Aqueous inkjet compositions including polymeric thickener
Incorporating a polymeric thickener with an acid number of at least 150 mg KOH/g solids into aqueous inkjet inks stabilizes pigment dispersion and reduces solvent loadings, addressing slow drying and jetting issues on low-absorption substrates, thereby improving print quality and manufacturing efficiency.
Patent Information
- Application Number
- JP2023217797
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-12-23
- Filing Date
- 2023-12-25
- Publication Date
- 2024-10-01
AI Technical Summary
Existing aqueous inkjet inks face challenges with slow drying times and poor jetting characteristics on low-absorption substrates due to high solvent loading, which can lead to image quality issues and adhesion problems, especially at high printing speeds.
Incorporation of a polymeric thickener with an acid number of at least 150 mg KOH/g solids into the ink composition to reduce solvent loadings while maintaining adequate drying and jetting characteristics, using self-dispersible pigments and optimized dispersants to stabilize the pigment dispersion.
The solution enables faster drying times and improved jetting performance on non-porous substrates, enhancing image quality and reducing the risk of print defects, while allowing for cost-effective and rapid manufacturing processes.
Smart Images

Figure 2024132865000001 
Figure 2024132865000002 
Figure 2024132865000003
Abstract
Description
[Technical field]
[0001] Digital printing methods such as inkjet printing are becoming increasingly important in markets outside of traditional desktop printing for small / home offices. Digital printing methods are gaining ground in textile printing and have many potential advantages over traditional printing methods such as screen printing. Digital printing eliminates the plate-making costs associated with making screens, potentially allowing for cost-effective short run production. Digital printing also allows for visual effects such as color gradients and infinite pattern repeat sizes that cannot be practically achieved with screen printing methods. [Background technology]
[0002] The expansion of inkjet commercial and packaging printing applications has created a need to print directly onto low-absorbency substrates such as coated paper, coated corrugated board, and folding cartons, non-absorbent plastic substrates such as vinyl, polystyrene, and polypropylene boards, and flexible substrates such as polypropylene, polyester, nylon, and polyethylene films. The lower absorption of these substrates can result in slower drying, poor image quality, and prints that stick to each other before use. These shortcomings can be exacerbated when printing at high speeds.
[0003] To address these issues, faster drying inks have been formulated with lower boiling water-soluble organic solvents (humectants) and lower solvent loadings. However, for these types of conventional ink formulations, the reduced solvent loading must be compensated for by using higher amounts of pigment and / or polymer binder. This often results in problems with poor jettability, which are exacerbated for solvents with boiling points below 200°C.
[0004] Thus, there is a continuing need for aqueous ink-jet inks that have reduced solvent loading while achieving adequate drying and jetting properties. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] U.S. Pat. No. 5,085,698 [Patent Document 2] U.S. Pat. No. 5,554,739 [Patent Document 3] U.S. Patent No. 6,852,156 [Patent Document 4] U.S. Patent No. 5,022,592 [Patent Document 5] U.S. Pat. No. 5,026,427 [Patent Document 6] U.S. Patent No. 5,310,778 [Patent Document 7] U.S. Pat. No. 5,891,231 [Patent Document 8] U.S. Pat. No. 5,679,138 [Patent Document 9] U.S. Pat. No. 5,976,232 [Patent Document 10] US Patent Publication No. 20030089277 [Patent Document 11] European Patent Application Publication No. EP-A-0556649 [Patent Document 12] U.S. Pat. No. 5,231,131 [Patent Document 13] U.S. Patent No. 6,117,921 [Patent Document 14] U.S. Patent No. 6,262,152 [Patent Document 15] U.S. Patent No. 6,306,994 [Patent Document 16] U.S. Pat. No. 6,433,117 [Patent Document 17] European Patent Application Publication No. 0,089,213A1 [Patent Document 18] European Patent Application Publication No. 0646,606A1 [Patent Document 19] European Patent Application Publication No. 0,979,833A1 [Patent Document 20] European Patent Application Publication No. 0,013,836A1 [Patent Document 21] International Publication No. 93 / 2454A1 Brochure [Patent Document 22] U.S. Patent No. 4,268,641A1 [Patent Document 23] U.S. Patent No. 4,421,902A1 [Patent Document 24] U.S. Patent No. 3,915,921A1 [Patent Document 25] U.S. Patent No. 5,272,201 [Patent Document 26] U.S. Patent No. 6,161,918 [Patent Document 27] U.S. Pat. No. 4,490,728 [Patent Document 28] U.S. Patent No. 6,648,463 [Patent Document 29] US Patent Application Publication No. 2012 / 0214939 [Patent Document 30] US Patent Publication No. 20030128246 [Non-patent literature]
[0006] [Non-Patent Document 1] The Color Index, Third Edition, 1971 [Non-Patent Document 2] H. Spinelli Adv. Mater, 1998, 10, no. 15, pp. 1215-1218 [Non-Patent Document 3] “Synthesis of an alkali-swellable emulsion and its effect on the rate of polymer diffusion in poly(vinyl acetate-butyl acrylate) latex films” Journal of Polymer Science,Part A: Polymer Chemistry,2005,43(22),pp.5632-5642 [Non-Patent Document 4] “Structural and rheological properties of hydrophobically modified alkali-soluble emulsion solutions” Journal of Polymer Science,Part B: Polymer Physics,2002,40(18),pp.1985-1994 [Non-Patent Document 5] “Viscoelastic properties of hydrophobically modified alkali-soluble emulsion in salt solutions” Polymer,1999,40(23),pp.6369-6379 [Non-Patent Document 6] “Dissolution behavior in water of a model hydrophobic alkali-swellable emulsion polymer with C20H41 groups” Canadian Journal of Chemistry,1998,76(11),pp.1779-1787 Summary of the Invention [Means for solving the problem]
[0007] An aqueous inkjet composition is provided that includes a pigment, water, a water-soluble organic solvent, and a polymeric thickener having an acid number of at least 150 mg KOH / g solids.
[0008] Another embodiment provides a method of coating a substrate comprising applying the aqueous inkjet composition to at least one surface of the substrate.
[0009] Yet another embodiment provides a coated substrate that includes a substrate and a layer derived from an aqueous inkjet composition disposed on at least one surface of the substrate.
[0010] The above and other features are illustrated by the following drawings and detailed description. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Reference will now be made in detail to exemplary embodiments, examples of which are illustrated in the present description. In this regard, the exemplary embodiments may have different forms and should not be construed as being limited to the description set forth herein. Thus, the exemplary embodiments are described below only to illustrate aspects of the present description. As used herein, the term "and / or" includes any and all combinations of one or more of the associated listed items. A phrase such as "at least one," when preceding a list of elements, modifies the entire list of elements and does not modify each individual element of the list.
[0012] When an element is said to be "on" another element, it will be understood that it can be in direct contact with the other element or that intervening elements can be present between them. In contrast, when an element is referred to as being "directly on" another element, there are no intervening elements present.
[0013] Terms such as first, second, third, etc. may be used herein to describe various elements, components, regions, layers, and / or sections, but it will be understood that these elements, components, regions, layers, and / or sections should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer, or section from another element, component, region, layer, or section. Thus, a first element, component, region, layer, or section discussed below can be referred to as a second element, component, region, layer, or section without departing from the teachings of the present embodiment.
[0014] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting. As used herein, the singular forms "a," "an," and "the" are intended to include the plural forms as well, unless the context clearly indicates otherwise.
[0015] It will be further understood that the terms "comprise" and / or "comprising" or "including" and / or "comprising", as used herein, specify the presence of stated features, regions, integers, steps, operations, elements, and / or components, but do not exclude the presence or addition of one or more other features, regions, integers, steps, operations, elements, components and / or groups thereof.
[0016] Unless otherwise defined, all terms used herein (including technical and scientific terms) have the same meaning as commonly understood by those skilled in the art to which the present invention belongs. Terms such as those defined in commonly used dictionaries should be interpreted to have a meaning consistent with their meaning in the context of the relevant technical field and this disclosure, and will be further understood not to be interpreted in an ideal or overly formal sense unless expressly defined in this specification.
[0017] As used herein, the term "dispersion" refers to a two-phase system in which one phase contains fine particles (often in the colloidal size range) distributed throughout a bulk material, where the particles are the dispersed or internal phase and the bulk material is the continuous or external phase.
[0018] As used herein, the term "dispersant" means a surfactant added to a suspension medium to promote uniform and maximum separation of very fine solid particles of colloidal size.
[0019] As used herein, the term "(meth)acrylate" collectively and alternatively refers to acrylate and methacrylate, and the term "(meth)acrylic acid" collectively and alternatively refers to acrylic acid and methacrylic acid, for example, "butyl (meth)acrylate" refers to butyl acrylate and / or butyl methacrylate.
[0020] As used herein, the term "polymer" includes both homopolymers and copolymers unless specifically stated otherwise. As used herein, the term "copolymer" means a polymer composition containing units of two or more different monomers, the term "terpolymer" means a polymer composition containing units of three or more different monomers, and the term "tetrapolymer" means a polymer composition containing units of four or more different monomers.
[0021] As used herein, the term "binder" refers to a polymeric compound or mixture of polymeric compounds that can be added to the aqueous inkjet composition. The binder can impart properties to the final printed material, such as, for example, imparting greater durability to the printed material. Binders are further described herein.
[0022] The inventors have developed a method to balance and optimize two opposing attributes of an aqueous inkjet composition: short drying time and good jettability. Optimization of these two parameters is important for printing on non-porous and less porous substrates such as flexible plastic films, foils, rigid plastics, and coated media. In this method, the aqueous inkjet composition, which may simply be referred to as an ink, is formulated with a small amount of a specific type of polymer thickener to reduce the overall organic solvent level without increasing the loading of binder and / or pigment. The aqueous inkjet composition allows for faster drying time while maintaining the jettability of the ink.
[0023] According to one embodiment, provided herein is an aqueous inkjet composition comprising a pigment, water, a water-soluble organic solvent, and a polymeric thickener comprising an acid number of at least 150 mg KOH / g solids, where the acid number represents the amount of KOH in milligrams (mg) required to completely neutralize the acidic groups in a 1 gram sample of the polymeric thickener.
[0024] The aqueous inkjet composition comprises a pigment. Pigments suitable for use are those generally well known in the art in aqueous inkjet inks. Traditionally, pigments are stabilized by dispersants, such as polymeric dispersants or surfactants, to produce a stable dispersion of the pigment in the vehicle. Recently, so-called "self-dispersible" or "self-dispersing" pigments (hereinafter "SDPs") have been developed. As the name implies, SDPs contain pigment particles that are dispersible in water without a dispersant and whose surface has been chemically modified with groups that impart hydrophilic dispersibility that allows the pigment to be stably dispersed in the aqueous vehicle without a separate dispersant. "Stably dispersed" means that the pigment is finely divided, uniformly distributed, and resistant to particle growth and agglomeration. In one or more embodiments, the pigment is a self-dispersed pigment or a polymer-dispersed pigment.
[0025] The pigment particles are small enough to allow free flow of the ink through the inkjet printing device, especially at the ejection nozzles, which typically have diameters in the range of 10 micrometers (μm) to 50 μm. Particle size also affects the dispersion stability of the pigment, which is important throughout the life of the ink. Brownian motion of small particles helps prevent particle agglomeration. It is also desirable to use small particles for maximum color strength and gloss. Useful particle sizes can range from 0.005 μm to 15 μm. Pigment particle sizes can be 0.005 μm to 5 μm, or 0.005 μm to 1 μm. The average particle size, as measured by dynamic light scattering, is less than 500 nanometers (nm), or less than 300 nm.
[0026] The selected pigment may be used in dry or wet form. For example, pigments are typically manufactured in an aqueous medium and the resulting pigment is obtained as a water-wet presscake. In presscake form, the pigment does not agglomerate to the same extent that it does in dry form. Thus, pigments in water-wet presscake form do not require as much mixing energy to deagglomerate in the premix process as pigments in dry form. Representative commercially available dry pigments are described in U.S. Pat. No. 5,399,343.
[0027] Examples of pigments having color properties useful in ink jet compositions include Pigment Blue 15:3 and Pigment Blue 15:4 (for cyan); Pigment Red 122 and Pigment Red 202 (for magenta); Pigment Yellow 14, Pigment Yellow 74, Pigment Yellow 95, Pigment Yellow 110, Pigment Yellow 114, Pigment Yellow 128 and Pigment Yellow 155 (for yellow); Pigment Orange 5, Pigment Orange 34, Pigment Orange 43, Pigment Orange 62, Pigment Red 17, Pigment Red 49:2, Pigment Yellow 55, Pigment Yellow 56, Pigment Yellow 57, Pigment Yellow 59, Pigment Yellow 60, Pigment Yellow 61, Pigment Yellow 62, Pigment Red 17, Pigment Red 49:2, Pigment Yellow 63, Pigment Yellow 64, Pigment Yellow 65, Pigment Yellow 66, Pigment Yellow 67, Pigment Yellow 68, Pigment Yellow 69, Pigment Yellow 70, Pigment Yellow 71, Pigment Yellow 72, Pigment Yellow 73, Pigment Yellow 74, Pigment Yellow 75, Pigment Yellow 76, Pigment Yellow 77, Pigment Yellow 78, Pigment Yellow 79, Pigment Yellow 80, Pigment Yellow 82, Pigment Yellow 83, Pigment Yellow 84, Pigment Yellow 85, Pigment Yellow 86, Pigment Yellow 87, Pigment Yellow 89, Pigment Yellow 88, Pigment Yellow 89, Pigment Yellow 90, Pigment Yellow 90, Pigment Yellow 90, Pigment Yellow 90, Pigment Yellow 90, Pigment Yellow 90, P Examples of pigments that may be mentioned include Pigment Red 112, Pigment Red 149, Pigment Red 177, Pigment Red 178, Pigment Red 188, Pigment Red 255 and Pigment Red 264 (for red); Pigment Green 1, Pigment Green 2, Pigment Green 7 and Pigment Green 36264 (for green); Pigment Blue 60, Pigment Violet 3, Pigment Violet 19, Pigment Violet 23, Pigment Violet 32, Pigment Violet 36 and Pigment Violet 38 (for blue); and carbon black. However, some of these pigments may not be suitable for preparation as SDPs. In this specification, colorants are referred to by their "CI" designation, which was established by the Society of Dyers and Colourists, Bradford, Yorkshire, UK, and published in (Non-Patent Document 1).
[0028] SDPs can be prepared by grafting functional groups or molecules containing functional groups onto the surface of the pigment, by physical treatment (such as vacuum plasma) or by chemical treatment (e.g., oxidation with ozone, hypochlorous acid, etc.). Single or multiple types of hydrophilic functional groups can be attached to one pigment particle. The hydrophilic groups are carboxylate or sulfonate groups that provide a negative charge to the SDP when dispersed in an aqueous vehicle. The carboxylate or sulfonate groups are usually accompanied by monovalent and / or divalent cationic counterions. Methods for preparing SDPs are well known and can be found, for example, in U.S. Pat. No. 5,399,433 and U.S. Pat. No. 5,499,433. SDPs can be black, such as those based on carbon black, or can be colored pigments.
[0029] The SDP can have a degree of functionalization, where the density of anionic groups is greater than 3.5 micromoles per square meter of pigment surface (3.5 μmol / m 2 ), more specifically less than about 3.0 μmol / m 2 Also, it is less than about 1.8 μmol / m 2 less than, more specifically, about 1.5 μmol / m 2 Degrees of functionalization less than 100% may also be suitable and may be preferred for certain specific types of SDPs.
[0030] The pigment can be present in the aqueous inkjet composition in an amount of 0.1 weight percent (wt%) to 15 wt%, or 0.1 wt% to 10 wt%, or 0.1 wt% to 8 wt%, based on the total weight of the aqueous inkjet composition.
[0031] The pigment stabilized by the added polymeric dispersant can be prepared by methods known in the art. It is generally desirable to have the stabilized pigment in a concentrated form. The stabilized pigment can be prepared by first premixing the selected pigment with the polymeric dispersant in an aqueous dispersion medium (such as water and optionally a water-miscible solvent) and then dispersing or peptizing the pigment. The dispersion step can be accomplished in a two-roll mill, media mill, horizontal mini mill, ball mill, attritor, or by passing the mixture through multiple nozzles in a liquid jet interaction chamber at a liquid pressure of at least 34,473.8 kilopascals (kPa) to produce a uniform dispersion of pigment particles in the aqueous dispersion medium (microfluidizer). Alternatively, the concentrate can be prepared by dry grinding the polymeric dispersant and pigment under pressure. The media for the media mill can be selected from commonly available media such as zirconia, YTZ, and / or nylon. These various dispersion processes are known in the art in a general sense, as exemplified by U.S. Patent No. 5,399,663; U.S. Patent No. 5,433,36 ... and U.S. Patent No. 5,433,366. The disclosures of each of these publications are incorporated herein by reference. Preferred are two-roll mills, media mills, as well as by passing the mixture through multiple nozzles in a liquid jet interaction chamber at a liquid pressure of at least 34,473.8 kPa.
[0032] After the milling process, the pigment concentrate can be "let down" into an aqueous system. As used herein, the term "let down" refers to the dilution of the concentrate by mixing or dispersion, where the intensity of the mixing / dispersion is usually determined by trial and error using conventional methodologies and often depends on the combination of polymeric dispersant, solvent, and pigment.
[0033] The dispersant used to stabilize the pigment is preferably a polymeric dispersant. Either structured or random polymers can be used, but structured polymers are preferred for use as dispersants. The term "structured polymer" refers to a polymer having a block, branched, or graft structure. Examples of structured polymers include AB or BAB block copolymers as disclosed in U.S. Pat. No. 5,399,413, ABC block copolymers as disclosed in U.S. Pat. No. 5,499,413, and graft polymers as disclosed in U.S. Pat. No. 5,499,413. Other polymeric dispersants that can be used are described, for example, in U.S. Pat. No. 5,499,423, U.S. Pat. No. 5,499,431, U.S. Pat. No. 5,499,442, and U.S. Pat. No. 5,499,451. In one or more embodiments, the polymeric dispersant can include a (meth)acrylic polymer, a polyurethane polymer, or a styrene-maleic anhydride copolymer.
[0034] A typical (meth)acrylic polymer dispersant generally contains both hydrophobic and hydrophilic monomers. Some examples of hydrophobic monomers include methyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, hexyl methacrylate, benzyl methacrylate, 2-phenylethyl methacrylate and the corresponding acrylates. Examples of hydrophilic monomers include methacrylic acid, acrylic acid, dimethylaminoethyl (meth)acrylate and their salts. Also, the quaternary salt of dimethylaminoethyl (meth)acrylate can be used.
[0035] As used herein, hydrophobic regions are those portions that contain the absorptive segments, which are the segments or functions of the dispersant that interact with the pigment surface to cause dispersion. Hydrophilic segments are those segments that stabilize the dispersion by interacting in the solute mixture to cause stabilization. This stabilization is characterized as steric or ionic stabilization. These phenomena are described in (J. Polymers, 1999, 144:133-134). The ionically stabilized polymeric dispersants mentioned above have little, if any, steric stabilization.
[0036] The polymeric dispersant may be neutralized before the start of the dispersion process; that is, the initial mixture of the solvent mixture and the polymeric dispersant has an appropriate amount of neutralizing agent. Alternatively, the neutralizing agent may be added with the polar solvent during the dispersion process. An additional option is to partially neutralize the polymeric dispersant in the initial mixture and add additional neutralizing agent in the polar solvent. The amount of neutralization of the polymeric dispersant in the final mixture is up to about 100% neutralization, or up to about 90% neutralization.
[0037] The neutralizing agent may be an alkali metal hydroxide, amine, etc. Examples of neutralizing agents include organic bases such as mono-, di-, tri-methylamine, morpholine, N-methylmorpholine, alcohol amines such as dimethylethanolamine (DMEA), methyldiethanolamine, mono-, di-, and tri-ethanolamine, pyridine, ammonium hydroxide, tetra-alkylammonium salts such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, and alkali metals such as lithium, sodium, and potassium. Preferred neutralizing agents include dimethylethanolamine, sodium hydroxide, and potassium hydroxide, with potassium hydroxide being particularly preferred for inks used in thermal inkjet printers.
[0038] Polyurethane polymer dispersants can be prepared from isocyanate compounds, isocyanate-reactive compounds, and isocyanates or isocyanate-reactive compounds having ionic substituents present in the polyurethane dispersant to stabilize it in aqueous solution. Often, these polyurethane dispersants can be prepared as polyurethane prepolymers with excess isocyanate groups. Chain-terminating isocyanate-reactive groups are then added to obtain the polyurethane dispersant. The ionic content of the polyurethane, measured as acid or amine groups depending on the source of the ionic substituents, can be 10-90 mg KOH per gram of polymer. The acid number represents the amount of KOH in milligrams (mg) required to completely neutralize the acid groups in a one gram sample of the polymer. The ionic component can be at least partially neutralized prior to its use as a dispersant. The number average molecular weight (M n ) can be from 2000 grams per mole (g / mol) to 9500 g / mol as measured by gel permeation chromatography (GPC).
[0039] When used, the polymeric dispersant may be included in the aqueous inkjet composition in an amount of from 0.1% to 5% by weight, or from 0.1% to 3% by weight, based on the total weight of the aqueous inkjet composition.
[0040] In one or more embodiments, the aqueous inkjet composition may further comprise a polymer binder. The binder may impart properties to the final printed material, such as providing the printed material with greater durability. Typical polymers used as binders in inkjet compositions include polyurethane dispersions and solutions, acrylics, styrene acrylics, styrene butadiene, styrene butadiene acrylonitrile ethylene acrylic acid, ethylene vinyl acetate emulsions, latexes, and the like. The binder may be in solution or may be stabilized as an emulsion by having ionic substituents such as carboxylic acids, sulfur-containing acids, amine groups, and other similar ionic groups.
[0041] The binder can be used alone or in combination with other binders. In one or more embodiments, the polymer binder comprises a polyurethane, a (meth)acrylic polymer, or a polyurethane-acrylic copolymer, and the polymer binder is different from the polymeric dispersant. For example, the polymer binder can be a polyurethane. The optional polyurethane binder can provide desirable crosslinking when used in the aqueous inkjet composition to enhance the durability of the printed image.
[0042] The polymeric binder may be present in the aqueous inkjet composition in an amount of at least 0.6 wt %, based on the total weight of the aqueous inkjet composition, or, for example, from 0.6 wt % to 15 wt %, or from 1 wt % to 15 wt %, based on the total weight of the aqueous inkjet composition.
[0043] The polymer binder can be added to the pigment dispersion along with other ingredients to prepare the aqueous inkjet composition. Although some polymers can function as both binders and dispersants, many binders are different from the dispersants that disperse the pigment to form the pigment dispersion. The polymer binder and polymer dispersant of the present disclosure are different polymers.
[0044] The aqueous inkjet composition also includes an aqueous vehicle that includes water and one or more water-soluble organic solvents. Examples of water-soluble organic solvents include alcohols, ketones, keto-alcohols, ethers, and others, such as thiodiglycol, sulfolane, 1,3-dimethyl-2-imidazolidinone, caprolactam, and the like; glycols such as ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, trimethylene glycol, butylene glycol, hexylene glycol, and the like; addition polymers of oxyethylene or oxypropylene such as polyethylene glycol and polypropylene glycol; triols such as glycerol and 1,2,6-hexanetriol; lower alkyl ethers of polyhydric alcohols such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, and the like; and lower dialkyl ethers of polyhydric alcohols such as diethylene glycol dimethyl and diethyl ether.
[0045] In one or more embodiments, the organic solvent can have a boiling point of 150°C to 230°C, or 150°C to 200°C, or 150°C to 180°C.
[0046] The aqueous inkjet composition can include water in an amount of 50% to 99% by weight, or 50% to 95% by weight, based on the total weight of the aqueous inkjet composition.
[0047] The aqueous inkjet composition may contain the water-soluble organic solvent in an amount of 35% by weight or less, or 30% by weight or less, based on the total weight of the aqueous inkjet composition. For example, the aqueous inkjet composition may contain the water-soluble organic solvent in an amount of 1% by weight to 35% by weight, or 1% by weight to 30% by weight, based on the total weight of the aqueous inkjet composition.
[0048] In some embodiments, the aqueous inkjet composition can have a pH of 8 to 9.5, or 8 to 9. A buffer may be used to maintain the pH. Buffers include, for example, tris(hydroxymethyl)-aminomethane ("Trizma" or "Tris").
[0049] The aqueous inkjet composition includes a polymeric thickener having an acid number of at least 150 mg KOH / g solids. In other words, the polymeric thickener includes at least one acid functional group and has an acid number of at least 150 mg KOH / g solids. The acid number represents the amount of KOH in milligrams (mg) required to completely neutralize the acid groups in a one gram sample of the polymeric thickener. In one or more embodiments, the aqueous inkjet composition can include a polymeric thickener having an acid number of 150 mg KOH / g solids to 650 mg KOH / g solids, or 175 mg KOH / g solids to 550 mg KOH / g solids, or 200 mg KOH / g solids to 450 mg KOH / g solids.
[0050] In one or more embodiments, the polymeric thickener comprises an alkali swellable acrylic emulsion (ASE) polymer, a hydrophobically modified alkali swellable emulsion (HASE) polymer, or a combination thereof.
[0051] ASE polymers thicken only in neutral conditions, hence the expression "alkali-swellable": the result is an ionic repulsion mechanism between the various carboxylate groups carried by the polymer chain. These ionizable groups polarize the water molecules, which increases the viscosity of the medium. In addition to the aforementioned ionic phenomena, HASE polymers involve interactions between associated hydrophobic groups, which also contribute to the thickening of the medium. These mechanisms, as well as in particular the alkali-swellable properties of these emulsions and their ability to thicken aqueous environments at near-neutral pH, are described in the documents WO 2007 / 144721 and "Practical guide to associative thickeners" (Proceedings of the Annual Meeting Technical Program of the FSCT, 2000, 78th, 644-702).
[0052] ASE and HASE polymers are made of anionic monomers (e.g., acrylic acid, methacrylic acid, maleic anhydride, etc.), lipophilic monomers (e.g., ethyl acrylate, butyl acrylate, methyl methacrylate, etc.), and associative monomers (e.g., long chain C5-C 22 The ASE and HASE polymers can be synthesized by free radical emulsion polymerization of various mixtures of vinyl monomers (acrylate or styrene derivative monomers). The ASE and HASE polymers can optionally contain polymerized units derived from other vinyl monomers selected from the group consisting of vinyl acetals, vinyl acetates, vinyl alcohols, vinyl halides, vinyl ethers, crosslinkers, and chain transfer agents.
[0053] ASE polymers can include homopolymers derived from ethylenically unsaturated monomers that contain negative charge when in aqueous basic solution, or copolymers thereof.As used herein, such monomers or repeat units that have negative charge in aqueous basic solution are referred to as "anionic monomers".ASE polymers can also be copolymers, as described above, and can further include additional repeat units derived from other monomers, such as lipophilic monomers.
[0054] Typical anionic monomers include (meth)acrylic acid, crotonic acid, phosphoethyl (meth)acrylate, 2-acrylamido-2-methyl-1-propanesulfonic acid, sodium vinylsulfonate, itaconic acid, fumaric acid, maleic acid, monomethyl itaconate, monomethyl fumarate, monobutyl fumarate, maleic anhydride, and the like. Preferred monomers are (meth)acrylic acid, itaconic acid, 2-acrylamido-2-methyl-1-propanesulfonic acid, maleic anhydride, or fumaric acid. In one or more embodiments, the ASE polymer comprises a (meth)acrylic acid homopolymer. In other embodiments, the ASE polymer can be a copolymer comprising at least one repeat unit derived from (meth)acrylic acid.
[0055] Typical lipophilic monomers include C1-C7 alkyl and C2-C7 hydroxyalkyl esters of acrylic and methacrylic acids such as ethyl (meth)acrylate, methyl (meth)acrylate, 2-ethylhexyl acrylate, butyl (meth)acrylate, 2-hydroxyethyl acrylate, 2-hydroxybutyl methacrylate, etc.; vinyl aromatics and substituted vinyl aromatics such as styrene, vinyl toluene, t-butylstyrene, isopropylstyrene, p-chlorostyrene, etc.; vinyl esters such as vinyl acetate, vinyl versatate, etc.; acrylonitrile; methacrylonitrile; dienes such as butadiene, isoprene, etc.; substituted poly(ethylenes) such as vinyl chloride, vinylidene chloride, etc.; or combinations thereof. Preferred lipophilic monomers include ethyl (meth)acrylate, methyl (meth)acrylate, 2-ethylhexyl acrylate, butyl (meth)acrylate, 2-hydroxyethyl acrylate, 2-hydroxybutyl methacrylate, or combinations thereof.
[0056] HASE polymers, like ASE polymers, further comprise one or more repeat units derived from associative monomers, as described above. The associative monomers of HASE polymers are long chain C5-C50 It can be an ethylenically unsaturated monomer having an acrylate group attached thereto. Examples of associative monomers include C8-C 30 Alkylphenoxy (ethylene epoxy) 6-100 Ethyl (meth)acrylate and C8-C 30 Alkoxy(ethylene epoxy) 6-50 Ethyl (meth)acrylate, C8~C 30 Alkylphenoxyethyl (meth)acrylate, and C8-C 30 Examples of associative monomers include esters such as alkoxyethyl (meth)acrylates. Other linkages may be used, such as, but not limited to, ethers, amides, and urethanes. Examples of associative monomers include C5-C 30 Vinyl esters of carboxylic acids and (meth)acrylates C5-C 30 Alkyl esters are included.
[0057] In certain embodiments, the ASE or HASE polymers can be crosslinked with a cross-coupling agent to provide a polymer having a network structure. In such embodiments, the polymer can include a small amount (0.01-5 wt%) of at least one polyethylenically unsaturated monomer. Suitable examples include allyl methacrylate (ALMA), ethylene glycol dimethacrylate (EGDMA), butylene glycol dimethacrylate (BGDMA), diallyl phthalate (DAP), methylene bisacrylamide, pentaerythritol di-, tri-, and tetra-acrylate, divinylbenzene, polyethylene glycol diacrylate, bisphenol A diacrylate, and the like, or combinations thereof.
[0058] ASE and HASE polymers can be prepared in the form of direct emulsions of alkali-swellable polymers in water, the active ingredient content of which can be between 10% and 45% of their total weight. The corresponding synthesis processes are described in detail in the following publications: (Non-Patent Document 3), (Non-Patent Document 4), (Non-Patent Document 5), (Non-Patent Document 6). Many patent applications also cover their preparation (for ASE: (Patent Document 17), (Patent Document 18), (Patent Document 19), and for HASE: (Patent Document 20), (Patent Document 21), (Patent Document 22), (Patent Document 23), (Patent Document 24)).
[0059] In one or more embodiments, the hydrophobically modified alkali-swellable polymer can be a copolymer derived from two or more of (meth)acrylic acid, a (meth)acrylate ester, and maleic acid.
[0060] The molecular weight of the ASE and HASE polymers can be measured by standard methods such as, for example, particle size exclusion chromatography (SEC) or intrinsic viscosity. In one or more embodiments, the ASE and HASE polymers have a weight average molecular weight (M) of greater than 50,000 g / mole as measured by gel permeation chromatography (GPC). w) The ASE and HASE polymers can have an M of 50,000 g / mol to 1,000,000 g / mol, or 50,000 g / mol to 500,000 g / mol, or 50,000 g / mol to 400,000 g / mol, as measured by GPC. w may have the following structure:
[0061] Exemplary ASE and HASE polymers can include, but are not limited to, RHEOVIS® HS1162, RHEOVIS® HS1152, RHEOVIS® HS1169, RHEOVIS® HS1212, RHEOVIS® HS1332, RHEOVIS® AS1130, RHEOVIS® AS1337, and RHEOVIS® AS1125 available from BASF, Germany. Other exemplary ASE and HASE polymers include ACRYSOL® ASE-60, ACRYSOL® ASE-75, and ACRYSOL® ASE-95NP available from Dow Chemical; ALCOGUM® L15, ALCOGUM® L29, ALCOGUM® L31, ALCOGUM® L350, ALCOGUM® L344, and ALCOGUM® SL920 available from Nouryon (Netherlands); and RHEOTECH® 146, RHEOTECH® 330, RHEOTECH® 53L, RHEOTECH® 1800, RHEOTECH® 2000, and RHEOTECH® 2800 available from Arkema (King of Prussia, PA).
[0062] The polymeric thickener may be present in the aqueous inkjet composition in an amount of from 0.01% to 0.5% by weight, or from 0.05% to 0.4% by weight, or from 0.05% to 0.3% by weight, based on the total weight of the aqueous inkjet composition.
[0063] Other additives may be incorporated into the aqueous ink-jet composition to the extent that such additives do not interfere with the stability and jettability of the aqueous ink-jet composition, which can be readily determined by one of ordinary skill in the art through routine experimentation.
[0064] Surfactants can be added to the aqueous inkjet composition to adjust surface tension and wettability.Typical surfactants include ethoxylated acetylenic diols (e.g., SURFYNOL series available from Evonik), ethoxylated alkyl primary alcohols (e.g., NEODOL series available from Shell), secondary alcohols (e.g., TERGITOL series available from DowChemical), sulfosuccinates (e.g., AEROSOL series available from Cytec), organosilicon (e.g., DYNOL or TEGO Wet series available from Evonik), fluorosurfactants (e.g., CAPSTONE series available from Chemours), etc., or combinations thereof.
[0065] When present, surfactants may be used in an amount of from 0.01% to 5% by weight, or from 0.2% to 2% by weight, based on the total weight of the aqueous inkjet composition.
[0066] The inclusion of a sequestering (or chelating) agent, such as ethylenediaminetetraacetic acid (EDTA), iminodiacetic acid (IDA), ethylenediamine-di(o-hydroxyphenylacetic acid) (EDDHA), nitrilotriacetic acid (NTA), dihydroxyethylglycine (DHEG), trans-1,2-cyclohexanediaminetetraacetic acid (CyDTA), diethylenetriamine-N,N,N',N'',N''-pentaacetic acid (DTPA), and glycoletherdiamine-N,N,N',N'-tetraacetic acid (GEDTA), and salts thereof, can be beneficial, for example, in removing the deleterious effects of heavy metal impurities.
[0067] Co-solvents, such as those exemplified in US Pat. No. 5,399,633, may be included to improve the pluggage inhibition properties of the aqueous ink jet composition.
[0068] To achieve post-printing curing, certain reagents can be used as additives. Post-printing curing is often accelerated by heating the sample after printing. Examples of suitable post-printing curing agents include amide and amine-formaldehyde resins, phenolic resins, urea resins, and blocked polyisocyanates. The selected post-printing curing agent should be soluble or dispersible in the aqueous inkjet composition. The aqueous inkjet composition containing the selected post-printing curing agent should be stable during storage, meaning that no curing reaction occurs before printing. Only after the ink is printed and when the printed image is fused with heat and optionally pressure, does the post-printing curing agent chemically react with one or more of the binder, dispersant, ink vehicle, substrate, etc. A specific example of a post-printing curing agent is CYMEL® 303ULF (available from Cytec, West Patterson, NJ).
[0069] Biocides may be used in the aqueous ink jet composition to inhibit microbial growth.
[0070] Droplet fall velocity, separation length of the droplets, drop size, and stream stability are greatly affected by the surface tension and viscosity of the ink composition. Aqueous inkjet compositions can have a surface tension of 20 dynes / cm to 70 dynes / cm at 25°C. The ink has physical properties that are tailored to the ejection conditions and printhead design. The ink should have excellent storage stability over time so as not to clog to any significant extent in the inkjet device. Additionally, the ink should not corrode parts of the inkjet printing device it comes in contact with, and it should be essentially odorless and non-toxic.
[0071] As mentioned above, the polymeric thickener is incorporated into the aqueous inkjet composition in a predetermined low amount, which allows for the use of less organic solvent without increasing the binder loading or pigment loading, while still achieving fast drying times and good jettability. Furthermore, the polymeric thickener also increases the viscosity of the aqueous inkjet composition to allow for the use of less water-soluble organic solvent.
[0072] In one or more embodiments, the aqueous inkjet composition can have a viscosity at 25°C that is greater than the viscosity at 25°C of an equivalent composition that includes a pigment, water, and a water-soluble organic solvent, but does not include a polymeric thickener. In other words, the equivalent composition includes the same components as the aqueous inkjet composition, except that it does not include a polymeric thickener. For example, in the equivalent composition, the amount of the polymeric thickener can be replaced with an equivalent amount of water or a water-soluble organic solvent. Alternatively, in the equivalent composition, the polymeric thickener can be replaced with another thickener that is different from the polymeric thickener defined herein.
[0073] In one or more embodiments, the aqueous inkjet composition can have a viscosity at 30° C. that is greater than the viscosity at 30° C. of a comparable composition comprising a pigment, water, and a water-soluble organic solvent, but not comprising a polymeric thickener.
[0074] In some embodiments, the aqueous inkjet composition (e.g., having at least 0.1 wt. % of a polymeric thickener) can have a viscosity at 25° C. that is at least 20% greater than the viscosity at 25° C. of a comparable composition comprising a pigment, water, and a water-soluble organic solvent, but not comprising the polymeric thickener. For example, the aqueous inkjet composition (e.g., having at least 0.1 wt. % of a polymeric thickener) can have a viscosity at 25° C. that is at least 30% greater, at least 40% greater, at least 50% greater, at least 75% greater, or at least 100% greater than the viscosity at 25° C. of a comparable composition comprising a pigment, water, and a water-soluble organic solvent, but not comprising the polymeric thickener.
[0075] In some embodiments, the aqueous inkjet composition (e.g., having at least 0.1 wt. % of a polymeric thickener) can have a viscosity at 30° C. that is at least 20% greater than the viscosity at 30° C. of a comparable composition comprising a pigment, water, and a water-soluble organic solvent, but not comprising the polymeric thickener. For example, the aqueous inkjet composition (e.g., having at least 0.1 wt. % of a polymeric thickener) can have a viscosity at 30° C. that is at least 30% greater, at least 40% greater, at least 50% greater, at least 75% greater, or at least 100% greater than the viscosity at 30° C. of a comparable composition comprising a pigment, water, and a water-soluble organic solvent, but not comprising the polymeric thickener.
[0076] The aqueous inkjet composition can have a viscosity at 25° C. of from 3 centipoise (cP) to 100 cP, or from 5 cP to 80 cP, or from 7 cP to 75 cP.
[0077] Viscosity is measured at 25 °C using a Brookfield Viscometer Model LVT with the appropriate spindle to give a reading between 20% and 80% of the full scale reading.
[0078] The term "ink set" as used herein means all the individual inks or other fluids that an inkjet printer is equipped to jet. An ink set can include at least three differently colored inks. For example, cyan (C), magenta (M) and yellow (Y) inks form a CMY ink set. In some embodiments, an ink set includes at least four differently colored inks, for example, by adding a black (K) ink to a CMY ink set to form a CMYK ink set. The magenta, yellow and cyan inks of an ink set can be water-based inks and can contain dyes, pigments or combinations thereof as colorants. Such other inks are known to those skilled in the art in a general sense.
[0079] In addition to the typical CMYK inks, the ink set may further include one or more "gamut expanding" inks, including differently colored inks such as orange, green, red and / or blue inks, and combinations of high intensity color inks with light intensity color inks such as light cyan and light magenta. These "gamut expanding" inks may be particularly useful in textile printing to simulate the color gamut of analog screen printing, as disclosed in U.S. Pat. No. 5,399,633.
[0080] Also provided is a method of coating a substrate, comprising applying an aqueous inkjet composition to at least one surface of the substrate. The resulting coated substrate comprises a substrate and a layer derived from the aqueous inkjet composition on at least one surface of the substrate. In the coated substrate, the water and water-soluble organic solvent can be removed, and the layer derived from the aqueous inkjet composition can comprise pigments and polymeric thickeners, and other optional solid components, but is free of water and water-soluble organic solvents. For example, the layer derived from the aqueous inkjet composition can be prepared by placing the aqueous inkjet composition on a surface of the substrate and then drying the applied layer.
[0081] The aqueous inkjet composition of the present disclosure can be printed by any suitable inkjet printer, such as a printer with a piezo or thermal printhead. Some examples of thermal inkjet printheads are Hewlett Packard Deskjet and Canon iPIXMA iP4200, and some examples of piezo printheads are BROTHER MFC3360C and Epson STYLUS C120. Some suitable printheads are disclosed in U.S. Pat. No. 5,399,411, U.S. Pat. No. 5,499,421, and U.S. Pat. No. 5,523,636, the disclosures of which are incorporated herein by reference.
[0082] Furthermore, the aqueous inkjet composition of the present disclosure can be printed on any substrate without limitation. The aqueous inkjet composition is particularly advantageous for inkjet printing on low-absorption and non-absorption media. Low-absorption media include coated paper, coated corrugated board, coated carton, and folding cartons that have low surface porosity for rendering and / or application of one or more layers of hydrophobic coating layers. Non-absorption substrates refer to plastic substrates such as acrylic, polyvinyl chloride, polycarbonate, polyethylene terephthalate, and polyolefin panels or films of various thicknesses and flexibilities. Substrates can be subjected to common surface treatments such as primer treatment or corona treatment before printing to improve ink fixing and adhesion performance.
[0083] A particularly advantageous application of the aqueous inkjet composition and ink set of the present disclosure is the inkjet printing of textiles. Textiles include, but are not limited to, cotton, wool, silk, nylon, polyester, and the like, and mixtures thereof. Finished forms of textiles include, but are not limited to, fabrics, clothing, T-shirts, furnishings such as carpets and upholstery fabrics, and the like. Furthermore, fibrous fiber materials that come into consideration are in particular hydroxyl group-containing fibrous materials, such as natural fibrous materials, such as cotton, hemp, and hemp, and regenerated fibrous materials, such as viscose and lyocell. Further fibrous materials include wool, silk, polyvinyl, polyacrylonitrile, polyamide, aramid, polypropylene, and polyurethane. These fibrous materials can preferably be in the form of sheet-like woven fiber fabrics, knitted fabrics, or webs.
[0084] Another particularly advantageous use of the aqueous inkjet compositions and ink sets of the present disclosure is in the inkjet printing of commercial coated offset media. Commercial offset paper can possess a non-porous smooth surface. The smooth non-porous surface is formed by a coating that requires a longer time for fluids to penetrate. Often, offset coatings contain polymers that are more hydrophobic than paper coatings designed specifically for inkjet inks, e.g., water-soluble polymers such as polyvinyl alcohol, e.g., styrene-butadiene based. As such, offset coatings are typically hydrophobic, have poor permeability properties, and are smooth / non-porous, so they tend to interact poorly with aqueous inks. Examples of polymers used to coat offset media include latex binders, polystyrene, polyolefins (polypropylene, polyethylene, polybutadiene), polyesters (PET), polyacrylates, polymethacrylates, and / or poly(maleic anhydride).
[0085] The present disclosure is further illustrated by the following non-limiting examples. EXAMPLES
[0086] Reagents were from commercial sources and used without further purification unless otherwise noted. Table 1 lists the reagents for the examples.
[0087] [Table 1]
[0088] Preparation of Cyan Pigment Dispersion The cyan dispersion was prepared according to the procedure described in US Pat. No. 5,399,633. Cyan TRB2 pigment was used and the dispersant was crosslinked after the pigment was dispersed.
[0089] Preparation of Yellow Pigment Dispersion The yellow dispersion was prepared similarly to the cyan pigment dispersion except that yellow pigment PY74 was used.
[0090] Preparation of black pigment dispersion The black dispersion was prepared similarly to the cyan pigment dispersion except that carbon black pigment was used.
[0091] Preparation of Magenta Pigment Dispersion The magenta dispersion was prepared similarly to the cyan pigment dispersion except that yellow pigment PR122 was used.
[0092] Preparation of polymer binder Polymer Binder 1 To a dry, alkali- and acid-free flask equipped with an addition funnel, condenser, stirrer, and nitrogen gas line was added 15.8 grams (g) of CHDM, 104.7 g of TERATHANE® T650, 4.0 g of TMP, and 118 g of acetone. The contents were heated to 40° C. and mixed well. 120 g of IPDI was then added to the flask via the addition funnel over a period of 5 minutes at 40° C., and the remaining IPDI was rinsed from the addition funnel into the flask with 2 g of acetone.
[0093] The flask temperature was heated to 50° C. and held at this temperature for 240 minutes. Then, 15.8 g of DMPA and 11 g of TEA were added to the flask via the addition funnel, which was then rinsed with 2 g of acetone. The flask was then heated to 50° C. and held at this temperature until the NCO% was 2.0% or less.
[0094] The temperature was maintained at 50° C. and 570 g of deionized (DI) water was added over 10 minutes, followed by 38 g of an aqueous solution of EDA (as a 10% solution in water) added via an addition funnel over 5 minutes. The resulting mixture was held at 50° C. for 1 hour and then cooled to room temperature.
[0095] The acetone was removed under vacuum leaving a final dispersion of polyurethane having a solids content of about 30.0% by weight.
[0096] Polymer Binder 2 To a dry, alkali- and acid-free flask equipped with an addition funnel, condenser, stirrer, and nitrogen gas line was added 280 g ETERNACOLL® UC-100, 4 g TMP, 10 g TEA, and 287 g acetone. The contents were heated to 40° C. and mixed well. 162 g IPDI was then added to the flask via the addition funnel over a period of 5 minutes at 40° C., and the remaining IPDI was rinsed from the addition funnel into the flask with 10 g acetone.
[0097] The flask temperature was increased to 50° C. and held at this temperature for 120 minutes. Then 35 g of DMPA and 13.5 g of TEA were added to the flask via the addition funnel, which was then rinsed with 10 g of acetone. The flask temperature was then increased again to 50° C. and held at this temperature until the NCO% was 1.4% or less.
[0098] At a temperature of 50° C., 28 g of VESTAMIN® A95 solution was added via an addition funnel over 5 minutes, followed by 950 g of DI water over 10 minutes, each via an addition funnel, followed by 28 g of diethylenetriamine aqueous solution (as a 10% aqueous solution) over 5 minutes. The resulting mixture was held at 50° C. for 1 hour and then cooled to room temperature.
[0099] The acetone was removed under vacuum leaving a final dispersion of polyurethane having a solids content of about 35.0% by weight.
[0100] Ink Formulation The inks used in the examples were made according to standard procedures in the inkjet art. Component amounts are in weight % of the final ink. Polymer binders and additives are listed on a solids basis. Pigment dispersions are listed on a pigment basis.
[0101] As an example of ink preparation, the ink vehicle was prepared and added to the aqueous ink binder with stirring. After stirring until a homogenous mixture was obtained, the solution was added to the pigment dispersion and mixed until the solution was homogenous again. The final step was to add the rheology modifier (or polymer thickener) to the above mixture, which was then mixed until homogenous and the pH was adjusted to 8.3-8.7 using aqueous KOH solution (3 wt% KOH in water). The composition of the ink before adding the rheology modifier was kept constant as shown in Table 2. When the rheology modifier was added, the % of the balancing water was adjusted so that the total amount of the components equaled a total of 100 wt%.
[0102] Table 2 lists the water-soluble organic solvents and their corresponding boiling points that were used to prepare the ink formulations.
[0103] [Table 2]
[0104] Table 3 shows the acid number (AN) and M of the polymeric thickeners / rheology modifiers used to prepare the ink formulations. w (g / mol) are listed.
[0105] [Table 3]
[0106] Acid number (AN) was determined by titration with KOH and calculated as mg of KOH per gram of polymer.
[0107] Polymer M wwas measured by GPC using polystyrene standards. The GPC was an Alliance e2695 separations module with a 2414 refractive index detector manufactured by Waters Corporation (Milford, MA). Measurements were performed using four different STYRAGEL® GPC columns suitable for measurements from 0 to 600 K, as detailed below, using a 2 wt% solution of acetic acid in tetrahydrofuran as the eluent. The four columns were: 1. STYRAGEL® WAT044225, a 7.8x300mm column packed with 5 μm polystyrene particles with 10000 Å pores. 2. STYRAGEL® WAT044237, a 7.8x300mm column packed with 5 μm polystyrene particles with 500 Å pores. 3. STYRAGEL® WAT044234, 7.8x300mm column packed with 5 μm polystyrene particles with 1000 Å pores. 4. STYRAGEL® WAT044231, 7.8x300mm column packed with 5 μm polystyrene particles with 50 Å pores.
[0108] Ink viscosity evaluation The viscosity of the aqueous inkjet compositions was measured at 25° C. or 30° C., as indicated below, using a Brookfield DVII viscometer equipped with a water jacket for precise temperature control and connected to a temperature controlled chamber.
[0109] Viscosity of black ink A black ink was prepared using the ingredients listed in Table 4, where the amounts are listed in weight percent. The viscosity is also reported in Table 4.
[0110] [Table 4]
[0111] As shown in Table 4, E1 achieved a 32.5% increase in viscosity and E2 achieved a 94.3% increase in viscosity, respectively, relative to the viscosity of CE1 without the rheology modifier. As shown by CE2 and CE3, the use of JONCRYL® 67 did not increase the viscosity, while CE4 and CE5 show that the use of the extra polymer binder did not result in a significant increase in viscosity.
[0112] Yellow Ink Viscosity A yellow ink was prepared using the components listed in Table 5, where the amounts are listed in weight percent. The viscosity is also reported in Table 5.
[0113] [Table 5]
[0114] As shown in Table 5, E3 achieved a 20.8% increase in viscosity, E4 achieved a 43% increase in viscosity, E5 achieved a 136% increase in viscosity, and E6 achieved a 490% increase in viscosity relative to the viscosity of CE6 without the rheology modifier. The results further show that the viscosity increased based on the amount of polymeric thickener included.
[0115] Cyan Ink Viscosity A cyan ink was prepared using the components listed in Table 6, where the amounts are listed in weight percent. The viscosity is also reported in Table 6.
[0116] [Table 6]
[0117] As shown in Table 6, E7 achieved a 48% increase in viscosity, E8 achieved a 98% increase in viscosity, E9 achieved a 160% increase in viscosity, E10 achieved a 73.6% increase in viscosity, E11 achieved a 179% increase in viscosity, E12 achieved a 418% increase in viscosity, and E13 achieved a 1249% increase in viscosity relative to the viscosity of CE7 without the rheology modifier. The results further show that the viscosity increased based on the amount of polymer thickener included, regardless of whether an ASE or HASE polymer thickener was used.
[0118] Open time inspection The open time behavior of the ink is often essential for good printing. In commercial printing situations, printheads can remain idle for minutes to hours without capping. During this time, ink is drying in the open nozzles. This phenomenon can result in print defects when printing resumes without removing the ink. Open time measurements have been used to characterize the jetting behavior of ink after drying near print nozzles for different times. Longer open times are preferred because they allow printing to resume with minimal print defects without the delays associated with removing the ink and cleaning the printhead after a pause.
[0119] The aqueous inkjet compositions listed in Table 7 were tested for their open time using a laboratory printing system, in which the inks were jetted from a mounted fixed SAMBA® G3L printhead manufactured by Fujifilm Dimatix (Santa Clara, CA) onto a substrate held in a rotating cylinder below. The open time performance was judged by the following test: After removing the ink and wiping the nozzle plate clean, 33 lines and a 2.2x7 cm color block were immediately printed. The printer was then left idle for 900 seconds without pulsing or removing ink through the head. After the idle time, the same pattern of lines and ink blocks were printed. Typically, the first few lines printed had defects as a result of ink evaporation during the idle time. The open time was characterized by the number of defective lines before the first complete line was printed. If the number of defective lines was less than 15 after 900 seconds of idling, the open time performance was considered acceptable. If the number of defective lines was greater than 20 after 900 seconds of idling, it was considered to have insufficient open time.
[0120] Aqueous inkjet compositions were prepared using the components listed in Table 7, where the amounts are listed in weight percent. Open time performance is also reported in Table 7.
[0121] [Table 7]
[0122] The results from the jetting experiments in Table 7 demonstrate that while the inks having the hydrophobically modified alkali swellable emulsion polymer thickeners of the present invention all have acceptable open times (E14-E16), the use of a HEUR type thickener, TEGO® Viscoplus 3000, in CE7 can result in poor jetting open time performance.
[0123] Drying speed inspection Mylar MLBT, a transparent PET film from DuPont Teijin Film, was coated with the aqueous inkjet composition using a Gardco film applicator rod with a wire size of 2.5 (Paul N. Gardner Inc., Florida, USA) to form coatings with various wet thicknesses from 3 μm to 5 μm. The coatings were dried for 1 min or 45 s in a 65° C. convection oven. Dryness was assessed by pressing the ink film with an index finger with moderate pressure for 1 s. Dryness ratings were determined using the following criteria: a rating of 1: the ink was completely intact; a rating of 2: the ink was intact with slight transfer; a rating of 3: the ink was slightly marred by finger contact; or a rating of 4: the ink was marred with a significant mark with its size similar to the size of the area pressed by the finger.
[0124] A cyan aqueous inkjet composition was prepared using the components listed in Table 8, where the amounts are listed in weight percent. Dry ratings after 1 minute and 45 seconds are also reported in Table 8.
[0125] [Table 8]
[0126] A magenta aqueous inkjet composition was prepared using the components listed in Table 9, where the amounts are listed in weight percent. Dry ratings after 1 minute and 45 seconds are also reported in Table 9.
[0127] [Table 9]
[0128] Yellow aqueous inkjet compositions were prepared using the components listed in Table 10, where the amounts are listed in weight percent. Dry ratings after 1 minute and 45 seconds are also reported in Table 10.
[0129] [Table 10]
[0130] The results of the drying rate tests shown in Tables 8-10 demonstrate that the drying rate can be significantly improved by using a small amount of the polymeric thickener of the present invention to replace a portion of the water-soluble organic solvent. Furthermore, the polymeric thickener of the present invention improved the drying time while maintaining a similar ink viscosity.
[0131] While particular embodiments have been described, unanticipated or as yet unforeseen alternatives, modifications, variations, improvements, and substantial equivalents will occur to applicant or others skilled in the art, and it is accordingly intended that the appended claims, as filed and as they may be amended, shall embrace all such alternatives, modifications, variations, improvements, and substantial equivalents.
Claims
1. A pigment, Water and a water-soluble organic solvent; a polymeric thickener having an acid number of at least 150 mg KOH / g solids; 1. An aqueous inkjet composition comprising:
2. The aqueous inkjet composition of claim 1 further comprising a polymeric dispersant.
3. 3. The aqueous ink jet composition of claim 1, wherein the polymeric dispersant comprises a (meth)acrylic polymer, a polyurethane polymer, or a styrene-maleic anhydride copolymer.
4. The aqueous inkjet composition of any one of claims 1 to 3, further comprising a polymer binder.
5. 5. The aqueous inkjet composition of claim 4, wherein the polymeric binder comprises a polyurethane, a (meth)acrylic polymer, or a polyurethane-acrylic copolymer, and the polymeric binder is different from the polymeric dispersant.
6. The aqueous inkjet composition of any one of claims 1 to 5, wherein the polymeric thickener has an acid value of from 150 mg KOH / g solids to 650 mg KOH / g solids.
7. 7. The aqueous inkjet composition of claim 1, wherein the polymeric thickener is present in an amount of from 0.01% to 0.5% by weight, based on the total weight of the composition.
8. 8. The aqueous inkjet composition of claim 1, wherein the pigment is present in an amount of from 0.1% to 15% by weight, based on the total weight of the composition.
9. 9. The aqueous inkjet composition of claim 1, wherein the water-soluble organic solvent is present in an amount of from 1% to 35% by weight, based on the total weight of the composition.
10. The aqueous inkjet composition according to any one of claims 1 to 9, wherein the water-soluble organic solvent has a boiling point of 150°C to 230°C.
11. The aqueous inkjet composition according to any one of claims 1 to 10, which has a pH of 8 to 9.
5.
12. 12. The aqueous inkjet composition of claim 1, having a viscosity at 25°C that is greater than the viscosity at 25°C of an equivalent composition comprising the pigment, the water, and the water-soluble organic solvent but not the polymeric thickener.
13. 13. The aqueous inkjet composition of any one of claims 1 to 12, having a viscosity at 25°C that is at least 20% greater than the viscosity at 25°C of an equivalent composition comprising the pigment, the water, and the water-soluble organic solvent but not the polymeric thickener.
14. 14. The aqueous inkjet composition of any one of claims 1 to 13, wherein the polymeric thickener has a weight average molecular weight of at least 50,000 grams per mole as measured by gel permeation chromatography.
15. The aqueous inkjet composition of any one of claims 1 to 14, wherein the polymeric thickener comprises an alkali-swellable acrylic emulsion polymer, a hydrophobically modified alkali-swellable emulsion polymer, or a combination thereof.
16. the alkali-swellable acrylic emulsion polymer comprises a (meth)acrylic acid homopolymer or copolymer; and the hydrophobically modified alkali-swellable polymer is a copolymer derived from two or more of (meth)acrylic acid, a (meth)acrylate ester, and maleic acid; The aqueous inkjet composition according to claim 15.
17. A method of coating a substrate, comprising applying the aqueous inkjet composition of any one of claims 1 to 16 to at least one surface of the substrate.
18. A substrate; a layer derived from the aqueous inkjet composition according to any one of claims 1 to 17, disposed on at least one surface of the substrate; A coated substrate comprising:
19. The layer The pigment; the polymeric thickener; 20. The coated substrate of claim 18, comprising:
20. The layer disposing the composition on at least one surface of the substrate; Drying and 20. The coated substrate of claim 18 or 19, prepared by a process comprising:
Citation Information
Patent Citations
EP0,013,836A1
EP0,089,213A1
EP0,979,833A1
Aqueous dispersions containing ABC triblock polymer dispersants
EP0556649A1
EP0646,606A1
Cited By
Aqueous inkjet ink composition and printed matter
WO2026163750A1