Friction member and method for manufacturing same
A friction material with a silicone resin-impregnated stainless steel sintered body addresses the issue of reduced friction in high humidity by maintaining contact integrity and preventing water adsorption, ensuring consistent performance in vibrating actuators.
Patent Information
- Application Number
- JP2024001515
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-15
- Filing Date
- 2024-01-09
- Publication Date
- 2024-10-01
AI Technical Summary
Friction materials used in vibrating actuators experience a decrease in frictional force in high humidity environments due to water adsorption forming a lubricating layer, which affects their performance.
A friction material comprising a stainless steel sintered body with pores impregnated with a silicone resin, characterized by a specific ratio of Si-H to Si-O-Si bond absorption peak intensities, enhances frictional force by preventing water adsorption and maintaining contact integrity.
The friction material maintains high frictional force in high humidity conditions, effectively suppressing the decrease in frictional force typically observed in such environments.
Smart Images

Figure 2024132872000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a friction material and a method for producing the same. [Background technology]
[0002] A vibration actuator is known that brings a vibrating body equipped with an electromechanical energy conversion element into pressure contact with a contact body, excites a predetermined vibration in the vibrating body, and applies a frictional driving force from the vibrating body to the contact body, thereby moving the vibrating body and the contact body relatively. The vibrating body includes a piezoelectric body and an elastic body bonded to the piezoelectric body, and transmits vibrations generated in the piezoelectric body by applying a voltage to the piezoelectric body to the contact body via the elastic body.
[0003] As mentioned above, the driving force of a vibration actuator depends on the frictional force acting between the elastic body and the contact body. The contact body is required to generate frictional force as a friction material, but there is a problem that the frictional force decreases when it is left in a high humidity environment. This is assumed to be due to the fact that moisture adsorbed on the contact body in a high humidity environment exists on the surface of the contact body as a water film, and the water film acts as a lubricating layer.
[0004] Furthermore, as wear progresses due to the sliding between the elastic body and the contact body, the distance around the real contact area between the elastic body and the contact body on the friction surface becomes closer, i.e., the so-called "break-in" progresses. Around the real contact area that has become closer in this way, the water film becomes more likely to act as a lubricant layer, and the decrease in frictional force becomes more apparent.
[0005] In response to these issues, Patent Document 1 proposes using a friction material made of a stainless steel sintered body impregnated with a silicone-based or polyester-based resin as a contact body. Patent Document 1 describes that a transfer film of the resin formed on the sliding surface prevents direct contact between the elastic body and the contact body, thereby suppressing the progression of "fitting-in" between the elastic body and the contact body.
[0006] There is a demand for the development of a friction material suitable for applications such as the contact body of a vibration actuator that requires a high frictional driving force even in a high humidity environment, that is, a friction material that reduces the decrease in frictional force even in a high humidity environment. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2022-155688 A Summary of the Invention [Problem to be solved by the invention]
[0008] An object of the present invention is to provide a friction material that reduces the decrease in frictional force in a high humidity environment and can be used as a contact body of a vibration actuator, etc. [Means for solving the problem]
[0009] The friction material disclosed in the present specification is a friction material that includes a stainless steel sintered body having pores, and a resin is present in at least a part of the inside of the pores, and the resin material is a silicone-based resin material, and in a spectrum obtained by infrared spectroscopy, -1 From 2415cm -1 The maximum absorption peak intensity Ia due to the stretching vibration of the Si-H bond in the range of 1000 cm -1 From 1070cm -1 The friction material is characterized in that the ratio Ia / Ib of the maximum absorption peak intensity Ib derived from the stretching vibration of the Si-O-Si bond in the range of 0.10 or more. Effect of the Invention
[0010] According to the present invention, it is possible to provide a friction material in which the decrease in frictional force in a high humidity environment is reduced and which can be used as a contact body of a vibration type actuator or the like. [Brief description of the drawings]
[0011] [Figure 1] 2 is a schematic diagram showing a surface of a friction material according to the first embodiment. FIG. [Diagram 2] FIG. 2 is a schematic diagram showing a friction and wear tester in the examples and comparative examples of the present invention. [Diagram 3] FIG. 2 is a schematic diagram showing a frictional force evaluation device in examples and comparative examples of the present invention. [Figure 4] 1A to 1C are diagrams illustrating the driving principle of a linear drive vibration actuator in a first embodiment. [Diagram 5] 1 is an IR spectrum in Example 1. [Figure 6] FIG. 11 is a schematic diagram showing the configuration of an imaging device according to a second embodiment. [Figure 7] FIG. 11 is a schematic diagram showing a configuration of a robot according to a third embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The friction material disclosed in the present specification is a friction material including a stainless steel sintered body having pores, and a resin is present in at least a part of the inside of the pores. Furthermore, the resin material impregnated in the pores is a silicone-based resin material.
[0013] [First embodiment] (Friction material and method of manufacturing the friction material) Hereinafter, the friction material and the method for manufacturing the friction material according to the first embodiment will be described in detail with reference to the drawings.
[0014] First, the stainless steel sintered body that serves as the base material of the friction material will be described. Note that hereinafter, the stainless steel sintered body may be abbreviated to "sintered body." The stainless steel sintered body in this embodiment contains stainless steel and has pores.
[0015] In the following description, C, Cr, etc. are not limited to simple substances but also include atoms contained in alloyed materials, etc. For example, when it is stated that the weight ratio of Cr is 10.5 wt%, it means that Cr atoms are contained at 10.5 wt% by weight regardless of the bonding state of Cr.
[0016] From the viewpoint of improving the wear resistance of the friction material, a mixed powder of stainless steel raw material powder and carbon raw material powder may be used as the raw material for the stainless steel sintered body. However, if an excessive amount of carbon powder is mixed into the raw material for the sintered body, the free carbon powder may act as a lubricant and reduce the frictional force, so the ratio of carbon powder to the raw material is set to an upper limit of 2.0 wt%. It is desirable that the raw material for the sintered body contains a small amount of carbon powder so that the sintered body contains the martensite phase described below.
[0017] A mold (die) of the desired shape for the application is prepared, the raw material powder is filled into the die, and pressure molding is performed to produce a green body. The obtained green body is fired at a specified temperature for a specified time, and then cooled to produce a sintered body. When carbon is mixed to improve wear resistance, it is desirable to perform a rapid cooling process after firing, since higher wear resistance can be obtained by forming a martensite phase.
[0018] The sintered body in this embodiment is a stainless steel containing a martensite phase and an austenite phase. In the sintered body in this embodiment, the volume ratio of the martensite phase to the sum of the volumes of the martensite phase and the austenite phase is preferably 45% or more. If rapid cooling is difficult, high wear resistance can be imparted by performing a separate quenching process or by adding a sub-zero treatment, carburizing treatment, nitriding treatment, or other post-processing. It is preferable to perform the sub-zero treatment after sintering the molded body, since this makes it possible to obtain a sintered body containing a large amount of the martensite phase. It is preferable to perform the sub-zero treatment as the final process in the manufacture of the sintered body.
[0019] The sintered body in this embodiment preferably contains 10.5 wt% or more of Cr from the viewpoint of corrosion resistance.The sintered body in this embodiment preferably contains more than 0 wt% and 2.0 wt% or less of C (carbon) from the viewpoint of improving the wear resistance of the friction material.
[0020] FIG. 1 shows a schematic diagram of the surface of the friction material according to the first embodiment. In the friction material 1, gaps generated when stainless steel raw material particles 2 are bonded remain as pores 3. In the impregnation process described later, at least a part of the inside of the pores 3 is impregnated with resin. Here, the surface porosity is the area ratio of the pores exposed on the surface of the friction material to the surface of the friction material. Since the surface porosity affects the area of the impregnated resin exposed on the surface, it is desirable to control the surface porosity to be within a predetermined range. In order to obtain the effect of maintaining the friction force, the surface porosity is desirably 1.0% or more, and from the viewpoint of the strength and wear resistance of the base material, the surface porosity is desirably 20% or less.
[0021] Factors that control the porosity of a sintered body include the particle size of the raw material powder, the pressure during molding, the sintering temperature, and the sintering time. Since the porosity is also greatly affected by the type of material and the shape to be produced, it is necessary to experimentally determine the appropriate sintering conditions.
[0022] Surface porosity can be measured by obtaining an observation image of the surface and quantifying the area ratio of pores on the surface using image processing software. Other methods include measuring the dimensions and converting the porosity from the volume and weight, and measuring using the Archimedes method, but accurate measurement can be difficult when the target has a complex shape. In addition, depending on the shape to be produced, density differences may occur between the inside and the surface during molding, and the condition of the pores exposed to the surface may change if the surface is polished in a later process, so it is preferable to measure the surface porosity directly.
[0023] Next, the resin material impregnated into the pores of the sintered body will be described. The resin material impregnated into the pores is a silicone-based resin material, and a material having a relatively large number of Si-H bonds is used. Here, the silicone-based resin material is a resin material having a siloxane skeleton (Si-O-Si). The silicone-based resin material may have one or more substituents such as alkyl groups or substituents in which a part of an alkyl group is substituted, on the side chain of the siloxane skeleton. The silicone-based resin material filled into the pores of the friction material may have a structure in which the siloxane skeleton is crosslinked.
[0024] In the FT-IR spectrum obtained by infrared spectroscopic analysis of the resin material of this embodiment, it is preferable that the ratio of maximum absorption peak intensities Ia / Ib is 0.10 or more. -1 From 2415cm -1 The maximum absorption peak intensity due to the stretching vibration of the Si-H bond in the range of 1000 cm was defined as the maximum absorption peak intensity Ia. -1 From 1070cm -1 The maximum absorption peak intensity Ib was determined as the maximum absorption peak intensity due to the stretching vibration of the Si-O-Si bond in the range. For reasons described below, the ratio of the maximum absorption peak intensities Ia / Ib is preferably 0.50 or less. Here, a nano-infrared spectroscopic analyzer manufactured by Photothermal Spectroscopy Corporation can be used to obtain an absorption spectrum in the evaluation of the impregnated resin. For example, a resolution of 4 cm -1 , 16 times of accumulation, measurement range is 650cm -1 From 2500cm -1 By setting this, impregnated resin can be analyzed.
[0025] The process of introducing the resin material into the pores of the sintered body may include an impregnation process of impregnating the pores with the resin material and a curing process of curing the resin material by subjecting the sintered body in a state in which the resin material has been impregnated to a heat treatment or the like. The resin material may be introduced into the pores of the sintered body only by the impregnation process without performing the curing process.
[0026] Furthermore, it is desirable to use a resin material with its composition adjusted to have a low viscosity at room temperature so that the impregnation proceeds efficiently. By performing heat curing or the like after impregnation, the resin material remains as a solid inside the pores of the sintered body. The amount of Si-H bonds detected from the resin material by infrared spectroscopy after curing is also affected by the curing conditions after impregnation. Therefore, it is necessary to select curing conditions that match the components of the resin material used for impregnation, or adjust the components of the resin material to match the curing conditions, so it is effective to investigate the relationship between these factors experimentally in advance.
[0027] The resin material used for impregnation can be impregnated into the sintered base material by a general vacuum impregnation process. One or more sintered bodies are placed in a vacuum chamber, and the chamber is evacuated to below atmospheric pressure. The air and absorbed moisture in the pores of the sintered body are removed by the effect of the vacuum, and then the resin material, which acts as the impregnation material, is poured into the chamber. In order to impregnate the resin material further into the pores, the pressure is increased to above atmospheric pressure. The chamber is then opened, and the resin on the surface is removed by centrifugation or wiping, and the resin is then cured.
[0028] As a means for curing the resin material, there are thermosetting and photosetting. It is preferable to select thermosetting from the viewpoint of efficiency and controlling the amount of Si-H bonds as described above. When thermosetting, the sintered body may be placed in an oven controlled at a predetermined temperature, or immersed in hot water. By using a vacuum chamber in this way, more resin can be impregnated to the inside. Note that the impregnation means is not limited to the above, and for example, a method of applying an appropriate amount of impregnating resin material to the friction surface and impregnating it by utilizing gravity or capillary action may be used.
[0029] Finally, post-processing such as polishing the friction surface is performed according to the application of the friction material. It is desirable that the arithmetic mean roughness of the area excluding pores on the friction surface of the friction material is 0 μm or more and 0.20 μm or less. For example, in the case of applications requiring high braking performance such as the contact body of a vibration type actuator, it is necessary to reduce the surface roughness, so polishing is performed. Examples of polishing methods include polishing using fixed abrasive grains, polishing using free abrasive grains, and barrel polishing. However, if the polishing abrasive grains are too large, large periodic polishing marks are formed on the surface, which may crush the pores generated by sintering, which is not desirable.
[0030] If it is not necessary to reduce the surface roughness depending on the application, post-processing is not necessarily required. In addition, if the shape obtained after sintering is significantly different from the part shape, it is necessary to process it into the shape required for the part by machining or the like. Here, if it becomes necessary to scrape off the friction surface, it is necessary to confirm that the resin remains after processing. If the amount of the friction surface removed by processing exceeds the impregnated depth of the resin material, the resin will no longer exist on the friction surface, which is undesirable. Therefore, by carrying out resin impregnation after machining and then performing finishing processing such as polishing as necessary, a friction material in which some of the pores are impregnated with resin can be obtained. The impregnated depth of the resin material is affected by the amount and size of the pores in the sintered body, the viscosity of the impregnating material, and the impregnation conditions, so it is desirable to check it in advance.
[0031] The friction material obtained in this way acts to prevent the decrease in frictional force in a high humidity environment will be described below. By impregnating the pores of the sintered body with resin, the existence of a transfer film has the effect of preventing the elastic body and the contact body from becoming "familiar," and the water-repellent effect of the silicone resin has the effect of reducing the decrease in frictional force caused by water adsorption.
[0032] As a result of further investigation of the impregnating resin, the authors found that even greater effects could be obtained by selecting a silicone resin material that contains many Si-H bonds. This is presumably due to the presence of Si-H bonds further enhancing the hydrophobic effect. Due to the difference in electronegativity, the H atoms of the Si-H bonds are strongly attracted to the Si atoms, so it is presumed that resin materials with many Si-H bonds have a large interfacial free energy and are more likely to repel water. However, if there are too many Si-H bonds, the mobility of the siloxane skeleton increases and the fluidity of the silicone resin increases, which may make it difficult for the silicone resin to be retained in the pores. Therefore, it is preferable that the value of the maximum absorption peak intensity ratio Ia / Ib mentioned above is 0.50 or less. Analysis of the resin inside the pores exposed on the surface of the friction material can be performed using a microscopic infrared spectroscopic analyzer.
[0033] (Vibration Actuator) FIG. 4 is a diagram explaining the driving principle of a linear drive type vibration motor as an example of a vibration type actuator. The vibration type motor shown in FIG. 4(a) is composed of a vibrating body 205 in which a piezoelectric element 204 is bonded to an elastic body 203, and a contact body 201 driven by the vibrating body 205. By applying an AC voltage to the piezoelectric element 204, two vibration modes are generated as shown in FIG. 4(c) and (d), and the contact body 201, which is in pressure contact with the protrusion 202, is moved in the direction of the arrow. FIG. 4(b) is a diagram showing the electrode pattern of the piezoelectric element 204. For example, the piezoelectric element 204 of the vibrating body 205 has electrode regions divided into two equal parts in the longitudinal direction. Moreover, the polarization direction in each electrode region is the same (+).
[0034] Of the two electrode regions of the piezoelectric element 204, an AC voltage (VB) is applied to the electrode region located on the right side in Fig. 4(b), and an AC voltage (VA) is applied to the electrode region located on the left side. If VB and VA are AC voltages with frequencies near the resonance frequency of the first vibration mode and in phase, the entire piezoelectric element 204 (two electrode regions) will expand at one moment and contract at another moment. As a result, vibration of the first vibration mode shown in Fig. 4(c) is generated in the vibrating body 205.
[0035] Also, if VB and VA are AC voltages with frequencies near the resonance frequency of the second vibration mode and with a phase difference of 180°, at a certain moment, the electrode area on the right side of the piezoelectric element 204 contracts and the electrode area on the left side expands. At another moment, the relationship is reversed. As a result, the vibration of the second vibration mode shown in FIG. 4(d) is generated in the vibrating body 205. In this way, by combining the two vibration modes, the contact body 201 is driven in the direction of the arrow in FIG. 4(a). Also, the generation ratio of the first vibration mode and the second vibration mode can be changed by changing the phase difference of the AC voltage input to the two equally divided electrodes. In this vibration type motor, it is possible to change the speed of the moving body by changing the generation ratio.
[0036] Note that this embodiment has been described using as an example a two-phase drive control device that drives a piezoelectric element, which is an electromechanical energy conversion element, in two phases. However, the present invention is not limited to two-phase drive, and can also be applied to a vibration type motor with two or more phases.
[0037] <Application examples of vibration actuators> Next, an imaging device and an industrial robot will be described as examples of equipment and devices to which the above-mentioned vibration type actuator is applied.
[0038] [Second embodiment] 6 is a top view showing a schematic configuration of an imaging device 700, which is an example of an optical device. The imaging device 700 includes a camera body 730 equipped with an imaging element 710 and a power button 720. The imaging device 700 also includes a lens group (not shown) and a lens barrel 740 equipped with a vibration actuator. The lens group, which is an example of an optical element, is driven by a vibration actuator. The lens barrel 740 is replaceable as an interchangeable lens, and a lens barrel 740 suitable for a subject to be photographed can be attached to the camera body 730. The vibration actuator can be the vibration actuator described above.
[0039] Driving a lens using a vibration actuator is considered to be suitable for driving an autofocus lens, but is not limited thereto, and it is considered possible to drive a zoom lens with a similar configuration. The vibration actuator can also be used to drive an image sensor, or a lens or image sensor for image stabilization.
[0040] [Third embodiment] FIG. 7 is a perspective view showing a schematic configuration of a robot 100 that is an example of an electronic device equipped with the above-mentioned vibration actuator, and shows a horizontal articulated robot, which is a type of industrial robot, as an example.
[0041] The robot 100 has an arm joint 111 and a hand 112. The arm joint 111 connects two arms 120 so that the angle at which the two arms 120 cross can be changed. The hand 112 has an arm 120, a gripper 121 attached to one end of the arm 120, and a hand joint 122 connecting the arm 120 and the gripper 121. A vibration actuator is built into the arm joint 111 or the gripper 121, and performs angle adjustment and rotational operation of the arm 120 or the hand joint. Note that a vibration actuator having a TN characteristic (drooping characteristic indicating the relationship between load torque and rotational speed) of high torque at a low rotational speed is preferably used for bending the arm joint 111 or for gripping operation of the hand 112.
[0042] Although the present invention has been described in detail based on the preferred embodiments, the present invention is not limited to these specific embodiments, and various forms within the scope of the gist of the present invention are also included in the present invention. For example, an XY stage can be cited as an example of a device capable of driving a flat contact body in any direction within its plane. In addition, each of the above-mentioned embodiments may be implemented alone or in combination.
[0043] [Examples and Comparative Examples] Next, examples and comparative examples will be described. As the raw material for the sintered body, a mixed powder obtained by mixing a predetermined amount of carbon powder with SUS410 powder was used. Here, the SUS410 powder is a JIS standard product (C: 0.15wt% or less, Cr: 11.5wt% to 13.0wt%, Si: 0.5wt% or less, Mn: 1wt% or less, P: 0.04wt% or less, S: 0.03wt% or less, the remainder being Fe). The raw material powder was put into a superhard mold having a cavity shape (a space for molding) of 40mm x 5mm, and compression molded until a predetermined plate thickness was obtained. The weight of the raw material put in and the plate thickness after molding in each example and comparative example are shown in Table 1. The obtained molded body was sintered at a temperature of 1050°C to 1150°C for 30 minutes, and then quenched to produce a sintered body. In order to further increase the hardness of the obtained sintered body, a subzero treatment was performed at -120°C for 30 minutes. The density of the sintered body measured by the Archimedes method after the subzero treatment is also shown in Table 1.
[0044] The ratio of martensite phase was also measured by magneto-dielectric method using FISCHERSCOPE manufactured by Fisher Instruments. However, since the measured value obtained by this method indicates the volume ratio of martensite phase component in the total volume including voids, it is necessary to convert it to the martensite phase ratio based on the volume excluding the total voids calculated from the theoretical density and bulk density. For example, if the measured value by the magnetic induction method is 40% and the total voids of the sintered body are 10%, the martensite phase ratio based on 90% excluding voids, that is, 40 / 90 = 44.4%, is the martensite phase ratio to be obtained. When the martensite phase ratio in the material excluding voids was obtained as described above based on the density shown in Table 1, all sintered bodies showed a high ratio of 47% to 50%. Some of the sintered bodies produced were not sent to the post-processing and the amount of carbon contained was analyzed. The carbon ratio analyzed by the combustion-infrared absorption method was 0.2wt% to 1.2wt%.
[0045] Next, we will explain about resin impregnation. The sintered body was impregnated with the resin material for impregnation, the various components of which were adjusted. The sintered body was placed in a metal mesh basket and placed in a vacuum chamber, the lid was placed on the basket and the pressure inside the chamber was reduced to 1 kPa or less. After the pressure was reduced, an amount of impregnation material sufficient to fully immerse the metal mesh basket was placed through a pipe connected to the chamber. The chamber was then pressurized, and when the pressure had risen to 0.5 MPa, the chamber was left for about 10 minutes. The chamber was opened to the atmosphere, the sintered body was removed, and the surface residue was removed by centrifugation. The impregnated resin was then hardened by leaving the sintered body in an oven at 100°C for 1 hour.
[0046] After the impregnation was completed, the surface opposite to the friction surface was ground by surface grinding to make the plate thickness uniform at 1.5 mm. After the plate thickness was uniform, the friction surface was finish-polished. The polishing process consisted of polishing for 3 minutes using a #1200 SiC abrasive polishing sheet, followed by lapping for 15 minutes using 3 μm diamond abrasives. The load in both polishing processes was 1000 g per sintered body. The surface roughness after polishing was measured using a Hitachi High-Tech Science scanning white light interference microscope, selecting an area without voids, and measuring the arithmetic mean roughness Ra over a distance of 0.7 mm. Measurements were performed at 10 points on the friction surface, and the average value was calculated, resulting in Ra being 0.03 or less in all cases.
[0047] In addition to evaluating the frictional force of the prepared friction material, the surface porosity was evaluated and the impregnated resin was analyzed. The frictional force was evaluated after performing a preliminary sliding test to emphasize the effect of humidity. Figure 2 shows a schematic diagram of the friction wear tester used for the preliminary sliding test. The frictional material 6 was placed on the movable stage 5 while being fixed with screws, and the pin material 8 and the frictional material 6 were brought into contact with each other while a load was applied by the weight 7. Then, the stage 5 was driven back and forth 10,000 times at a moving speed of 25 mm / s within a range of 30 mm to perform frictional sliding.
[0048] Next, the friction force was evaluated under a high temperature and high humidity environment using the friction force evaluation device shown in Figure 3. The friction material 6 was fixed to the stage 5 and then fixed to a slide rail 11 installed in a temperature and humidity chamber 10. The slide rail 11 was of the ball slide type so as not to generate sliding resistance. The pin material 8 used in the pre-sliding was used as it was. The pin material 8 was fixed by an arm as in the friction and wear test, and was brought into contact with the friction material 6 with a load of a weight 7 of 150 g applied. The contact position between the pin material 8 and the friction material 6 was adjusted so that it was located at the sliding end where the pre-sliding was performed.
[0049] The stage 5 was connected to a force gauge 13 outside the thermostatic chamber by a string 12 that passed through a hole at the tip. The string 12 was made of high-strength Kevlar (registered trademark) thread and passed through an access window 15 provided in the thermostatic chamber inner door. The access window 15 was selected to provide a space so that the string 12 would not come into contact with surrounding parts during measurement. The force gauge 13 was connected to a single-axis robot 14, and the stage 5 was pulled by driving the robot 14, and the friction resistance acting between the pin material 8 and the friction material 6 could be measured by the force gauge 13. To prevent errors due to the pulling angle, the slide rail 11 and the single-axis robot 14 were installed on the same axis, and the positions of the stage 5 and the force gauge 13 were adjusted so that their heights were the same.
[0050] The thermo-hygrostat 10 was operated, and after the temperature inside the chamber reached 40°C and humidity 90%, it was left for 6 hours and the frictional force was measured. The pulling speed was 1 mm / s, the pulling distance was 30 mm, and the average value of the frictional force was calculated from the position 2 mm to the position 28 mm from the starting position, where the measured value was relatively stable, and the friction coefficient calculated based on the average value is shown in Table 1. The surface porosity was obtained by photographing the friction surface with an optical microscope at a magnification of 200 times, binarizing the obtained image data, and calculating the area where pores existed. The average value of 10 points on the friction surface is shown in Table 1.
[0051] The impregnated resin was evaluated using a nano infrared spectroscopic analyzer manufactured by Photothermal Spectroscopy, Inc., and the resin present inside the pores was analyzed. The resolution was 4 cm -1, 16 times of accumulation, measurement range is 650cm -1 From 2500cm -1 The IR spectrum measured in Example 1 is shown in FIG. 5. The arrows in the figure indicate the peaks due to the stretching vibration of the Si-H bond and the peaks due to the stretching vibration of the Si-O-Si bond. In the obtained spectrum, -1 From 2415cm -1 The maximum absorption peak intensity due to the stretching vibration of the Si-H bond detected in the range of 1000 cm was defined as the maximum absorption peak intensity Ia. -1 From 1070cm -1 The maximum absorption peak intensity Ib was determined as the maximum absorption peak intensity due to the stretching vibration of the Si-O-Si bond detected in the range of 100 nm. Furthermore, the ratio of the maximum absorption peak intensities Ia / Ib was calculated and is shown in Table 1.
[0052] [Table 1]
[0053] As shown in Table 1, the friction materials of Examples 1 to 6 impregnated with a silicone resin having a maximum absorption peak intensity ratio Ia / Ib of 0.10 or more obtained by infrared spectroscopy showed a high friction coefficient even when left for a long time in a high humidity environment. On the other hand, as shown in Comparative Example 1, the friction material impregnated with a silicone resin having a maximum absorption peak intensity ratio Ia / Ib of less than 0.10 showed a low friction coefficient. In Comparative Example 2, a friction material impregnated with a silicone resin adjusted to contain more Si-H bonds was produced, but after all steps were completed, the surface was observed and no resin remained in the pores. A resin test piece cured under the same curing conditions without being impregnated with this resin was produced and subjected to infrared spectroscopy analysis, resulting in a maximum absorption peak intensity ratio Ia / Ib of 0.55. In addition, as shown in Comparative Example 3, the friction material impregnated with a polyester resin had a low friction coefficient similar to Comparative Example 1. From the above results, it was confirmed that by producing a friction material impregnated with a silicone-based resin having a maximum absorption peak intensity ratio Ia / Ib of 0.10 or more, it is possible to obtain high frictional force even in a high humidity environment.
[0054] The disclosure of the present embodiment includes the following methods and configurations.
[0055] (Configuration 1) A friction material comprising a stainless steel sintered body having pores, and a resin present in at least a portion of the interior of the pores, The resin material is a silicone-based resin material, and in a spectrum obtained by infrared spectroscopy, -1 From 2415cm -1 The maximum absorption peak intensity Ia due to the stretching vibration of the Si-H bond in the range of 1000 cm -1 From 1070cm -1 The friction material is characterized in that the ratio Ia / Ib of the maximum absorption peak intensity Ib derived from the stretching vibration of the Si-O-Si bond in the range of 0.10 or more.
[0056] (Configuration 2) The friction material according to configuration 1, wherein the sintered body is stainless steel containing a martensite phase and an austenite phase, and contains the martensite phase at a volume ratio of 45% or more.
[0057] (Configuration 3) 3. The friction material according to configuration 1 or 2, wherein an arithmetic mean roughness of a region excluding pores on the friction surface of the friction material is 0 μm or more and 0.20 μm or less.
[0058] (Configuration 4) 4. The friction material according to any one of claims 1 to 3, wherein an area ratio of pores in the surface of the sintered body is 1.0% or more and 20% or less.
[0059] (Configuration 5) 5. The friction material according to any one of claims 1 to 4, wherein a ratio of maximum absorption peak intensities Ia / Ib obtained by the infrared spectroscopic analysis is 0.50 or less.
[0060] (Configuration 6) The friction material according to any one of configurations 1 to 5, wherein the sintered body contains carbon in an amount of more than 0 wt % and not more than 2.0 wt %.
[0061] (Configuration 7) A vibration actuator comprising a vibrating body having an electromechanical energy conversion element and an elastic body, and a contact body that is in pressure contact with the vibrating body, and which moves the vibrating body and the contact body relative to each other by vibration excited in the vibrating body, wherein the contact body is a friction material described in any one of configurations 1 to 6.
[0062] (Configuration 8) A vibration actuator according to configuration 7, An optical device comprising at least one of an optical element and an imaging element driven by the vibration type actuator.
[0063] (Configuration 9) The material, 8. An electronic device comprising the vibration actuator according to configuration 7 for driving the member.
[0064] (Method 1) A step of producing a stainless steel sintered body having pores; The pores of the sintered body are impregnated with a silicone resin, and in the spectrum obtained by infrared spectroscopy, -1 From 2415cm -1 The maximum absorption peak intensity Ia due to the stretching vibration of the Si-H bond in the range of 1000 cm -1 From 1070cm -1 obtaining a friction material having a resin material in pores, the resin material having a ratio Ia / Ib of 0.10 or more to a maximum absorption peak intensity Ib derived from the stretching vibration of Si-O-Si bonds in the range of Ia / Ib; A method for producing a friction material, comprising:
[0065] (Method 2) The process for producing the sintered body includes: A step of mixing a stainless steel raw material powder and a carbon raw material powder to obtain a mixed powder; a sintering step of press-molding the mixed powder in a die, and then sintering and quenching the resulting molded body; A method for producing the friction material according to method 1, comprising:
[0066] (Method 3) The method for producing a friction material according to Method 2, wherein the step of producing the sintered body includes a sub-zero treatment step that is carried out subsequent to the firing step, and the sub-zero treatment step is the final step. [Explanation of symbols]
[0067] 1 Friction material 2. Stainless steel particles 3 Holes (partially filled with resin) 4. Friction and wear testing equipment 5 Stage 6 Friction material 7. Weight 8 Pin Material 9 Arm 10 Constant temperature and humidity chamber 11 Slide rail 12. Thread 13 Force Gauge 14 Single-axis robot 15 Access window
Claims
1. A friction material comprising a stainless steel sintered body having pores, and a resin present in at least a portion of the interior of the pores, The resin material is a silicone-based resin material, and in a spectrum obtained by infrared spectroscopy, -1 From 2415 cm -1 The maximum absorption peak intensity Ia due to the stretching vibration of the Si-H bond in the range of 1000 cm -1 From 1070cm -1 The friction material is characterized in that the ratio Ia / Ib of the maximum absorption peak intensity Ib derived from the stretching vibration of the Si-O-Si bond in the range of Ia / Ib is 0.10 or more.
2. 2. The friction material according to claim 1, wherein the sintered body is stainless steel containing a martensite phase and an austenite phase, and the martensite phase is contained in a volume ratio of 45% or more.
3. 2. The friction material according to claim 1, wherein an arithmetic mean roughness of a region excluding pores on the friction surface of the friction material is 0 μm or more and 0.20 μm or less.
4. 2. The friction material according to claim 1, wherein an area ratio of pores in the surface of the sintered body is 1.0% or more and 20% or less.
5. 2. The friction material according to claim 1, wherein a ratio of maximum absorption peak intensities Ia / Ib obtained by the infrared spectroscopic analysis is 0.50 or less.
6. 2. The friction material according to claim 1, wherein the sintered body contains carbon in an amount of from 0 wt % to 2.0 wt %.
7. A vibration actuator comprising a vibrating body having an electromechanical energy conversion element and an elastic body, and a contact body that is in pressure contact with the vibrating body, and which moves the vibrating body and the contact body relative to each other by vibration excited in the vibrating body, wherein the contact body is a friction material described in any one of claims 1 to 6.
8. The vibration actuator according to claim 7 , An optical device comprising at least one of an optical element and an imaging element driven by the vibration type actuator.
9. The material, An electronic device comprising the vibration actuator according to claim 7 for driving the member.
10. A step of producing a stainless steel sintered body having pores; The pores of the sintered body are impregnated with a silicone resin, and the spectrum obtained by infrared spectroscopy shows a peak at 2079 cm -1 From 2415 cm -1 The maximum absorption peak intensity Ia due to the stretching vibration of the Si-H bond in the range of 1000 cm -1 From 1070cm -1 obtaining a friction material having a resin material in pores, the resin material having a ratio Ia / Ib of 0.10 or more to a maximum absorption peak intensity Ib derived from the stretching vibration of Si-O-Si bonds in the range of Ia / Ib; A method for producing a friction material, comprising:
11. The process for producing the sintered body includes: A step of mixing a stainless steel raw material powder and a carbon raw material powder to obtain a mixed powder; a sintering step of press-molding the mixed powder in a die, and then sintering and quenching the resulting molded body; The method for producing the friction material according to claim 10, comprising:
12. The method for producing a friction material according to claim 11, wherein the step of producing the sintered body includes a sub-zero treatment step that is performed following the firing step, and the sub-zero treatment step is a final step.
Citation Information
Patent Citations
Friction material and method for producing the same
JP2022155688A