Composition containing metal particles

By integrating modified cellulose fibers with covalently bonded groups and organic compounds, the composition maintains high viscosity and metal particle content, addressing the trade-off issue and enhancing film and conductive member production.

JP2024132964APending Publication Date: 2024-10-01KAO CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024036625
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-14
Filing Date
2024-03-11
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing metal particle-containing compositions face a trade-off between high metal particle content and high viscosity, as increasing metal particle content typically reduces the amount of thickener, leading to deteriorated properties.

Method used

Incorporating modified cellulose fibers with covalently bonded modifying groups and organic compounds that are liquid at 25°C, allowing for a metal particle content of 70 parts by mass or more while maintaining high viscosity.

Benefits of technology

The composition achieves high metal particle content with stable viscosity, enabling the production of films and conductive members with improved properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024132964000001
    Figure 2024132964000001
  • Figure 2024132964000002
    Figure 2024132964000002
  • Figure 2024132964000003
    Figure 2024132964000003
Patent Text Reader

Abstract

To provide a composition containing metal particles having a high content of metal particles and a high viscosity, a method for producing a film using the composition containing metal particles, and a method for producing a conductive member.SOLUTION: A composition containing metal particles comprises the following components (A), (B) and (C), in which the content of the component (B) to 100 pts.mass of the solid content in the composition containing metal particles is 70 pts.mass or more. A method for producing a film using the composition containing metal particles, and a method for producing a conductive member are provided. (A) a modified cellulose fiber having a modified group via a covalent bond to an anionic group of an anionic modified cellulose fiber. (B) metal particles. (C) an organic compound which is liquid at 25°C and 1 atm.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a metal particle-containing composition, and a method for producing a film and a method for producing a conductive member using the metal particle-containing composition. [Background technology]

[0002] In recent years, technologies that place less of a burden on the environment have come into the spotlight, and against this technological background, materials using cellulose fibers, which are naturally occurring biomass, have been attracting attention. For example, Patent Document 1 discloses a thickener composition that contains a specific modified cellulose fiber and a non-aqueous solvent and is used at 50°C or higher, with the aim of providing a non-aqueous solvent thickener composition that is suitable for use at 50°C or higher and suppresses viscosity reduction even at high temperatures. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2022-001634 A Summary of the Invention [Problem to be solved by the invention]

[0004] In general, the viscosity of a composition can be increased by increasing the amount of thickener used; however, as the amount of thickener used increases, the amount of solids other than the thickener in the composition relatively decreases, and therefore the properties of the composition other than viscosity tend to decrease. Such problems are more pronounced in metal particle-containing compositions that contain a large amount of metal particles, and there is a trade-off between the properties that are affected by the metal particle content and the viscosity. When the metal particle content is increased to obtain the desired properties, the thickener content cannot be increased, and it tends to be difficult to obtain a composition with a high viscosity. In contrast, Patent Document 1 examines the prevention of viscosity reduction at high temperatures, but does not examine at all the improvement of viscosity when the content of metal particles is increased.

[0005] Thus, in metal particle-containing compositions having a high content of metal particles, further improvements are required to achieve high viscosity. An object of the present invention is to provide a metal particle-containing composition having a high metal particle content and high viscosity, as well as a method for producing a film and a method for producing a conductive member using the metal particle-containing composition. [Means for solving the problem]

[0006] The present inventors have found that by containing the specified components (A) to (C), the above-mentioned problems can be solved even if the content of metal particles as component (B) is equal to or greater than a specified value. That is, the present invention provides the following [1] to [3]. [1] A metal particle-containing composition comprising the following components (A), (B), and (C): The metal particle-containing composition, wherein the content of component (B) per 100 parts by mass of solids in the metal particle-containing composition is 70 parts by mass or more. (A) Modified cellulose fiber having a modifying group via a covalent bond to the anionic group of the anion-modified cellulose fiber (B) Metal particles (C) An organic compound that is liquid at 25°C and 1 atmosphere [2] A method for producing a film, comprising the step of applying the metal particle-containing composition described in [1] above onto a substrate. [3] A method for producing a conductive member, comprising the step of applying the metal particle-containing composition described in [1] above onto a substrate. Effect of the Invention

[0007] According to the present invention, it is possible to provide a metal particle-containing composition having a high metal particle content and high viscosity, as well as a method for producing a film and a method for producing a conductive member using the metal particle-containing composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] [Metal particle-containing composition] The metal particle-containing composition of the present invention contains the following components (A), (B), and (C), and the content of component (B) per 100 parts by mass of solids in the metal particle-containing composition is 70 parts by mass or more. (A) Modified cellulose fiber having a modifying group via a covalent bond to the anionic group of the anion-modified cellulose fiber (B) Metal particles (C) An organic compound that is liquid at 25°C and 1 atmosphere

[0009] According to the present invention, it is possible to obtain a metal particle-containing composition having a high content of metal particles and a high viscosity. The reason for this is not clear, but is thought to be as follows. The metal particle-containing composition of the present invention contains, as component (A), modified cellulose fibers having modifying groups on the anionic groups of the anion-modified cellulose fibers via covalent bonds, and thus can further improve the dispersibility of the modified cellulose fibers compared to the case of using modified cellulose fibers having modifying groups via non-covalent bonds. As a result, even when the content of component (A) is small, the component (A) can exhibit a stable thickening effect, and therefore it is believed that a metal particle-containing composition having high viscosity can be provided even when the content of metal particles as component (B) is high.

[0010] <Component (A): Modified cellulose fiber having modifying groups via covalent bonds to the anionic groups of the anionically modified cellulose fiber> The metal particle-containing composition of the present invention contains, as component (A), modified cellulose fibers having modifying groups attached to anionic groups of the anion-modified cellulose fibers via covalent bonds (hereinafter, sometimes simply referred to as "component (A)"). Component (A) plays a role in increasing the viscosity of the metal particle-containing composition.

[0011] (Anion-modified cellulose fiber) In the present invention, the term "anion-modified cellulose fiber" refers to a cellulose fiber in which some or all of the hydroxy groups of the glucose units of the cellulose fiber have been converted to anionic groups. Note that the glucose units in this specification also include glucose units in which the hydroxymethyl groups have been converted to anionic groups. Preferred examples of the anionic group include at least one selected from the group consisting of a carboxy group, a sulfonic acid group, and a (phosphorous) group. From the viewpoints of availability and effectiveness, the anion-modified cellulose fiber is preferably anion-modified cellulose fiber having a carboxy group as the anionic group (hereinafter also referred to as "carboxy-modified cellulose fiber"). The carboxy-modified cellulose fiber is preferably a carboxy-modified cellulose fiber in which the hydroxymethyl group (-CHOH) at the C6 position of the glucose unit constituting the cellulose fiber is selectively converted to a carboxy group. The counter ion of the anionic group is preferably a proton.

[0012] The anionic group content in the anion-modified cellulose fiber is preferably 0.1 mmol / g or more, more preferably 0.5 mmol / g or more, and even more preferably 1.0 mmol / g or more, from the viewpoint of stable introduction of the modifying group and of increasing defibrability by the introduction of the modifying group. From the viewpoint of ease of production, it is preferably 3 mmol / g or less, more preferably 2 mmol / g or less, and even more preferably 1.8 mmol / g or less. The "anionic group content" means the total amount of anionic groups in the glucose constituting the cellulose fiber, and is specifically measured by the method described in the Examples below.

[0013] In the present invention, "the anionic group of the anion-modified cellulose fiber has a modifying group via a covalent bond" means that a carbon atom derived from an anionic group, preferably a carboxy group, of the anion-modified cellulose fiber forms a covalent bond and has a modifying group via the covalent bond. In the modified cellulose fiber used as component (A) of the present invention, the bond between the modifying group and the anionic group is a covalent bond. Examples of the covalent bond include an amide bond and an ester bond, and an amide bond is preferable. In such modified cellulose fibers, when the covalent bond is an amide bond or an ester bond, component (A) is preferably a modified cellulose fiber obtained by introducing a modifying group by amidation or esterification of the anionic group of the anion-modified cellulose fiber, and more preferably a modified cellulose fiber obtained by introducing a modifying group by amidation of the anionic group of the anion-modified cellulose fiber. More specifically, when the anion-modified cellulose fiber is a carboxy-modified cellulose fiber in which the hydroxymethyl group (-CHOH) at the C6 position of the glucose unit constituting the cellulose fiber is selectively converted to a carboxy group, the modified cellulose fiber is preferably one in which the carbon atom at the 6th position of the glucose unit forms an amide bond or an ester bond and has a modifying group via the amide bond or the ester bond, and more preferably one in which the carbon atom at the 6th position of the glucose unit forms an amide bond and has a modifying group via the amide bond.

[0014] (modifying group) The modifying group is preferably one or more selected from the group consisting of (a) a hydrocarbon group and (b) a polymer group. One or more of these modifying groups may be bonded to the anion-modified cellulose fiber in combination. (a) Hydrocarbon group Preferred examples of the (a) hydrocarbon group include monovalent hydrocarbon groups, such as at least one selected from the group consisting of linear or branched chain saturated hydrocarbon groups, linear or branched chain unsaturated hydrocarbon groups, cyclic saturated hydrocarbon groups, aryl groups, aralkyl groups, and heterocyclic aromatic hydrocarbon groups. From the viewpoint of increasing the viscosity of the metal particle-containing composition, the carbon number of the (a) hydrocarbon group is preferably 1 or more, more preferably 3 or more, even more preferably 8 or more, and even more preferably 10 or more, and from the same viewpoint as above, it is preferably 30 or less, more preferably 22 or less, and even more preferably 18 or less. The (a) hydrocarbon group may have a substituent described later, and a part of the hydrocarbon group may be substituted with a hydrogen nitride group. The linear or branched chain saturated hydrocarbon group is preferably a linear chain saturated hydrocarbon group from the viewpoint of increasing the viscosity of the metal particle-containing composition. Examples of the linear or branched chain saturated hydrocarbon group include a propyl group, an isopropyl group, a butyl group, a sec-butyl group, a tert-butyl group, an isobutyl group, a pentyl group, a tert-pentyl group, an isopentyl group, a hexyl group, an isohexyl group, a heptyl group, an octyl group, a 2-ethylhexyl group, a nonyl group, a decyl group, a dodecyl group, a tridecyl group, a tetradecyl group, an octadecyl group, a docosyl group, and an octacosanyl group. Examples of linear or branched chain unsaturated hydrocarbon groups include propenyl, butenyl, isobutenyl, isoprenyl, pentenyl, hexenyl, heptenyl, octenyl, nonenyl, decenyl, dodecenyl, tridecenyl, tetradecenyl, and octadecenyl groups. Examples of cyclic saturated hydrocarbon groups include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, a cyclooctyl group, a cyclononyl group, a cyclodecyl group, a cyclododecyl group, a cyclotridecyl group, a cyclotetradecyl group, and a cyclooctadecyl group. Examples of the aryl group include a phenyl group, a naphthyl group, an anthryl group, a phenanthryl group, a biphenyl group, a triphenyl group, a terphenyl group, and groups in which these groups are substituted with the substituents described below. Examples of the aralkyl group include a benzyl group, a phenethyl group, a phenylpropyl group, a phenylpentyl group, a phenylhexyl group, a phenylheptyl group, a phenyloctyl group, and groups in which these groups are substituted with the substituents described below. Examples of the heterocyclic aromatic hydrocarbon group include an imidazole group, a methylimidazole group, an ethylimidazole group, a propylimidazole group, a 2-phenylimidazole group, a benzimidazole group, and groups in which these groups are substituted with a substituent. The above-mentioned (a) hydrocarbon group is preferably introduced using an amine compound as a compound (also referred to as a "modifying compound") for introducing a modifying group into the anionic group of the anion-modified cellulose fiber via a covalent bond. That is, when the modifying group of the present invention is (a) a hydrocarbon group, the modifying group is preferably derived from an amine compound containing the above-mentioned (a) hydrocarbon group. Examples of such an amine compound include primary amines and secondary amines.

[0015] (b) Polymer group In the present invention, the term "polymer group" refers to a functional group containing two or more repeating structures of the same structural unit. Note that in the present invention, the term "polymer group" excludes the above (a) hydrocarbon group. (b) The formula weight (molecular weight) of the polymer group is, from the viewpoint of increasing the viscosity of the metal particle-containing composition, preferably 100 or more, more preferably 500 or more, and even more preferably 1,000 or more, and, from the same viewpoint as above, is preferably 1,000,000 or less, more preferably 100,000 or less, even more preferably 10,000 or less, even more preferably 7,000 or less, even more preferably 5,000 or less, even more preferably 4,000 or less, even more preferably 3,500 or less, and even more preferably 2,500 or less. (b) From the viewpoint of increasing the viscosity of the metal particle-containing composition, the polymer group is preferably a functional group having a repeating structure linked by a structure having oxygen atoms, more preferably a functional group having a repeating structure linked by oxygen atoms, such as a polyoxyalkylene structure or a polysiloxane structure, even more preferably a polyoxyalkylene structure, and even more preferably an alkoxypolyoxyalkylene group. From the viewpoint of increasing the viscosity of the metal particle-containing composition, the polyoxyalkylene structure is preferably a (co)polymer structure of one or more oxyalkylenes selected from the group consisting of oxyalkylenes having 2 or more and 8 or less carbon atoms, more preferably a (co)polymer structure of one or more oxyalkylenes selected from the group consisting of oxyalkylenes having 2 or more and 4 or less carbon atoms, even more preferably a (co)polymer structure of one or two oxyalkylenes selected from the group consisting of ethylene oxide (EO) and propylene oxide (PO), and even more preferably a copolymer structure in which ethylene oxide and propylene oxide are polymerized randomly or in a block form (also referred to as an "EO / PO copolymer structure"). When the modifying group of component (A) (b) is a polymer group having an EO / PO copolymer structure, the modifying group of component (A) preferably has a structure represented by the following formula (1) when the covalent bond is represented by Z.

[0016] [ka]

[0017] In the formula (1), R 1 represents a hydrogen atom or a hydrocarbon group having from 1 to 6 carbon atoms. The EO-derived units and the PO-derived units are present randomly or in a block form, a is a positive number indicating the average number of moles of EO added, and b is a positive number indicating the average number of moles of PO added. In addition, Z in the above formula (1) represents a bond between a functional group capable of reacting with an anionic group present at the end of the EO / PO copolymer and an anionic group introduced into the anion-modified cellulose fiber, and represents a covalent bond.

[0018] R 1 From the viewpoint of increasing the viscosity of the metal particle-containing composition, is preferably a linear or branched alkyl group having from 1 to 6 carbon atoms, and more preferably a methyl group. From the viewpoint of increasing the viscosity of the metal particle-containing composition, a is preferably 1 or more, more preferably 3 or more, even more preferably 6 or more, even more preferably 11 or more, even more preferably 15 or more, even more preferably 20 or more, even more preferably 25 or more, and even more preferably 30 or more, and from the same viewpoint as above, a is preferably 100 or less, more preferably 70 or less, even more preferably 60 or less, even more preferably 50 or less, and even more preferably 40 or less. From the viewpoint of increasing the viscosity of the metal particle-containing composition, b is preferably 1 or more, more preferably 3 or more, even more preferably 5 or more, and is preferably 50 or less, more preferably 40 or less, even more preferably 30 or less, even more preferably 25 or less, even more preferably 20 or less, even more preferably 15 or less, even more preferably 10 or less. In the formula (1), a+b represents the average total number of moles of EO and PO added. From the viewpoint of increasing the viscosity of the metal particle-containing composition, a+b is preferably 2 or more, more preferably 4 or more, even more preferably 6 or more, even more preferably 8 or more, even more preferably 10 or more, even more preferably 20 or more, and even more preferably 30 or more, and from the same viewpoint as above, it is preferably 150 or less, more preferably 100 or less, even more preferably 70 or less, even more preferably 60 or less, and even more preferably 50 or less.

[0019] The content (mol%) of the PO-derived unit in the EO / PO copolymer structure can be calculated based on the above a and b, specifically, it can be obtained by b×100 / (a+b). From the viewpoint of increasing the viscosity of the metal particle-containing composition, the content of the PO-derived unit is preferably 1 mol% or more, more preferably 5 mol% or more, even more preferably 7 mol% or more, even more preferably 10 mol% or more, even more preferably 15 mol% or more, and from the same viewpoint as above, it is preferably 100 mol% or less, more preferably 90 mol% or less, even more preferably 85 mol% or less, even more preferably 75 mol% or less, even more preferably 60 mol% or less, even more preferably 50 mol% or less, even more preferably 40 mol% or less, even more preferably 30 mol% or less.

[0020] Z represents a bond between a functional group capable of reacting with an anionic group present at the end of the EO / PO copolymer and an anionic group introduced into the anion-modified cellulose fiber, and represents a covalent bond. From the viewpoint of increasing the viscosity of the metal particle-containing composition, Z is preferably at least one bond selected from the group consisting of an amide bond and an ester bond, and more preferably an amide bond.

[0021] When Z is an amide bond, it is preferably represented by -NH-OC-, where -NH is preferably a group derived from an amino group present at one end of the EO / PO copolymer, and OC- is preferably a group derived from a carboxy group of the anion-modified cellulose fiber.

[0022] The above-mentioned (b) polymer group is preferably introduced using an amine compound as a modifying compound. That is, when the modifying group of the present invention is a (b) polymer group, the modifying group is preferably derived from an amine compound containing the above-mentioned (b) polymer group. Such an amine compound may be a primary amine or a secondary amine. When the functional group present at one end of the EO / PO copolymer structure is an amino group, examples of commercially available modifying compounds include Jeffamine M series manufactured by Huntsman, USA.

[0023] (c) Further Substituents The modifying group may further have a substituent on the (a) hydrocarbon group and / or (b) polymer group. Examples of the substituent include alkoxy groups having 1 to 6 carbon atoms, such as methoxy, ethoxy, propoxy, isopropoxy, butoxy, isobutoxy, sec-butoxy, tert-butoxy, pentyloxy, isopentyloxy, and hexyloxy; methoxycarbonyl, ethoxycarbonyl, propoxycarbonyl, isopropoxycarbonyl, butoxycarbonyl, isobutoxycarbonyl, sec-butoxycarbonyl, and tert-butoxy groups; Examples of such groups include alkoxy-carbonyl groups having 1 to 6 carbon atoms in the alkoxy group, such as rt-butoxycarbonyl, pentyloxycarbonyl, and isopentyloxycarbonyl groups; halogen atoms, such as fluorine, chlorine, bromine, and iodine atoms; acyl groups having 1 to 6 carbon atoms, such as acetyl and propionyl groups; aralkyl groups; aralkyloxy groups; alkylamino groups having 1 to 6 carbon atoms; dialkylamino groups having an alkyl group of 1 to 6 carbon atoms; and hydroxy groups.

[0024] (Production method of component (A)) Component (A) is preferably produced, for example, by introducing anionic groups into raw cellulose fibers to produce anion-modified cellulose fibers (step 1), and then introducing modifying groups into the anionic groups of the anion-modified cellulose fibers (step 2).

[0025] [Process 1] <Cellulose fiber raw material> As the cellulose fiber that is the raw material for the anion-modified cellulose fiber, natural cellulose is preferred from an environmental perspective, and examples thereof include wood pulp such as coniferous pulp and broadleaf pulp; cotton pulp such as cotton linter and cotton lint; non-wood pulp such as straw pulp and bagasse pulp; bacterial cellulose, etc., and these can be used alone or in combination of two or more. The average fiber diameter of the raw cellulose fibers is preferably 5 μm or more from the viewpoints of handleability and cost, and is preferably 500 μm or less from the same viewpoints as above. The average fiber diameter of the raw cellulose fibers is determined by the method described in the Examples below. The average fiber length of the raw cellulose fibers is not particularly limited, but is preferably 5 μm or more from the viewpoints of availability and cost, and is preferably 5,000 μm or less from the same viewpoints as above. The average fiber length of the raw cellulose fibers can be measured according to the method described in the Examples below.

[0026] <Method for introducing anionic groups> Methods for introducing carboxy groups as anionic groups into cellulose fibers include, for example, a method of oxidizing hydroxy groups of the cellulose fibers to convert them to carboxy groups, and a method of reacting the hydroxy groups of the cellulose fibers with at least one selected from the group consisting of compounds having a carboxy group, acid anhydrides of compounds having a carboxy group, and derivatives thereof. Examples of methods for oxidizing the hydroxyl groups of cellulose fibers include a method described in JP 2015-143336 A or JP 2015-143337 A in which an oxidizing agent such as sodium hypochlorite and a bromide such as sodium bromide are reacted with the raw cellulose fibers using 2,2,6,6-tetramethyl-1-piperidine-N-oxyl (TEMPO) as a catalyst. By oxidizing the cellulose fibers using TEMPO as a catalyst, the hydroxymethyl group (-CH2OH) at the C6 position of the glucose unit constituting the cellulose fibers is selectively converted to a carboxy group (-COOH), and the above-mentioned carboxy-modified cellulose fibers can be obtained. As a method for introducing sulfonic acid groups as anionic groups into cellulose fibers, a method of adding sulfuric acid to cellulose fibers and heating the fibers can be given. Methods for introducing phosphorous acid groups as anionic groups into cellulose fibers include a method for mixing a powder or an aqueous solution of phosphorous acid or a phosphorous acid derivative with dry or wet cellulose fibers, a method for adding an aqueous solution of phosphorous acid or a phosphorous acid derivative to a dispersion of cellulose fibers, etc. When these methods are employed, a dehydration treatment, a heat treatment, etc. are generally carried out after mixing or adding a powder or an aqueous solution of phosphorous acid or a phosphorous acid derivative.

[0027] [Process 2] The introduction of a modifying group into the anionic group of the anion-modified cellulose fiber is achieved by reacting the anion-modified cellulose fiber with a compound (modifying compound) for introducing a modifying group into the anionic group, thereby obtaining the modified cellulose fiber of component (A). As a method for introducing the modifying group, when obtaining a cellulose fiber having a modifying group via an amide bond, JP 2015-143337 A can be referred to. After completion of step 2, post-treatment may be appropriately carried out in order to remove unreacted compounds, etc. Examples of methods for the post-treatment include filtration, centrifugation, dialysis, etc.

[0028] (Refining process) By micronizing the cellulose fibers at any stage of the production method of component (A), it is possible to micronize the cellulose fibers from the micrometer scale to the nanometer scale. From the viewpoint of efficiently micronizing the cellulose fibers, the micronization step is preferably carried out before or after the above step 2, and more preferably after the above step 2. In addition, by reducing the average fiber diameter of the cellulose fibers to the nanometer size, it is possible to increase the viscosity of the metal particle-containing composition, which is preferable. For the micronization treatment, a known micronization treatment method can be used. For example, when the average fiber diameter of component (A) is to be nanometer-sized, a treatment method using a grinding machine such as a mass colloider or a treatment method using a high-pressure homogenizer in a medium may be carried out. Examples of the medium include water, alcohols having 1 to 6 carbon atoms, such as methanol, ethanol, propanol, and 1-methoxy-2-propanol (PGME); ketones having 3 to 6 carbon atoms, such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; esters having 4 to 6 carbon atoms, such as ethyl acetate and butyl acetate; saturated or unsaturated hydrocarbons having 5 or 6 carbon atoms; aromatic hydrocarbons, such as benzene and toluene; halogenated hydrocarbons, such as methylene chloride and chloroform; lower alkyl ethers having 2 to 5 carbon atoms; and polar solvents, such as N,N-dimethylformamide (DMF), N,N-dimethylacetamide, and dimethylsulfoxide. These can be used alone or in combination of two or more. The amount of the medium used may be an effective amount for dispersing the cellulose fibers, and is preferably 1 or more times by mass, and preferably 500 or less times by mass, relative to the cellulose fibers.

[0029] (Short fiber processing) At any stage in the process for producing component (A), the cellulose fibers may be subjected to a fiber shortening treatment. The fiber shortening process can be carried out by subjecting the target cellulose fibers to at least one treatment method selected from the group consisting of (i) alkali treatment, (ii) acid treatment, and (iii) heat treatment, ultraviolet treatment, electron beam treatment, mechanical treatment, and enzyme treatment.

[0030] (Properties of component (A)) The main properties of the modified cellulose fiber having modifying groups attached via covalent bonds to the anionic groups of the anionically modified cellulose fiber as component (A) in the present invention are as follows: [Crystal structure] From the viewpoint of increasing the viscosity of the metal particle-containing composition, the component (A) preferably has a cellulose type I crystal structure. The crystallinity of component (A) is preferably 20% or more, more preferably 25% or more, more preferably 30% or more, more preferably 35% or more, and more preferably 40% or more from the viewpoint of increasing the viscosity of the metal particle-containing composition, and is preferably 90% or less, more preferably 85% or less, and more preferably 80% or less from the viewpoint of raw material availability. In this specification, the crystallinity of cellulose fibers is the cellulose I type crystallinity calculated from the diffraction intensity value by X-ray diffraction method, and can be measured according to the method described in the Examples below. In addition, "cellulose I type" refers to the crystalline form of natural cellulose, and "cellulose I type crystallinity" means the proportion of the crystalline region amount in the entire cellulose fibers. The presence or absence of cellulose I type crystal structure can be determined by the presence of a peak at 2θ=22.6° in X-ray diffraction measurement.

[0031] [Average fiber diameter] Component (A) is preferably one that has been subjected to a micronization treatment to have nanometer size. Therefore, the average fiber diameter of component (A) is preferably 1 nm or more, more preferably 2 nm or more, from the viewpoints of handling, availability, and cost, and is preferably 300 nm or less, more preferably 200 nm or less, even more preferably 100 nm or less, even more preferably 50 nm or less, even more preferably 30 nm or less, even more preferably 20 nm or less, even more preferably 15 nm or less, even more preferably 10 nm or less, even more preferably 5 nm or less, from the viewpoints of handling, dispersibility, and increasing the viscosity of the metal particle-containing composition.

[0032] [Average fiber length] From the viewpoint of increasing the viscosity of the metal particle-containing composition, the average fiber length of component (A) is preferably 10 nm or more, more preferably 30 nm or more, more preferably 50 nm or more, more preferably 80 nm or more, more preferably 100 nm or more, more preferably 130 nm or more, more preferably 150 nm or more, more preferably 180 nm or more, more preferably 200 nm or more, and is preferably 1000 nm or less, more preferably 500 nm or less, more preferably 400 nm or less, more preferably 350 nm or less, and more preferably 320 nm or less.

[0033] [Average aspect ratio (average fiber length / average fiber diameter)] From the viewpoint of increasing the viscosity of the metal particle-containing composition, the average aspect ratio (average fiber length / average fiber diameter) of component (A) is preferably 5 or more, more preferably 10 or more, even more preferably 30 or more, even more preferably 50 or more, even more preferably 70 or more, even more preferably 80 or more, and is preferably 300 or less, more preferably 200 or less, even more preferably 120 or less, even more preferably 95 or less. The average fiber diameter, average fiber length and average aspect ratio of component (A) can be determined by the method described in the Examples below.

[0034] [Amount and introduction rate of modifying group] From the viewpoint of increasing the viscosity of the metal particle-containing composition, the amount of the modifying group bonded in component (A) is preferably 0.01 mmol / g or more, more preferably 0.1 mmol / g or more, even more preferably 0.3 mmol / g or more, even more preferably 0.6 mmol / g or more, and is preferably 3.0 mmol / g or less, more preferably 2.0 mmol / g or less, even more preferably 1.4 mmol / g or less, even more preferably 1.0 mmol / g or less. The introduction rate of the modifying group in component (A) is preferably 10 mol% or more, more preferably 15 mol% or more, even more preferably 20 mol% or more, even more preferably 30 mol% or more, even more preferably 40 mol% or more, and even more preferably 50 mol% or more from the viewpoint of dispersibility, and is preferably 100 mol% or less, more preferably 90 mol% or less, and even more preferably 80 mol% or less from the viewpoint of improving the productivity of the modified cellulose. When any two or more kinds of modifying groups are simultaneously introduced as the modifying group, it is preferable that the introduction rate is within the above range as long as the total introduction rate does not exceed the upper limit of 100 mol%. The bonded amount and introduction rate of the modifying group can be adjusted by the type and amount of the modifying compound, the reaction temperature, the reaction time, the type of solvent, etc. "Bound amount of modifying group (mmol / g)" and "introduction rate (mol%)" refer to the amount and ratio of the modifying group introduced (bonded) to the anionic group in the modified cellulose fiber. For example, when the anionic group is a carboxy group, the bound amount and introduction rate of the modifying group in the modified cellulose fiber are calculated by the method described in the Examples below.

[0035] [Glucose unit] The content of glucose units in component (A) is preferably 1 mass% or more, more preferably 10 mass% or more, and even more preferably 30 mass% or more, from the viewpoint of increasing the viscosity of the metal particle-containing composition, and from the viewpoint of increasing the content of metal particles as component (B), it is preferably 95 mass% or less, more preferably 80 mass% or less, even more preferably 70 mass% or less, even more preferably 60 mass% or less, even more preferably 50 mass% or less, and even more preferably 40 mass% or less.

[0036] The content of component (A) in the metal particle-containing composition of the present invention is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, and even more preferably 0.1% by mass or more from the viewpoint of increasing the viscosity of the metal particle-containing composition, and is preferably 1.0% by mass or less, more preferably 0.6% by mass or less, even more preferably 0.4% by mass or less, even more preferably 0.3% by mass or less, and even more preferably 0.2% by mass or less from the viewpoint of increasing the content of metal particles as component (B). More specifically, it is preferably 0.01% by mass or more and 1.0% by mass or less, more preferably 0.05% by mass or more and 0.6% by mass or less, even more preferably 0.1% by mass or more and 0.4% by mass or less, even more preferably 0.1% by mass or more and 0.3% by mass or less, and even more preferably 0.1% by mass or more and 0.2% by mass or less.

[0037] In the metal particle-containing composition of the present invention, the content of component (A) relative to 100 parts by mass of component (B) is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, and even more preferably 0.1 parts by mass or more from the viewpoint of increasing the viscosity of the metal particle-containing composition, and is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, even more preferably 1 part by mass or less, even more preferably 0.5 parts by mass or less, and even more preferably 0.2 parts by mass or less from the viewpoint of increasing the content of metal particles as component (B). More specifically, it is preferably 0.01 parts by mass or more and 10 parts by mass or less, more preferably 0.05 parts by mass or more and 5 parts by mass or less, even more preferably 0.1 parts by mass or more and 1 part by mass or less, even more preferably 0.1 parts by mass or more and 0.5 parts by mass or less, and even more preferably 0.1 parts by mass or more and 0.2 parts by mass or less.

[0038] The content of glucose units contained in component (A) in the metal particle-containing composition of the present invention is preferably 0.01% by mass or more, more preferably 0.02% by mass or more, and even more preferably 0.03% by mass or more from the viewpoint of increasing the viscosity of the metal particle-containing composition, and is preferably 1% by mass or less, more preferably 0.5% by mass or less, even more preferably 0.2% by mass or less, and even more preferably 0.1% by mass or less from the viewpoint of increasing the content of metal particles as component (B). More specifically, it is preferably 0.01% by mass or more and 1% by mass or less, more preferably 0.02% by mass or more and 0.5% by mass or less, even more preferably 0.03% by mass or more and 0.2% by mass or less, and even more preferably 0.03% by mass or more and 0.1% by mass or less.

[0039] In the metal particle-containing composition of the present invention, the content of glucose units contained in component (A) relative to 100 parts by mass of component (B) is preferably 0.003 parts by mass or more, more preferably 0.005 parts by mass or more, even more preferably 0.01 parts by mass or more, and even more preferably 0.03 parts by mass or more, from the viewpoint of increasing the viscosity of the metal particle-containing composition, and is preferably 5 parts by mass or less, more preferably 1 part by mass or less, even more preferably 0.5 parts by mass or less, even more preferably 0.2 parts by mass or less, and even more preferably 0.1 parts by mass or less, from the viewpoint of increasing the content of metal particles as component (B). More specifically, it is preferably 0.003 parts by mass or more and 5 parts by mass or less, more preferably 0.005 parts by mass or more and 5 parts by mass or less, even more preferably 0.01 parts by mass or more and 1 part by mass or less, even more preferably 0.03 parts by mass or more and 0.5 parts by mass or less, even more preferably 0.03 parts by mass or more and 0.2 parts by mass or less, and even more preferably 0.03 parts by mass or more and 0.1 parts by mass or less.

[0040] <Component (B): Metal particles> The metal particle-containing composition of the present invention contains metal particles as component (B) (hereinafter, sometimes simply referred to as "component (B)").

[0041] Furthermore, since component (B) is metal particles, the metal particle-containing composition of the present invention can be used as a printing paste or ink, and the coating film can be sintered to form a conductive member. Examples of metals (metal atoms) constituting the metal particles include Group 4 transition metals such as titanium and zirconium, Group 5 transition metals such as vanadium and niobium, Group 6 transition metals such as chromium, molybdenum, and tungsten, Group 7 transition metals such as manganese, technetium, and rhenium, Group 8 transition metals such as iron and ruthenium, Group 9 transition metals such as cobalt, rhodium, and iridium, Group 10 transition metals such as nickel, palladium, and platinum, Group 11 transition metals such as copper, silver, and gold, Group 12 transition metals such as zinc and cadmium, Group 13 metals such as aluminum, gallium, and indium, and Group 14 metals such as germanium, tin, and lead. The metals constituting the metal particles may be used as a single metal, or may be used in combination of two or more types as an alloy. In particular, from the viewpoint of reducing the resistivity of the resulting metal film, the metal constituting the metal particles preferably contains at least one metal selected from the group consisting of metals in Groups 4 to 14 and Periods 4 to 6, and more preferably contains at least one metal selected from the group consisting of transition metals in Groups 4 to 11 and Periods 4 to 6. More specifically, from the viewpoint of reducing the resistivity of the resulting metal film, the metal constituting the metal particles preferably contains at least one selected from the group consisting of copper, silver, nickel and tin, more preferably contains copper or silver, and even more preferably contains copper. The total content of metals of Groups 4 to 14 and Periods 4 to 6 in component (B) is preferably 80 mass % or more, more preferably 90 mass % or more, even more preferably 95 mass % or more, even more preferably 98 mass % or more, and even more preferably 99 mass % or more, from the viewpoint of reducing the resistivity of the resulting metal film. The total content of the transition metals of Groups 4 to 11 and Periods 4 to 6 in component (B) is preferably 80 mass % or more, more preferably 90 mass % or more, even more preferably 95 mass % or more, even more preferably 98 mass % or more, and even more preferably 99 mass % or more, from the viewpoint of reducing the resistivity of the resulting metal film. The total content of at least one selected from the group consisting of copper, silver, nickel and tin in component (B) is preferably 80 mass % or more, more preferably 90 mass % or more, even more preferably 95 mass % or more, even more preferably 98 mass % or more, and even more preferably 99 mass % or more, from the viewpoint of reducing the resistivity of the obtained metal film. From the viewpoint of reducing the resistivity of the resulting metal film, the content of copper or silver in component (B) is preferably 80 mass % or more, more preferably 90 mass % or more, even more preferably 95 mass % or more, even more preferably 98 mass % or more, and even more preferably 99 mass % or more. From the viewpoint of reducing the resistivity of the resulting metal film, the metal constituting the metal particles is preferably one or more selected from the group consisting of metals in Groups 4 to 14 and Periods 4 to 6, and more preferably one or more selected from the group consisting of transition metals in Groups 4 to 11 and Periods 4 to 6. More specifically, from the viewpoint of reducing the resistivity of the resulting metal film, the metal constituting the metal particles is preferably copper, silver, nickel or tin, more preferably copper or silver, and even more preferably copper. The type of metal can be confirmed by high-frequency inductively coupled plasma atomic emission spectrometry.

[0042] The average particle size of component (B) is, from the viewpoints of improving the dispersion stability of the metal particles and increasing the viscosity of the metal particle-containing composition, preferably 0.1 μm or more, more preferably 0.3 μm or more, even more preferably 0.4 μm or more, even more preferably 0.5 μm or more, even more preferably 0.6 μm or more, and even more preferably 0.7 μm or more, and from the same viewpoints as above, it is preferably 10 μm or less, more preferably 8 μm or less, even more preferably 6 μm or less, even more preferably 4 μm or less, and even more preferably 2 μm or less. The average particle size of component (B) is the particle size at 50% cumulative volume (D50) obtained by measuring the volume-based particle size distribution based on the laser diffraction / scattering method. When using a product as component (B), the average particle size of component (B) may be the value in the manufacturer's catalog. The particle size of component (B) can also be evaluated by measuring the fraction that passes through a sieve. From the viewpoint of improving the dispersion stability of the metal particles and increasing the viscosity of the metal particle-containing composition, the particle size of component (B) is preferably 95% or more passing through a sieve with an opening of 300 μm, more preferably 95% or more passing through a sieve with an opening of 150 μm, and even more preferably 95% or more passing through a sieve with an opening of 75 μm. In addition, when a product is obtained and used as component (B), the particle size of component (B) may be the value in the manufacturer's catalog or product specification.

[0043] From the viewpoint of the electrical conductivity of the resulting conductive member, the specific surface area of ​​component (B) is preferably 0.1 m 2 / g or more, more preferably 0.3m 2 / g or more, more preferably 0.5m 2 / g or more, and preferably 3.0m 2 / g or less, more preferably 2.0m 2 / g or less, more preferably 1.5m 2 / g or less. The specific surface area of ​​component (B) can be measured by the BET method. When a product is procured and used as component (B), the specific surface area of ​​component (B) may be the value in the manufacturer's catalog.

[0044] The content of component (B) per 100 parts by mass of solids in the metal particle-containing composition of the present invention is, from the viewpoint of increasing the content of metal particles as component (B), 70 parts by mass or more, preferably 80 parts by mass or more, more preferably 85 parts by mass or more, even more preferably 90 parts by mass or more, even more preferably 95 parts by mass or more, even more preferably 96 parts by mass or more, even more preferably 97 parts by mass or more, and even more preferably 98 parts by mass or more, and from the viewpoint of the dispersion stability of the metal particles and the viewpoint of increasing the viscosity of the metal particle-containing composition, it is preferably 99.9 parts by mass or less.

[0045] Furthermore, the content of component (B) in the metal particle-containing composition of the present invention is, from the viewpoint of increasing the content of metal particles as component (B), preferably 50 mass% or more, more preferably 60 mass% or more, even more preferably 70 mass% or more, even more preferably 80 mass% or more, and even more preferably 85 mass% or more, and from the viewpoint of the dispersion stability of the metal particles and increasing the viscosity of the metal particle-containing composition, it is preferably 97 mass% or less, more preferably 95 mass% or less, even more preferably 93 mass% or less, and even more preferably 91 mass% or less.

[0046] <Component (C): An organic compound that is liquid at 25°C and 1 atmosphere> The metal particle-containing composition of the present invention contains, as component (C), an organic compound that is liquid at 25° C. and 1 atmospheric pressure (hereinafter sometimes simply referred to as “component (C)”). From the viewpoint of workability when used together with metal particles, component (C) is preferably a hydrophobic solvent. The dissolution amount of the hydrophobic solvent per 100 g of water (at 20° C. and 1 atm) is preferably 100 g or less, more preferably 50 g or less, even more preferably 30 g or less, and even more preferably 10 g or less.

[0047] Specific examples of the component (C) include alcohol-based solvents such as methanol, normal and isopropanol, t-butanol, 1-butanol, 1-hexanol, hexanal, and glycerin; ketone-based solvents such as acetone, methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK), cyclohexanone, methylhexyl ketone, diisobutyl ketone, diacetone alcohol, and isophorone; ether-based solvents such as diethyl ether, tetrahydrofuran (THF), and dioxane; methyl acetate, ethyl acetate, butyl acetate, ethyl lactate, and polyvalent carboxylate esters (e.g., phthalates, succinates, azides, etc.). ester-based solvents such as carboxylic acid esters, fatty acid esters of aliphatic polyols such as glycerin; highly polar solvents such as N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), ethylene carbonate, N,N-dimethylacetamide (DMAc), N-methylpyrrolidone; halogen-based solvents such as methylene chloride, dichloromethane, chloroform, trichloroethylene, perchloroethylene, and chlorobenzene; non-aromatic hydrocarbon-based solvents such as hexane, petroleum ether, liquid paraffin, squalane, and squalene; aromatic hydrocarbon-based solvents such as benzene, toluene, and xylene; nitrile-based solvents such as acetonitrile;Glycol ether-based solvents such as t-butyl glycol, methyl diglycol, ethyl diglycol, diethylene glycol, triethylene glycol, butyl diglycol, 1-methoxy-2-propanol, methyl dipropylene glycol, 3-methoxybutanol, 3-methyl-3-methoxybutanol, (mono-, di-, tri-, poly)ethylene glycol methyl ether, ethylene glycol monophenyl ether, (mono-, di-, tri-, poly)ethylene glycol dimethyl (ethyl) ether, (mono-, di-, tri-, poly)ethylene glycol monobutyl ether, polyethylene glycol, methoxypolyethylene glycol, polyoxyethylene bisphenol A, polyoxypropylene bisphenol A, etc. (Glycol ether-based solvents include the following glycol ether (ester)-based solvents: butyl cellosolve acetate, ethyl carbitol acetate, butyl carbitol acetate, propylene glycol ... Glycol ether ester solvents such as glycol monomethyl ether acetate, methoxybutyl acetate, methyl methoxybutyl acetate, ethyl 3-ethoxypropionate, propylene glycol monomethyl ether propionate, and dimethyl carbonate; polymerizable compounds, such as epoxy prepolymers (e.g., bisphenol type, novolac type, biphenyl type, biphenyl aralkyl type, aryl alkylene type, tetraphenylolethane type, naphthalene type, anthracene type, phenoxy type, dicyclopentadiene type, norbornene type, adamantane type, fluorene type, glycidyl methacrylate copolymerization system, etc.); isocyanates (e.g., aromatic systems such as tolylene diisocyanate and diphenylmethane diisocyanate, and aliphatic systems such as hexamethylene diisocyanate, xylylene diisocyanate, isophorone diisocyanate, and tetramethylxylylene diisocyanate);Acrylic prepolymers (e.g., methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, butyl methacrylate, n-hexyl acrylate, n-hexyl methacrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, nonanediol diacrylate, phenoxyethyl acrylate, (meth)acrylates of bisphenol A-alkylene oxide adducts, epoxy (meth)acrylates (bisphenol A type epoxy (meth)acrylate, novolac type epoxy (meth)acrylate, etc.); polyester (meth)acrylates acrylates (e.g., aliphatic polyester type (meth)acrylates, aromatic polyester type (meth)acrylates, etc.); urethane (meth)acrylates (polyester type urethane (meth)acrylates, polyether type urethane (meth)acrylates, etc.); silicone (meth)acrylates, cyanoacrylate mono(meth)acrylates, etc.] and oligomers of these polymerizable compounds; natural resins such as rosin; fatty acids such as oleic acid, palmitic acid, stearic acid, etc.; animal and vegetable oils such as olive oil, jojoba oil, castor oil, etc.; silicone oils, fluorine-based inert liquids, process oils, etc.;

[0048] When the metal particle-containing composition of the present invention is used as a printing paste or ink, it is preferable that component (C) functions as a dispersion medium. From the viewpoint of dispersion stability of the metal particles (component (B)) and of increasing the viscosity of the metal particle-containing composition to improve print dimensionality, it is preferable that component (C) as a dispersion medium contains at least one selected from the group consisting of (poly)alkylene glycol, (poly)alkylene glycol derivative, terpene alcohol, glycerin (boiling point: 290°C, molecular weight: 92) and glycerin derivative. In the present specification, the term "(poly)alkylene glycol" refers to at least one selected from the group consisting of alkylene glycol and polyalkylene glycol. The term "(poly)alkylene glycol derivative" has the same meaning. In addition, in the present specification, the term "polyalkylene glycol" refers to a glycol in which two or more alkylene glycol structures are linked together.

[0049] Examples of (poly)alkylene glycols include ethylene glycol (boiling point: 197° C., molecular weight: 62), propylene glycol (boiling point: 188° C., molecular weight: 76), diethylene glycol (boiling point: 244° C., molecular weight: 106), triethylene glycol (boiling point: 287° C., molecular weight: 150), dipropylene glycol (boiling point: 232° C., molecular weight: 134), tripropylene glycol (boiling point: 273° C., molecular weight: 192), tetrapropylene glycol (boiling point: 300°C or higher, molecular weight: 250), polyethylene glycol (number average molecular weight is preferably 180 to 1000, more preferably 180 to 600, and even more preferably 180 to 400), polypropylene glycol (number average molecular weight is preferably 232 to 1000, more preferably 232 to 600, and even more preferably 232 to 500), 2-ethyl-1,3-hexanediol (boiling point: 244°C, molecular weight: 146), etc. Among them, one or more selected from the group consisting of diethylene glycol, dipropylene glycol, and polyethylene glycol (number average molecular weight is preferably 180 to 1000, more preferably 180 to 600, and even more preferably 180 to 400) are more preferred, and one or more selected from the group consisting of diethylene glycol and polyethylene glycol (average molecular weight is 180 to 400).

[0050] Examples of the (poly)alkylene glycol derivative include compounds in which the terminal hydroxyl groups of the (poly)alkylene glycols are etherified or esterified. Examples of the compound in which the hydroxy groups at both ends of the polyalkylene glycol are etherified or esterified include diethylene glycol dimethyl ether (boiling point: 162°C, molecular weight: 134), diethylene glycol dibutyl ether (boiling point: 254°C, molecular weight: 218), triethylene glycol dimethyl ether (boiling point: 216°C, molecular weight: 178), diethylene glycol monoethyl ether acetate (boiling point: 217°C, molecular weight: 176), diethylene glycol monobutyl ether acetate (boiling point: 247°C, molecular weight: 204), and the like. Examples of the compound in which the hydroxy group at one end of the polyalkylene glycol is etherified or esterified include diethylene glycol monoethyl ether (boiling point: 202° C., molecular weight: 134), diethylene glycol monobutyl ether (boiling point: 231° C., molecular weight: 162), diethylene glycol monohexyl ether (boiling point: 258° C., molecular weight: 190), etc. Among these, diethylene glycol monobutyl ether is preferred.

[0051] Examples of terpene alcohols include monoterpene alcohols such as α-terpineol (boiling point: 219° C., molecular weight: 154), linalool (boiling point: 198° C., molecular weight: 154), geraniol (boiling point: 229° C., molecular weight: 154), and citronellol (boiling point: 225° C., molecular weight: 156). Among these, α-terpineol is preferred.

[0052] The glycerin derivative is not particularly limited as long as it is a solvent containing a structure derived from glycerin, and examples thereof include ether derivatives of glycerin, ester derivatives of glycerin, polyglycerin, and alkylene oxide adducts of glycerin (e.g., ethylene oxide adducts and propylene oxide adducts). Examples of polyglycerin include diglycerin and triglycerin, and examples of commercially available polyglycerin include polyglycerin #310, polyglycerin #500, and polyglycerin #750 manufactured by Sakamoto Pharmaceutical Co., Ltd. Examples of ether derivatives of glycerin include 3-(2-ethylhexyloxy)-1,2-propanediol (boiling point: 325°C, molecular weight: 204), and the like. Examples of ester derivatives of glycerin include glyceryl tributyrate (boiling point: 305°C, molecular weight: 302), and the like.

[0053] From the viewpoint of the dispersion stability of the metal particles and of increasing the viscosity of the metal particle-containing composition to improve printing dimensional properties, component (C) preferably contains at least one selected from the group consisting of (poly)alkylene glycol, (poly)alkylene glycol derivatives, and terpene alcohols, more preferably contains at least one selected from diethylene glycol, dipropylene glycol, polyethylene glycol (number average molecular weight preferably being 180 or more and 1000 or less, more preferably 180 or more and 600 or less, even more preferably 180 or more and 400 or less), α-terpineol, and diethylene glycol monobutyl ether, and even more preferably contains at least one selected from diethylene glycol, polyethylene glycol (number average molecular weight being 180 or more and 400 or less), α-terpineol, and diethylene glycol monobutyl ether.

[0054] Furthermore, when component (B) is a sinterable metal particle, the boiling point of component (C) at 1 atmospheric pressure is, from the viewpoint of enhancing the sinterability of the metal particle, preferably 180° C. or higher, more preferably 200° C. or higher, even more preferably 210° C. or higher, and even more preferably 215° C. or higher, and from the same viewpoint as above, is preferably 400° C. or lower, more preferably 360° C. or lower, even more preferably 330° C. or lower, and even more preferably 300° C. or lower. When two or more liquid organic compounds are used in combination as component (C), the boiling point of component (C) is a weighted average value weighted by the content (mass%) of the organic compound in each liquid.

[0055] From the viewpoint of enhancing the sinterability of the metal particles, the molecular weight of component (C) is preferably 60 or more, more preferably 100 or more, even more preferably 130 or more, and even more preferably 150 or more, and from the same viewpoint as above, it is preferably 450 or less, more preferably 400 or less, even more preferably 350 or less, and even more preferably 300 or less. When two or more liquid organic compounds are used in combination as component (C), the molecular weight of component (C) is a weighted average weighted by the content (mass%) of each liquid organic compound. In particular, from the viewpoint of enhancing the sinterability of the metal particles, it is preferable that the boiling point of component (C) is 180° C. or higher and the molecular weight of component (C) is 450 or less.

[0056] The total content of (poly)alkylene glycol, (poly)alkylene glycol derivative, terpene alcohol, glycerin and glycerin derivative (hereinafter also referred to as "component C1") in component (C) is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, even more preferably 99% by mass or more, even more preferably 99.9% by mass or more, even more preferably substantially 100% by mass, from the viewpoint of increasing the sinterability of metal particles. Here, "substantially 100% by mass" means that it may contain components that are unintentionally contained. Examples of components that are unintentionally contained include components other than component C1 that are contained in component C1.

[0057] The total content of (poly)alkylene glycol, (poly)alkylene glycol derivative and terpene alcohol (hereinafter also referred to as "component C2") in component (C) is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, even more preferably 99% by mass or more, even more preferably 99.9% by mass or more, even more preferably substantially 100% by mass, from the viewpoint of increasing the sinterability of metal particles. Here, "substantially 100% by mass" means that it may contain components that are unintentionally contained. Examples of components that are unintentionally contained include components other than component C2 that are contained in component C2.

[0058] The total content of diethylene glycol, polyethylene glycol (number average molecular weight 180 to 400), α-terpineol, and diethylene glycol monobutyl ether (hereinafter also referred to as "component C3") in component (C) is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, even more preferably 99% by mass or more, even more preferably 99.9% by mass or more, and even more preferably substantially 100% by mass, from the viewpoint of increasing the sinterability of the metal particles. Here, "substantially 100% by mass" means that it may contain components that are unintentionally contained. Examples of components that are unintentionally contained include components other than component C3 that are contained in component C3.

[0059] The content of component (C) in the metal particle-containing composition of the present invention is preferably 4 mass% or more, more preferably 5 mass% or more, and even more preferably 6 mass% or more from the viewpoint of improving the dispersion stability of the metal particles, and is preferably 40 mass% or less from the viewpoint of handling the metal particle-containing composition. In particular, when the metal particle-containing composition of the present invention is used as a printing paste or ink, from the viewpoint of improving the printing dimensional properties of the metal particle-containing composition, the content of component (C) is more preferably 30 mass % or less, even more preferably 20 mass % or less, even more preferably 15 mass % or less, and even more preferably 13 mass % or less.

[0060] In the metal particle-containing composition of the present invention, the content of component (C) relative to 100 parts by mass of component (B) is preferably 1 part by mass or more, more preferably 5 parts by mass or more, even more preferably 8 parts by mass or more, and even more preferably 10 parts by mass or more from the viewpoint of improving the dispersion stability of the metal particle-containing composition, and is preferably 20 parts by mass or less, more preferably 18 parts by mass or less, and even more preferably 15 parts by mass or less from the viewpoint of increasing the viscosity of the metal particle-containing composition. More specifically, it is preferably 1 part by mass or more and 20 parts by mass or less, more preferably 5 parts by mass or more and 18 parts by mass or less, even more preferably 8 parts by mass or more and 15 parts by mass or less, and even more preferably 10 parts by mass or more and 15 parts by mass or less.

[0061] <Other ingredients> The metal particle-containing composition of the present invention may contain water within a range that does not impair the effects of the present invention. The content of water in the metal particle-containing composition is preferably 5% by mass or less, more preferably 1% by mass or less, even more preferably 0.5% by mass or less, even more preferably 0.1% by mass or less, and even more preferably 0.01% by mass or less, from the viewpoint of suppressing oxidation of the metal particles when the metal particles are metal, and from the viewpoint of increasing the dispersion stability, storage stability, and viscosity of the metal particle-containing composition.

[0062] In addition, the metal particle-containing composition of the present invention may contain various additives other than the above components, as long as the effects of the present invention are not impaired. Examples of the additives include plasticizers, crystal nucleating agents, fillers (organic fillers), hydrolysis inhibitors, flame retardants, antioxidants, lubricants such as hydrocarbon waxes and anionic surfactants, ultraviolet absorbers, antistatic agents, antifogging agents, light stabilizers, pigments different from component (B), antifungal agents, antibacterial agents, foaming agents, surfactants; starches, polysaccharides such as alginic acid; natural proteins such as gelatin, glue, and casein; tannins; fragrances; flow regulators; leveling agents; conductive agents; ultraviolet dispersion agents; deodorants, etc. Furthermore, it is also possible to add other polymeric materials and other compositions as long as the effects of the present invention are not impaired. The content of the additive in the metal particle-containing composition of the present invention is preferably 5% by mass or less, more preferably 1% by mass or less, and even more preferably 0.5% by mass or less.

[0063] [Method for producing metal particle-containing composition] The metal particle-containing composition of the present invention can be produced, for example, by mixing components (A), (B), and (C) and, if necessary, the above-mentioned additives. For example, the above-mentioned components can be mixed by stirring using a known mixing device such as a rotation-revolution type mixing device, or by kneading using a known kneading machine such as an internal kneader, a single-screw or twin-screw extruder, a roll mill, or an open-roll type kneader, or by a solvent casting method, or by shearing using a shearing device such as a high-shear processing machine.

[0064] [Physical Properties of Metal Particle-Containing Composition] The viscosity (Pa s) of the metal particle-containing composition of the present invention at 25°C is -1With these conditions in mind, from the viewpoint of handleability of the metal particle-containing composition and from the viewpoint of improving the printing dimensionality of the metal particle-containing composition, the molecular weight is preferably 30 or more, more preferably 50 or more, even more preferably 90 or more, even more preferably 100 or more, even more preferably 120 or more, and even more preferably 140 or more; on the other hand, from the viewpoint of workability when used as a metal particle-containing composition, the molecular weight is preferably 500 or less, more preferably 400 or less, and even more preferably 300 or less. The viscosity in this specification can be measured by a method using a rheometer as described in the Examples below.

[0065] [Uses of metal particle-containing composition] The metal particle-containing composition of the present invention can be used in various products without any particular restrictions. Specific examples of products to which the metal particle-containing composition of the present invention can be applied include food and beverages, cosmetics, quasi-drugs, medicines, daily necessities, feed, miscellaneous goods, agricultural chemicals, and chemical industrial products. More specifically, in the fields of home appliance parts, electronic materials (electronics), packaging containers, aerospace, civil engineering and construction, automobiles, and vehicle-mounted products, resin molding materials, electrical insulating materials, paints, printing pastes, inks, coating agents, adhesives, repair materials, pressure-sensitive adhesives, lubricants, sealing materials, heat insulating materials, sound absorbing materials, artificial leather materials, electronic materials, semiconductor materials, tires, automobile parts, fiber composite materials, and the like can be mentioned. Among them, it is preferably used as a printing paste and ink. It is also preferably used as an electronic material, an optical material, or a structural material.

[0066] In particular, the metal particle-containing composition of the present invention can be used to form conductive members for various electronic and electrical devices because the component (B) is metal particles. The conductive members are preferably used for adhesives such as solder; antennas such as RFID (radio frequency identifier) ​​tags; capacitors such as MLCCs (multilayer ceramic capacitors); electronic paper; image display devices such as liquid crystal displays and organic EL displays; organic EL elements; organic transistors; wiring boards such as printed wiring boards and flexible wiring boards; organic solar cells; sensors such as flexible sensors, and the like. Among these, the metal particle-containing composition of the present invention is preferably used to bond a plurality of metal members.

[0067] [Method of producing the membrane] The method for producing a film using the metal particle-containing composition of the present invention includes a step of applying the metal particle-containing composition onto a substrate, and preferably further includes a step of drying the applied film of the metal particle-containing composition.

[0068] Specifically, the metal particle-containing composition is applied to a substrate, for example, a hard surface made of glass, resin, metal, ceramics, concrete, wood, stone, etc., or to fibers, skin, hair, paper, etc. It can also be preferably used in fields such as coatings for various surfaces disposed outdoors, for example, road facilities such as signs, road signs, and traffic lights, bodies, glass surfaces and headlights of automobiles, airplanes, trains, ships, etc., roofs, exterior walls, windows, etc. of buildings, and solar panels, etc.

[0069] The thickness of the coating film of the metal particle-containing composition applied onto a substrate is preferably 10 μm or more, more preferably 20 μm or more, and even more preferably 30 μm or more from the viewpoint of film durability, and is preferably 2000 μm or less, and more preferably 1500 μm or less from the viewpoint of coatability.

[0070] The coating of the metal particle-containing composition can then be dried to obtain a film. The drying conditions may be under reduced pressure or normal pressure, and the temperature range is preferably 15° C. to 75° C. The drying time is preferably 10 minutes to 24 hours.

[0071] The thickness of the film obtained by the manufacturing method of the present invention is not particularly limited, and from the viewpoint of film durability, it is preferably 1 μm or more, more preferably 3 μm or more, and even more preferably 5 μm or more, and from the viewpoint of economy, it is preferably 2000 μm or less, more preferably 1200 μm or less, even more preferably 500 μm or less, and even more preferably 200 μm or less. The thickness of the film can be adjusted to a desired value by setting the coating thickness using a coating tool such as an applicator, or by adjusting the amount of coating by a spray or the ratio of the medium.

[0072] [Method for manufacturing conductive member] The method for producing a conductive member of the present invention includes a step of applying a metal particle-containing composition onto a substrate. From the viewpoint of electrical conductivity, the metal particle-containing composition preferably contains metal particles as component (B).

[0073] Examples of the conductive member include a joint such as solder, and an electronic circuit. The substrate may be made of, for example, glass, resin, metal, ceramics, or the like.

[0074] In particular, when the conductive member is a bonded body, the method preferably further includes a step of placing the metal particle-containing composition between a plurality of metal members and heating the composition. In this way, when the metal particle-containing composition contains sinterable metal particles as component (B), the metal particles can be sintered to form a bonded body having excellent electrical conductivity. Here, at least one of the metal members is the substrate.

[0075] The temperature of the heat treatment in the heating step is preferably 100°C or higher, more preferably 150°C or higher, and even more preferably 200°C or higher from the viewpoints of bonding strength and electrical conductivity, and is preferably 350°C or lower, more preferably 300°C or lower, and even more preferably 260°C or lower from the viewpoints of improving low-temperature sintering properties and bonding strength. The heat treatment in the heating step can be carried out either without pressure or under pressure, but from the viewpoint of bonding strength and electrical conductivity, it is preferably carried out under pressure. The pressure of the heat treatment in the heating step is preferably 5 MPa or more, more preferably 8 MPa or more, even more preferably 10 MPa or more, even more preferably 15 MPa or more, from the viewpoint of improving low-temperature sintering property and bonding strength, and is preferably 50 MPa or less, more preferably 30 MPa or less, even more preferably 20 MPa or less, from the viewpoint of productivity. The heat treatment time in the heating step can be appropriately adjusted depending on the temperature and pressure of the heat treatment. The atmosphere in the heating step may be an air atmosphere, an inert gas atmosphere such as nitrogen gas, or a reducing gas atmosphere such as hydrogen gas. From the viewpoints of inhibiting oxidation of the metal and safety, however, a nitrogen gas atmosphere is more preferable.

[0076] Examples of metal members to be joined in the present invention include metal-based or metal substrates such as gold substrates, gold-plated substrates, silver substrates, silver-plated metal substrates, copper substrates, palladium substrates, palladium-plated metal substrates, platinum substrates, platinum-plated metal substrates, aluminum substrates, nickel substrates, nickel-plated metal substrates, tin substrates, and tin-plated metal substrates; metal parts such as electrodes of electrically insulating substrates; etc. The multiple metal members used in the present invention may be the same type of metal members or different types of metal members. Among these, the metal member preferably includes at least one selected from a gold substrate, a gold-plated substrate, a silver substrate, a silver-plated metal substrate, a copper substrate, a palladium substrate, a palladium-plated metal substrate, a platinum substrate, a platinum-plated metal substrate, an aluminum substrate, a nickel substrate, a nickel-plated metal substrate, a tin substrate, a tin-plated metal substrate, and a metal portion of an electrically insulating substrate. The joining of metal members in the present invention can be used for joining chip components such as capacitors and resistors to circuit boards; joining semiconductor chips such as memories, diodes, transistors, ICs and CPUs to lead frames or circuit boards; joining high-heat-generating semiconductor chips to cooling plates, etc.

[0077] Methods for applying the metal particle-containing composition to a metal member include various coating methods such as slot die coating, dip coating, spray coating, spin coating, doctor blading, knife edge coating, bar coating, etc., and various patterning printing methods such as stencil printing, screen printing, flexographic printing, gravure printing, offset printing, dispenser printing, inkjet printing, etc. Among these, stencil printing is preferred. The amount of the metal particle-containing composition applied to the metal members can be appropriately adjusted depending on the size and type of the metal members to be joined. EXAMPLES

[0078] The present invention will be described in more detail below with reference to examples. However, the scope of the present invention is not limited to such examples. "Normal pressure" refers to 101.3 kPa, and "normal temperature" refers to 25°C. Various physical properties were measured or calculated by the following methods.

[0079] [Average fiber diameter, average fiber length, and average aspect ratio (average fiber length / average fiber diameter) of anionically modified cellulose fibers, shortened anionically modified cellulose fibers, and modified cellulose fibers] Depending on the size of the cellulose fibers to be measured, one of the following measurement methods (1) and (2) was selected for measurement. (1) Measurement of modified cellulose fibers Deionized water or N,N-dimethylformamide (DMF) was added to the cellulose fibers to be measured to prepare a dispersion with a content of 0.0001% by mass. The dispersion was dropped onto mica and dried to prepare an observation sample, and the fiber height (difference in height between where the fibers are present and where they are not present) of the cellulose fibers in the observation sample was measured using an atomic force microscope (AFM) (Nanoscope II Tapping mode AFM manufactured by Digital Instrument; the probe used was Point Probe (NCH) manufactured by Nanosensors). At that time, 100 cellulose fibers were extracted from a microscope image in which the cellulose fibers could be confirmed, and the average fiber diameter was calculated from the fiber height. The average fiber length was calculated from the distance in the fiber direction. In addition, the average aspect ratio (average fiber length / average fiber diameter) was calculated from the calculated average fiber diameter and average fiber length. (2) Measurement of anion-modified cellulose fiber and shortened anion-modified cellulose fiber Deionized water was added to the cellulose fibers to be measured to prepare a dispersion with a content of 0.01% by mass. The dispersion was measured using a wet dispersion type image analysis particle size distribution meter (manufactured by Jusco International, IF-3200) under the following conditions: front lens: 2x, telecentric zoom lens: 1x, image resolution: 0.835 μm / pixel, syringe inner diameter: 6515 μm, spacer thickness: 500 μm, image recognition mode: ghost, threshold: 8, analysis sample amount: 1 mL, sampling: 15%. The length of the short axis of the cellulose fibers approximated as a rectangle was taken as the fiber diameter, and the length of the long axis was taken as the fiber length. Each value was measured for 100 cellulose fibers, and the average value was calculated. In addition, the average aspect ratio (average fiber length / average fiber diameter) was calculated from the calculated average fiber diameter and average fiber length. Incidentally, "average aspect ratio (average fiber length / average fiber diameter)" is also simply referred to as "aspect ratio".

[0080] [Anionic group (carboxy group) content of anionically modified cellulose fiber, shortened anionically modified cellulose fiber, and modified cellulose fiber] Cellulose fibers to be measured with a dry mass of 0.5 g were placed in a beaker, and deionized water or a mixed solvent of methanol / deionized water = 2 / 1 (volume ratio) was added to make a total of 55 mL, to which 5 mL of 0.01 M sodium chloride aqueous solution was added to prepare a dispersion. The dispersion was stirred until the cellulose fibers to be measured were sufficiently dispersed. 0.1 M hydrochloric acid was added to the dispersion to adjust the pH to 2.5 to 3, and an automatic titration device (manufactured by DKK-TOA, AUT-701) was used to drop 0.05 M sodium hydroxide aqueous solution into the dispersion under the condition of a waiting time of 60 seconds, and the conductivity and pH value were measured every minute. The measurement was continued until the pH was about 11, and a conductivity curve was obtained. The titration amount of the sodium hydroxide aqueous solution was determined from this conductivity curve, and the anionic group content of the cellulose fibers to be measured was calculated by the following formula. Anionic group content (mmol / g) = [amount of sodium hydroxide solution titrated (mL) × concentration of sodium hydroxide solution (0.05M)] / [mass of cellulose fiber to be measured (0.5g)]

[0081] [Modification group bond amount and introduction rate of modified cellulose fiber] The amount of modified group bonded was determined by the following IR measurement method, and the amount of bonded and the introduction rate were calculated by the following formula. Specifically, the IR measurement was performed by measuring the infrared absorption spectrum of the dried modified cellulose fiber by the ATR method using an infrared absorption spectrometer (IR) (Nicolet 6700, manufactured by Thermo Fisher Scientific), and the amount of modified group bonded and the introduction rate were calculated by formulas A and B. The following shows the case where the anionic group is a carboxy group, that is, the case of a carboxy-modified cellulose fiber (anion-modified cellulose fiber). The following "1720 cm" -1 The peak intensity of "is the peak intensity derived from the carbonyl group. In the case of an anionic group other than the carboxy group, the value of the wave number is appropriately changed, and the bond amount and introduction rate of the modifying group can be calculated. <Formula A> Amount of modified group bound: d (mmol / g) = a × (bc) ÷ b a: Carboxy group content (mmol / g) of carboxy-modified cellulose fiber (anion-modified cellulose fiber) b: 1720 cm of carboxy-modified cellulose fiber (anion-modified cellulose fiber) -1 Peak intensity of c: 1720 cm of modified cellulose fiber -1 Peak intensity of <Formula B> Modification group introduction rate e (mol%) = 100 × d / a

[0082] [Crystallization degree of anionically modified cellulose fibers, short fiber anionically modified cellulose fibers, and modified cellulose fibers] The crystallinity of the anionically modified cellulose fibers, the shortened anionically modified cellulose fibers, and the modified cellulose fibers was determined by measurement under the following conditions using an X-ray diffractometer (MiniFlexII, manufactured by Rigaku Corporation). Measurement pellet preparation conditions: A pressure of 10 to 20 MPa was applied to the target cellulose fiber using a tablet forming machine to produce pellets with an area of ​​320 mm. 2 A smooth pellet measuring 1 mm in thickness was prepared. X-ray diffraction analysis conditions: step angle 0.01°, scan speed 10° / min, measurement range: diffraction angle 2θ=5~40° X-ray source: Cu / Kα-radiation, tube voltage: 15kV, tube current: 30mA Peak splitting conditions: After removing background noise, the peaks were fitted with a Gaussian function so that the error between 2θ=13° and 23° was within 5%. The crystallinity of the cellulose type I crystal structure of the anion-modified cellulose fibers, the shortened anion-modified cellulose fibers, and the modified cellulose fibers was calculated based on the following formula (A) using the area of ​​the X-ray diffraction peak obtained by the above-mentioned peak division. Cellulose type I crystallinity (%) = [Icr / (Icr+Iam)] x 100 (A) (In the formula, Icr represents the area of ​​the diffraction peak of the lattice plane (002 plane) (diffraction angle 2θ=22-23°) in X-ray diffraction, and Iam represents the area of ​​the diffraction peak of the amorphous portion (diffraction angle 2θ=18.5°).)

[0083] [Solid content] The solid content was determined by measurement under the following conditions using a halogen moisture meter (Shimadzu Corporation, MOC-120H). Measurements were made every 30 seconds for 1 g of sample at a constant temperature of 150°C, and the value where the mass loss was 0.1% or less of the initial amount of the sample was taken as the solid content. If it is difficult to analyze the solid content by the above analytical method because a high boiling point organic solvent was used, a known alternative method such as the phenol-sulfuric acid method may be used. The amount of solid content obtained by the above measurement was divided by the mass of the sample before heating, and the percentage obtained was taken as the solid content (mass %).

[0084] [Concentration of component (A) in dispersion] The concentration of component (A) in the dispersion was expressed as the solid content (% by mass) in the dispersion.

[0085] [Concentration of component (A') in dispersion] The concentration of the modified cellulose fiber having a modifying group via an ionic bond (hereinafter referred to as component (A')) used in the comparative examples described below in the dispersion was calculated from the amounts of each component blended when preparing the dispersion of component (A') on the assumption that all of the blended anion-modified cellulose fiber and amines were ionic bonds.

[0086] [Concentration of glucose units contained in component (A) or component (A') in dispersion] The concentration of glucose units contained in component (A) or component (A') in the dispersion was calculated using the following formula. Concentration (mass%) of glucose units contained in component (A) or component (A') in the dispersion liquid = 1000 × content (mass%) of component (A) or component (A') in the dispersion liquid / [1000 + molecular weight (g / mol) of modifying compound × bond amount of modifying group (mmol / g)]

[0087] [Viscosity of Dispersion of Component (A) or Component (A')] The viscosity of the dispersion of component (A) or component (A') was measured using a rheometer (Anton Paar, PHYSICA MCR300). The measurement tool used was a cone-type tool CP25-1 or CP50-1 depending on the viscosity of the dispersion, and the measurement conditions were a shear rate of 0.001 to 1000 s for the first run and 0.001 to 1000 s for the second run. -1 2nd time 1000~0.001s -1 , 3rd time 0.001~1000s -1 From the viewpoint of viscosity stability, the third measurement was performed at 25°C, 1 atm, and a shear rate of 1.0 s -1 The viscosity at this time was determined.

[0088] [Transmittance of Dispersion of Component (A) or Component (A')] The light transmittance at a wavelength of 660 nm of the dispersion of component (A) or component (A') was measured using a double beam spectrophotometer (U-2910, manufactured by Hitachi High-Tech Science Corporation) and a quartz cell with an optical path length of 10 mm under conditions of 25°C and 1 minute. The higher the transmittance, the better the dispersion of the modified cellulose fiber.

[0089] [Content of component (A) or component (A') in metal particle-containing composition] The content of component (A) or component (A') in the metal particle-containing composition was calculated from the concentration of component (A) or component (A') in the dispersion and the blending composition of the metal particle-containing composition.

[0090] [Content of glucose units contained in component (A) or component (A') in metal particle-containing composition] The content of glucose units in the metal particle-containing composition was calculated from the concentration of glucose units in the dispersion and the blending composition of the metal particle-containing composition.

[0091] [Content of each component in metal particle-containing composition] The content of each component in the metal particle-containing composition was calculated from the blending amount of each component when the metal particle-containing composition was produced.

[0092] Preparation of anionically modified cellulose fibers In a 2L PP beaker equipped with a mechanical stirrer and stirring blades, 10 g of bleached kraft pulp fiber of coniferous wood as the raw material natural cellulose fiber and 990 g of deionized water are added and stirred at 25 ° C and 100 rpm for 30 minutes. Next, 0.13 g of TEMPO, 1.3 g of sodium bromide, and 35.5 g of 10.5 mass% sodium hypochlorite aqueous solution are added in this order to 10 g of the pulp fiber. Next, pH stat titration is performed using an automatic titration device, and 0.5 M sodium hydroxide aqueous solution is dropped to maintain the pH at 10.5. The reaction is performed at 25 ° C for 120 minutes at a stirring speed of 100 rpm. Next, 0.01 M hydrochloric acid is further added while stirring to make the pH of the suspension 2. Next, the solid content is filtered out by suction filtration. The filtered solid is then dispersed in deionized water and the solid is separated by suction filtration. This operation is repeated until the conductivity of the filtrate reaches 200 μS / cm or less. The obtained solid is subjected to a dehydration treatment to obtain anion-modified cellulose fibers that are the raw material for shortened anion-modified cellulose fibers. The physical properties of the resulting anionically modified cellulose fibers are shown in Table 1.

[0093] [Table 1]

[0094] Preparation of short anion-modified cellulose fibers (1) Preparation of Short Anion-Modified Cellulose Fiber 1 Deionized water was added to the anion-modified cellulose fibers to prepare a mixture with a solid content of 5.00% by mass. The mixture was then stirred at 80° C. and normal pressure for 29 hours to obtain an aqueous suspension of short anion-modified cellulose fibers 1 with a solid content of 13.1% by mass. The physical properties of the resulting shortened anionically modified cellulose fiber 1 are shown in Table 2. (2) Preparation of Short Anion-Modified Cellulose Fiber 2 193 g of deionized water was added to the anion-modified cellulose fiber, and the mixture was stirred with a mechanical stirrer at room temperature (25°C) for 30 minutes to prepare a dispersion with a solid content of 1% by mass. 24.5 g of 1M hydrochloric acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was then added to the mixture, and the mixture was stirred at room temperature for 1 hour to react. After the reaction was completed, the solid content was filtered off by suction filtration. The filtered solid content was then dispersed in deionized water, and the operation of filtering off the solid content by suction filtration was repeated until the conductivity of the filtrate was 200 μS / cm or less, and hydrochloric acid and the salt produced were removed. Then, 1.8 g of the obtained anion-modified cellulose fiber was placed in a vial equipped with a magnetic stirrer and a stirring bar on an absolute dry basis, and ion-exchanged water was added until the mass of the treatment liquid reached 36 g. The treatment liquid was reacted at 95° C. for 12 hours to obtain an aqueous suspension of shortened anion-modified cellulose fiber 2. The aqueous suspension of shortened anion-modified cellulose fiber 2 was centrifuged (manufactured by Hitachi Koki Co., Ltd., CR21G III, centrifugal acceleration 10,000 G, 1 minute) to obtain a composition containing shortened anion-modified cellulose fiber 2 with a solid content of 25.7 mass%. The physical properties of the resulting short anion-modified cellulose fibers 2 are shown in Table 2.

[0095] [Table 2]

[0096] Preparation of dispersion of component (A) (1) Preparation of dispersion of modified cellulose fiber A-1 A water suspension of the short fiber anion-modified cellulose fiber 1 obtained above was placed in a beaker equipped with a magnetic stirrer and a stirring bar. Then, 1.3 g of 4-methylmorpholine and 8.2 g of 4-(4,6-dimethoxy-1,3,5-triazin-2-yl)-4-methylmorpholinium chloride (manufactured by Kokusan Kagaku Co., Ltd.) as a condensation agent were placed and dissolved in 371 g of methyl ethyl ketone (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.). 52.2 g of methoxypoly(oxyethylene / oxypropylene)-2-propylamine (manufactured by HUNTSMAN, JEFFAMINE M2070, PO / EO (molar ratio) = 10 / 31, molecular weight 2000, hereinafter abbreviated as "EOPO amine") was added in an amount equivalent to 1 mol of amino group per 1 mol of carboxy group of the cellulose fiber, and the reaction solution was reacted at 25 ° C. for 14 hours. After the reaction was completed, 25.0 g of 1M hydrochloric acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added and stirred to suspend the mixture. The solid matter was filtered out from the suspension by vacuum filtration. 350 g of ethanol was added to the solid matter, the mixture was suspended, and the solid matter was filtered out by vacuum filtration. Next, 350 g of 1-methoxy-2-propanol (manufactured by Daicel Corporation, hereinafter abbreviated as "PGME") was added to the solid matter, the suspension was suspended, and the resulting suspension was separated by centrifugation (manufactured by Hitachi Koki Co., Ltd., CR21G III, centrifugal acceleration 10000G, 1 minute), and the ethanol layer was removed to obtain a modified cellulose fiber PGME dispersion. The solid content of the obtained modified cellulose fiber PGME dispersion was 12.2% by mass. Next, 15.0 g of the modified cellulose fiber PGME dispersion (solid content 12.2 mass%), 43 g of deionized water, 53 g of PGME, and 60.0 g of polyethylene glycol 200 (manufactured by Fujifilm Wako Pure Chemical Industries, hereinafter abbreviated as "PEG200") were added to a beaker equipped with a magnetic stirrer and a stirring bar and stirred. After stirring this solution at room temperature for 1 hour with a magnetic stirrer, the modified cellulose fiber was finely divided by five passes at 150 MPa with a high-pressure homogenizer (manufactured by Yoshida Kikai Kogyo Co., Ltd., Nanovater L-ES). The dispersion was dried under reduced pressure at 85 ° C. to remove solvents other than PEG200, and a dispersion of modified cellulose fiber A-1 having methoxypoly(oxyethylene / oxypropylene)-2-propyl groups via amide bonds was obtained. (2) Preparation of dispersion of modified cellulose fiber A-2 In a beaker equipped with a magnetic stirrer and a stirrer, 30.3 g of the composition containing the short fiber anion-modified cellulose fiber 2 obtained above and 3.8 g of 4-(4,6-dimethoxy-1,3,5-triazin-2-yl)-4-methylmorpholinium chloride (manufactured by Kokusan Kagaku Co., Ltd.) as a condensation agent were charged and dissolved in 144 g of methyl ethyl ketone (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.). 24.3 g of EOPO amine was added thereto in an amount equivalent to 1 mol of amino group per 1 mol of carboxyl group of the cellulose fiber, and the reaction liquid was reacted at 50 ° C. for 6 hours. After the reaction was completed, 12.1 g of 1 M hydrochloric acid was added and stirred, and the solid matter was filtered out by vacuum filtration. 180 g of ethanol was added to the obtained solid matter, suspended, and the solid matter was filtered out by vacuum filtration. Next, 180 g of PGME was added to the solid matter, and the resulting suspension was centrifuged (Hitachi Koki Co., Ltd., CR21G III, centrifugal acceleration 10,000G, 1 minute) to separate the layers, and the ethanol layer was removed to obtain a modified cellulose fiber PGME dispersion. The solid content of the resulting modified cellulose fiber PGME dispersion was 19.4 mass%. Next, 1.9 g of the above-mentioned modified cellulose fiber PGME dispersion (solid content 19.4 mass%), 57.9 g of deionized water, 39.7 g of PGME, and 15.0 g of PEG200 were added to a beaker equipped with a magnetic stirrer and a stirring bar and stirred. After stirring this solution at room temperature for 1 hour with a magnetic stirrer, the modified cellulose fiber was finely processed by 10 passes at 150 MPa with a high-pressure homogenizer (Yoshida Kikai Kogyo Co., Ltd., Nanovater L-ES). The dispersion was dried under reduced pressure at 85 ° C. to remove solvents other than PEG200, and a dispersion of modified cellulose fiber A-2 having methoxypoly(oxyethylene / oxypropylene)-2-propyl groups was obtained via amide bonds. (3) Preparation of dispersion of modified cellulose fiber A-3 A dispersion of modified cellulose fiber A-3 having methoxypoly(oxyethylene / oxypropylene)-2-propyl groups via amide bonds was obtained by carrying out the same operations as in the preparation of the dispersion of modified cellulose fiber A-2, except that 5.9 g of modified cellulose fiber PGME dispersion (solid content 19.4% by mass), 56.3 g of deionized water, 39.7 g of PGME, and 15.0 g of PEG200 were added to a beaker equipped with a magnetic stirrer and a stirring bar and stirred. (4) Preparation of dispersion of modified cellulose fiber A-4 In a beaker equipped with a magnetic stirrer and a stirring bar, 36.8 g of the composition containing the short fiber anion-modified cellulose fiber 2 obtained above and 13.8 g of 4-(4,6-dimethoxy-1,3,5-triazin-2-yl)-4-methylmorpholinium chloride (manufactured by Kokusan Chemical Co., Ltd.) were charged and dissolved in 102 g of PGME. 1.8 g of octylamine (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added in an amount equivalent to 1 mol of amino groups per 1 mol of carboxyl groups of the cellulose fiber, and the reaction solution was reacted at 50 ° C. for 6 hours. After the reaction was completed, the solid matter was filtered off by vacuum filtration. 190 g of ethanol was added to the obtained solid matter, suspended, and the solid matter was filtered off by vacuum filtration. Next, 12.1 g of 1M hydrochloric acid was added and stirred, and 190 g of PGME was added to the solid matter to suspend it. The resulting suspension was separated by centrifugation (Hitachi Koki Co., Ltd., CR21G III, centrifugal acceleration 10,000G, 1 minute), and the ethanol layer was removed to obtain a modified cellulose fiber PGME dispersion. The solid content of the resulting modified cellulose fiber PGME dispersion was 13.0 mass%. Next, 10.5 g (solid content 13.0 mass%) of the modified cellulose fiber PGME dispersion, 200.0 g of PGME, and 40.0 g of PEG200 were added to a beaker equipped with a magnetic stirrer and a stirrer and stirred. After stirring this solution at room temperature for 1 hour with a magnetic stirrer, the modified cellulose fiber was finely divided by 10 passes at 150 MPa with a high-pressure homogenizer (Yoshida Kikai Kogyo Co., Ltd., Nanovaita L-ES). The dispersion was dried under reduced pressure at 85 ° C to remove solvents other than PEG200, and a dispersion of modified cellulose fiber A-4 having octyl groups via amide bonds was obtained.

[0097] Preparation of dispersion of component (A') (1) Preparation of dispersion of modified cellulose fiber A'-1 In a beaker equipped with a magnetic stirrer and a stirrer, 7.90 g of the aqueous suspension of the short fiber anion-modified cellulose fiber 1 obtained above, 86.0 g of deionized water, 88.0 g of PGME, and 100 g of PEG200 were added and stirred. 1.7 g of EOPO amine, an amount equivalent to 0.5 mol of amino groups per 1 mol of carboxyl groups of the cellulose fiber, was added thereto, and the solution was stirred with a magnetic stirrer for 1 hour at room temperature, and then the modified cellulose fiber was finely processed by five passes at 150 MPa with a high-pressure homogenizer (Yoshida Kikai Kogyo Co., Ltd., Nanovaita L-ES). The dispersion was dried under reduced pressure at 85 ° C to remove solvents other than PEG200, and a dispersion of modified cellulose fiber A'-1 having methoxypoly(oxyethylene / oxypropylene)-2-propyl groups via ionic bonds was obtained.

[0098] (2) Preparation of dispersion of modified cellulose fiber A'-2 A dispersion of modified cellulose fiber A'-2 having methoxypoly(oxyethylene / oxypropylene)-2-propyl groups via ionic bonds was obtained by the same procedure as in Comparative Preparation Example 1, except that the aqueous suspension of shortened anionically modified cellulose fiber 1 obtained above was changed to 34.0 g, the deionized water to 156 g, the PGME to 176 g, and the EOPO amine to 7.70 g.

[0099] Table 3 shows the physical properties, structure, and composition of each dispersion of the modified cellulose fibers A-1 to A-4, and the modified cellulose fibers A'-1 and A'-2.

[0100] [Table 3]

[0101] Examples 1 to 7, Comparative Examples 1 to 3, and Reference Examples 1 to 4 (Preparation of Metal Particle-Containing Composition) The components were added to an agate mortar so that the dispersion of component (A) or component (A') had the glucose unit content shown in Table 4, and the components (B) and (C) had the blending composition shown in Table 4. The components were kneaded until the dry powder of component (B) was no longer visible to the naked eye, and the resulting mixture was transferred to a plastic bottle. The sealed plastic bottle was stirred for 2000 min using a planetary vacuum mixer (Thinky Corporation, Planetary Vacuum Mixer ARV-310). -1 The mixture was stirred for 5 minutes at (2000 rpm) to obtain metal particle-containing compositions of Examples 1 to 7, Comparative Examples 1 to 3, and Reference Examples 1 to 4, respectively.

[0102] The raw materials used in the production of the metal particle-containing composition are shown below. <Ingredient (B)> Copper particles B-1: Spherical copper powder manufactured by Mitsui Mining & Smelting Co., Ltd., variety: 1050Y (specific surface area 1.1 m 2 / g (catalog value), average particle size (D50 diameter) 0.81 μm (catalog value) Silver particles B-2: Mitsui Mining & Smelting Co., Ltd., spherical highly-filled silver powder, grade: SL01 (specific surface area 0.74 m 2 / g (catalog value), average particle size (D50 diameter) 1.23 μm (catalog value) Tin particles B-3: Manufactured by Fujifilm Wako Pure Chemical Industries, powder form, particle size: 95% or more passes through a sieve with 75 μm openings (product specification value) Nickel particles B-4: Manufactured by Fujifilm Wako Pure Chemical Industries, powder form, particle size: 95% or more passes through a sieve with 150 μm openings (product specification value) <Component (C)> ·PEG200: Same as above α-Terpineol: Fujifilm Wako Pure Chemical Industries, Ltd., special grade reagent

[0103] The following evaluations were carried out using each of the metal particle-containing compositions obtained in Examples 1 to 7, Comparative Examples 1 to 3, and Reference Examples 1 to 4. The results are shown in Table 4.

[0104] <Evaluation> [Evaluation of Viscosity of Metal Particle-Containing Composition] The viscosity of the metal particle-containing composition was evaluated using a rheometer (Anton Paar, PHYSICA MCR300). The measurement jig used was a parallel type jig PP25, and the measurement conditions were a shear rate of 0.001 to 1000 s for the first run and 0.001 to 1000 s for the second run. -1 2nd time 1000~0.001s -1 , 3rd time 0.001~1000s -1 From the viewpoint of viscosity stability, the third measurement was performed at 25°C, 1 atm, and a shear rate of 1.0 s -1 The viscosity at this time was determined.

[0105] [Print Dimensionality] According to the following procedure, the print dimensional properties of each of the metal particle-containing compositions obtained in the Examples, Comparative Examples, and Reference Examples were evaluated. First, a stainless steel metal mask (thickness: 150 μm) having three rows of 6 mm × 6 mm square openings was placed on a 30 mm × 30 mm copper plate (total thickness: 1 mm), and the metal particle-containing composition was applied to the copper plate by stencil printing using a metal squeegee. Then, using a digital microscope (Keyence Corporation, VHX-7000), the width and length of the image of the metal particle-containing composition transferred onto the copper plate were measured. Then, the print dimensionality (%) was calculated using the following formula (I). The print dimensionality was calculated for each of the three images of the metal particle-containing composition transferred onto the copper plate, and the average value of the values ​​calculated from the three images was taken as the print dimensionality of the metal particle-containing composition. The lower the numerical value, the better the print dimensionality. The results are shown in Table 4. Printing dimensionality (%) = [(length + width) / (6mm + 6mm)-1] x 100 (I)

[0106] [Table 4]

[0107] The metal particle-containing compositions of Examples 1 to 7 had higher viscosity and better print dimensional properties than the metal particle-containing compositions of Comparative Examples 1 to 3 and Reference Examples 1 to 4. From the above, the metal particle-containing composition of the present invention has a high viscosity even if the content of metal particles is high.

Claims

1. A metal particle-containing composition comprising the following components (A), (B), and (C): A metal particle-containing composition, wherein the content of component (B) per 100 parts by mass of solids in the metal particle-containing composition is 70 parts by mass or more. (A) Modified cellulose fiber having a modifying group via a covalent bond to the anionic group of the anion-modified cellulose fiber (B) Metal particles (C) An organic compound that is liquid at 25°C and 1 atmosphere

2. 2. The metal particle-containing composition according to claim 1, wherein the average particle size of the component (B) is 0.1 μm or more and 10 μm or less.

3. 2. The metal particle-containing composition according to claim 1, wherein the particle size of component (B) is such that 95% or more of the component passes through a sieve having openings of 300 μm.

4. 2. The metal particle-containing composition according to claim 1, wherein the content of the component (C) relative to 100 parts by mass of the component (B) is 1 part by mass or more and 20 parts by mass or less.

5. 2. The metal particle-containing composition according to claim 1, wherein the content of the component (A) relative to 100 parts by mass of the component (B) is 0.01 parts by mass or more and 10 parts by mass or less.

6. 2. The metal particle-containing composition according to claim 1, wherein the content of glucose units contained in said component (A) relative to 100 parts by mass of said component (B) is 0.003 parts by mass or more and 5 parts by mass or less.

7. The metal particle-containing composition according to claim 1 , wherein the content of the component (B) is 50 mass % or more.

8. The metal particle-containing composition according to any one of claims 1 to 7, which is used in a printing paste.

9. The metal particle-containing composition according to any one of claims 1 to 7, which is used in an ink.

10. A method for producing a film, comprising the step of applying the metal particle-containing composition according to any one of claims 1 to 7 onto a substrate.

11. A method for producing a conductive member, comprising the step of applying the metal particle-containing composition according to any one of claims 1 to 7 onto a substrate.

Citation Information

Patent Citations

  • Thickener composition