Electroless plating method
The use of palladium fine particles formed by electric discharge in a liquid as a catalyst application treatment liquid addresses the high cost and complexity of conventional electroless plating methods, achieving efficient and safe electroless plating with reduced noble metal usage.
Patent Information
- Application Number
- JP2023043223
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-17
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional electroless plating methods require high concentrations of noble metals, leading to increased costs and complexity, and often involve post-treatments with strong acids, posing safety and environmental risks.
A method using palladium fine particles formed by electric discharge in a liquid as a catalyst application treatment liquid, reducing the need for high noble metal concentrations and eliminating the requirement for post-treatments with strong acids.
Enables efficient and cost-effective electroless plating with improved safety and reduced operational complexity, achieving good plating results with lower palladium usage.
Smart Images

Figure 2024132457000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a plating method. [Background technology]
[0002] Conventionally, electroless plating has been widely used as a method for directly forming a metal or alloy coating on various substrates, including not only metal substrates but also polymer molded bodies, fiber structures, glass, ceramics, etc. In particular, products in which a plating film is formed on the surface of a resin substrate are lighter and less expensive than products made from metal materials, and are therefore used as various components, including automobile components, building material components, and electronic components such as circuit boards.
[0003] When the substrate is insulating, such as a polymer molded product of resin, catalytic nuclei are generally formed in advance on the substrate surface to facilitate the deposition of metal for electroless plating. Usually, the insulating substrate is brought into contact with a pretreatment liquid by immersion or the like, and a treatment is performed to apply a catalyst for electroless plating to the portions requiring plating.
[0004] Catalysts for electroless plating are generally fine particles of metals, primarily gold (Au), platinum (Pt), and palladium (Pd), or alloys thereof.
[0005] For example, Patent Documents 1 and 2 disclose an electroless plating method using a palladium / tin mixed colloidal catalyst solution as a catalyst-imparting treatment solution. This method is usually accompanied by a treatment (accelerator treatment) in which the colloidal catalyst applied to the substrate is treated with an acid or the like to activate it, and is therefore also called a catalyzer-accelerator method. Patent Documents 2 and 3 disclose a so-called sensitizing-activating method in which tin is adsorbed to oxygen atoms or the like on the substrate surface to form an adsorption site for palladium (sensitizing), and then palladium, which has high catalytic ability, is adsorbed to the adsorption site of the tin (activating). Patent Document 4 discloses a method in which a catalyst is applied to the substrate surface using a catalyst solution containing palladium ions, and then the catalyst is brought into contact with a reducing agent solution. Patent Document 5 discloses a technology in which a metal salt such as palladium is reduced to prepare a catalyst for electroless plating. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent No. 4275157 [Patent Document 2] JP 2016-029209 A [Patent Document 3] JP 2007-063646 A [Patent Document 4] JP 2015-086429 A [Patent Document 5] JP 2013-184425 A Summary of the Invention [Problem to be solved by the invention]
[0007] In these conventional methods, if a catalyst-imparting treatment solution with a low precious metal concentration is used, the metal plating layer is difficult to deposit, and plating defects are likely to occur. Usually, a catalyst-imparting treatment solution with a precious metal concentration of several tens of ppm or more, sometimes 100 ppm or more, is used, which increases production costs. In addition, in many cases, post-treatment such as reduction and activation of the precious metal catalyst is required. Moreover, in the post-treatment, strong acids such as hydrochloric acid and sulfuric acid, which generally have a concentration of about 1 mol / L or more, are often used, which may corrode surrounding equipment and have adverse effects on the human body. Thus, the conventional methods require a high-concentration precious metal treatment solution and multiple steps for catalyst impartation, which is cumbersome, costly, and time-consuming.
[0008] The present invention aims to solve the above-mentioned problems by providing a plating method which can obtain good electroless plated parts even when the amount of palladium used for catalyst application is reduced, does not require post-treatment with a strong acid or the like after catalyst application, and can be carried out simply and at low cost. [Means for solving the problem]
[0009] The inventors discovered that by using a liquid containing palladium microparticles formed by discharging in the liquid in the catalyst application step prior to the electroless plating step, good plated parts can be produced even with a low concentration catalyst application treatment liquid, and post-treatment with strong acid is no longer necessary, making it possible to perform electroless plating safely and simply at low cost, thereby completing the present invention.
[0010] That is, the present invention provides the following (1) to (12). (1) A plating method including at least a catalyst imparting step of contacting a catalyst imparting treatment solution with a treated surface of a substrate to impart a catalyst thereto, and an electroless plating step of applying metal plating to the treated surface to which the catalyst has been imparted, In the catalyst application step, a liquid containing palladium fine particles formed by discharging between a palladium electrode and a counter electrode disposed in the liquid is used as the catalyst application treatment liquid. Plating method. (2) The catalyst application step is preparing the catalyst imparting treatment liquid containing the palladium fine particles by discharging between the palladium electrode and the counter electrode disposed in the liquid; an operation of contacting the catalyst application treatment liquid with the surface to be treated; The plating method according to (1) above, (3) The plating method according to (1) or (2) above, wherein the average zeta potential of the palladium fine particles in the catalyst imparting treatment solution is 0 mV or less. (4) The plating method according to any one of the above (1) to (3), wherein the catalyst application treatment liquid contains a polyvalent carboxylic acid and / or a salt thereof. (5) The plating method according to any one of the above (1) to (4), wherein the substrate is made of one or more materials selected from the group consisting of polymers, glass, ceramics, carbon materials, and metals. (6) The plating method according to any one of the above (1) to (5), wherein the base material is a substrate. (7) The plating method according to any one of (1) to (6) above, further comprising a conditioning step of contacting the surface to be treated with a catalyst application enhancing liquid containing a polyamine compound prior to the catalyst application step. (8) The plating method according to (7) above, further comprising a step of rinsing the treated surface with water between the conditioning step and the catalyst application step. (9) The plating method according to any one of (1) to (8) above, further comprising an activation treatment step between the catalyst application step and the electroless plating step, in which the treatment surface is contacted with a hypophosphorous acid solution, a reducing agent, and / or an inorganic acid. (10) The plating method according to any one of (1) to (9) above, further comprising a step of modifying the surface to be treated prior to the catalyst application step. (11) The plating method according to any one of (1) to (9) above, further comprising, prior to the catalyst application step, an etching step of contacting the treated surface with an acidic solution containing an oxidizing agent. (12) A plated part produced by any one of the plating methods (1) to (11) above. Effect of the Invention
[0011] According to the plating method of the present invention, it is possible to obtain good electroless plated parts even if the amount of palladium used for applying the catalyst is reduced. In addition, since there is no need for post-treatment with a strong acid or the like after applying the catalyst, electroless plating can be performed safely and easily without spending time and money. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a conceptual diagram showing a schematic configuration of an example of a production apparatus used for preparing a catalyst application treatment liquid according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a flow diagram showing an example of a plating process according to one embodiment of the present invention. [Diagram 3] FIG. 4 is a conceptual diagram showing an example of a catalyst application step in a plating treatment step according to another embodiment of the present invention. [Figure 4] FIG. 13 is a photograph showing the results of a backlight test of a printed wiring board after electroless copper plating in Example 16 according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The present invention will be described in detail below based on the embodiments, but the present invention is not limited to these embodiments.
[0014] ≪1. Overview of plating method≫ The present embodiment is a plating method including at least a catalyst imparting step in which a catalyst is imparted to a treated surface of a substrate by contacting the treated surface with a catalyst imparting treatment liquid, and an electroless plating step in which metal plating is performed on the treated surface to which the catalyst has been imparted, in which the catalyst imparting treatment step uses a liquid containing palladium fine particles formed by discharge between a palladium electrode and a counter electrode placed in the liquid as the catalyst imparting treatment liquid.
[0015] In this embodiment, a liquid containing palladium fine particles formed by discharging between a palladium electrode and a counter electrode (palladium electrode-counter electrode) in the liquid is used.
[0016] Palladium fine particles are generally produced by chemical synthesis methods such as the reduction of palladium ions described above, as well as physical means such as laser evaporation and CVD. However, these methods often require conditions accompanied by energy consumption, such as high temperatures, and have the disadvantage that the produced particles tend to aggregate.
[0017] In contrast, by discharging between the palladium electrode and the counter electrode in a liquid, a catalyst-imparting treatment liquid in which fine particles of uniform size are uniformly dispersed can be easily formed, and energy consumption can be reduced. First, the formation of a catalyst-imparting treatment liquid by discharging in liquid is described below.
[0018] 2. Formation of catalyst application treatment solution The catalyst-imparting treatment liquid used in the plating method of this embodiment is formed by discharging between a palladium electrode and a counter electrode placed in the liquid. The fine particles thus formed are easily adsorbed to the substrate, and do not require post-treatment such as activation. Moreover, compared with fine particles generated by laser evaporation or deposition, the fine particles tend to have a uniform particle size and are easily dispersed uniformly in the liquid. Therefore, a liquid containing palladium fine particles formed by discharging between electrodes in a liquid can exhibit excellent effects as a catalyst-imparting treatment liquid even if it is low in concentration. The formation of the palladium fine particles themselves can be performed without requiring conditions such as high temperature or complicated processes. Therefore, according to this embodiment, it is possible to easily obtain good electroless plated parts with a smaller amount of palladium used.
[0019] (1) Catalyst application treatment solution By discharging between the palladium electrode and the counter electrode, palladium fine particles having an average particle size of, for example, 1 to 500 nm, particularly about 200 to 400 nm, are formed in the catalyst-imparting treatment liquid by the cumulant method (a measurement method based on scattered light intensity, see JIS Z8828, etc.). The catalyst-imparting treatment liquid formed by the in-liquid discharge contains such nano-order fine particles, and therefore exhibits excellent functions as a catalyst-imparting treatment liquid for electroless plating.
[0020] In addition, by discharging between the palladium electrode and the counter electrode, fine palladium particles can be easily formed in the catalyst-imparting treatment solution at a concentration of, for example, 1 to 3000 mg / L, particularly about 10 to 100 mg / L, but the catalyst-imparting treatment solution in this embodiment exhibits catalytic function even at a lower palladium concentration. For example, even if the concentration of palladium fine particles in the catalyst-imparting treatment solution is low, such as 1 to 50 mg / L, particularly 2 to 30 mg / L, further 3 to 15 mg / L, particularly about 4 to 10 mg / L, it is possible to obtain good electroless plated parts. The present invention also encompasses a catalyst-imparting treatment solution containing fine palladium particles thus formed by discharging in liquid.
[0021] As described above, the palladium fine particles used in the method of the present embodiment do not require post-treatment with a reducing agent solution or an activation treatment solution containing hydrochloric acid, sulfuric acid, or the like, unlike palladium particles formed by a conventionally known reduction method. Therefore, in a series of plating methods, not only can the number of steps be reduced, but it is also possible to avoid, for example, deterioration of a substrate such as a polymer molded body or side reactions caused by a reducing agent or acid. In other words, the catalyst application treatment solution used in the method of the present embodiment can be one that does not contain a reducing agent.
[0022] The palladium fine particles contained in the catalyst imparting treatment solution preferably have an average zeta potential of 0 mV or less, for example, about −10 to −50 mV, and particularly about −20 to −40 mV. A solution containing palladium fine particles with such a zeta potential has the advantage of being stable for a long period of time.
[0023] (2) Method for preparing catalyst imparting treatment solution Next, a method for preparing the catalyst application treatment liquid as described above will be described by taking a preferred embodiment as an example.
[0024] (Palladium electrode) The palladium fine particles contained in the catalyst imparting treatment liquid are formed by discharge between a palladium electrode and a counter electrode placed in the liquid. The palladium electrode used is not particularly limited in structure or shape. For example, it may be a plate, rod, or hollow cylinder made of palladium, or may have a structure in which a metal plate such as copper or iron is coated with palladium. A structure in which a part of the electrode surface is coated with an insulator may also be used.
[0025] In addition, the purity of palladium in the electrode is not particularly limited. From the viewpoint of catalyst application efficiency, it is preferable to use high-purity palladium, for example, 90% or more, further 99% or more, and especially high-purity products with a purity of 99.9% or more that contain nothing but unavoidable impurities. Depending on the purpose, alloys of palladium with platinum, nickel, and / or tin can also be used. By using alloys, fine particles in which two or more elements are mixed on a nanoscale can be formed.
[0026] There is also no particular limitation on the size of the palladium electrode. In the case of in-liquid discharge, the amount of fine particles formed can be increased by increasing the area of the discharge portion.
[0027] (opposite) There is no particular restriction on the material, structure, or shape of the counter electrode. For example, it may be a plate, rod, or hollow cylinder made of a metal such as tungsten or graphite, and may have a structure in which a part of the surface is covered with an insulator. The purity of the metal is not particularly limited, and the shape of the counter electrode may be the same as or different from that of the palladium electrode. The same as the above-mentioned palladium electrode may be used as the counter electrode, and in-liquid discharge may be performed between a pair of palladium electrodes. Note that, during discharge, only the above-mentioned palladium electrode needs to be placed in the liquid, and the counter electrode may be placed in, for example, air. However, from the viewpoint of the efficiency of forming palladium fine particles, it is preferable that the counter electrode is placed in the same liquid as the palladium electrode.
[0028] (dispersion medium) The catalyst-imparting treatment liquid is formed by dispersing palladium fine particles formed by in-liquid discharge in a dispersion medium. There are no particular limitations on the dispersion medium constituting the catalyst-imparting treatment liquid as long as there are no problems such as dissolving the generated palladium fine particles. For example, water or hydrogen peroxide solution; alcohols such as methanol, ethanol, propanol, butanol, ethylene glycol, propylene glycol, and 1,4-butanediol; ethers such as tetrahydrofuran, tetrahydropyran, dipropyl ether, dibutyl ether, diethylene glycol, and tetraethylene glycol; carbonates such as ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, and methyl ethyl carbonate; esters such as methyl acetate, ethyl acetate, butyl acetate, methyl benzoate, and dimethyl phthalate; and other aliphatic hydrocarbons, aromatic hydrocarbons, silicones, ionic liquids, and the like can be used. In addition, a mixture of multiple solvents may be used to form a mixed dispersion medium.
[0029] Among these, in consideration of suitability in the plating process, dispersibility of palladium fine particles, conductivity during discharge, safety, etc., it is preferable to use water and / or alcohol such as ethanol as the dispersion medium, and it is particularly preferable to use water. Note that the palladium fine particles formed in a liquid by in-liquid discharge can be once filtered with a filter or the like and re-dispersed in a liquid such as water for use, but from the viewpoints of dispersibility and ease of operation, it is preferable to use the liquid obtained by discharging in water and / or alcohol as it is as the catalyst application treatment liquid.
[0030] (Conductive agent) When forming palladium fine particles by discharging between a palladium electrode and a counter electrode in a liquid, the liquid preferably contains a conductivity imparting agent.
[0031] There is no particular limit to the type of the conductivity imparting agent, and various inorganic salts, tetraalkylammonium salts, pyridinium salts, sulfonates, and other organic salts can be used. Among them, organic acid salts such as carboxylates are preferred. There is no particular limit to the carboxylate, and various carboxylic acid salts such as acetic acid, propionic acid, glycolic acid, lactic acid, benzoic acid, and salicylic acid can be used. More preferably, a polycarboxylic acid salt is used. Polycarboxylic acid salts not only function as a conductivity imparting agent, but can also increase the dispersion stability of the generated palladium fine particles. Therefore, they are suitable as additives for the catalyst imparting treatment liquid. In addition, the conductivity imparting agent such as polycarboxylic acid salts may be referred to as a "dispersant" below.
[0032] The polycarboxylic acid salt may be any salt that can be dissolved in a dispersion medium, such as water. Examples include aliphatic dicarboxylic acids such as oxalic acid (ethanedioic acid), malonic acid (propanedioic acid), succinic acid (butanedioic acid), glutaric acid (pentanedioic acid), adipic acid (hexanedioic acid), pimelic acid (heptanedioic acid), suberic acid (octanedioic acid), azelaic acid (nonanedioic acid), sebacic acid (decanedioic acid), fumaric acid (E-butenedioic acid), and maleic acid (cis-butenedioic acid); aromatic dicarboxylic acids such as phthalic acid, isophthalic acid, and terephthalic acid; tricarballylic acid (propanetricarboxylic acid), aconitic acid (propanedioic acid), and the like. tricarboxylic acids such as tricarboxylic acid (1,2,4-benzenetricarboxylic acid), trimellitic acid (1,2,4-benzenetricarboxylic acid), and trimesic acid (1,3,5-benzenetricarboxylic acid); and salts of hydroxy polycarboxylic acids such as malic acid (hydroxybutanedioic acid), tartaric acid (dihydroxybutanedioic acid), citramalic acid (hydroxymethylbutanedioic acid), citric acid (2-hydroxypropane-1,2,3-tricarboxylic acid), and isocitric acid (1-hydroxypropane-1,2,3-tricarboxylic acid), but are not limited thereto. The type of cation constituting the salt is also not particularly limited, and examples thereof include alkali metal ions such as sodium and potassium, substituted or unsubstituted ammonium ions, such as tetramethylammonium ions, but are not limited thereto. It is also possible to use a plurality of polycarboxylic acid salts in combination.
[0033] From the viewpoint of dispersibility of palladium fine particles, it is preferable to use, as the polycarboxylic acid salt, a salt of a hydroxy polycarboxylic acid, for example, a sodium salt or a potassium salt of malic acid, tartaric acid, citric acid, etc. Among them, when a citrate salt, particularly sodium citrate, is used, the dispersion state of the palladium fine particles becomes stable, and it is also possible to obtain a better electroless plated part.
[0034] These polycarboxylic acid salts are preferably used so that the electrical conductivity of the liquid forming the palladium fine particles is, for example, about 150 to 500 μS / cm, particularly about 300 to 400 μS / cm. If the electrical conductivity of the liquid is within this range, the formation of palladium fine particles by discharging between the electrodes is easy. Such electrical conductivity can be easily adjusted, for example, by setting the concentration of the polycarboxylic acid salt of malic acid or tartaric acid to about 0.1 to 0.5 g / L, particularly about 0.2 to 0.4 g / L. From the viewpoint of dispersibility of the palladium fine particles, it is preferable to set the polycarboxylic acid salt to such a concentration. Note that a compound other than the polycarboxylic acid salt may be used as the electrical conductivity imparting agent, and the polycarboxylic acid salt may be added after discharging.
[0035] In addition to the above-mentioned conductivity imparting agent and dispersant, the liquid for forming the palladium fine particles and / or the catalyst imparting treatment liquid may contain various additives such as a dispersing aid, an emulsifier, a surfactant, a pH adjuster, a pH buffer, a complexing agent, a viscosity adjuster, etc. From the viewpoint of increasing the catalytic activity, these additives may not be added, but if they are added, the amount is preferably about 0.1 to 1 g / L in total.
[0036] (Discharge treatment) In preparing the catalyst-imparting treatment liquid, a palladium electrode and a counter electrode are placed in the prepared liquid, and a discharge is caused between them to form a catalyst-imparting treatment liquid containing palladium fine particles. The preparation of the catalyst-imparting treatment liquid will be described in more detail below with reference to the discharge device 1 shown in FIG. 1. Note that the discharge device and discharge conditions are not limited to the following embodiments.
[0037] As shown in FIG. 1, first, a pair of electrodes 10 are arranged opposite each other with a predetermined gap therebetween. Next, the liquid 20 is filled in the container 30, and each electrode 10 is immersed in the liquid 20. In the embodiment shown in FIG. 1, both electrodes 10 have the same shape and size, but these two electrodes 10 may be different. For example, the material of one of the electrodes (counter electrode) may be other than palladium. In addition, both electrodes 10 are attached in advance to the side of the container 30 via the insulating part 12, but the electrode 10 may be immersed in the liquid 20 from the top of the container 30. Furthermore, either the arrangement of the electrodes 10 or the filling of the liquid 20 may be performed first. The materials of the electrodes 10 and the liquid 20 are as described above.
[0038] Next, a voltage is applied from the power supply unit 40 of the discharge device 1 to generate a discharge between the two electrodes in the liquid 20. At this time, a cooling treatment may be performed so that the electrodes 10 and the like do not become hot. For example, a mechanism for cooling the electrodes 10 may be provided with the discharge device 1. Also, one or both of the electrodes 10 may be vibrated to promote the generation of palladium fine particles. Furthermore, air bubbles such as microbubbles may be supplied to the periphery of the electrodes 10.
[0039] Here, the discharge method and the applied voltage are not particularly limited, and can be performed under appropriate conditions according to the device used. For example, any type of discharge, such as glow discharge, arc discharge, pulse discharge, etc., may be used. Glow discharge is preferable because it has good energy efficiency and is easy to obtain spatial uniformity. For example, a voltage of about 500 to 3000 V, particularly about 800 to 2000 V, is applied to the electrode 10 from the power supply unit 40. This makes it easy to form a liquid in which nano-sized palladium particles are uniformly dispersed. In addition, the current value at that time is not particularly limited, and can be, for example, 200 to 2000 mA.
[0040] Pulsed glow discharge may also be used. Since glow discharge is not in thermal equilibrium, driving with pulses may also contribute to preventing arc transition. For example, a pulse may be applied from the power supply unit 40 at a frequency of 20 Hz to 200 kHz, particularly about 800 Hz to 60 kHz. In addition, by setting the rising period of the pulse to, for example, 0.1 to several μs (microseconds), particularly about 0.2 to 2 μs, and applying a pulse of 0.2 to 10 μs, particularly about 0.5 to 1.5 μs, there is an advantage that a stable discharge at a low temperature can be obtained.
[0041] The discharge treatment can be carried out, for example, at room temperature, and does not require heating of the liquid, etc. Therefore, the catalyst application treatment liquid in this embodiment can be formed at low cost while suppressing energy consumption.
[0042] ≪3. Base material to be plated≫ In the plating method of the present embodiment, for example, a liquid containing palladium fine particles formed as described above is brought into contact with the surface of a substrate to be treated to provide a catalyst. The substrate to be plated is not particularly limited, and a substrate made of one or more materials selected from the group consisting of polymers, glass, ceramics, carbon materials, and metals can be used. Composite materials of polymers or ceramics and metals can also be plated in the present embodiment. Among these, a molded product of a thermoplastic polymer or a thermosetting polymer, or a composite material thereof, is particularly preferred.
[0043] (polymer molded body) The material of the polymer molded body to be plated in this embodiment is not particularly limited, and various resins and elastomers can be used. Examples include ABS (acrylonitrile-butadiene-styrene resin), PC (polycarbonate), PC-containing ABS, SBS (styrene-butadiene-styrene copolymer), ASA (acrylonitrile-styrene-acrylate copolymer), SAS (silicone-based composite rubber-acrylonitrile-styrene copolymer), acrylic resin, polyolefin resin such as polypropylene or polyethylene, polyphenylene oxide, polyphenylene sulfide, polyacetal, polyamide, polyimide, (aliphatic) polyester, polyethylene terephthalate, polybutylene terephthalate, polyvinyl acetate, polyurethane, polyether ketone, polysulfone, polyether ether sulfone, polyetherimide, liquid crystal polymer, epoxy resin, phenolic resin, fluororesin, Ajinomoto Build-up Film (trademark, ABF), etc., but are not limited thereto. Among them, the polymer molded body based on ABS resin is suitable as a substrate because it is easy to electrolessly plate.
[0044] The substrate may also be a composite of a polymer material and glass, ceramics, metal, carbon material, etc. For example, a composite of glass fiber or paper and epoxy resin or phenol resin, a composite of glass fiber and polyimide, a composite of glass fiber and fluororesin, a composite of glass fiber and polyphenylene oxide, a composite of glass fiber and bismaleimide / triazine / epoxy resin (BT resin), CFRP (carbon fiber reinforced plastic), CNF (cellulose nanofiber)-containing resin, etc. can be plated.
[0045] (other materials) In this embodiment, in addition to the above-mentioned polymer molded bodies, substrates based on fibrous polymer materials such as cellulose and synthetic resin fibers; substrates based on glasses such as E-glass, C-glass, and S-glass; substrates based on ceramics such as silicon, silicon carbide, silicon nitride, alumina, titania, and gallium nitride; substrates based on carbon materials such as carbon black, graphite, fullerene, carbon nanotubes, and carbon fibers; and even substrates based on metal materials such as aluminum and silver can be plated.
[0046] (Shape / Usage) The shape of the substrate is not particularly limited. For example, the substrate may have any shape and purpose, such as industrial materials such as sheets and pipes, automobile parts such as handles, grills, moldings, and emblems of various shapes, outboard motor parts, faucet fittings, building parts such as doorknobs and window frames, home appliance parts, electronic parts including various boards such as printed wiring boards, power devices (semiconductors), etc. Fiber structures made of carbon fibers, cellulose fibers, etc. may also be plated.
[0047] (substrate) The plating method of the present embodiment can produce good plated parts with a small amount of palladium without requiring post-treatment with strong acid or the like, and is therefore useful for plating various electronic components, particularly substrates for printed wiring boards and the like. There are no particular limitations on the substrate to be plated, and the substrate may be, for example, rigid substrates based on the above-mentioned epoxy resin, phenolic resin, polyimide, fluororesin, polyphenylene oxide, BT resin, etc., or composites of these resins with glass fiber or paper; flexible substrates based on polyimide films, polyethylene terephthalate films, etc.; and even metal substrates, glass substrates, and ceramic substrates. Substrates having through holes or via holes, or composite substrates may also be plated.
[0048] 4. Specific aspects of plating method In the plating method of this embodiment, as described above, a catalyst is applied by contacting a catalyst application treatment liquid containing palladium fine particles with the treated surface of a substrate, and then metal plating is performed on the treated surface to which the catalyst has been applied. In a preferred embodiment of this embodiment, the method further includes a step of surface-modifying the treated surface of the substrate to be plated prior to the catalyst application treatment. This surface modification step is not essential, but is useful for generating functional groups, such as hydrophilic functional groups such as hydroxyl groups and carboxyl groups, on the treated surface of the substrate, particularly the polymer molded body, and for applying more palladium fine particles as a catalyst.
[0049] (Surface modification process) There is no particular limitation on the surface modification method, and various known methods can be adopted depending on the object to be plated and the intended plated parts. Examples include (wet) etching using an etching solution such as an acidic solution or an alkaline solution, and dry etching using plasma or ultraviolet light (UV), but are not limited to these. In particular, a surface modification method using an etching solution is preferred.
[0050] <Particularly preferred embodiments> The plating method of this embodiment will be specifically described below by taking a particularly preferred embodiment as an example, based on the flow chart in Fig. 2. This embodiment includes an etching step - a conditioning step - a catalyst application step - an activation treatment step - an electroless plating step in this order, but the present invention is not limited to this embodiment.
[0051] (1) Etching process In this embodiment, the treated surface of the substrate to be plated is first etched prior to the catalyst application step. It is preferable to perform pretreatment (step S1-0) such as degreasing and cleaning on the treated surface prior to the etching step. There are no particular limitations on the methods of pretreatment and etching, and the treated surface of the substrate may be subjected to a degreasing method using a conventional caustic alkali or the like, water washing, etching using a general-purpose etching solution, or the like.
[0052] (Etching solution) There is no particular limitation on the type of processing liquid used in the etching process (step S1-1), and examples include chromic acid-based etching liquids such as chromic acid-sulfuric acid etching liquid, phosphoric acid-chromic acid-sulfuric acid etching liquid, etc.; dichromate-based etching liquids such as potassium dichromate-sulfuric acid etching liquid, potassium dichromate-phosphoric acid etching liquid, etc.; permanganate-based etching liquids such as sodium permanganate etching liquid, potassium permanganate etching liquid, phosphoric acid-perchloric acid-potassium permanganate etching liquid, potassium permanganate-phosphoric acid etching liquid, etc.; and further, ozone-containing etching liquid, sulfuric acid etching liquid, persulfuric acid etching liquid, hydrochloric acid etching liquid, and sulfuric acid-hydrochloric acid etching liquid, etc., but are not limited to these.
[0053] The property of the etching solution is not particularly limited, but it is preferable that the pH is acidic, about 0 to less than 7, for example, pH 2 or less, particularly 1.0 or less. More preferably, chromic acid-based, dichromate-based, permanganate-based, manganese salt-based, such as manganese sulfate, manganese nitrate, manganese carbonate, manganese chloride, manganese acetate, manganese dioxide, sodium manganate, potassium manganate, etc., persulfate-based, and / or ozone-based etching solutions are used. These etching solutions have the advantage of being excellent in roughening and surface modification of resins such as ABS. In particular, permanganate-based etching agents have the advantage that etching is easily carried out sufficiently and are unlikely to cause environmental pollution due to chromium and the like. This embodiment preferably further includes an etching step of contacting the treated surface of a substrate such as a polymer molded body with an acidic solution containing an oxidizing agent, more preferably an etching step of contacting the treated surface with an acidic solution containing permanganate ions, prior to the catalyst application step.
[0054] When the etching solution contains permanganate ions, the concentration is preferably 0.5 mmol / L or more, more preferably 5 mmol / L to 2.0 mol / L, and particularly preferably about 50 mmol / L to 0.5 mol / L. In addition, it is preferable that the etching solution contains at least one inorganic acid selected from the group consisting of phosphoric acid, sulfuric acid, and nitric acid, more preferably phosphoric acid or sulfuric acid, and particularly preferably sulfuric acid. The concentration of these inorganic acids in the etching solution is preferably, for example, 2 mol / L or more, and particularly preferably about 6 to 12 mol / L.
[0055] In the etching step (step S1-1), the temperature of the etching solution is set to, for example, 0 to 100°C, particularly about 25 to 70°C, and the substrate is immersed therein for, for example, 0.5 to 30 minutes, particularly about 1 to 15 minutes. The etching solution may be sprayed or otherwise brought into contact with the substrate surface to be treated. After the etching step, it is preferable to wash the substrate surface, particularly by washing with water (step S1-2). Depending on the conditions of the etching step, neutralization treatment, reduction treatment, or the like may be performed subsequently. In this embodiment, various surface modification treatments can be performed together with or instead of the etching treatment.
[0056] The etching treatment can be carried out in a plurality of steps. For example, the above-mentioned etching treatment can be repeated a plurality of times. In addition, the surface to be treated can be treated with an oxidizing agent-containing etching treatment liquid having a lower acidity than the above-mentioned, for example, a permanganate ion-containing liquid having a pH of about 3.0 to 10.0, particularly about 6.0 to 7.0, and then optionally washed with water, followed by post-treatment to activate the oxidizing agent. This post-treatment can be carried out by contacting the surface to be treated with a solution containing one or more activators selected from inorganic acids such as sulfuric acid, hydrochloric acid, nitric acid, phosphoric acid, and hydrofluoric acid; organic acids such as acetic acid and methanesulfonic acid; hydrogen peroxide; halogen oxoacids, potassium perchlorate, sodium periodate, and perbromic acid; and persulfates such as sodium peroxodisulfate and ammonium peroxodisulfate, at a concentration of 0.05 mol / L or more, and particularly about 0.5 to 17 mol / L, at a temperature of 0 to 100°C, and particularly 60 to 70°C, for 30 seconds or more, and particularly 1 to 5 minutes.
[0057] The above-mentioned etching solution and the solution of the activator used in the post-treatment may contain one or more pH buffers, such as phosphates, citrates, borates, carbonates, acetates, diethyl barbiturates, trishydroxymethylaminomethane, hydroxyethylpiperazineethanesulfonic acid, ethylenediaminetetraacetic acid, and the like; and / or one or more surfactants, such as amine salt type surfactants, quaternary amine salt type surfactants, amino acid type surfactants, betaine type surfactants, carboxylate type surfactants, sulfonate type surfactants, sulfate ester salt type surfactants, phosphate ester salt type surfactants, ether type surfactants, ester type surfactants, nitrogen-containing surfactants, fluorine-containing surfactants, and the like.
[0058] (Other surface modification treatments) In this embodiment, various surface modification treatments as described above may be performed together with or instead of the etching treatment. For example, the treated surface may be subjected to an alkali treatment or a concentrated sulfuric acid heat treatment. These treatments may carboxylate or sulfonate the treated surface, which may improve the adhesion to the palladium catalyst or the catalyst application efficiency. For the same reason, the treated surface may be subjected to a plasma treatment or dry etching by UV irradiation.
[0059] In particular, when the plating target is a polyimide, for example a polyimide substrate, the imide ring is hydrolyzed and opened to form a polyamic acid ion, and a carboxyl group is easily generated as a result of the alkali treatment. Therefore, it is possible to proceed to the catalyst application step immediately after the alkali treatment without carrying out the above-mentioned etching treatment or the conditioning treatment described below, and to more simply produce a good electroless plated part. Of course, the alkali treatment, concentrated sulfuric acid heating treatment, or dry etching treatment may be used in combination with the etching treatment and / or conditioning treatment.
[0060] (Alkaline treatment) There is no particular limitation on the method of alkali treatment, and any alkali solution capable of opening the imide ring constituting the polyimide can be used. Preferred examples include aqueous solutions of lithium hydroxide, sodium hydroxide, potassium hydroxide, etc., but are not limited thereto. The alkali treatment may be performed, for example, by immersing a substrate such as polyimide in an alkali solution having a concentration of about 0.01 to 10 mol / L at a temperature range of about 20 to 100°C for about 10 seconds to 50 minutes. The treatment surface of the substrate can also be treated by spraying the alkali solution, etc. Note that it is preferable to wash the treatment surface after the alkali treatment by washing with water, etc.
[0061] (2) Conditioning process In this embodiment, next, prior to the catalyst application step, a conditioning step (step S2-1) is performed in which the treated surface is brought into contact with a catalyst application enhancing liquid (also called a conditioner). This conditioning step is not essential, but is useful in further improving the quality of electroless plated parts. As described above, functional groups such as hydrophilic groups may be generated on the treated surface of a substrate such as a polymer molded body, particularly on the treated surface after the etching step. A treatment liquid containing a compound that is selectively adsorbable to these functional groups (hereinafter referred to as a "selectively adsorbable compound") is the catalyst application enhancing liquid.
[0062] (Selective Adsorption Compound) The selectively adsorbing compound contained in the catalyst-imparting enhancing liquid is not particularly limited as long as it is a compound having a functional group with selective adsorption as described above, but for example, a compound containing a nitrogen atom is preferable.Specific examples include ethylenediamine-based compounds such as ethylenetriamine and triethylenetetramine; ethyleneimine-based polymer compounds such as Epomin SP-003, Epomin SP-012, and Epomin SP-200 (all manufactured by Nippon Shokubai Co., Ltd.); allylamine-based polymer compounds such as PAA-03 and PAA-D41-HCl (all manufactured by Nitto Boseki Co., Ltd.); diallylamine-based polymer compounds such as PAS-92, PAS-M-1, and PAS-880 (all manufactured by Nitto Boseki Co., Ltd.); and vinylamine-based polymer compounds such as PVAM-0570-B (manufactured by Mitsubishi Chemical Co., Ltd.), but are not limited thereto.
[0063] In order to develop good plating characteristics, it is preferable to use a polyvalent amine compound as the selective adsorptive compound. That is, this embodiment includes a plating method further including a conditioning step of contacting the treated surface with a catalyst application enhancing liquid containing a polyvalent amine compound prior to the catalyst application step. More preferably, a compound containing three or more nitrogen atoms is used. More preferably, ethyleneimine-based polymer compounds, allylamine-based polymer compounds, and diallylamine-based polymer compounds are used, and among them, polyethyleneimine is suitable. The polyethyleneimine may be linear or branched. There is no particular restriction on the molecular weight, and for example, a molecular weight of 100 or more, of which 300 to 70,000, and particularly about 10,000 is preferable. There is no particular restriction on the amine value, and for example, a polyvalent amine compound with an amine value of about 15 to 25 mgKOH / g, particularly polyethyleneimine with an amine value of about 18 to 21 mgKOH / g, can be preferably used. If the plating surface is treated with a catalyst application enhancing liquid containing such a nitrogen compound, the plating characteristics can be further improved.
[0064] The concentration of the selective adsorptive compound in the catalyst-imparting enhancing liquid can be, for example, 10 mg / L or more, particularly about 100 to 3000 mg / L. The pH of the catalyst-imparting enhancing liquid is not particularly limited, and may be, for example, about 10 to 13. The pH can also be adjusted to, for example, 5 to 12, particularly about 8 to 10, using, for example, sodium hydroxide, sulfuric acid, or the like. To treat the surface of the substrate with the catalyst-imparting enhancing liquid, the liquid temperature is, for example, 0 to 70°C, particularly about 25 to 35°C, and the substrate is immersed therein for, for example, 1 to 20 minutes, particularly about 2 to 3 minutes. The catalyst-imparting enhancing liquid may be sprayed or the like to contact the surface of the substrate.
[0065] (Other additives) The catalyst imparting enhancing solution may contain additives such as the above-mentioned dispersants, for example, citric acid, and stannates, together with the selective adsorptive compound. The plating characteristics may be further improved by adding stannates, for example, potassium stannate. For example, even if the concentration of palladium in the catalyst imparting treatment solution is set to a low concentration of 10 mg / L or less, a plated part having an electroless plating layer applied to the entire surface of the treatment target can be produced.
[0066] (washing with water) When the conditioning treatment is performed in this embodiment, it is preferable to wash the treated surface of the substrate, particularly rinse with water, prior to the next catalyst application step. If palladium fine particles are bound to the selective adsorptive compound that is not bound to the substrate, such as a polymer molded body, there is a risk that they will no longer function as a catalyst for electroless plating, but this risk is reduced by washing with water. In addition, washing with water has the advantage of extending the life of the catalyst solution. In other words, this embodiment also includes a plating method that further includes a step of washing the treated surface with water (step S2-2) between the conditioning step and the catalyst application step.
[0067] (3) Catalyst application step In this embodiment, the surface to be treated of the substrate as described above is degreased, cleaned, etched, conditioned, and / or washed with water, and then the catalyst is applied by contacting the surface with a catalyst application treatment liquid. As the catalyst application treatment liquid, a liquid containing palladium fine particles formed by the above-mentioned in-liquid discharge between the electrodes is used. For example, the catalyst application treatment liquid may be separately prepared (step S3-1) and brought into contact with the surface to be treated as the catalyst application step (step S3-2).
[0068] The fine particles in the catalyst imparting treatment solution in this embodiment have a nanoscale size and high activity as described above. Therefore, they are easily adsorbed onto the substrate surface, and even if the amount of palladium adsorbed onto the substrate surface is less than that in a normal plating method, excellent plating properties are exhibited. For example, when a conventional palladium / tin colloid is used as the catalyst, at least 5 to 10 mg / m is required to electrolessly plate the entire surface to be treated. 2 Generally, a larger amount of palladium is required. In contrast, in this embodiment, the amount of palladium fine particles applied to the treatment surface of the substrate is, for example, 3 to 8 mg / m per unit area. 2 , especially 4.0 to 6.0 mg / m 2 Even with only a small amount of this, it is possible to obtain good electroless plated parts.
[0069] To apply a catalyst to the treated surface of the substrate, the temperature of the catalyst application treatment solution is set to, for example, 10 to 60°C, particularly 20 to 50°C, and the substrate such as a polymer molded product is immersed in the solution for 1 to 20 minutes, particularly 2 to 5 minutes. The catalyst application treatment solution may be sprayed or otherwise contacted with the treated surface of the substrate. After the catalyst application step, it is preferable to perform a washing operation, particularly washing with water (step S3-3).
[0070] As described above, the fine particles formed by discharging in a liquid do not require post-treatment such as activation with hydrochloric acid or reduction, which is usually performed after a catalyst application process. Therefore, according to this embodiment, electroless plating of a substrate can be easily performed with fewer steps than in a normal method, without spending time or money.
[0071] In addition, the palladium fine particles themselves do not require a reducing agent or the like, and can be formed only with a palladium electrode, a liquid, and an optional conductive agent and / or a dispersant. Therefore, even if the operation of preparing the catalyst-imparting treatment liquid and the operation of contacting the catalyst-imparting treatment liquid with the treated surface are performed simultaneously in the same device or reactor, for example, problems such as unexpected side reactions and a reduction in the amount of catalyst attached are unlikely to occur. In other words, it is also possible to simultaneously and in parallel prepare the catalyst-imparting treatment liquid and contact the treated surface with the catalyst-imparting treatment liquid, for example, as shown in FIG. 3. Therefore, the catalyst-imparting step in this embodiment can be carried out not only by a method in which a catalyst-imparting treatment liquid in which palladium fine particles are formed is prepared in advance and this is brought into contact with the treated surface that has been subjected to optional pretreatment, but also by a plating method having an operation of preparing a catalyst-imparting treatment liquid containing palladium fine particles by in-liquid discharge (step S3-1') and an operation of contacting the treated surface with the catalyst-imparting treatment liquid (step S3-2').
[0072] (4) Activation treatment process In this embodiment, the activation treatment using hydrochloric acid or the like is not necessary as described above, but it is not necessary to avoid it. For example, between the catalyst application step and the electroless plating step described below, an activation treatment step (step S4-1) of contacting the treated surface with a hypophosphorous acid solution or the like may be further included. The activation treatment makes it difficult for palladium to be mixed into the plating solution. In addition, in cases where the catalyst is deactivated due to a gap between the preparation of the catalyst application treatment solution or the catalyst application step and the electroless plating step, the catalyst can be reactivated by the activation treatment.
[0073] There is no particular limitation on the treatment solution used in the activation treatment step, and for example, the above-mentioned hypophosphorous acid solution, hypophosphite solution, reducing agent, and / or inorganic acid can be used. Examples include, but are not limited to, hypophosphorous acid, sodium hypophosphite, potassium hypophosphite; reducing agents such as dimethylamine borane (DMAB) and sodium borohydride (SBH); inorganic acids such as hydrochloric acid; and solutions containing them. It is also possible to use multiple types of hypophosphorous acid (salt), reducing agents, inorganic acids, etc. in combination. In particular, treatment with hypophosphorous acid (salt) is preferred. Hypophosphorous acid is not a strong acid like hydrochloric acid used in the catalyzer-accelerator method and the sensitizing-activating method, so there is little risk of adversely affecting peripheral devices, etc.
[0074] In the activation treatment step, for example, an aqueous solution containing sodium hypophosphite or potassium hypophosphite at 5 to 40 g / L, particularly about 10 to 25 g / L, can be used. For example, the pH is adjusted to about 7, and the liquid temperature is set to 0 to 70°C, particularly about 25 to 35°C, and the substrate to which the catalyst is applied may be immersed for a few seconds to a few minutes, for example, about 1 minute, in the treatment solution. The treatment surface of the substrate may be contacted with the treatment liquid by spraying, etc., after the activation treatment step is completed. It is preferable to wash the substrate or its treatment surface, particularly by washing with water (step S4-2).
[0075] (5) Electroless plating process The substrate to which the catalyst has been applied as described above is then subjected to metal plating on the surface to which the catalyst has been applied in the electroless plating step (step S5). There is no particular limitation on the electroless plating method, and the electroless plating can be performed according to a conventional method using, for example, a known electroless metal plating solution such as an electroless nickel plating solution, an electroless copper plating solution, or an electroless cobalt plating solution. Specifically, when electroless plating is performed using an electroless nickel plating solution, for example, a substrate such as a polymer molded body may be immersed in the electroless nickel plating solution at a pH of 8 to 10 and a temperature of 30 to 50° C. for about 5 to 15 minutes.
[0076] (6) Post-process The substrate that has been electrolessly plated as described above can be used as a plated part as is after optional rinsing and drying, or it may be subjected to a post-step (S6) such as electroplating. For example, strike plating such as copper strike plating, nickel strike plating, silver strike plating, and gold strike plating; general-purpose plating such as nickel plating, chrome plating, nickel chrome plating, tin plating, tin silver plating, copper plating, gold plating, and silver plating can be performed. There are no particular limitations on the method and conditions for these electroplating processes, and they can be performed using conventional methods and conditions.
[0077] An electrolytic chemical conversion coating film and / or an immersion chemical conversion coating film may be further applied onto the electroless plating layer or the electroplating layer. These treatment films can further increase the corrosion resistance of the plated parts. There are no particular limitations on the electrolytic chemical conversion coating and the immersion chemical conversion coating, and conventional treatment methods can be applied as desired. Examples include, but are not limited to, chromate treatment, wax treatment, treatment with a solution of benzotriazole or triazinethiol, treatment with a solution of a compound having an amino group or an imino group, anodization treatment, and heat treatment.
[0078] 5. Plated parts The plating method of the present embodiment as described above allows plated parts to be manufactured easily and at low cost. Plated parts manufactured in this manner are less likely to suffer from poor appearance such as blistering, have excellent adhesion between the plating layer and the substrate, and have high peel strength. Therefore, the plating method is suitable for various shapes and applications, such as industrial materials of various shapes, automobile parts, outboard motor parts, faucet fittings, building material parts, home appliance parts, electronic parts including various substrates such as printed wiring boards, power devices including silicon carbide (SiC) power devices, etc. The present invention also includes plated parts manufactured by the plating method. The present invention further includes electronic parts obtained by subjecting various substrates such as polyimide substrates to the plating method, such as bare substrates such as copper-clad laminates, printed substrates, printed wiring boards, printed circuit boards, single-sided substrates, double-sided substrates, multilayer substrates, etc. EXAMPLES
[0079] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these descriptions in any way.
[0080] Example 1 According to the present invention, plated parts were produced as follows. (Etching of plated objects) An ABS resin molded product (flat plate shape of 90 x 50 x 0.3 mm) was immersed in an aqueous solution of sodium permanganate (pH = 7) maintained at 68°C for 2 minutes. This treatment was repeated twice to etch the surface (treated surface). After etching, the product was washed with water.
[0081] (conditioning) After etching and rinsing, the resin molded product was immersed in the conditioner at room temperature for 5 minutes for conditioning, and then rinsed again to prepare the substrate for electroless plating. The conditioner used was an aqueous solution containing 10 g of polyethyleneimine (branched, 30% solution with mass average molecular weight of 70,000) in 1 L of ion-exchanged water.
[0082] (Preparation of catalyst imparting treatment solution) In parallel with the above, a catalyst-imparting treatment liquid was prepared. A pair of palladium electrodes (99.5% purity, rod-shaped with a diameter of 2 mm) was placed in a liquid in which trisodium citrate was dissolved in ion-exchanged water at a concentration of 300 mg / L as a conductive agent and dispersant, as shown in FIG. 1, and a discharge voltage of about 1000 V was applied between the two electrodes to perform submerged glow discharge for about 13 minutes. The average particle size of the palladium fine particles in the resulting dispersion liquid (catalyst-imparting treatment liquid-0) was measured by the cumulant method and found to be 248 nm. In addition, the palladium concentration in the catalyst-imparting treatment liquid-0 was analyzed by atomic absorption spectrometry and found to be 11.2 ppm. The same results were obtained by ICP emission measurement.
[0083] Next, the catalyst-imparting treatment liquid-0 was diluted with ion-exchanged water to prepare a dispersion liquid (catalyst-imparting treatment liquid-1) with a palladium concentration of 8 ppm and a trisodium citrate concentration of 2.4 mg / L. The average particle size of the palladium particles in the catalyst-imparting treatment liquid-1 was measured by the cumulant method to be 294.9 nm. The zeta potential of the catalyst-imparting treatment liquid-1 was measured to be -50.1 mV. The catalyst-imparting treatment liquid-1 had excellent dispersion stability, with no suspended matter or precipitates being observed.
[0084] (Addition of catalyst) The substrate prepared as described above was immersed in catalyst application treatment solution-1 maintained at 35°C for 5 minutes, and then washed with water and dried. A part of the dried sample was immersed in aqua regia and stirred in the immersion solution for 5 minutes, after which atomic absorption spectrometry was performed. The amount of palladium attached (adsorbed amount) per unit surface area of the substrate was 4.4 mg / m 2 It was.
[0085] (Electroless plating) The substrate after the catalyst application was immersed in NI-100 plating solution manufactured by JCU Corp. at a temperature of 35°C and pH 8.6 for 10 minutes to perform electroless nickel plating. In the obtained plated part, metallic nickel was deposited on the entire surface of the substrate.
[0086] Example 2 The same operation as in Example 1 was carried out, except that the catalyst imparting treatment solution-2 (palladium concentration 4 ppm, trisodium citrate concentration 1.2 mg / L, zeta potential -14.5 mV) obtained by diluting the catalyst imparting treatment solution-1 by twofold with ion-exchanged water was used as the catalyst imparting treatment solution. In the obtained plated part, metallic nickel was deposited on the entire surface of the substrate.
[0087] Comparative Example 1 A palladium colloidal solution obtained by a reduction method was used as the catalyst-imparting treatment solution. 0.8 mg of L-glutathione, 3.76 ml of PdCl2 / 5NaCl solution (concentration 20 mM), and 11.4 mg of NaBH4 were mixed per 1 L of ion-exchanged water to prepare catalyst-imparting treatment solution-C1 with a palladium concentration of 8 ppm. The same operation as in Example 1 was performed except that this catalyst-imparting treatment solution-C1 was used instead of catalyst-imparting treatment solution-1. In the obtained plated parts, there were some areas where metallic nickel was not deposited.
[0088] Comparative Example 2 Using catalyst imparting treatment solution-C2 (palladium concentration 4 ppm) obtained by diluting catalyst imparting treatment solution-C1 by twofold with ion-exchanged water, the same operations as in Example 1 and Comparative Example 1 were carried out. In the obtained plated parts, metallic nickel was deposited only on the edge of the sample.
[0089] Comparative Example 3 A catalyst-imparting treatment solution-C3 with a palladium concentration of 8 ppm was prepared by mixing 1.6 g of sucrose, 3.76 ml of PdCl2 / 5NaCl solution (concentration 20 mM), and 11.4 mg of NaBH4 per 1 L of ion-exchanged water. Using this catalyst-imparting treatment solution-C3, the same operations as in Example 1 and Comparative Example 1 were carried out. In the obtained plated part, a portion where metallic nickel was not deposited was observed in the center of the sample.
[0090] Comparative Example 4 A catalyst-imparting treatment solution-C4 with a palladium concentration of 8 ppm was prepared by mixing 34.3 mg of glycerin, 3.76 ml of PdCl2 / 5NaCl solution (concentration 20 mM), and 113.6 mg of sodium hypophosphite per 1 L of ion-exchanged water. Electroless plating was attempted using this catalyst-imparting treatment solution-C4 in the same manner as in Example 1 and Comparative Example 1, but metallic nickel was not deposited on the surface of the substrate sample.
[0091] The test results of Examples 1 and 2 and Comparative Examples 1 to 4, together with the type of catalyst imparting treatment solution, are summarized in the following Table 1. The evaluation results of plating deposition properties in Table 1 are based on the following criteria. ◎: Metallic nickel is deposited on the entire surface of the substrate sample. ○: Metallic nickel is deposited on 50% to almost the entire surface of the substrate sample. △: Metallic nickel deposition was observed, but non-deposited areas accounted for 50% or more of the total. ×: Metallic nickel is not deposited.
[0092] [Table 1]
[0093] It was found that good plating deposition properties were achieved by using a solution containing palladium fine particles formed by in-liquid discharge according to the present invention as the catalyst-imparting treatment solution. As described above, in the catalyst-imparting treatment solution using the reduction method, the palladium concentration is usually set to several tens of ppm or more. In fact, good test results were not obtained with the catalyst-imparting treatment solutions C1 to C3, which have palladium concentrations of 4 to 8 ppm. It was shown that the present invention can reduce the amount of expensive palladium catalyst used and perform electroless plating at a lower cost.
[0094] Example 3 The same operation as in Example 1 was carried out, except that an aqueous solution containing only 3 ml of polyethyleneimine in 1 L of ion-exchanged water was used as the conditioner. Metallic nickel was deposited on the entire surface of the substrate, and a plated part having a glossy appearance was obtained.
[0095] <Examples 4 to 6> The same operation as in Example 3 was carried out, except that the dispersant (conductivity imparting agent) was changed to one other than trisodium citrate (triNa citrate). The test results are shown in Table 2 together with the results of Example 3 and the type of dispersant. The evaluation criteria for plating deposition were the same as those in Table 1.
[0096] [Table 2]
[0097] It was found that when a liquid containing palladium fine particles formed by in-liquid discharge according to the present invention is used as a catalyst imparting treatment liquid, the plating deposition properties are generally good regardless of the type of conductivity imparting agent. It was also found that particularly excellent plating deposition properties are exhibited when a salt of a polyvalent carboxylic acid is used as a dispersing agent (conductivity imparting agent).
[0098] <Examples 7 to 14> The same operation as in Example 3 was carried out by changing the type and content of polyethyleneimine (PEI) in the conditioner. Note that the polyethyleneimine used here was a branched polymer. The test results are shown in Table 3.
[0099] [Table 3]
[0100] It has been found that when a liquid containing palladium microparticles formed by submerged discharge according to the present invention is used as a catalyst imparting treatment liquid, excellent plating deposition properties are exhibited regardless of the molecular weight and content of polyethyleneimine in the conditioner.
[0101] Example 15 The same operation as in Example 1 was carried out, except that the material of the substrate to be plated was changed from ABS resin to PC-containing ABS. Metallic nickel was precipitated over the entire surface of the obtained plated parts. It was revealed that the plating method of the present invention can produce good plated parts regardless of the material of the substrate. Thus, it was shown that the plating method of the present invention can easily produce good electroless plated parts without the need for the use of a high-concentration palladium catalyst imparting solution or post-treatment with a strong acid or the like.
[0102] Example 16 Using the catalyst imparting treatment solution-1, plating of a through-hole board was attempted. Through-holes of diameter (φ) 0.3 mm and 1.0 mm were formed in a glass epoxy copper-clad laminate (R-1705 FR-4 manufactured by Panasonic Corporation, thickness 1.6 mm) to prepare a through-hole board. This through-hole board was subjected to a swelling treatment at 70°C for 7 minutes using the DS-SW12A process (manufactured by JCU Corporation), a desmear treatment (treatment to remove resin residues during hole drilling) at 70°C for 10 minutes using the DS-250NA process (manufactured by JCU Corporation), and a neutralization treatment at 25°C for 5 minutes using the DS-RD31 process (manufactured by JCU Corporation) in that order, and then washed with water.
[0103] The through-hole substrate after washing with water was subjected to the same conditioning treatment and catalyst application treatment as in Example 3 (however, the catalyst was applied at room temperature). Next, the substrate was immersed at 32°C for 15 minutes using a PB-507F process (manufactured by JCU Corporation) to perform electroless copper plating. A backlight test was performed on the through-hole substrate after copper plating to evaluate the plating state.
[0104] (Backlight test) The through-hole was polished until the center thereof was exposed, and a light was shone on it from below. The degree of light blocking was evaluated according to the following criteria. Rating No.0: The through-hole is not covered with copper plating at all. Rating No. 10: The through-hole is completely covered with copper plating and is shielded from light. (Ratings 1 to 9 are intermediate between the above.)
[0105] The results of the backlight test are shown in Figure 4. The light was completely blocked in both the φ=0.3mm and φ=1.0mm through-holes, and the test result was rated No. 10. In other words, the inside of the through-hole was completely covered. Thus, it has become clear that the plating method according to the present invention is also useful in the manufacture of electronic components. [Explanation of symbols]
[0106] 1 Discharge device 10 electrodes 12 Insulation 20 liquid 30 containers 40 Power supply section
Claims
1. A plating method including at least a catalyst imparting step of contacting a catalyst imparting treatment solution with a treated surface of a substrate to impart a catalyst, and an electroless plating step of performing metal plating on the treated surface to which the catalyst has been imparted, In the catalyst application step, a liquid containing palladium fine particles formed by discharging between a palladium electrode and a counter electrode disposed in the liquid is used as the catalyst application treatment liquid. Plating method.
2. The catalyst application step includes: preparing the catalyst imparting treatment liquid containing the palladium fine particles by discharging between the palladium electrode and the counter electrode disposed in the liquid; an operation of contacting the catalyst application treatment liquid with the surface to be treated; The plating method of claim 1 , comprising:
3. 3. The plating method according to claim 1, wherein the average zeta potential of the fine palladium particles in the catalyst imparting treatment solution is 0 mV or less.
4. 3. The plating method according to claim 1, wherein the catalyst application treatment solution contains a polyvalent carboxylic acid and / or a salt thereof.
5. 3. The plating method according to claim 1, wherein the substrate is made of at least one material selected from the group consisting of polymers, glass, ceramics, carbon materials, and metals.
6. The plating method according to claim 1 or 2, wherein the base material is a substrate.
7. 3. The plating method according to claim 1, further comprising a conditioning step of contacting the surface to be treated with a catalyst application enhancing liquid containing a polyamine compound prior to the catalyst application step.
8. 8. The plating method according to claim 7, further comprising a step of rinsing the treatment surface with water between the conditioning step and the catalyst application step.
9. 3. The plating method according to claim 1, further comprising an activation treatment step between the catalyst application step and the electroless plating step, in which the treatment surface is brought into contact with a hypophosphorous acid solution, a reducing agent, and / or an inorganic acid.
10. 3. The plating method according to claim 1, further comprising a step of modifying the surface to be treated prior to the catalyst application step.
11. 3. The plating method according to claim 1, further comprising, prior to the catalyst application step, an etching step of contacting the treatment surface with an acidic solution containing an oxidizing agent.
12. A plated part produced by the plating method according to claim 1 or 2.
Citation Information
Patent Citations
Electroless plating method and sensitizing solution therefor
JP2007063646A
Resin / copper plating laminate and method of manufacturing the same
JP2013184425A
Catalyst solution for electroless plating
JP2015086429A
Plating part manufacturing method
JP2016029209A
Metallization method for plastic surface
JP4275157B2