Optical film containing spherical silica particles, and optical laminate
Spherical silica particles with controlled size distribution and properties address glare and haze issues in anti-glare films, improving display quality by minimizing optical defects and structural color interference.
Patent Information
- Application Number
- JP2023043152
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-17
- Publication Date
- 2024-10-01
AI Technical Summary
Existing anti-glare films cause glare and haze issues, and silica particles with specific wavelengths can intensify light, leading to structural color interference affecting display quality.
The use of spherical silica particles with a uniform particle size distribution, specifically D10, D50, and D90 ratios of 2.0 to 4.0 and D50 between 1 to 20 μm, along with controlled pore volume, surface area, and impurity levels, to minimize glare and haze.
The solution effectively suppresses glare, haze, and structural color interference, enhancing display quality by maintaining uniform light scattering and reducing optical film defects.
Smart Images

Figure 2024132406000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an optical film and an optical laminate containing spherical silica particles. [Background technology]
[0002] Displays used in personal computers, monitors, touch panels, etc. are increasingly being used in bright environments in recent years, and there is a demand for them to have sufficient brightness and viewing angle in bright environments, as well as to suppress glare caused by external light reflections from fluorescent lights and sunlight.
[0003] To address these issues, an optical laminate containing light-diffusing particles inside can be formed inside a liquid crystal cell, and the transmitted light from the backlight can be scattered to improve display quality by expanding the viewing angle. In addition, by forming an optical film with microscopic irregularities on its surface and an anti-glare film equipped with this on the display surface and inside the liquid crystal cell, the incident light can be scattered and anti-glare properties can be imparted to the display.
[0004] As prior art, for example, Patent Document 1 describes the preparation of an antiglare film having an uneven surface by adding silica-based fine particles, and Patent Document 2 describes the formation of a cured coating film by a photocurable resin composition containing spherical silica particles with a very narrow particle size distribution. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2009-251378 A [Patent Document 2] Patent No. 6822792 Summary of the Invention [Problem to be solved by the invention]
[0006] However, the antiglare film described in Patent Document 1 has a problem of being prone to glare and increasing haze. In addition, when silica particles as described in Patent Document 2 are used, light of a specific wavelength is selectively interfered with and intensified, resulting in a specific color (structural color) that affects the color of the display.
[0007] The present invention has been made in view of the above problems, and an object of the present invention is to provide an optical film and an optical laminate that suppress glare and haze. [Means for solving the problem]
[0008] The present inventors have found that the silica particles contained in the antiglare film are too large, causing glare, and the presence of small particles causes haze to worsen. They have also found that the above problems can be solved by using spherical silica particles with a uniform particle size distribution, and have completed the present invention.
[0009] The present invention relates to the following (1) to (14). (1) An optical film having a resin layer containing spherical silica particles, wherein the spherical silica particles have a D90 / D10 ratio of 2.0 to 4.0 and a D50 ratio of 1 to 20 μm, where D10, D50 and D90 are the cumulative 10%, 50% and 90% particle diameters from the smallest end in a volume-based particle size distribution, respectively. (2) The pore volume of the spherical silica particles is 0.001 to 1.0 cm 3 / g. (3) The optical film according to (1), wherein the volume ratio of particles having a particle size of 1 μm or less among the spherical silica particles is 7% or less. (4) The optical film according to (1), wherein the volume ratio of particles having a particle size of 20 μm or more among the spherical silica particles is 10% or less. (5) The BET specific surface area of the spherical silica particles is 0.3 to 800 m 2 / g. (6) The optical film according to (1), wherein the resin layer contains a cured product of a curable resin. (7) The method for producing an optical film according to any one of (1) to (6), wherein the resin layer is formed by kneading spherical silica particles and a resin. (8) An optical laminate having a resin layer containing spherical silica particles, wherein the spherical silica particles have a D90 / D10 ratio of 2.0 to 4.0 and a D50 ratio of 1 to 20 μm, where D10, D50 and D90 are the particle sizes of the smallest cumulative 10%, smallest cumulative 50% and smallest cumulative 90% particles in a volume-based particle size distribution. (9) The method for producing an optical laminate according to (8), further comprising kneading spherical silica particles and a resin to form a resin layer. (10) A display device comprising the optical film according to any one of (1) to (6) or the optical laminate according to (8). (11) The display device according to (10), which is a liquid crystal display device or an organic electroluminescence display device. (12) An antiglare film comprising the optical film according to any one of (1) to (6) or the optical laminate according to (8). (13) A display device comprising the antiglare film according to (12). (14) The display device according to (13), which is a liquid crystal display device or an organic electroluminescence display device. Effect of the Invention
[0010] According to the present invention, by using spherical silica particles having a uniform particle size distribution, it is possible to provide an optical film and an optical laminate in which glare and haze are suppressed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The present invention will be described below, but the present invention is not limited to the examples in the following description. In this specification, the symbol "to" indicating a numerical range means that the numerical range includes the numerical ranges before and after the symbol as the lower and upper limits. In this embodiment, the term "optical film" refers to a film having a resin layer containing spherical silica particles. In the present embodiment, the term "optical laminate" refers to a laminate having an optical functional layer which is a resin layer containing spherical silica particles.
[0012] (Spherical silica particles) The optical film of the present embodiment contains spherical silica particles, and when the spherical silica particles have particle sizes D10, D50 and D90 that are the cumulative 10%, 50% and 90% smaller particle sizes from the smallest side in a volume-based particle size distribution, respectively, D90 / D10 is 2.0 to 4.0 and D50 is 1 to 20 μm.
[0013] When the spherical silica particles have a D90 / D10 of 2.0 or more, the optical film is less likely to exhibit structural colors caused by selective interference of light of a specific wavelength, and is less likely to affect the color of the display. When the spherical silica particles have a D90 / D10 of 4.0 or less, the optical film is less likely to suffer from glare or haze deterioration. D90 / D10 is more preferably 2.0 to 3.5, and even more preferably 2.0 to 3.0.
[0014] Furthermore, when the spherical silica particles have a D50 of 1 μm or more, the haze of the optical film is less likely to deteriorate, and when the D50 is 20 μm or less, the glare of the optical film is easily suppressed. D50 is more preferably 1 to 15 μm, even more preferably 1 to 12 μm, particularly preferably 1 to 10 μm, and most preferably 1.5 to 5 μm.
[0015] D10, D50 and D90 can be calculated using a particle size distribution measuring device using an electrical detection method (e.g., Multisizer4e, manufactured by Beckman Coulter).
[0016] The spherical silica particles in this embodiment have a pore volume of 0.001 to 1.0 cm 3 / g. Here, the pore volume means the pore volume derived from pores having a pore diameter of 1 to 100 nm.3 When the ratio is 1 / g or less, the pore volume inside the spherical silica particles is appropriately adjusted, and the deterioration of haze due to this is unlikely to occur. The pore volume of a spherical silica particle is 0.5 cm 3 / g or less is more preferable, and 0.1 cm 3 / g or less is more preferable, and 0.04 cm 3 / g or less is particularly preferred.
[0017] The pore volume can be calculated by the nitrogen adsorption method using the BJH method.
[0018] In the present embodiment, the spherical silica particles preferably have a volume ratio of particles having a particle size of 1 μm or less of 7% or less, more preferably 5% or less, from the viewpoint of preventing deterioration of the haze of the optical film.
[0019] Moreover, from the viewpoint of preventing glare, the volume ratio of the spherical silica particles of this embodiment having a particle size of 20 μm or more is preferably 10% or less, and more preferably 5% or less.
[0020] The volume fraction of particles with a particle size of 1 μm or less and the volume fraction of particles with a particle size of 20 μm or more can be calculated using a particle size distribution measuring device using an electrical detection method (e.g., Multisizer4e, manufactured by Beckman Coulter, Inc.).
[0021] The spherical silica particles in this embodiment have a BET specific surface area of 0.3 to 800 m as determined by a nitrogen adsorption method. 2 / g. The BET specific surface area is preferably 800 m 2 When the refractive index is 1.0 to 1.5 μm, scattering between different phases in the optical film can be suppressed, and glare can be suppressed. The specific surface area of spherical silica particles is 500m 2 / g or less is more preferable, and 2 From the viewpoint of ensuring the adhesion between the optical film and the optical laminate, the BET specific surface area is preferably 0.3 m 2 / g or more, and 0.5m 2 / g or more is more preferable, and 1.0m 2 / g or more is most preferred.
[0022] The BET specific surface area can be calculated using the BET theory after obtaining an adsorption isotherm by a nitrogen adsorption method.
[0023] The spherical silica particles in this embodiment refer to silica particles having a sphericity of 0.75 or more. If the sphericity is 0.75 or more, the particle shape becomes close to a sphere, so that anisotropic scattering can be suppressed. The sphericity is preferably 0.80 or more, more preferably 0.85 or more, even more preferably 0.90 or more, and particularly preferably 0.95 or more. The upper limit of the sphericity is not particularly limited, and is most preferably 1.
[0024] The sphericity is expressed as the average value of the ratio (DS / DL) of the minimum diameter (DS) to the maximum diameter (DL) of 100 random particles in a photographic projection obtained by photographing with a scanning electron microscope (SEM).
[0025] The spherical silica particles in this embodiment may contain sodium at a concentration of 1 to 300 ppm by mass. By containing sodium in the above range, it is possible to perform calcination at high temperatures while suppressing crystallization. The sodium concentration is preferably 2 ppm by mass or more, more preferably 3 ppm by mass or more, and even more preferably 10 ppm by mass or more. The sodium concentration is preferably 200 ppm by mass or less, more preferably less than 200 ppm by mass, even more preferably 150 ppm by mass or less, particularly preferably 100 ppm by mass or less, and most preferably 50 ppm by mass or less.
[0026] The spherical silica particles in this embodiment may contain impurity elements other than sodium, as long as the effects of the present invention are not impaired. Examples of other impurity elements include Mg, Ca, Al, Fe, and Ti. The concentration of each of the other impurity elements is preferably 500 ppm by mass or less, more preferably 300 ppm by mass or less, and even more preferably 100 ppm by mass or less.
[0027] The concentrations of sodium and other impurity elements can be measured by inductively coupled plasma (ICP) emission spectrometry after adding perchloric acid and hydrofluoric acid to spherical silica particles and igniting them to remove the main component silicon.
[0028] The spherical silica particles in this embodiment may be obtained by manufacturing, or may be commercially available. For example, the manufacturing method of spherical silica particles may be a wet method or a granulation method. Among them, from the viewpoint of obtaining spherical silica particles with a small specific surface area and a moderately narrow particle size distribution, the silica particles manufactured by the wet method are preferred.
[0029] The wet method refers to a method that includes a process of using a liquid silica source and gelling it to obtain raw material for silica particles. By using the wet method, it is easy to adjust the shape of the silica particles. In particular, it is easy to prepare spherical silica particles, and there is no need to adjust the shape of the particles by crushing, etc., and as a result, it is easy to obtain particles with a small specific surface area. In addition, the wet method is difficult to produce particles that are significantly smaller than the average particle size, and the specific surface area tends to be small after firing. In addition, in the wet method, the amount of impurity elements such as titanium can be adjusted by adjusting the impurities in the silica source, and the above-mentioned impurity elements can be uniformly dispersed in the particles.
[0030] Examples of the wet method include the spray method and the emulsion-gelling method. In the emulsion-gelling method, for example, a dispersed phase containing a silica precursor and a continuous phase are emulsified, and the resulting emulsion is gelled to obtain spherical silica particles. As an emulsification method, a method in which a dispersed phase containing a silica precursor is supplied to a continuous phase through a micropore or a porous membrane to produce an emulsion is preferred. This produces an emulsion with a uniform droplet size, resulting in spherical silica particles with a uniform particle size. Here, the particle size of the silica particles can be adjusted by adjusting the stirring speed during emulsification.
[0031] As such an emulsification method, a micromixer method or a membrane emulsification method can be used. For example, the micromixer method is disclosed in International Publication No. 2013 / 062105.
[0032] The spherical silica particles in this embodiment are preferably subjected to a heat treatment, which has the effect of sintering the spherical silica particles and densifying the shell.
[0033] The heat treatment means is not particularly limited, and examples thereof include heat treatment by standing, heat treatment by rotary furnace, and heat treatment by spray combustion. For heat treatment by standing, a stationary electric furnace, a roller hearth kiln, a continuous furnace classified as a tunnel furnace, and the like can be used. For heat treatment by rotary furnace, a horizontal rotary furnace (rotary kiln), a rotary tubular furnace, and the like can be used. Among these, from the viewpoint of uniformity of firing, it is preferable to perform firing by heat treatment by a continuous furnace or a rotary furnace.
[0034] The heat treatment temperature is preferably 700° C. or higher, more preferably 800° C. or higher, even more preferably 900° C. or higher, and particularly preferably 1000° C. or higher. From the viewpoint of suppressing crystallization, the heat treatment temperature is preferably 1600° C. or lower, more preferably 1500° C. or lower, and even more preferably 1400° C. or lower.
[0035] The heat treatment time may be appropriately adjusted depending on the apparatus used, but is preferably performed for, for example, 0.5 to 50 hours, and more preferably 1 to 10 hours.
[0036] The spherical silica particles in this embodiment may be surface-treated with a silane coupling agent. By treating the surfaces of the spherical silica particles with a silane coupling agent, the affinity with the resin is improved, and the dispersibility and strength of the optical film can be improved.
[0037] The conditions for the surface treatment are not particularly limited, and general surface treatment conditions may be used, and a wet treatment method or a dry treatment method may be used. From the viewpoint of performing uniform treatment, the wet treatment method is preferred.
[0038] Examples of the silane coupling agent include epoxysilane coupling agents, aminosilane coupling agents, mercaptosilane coupling agents, silane coupling agents, silane coupling agents, organosilazane compounds, etc. These may be used alone or in combination of two or more. In addition, from the viewpoint of not affecting the color of the optical film, it is preferable to use a silane coupling agent that does not have a double bond.
[0039] Specific examples of the surface treatment agent include epoxysilane coupling agents such as glycidoxypropyltrimethoxysilane, glycidoxypropyltriethoxysilane, glycidoxypropylmethyldiethoxysilane, glycidylbutyltrimethoxysilane, and (3,4-epoxycyclohexyl)ethyltrimethoxysilane; aminosilane coupling agents such as aminopropylmethoxysilane, aminopropyltriethoxysilane, N-phenylaminopropyltrimethoxysilane, and N-2(aminoethyl)aminopropyltrimethoxysilane; and mercaptosilane coupling agents such as mercaptopropyltrimethoxysilane and mercaptopropyltriethoxysilane. , silane coupling agents such as methyltrimethoxysilane, vinyltrimethoxysilane, octadecyltrimethoxysilane, phenyltrimethoxysilane, methacryloxypropyltrimethoxysilane, imidazole silane, and triazine silane, CF3(CF2)7CH2CH2Si(OCH3)3, CF3(CF2)7CH2CH2SiCl3, CF3(CF2)7CH2CH2Si(CH3)(OCH3)2, CF3(CF2)7CH2CH2Si(CH3)C12, CF3(CF2)5CH2CH2SiCl3, CF3(CF2)5CH2CH2Si(OCH3)3, CF3CH2CH2SiCl3, CF3CH2CH2Si(OCH3)3, C8F 17 SO2N(C3H7)CH2CH2CH2Si(OCH3)3, C7F 15CONHCH2CH2CH2Si(OCH3)3, C8F 17 CO2CH2CH2CH2Si(OCH3)3, C8F 17 Examples of suitable coupling agents include fluorine-containing silane coupling agents such as -O-CF(CF3)CF2-O-C3H6SiCl3 and C3F7-O-(CF(CF3)CF2-O)2-CF(CF3)CONH-(CH2)3Si(OCH3)3, and organosilazane compounds such as hexamethyldisilazane, hexaphenyldisilazane, trisilazane, cyclotrisilazane, and 1,1,3,3,5,5-hexamethylcyclotrisilazane.
[0040] The amount of the silane coupling agent used for treatment is preferably 0.01 parts by mass or more, more preferably 0.02 parts by mass or more, and even more preferably 0.10 parts by mass or more, per 100 parts by mass of the spherical silica particles, and is preferably 5 parts by mass or less, and more preferably 2 parts by mass or less.
[0041] Examples of methods for treating with a silane coupling agent include a dry method in which the silane coupling agent is sprayed onto spherical silica particles, and a wet method in which the spherical silica particles are dispersed in a solvent and then a silane coupling agent is added to cause a reaction.
[0042] The fact that the surface of the spherical silica particles has been treated with a silane coupling agent can be confirmed by detecting a peak due to a substituent of the silane coupling agent by IR. The amount of the silane coupling agent attached can be measured by the amount of carbon.
[0043] (Optical film) The optical film in this embodiment is a film having a resin layer containing spherical silica particles, and exhibits optical properties such as antiglare properties by forming irregularities on the surface due to the spherical silica particles. The spherical silica particles are the particles described above.
[0044] The resin used in the resin layer is not particularly limited, but is preferably transparent from the viewpoint of optical properties. From the viewpoint of improving mechanical strength, the resin layer preferably contains a cured product of a curable resin. Examples of the curable resin include a thermosetting resin and an ionizing radiation curable resin. That is, the resin layer preferably contains a cured product of a thermosetting resin composition or a cured product of an ionizing radiation curable resin composition, and more preferably contains a cured product of an ionizing radiation curable resin composition.
[0045] The thermosetting resin composition is a composition that contains at least a thermosetting resin, and is a resin composition that is cured by heating.
[0046] Examples of the thermosetting resin include acrylic resin, urethane resin, phenol resin, urea melamine resin, epoxy resin, unsaturated polyester resin, silicone resin, etc. In the thermosetting resin composition, a curing agent is added to the curable resin as required.
[0047] The ionizing radiation curable resin composition is a composition containing a compound having an ionizing radiation curable functional group (hereinafter, also referred to as "ionizing radiation curable compound"). Examples of the ionizing radiation curable functional group include ethylenically unsaturated bond groups such as (meth)acryloyl group, vinyl group, and allyl group, as well as epoxy group, oxetanyl group, and the like. "(meth)acryloyl" refers to acryloyl and methacryloyl in general. As the ionizing radiation curable compound, a compound having an ethylenically unsaturated bond group is preferred, a compound having two or more ethylenically unsaturated bond groups is more preferred, and among them, a polyfunctional (meth)acrylate-based compound having two or more ethylenically unsaturated bond groups is even more preferred. "(meth)acrylate" refers to a general term for acrylate and methacrylate. As the polyfunctional (meth)acrylate-based compound, either a monomer or an oligomer can be used.
[0048] Here, ionizing radiation refers to electromagnetic waves or charged particle beams that have an energy quantum capable of polymerizing or crosslinking molecules. Usually, ultraviolet rays (UV) or electron beams (EB) are used, but other types of radiation, such as electromagnetic waves such as X-rays and gamma rays, and charged particle beams such as alpha rays and ion beams, can also be used.
[0049] Among the polyfunctional (meth)acrylate compounds, examples of bifunctional (meth)acrylate monomers include ethylene glycol di(meth)acrylate, bisphenol A tetraethoxy diacrylate, bisphenol A tetrapropoxy diacrylate, and 1,6-hexanediol diacrylate. Examples of trifunctional or higher (meth)acrylate monomers include trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol tetra(meth)acrylate, and isocyanuric acid-modified tri(meth)acrylate. The (meth)acrylate monomers may have a part of the molecular skeleton modified, and those modified with ethylene oxide, propylene oxide, caprolactone, isocyanuric acid, alkyl, cyclic alkyl, aromatic, bisphenol, and the like may also be used.
[0050] In addition, examples of the polyfunctional (meth)acrylate oligomer include acrylate polymers such as urethane (meth)acrylate, epoxy (meth)acrylate, polyester (meth)acrylate, and polyether (meth)acrylate. The urethane (meth)acrylate is obtained, for example, by reacting a polyhydric alcohol and an organic diisocyanate with a hydroxy (meth)acrylate. In addition, preferred epoxy (meth)acrylates are (meth)acrylates obtained by reacting trifunctional or higher aromatic epoxy resins, alicyclic epoxy resins, aliphatic epoxy resins, etc. with (meth)acrylic acid, (meth)acrylates obtained by reacting difunctional or higher aromatic epoxy resins, alicyclic epoxy resins, aliphatic epoxy resins, etc. with polybasic acids and (meth)acrylic acid, and (meth)acrylates obtained by reacting difunctional or higher aromatic epoxy resins, alicyclic epoxy resins, aliphatic epoxy resins, etc. with phenols and (meth)acrylic acid.
[0051] In addition, for the purpose of adjusting the viscosity of the resin kneaded product, a monofunctional (meth)acrylate may be used in combination as an ionizing radiation curable compound. Examples of the monofunctional (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, and isobornyl (meth)acrylate. The above ionizing radiation curable compounds may be used alone or in combination of two or more.
[0052] When the ionizing radiation curable compound is an ultraviolet ray curable compound, the ionizing radiation curable composition preferably contains additives such as a photopolymerization initiator and a photopolymerization accelerator. The photopolymerization initiator may be one or more selected from acetophenone, benzophenone, α-hydroxyalkylphenone, Michler's ketone, benzoin, benzyl dimethyl ketal, benzoyl benzoate, α-acyloxime ester, thioxanthones, etc. The photopolymerization accelerator is capable of reducing polymerization inhibition caused by air during curing and accelerating the curing speed, and may be one or more selected from p-dimethylaminobenzoic acid isoamyl ester, p-dimethylaminobenzoic acid ethyl ester, etc.
[0053] When the resin layer contains a cured product of the ionizing radiation curable resin composition, it is preferable that the resin layer contains a thermoplastic resin in addition to the cured product of the ionizing radiation curable resin composition. By containing the thermoplastic resin, the viscosity of the resin mixture is increased, so that the spherical silica particles are less likely to sink, and the binder resin is less likely to flow down between the protrusions based on the spherical silica particles.
[0054] Examples of thermoplastic resins include polystyrene-based resins, polyolefin-based resins, acrylonitrile-butadiene-styrene (ABS) resins (including heat-resistant ABS resins), acrylonitrile-styrene (AS) resins, acrylonitrile (AN) resins, polyphenylene oxide-based resins, polycarbonate-based resins, polyacetal-based resins, acrylic-based resins, polyethylene terephthalate (PET)-based resins, polybutylene terephthalate-based resins, polysulfone-based resins, and polyphenylene sulfide-based resins, with acrylic-based resins being preferred from the viewpoint of transparency.
[0055] The thickness of the optical film is not particularly limited, but is, for example, preferably from 1.0 to 100 μm, more preferably from 1.5 to 50 μm, and further preferably from 2.0 to 30 μm.
[0056] (Optical film manufacturing) The optical film in this embodiment is manufactured by kneading spherical silica particles and resin to form a resin layer.The manufacturing method is not particularly limited, but for example, after preparing a resin mixture by kneading spherical silica particles and a resin composition, the resin mixture is applied to a support to form a coating film, and the coating film is dried to remove volatile components such as solvent, thereby forming a resin layer on the support.The resin mixture may contain various solvents, and may appropriately contain the above-mentioned additives as long as the optical film after preparation does not lose anti-glare properties.
[0057] The solvent to be used can be appropriately selected depending on the type of resin or additive, and can dissolve at least the solid content uniformly. Examples of the solvent include ketones (acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, etc.), ethers (dioxane, tetrahydrofuran, etc.), aliphatic hydrocarbons (hexane, etc.), alicyclic hydrocarbons (cyclohexane, etc.), aromatic hydrocarbons (toluene, xylene, etc.), halogenated carbons (dichloromethane, dichloroethane, etc.), esters (methyl acetate, ethyl acetate, butyl acetate, etc.), water, alcohols (ethanol, isopropanol, butanol, cyclohexanol, etc.), cellosolves (methyl cellosolve, ethyl cellosolve, etc.), cellosolve acetates, sulfoxides (dimethyl sulfoxide, etc.), amides (dimethylformamide, dimethylacetamide, etc.), etc. These solvents may be used alone, or two or more solvents may be used. From the viewpoint of the solubility of the resin, it is preferable that the solvent contains a polar group.
[0058] The support is not particularly limited, and examples thereof include known films such as polyethylene terephthalate (PET) film, polyphenylene sulfide film, and polyimide film. The surface of the support may be previously surface-treated with a surface treatment agent such as silicone, a silane coupling agent, an aluminum chelating agent, or polyurea in order to improve the releasability of the resin kneaded product, which is the formed sheet. The thickness of the support is not particularly limited, and examples thereof include 10 to 100 μm.
[0059] Examples of a method for applying the resin mixture onto a support include rotation coating using a spinner, spray coating, roll coating, screen printing, and methods using a blade coater, a die coater, a calendar coater, a meniscus coater, a bar coater, a roll coater, a comma roll coater, a gravure coater, a screen coater, and a slit die coater.
[0060] The coating film can be dried using, for example, an oven, a hot plate, infrared rays, etc. The drying temperature and drying time are not particularly limited, and examples of the drying temperature are within the range of 60 to 200° C. and the drying time is within the range of 1 to 360 minutes.
[0061] The thickness of the coating film is not particularly limited, and may be, for example, 1.0 to 100 μm, or may be 1.5 to 50 μm, or may be 2.0 to 30 μm, in terms of thickness after drying.
[0062] After the drying step, the resin may be cured by irradiation with ionizing radiation or heating depending on the type of resin, such as an ionizing radiation curable resin or a thermosetting resin. When the ionizing radiation is ultraviolet radiation, a far ultraviolet lamp, a low pressure mercury lamp, a high pressure mercury lamp, an extra-high pressure mercury lamp, a halogen lamp, a laser light source (light source such as a helium-cadmium laser or an excimer laser), etc. can be used as the light source.
[0063] From the viewpoint of adhesion of the silica particles, the total content of the silica particles in the resin mixture is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 5.0 parts by mass, and even more preferably 1.0 to 3.0 parts by mass.
[0064] The resin layer formed on the support is then separated from the support to obtain an optical film.
[0065] (optical laminate) The optical laminate of this embodiment has a resin layer containing spherical silica particles. The resin layer is an optical functional layer having an optical function due to the spherical silica particles, and an example of the optical functional layer is an anti-glare layer exhibiting anti-glare properties. When the particle diameters of the spherical silica particles at the cumulative 10%, cumulative 50% and cumulative 90% from the smallest side in the volume-based particle size distribution are respectively D10, D50 and D90, the D90 / D10 is 2.0 to 4.0, and the D50 is 1 to 20 μm.
[0066] In addition to the resin layer, the optical laminate may have a base layer, an antireflection layer, an antistatic layer, an antifouling layer, an electromagnetic wave shielding layer, an infrared absorbing layer, an ultraviolet absorbing layer, a color correction layer, etc., and the order of these layers is not particularly limited. The resin layer may be a single layer, or a laminate of multiple layers. In addition, the resin layer itself may be further provided with functions such as ultraviolet absorbing performance, antistatic performance, refractive index adjustment function, and hardness adjustment function. In order to improve the adhesion between each layer, a primer layer, an adhesive layer, etc. may be provided between each layer.
[0067] An example of the configuration of the optical laminate is one having an antiglare layer, which is an optically functional layer, on a substrate layer, and the surface of the antiglare layer opposite to the substrate is the uneven surface of the optical laminate. The antiglare layer may be laminated on at least one surface of the substrate layer, and may be laminated on both surfaces, but from the viewpoints of handling, mechanical properties, productivity, etc., it is usually preferable that the antiglare layer is laminated on only one surface.
[0068] The spherical silica particles and resin used in the resin layer may be the same as those used in the optical film. In addition, as in the optical film, various additives may be contained as necessary.
[0069] The thickness of the resin layer is not particularly limited, but is, for example, preferably from 1.0 to 100 μm, more preferably from 1.5 to 50 μm, and further preferably from 2.0 to 30 μm.
[0070] When the optical laminate in this embodiment has a substrate layer, the material of the substrate layer is not particularly limited, and glass, ceramics, and resins can be used. Among these, from the viewpoint of processability, it is preferable to use a resin. Preferred resins include transparent polymers, such as cellulose derivatives (cellulose acetates such as cellulose triacetate (TAC) and cellulose diacetate), polyester resins (polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), polyarylate resins, etc.), polysulfone resins (polysulfone, polyethersulfone (PES), etc.), polyetherketone resins (polyetherketone (PEK), polyetheretherketone (PEEK), etc.), polycarbonate resins (PC), polyolefin resins (polyethylene, polypropylene, etc.), cyclic polyolefin resins, halogen-containing resins (polyvinylidene chloride, etc.), (meth)acrylic resins, styrene resins (polystyrene, etc.), vinyl acetate or vinyl alcohol resins (polyvinyl alcohol, etc.), etc. can be exemplified. The term "(meth)acrylic" refers collectively to acrylic and methacrylic. Among these, acrylic resins are more preferred from the viewpoint of transparency.
[0071] The thickness of the base layer is not particularly limited, but is, for example, preferably from 1.0 to 100 μm, more preferably from 1.5 to 50 μm, and further preferably from 2.0 to 50 μm.
[0072] The thickness of the optical laminate may be adjusted appropriately depending on the application. For example, when used in a display device such as a liquid crystal display device or an organic EL display, the thickness is preferably 3 to 100 μm, more preferably 5 to 70 μm, and even more preferably 20 to 50 μm.
[0073] (Production of optical laminate) The optical laminate in this embodiment is manufactured by kneading spherical silica particles and resin to form a resin layer.The manufacturing method is not particularly limited, but for example, after preparing a resin mixture by kneading spherical silica particles and a resin composition, the resin mixture is applied onto a base layer to form a coating film, and the coating film is dried to remove volatile components such as solvent, thereby forming the resin layer on the base layer.The resin mixture may contain various solvents, and may appropriately contain the above-mentioned additives as long as the optical laminate after manufacturing does not lose anti-glare properties.
[0074] In addition to the resin layer, the optical laminate may include a base layer, an antireflection layer, an antistatic layer, an antifouling layer, an electromagnetic wave shielding layer, an infrared absorbing layer, an ultraviolet absorbing layer, a color correction layer, etc., and the order of these layers is not particularly limited. The resin layer may be a single layer, or may be a laminate of multiple layers. In addition, the resin layer itself may be further provided with functions such as ultraviolet absorbing performance, antistatic performance, refractive index adjustment function, and hardness adjustment function. In order to improve the adhesion between each layer, a primer layer, an adhesive layer, etc. may be provided between each layer. When the optical laminate in this embodiment has a base layer, the material of the base layer is not particularly limited, and the above-mentioned materials can be used.
[0075] As the solvent, the same solvent as that used for the optical film can be used.
[0076] Methods for applying the resin mixture onto the substrate layer include rotational application using a spinner, spray application, roll coating, screen printing, and methods using a blade coater, die coater, calendar coater, meniscus coater, bar coater, roll coater, comma roll coater, gravure coater, screen coater, and slit die coater.
[0077] The coating film can be dried, for example, by using an oven, a hot plate, infrared rays, etc. The drying temperature and drying time are not particularly limited, and examples thereof include a drying temperature of 40 to 120° C. and a drying time of 1 to 20 minutes.
[0078] The thickness of the coating film is not particularly limited, and may be, for example, 1.0 to 100 μm, or may be 1.5 to 50 μm, or may be 2.0 to 30 μm, in terms of thickness after drying.
[0079] After the drying step, the resin may be cured by irradiation with ionizing radiation or heating depending on the type of resin, such as an ionizing radiation curable resin or a thermosetting resin.
[0080] When the ionizing radiation is ultraviolet radiation, a far ultraviolet lamp, a low pressure mercury lamp, a high pressure mercury lamp, an extra-high pressure mercury lamp, a halogen lamp, a laser light source (light source such as a helium-cadmium laser or an excimer laser), etc. can be used as the light source.
[0081] From the viewpoint of adhesion of the silica particles, the total content of the silica particles in the resin mixture is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 5.0 parts by mass, and even more preferably 1.0 to 3.0 parts by mass.
[0082] (Evaluation of Optical Properties of Optical Films and Optical Laminates) <Anti-glare index value (Diffusion)> The antiglare property of the optical film and the optical laminate in this embodiment is represented by an antiglare index value (Diffusion). Diffusion can be measured using a goniophotometer, GC5000L, manufactured by Nippon Denshoku Industries Co., Ltd., according to the following procedure.
[0083] The direction parallel to the thickness direction of the anti-glare film-coated substrate is defined as 0 degrees. At this time, a first light is irradiated onto the main surface of the anti-glare film-coated substrate from a direction of angle θ=-45 degrees±0.5 degrees (hereinafter also referred to as "direction of angle -45 degrees"). The first light is reflected by the main surface of the anti-glare film-coated substrate. The luminance of the 45-degree reflected light reflected in a direction of angle 45 degrees from the main surface of the anti-glare film-coated substrate is measured and defined as the "luminance of the 45-degree reflected light." Next, the angle θ at which the luminance of the light reflected by the main surface of the anti-glare film-coated substrate is measured is changed in the range of 5 degrees to 85 degrees, and the same operation is performed to measure the luminance distribution of the reflected light in the range of 5 degrees to 85 degrees reflected by the main surface of the anti-glare film-coated substrate, and the total is used as the "luminance of the total reflected light." Next, the anti-glare index value (Diffusion) is calculated by using the formula: anti-glare index value={(luminance of total reflected light-luminance of 45-degree reflected light) / (luminance of total reflected light)}.
[0084] The antiglare index value is preferably from 0.3 to 1.0, and more preferably from 0.4 to 0.8. In addition, when evaluating the antiglare property, a relative evaluation is made in addition to a visual evaluation, and the optical film and optical laminate are evaluated based on the degree of reflection when placed on black felt.
[0085] <haze> The haze of the optical film and the optical laminate in this embodiment is represented by haze. Haze can be measured using a haze meter (HR-100 model, manufactured by Murakami Color Research Laboratory) according to the method specified in JIS K7136:2000.
[0086] The haze is preferably 45% or less, and more preferably 35% or less. Since the smaller the haze measurement value, the more preferable it is, there is no particular lower limit.
[0087] <sparkle> The degree of sparkle of the optical film and optical laminate in this embodiment is represented by a sparkle index value (Sparkle). Sparkle can be measured by placing a substrate with an anti-glare film on the display surface of a liquid crystal display (LG, 24 inches) with the main surface on which the anti-glare film is formed (the surface with projections and recesses) facing up, and using an i-Scale ISC-A manufactured by i-Systems.
[0088] The glare index value is preferably from 1.0 to 5.0, and more preferably from 2.0 to 4.0. The degree of glare is evaluated in combination with visual evaluation, and is evaluated based on the degree of glare when the optical film and optical laminate are placed on the above-mentioned display.
[0089] The optical film and optical laminate of the present invention exhibit optical functions such as antiglare properties, and can suppress the effects of glare, haze, and structural color due to interference, and can therefore be used as antiglare films, light-diffusing OCRs, and light-diffusing adhesive layers in various display devices, such as liquid crystal displays (LCDs), organic EL displays, and display devices with touch panels, and are particularly useful as optical elements for LCDs and organic EL displays.
[0090] As described above, the present specification discloses the following configurations. <1> An optical film comprising a resin layer containing spherical silica particles, wherein the spherical silica particles have a D90 / D10 ratio of 2.0 to 4.0 and a D50 ratio of 1 to 20 μm, where D10, D50 and D90 are the cumulative 10%, 50% and 90% particle diameters from the smallest end in a volume-based particle size distribution, respectively. <2> The pore volume of the spherical silica particles is 0.001 to 1.0 cm 3 / g <1> The optical film according to claim 1. <3> The volume ratio of the spherical silica particles having a particle size of 1 μm or less is 7% or less. <1> or <2> The optical film according to claim 1. <4> The volume ratio of the spherical silica particles having a particle size of 20 μm or more is 10% or less. <1> ~ <3> 13. The optical film according to claim 12 . <5> The BET specific surface area of the spherical silica particles is 0.3 to 800 m 2 / g <1> ~ <4> 13. The optical film according to claim 12 . <6> The resin layer includes a cured product of a curable resin. <1> ~ <5> 13. The optical film according to claim 12 . <7> The spherical silica particles and the resin are kneaded to form a resin layer. <1> ~ <6> 13. A method for producing an optical film according to any one of claims 1 to 12. <8> An optical laminate having a resin layer containing spherical silica particles, wherein the spherical silica particles have a D90 / D10 ratio of 2.0 to 4.0 and a D50 ratio of 1 to 20 μm, where D10, D50 and D90 are the particle diameters at cumulative 10%, cumulative 50% and cumulative 90% from the smallest particle size in a volume-based particle size distribution, respectively. <9> The spherical silica particles and the resin are kneaded to form a resin layer. <8> A method for producing the optical laminate described in claim 1. <10> The above <1> ~ <6> 10. The optical film according to claim 9, <8> A display device comprising the optical laminate according to claim 1. <11> The display device is a liquid crystal display device or an organic electroluminescence display device. <10> The display device according to claim 1 . <12> The above <1> ~ <6> 10. The optical film according to claim 9, <8> An antiglare film comprising the optical laminate according to claim 1. <13> The above <12> A display device comprising the antiglare film according to claim 1. <14> The display device is a liquid crystal display device or an organic electroluminescence display device. <13> The display device according to claim 1 . EXAMPLES
[0091] Next, the embodiments of the present disclosure will be specifically described with reference to examples, but the embodiments of the present disclosure are not limited to these examples. Examples 1 to 4 and 10 are examples, and Examples 5 to 9 are comparative examples.
[0092] (Example 1) Polyvinyl butyral (PVB) was used as the resin, and 20 parts by mass of PVB was dissolved in 80 parts by mass of methyl ethyl ketone, and the solution was stirred under the conditions of 2000 rpm x 15 minutes x 1 set to prepare a PVB solution. 87 parts by mass of the PVB solution, 3 parts by mass of spherical silica particles NP-30 (manufactured by AGC Si-Tech Co., Ltd.), and 10 parts by mass of methyl ethyl ketone were placed in a container and stirred under conditions of 2000 rpm x 3 minutes x 2 sets to prepare a resin mixture containing spherical silica particles. This resin mixture was cast onto a polyethylene terephthalate (PET) film using a wire bar (#9), and then left indoors for 5 minutes to evaporate the solvent, forming a resin layer and obtaining an optical film with a thickness of 4.0 μm.
[0093] (Example 2) An optical film was obtained in the same manner as in Example 1, except that HNP-20B (manufactured by AGC Si-Tech Co., Ltd.) was used as the spherical silica particles.
[0094] (Example 3) A spherical silica powder 1 (E-2C, D50=2.3 μm, manufactured by Suzuki Oil & Fat Co., Ltd.) manufactured by a wet method was prepared. The titanium (Ti) content of the silica powder 1 was measured and found to be 300 mass ppm. 15 g of the silica powder 1 was filled into an alumina crucible and heat-treated at an electric furnace temperature of 1300° C. for 1 hour. After the heat treatment, the mixture was cooled to room temperature and crushed in an agate mortar to obtain spherical silica particles. An optical film was obtained in the same manner as in Example 1, except that the spherical silica particles thus obtained were used.
[0095] (Example 4) An optical film was obtained in the same manner as in Example 1, except that H-31 (manufactured by AGC Si-Tech Co., Ltd.) was used as the spherical silica particles.
[0096] (Example 5) An optical film was obtained in the same manner as in Example 1, except that NP-200 (manufactured by AGC Si-Tech Co., Ltd.) was used as the spherical silica particles.
[0097] (Example 6) An optical film was obtained in the same manner as in Example 1, except that SC5500-SQ (manufactured by Admatechs Co., Ltd.) was used as the spherical silica particles.
[0098] (Example 7) An optical film was obtained in the same manner as in Example 1, except that DM-10-1000 (manufactured by AGC Si-Tech Co., Ltd.) was used as the spherical silica particles.
[0099] (Example 8) An optical film was obtained in the same manner as in Example 1, except that amorphous silica particles (Mizukasil: P-707 (manufactured by Mizusawa Chemical Industry Co., Ltd.)) were used instead of the spherical silica particles.
[0100] (Example 9) An optical film was obtained in the same manner as in Example 1, except that 1.5 parts by mass of NP-30 and 1.5 parts by mass of NP-200 were used as the spherical silica particles.
[0101] The silica particles used in Examples 1 to 9 and the resulting optical films were subjected to the following measurements. The results are shown in Table 1.
[0102] <D50, D90 / D10 of Silica Particles> Distilled water was added to the silica particles to make a slurry of 0.05 parts by mass, which was then treated in an ultrasonic cleaner at a frequency of 45 kHz for 2 minutes. The 50% particle size (D50) in the cumulative particle size distribution based on volume was calculated using an electrical detection particle size distribution measuring device (Beckman Coulter, Multisizer4e) (settings: aperture diameter 50 μm, effective N number 50,000, current 800 μA, gain 4, stirring speed 15, electrolyte isoton). In addition, the 90% particle size (D90) and the 10% particle size (D10) in the cumulative particle size distribution based on volume were calculated using the same procedure as above, and the ratio of D90 to D10 (D90 / D10) was calculated from the obtained values.
[0103] <Proportion of particles with diameters of 1 μm or less and 20 μm or more> The proportion of silica particles with a particle size of 1 μm or less and 20 μm or more was measured by the laser diffraction method using a particle size distribution analyzer (Microtrack Bell, MT3300EXII). Specifically, the silica particles were dispersed by irradiating them with ultrasonic waves three times for 60 seconds in the device, and then the measurement was performed. From the obtained particle size distribution, the proportion of particles with a size of 1 μm or less and the proportion of particles with a size of 20 μm or more were calculated.
[0104] <BET specific surface area and pore volume of silica particles> The silica particles were dried under reduced pressure at 230°C to completely remove moisture and used as a sample. The specific surface area and pore volume of this sample were determined using the multipoint BET method with nitrogen gas using an automatic specific surface area and pore distribution measurement device "Tristar II" manufactured by Micromeritics.
[0105] <Sphericity of Silica Particles> The sphericity of silica particles was determined by measuring the maximum diameter (DL) and the perpendicular minor diameter (DS) of each of 100 random particles in a photograph obtained by a scanning electron microscope (SEM), calculating the ratio (DS / DL) of the minimum diameter (DS) to the maximum diameter (DL), and then calculating the average.
[0106] <Anti-glare index value of optical film (Diffusion)> The antiglare index value was measured using a goniophotometer, GC5000L, manufactured by Nippon Denshoku Industries Co., Ltd., according to the following procedure. The direction parallel to the thickness direction of the anti-glare film-coated substrate was defined as 0 degrees. At this time, a first light was irradiated onto the main surface of the anti-glare film-coated substrate from a direction of angle θ=-45 degrees±0.5 degrees (hereinafter also referred to as "direction of angle -45 degrees"). The first light was reflected by the main surface of the anti-glare film-coated substrate. The luminance of the 45-degree reflected light reflected in a direction of angle 45 degrees from the main surface of the anti-glare film-coated substrate was measured and defined as "luminance of 45-degree reflected light." Next, the angle θ for measuring the luminance of the light reflected by the main surface of the anti-glare film-coated substrate was changed in the range of 5 degrees to 85 degrees, and the same operation was performed. The luminance distribution of the reflected light in the range of 5 degrees to 85 degrees reflected by the main surface of the anti-glare film-coated substrate was measured and summed up to obtain the "luminance of the total reflected light." Next, the anti-glare index value (Diffusion) was calculated using the formula: anti-glare index value = {(luminance of total reflected light - luminance of 45-degree reflected light) / (luminance of total reflected light)}, and evaluated relatively together with the visual evaluation. When the optical film was placed on the black felt, those that showed no reflection were rated as "A," those that showed slight reflection were rated as "B," and those that showed noticeable reflection were rated as "C." Note that ratings A and B are suitable for practical use.
[0107] <Haze of optical film> The haze was measured using a haze meter (HR-100 model, manufactured by Murakami Color Research Laboratory) in accordance with the method specified in JIS K7136:2000, and evaluated relatively. Measurement values of 35% or less were given an "A," values between 35% and 45% were given a "B," and values over 45% were given a "C." Ratings A and B are suitable for practical use.
[0108] <Optical film Sparkle> The substrate with the anti-glare film was placed on the display surface of a liquid crystal display (LG, 24 inches) with the main surface on which the anti-glare film was formed (the surface with projections and recesses) facing up, and the glare index value was measured using the Eye Scale ISC-A manufactured by Eye System, and a relative evaluation was made in conjunction with the visual evaluation. When the optical film was placed on a display, those that showed no glare were rated as "A," those that showed slight glare were rated as "B," and those that showed noticeable glare were rated as "C." Ratings A and B are suitable for practical use.
[0109] [Table 1]
[0110] From the results shown in Table 1, it was confirmed that the optical films of Examples 1 to 4 have excellent antiglare properties while suppressing glare compared to Examples 5 to 9. In particular, it was confirmed that Examples 1 to 4 have few fine particles of 1.0 μm or less and few coarse particles of 20 μm or more, and can suppress interference and anisotropic scattering of light of specific wavelengths, thereby achieving low glare and low haze.
[0111] Moreover, when the optical film of Example 10 was produced by the following procedure, it exhibited optical properties equivalent to those of Examples 1-4.
[0112] (Example 10) An optical film was prepared according to the following procedure. The mixture was mixed with 45.75 parts by mass of butyl acetate, which is an organic solvent, 17.5 parts by mass of urethane acrylate oligomer, 25.0 parts by mass of a multifunctional acrylic monomer ("Laromer DPHA-A ap." manufactured by BASF Japan Ltd.), 2.0 parts by mass of an ultraviolet absorber having a triazine skeleton ("Tinuvin 479" manufactured by BASF Japan Ltd.), 4.0 parts by mass of an ultraviolet absorber having a benzotriazole skeleton ("RUVA-93" manufactured by Otsuka Chemical Co., Ltd.), 0.5 parts by mass of a fluorine-based compound having a photopolymerizable unsaturated group ("Megafac RS-75" manufactured by DIC Corporation), 2.0 parts by mass of a photopolymerization initiator ("IRGACURE 184D" manufactured by BASF Japan Ltd.), and 1.0 parts by mass of a photopolymerization initiator ("IRGACURE 184D" manufactured by BASF Japan Ltd.). 1.0 part by mass of "TPO" and 1.0 part by mass of a light stabilizer (BASF Japan Ltd.'s "Tinuvin 123") were added and dissolved. Then, 1.25 parts by mass of spherical silica particles NP-30 (AGC Si-Tech Co., Ltd.) were added to the solution and stirred to obtain a photocurable resin composition in which the spherical silica was dispersed. This resin composition was cast onto a polyethylene terephthalate (PET) film using a wire bar (#9), and then irradiated with ultraviolet light from an electrodeless lamp (irradiation dose: 400 mJ / cm 2 ) The coating was cured to obtain an optical film with a thickness of 4.0 μm.< / sparkle> < / haze>
Claims
1. An optical film comprising a resin layer containing spherical silica particles, the spherical silica particles being characterized in that, when the particle diameters of the spherical silica particles at cumulative 10%, cumulative 50% and cumulative 90% from the smallest side in a volume-based particle size distribution are defined as D10, D50 and D90, respectively, D90 / D10 is 2.0 to 4.0 and D50 is 1 to 20 μm.
2. The pore volume of the spherical silica particles is 0.001 to 1.0 cm 3 The optical film according to claim 1 , wherein the refractive index is 1 / g.
3. 2. The optical film according to claim 1, wherein the volume ratio of particles having a particle size of 1 μm or less among the spherical silica particles is 7% or less.
4. 2. The optical film according to claim 1, wherein the volume ratio of particles having a particle size of 20 μm or more among the spherical silica particles is 10% or less.
5. The BET specific surface area of the spherical silica particles is 0.3 to 800 m 2 The optical film according to claim 1 , wherein the refractive index is 1 / g.
6. The optical film according to claim 1 , wherein the resin layer comprises a cured product of a curable resin.
7. The method for producing an optical film according to any one of claims 1 to 6, wherein the resin layer is formed by kneading the spherical silica particles and a resin.
8. An optical laminate having a resin layer containing spherical silica particles, wherein the spherical silica particles have a D90 / D10 ratio of 2.0 to 4.0 and a D50 ratio of 1 to 20 μm, where D10, D50 and D90 are the particle diameters at cumulative 10%, cumulative 50% and cumulative 90% from the smallest particle size in a volume-based particle size distribution, respectively.
9. The method for producing an optical laminate according to claim 8 , wherein the resin layer is formed by kneading the spherical silica particles and a resin.
10. A display device comprising the optical film according to any one of claims 1 to 6 or the optical laminate according to claim 8.
11. The display device according to claim 10 , wherein the display device is a liquid crystal display device or an organic electroluminescence display device.
12. An antiglare film comprising the optical film according to any one of claims 1 to 6 or the optical laminate according to claim 8.
13. A display device comprising the antiglare film according to claim 12.
14. The display device according to claim 13 , wherein the display device is a liquid crystal display device or an organic electroluminescence display device.
Citation Information
Patent Citations
Antiglare film, antiglare sheet polarizer and image display apparatus
JP2009251378A
Photocurable resin composition, cured coating and coated substrate formed from said composition, and method for producing cured coating and coated substrate
JP6822792B2
Cited By
Resin composition, cured product, and optical fiber array
WO2025070440A1