 1-10ml / L hydrogen peroxide (H2O2), 0.3-5ppm tungsten (W) and organic additives.

[0085] In order to facilitate the formation of copper film 111 by electrodeposition of copper, the concentration of copper ions and the concentration of sulfuric acid in electrolytic solution 20 are adjusted to 70 to 100 g / L and 70 to 150 g / L, respectively.

[0086] In one embodiment of the present invention, chlorine (Cl) is a chloride ion (Cl - ) and all chlorine atoms present in the molecule. Chlorine (Cl) can be used to remove silver (Ag) ions that flow into the electrolyte 20 during the process of forming the copper film 111. Specifically, chlorine (Cl) can precipitate silver (Ag) ions in the form of silver chloride (AgCl). Such silver chloride (AgCl) can be removed by filtration.

[0087] If the chlorine (Cl) concentration is less than 15 ppm, silver (Ag) ions are not removed smoothly. On the other hand, if the chlorine (Cl) concentration exceeds 25 ppm, unnecessary reactions may occur due to the excess chlorine (Cl). Therefore, the chlorine (Cl) concentration in the electrolyte 20 is controlled within the range of 15 to 25 ppm.

[0088] According to an embodiment of the present invention, the electrolyte 20 containing the organic additive may further contain hydrogen peroxide (H2O2). The electrolyte 20 to be continuously plated contains organic impurities due to the organic additive, and the organic impurities are decomposed by treating with hydrogen peroxide (H2O2), so that the carbon (C) content inside the copper foil can be appropriately adjusted. The higher the TOC concentration in the electrolyte 20, the more carbon (C) elements flow into the copper film 111, and therefore the total amount of elements released from the copper film 111 during heat treatment can increase. As a result, it may not be possible to obtain the first stress coefficient, the second stress coefficient, and the third stress coefficient values ​​that are desired to be obtained, and as a result, wrinkles or ruptures may occur, and pinholes or curls may occur on the surface of the copper foil 110.

[0089] The amount of hydrogen peroxide (H2O2) to be added is 1 to 10 ml per L of electrolyte. Specifically, it is preferable to add 2 to 8 ml of hydrogen peroxide (H2O2) per L of electrolyte. If the amount of hydrogen peroxide (H2O2) added is less than 1 ml / L, the organic impurity decomposition effect is almost zero, and the amount of carbon (C) element flowing into the copper film 111 increases, so that the amount of all elements released from the copper film 111 during heat treatment may increase. As a result, it may not be possible to obtain the first stress coefficient, the second stress coefficient, and the third stress coefficient values ​​that are desired to be obtained, and as a result, wrinkles or ruptures may occur, and pinholes or curls may occur on the surface of the copper foil 110.

[0090] If the amount of hydrogen peroxide (H2O2) added exceeds 10ml / L, organic impurities will be decomposed excessively, and the effects of organic additives such as brighteners, retarders and leveling agents will also be suppressed.

[0091] According to an embodiment of the present invention, the electrolyte 20 including the organic additive may further include tungsten (W). When the electrolyte 20 is treated with tungsten (W), the average size of the crystalline particles included in the copper film 111 may become smaller, and the strength of the copper foil 110 may become higher. The concentration of tungsten (W) in the electrolyte 20 may be 0.3 to 5 ppm. Specifically, it is preferable to add 1 to 4 ppm of tungsten (W).

[0092] If the amount of tungsten (W) added is less than 0.3 ppm, the size of the crystalline average grains of the copper film 111 is not sufficiently small, resulting in a decrease in the strength of the copper foil 110. In addition, the size of the crystalline average grains of the copper film 111 becomes non-uniform, and the first stress coefficient, the second stress coefficient, and the third stress coefficient values ​​that are desired to be obtained may not be obtained. As a result, wrinkles or ruptures may occur, and pinholes or curls may occur on the surface of the copper foil 110.

[0093] On the other hand, if the amount of tungsten (W) added exceeds 5 ppm, the amount of impurities increases, which may suppress the effect of the organic additive. In addition, the excessive amount of impurities may cause a sudden change in the stress value of the copper foil 110. As a result, it may not be possible to obtain the first stress coefficient, the second stress coefficient, and the third stress coefficient values ​​that are desired, which may result in wrinkles or ruptures, and pinholes or curls on the surface of the copper foil 110.

[0094] According to one embodiment of the present invention, the electrolyte 20 containing the organic additive contains 1 to 20 ppm of lead ions (Pb 2+ ) may further be included. 2+ ) is controlled at a concentration of 1 to 20 ppm. 2+ In order to maintain the concentration of lead (Pb), the raw materials added to the electrolyte 20 may be materials that do not contain lead (Pb).

[0095] Lead ion (Pb 2+If the concentration of is less than 1 ppm, the effect of maintaining the physical properties of the present invention may be reduced, and as a result, the first stress coefficient, the second stress coefficient, and the third stress coefficient values ​​that are desired to be obtained may not be obtained, which may result in wrinkles or ruptures, and pinholes or curls on the surface of the copper foil 110.

[0096] Lead ion (Pb 2+ If the concentration of lead ions (Pb) exceeds 20 ppm, an ion exchange filter should be used to remove the lead ions (Pb 2+ ) must be removed from the electrolyte 20, and copper may be unevenly deposited, causing wrinkles or ruptures, and pinholes or curls may occur on the surface of the copper foil 110. In addition, uneven deposition of copper may cause a sudden change in the stress value of the copper foil 110. As a result, it may not be possible to obtain the first stress coefficient, the second stress coefficient, and the third stress coefficient values ​​that are desired, and as a result, wrinkles or ruptures may occur, and pinholes or curls may occur on the surface of the copper foil 110.

[0097] According to an embodiment of the present invention, the electrolyte 20 containing the organic additive may further contain nickel (Ni) in the range of 15 to 150 ppm. The nickel (Ni) in the electrolyte 20 is controlled at a concentration in the range of 15 to 150 ppm.

[0098] If the concentration of nickel (Ni) exceeds 150 ppm, the strength of the copper foil 110 decreases, making it difficult to manufacture a high-strength copper foil 110. In addition, a sudden change in the stress value of the copper foil 110 may occur. As a result, it may not be possible to obtain the first stress coefficient, the second stress coefficient, and the third stress coefficient values ​​that are desired, which may result in wrinkles or ruptures, and pinholes or curls on the surface of the copper foil 110.

[0099] On the other hand, if the concentration of nickel (Ni) is less than 15 ppm, the surface roughness of the copper foil 110 may increase excessively, the strength may decrease, and curls may occur on the surface of the copper foil 110. In addition, a sudden change may occur in the stress value of the copper foil 110. As a result, it may not be possible to obtain the first stress coefficient, the second stress coefficient, and the third stress coefficient values ​​that are desired, and as a result, wrinkles or ruptures may occur, and pinholes or curls may occur on the surface of the copper foil 110.

[0100] The organic additives contained in the electrolyte 20 include at least one of a brightener (component A), a moderator (component B), a leveling agent (component C), and a relaxation agent (component D). The organic additives in the electrolyte 20 have a concentration of 1 to 100 ppm.

[0101] The organic additive may include two or more of the brightener (component A), the moderator (component B), the leveling agent (component C) and the mitigating agent (component D), or may include all four components. Even in such a case, the concentration of the organic additive is 100 ppm or less. When the organic additive includes all of the brightener (component A), the moderator (component B), the leveling agent (component C) and the mitigating agent (component D), the organic additive may have a concentration of 10 to 100 ppm.

[0102] The brightener (component A) contains sulfonic acid or a metal salt thereof. The brightener (component A) may have a concentration of 1 to 25 ppm in the electrolyte 20.

[0103] The brightener (component A) increases the charge of the electrolyte 20 to increase the electrodeposition speed of copper, improves the curling property of the copper foil, and enhances the gloss of the copper foil 110. If the concentration of the brightener (component A) is less than 1 ppm, the gloss of the copper foil 110 decreases, and if it exceeds 25 ppm, wrinkles or ruptures may occur in the copper foil 110, pinholes or curls may occur on the surface of the copper foil 110, and a sudden change may occur in the stress value of the copper foil 110. As a result, it may not be possible to obtain the first stress coefficient, the second stress coefficient, and the third stress coefficient values ​​that are desired to be obtained, and as a result, wrinkles or ruptures may occur, and pinholes or curls may occur on the surface of the copper foil 110.

[0104] More specifically, the brightener (component A) may have a concentration in the electrolyte 20 of 5 to 20 ppm.

[0105] The brightener may include, for example, at least one of bis-(3-sulfopropyl)-disulfide disodium salt, 3-mercapto-1-propanesulfonic acid, 3-(N,N-dimethylthiocarbamoyl)-thiopropanesulfonate sodium salt, 3-[(amino-iminomethyl)thio]-1-propanesulfonate sodium salt, o-ethyldithiocarbonate-S-(3-sulfopropyl)-ester sodium salt, 3-(benzothiazolyl-2-mercapto)-propyl-sulfonic acid sodium salt, and ethylenedithiodipropylsulfonic acid sodium salt.

[0106] The moderator (component B) includes a non-ionic water-soluble polymer. The moderator (component B) may have a concentration of 1 to 15 ppm in the electrolyte 20.

[0107] The moderator (component B) reduces the rate of copper electrodeposition to prevent a rapid increase in roughness and a decrease in strength of the copper foil 110. Such a moderator (component B) is also called a suppressor.

[0108] If the concentration of the moderator (B component) is less than 1 ppm, the roughness of the copper foil 110 increases rapidly, and a problem of a decrease in the strength of the copper foil 110 may occur. In addition, wrinkles or ruptures may occur in the copper foil 110, and pinholes or curls may occur on the surface of the copper foil 110. In addition, a sudden change may occur in the stress value of the copper foil 110. As a result, it may not be possible to obtain the first stress coefficient, the second stress coefficient, and the third stress coefficient values ​​that are desired, and as a result, wrinkles or ruptures may occur, and pinholes or curls may occur on the surface of the copper foil 110.

[0109] On the other hand, even if the concentration of the moderator (component B) exceeds 15 ppm, there is almost no change in the physical properties such as the appearance, gloss, roughness, strength, and elongation rate of the copper foil 110. Therefore, it is possible to adjust the concentration of the moderator (component B) to the range of 1 to 10 ppm without increasing the concentration of the moderator (component B) unnecessarily, thereby increasing the manufacturing cost and wasting raw materials.

[0110] The moderator (B component) may include at least one non-ionic water-soluble polymer selected from, for example, polyethylene glycol (PEG), polypropylene glycol, polyethylene polypropylene copolymer, polyglycerin, polyethylene glycol dimethyl ether, hydroxyethylene cellulose, polyvinyl alcohol, stearic acid polyglycol ether, and stearyl alcohol polyglycol ether. However, the type of moderator is not limited thereto, and other non-ionic water-soluble polymers that can be used in the manufacture of the high strength copper foil 110 may be used as the moderator.

[0111] The leveling agent (component C) contains at least one of nitrogen (N) and sulfur (S). That is, the leveling agent (component C) can contain one or more nitrogen atoms (N) or one or more sulfur atoms (S) in one molecule, or may contain one or more nitrogen atoms (N) and one or more sulfur atoms (S). For example, the leveling agent (component C) is an organic compound containing at least one of nitrogen (N) and sulfur (S).

[0112] The leveling agent (component C) prevents excessively high peaks or excessively large protrusions from being generated in the copper film 111, thereby making the copper film 111 macroscopically flat. The leveling agent (component C) may have a concentration of 1 to 15 ppm in the electrolyte 11.

[0113] If the concentration of the leveling agent (component C) is less than 1 ppm, the strength of the copper foil 110 decreases, making it difficult to manufacture a high-strength copper foil 110. In addition, the stress value of the copper foil 110 may fluctuate rapidly. As a result, it may not be possible to obtain the first stress coefficient, the second stress coefficient, and the third stress coefficient values ​​that are desired, which may result in wrinkles or ruptures, and pinholes or curls on the surface of the copper foil 110.

[0114] On the other hand, if the concentration of the leveling agent (component C) exceeds 15 ppm, the surface roughness of the copper foil 110 may increase excessively, reducing the strength, and pinholes or curls may occur on the surface of the copper foil 110, making it difficult to separate the copper foil 110 from the winder (WR) after manufacturing. Also, if the concentration of the leveling agent (component C) exceeds 15 ppm, a sudden change may occur in the stress value of the copper foil 110. As a result, it may not be possible to obtain the first stress coefficient, second stress coefficient, and third stress coefficient values ​​that are desired.

[0115] Examples of the leveling agent (component C) include diethylthiourea, ethylenethiourea, acetylenethiourea, dipropylthiourea, dibutylthiourea, N-trifluoroacetylthiourea, N-ethylthiourea, N-cyanoacetylthiourea, N-allylthiourea, o-tolylthiourea, N,N'-butylenethiourea, and the like. thiourea, thiazolidinethiol, 4-thiazolinethiol, 4-methyl-2-pyrimidinethiol, 2-thiouracil, 3-(benzotriazole-2-mercapto)-propanesulfonic acid, 2-mercaptopyridine, 3(5-mercapto-1H-tetrazole)benzenesulfonate, 2-mercaptobenzothiazole, dimethylpyridine, 2,2'-bipyridine, 4,4'-bipyridine, pyrimidine, pyridazine, pyrimidine, pyrino The compound may include at least one of phosphorus, oxazole, thiazole, 1-methylimidazole, 1-benzylimidazole, 1-methyl-2-methylimidazole, 1-benzyl-2-methylimidazole, 1-ethyl-4-methylimidazole, 1-ethyl-2-ethyl-4-methylol, N-methylpyrrole, N-ethylpyrrole, N-butylpyrrole, N-methylpyrroline, N-ethylpyrrole, N-butylpyrroline, N-methylpyrroline, N-ethylpyrroline, N-butylpyrroline, pyrimidine, purine, quinoline, isoquinoline, N-methylcarbazole, N-ethylcarbazole, and N-butylcarbazole.

[0116] The buffer (component D) may include citric acid (CA). Specifically, the electrolyte 20 may include 1 to 5 ppm of citric acid (CA).

[0117] If the concentration of citric acid (CA) in the electrolyte 20 exceeds 5 ppm, the surface roughness of the copper foil 110 may increase excessively, resulting in a decrease in strength and curling of the surface of the copper foil 110. In addition, a sudden change in the stress value of the copper foil 110 may occur. As a result, it may not be possible to obtain the first stress coefficient, the second stress coefficient, and the third stress coefficient values ​​that are desired.

[0118] On the other hand, if the concentration of citric acid (CA) in the electrolyte 20 is less than 1 ppm, the strength of the copper foil 110 decreases, making it difficult to manufacture a high-strength copper foil 110. In addition, a sudden change in the stress value of the copper foil 110 may occur. As a result, it may not be possible to obtain the first stress coefficient, the second stress coefficient, and the third stress coefficient values ​​that are desired, which may cause wrinkles or ruptures, and pinholes or curls on the surface of the copper foil 110.

[0119] When the copper film 111 is formed, the flow rate of the electrolyte 20 supplied to the electrolytic cell 10 is 41 to 45 m 3 / hour.

[0120] The step of forming the copper film 111 may include at least one of a step of filtering the electrolyte 20 using activated carbon, a step of filtering the electrolyte 20 using diatomaceous earth, and a step of treating the electrolyte 20 with ozone (O3).

[0121] Specifically, for filtration of the electrolyte 20, the electrolyte 20 is 35 to 45 m 3 That is, during the electroplating for forming the copper film 111, the electrolyte 20 may be circulated at a flow rate of 35 to 45 m3 / hour to remove solid impurities present in the electrolyte 20. 3 Filtration may be performed at a flow rate of 1000 ml / hour. Activated carbon or diatomaceous earth may be used.

[0122] To maintain the cleanliness of the electrolyte 20, the electrolyte 20 may be treated with ozone (O3).

[0123] In addition, to ensure the cleanliness of the electrolyte 20, the copper wire from which the electrolyte 20 is made may be washed.

[0124] According to one embodiment of the present invention, the step of preparing the electrolyte 20 may include the steps of heat treating a copper wire, pickling the heat-treated copper wire, rinsing the pickled copper wire with water, and introducing the rinsed copper wire into sulfuric acid for the electrolyte.

[0125] More specifically, in order to maintain the cleanliness of the electrolyte 20, a high-purity (99.9% or more) copper wire is heat-treated in an electric furnace at 750°C to 850°C to burn off various organic impurities adhering to the copper wire, and the heat-treated copper wire is pickled using a 10% sulfuric acid solution for 10 to 20 minutes, and the pickled copper wire is washed using distilled water, thereby producing copper for producing the electrolyte 20. The washed copper wire can be put into sulfuric acid for the electrolyte to produce the electrolyte 20.

[0126] According to an embodiment of the present invention, the concentration of total organic carbon (TOC) in the electrolyte 20 is controlled to be 50 ppm or less in order to satisfy the characteristics of the copper foil 110. That is, the electrolyte 20 may have a total organic carbon (TOC) concentration of 50 ppm or less.

[0127] The copper film 111 thus produced can be cleaned in a cleaning bath.

[0128] For example, acid cleaning for removing impurities, such as resin components or natural oxide, on the surface of the copper film 111 and water cleaning for removing the acid solution used in the acid cleaning may be performed in sequence. The cleaning process may be omitted.

[0129] Next, a protective layer 112 is formed on the copper film 111 .

[0130] 6, the method may further include the step of immersing the copper film 111 in an anticorrosion solution 60. When the copper film 111 is immersed in the anticorrosion solution 60, the copper film 111 may be guided by a guide roll disposed in the anticorrosion solution 60.

[0131] As described above, the anticorrosive solution 60 may include at least one of a chromium compound, a silane compound, and a nitrogen compound. For example, the copper film 111 may be immersed in a 1 to 10 g / L potassium dichromate solution at room temperature for 1 to 30 seconds.

[0132] On the other hand, the protective layer 112 may contain a silane compound obtained by silane treatment, or may contain a nitrogen compound obtained by nitrogen treatment.

[0133] By forming the protective layer 112 in this manner, the copper foil 110 is produced.

[0134] The electrode for a secondary battery (i.e., anode) of the present invention may be manufactured by coating one or both sides of the copper foil 110 of the present invention manufactured by the above-mentioned method with one or more negative electrode active materials selected from the group consisting of carbon; metal (Me) of Si, Ge, Sn, Li, Zn, Mg, Cd, Ce, Ni or Fe; alloys containing the metal (Me); oxides (MeOx) of the metal (Me); and composites of the metal (Me) and carbon.

[0135] For example, 100 parts by weight of carbon for the negative electrode active material is mixed with 1 to 3 parts by weight of styrene butadiene rubber (SBR) and 1 to 3 parts by weight of carboxymethyl cellulose (CMC), and then a slurry is prepared using distilled water as a solvent. The slurry is then applied to the copper foil 110 in a thickness of 20 to 60 μm using a doctor blade, and is heated at 110 to 130° C. with a pressure of 0.5 to 1.5 ton / cm. 2 Press with a pressure of .

[0136] A secondary battery can be manufactured by using the secondary battery electrode (negative electrode) of the present invention manufactured by the above method together with a normal positive electrode, electrolyte, and separator.

[0137] The present invention will be described in detail below through examples and comparative examples. However, the following examples are merely intended to aid in understanding the present invention, and the scope of the present invention is not limited to these examples.

[0138] Examples 1-5 and Comparative Examples 1-4

[0139] Copper foil was produced using a foil-making machine including an electrolytic cell 10, a rotating cathode drum 40 disposed in the electrolytic cell 10, and an anode plate 30 disposed at a distance from the rotating cathode drum 40. The electrolyte 20 was a copper sulfate solution. The concentration of copper ions in the electrolyte 20 was set to 87 g / L, the concentration of sulfuric acid to 110 g / L, the temperature of the electrolyte to 55° C., and the current density to 60 ASD.

[0140] The concentrations of chlorine (Cl), nickel (Ni), lead (Pb), hydrogen peroxide, tungsten (W) and organic additives contained in the electrolyte 20 are as shown in Table 1 below.

[0141] Among the organic additives, bis-(3-sulfopropyl)-disulfide disodium salt (SPS) was used as a brightener (component A), polyethylene glycol (PEG) was used as a retarder (component B), and ethylenethiourea (ETU) was used as a leveling agent (component C).

[0142] A current was applied between the rotating cathode drum 40 and the anode plate 30 at a current density of 60 ASD to produce a copper film 111. Next, the copper film 111 was immersed in an anti-rust solution for about 2 seconds to perform a chromate treatment on the surface of the copper film 111 to form a protective layer 112, thereby producing a copper foil 110. An anti-rust solution containing chromic acid as a main component was used as the anti-rust solution, and the concentration of chromic acid was 5 g / L.

[0143] As a result, copper foils of Examples 1-5 and Comparative Examples 1-4 were produced.

[0144] [Table 1]

[0145] [Table 2]

[0146] The copper foils of Examples 1-5 and Comparative Examples 1-4 thus manufactured were checked for i) A, A', B, B', C and C', ii) the first stress coefficient, iii) the second stress coefficient, 4) the third stress coefficient and v) the occurrence of wrinkles / bursts.

[0147] i) A, A', B, B', C and C' measurements

[0148] A is the stress when the copper foil is elongated by 50% in the MD direction, A' is the stress when the copper foil is elongated by 50% in the TD direction, B is the stress when the copper foil is elongated by 10% in the MD direction, B' is the stress when the copper foil is elongated by 10% in the TD direction, C is the stress when the copper foil is elongated by 5% in the MD direction, and C' is the stress when the copper foil is elongated by 5% in the TD direction.

[0149] A, A', B, B', C and C' are measured by a universal testing machine (UTM, Instron) according to the IPC-TM-650 Test Method Manual. The sample width is 12.7 mm, the grip distance is 50 mm, and the measurement speed is 50 mm / min.

[0150] For A, the copper foil was measured after being raised 50% in the MD direction under the above conditions, for A', the copper foil was measured after being raised 50% in the TD direction under the above conditions, for B, the copper foil was measured after being raised 10% in the MD direction under the above conditions, for B', the copper foil was measured after being raised 10% in the TD direction, for C, the copper foil was measured after being raised 5% in the MD direction under the above conditions, and for C', the copper foil was measured after being raised 5% in the TD direction under the above conditions.

[0151] ii) First stress coefficient calculation

[0152] The first stress coefficient value can be obtained by calculating the measured i) A, A', B, B', C and C' values ​​according to the following formula 1.

[0153] [Formula 1]

[0154] First stress coefficient = A / A' + B / B' + C / C'

[0155] iii) Second stress coefficient calculation

[0156] The second stress coefficient value can be obtained by calculating the measured i) A, A', B and B' values ​​according to the following formula 2.

[0157] [Formula 2]

[0158] Second stress coefficient = A / B + A' / B'

[0159] 4) 3rd stress coefficient calculation

[0160] The third stress coefficient value can be obtained by calculating the measured i) A, A', C and C' values ​​according to the following formula 3.

[0161] [Formula 3]

[0162] Third stress coefficient = A / C + A' / C'

[0163] v) Presence or absence of wrinkles / bursts

[0164] After 100 charge / discharge cycles, the secondary battery was disassembled and observed for wrinkles or ruptures in the copper foil. If wrinkles or ruptures occurred in the copper foil, it was marked as "occurred" and if not, it was marked as "none."

[0165] Referring to Tables 1 and 2, the following results can be seen.

[0166] The copper foil of Comparative Example 1, which was manufactured using an electrolyte containing an excessive amount of brightener (component A) and trace amounts of nickel, lead, and tungsten, experienced rupture / wrinkling.

[0167] The copper foil of Comparative Example 2, which was manufactured using an electrolyte containing an excessive amount of moderator (component B) and trace amounts of lead and hydrogen peroxide, experienced rupture / wrinkling.

[0168] The copper foil of Comparative Example 3, which was produced using an electrolyte containing an excessive amount of a leveling agent (component C), hydrogen peroxide, and tungsten, experienced rupture / wrinkling.

[0169] The copper foil of Comparative Example 4, which was manufactured using an electrolyte containing excess amounts of the relaxation agent (component D), nickel, and lead, experienced bursting / wrinkling.

[0170] In contrast, the copper foils of Examples 1 to 5 according to the present invention all satisfied the numerical values ​​within the standards, and as a result, no ruptures or wrinkles occurred.

[0171] The present invention described above is not limited to the above-mentioned embodiments and the attached drawings, and various substitutions, modifications and changes are possible within the scope of the technical subject of the present invention, which will be apparent to those skilled in the art to which the present invention pertains. Therefore, the scope of the present invention is expressed by the following claims, and all modifications or alterations derived from the meaning, scope and equivalent concept of the claims should be interpreted as being included in the scope of the present invention. [Explanation of symbols]

[0172] 100: Electrode for secondary batteries 110: Copper foil 111: Copper film 120: Active material layer 10: Electrolytic cell 20: Electrolyte

Claims

1. A copper film containing 99.9% by weight or more of copper; having a first stress coefficient of 2.8 or greater; A second stress coefficient of 2.5 or greater; A copper foil having a third stress factor of 3.5 or greater, comprising: The first stress coefficient is calculated by the following Equation 1: [Formula 1] First stress coefficient=A / A'+B / B'+C / C' The second stress coefficient is calculated by the following Equation 2: [Formula 2] Second stress coefficient=A / B+A' / B' The third stress coefficient is calculated by the following Equation 3: [Formula 3] Third stress coefficient=A / C+A' / C' In [Equation 1] to [Equation 3], A is the stress at 50% elongation in the MD direction, In [Equation 1] to [Equation 3], A' is the stress at 50% elongation in the TD direction, In [Equation 1] to [Equation 3], B is the stress at 10% elongation in the MD direction, In [Equation 1] to [Equation 3], B' is the stress at 10% elongation in the TD direction, In [Equation 1] to [Equation 3], C is the stress at 5% elongation in the MD direction, In [Equation 1] to [Equation 3], C' is the stress at 5% elongation in the TD direction of the copper foil.

2. The copper foil of claim 1 further comprising a protective layer on said copper film.

3. The copper foil of claim 2 , wherein the protective layer comprises at least one of a chromium compound, a silane compound, and a nitrogen compound.