Manufacturing method for light-emitting element and light-emitting element

The use of a conductive carbon film with a Schottky barrier structure addresses metal migration in light-emitting elements, improving reliability and efficiency by minimizing electrode migration and maintaining electrical connections.

JP2024132470APending Publication Date: 2024-10-01NICHIA CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023043240
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-17
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The migration of metal contained in electrodes during the manufacturing process of light-emitting elements leads to reliability issues in existing technologies.

Method used

A method involving the formation of a conductive carbon film with a Schottky barrier structure between semiconductor layers, using a hybrid orbital carbon film to reduce potential differences and minimize metal migration, combined with a mask etching process to form electrodes.

Benefits of technology

Improves the reliability of light-emitting devices by reducing metal migration and maintaining electrical integrity, enhancing manufacturing efficiency and light output.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024132470000001_ABST
    Figure 2024132470000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing method for a light-emitting element whose reliability can be improved, and the light-emitting element.SOLUTION: A manufacturing method for a light-emitting element includes steps of: preparing a semiconductor structure including a first exposed part where an n-side semiconductor layer is exposed from a p-side semiconductor layer and an active layer; forming a carbon film with conductivity continuing to an upper surface of the first exposed part of the n-side semiconductor layer and an upper surface of the p-side semiconductor layer; removing at least a part of the carbon film existing on the upper surface of the p-side semiconductor layer to form a second exposed part that is exposed from the carbon film on the upper surface of the p-side semiconductor layer; forming a first mask that is formed on the carbon film and has an opening on the second exposed part; and forming a first electrode in the second exposed part. The step of forming the first electrode includes steps of: forming a first conductive member on the first mask and in the second exposed part; and removing the conductive member on the first mask by removing the first mask through wet etching, and leaving the first conductive member in the second exposed part.SELECTED DRAWING: Figure 6
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for manufacturing a light-emitting device and a light-emitting device. [Background technology]

[0002] Patent Document 1 discloses that Ag migration is suppressed by blocking the Ag-containing first metal layer from the Ag-free second metal layer with a protective film, except for a part of the region. When forming an electrode in a manufacturing method for a light-emitting element, migration of the metal contained in the electrode can become a problem. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2003-168823 A Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the embodiments of the present disclosure is to provide a method for manufacturing a light-emitting device and a light-emitting device that can improve reliability. [Means for solving the problem]

[0005] According to an aspect of the present disclosure, a method for manufacturing a light-emitting element includes the steps of: preparing a semiconductor structure having an n-side semiconductor layer, a p-side semiconductor layer, and an active layer located between the n-side semiconductor layer and the p-side semiconductor layer, the n-side semiconductor layer having a first exposed portion exposed from the p-side semiconductor layer and the active layer; forming a conductive carbon film continuous with an upper surface of the first exposed portion of the n-side semiconductor layer and an upper surface of the p-side semiconductor layer; removing at least a part of the carbon film located on the upper surface of the p-side semiconductor layer to form a second exposed portion exposed from the carbon film on the upper surface of the p-side semiconductor layer; forming a first mask formed on the carbon film and having an opening on the second exposed portion; and forming a first electrode on the second exposed portion, wherein the step of forming the first electrode includes the steps of forming a first conductive member on the first mask and on the second exposed portion; and removing the first mask by wet etching to remove the first conductive member on the first mask and leave the first conductive member on the second exposed portion. According to one aspect of the present disclosure, a light-emitting device includes a semiconductor structure having an n-side semiconductor layer, a p-side semiconductor layer, and an active layer located between the n-side semiconductor layer and the p-side semiconductor layer, a first electrode disposed on an upper surface of the p-side semiconductor layer, a first portion that contacts the first electrode on the upper surface of the p-side semiconductor layer, and a second portion that is continuous with the first portion and contacts a side surface of the n-side semiconductor layer, 2 Hybrid orbitals of carbon and sp 3 and a carbon film including a hybrid orbital carbon, the carbon film having a Schottky barrier structure between the first portion and the second portion. Effect of the Invention

[0006] According to an embodiment of the present disclosure, it is possible to provide a method for manufacturing a light-emitting element and a light-emitting element capable of improving reliability. [Brief description of the drawings]

[0007] [Figure 1] FIG. 2 is a schematic plan view illustrating a step of the method for manufacturing the light-emitting element according to the first embodiment. [Diagram 2] 3 is a schematic cross-sectional view illustrating a step of the method for manufacturing the light-emitting element according to the first embodiment. FIG. [Diagram 3] 3 is a schematic cross-sectional view illustrating a step of the method for manufacturing the light-emitting element according to the first embodiment. FIG. [Figure 4] 3 is a schematic cross-sectional view illustrating a step of the method for manufacturing the light-emitting element according to the first embodiment. FIG. [Diagram 5] 3 is a schematic cross-sectional view illustrating a step of the method for manufacturing the light-emitting element according to the first embodiment. FIG. [Figure 6] 3 is a schematic cross-sectional view illustrating a step of the method for manufacturing the light-emitting element according to the first embodiment. FIG. [Figure 7] 3 is a schematic cross-sectional view illustrating a step of the method for manufacturing the light-emitting element according to the first embodiment. FIG. [Figure 8] 3 is a schematic cross-sectional view illustrating a step of the method for manufacturing the light-emitting element according to the first embodiment. FIG. [Figure 9] 3 is a schematic cross-sectional view illustrating a step of the method for manufacturing the light-emitting element according to the first embodiment. FIG. [Figure 10] 3 is a schematic cross-sectional view illustrating a step of the method for manufacturing the light-emitting element according to the first embodiment. FIG. [Figure 11] 3 is a schematic cross-sectional view illustrating a step of the method for manufacturing the light-emitting element according to the first embodiment. FIG. [Figure 12] 1 is a schematic cross-sectional view of a light-emitting element according to a first embodiment. [Figure 13] FIG. 1 is a schematic plan view of a light-emitting element according to a first embodiment. [Figure 14] 11 is a schematic plan view illustrating a step of a method for manufacturing a light-emitting element according to a second embodiment. FIG. [Figure 15] 10 is a schematic cross-sectional view illustrating a step of a method for manufacturing a light-emitting element according to a second embodiment. FIG. [Figure 16] 10 is a schematic cross-sectional view illustrating a step of a method for manufacturing a light-emitting element according to a second embodiment. FIG. [Figure 17]10 is a schematic cross-sectional view illustrating a step of a method for manufacturing a light-emitting element according to a second embodiment. FIG. [Figure 18] 10 is a schematic cross-sectional view illustrating a step of a method for manufacturing a light-emitting element according to a second embodiment. FIG. [Figure 19] FIG. 5 is a schematic cross-sectional view of a light-emitting device according to a second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Hereinafter, the embodiments will be described with reference to the drawings. The dimensions, materials, shapes, relative arrangements, etc. of the components described in the embodiments are not intended to be limited thereto, and are merely illustrative examples, unless otherwise specified. The sizes and positional relationships of the components shown in each drawing may be exaggerated to clarify the explanation. In the following explanation, the same names and symbols indicate the same or similar components, and detailed explanations will be omitted as appropriate. In addition, as a cross-sectional view, an end view showing only a cut surface may be shown.

[0009] In the following description, terms indicating a specific direction or position (e.g., "upper", "lower", and other terms including these terms) may be used. However, these terms are merely used for the purpose of making the relative direction or position in the referenced drawings easier to understand. As long as the relationship of the relative direction or position by terms such as "upper" and "lower" in the referenced drawings is the same, the arrangement in drawings other than the present disclosure, in actual products, etc., may not be the same as that in the referenced drawings. In this specification, the positional relationship expressed as "upper (or lower)" includes, for example, when two members are assumed to exist, a case in which the two members are in contact with each other, and a case in which the two members are not in contact with each other and one member is located above (or below) the other member. In addition, unless otherwise specified, a member covering a covered object includes a case in which the member is in contact with the covered object and directly covers the covered object, and a case in which the member indirectly covers the covered object without contacting the covered object.

[0010] [First embodiment] A method for manufacturing a light-emitting device and the light-emitting device according to the first embodiment will be described with reference to FIGS.

[0011] The method for manufacturing the light-emitting device according to the first embodiment includes the steps of preparing a semiconductor structure 10, forming a carbon film 20, forming a second exposed portion 13b, arranging a first mask 80, and forming a first electrode 31. Each step will be described in detail below.

[0012] First, a step of preparing a semiconductor structure 10 is performed. Fig. 1 is a schematic plan view of the semiconductor structure 10 to be prepared. Fig. 2 is a schematic cross-sectional view taken along line II-II in Fig. 1.

[0013] The semiconductor structure 10 is made of a nitride semiconductor. In this specification, the term "nitride semiconductor" refers to, for example, In x Al y Ga 1-x-y It includes all semiconductors with compositions in which the composition ratios x and y are changed within the respective ranges in the chemical formula N (0≦x≦1, 0≦y≦1, x+y≦1). In addition, in the above chemical formula, those that further contain Group V elements other than N (nitrogen) and those that further contain various elements added to control various physical properties such as the conductivity type are also included in the "nitride semiconductor".

[0014] As shown in Fig. 2, the semiconductor structure 10 has an n-side semiconductor layer 11, a p-side semiconductor layer 13, and an active layer 12 located between the n-side semiconductor layer 11 and the p-side semiconductor layer 13. The active layer 12 is a light-emitting layer that emits light, and has, for example, an MQW (Multiple Quantum Well) structure including a plurality of barrier layers and a plurality of well layers. The active layer 12 emits light having, for example, an emission peak wavelength of 210 nm or more and 580 nm or less. The n-side semiconductor layer 11 has a semiconductor layer including an n-type impurity. The p-side semiconductor layer 13 has a semiconductor layer including a p-type impurity.

[0015] The n-side semiconductor layer 11 has a first exposed portion 11a exposed from the p-side semiconductor layer 13 and the active layer 12. The first exposed portion 11a has an upper surface 11a1. The first exposed portion 11a may also have a side surface 11a2. The side surface 11a2 is located between the upper surface 11a1 and an upper surface 13a of the p-side semiconductor layer 13, and is continuous with the side surface of the active layer 12 and the side surface of the p-side semiconductor layer 13.

[0016] As shown in FIG. 1, in a plan view, the semiconductor structure 10 has a quadrangular outer edge having four corners (a first corner C1, a second corner C2, a third corner C3, and a fourth corner C4). In a plan view, the first corner C1 and the fourth corner C4 are diagonally positioned, and the second corner C2 and the third corner C3 are diagonally positioned. The upper surface 11a1 and the side surface 11a2 of the first exposed portion 11a are disposed along the outer edges of the p-side semiconductor layer 13 and the active layer 12. Of the upper surfaces 11a1 of the first exposed portion 11a, for example, the upper surface 11a1 located near the first corner C1 extends from the first corner C1 toward the center of the semiconductor structure 10 in a plan view, and has a larger area than the other upper surfaces 11a1 located near the second corner C2 to the fourth corner C4.

[0017] As shown in FIG. 2, the semiconductor structure 10 may be supported on a substrate 100. The semiconductor structure 10 may be formed, for example, by forming an n-side semiconductor layer 11, an active layer 12, and a p-side semiconductor layer 13 in this order on the substrate 100. The semiconductor structure 10 may be formed, for example, by MOCVD (metal organic chemical vapor deposition). For example, a sapphire substrate may be used as the substrate 100. The substrate 100 may be peeled off from the semiconductor structure 10.

[0018] Next, as shown in FIG. 3, a step of forming a carbon film 20 is performed.

[0019] The carbon film 20 is formed continuously on the upper surface 11a1 of the first exposed portion 11a of the n-side semiconductor layer 11 and the upper surface 13a of the p-side semiconductor layer 13. The carbon film 20 contacts the upper surface 11a1 of the first exposed portion 11a of the n-side semiconductor layer 11 and the upper surface 13a of the p-side semiconductor layer 13. The carbon film 20 is conductive and electrically connected to the n-side semiconductor layer 11 and the p-side semiconductor layer 13. Therefore, the n-side semiconductor layer 11 and the p-side semiconductor layer 13 are short-circuited through the carbon film 20.

[0020] The carbon film 20 continuously covers the upper surface 11a1 of the first exposed portion 11a of the n-side semiconductor layer 11, the side surface of the active layer 12, the side surface of the p-side semiconductor layer 13, and the upper surface 13a of the p-side semiconductor layer 13. As shown in FIG. 3, when the first exposed portion 11a has a side surface 11a2, the carbon film 20 continuously covers the upper surface 11a1 of the first exposed portion 11a, the side surface 11a2 of the first exposed portion 11a, the side surface of the active layer 12, the side surface of the p-side semiconductor layer 13, and the upper surface 13a of the p-side semiconductor layer 13.

[0021] The carbon film 20 has an amorphous structure. For example, the carbon film 20 is made of sp 2 Hybrid orbitals of carbon and sp 3 The carbon film 20 is a so-called DLC (Diamond Like Carbon) film containing carbon with a hybrid orbital. The carbon film 20 is formed by controlling the bias voltage applied to the semiconductor structure 10 side. 2 Ratio of carbons in hybrid orbitals and / or sp 3 The ratio of carbons in hybrid orbitals can be controlled.

[0022] The carbon film 20 can be formed by, for example, a filtered cathodic vacuum arc (FCVA) method or a chemical vapor deposition (CVD) method. The FCVA method is a deposition method that uses carbon ions generated by arc discharge without introducing gas into a vacuum discharge space. For example, 5×10 -5 Torr or less, preferably 2×10 -5An arc discharge is generated on a carbon material (e.g., a graphite ingot) placed in a vacuum of Torr or less to generate plasma containing positively ionized carbon. The carbon ions are guided in the vacuum chamber toward the semiconductor structure 10 to which a negative bias voltage is applied, and collide with the semiconductor structure 10 to form a carbon film 20.

[0023] Next, at least a part of the carbon film 20 located on the upper surface 13a of the p-side semiconductor layer 13 is removed, and as shown in FIG. 5, a process is performed to form a second exposed portion 13b exposed from the carbon film 20 on the upper surface 13a of the p-side semiconductor layer 13. As shown in FIG. 4, the second exposed portion 13b of the p-side semiconductor layer 13 can be formed by forming a mask having an opening at a position where the second exposed portion 13b is to be formed on the carbon film 20, and removing the carbon film 20 located at the opening of the mask. The carbon film 20 can be removed by an ashing method using oxygen plasma, for example. The mask used in the process of forming the second exposed portion 13b may be removed or may be used as a first mask 80 described later. In the example shown in FIG. 4 to FIG. 6, the same first mask 80 is used from the process of forming the second exposed portion 13b to the process of forming the first electrode 31 described later.

[0024] Next, a step of forming a first mask 80 that is formed on the carbon film 20 and has an opening above the second exposed portion 13b is performed. As shown in FIG. 5, the first mask 80 having a first opening 81 is formed on the carbon film 20.

[0025] The material of the first mask 80 may be, for example, a resist film mainly containing an acrylic resin or a novolac resin. The resist film is, for example, a negative resist film in which an exposed portion dissolves in a developer. The first mask 80 is formed by forming a resist film on the entire surface of the carbon film 20, and by exposing and developing the resist film, the first opening 81 shown in FIG. 4 can be formed.

[0026] The first mask 80 has an inner surface 80a that defines a side surface of the first opening 81. As shown in Fig. 5, the inner surface 80a is inclined from the upper surface of the first mask 80 toward the carbon film 20. The angle formed between the upper surface of the first mask 80 and the inner surface 80a is an acute angle.

[0027] Next, as shown in FIG. 6, a step of forming a first electrode 31 on the second exposed portion 13b using a first mask 80 is performed.

[0028] By using the first mask 80 to form the second exposed portion 13b and the first electrode 31, the steps of forming a mask for forming the second exposed portion 13b and a mask for forming the first electrode 31 are not necessary, and the number of steps can be reduced.

[0029] The step of forming the first electrode 31 includes a step of forming the first conductive member 30 on the first mask 80 and the second exposed portion 13b, as shown in FIG. 6. The first conductive member 30 is formed in the second exposed portion 13b located in the first opening 81. The first conductive member 30 contacts the upper surface 13a of the p-side semiconductor layer 13 located in the first opening 81. The end of the first conductive member 30 formed on the upper surface 13a of the p-side semiconductor layer 13 may or may not contact the end of the carbon film 20. In addition, when the first conductive member 30 is formed by a sputtering method, the first conductive member 30 is unlikely to be formed on the inner side surface 80a of the first mask 80 having the above-mentioned inclination, and at least a part of the inner side surface 80a is exposed from the first conductive member 30.

[0030] Metals such as silver and aluminum can be used as the material of the first conductive member 30. The first conductive member 30 can be formed by, for example, a sputtering method.

[0031] The step of forming the first electrode 31 includes a step of forming the first conductive member 30, and then removing the first mask 80 by wet etching to remove the first conductive member 30 on the first mask 80 and leave the first conductive member 30 in the second exposed portion 13b. As shown in Fig. 7, the first conductive member 30 left in the second exposed portion 13b becomes the first electrode 31 electrically connected to the p-side semiconductor layer 13. A current supplied from the outside to the light-emitting element is diffused in the planar direction of the upper surface 13a of the p-side semiconductor layer 13 through the first electrode 31.

[0032] When the first mask 80 is removed by wet etching, the etching liquid comes into contact with the inner surface 80a exposed from the first conductive member 30, and dissolution of the first mask 80 proceeds from the inner surface 80a. As the first mask 80 is dissolved by the etching liquid and removed from the carbon film 20, the first conductive member 30 on the first mask 80 is also removed together with the first mask 80.

[0033] As an etching solution for dissolving the first mask 80 made of resist, for example, N-methyl-2-pyrrolidone can be used.

[0034] When the first mask 80 is removed by wet etching, the metal contained in the first electrode 31 is ionized in the etching solution, and migration of the metal due to the potential difference between the p-side semiconductor layer 13 and the n-side semiconductor layer 11 tends to occur. In this embodiment, the first mask 80 is removed by wet etching in a state in which the p-side semiconductor layer 13 and the n-side semiconductor layer 11 are short-circuited through the conductive carbon film 20. Therefore, the potential difference between the p-side semiconductor layer 13 and the n-side semiconductor layer 11 is reduced, and migration of the metal contained in the first electrode 31 is unlikely to occur. This makes it difficult for the metal to deposit in unintended areas, and improves the reliability of the light-emitting device.

[0035] When the first mask 80 is removed by wet etching, the etching rate of the carbon film 20 is preferably lower than the etching rate of the first mask 80. This makes it possible to make the carbon film 20 less susceptible to etching when the first mask 80 is removed by wet etching, making it easier to maintain the state in which the p-side semiconductor layer 13 and the n-side semiconductor layer 11 are short-circuited through the carbon film 20.

[0036] The carbon film 20 is easier to remove than a transparent conductive film such as, for example, ITO (Indium Tin Oxide), IZO (Indium Zinc Oxide), etc. By using the carbon film 20 as a conductive film that shorts the p-side semiconductor layer 13 and the n-side semiconductor layer 11, the carbon film 20 can be easily removed by an ashing method using oxygen plasma in the step of forming the second exposed portion 13b.

[0037] When the first mask 80 used in the step of forming the second exposed portion 13b is also used in the step of forming the first electrode 31, the first mask 80 is prevented from being removed when the carbon film 20 is removed in the step of forming the second exposed portion 13b. For example, in an ashing method using oxygen plasma, the etching rate of the first mask 80 made of resist is made higher than the etching rate of the carbon film 20, so that the first mask 80 is less likely to be removed. In the step of forming the first mask 80, the thickness of the first mask 80 is formed to be thicker than the thickness of the carbon film 20. The thickness of the first mask 80 is preferably 10 times or more the thickness of the carbon film 20. The thickness of the first mask 80 can be, for example, 1 μm or more.

[0038] The carbon film 20 is sp 3 The ratio of carbons in the hybrid orbitals is sp 2 If the ratio of carbon to hybrid orbitals is higher, sp 3 The ratio of carbons in the hybrid orbitals is sp 2In comparison with the case where the ratio of carbon in the hybrid orbital is lower than that of graphite, the carbon film 20 exhibits the properties of diamond more strongly than graphite, and has a higher hardness. Since a carbon film 20 with a low hardness is easier to remove than a carbon film 20 with a high hardness, in the process of forming the carbon film 20, the sp 3 It is preferable to form the carbon film 20 so that the ratio of the hybrid orbital carbon is 70% or less. 3 Hybrid orbital carbon ratio and sp 2 The ratio of carbon in a hybrid orbital can be measured, for example, by micro-Raman spectroscopy.

[0039] In the step of forming the carbon film 20, it is preferable to form the carbon film 20 to a thickness of 15 nm or more and 10 μm or less, so that the time required to remove the carbon film 20 can be reduced.

[0040] In the carbon film 20, sp 3 The ratio of carbons in the hybrid orbitals is sp 2 If the ratio of carbon to hybrid orbitals is higher, sp 3 The ratio of carbons in the hybrid orbitals is sp 2 The electrical resistivity is higher than when the ratio of carbon in the hybrid orbital is lower than that of the carbon in the hybrid orbital. 3 It is preferable to form the ratio of carbon in the hybrid orbital to 10% or more and 50% or less. By increasing the thickness of the carbon film 20, the electrical resistivity of the carbon film 20 can be reduced. However, the thick carbon film 20 requires a longer time to remove. Therefore, the sp 3 When the ratio of carbon in the hybrid orbital is set to 10% or more and 50% or less, the thickness of the carbon film 20 is preferably formed to 100 nm or more and 1 μm or less, which can reduce the time required to remove the carbon film 20 while ensuring the electrical conductivity of the carbon film 20, thereby improving the manufacturing efficiency.

[0041] The method for manufacturing the light-emitting element according to the first embodiment may further include a step of forming a third exposed portion 11b exposed from the carbon film 20 on the upper surface 11a1 of the first exposed portion 11a as shown in FIG. 9 after forming the first electrode 31, and a step of forming a second electrode 41 on the third exposed portion 11b as shown in FIG. 10. The second electrode 41 functions as an external connection terminal on the cathode side of the light-emitting element. In addition, the method for manufacturing the light-emitting element according to the first embodiment may further include a step of forming a third electrode 42 after forming the first electrode 31. The third electrode 42 functions as an external connection terminal on the anode side of the light-emitting element. The second electrode 41 and the third electrode 42 may be formed simultaneously.

[0042] 8, the step of forming the third exposed portion 11b can be performed by using a second mask 90 formed on the carbon film 20 and the first electrode 31. The second mask 90 has a second opening 91 on the upper surface 11a1 of the first exposed portion 11a of the n-side semiconductor layer 11.

[0043] For example, a resist film is formed so as to cover the carbon film 20 and the first electrode 31, and then the resist film is subjected to an exposure process and a development process, thereby forming a second opening 91 in the second mask 90. ​​In the second opening 91, at least a part of the carbon film 20 located on the upper surface 11a1 of the first exposed portion 11a is exposed from the second mask 90.

[0044] Moreover, the second mask 90 can have a third opening 92 above the first electrode 31. In the third opening 92, at least a part of the first electrode 31 is exposed from the second mask 90. ​​The third opening 92 can be formed in the same process as the second opening 91.

[0045] 10, the second electrode 41 can be formed using a second mask 90. ​​By using the same second mask 90 in the step of forming the third exposed portion 11b and the step of forming the second electrode 41, the steps of forming a mask for forming the third exposed portion 11b and a mask for forming the second electrode 41 are not necessary, and the number of steps can be reduced.

[0046] The second mask 90 may be made of the same material as the first mask 80 described above.

[0047] The second mask 90 has an inner side surface 90a that defines a side surface of the second opening 91, and an inner side surface 90b that defines a side surface of the third opening 92. As shown in Fig. 8, the inner side surface 90a is inclined from the upper surface of the second mask 90a toward the carbon film 20. The inner side surface 90b is inclined from the upper surface of the second mask 90a toward the first electrode 31. The angle between the upper surface of the second mask 90a and the inner side surface 90a and the angle between the upper surface of the second mask 90a and the inner side surface 90b are acute angles.

[0048] In the step of forming the third exposed portion 11b, the third exposed portion 11b is formed by removing the carbon film 20 exposed from the second mask 90 in the second opening 91. As shown in Fig. 9, the third exposed portion 11b is a portion of the upper surface 11a1 of the first exposed portion 11a of the n-side semiconductor layer 11 that is exposed from the carbon film 20.

[0049] 10, the step of forming the second electrode 41 includes a step of forming the second conductive member 40 on the second mask 90 and in the third exposed portion 11b. In the third exposed portion 11b, the second conductive member 40 contacts the n-side semiconductor layer 11. The second conductive member 40 can be formed on the first electrode 41 exposed from the second mask 90 in the third opening 92.

[0050] The second conductive member 40 may be made of a metal such as titanium. The second conductive member 40 may be formed by, for example, a sputtering method. When the second conductive member 40 is formed by a sputtering method, the second conductive member 40 is unlikely to be formed on the inner side surface 90a and the inner side surface 90b having the above-described inclination of the second mask 90, and at least a part of the inner side surface 90a and at least a part of the inner side surface 90b are exposed from the second conductive member 40.

[0051] After the second conductive member 40 is formed, the second mask 90 is removed by wet etching, thereby removing the second conductive member 40 on the second mask 90 and leaving the second conductive member 40 in the third exposed portion 11b. Also, the second conductive member 40 is left on the first electrode 41. As shown in FIG. 11 , after the second mask 90 is removed, the second conductive member 40 left in the third exposed portion 11b becomes the second electrode 41 electrically connected to the n-side semiconductor layer 11. The second conductive member 40 left on the first electrode 31 becomes the third electrode 42 electrically connected to the first electrode 31.

[0052] When the second mask 90 is removed by wet etching, the etching liquid comes into contact with the inner side surfaces 90a and 90b exposed from the second conductive member 40, and dissolution proceeds from the inner side surfaces 90a and 90b. As the second mask 90 is removed by dissolution, the second conductive member 40 on the second mask 90 is also removed together with the second mask 90. ​​The same etching liquid as the etching liquid that dissolves the first mask 80 can be used as the etching liquid that dissolves the second mask 90.

[0053] When the second mask 90 is removed by wet etching, the metals contained in the first electrode 31, the second electrode 41, and the third electrode 42 are ionized in the etching solution, and migration of the metals due to the potential difference between the p-side semiconductor layer 13 and the n-side semiconductor layer 11 tends to occur. In this embodiment, when the second mask 90 is removed by wet etching, the second mask 90 is removed by wet etching in a state in which the p-side semiconductor layer 13 and the n-side semiconductor layer 11 are short-circuited through the conductive carbon film 20. Therefore, the potential difference between the p-side semiconductor layer 13 and the n-side semiconductor layer 11 is reduced, and migration of the metals contained in the first electrode 31, the second electrode 41, and the third electrode 42 is less likely to occur.

[0054] When the second mask 90 is removed by wet etching, the etching rate of the carbon film 20 is preferably lower than the etching rate of the second mask 90. ​​This makes it possible to make the carbon film 20 less susceptible to etching when the second mask 90 is removed by wet etching, making it easier to maintain the state in which the p-side semiconductor layer 13 and the n-side semiconductor layer 11 are short-circuited through the carbon film 20.

[0055] When the second mask 90 used in the step of forming the third exposed portion 11b is also used in the step of forming the second electrode 41 and the third electrode 42, the second mask 90 is prevented from being removed when the carbon film 20 is removed in the step of forming the third exposed portion 11b. For example, in an ashing method using oxygen plasma, the etching rate of the second mask 90 made of resist is made higher than the etching rate of the carbon film 20, so that the second mask 90 is less likely to be removed. In the step of forming the second mask 90, the second mask 90 is formed to have a thickness greater than that of the carbon film 20. The thickness of the second mask 90 is preferably 10 times or more the thickness of the carbon film 20. The thickness of the second mask 90 can be, for example, 1 μm or more.

[0056] The method for manufacturing the light-emitting device according to the first embodiment may include a step of removing the carbon film 20 after forming the second electrode 41 and the third electrode 42. The light-emitting device 1 shown in FIGS. 12 and 13 is obtained by removing all of the carbon film 20 formed on the semiconductor structure 10 shown in FIG. 11. FIG. 12 is a schematic cross-sectional view taken along line XII-XII in FIG.

[0057] By completely removing the carbon film 20, the first electrode 31 and the second electrode 41 in the light-emitting element 1 are not short-circuited through the carbon film 20. In addition, the carbon film 20 has a high absorption rate for the light emitted by the active layer 12. By completely removing the carbon film 20, the light absorption in the carbon film 20 of the light emitted by the active layer 12 can be reduced, and the light output of the light-emitting element 1 can be improved. To remove the carbon film 20, for example, the ashing method using oxygen plasma described above can be used. Note that in the step of removing the carbon film 20, the carbon film 20 may remain to the extent that the first electrode 31 and the second electrode 41 are not short-circuited.

[0058] [Second embodiment] After the second electrode 41 is formed, the carbon film 20 need not be entirely removed, and at least a portion of it may remain on the semiconductor structure 10. As an example of this, a method for manufacturing a light-emitting element according to a second embodiment and the light-emitting element will be described with reference to Figs.

[0059] In the method for manufacturing the light emitting device according to the second embodiment, the steps up to the formation of the second electrode 41 shown in FIG. 11 are basically the same as those in the first embodiment.

[0060] The method for manufacturing the light-emitting device according to the second embodiment further includes, after the step of forming the second electrode 41, a step of performing a plasma treatment on the carbon film 20 in contact with the side surface 11a2 of the n-side semiconductor layer 11, thereby forming a Schottky barrier structure in the carbon film 20. In the step of forming the Schottky barrier structure in the carbon film 20, the carbon film 20 is subjected to the plasma treatment using a third mask 60 described later.

[0061] The method for manufacturing the light-emitting element according to the second embodiment may include a step of covering a portion of the carbon film 20 to be left with a fourth mask and removing the carbon film 20 exposed from the fourth mask after the step of forming the second electrode 41. Note that the step of removing the carbon film 20 exposed from the fourth mask may not be performed, and a step of forming a Schottky barrier structure in the carbon film 20 may be performed in a state in which the entire carbon film 20 shown in Fig. 11 remains. Note that Figs. 14 to 19 will be described taking as an example a case in which a part of the carbon film 20 is removed and the other carbon film 20 remains after the step of forming the second electrode 41.

[0062] In the plan view of Fig. 14, the remaining carbon film 20 is indicated by diagonal lines. Fig. 15 is a schematic cross-sectional view taken along line XV-XV of Fig. 14. The carbon film 20 is left, for example, on the upper surface 13a of the p-side semiconductor layer 13. In addition, the carbon film 20 is left, for example, on the first exposed portion 11a of the first semiconductor layer 11 located in a region between the third corner C3 and the fourth corner C4 of the semiconductor structure 10 in plan view, and on the first exposed portion 11a of the first semiconductor layer 11 located in a region between the second corner C2 and the fourth corner C4.

[0063] 15, the carbon film 20 on the upper surface 13a of the p-side semiconductor layer 13 is in contact with the first electrode 31. The carbon film 20 left in the first exposed portion 11a is in contact with the upper surface 11a1 and the side surface 11a2 of the first exposed portion 11a. The carbon film 20 on the upper surface 13a of the p-side semiconductor layer 13 and the carbon film 20 on the first exposed portion 11a are connected by the carbon film 20 formed on the side surface of the p-side semiconductor layer 13 and the side surface of the active layer 12.

[0064] The carbon film 20 remaining on the upper surface 13a of the p-side semiconductor layer 13 is preferably covered with a protective film 50 before the step of forming a Schottky barrier structure in the carbon film 20. As shown in Fig. 16, the protective film 50 covers the upper surface of the carbon film 20 on the upper surface 13a of the p-side semiconductor layer 13. The protective film 50 also covers the upper surface of the first electrode 31. The protective film 50 can be made of, for example, silicon nitride.

[0065] For example, the protective film 50 is formed using a fifth mask having openings on the carbon film 20 and the first electrode 31 on the upper surface 13a of the p-side semiconductor layer 13. The protective film 50 is formed on the carbon film 20 and the first electrode 31 on the upper surface 13a of the p-side semiconductor layer 13 exposed from the openings of the fifth mask. The fifth mask is removed by wet etching. At this time, the material film of the protective film 50 formed on the upper surface of the fifth mask is also removed together with the fifth mask.

[0066] In the step of removing the fifth mask by wet etching, migration of metals contained in the second electrode 41 and the third electrode 42 is unlikely to occur because the p-side semiconductor layer 13 and the n-side semiconductor layer 11 are short-circuited through the carbon film 20. In addition, since the first electrode 31 is covered with the protective film 50, it is not exposed to the etching solution in the step of removing the fifth mask by wet etching.

[0067] 17, in the process of forming a Schottky barrier structure in the carbon film 20, a plasma treatment is performed on the carbon film 20 in contact with the side surface 11a2 of the n-side semiconductor layer 11 by using a third mask 60. As the third mask 60, for example, a resist film or a metal film can be used.

[0068] Of the carbon film 20 exposed from the protective film 50, a portion in contact with the side surface 11a2 and a portion in contact with the upper surface 11a1 of the first exposed portion 11a of the n-side semiconductor layer 11 are exposed from the third mask 60. The third mask 60 is formed so as not to cover the portion of the carbon film 20 in contact with the n-side semiconductor layer 11. The third mask 60 covers the upper surface and side surfaces of the protective film 50 and the upper surface 13a of the p-side semiconductor layer 13. The third mask 60 may be formed so as to cover the portion of the carbon film 20 in contact with the side surface of the p-side semiconductor layer 13 and the portion of the carbon film 20 in contact with the side surface of the active layer 12.

[0069] The step of forming a Schottky barrier structure in the carbon film 20 involves performing a plasma treatment using a gas containing at least one of nitrogen, fluorine, and chlorine. A portion of the carbon film 20 exposed from the third mask 60 is exposed to plasma of a gas containing at least one of nitrogen, fluorine, and chlorine. That is, the carbon film 20 in contact with the side surface 11a2 of the n-side semiconductor layer 11 is exposed to plasma of a gas containing at least one of nitrogen, fluorine, and chlorine. The carbon film 20 on the upper surface 13a of the p-side semiconductor layer 13 is not exposed to plasma because it is covered with the protective film 50.

[0070] By subjecting the carbon film 20 to a plasma treatment, a first portion 21 that has not been plasma-treated and a second portion 22 that has been plasma-treated are formed in the carbon film 20, as shown in FIG. 18. A Schottky barrier structure is formed between the plasma-treated second portion 22 and the first portion 21 that has not been plasma-treated. The carbon film 20 has the first portion 21 that contacts the first electrode 31 on the upper surface 13a of the p-side semiconductor layer 13, and the second portion 22 that is continuous with the first portion 21 and contacts at least the side surface 11a2 of the n-side semiconductor layer 11, and further has a Schottky barrier structure between the first portion 21 and the second portion 22. Here, the Schottky barrier structure refers to a diode structure having a band structure similar to the band structure in a Schottky barrier formed between a metal and a semiconductor.

[0071] When the light-emitting element is driven, a positive potential is applied to the first electrode 31, a potential of 0 V or less is applied to the second electrode 41, and a current flows from the first electrode 31 through the p-side semiconductor layer 13, the active layer 12, and the n-side semiconductor layer 11 to the second electrode 41. This causes the active layer 12 to emit light. When this light-emitting element is driven, no current flows from the first electrode 31 to the n-side semiconductor layer 11 through the first portion 21 and the second portion 22 of the carbon film 20.

[0072] When a reverse voltage is applied to the light-emitting element, in which a potential of 0 V or less is applied to the first electrode 31 and a positive potential is applied to the second electrode 41, no current flows through the active layer 12, but a current flows from the n-side semiconductor layer 11 to the first electrode 31 via the second portion 22 and the first portion 21 of the carbon film 20. This makes it possible to prevent destruction of the light-emitting element. The carbon film 20 having a Schottky barrier structure can function as a protection element against ESD (Electro Static Discharge).

[0073] The carbon film 20 can be formed, for example, by using the above-mentioned FCVA method. By using the FCVA method, carbon ions generated by arc discharge without introducing gas into a vacuum discharge space are used, so that the carbon film 20 containing almost no hydrogen can be formed. The hydrogen composition ratio in the carbon film 20 can be 1% or less. The carbon film 20 containing almost no hydrogen has many dangling bonds that are not terminated with hydrogen. Nitrogen, fluorine, or chlorine are easily bonded to the dangling bonds by the above-mentioned plasma treatment, and a Schottky barrier structure is easily formed in the carbon film 20. Therefore, the hydrogen composition ratio in the carbon film 20 is preferably 1% or less.

[0074] In addition, if the first portion 21 that is not plasma-treated is formed in the carbon film 20 in a portion in contact with the first electrode 31, the first portion 21 is not formed in a portion in contact with the n-side semiconductor layer 11, and the second portion 22 that is plasma-treated is formed, a Schottky barrier structure can be developed. Therefore, as shown in FIG. 16, when the carbon film 20 on the upper surface 13a of the p-side semiconductor layer 13 is covered with a protective film 50, the above-mentioned plasma treatment may be performed without forming the third mask 60. Even in this case, a Schottky barrier structure can be formed between the second portion 22 (plasma-treated portion) in contact with the side surface 11a2 of the n-side semiconductor layer 11 in the carbon film 20 and the first portion 21 (plasma untreated portion) in contact with the first electrode 31 on the upper surface 13a of the p-side semiconductor layer 13.

[0075] After forming the Schottky barrier structure in the carbon film 20, the third mask 60 is removed to obtain the light-emitting element 2 shown in Fig. 19. When a resist film is used as the third mask 60, the third mask 60 can be removed by wet etching. When a metal film is used as the third mask 60, the metal film may be removed from the semiconductor structure 10.

[0076] As shown in FIG. 19, the light-emitting device 2 according to the second embodiment includes a semiconductor structure 10, a first electrode 31 disposed on an upper surface 13a of a p-side semiconductor layer 13, and a sp 2 Hybrid orbitals of carbon and sp 3 and a carbon film 20 containing carbon in a hybrid orbital. The carbon film 20 has a first portion 21 in contact with the first electrode 31 on the upper surface 13a of the p-side semiconductor layer 13, and a second portion 22 continuous with the first portion 21 and in contact with the side surface 11a2 of the n-side semiconductor layer 11, and further has a Schottky barrier structure between the first portion 21 and the second portion 22. In addition, the light-emitting element 2 according to the second embodiment can include the second electrode 41, the third electrode 42, and the protective film 50 described above.

[0077] In the second embodiment, after the first electrode 41 is formed, the entire carbon film 20 may be left on the semiconductor structure 10. If the entire portion of the carbon film 20 remaining on the semiconductor structure 10 in contact with the n-side semiconductor layer 11 is subjected to plasma treatment to form the second portion 22, a short circuit between the first electrode 31 and the second electrode 41 through the carbon film 20 can be prevented when the light-emitting element 2 is driven, while a current can be passed from the n-side semiconductor layer 11 to the first electrode 31 through the carbon film 20 when a reverse voltage is applied, thereby protecting the light-emitting element 2.

[0078] In order to make it easier to determine the position where the third mask 60 is to be disposed, a step may be formed in the p-side semiconductor layer 13. If the third mask 60 is disposed above the step in the p-side semiconductor layer 13, the side surface 11a2 of the n-side semiconductor layer 11 can be exposed from the third mask 60.

[0079] The embodiments of the present invention may include the following light-emitting device manufacturing method and light-emitting device.

[0080] [Section 1] A step of preparing a semiconductor structure having an n-side semiconductor layer, a p-side semiconductor layer, and an active layer located between the n-side semiconductor layer and the p-side semiconductor layer, the n-side semiconductor layer having a first exposed portion exposed from the p-side semiconductor layer and the active layer; forming a conductive carbon film continuously on an upper surface of the first exposed portion of the n-side semiconductor layer and an upper surface of the p-side semiconductor layer; removing at least a portion of the carbon film located on the upper surface of the p-side semiconductor layer to form a second exposed portion on the upper surface of the p-side semiconductor layer that is exposed from the carbon film; forming a first mask on the carbon film, the first mask having an opening above the second exposed portion; forming a first electrode on the second exposed portion; The step of forming the first electrode includes: forming a first conductive member on the first mask and in the second exposed portion; removing the first mask by wet etching to remove the first conductive member on the first mask and leave the first conductive member in the second exposed portion; A method for manufacturing a light-emitting device comprising the steps of: [Section 2] a step of removing a part of the carbon film located on the upper surface of the first exposed portion of the n-side semiconductor layer after forming the first electrode, and forming a third exposed portion exposed from the carbon film on the upper surface of the first exposed portion; 2. The method for manufacturing a light-emitting element according to item 1, further comprising the step of forming a second electrode on the third exposed portion. [Section 3] 3. The method for manufacturing a light-emitting element according to item 2, wherein in the step of forming the second exposed portion or the step of forming the third exposed portion, the carbon film is removed using oxygen plasma. [Section 4] 4. The method for manufacturing a light-emitting device according to any one of items 1 to 3, wherein in the step of forming the carbon film, the carbon film is formed by a Filtered Cathodic Vacuum Arc (FCVA) method or a Chemical Vapor Deposition (CVD) method. [Section 5] 5. The method for manufacturing a light-emitting element according to any one of items 1 to 4, wherein, in the step of leaving the first conductive member in the second exposed portion, when the first mask is removed by the wet etching, an etching rate of the carbon film is lower than an etching rate of the first mask. [Section 6] In the step of forming the carbon film, the carbon film is formed of sp 2 Hybrid orbitals of carbon and sp 3 and carbon in a hybrid orbital, The sp 3 6. A method for producing a light-emitting device according to item 5, wherein the ratio of carbon in the hybrid orbital is formed to 70% or less. [Section 7] 7. The method for producing a light-emitting element according to item 6, wherein in the step of forming the carbon film, the carbon film is formed to a thickness of 10 μm or less. [Section 8] In the step of forming the carbon film, the carbon film is formed to a thickness of 100 nm or more and 1 μm or less; The sp 3 7. A method for producing a light-emitting device according to item 6, wherein the ratio of carbon in the hybrid orbital is set to 10% or more and 50% or less. [Section 9] After the step of forming the second electrode, 4. The method for producing a light-emitting element according to item 2 or 3, further comprising the step of forming a Schottky barrier structure in the carbon film by performing a plasma treatment on the carbon film in contact with a side surface of the n-side semiconductor layer. [Section 10] 10. The method for manufacturing a light-emitting element according to item 9, further comprising the step of forming a protective film covering the carbon film on the upper surface of the p-side semiconductor layer before the step of forming the Schottky barrier structure on the carbon film. [Section 11] 11. The method for producing a light-emitting element according to item 9 or 10, wherein in the step of forming the Schottky barrier structure in the carbon film, a plasma treatment is performed using a gas containing at least one of nitrogen, fluorine, and chlorine. [Section 12] A semiconductor structure having an n-side semiconductor layer, a p-side semiconductor layer, and an active layer located between the n-side semiconductor layer and the p-side semiconductor layer; A first electrode disposed on an upper surface of the p-side semiconductor layer; a first portion that is in contact with the first electrode on the top surface of the p-side semiconductor layer, and a second portion that is continuous with the first portion and in contact with a side surface of the n-side semiconductor layer, 2 Hybrid orbitals of carbon and sp 3 a carbon film containing a hybrid orbital carbon; Equipped with The carbon film has a Schottky barrier structure between the first portion and the second portion. [Section 13] 13. The light-emitting device according to item 12, wherein the carbon film has a hydrogen composition ratio of 1% or less.

[0081] The embodiments of the present disclosure have been described above with reference to specific examples. However, the present invention is not limited to these specific examples. All forms that can be implemented by a person skilled in the art through appropriate design modifications based on the above-mentioned embodiments of the present disclosure also belong to the scope of the present invention as long as they include the gist of the present invention. In addition, within the scope of the concept of the present invention, a person skilled in the art may come up with various modified examples and examples of modifications, and these modified examples and examples of modifications also belong to the scope of the present invention. [Explanation of symbols]

[0082] Reference Signs List 1, 2...light-emitting element, 10...semiconductor structure, 11...n-side semiconductor layer, 11a...first exposed portion, 11a1...upper surface of first exposed portion, 11a2...side surface of first exposed portion, 11b...third exposed portion, 12...active layer, 13...p-side semiconductor layer, 13a...upper surface of p-side semiconductor layer, 13b...second exposed portion, 20...carbon film, 21...first portion of carbon film, 22...second portion of carbon film, 30...first conductive member, 31...first electrode, 40...second conductive member, 41...second electrode, 42...third electrode, 50...protective film, 60...third mask, 80...first mask, 81...first opening, 90...second mask, 91...second opening, 92...third opening, 100...substrate

Claims

1. A step of preparing a semiconductor structure having an n-side semiconductor layer, a p-side semiconductor layer, and an active layer located between the n-side semiconductor layer and the p-side semiconductor layer, the n-side semiconductor layer having a first exposed portion exposed from the p-side semiconductor layer and the active layer; forming a conductive carbon film continuously on an upper surface of the first exposed portion of the n-side semiconductor layer and an upper surface of the p-side semiconductor layer; removing at least a portion of the carbon film located on the upper surface of the p-side semiconductor layer to form a second exposed portion on the upper surface of the p-side semiconductor layer that is exposed from the carbon film; forming a first mask on the carbon film, the first mask having an opening above the second exposed portion; forming a first electrode on the second exposed portion; The step of forming the first electrode includes: forming a first conductive member on the first mask and in the second exposed portion; removing the first mask by wet etching to remove the first conductive member on the first mask and leave the first conductive member in the second exposed portion; A method for manufacturing a light-emitting device comprising the steps of:

2. a step of removing a part of the carbon film located on the upper surface of the first exposed portion of the n-side semiconductor layer after forming the first electrode, and forming a third exposed portion exposed from the carbon film on the upper surface of the first exposed portion; The method for manufacturing a light-emitting element according to claim 1 , further comprising the step of forming a second electrode on the third exposed portion.

3. The method for manufacturing a light-emitting element according to claim 2 , wherein in the step of forming the second exposed portion or the step of forming the third exposed portion, the carbon film is removed by using oxygen plasma.

4. 4. The method for manufacturing a light-emitting element according to claim 1, wherein in the step of forming the carbon film, the carbon film is formed by a Filtered Cathodic Vacuum Arc (FCVA) method or a Chemical Vapor Deposition (CVD) method.

5. 4. The method for manufacturing a light-emitting element according to claim 1, wherein, in the step of leaving the first conductive member in the second exposed portion, when the first mask is removed by the wet etching, an etching rate of the carbon film is lower than an etching rate of the first mask.

6. In the step of forming the carbon film, the carbon film is 2 Hybrid orbitals of carbon and sp 3 and carbon in a hybrid orbital, The sp in the carbon film 3 The method for manufacturing a light emitting device according to claim 5 , wherein the ratio of carbon in the hybrid orbital is formed to 70% or less.

7. The method for manufacturing a light-emitting element according to claim 6 , wherein in the step of forming the carbon film, the carbon film is formed to a thickness of 10 μm or less.

8. In the step of forming the carbon film, the carbon film is formed to a thickness of 100 nm or more and 1 μm or less; The sp in the carbon film 3 The method for producing a light emitting device according to claim 6, wherein the ratio of carbon in the hybrid orbital is set to 10% or more and 50% or less.

9. After the step of forming the second electrode, The method for manufacturing a light-emitting element according to claim 2 , further comprising the step of forming a Schottky barrier structure in the carbon film by performing a plasma treatment on the carbon film in contact with a side surface of the n-side semiconductor layer.

10. The method for manufacturing a light-emitting element according to claim 9 , further comprising the step of forming a protective film covering the carbon film on the upper surface of the p-side semiconductor layer before the step of forming the Schottky barrier structure in the carbon film.

11. 11. The method for manufacturing a light-emitting element according to claim 9, wherein in the step of forming the Schottky barrier structure in the carbon film, a plasma treatment is performed using a gas containing at least one of nitrogen, fluorine, and chlorine.

12. A semiconductor structure having an n-side semiconductor layer, a p-side semiconductor layer, and an active layer located between the n-side semiconductor layer and the p-side semiconductor layer; A first electrode disposed on an upper surface of the p-side semiconductor layer; a first portion that is in contact with the first electrode on the top surface of the p-side semiconductor layer, and a second portion that is continuous with the first portion and in contact with a side surface of the n-side semiconductor layer; 2 Hybrid orbitals of carbon and sp 3 a carbon film containing a hybrid orbital carbon; Equipped with The carbon film has a Schottky barrier structure between the first portion and the second portion.

13. The light emitting device according to claim 12, wherein the hydrogen composition ratio in the carbon film is 1% or less.

Citation Information

Patent Citations

  • Iii nitride based compound semiconductor light emitting element