Glass fiber-reinforced resin composition
A glass fiber reinforced resin composition using municipal waste glass with a controlled T/S ratio and specific coatings enhances mechanical strength and reduces emissions, addressing the limitations of existing recycling methods.
Patent Information
- Application Number
- JP2024110896
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-01
AI Technical Summary
Existing methods for recycling glass fiber-reinforced resin products face challenges in reducing CO2 emissions and achieving mechanical strength comparable to E-glass fibers, particularly in the production of long glass fibers for reinforced resins.
A glass fiber reinforced resin composition using municipal waste glass as a raw material, with a specific T/S ratio of 361.5 to 457.0, which includes long glass fibers coated with aminosilane and urethane resin, and a resin with intrinsic viscosity of 0.3 to 1.5 dl/g, to enhance mechanical strength and reduce emissions.
The composition achieves a reinforcement efficiency greater than 1, maintaining high mechanical strength in glass fiber reinforced resin molded products while significantly reducing CO2 emissions, surpassing the performance of E-glass fibers.
Smart Images

Figure 2024133149000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a glass fiber reinforced resin composition. [Background technology]
[0002] Glass fiber reinforced plastic (GFRP) is lightweight, has excellent strength and durability, and is not susceptible to metal corrosion, so it is used in a very wide range of fields, including parts for automobiles, trains, ships, housing equipment, and sporting goods.
[0003] In recent years, there has been a strong demand in the industrial sector to reduce the environmental burden and ensure sustainable production and consumption patterns. One of the efforts being made in the industrial sector to achieve this is recycling, in which products that have been sold or used as final products are collected and used as raw materials to manufacture final products again.
[0004] Recycling of glass products has also been attempted. For example, Patent Document 1 describes a method for producing long glass fibers, which is characterized by melting a glass raw material containing glass fibers recovered from a glass fiber-reinforced resin molded product to obtain molten glass, and spinning the molten glass to obtain long glass fibers. Patent Document 2 describes a glass composition for producing inorganic fibers, which is composed of 5 to 100% by weight of cathode ray tube glass in the raw material for producing the composition. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2023 / 276617 [Patent Document 2] JP 2003-267753 A Summary of the Invention [Problem to be solved by the invention]
[0006] The manufacturing method described in Patent Document 1 achieves a reduction in the environmental impact by using glass fibers recovered from glass fiber reinforced resin molded products. However, since the recovery of glass fibers often includes a step of heating at high temperatures (500°C or higher), there is room for improvement in the amount of CO2 generated during the recovery process.
[0007] Patent Document 2 describes that glass fibers, glass wool, rock wool, etc. can be manufactured using a glass composition for manufacturing inorganic fibers, but it is difficult to obtain fiber strength comparable to that of glass fibers made of E glass, which is often used in glass fiber reinforced resins, with the disclosed glass composition, particularly a glass composition containing 5 to 100% by weight of cathode ray tube glass. Note that the document only gives an example of obtaining a glass wool molded product by adhering a binder to glass wool (short glass fibers), and does not mention obtaining long glass fibers to manufacture glass fiber reinforced resins.
[0008] An object of the present disclosure is to provide a glass fiber reinforced resin composition that is made from city waste glass as a raw material, reduces CO2 emissions during its production, and can be used to form glass fiber reinforced resin molded products that have sufficiently high mechanical strength, such as tensile strength. [Means for solving the problem]
[0009] This disclosure provides the following [1] to [7].
[0010] [1] A glass fiber-reinforced resin composition comprising: a glass fiber material which is a long glass fiber obtained by melting and spinning a glass raw material containing more than 50% by mass of commercially waste glass, or a cut or crushed product thereof; and a resin, wherein the ratio (T / S) of the liquidus temperature T (°C) of the glass forming the long glass fiber to the tensile strength S (GPa) of a glass monofilament constituting the long glass fiber at 23°C and a pulling speed of 5 mm / min is 361.5 to 457.0.
[0011] This glass fiber reinforced resin composition can provide a glass fiber reinforced resin composition that can be used to form glass fiber reinforced resin molded products having sufficiently high mechanical strength such as tensile strength, while using municipal waste glass as a raw material and reducing CO2 emissions in the production. In the glass fiber reinforced resin molded product formed using the above glass fiber reinforced resin composition, the T / S of the glass forming the long glass fiber is within the above range, so that the efficiency of increasing the mechanical strength of the glass fiber reinforced resin molded product is high.
[0012] When the value obtained by dividing the tensile strength of a glass fiber reinforced resin molded product formed using the above glass fiber reinforced resin composition by the tensile strength of a glass fiber reinforced resin molded product formed using a glass fiber reinforced resin composition containing long glass fibers satisfying the E glass composition is defined as X, and the value obtained by dividing the tensile strength of a glass monofilament in the glass fiber material contained in the above glass fiber reinforced resin composition by the tensile strength of a glass monofilament satisfying the E glass composition is defined as Y (the tensile strengths are all measured at 23°C, the tensile strength of the glass monofilament is measured at a pulling speed of 5 mm / min, and the tensile strength of the glass fiber reinforced resin molded product is measured at a pulling speed of 2 mm / min), if X / Y is defined as the reinforcement efficiency of the glass fiber reinforced resin molded product (hereinafter sometimes abbreviated as "reinforcement efficiency"), the reinforcement efficiency of the glass fiber reinforced resin molded product exceeds 1. That is, the reinforcement efficiency is improved compared to when the product is manufactured using long glass fibers satisfying the E glass composition. And, if T / S is within the range of 361.5 to 457.0, the reinforcement efficiency is sufficiently high.
[0013] The glass fiber reinforced resin composition having a T / S in the range of 361.5 to 457.0 not only has a sufficiently high reinforcement efficiency, but also realizes a reduction in CO2 emissions during its production, even though it uses commercially waste glass as a raw material. That is, the glass fiber reinforced resin composition has a sufficiently high reinforcement efficiency in mechanical strength such as tensile strength, and can be produced by a method that reduces the environmental load.
[0014] [2] The glass fiber reinforced resin composition according to [1], wherein the ratio (T / S) is 410.2 to 447.0.
[0015] The glass fiber reinforced resin composition having a T / S ratio of 410.2 to 447.0 has a higher reinforcement efficiency, and therefore, although it uses city waste glass as a raw material, it is possible to manufacture a glass fiber reinforced resin molded product having sufficiently high mechanical strength such as tensile strength while reducing CO2 emissions during the manufacturing process.
[0016] [3] The glass raw material is a glass composition having 63.5 to 66.5 mass% SiO2, 1.5 to 3.5 mass% Al2O3, 3.0 to 4.5 mass% B2O3, 7.5 to 10.0 mass% in total of CaO and MgO, 3.5 to 5.5 mass% in total of BaO and SrO, and 15.0 to 17.3 mass% in total of Na2O and K2O.
[0017] If commercial waste glass satisfies the above glass composition, it becomes possible to further increase the tempering efficiency and further reduce CO2 emissions.
[0018] [4] The glass fiber reinforced resin composition according to any one of [1] to [3], wherein the content of the glass fiber material in the glass fiber reinforced resin composition is 10.0 to 50.0 mass% based on the total amount of the glass fiber reinforced resin composition.
[0019] If the content of the glass fiber material is within the above range, the reinforcing efficiency can be further improved.
[0020] [5] The glass fiber reinforced resin composition according to any one of [1] to [4], wherein the glass fiber material is coated with an aminosilane and a urethane resin.
[0021] By coating the glass fiber material with aminosilane and urethane resin, the reinforcement efficiency can be further improved.
[0022] [6] The glass fiber reinforced resin composition according to any one of [1] to [5], wherein the resin has an intrinsic viscosity of 0.3 to 1.5 dl / g. For example, in the glass fiber reinforced resin composition according to any one of [1] to [5], the resin may have an intrinsic viscosity of 0.3 to 1.5 dl / g measured at 30° C. in a mixed solvent of phenol / 1,1,2,2-tetrachloroethane (mass ratio 1 / 1).
[0023] By setting the intrinsic viscosity of the resin within the above range, the reinforcement efficiency can be further improved.
[0024] [7] The glass fiber reinforced resin composition according to any one of [1] to [6], wherein the resin is at least one selected from the group consisting of polybutylene terephthalate, polyethylene terephthalate, polycarbonate, and polyphenylene sulfide.
[0025] At least one resin selected from the above group can further increase the reinforcing efficiency when combined with the above-mentioned glass fiber material. Effect of the Invention
[0026] According to the present disclosure, it is possible to provide a glass fiber reinforced resin composition that is made from city waste glass as a raw material, reduces CO2 emissions during its production, and yet has sufficiently high mechanical strength, such as tensile strength.
[0027] When a long glass fiber is obtained using waste glass and a glass fiber reinforced resin is produced using the long glass fiber, it is expected that the mechanical strength such as tensile strength of the glass fiber reinforced resin will be insufficient because the waste glass has various glass compositions. However, the present inventors have found that by controlling T / S to 361.5 to 457.0, an unexpected result that the reinforcement efficiency is high even when waste glass is used is obtained. This is explained from the viewpoint of reinforcement efficiency as follows. When the above-mentioned value of Y is less than 1, that is, even when the strength of the glass monofilament obtained from waste glass does not exceed the strength of the glass monofilament of E glass composition, the above-mentioned value of X (a value measured as a glass fiber reinforced resin molded product) is maintained near 1, and as a result, the reinforcement efficiency represented by X / Y becomes large (X / Y exceeds 1). The fact that X / Y exceeds 1 means that even if the strength of the long glass fiber itself is lower than that of E glass due to the use of commercial waste glass, once it is combined with resin to form a glass fiber reinforced resin, the strength of the glass fiber reinforced resin molded product can be maintained high to such an extent that the decrease in strength of the long glass fiber can be ignored. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Although the embodiments for carrying out the present disclosure will be described below, the present disclosure is not limited to the following embodiments.
[0029] One embodiment of the present disclosure is a glass fiber reinforced resin composition, which includes a glass fiber material that is long glass fiber or cut or crushed glass fiber obtained by melting and spinning a glass raw material containing more than 50 mass% of commercial waste glass, and a resin.
[0030] In this disclosure, glass fiber reinforced plastic (GFRP) refers to a mixture containing resin and glass fiber material as a reinforcing material. Glass fiber reinforced plastic has higher mechanical strength (e.g., tensile strength) than resin alone due to the inclusion of glass fibers. Glass fiber reinforced plastic is lightweight, has excellent strength and durability, and does not have the problem of metal corrosion, so it is used in a very wide range of fields, including parts for automobiles, trains, ships, etc., housing equipment, and sporting goods.
[0031] In the present disclosure, the glass raw material is a raw material that can be made into long glass fibers by melting and spinning, and refers to the entire raw materials used in the production of all the long glass fibers contained in a glass fiber reinforced resin composition or a glass fiber reinforced resin molded product. Such raw materials include inorganic oxides that form glass by melting.
[0032] In the present disclosure, the term "commercial waste glass" refers to glass recovered from municipal waste (e.g., waste containing 30% or more by mass of glass of undefined shape relative to the total amount) without a process of heating at 500°C or higher. Commercial waste includes waste that has been used in the city and then discarded, as well as waste that has been manufactured and completed as a product but has been discarded without being used or distributed in the city. The commercial waste glass according to the present disclosure does not include waste glass generated in factories or the like during the manufacturing process of glass or products using glass. Examples of the commercial waste glass according to the present disclosure include glass cullet recovered by crushing fluorescent tubes, glass cullet recovered by crushing automobile windshields, glass cullet recovered by crushing digital device screens, and glass cullet recovered by crushing glass bottles used as containers for beverages, etc. Such commercial waste glass may be glass made of a glass composition having a basic composition of SiO2, Al2O3, and B2O3, and further containing at least one of CaO and MgO, at least one of BaO and SrO, and at least one of Na2O and K2O.
[0033] The waste glass according to the present disclosure may be glass recovered from municipal waste by a method normally performed by a person skilled in the art, so long as it does not include a step of heating at 500°C or higher. The method of recovering such waste glass may, for example, be performed by separating the recovered municipal waste into a glass portion that can be recycled as a glass raw material and the other portion, and the municipal waste may be crushed during the separation process to recover glass as glass cullet, and organic matter derived from the portion of the municipal waste other than glass may be removed as necessary by dissolving it in a solvent such as benzyl alcohol. If glass recovered without a step of heating at 500°C or higher is used as a glass raw material, it is possible to reduce the generation of carbon dioxide (CO2), which may be generated in an increased amount when glass fibers are heated at 500°C or higher in the production, and thus to reduce the environmental load. In the present disclosure, the step of preparing a glass raw material (e.g., glass cullet) containing municipal waste glass may be referred to as a "preparation step". The preparation step includes recovering glass from municipal waste.
[0034] In one embodiment of the present disclosure, the commercial waste glass is made of a glass composition having SiO2 of 63.5 to 66.5 mass%, Al2O3 of 1.5 to 3.5 mass%, B2O3 of 3.0 to 4.5 mass%, the sum of CaO and MgO of 7.5 to 10.0 mass%, the sum of BaO and SrO of 3.5 to 5.5 mass%, and the sum of Na2O and K2O (R2O) of 15.0 to 17.3 mass%. In the present disclosure, the expressions "made of a glass composition where A is B", "satisfies a glass composition where A is B", "has a glass composition where A is B", and "has a glass composition where A is B" mean that A is a glass obtained by melting a mineral material that satisfies B.
[0035] The glass fiber reinforced resin composition according to one embodiment of the present disclosure uses a glass fiber material that is a long glass fiber obtained by melting and spinning a glass raw material containing more than or equal to a predetermined lower limit of waste glass from the community, or a cut or crushed product thereof. The content of waste glass from the community in the glass raw material may be at least more than 50% by mass, and in one embodiment, it may be more than 55% by mass, more than 60% by mass, more than 65% by mass, more than 70% by mass, more than 74% by mass, more than 75% by mass, more than 76% by mass, more than 80% by mass, more than 85% by mass, more than 90% by mass, more than 95% by mass, more than 98% by mass, or more than 99% by mass, and in a preferred embodiment, it may be 100% by mass. The glass fiber reinforced resin composition according to the present disclosure can recycle waste glass from the community as a raw material for glass fiber reinforced resin by satisfying the above-mentioned conditions in the content of waste glass in the glass raw material, thereby reducing the environmental load. In addition, in the glass fiber reinforced resin composition according to the present disclosure, the content of commercial waste glass in the glass raw material satisfies the above-mentioned condition, and therefore the majority of the glass in the glass raw material is glass recovered without a process of heating at 500°C or higher, so that the generation of carbon dioxide (CO2), which may be increased when the glass fiber is heated at 500°C or higher in the production, can be reduced, and thus the environmental load can be reduced. In a most preferred embodiment, the glass raw material may be a glass raw material consisting of commercial waste glass.
[0036] The glass raw materials other than waste glass contained in the glass raw materials in the glass fiber reinforced resin composition according to an embodiment of the present disclosure and their compositions are not particularly limited, and for example, glass raw materials designed for the production of glass fibers and generally used by those skilled in the art can be used. For example, silica sand, feldspar, clay, limestone, silica powder, dolomite, talc, clay, alumina, soda ash, or mixtures thereof can also be used as glass raw materials. Examples of compositions that can be taken by such glass raw materials other than waste glass include the most general-purpose E-glass composition, a high-strength, high-elasticity glass composition, a high-elasticity, easily manufacturable glass composition, and a low-dielectric-constant, low-dielectric-tangent glass composition.
[0037] The E-glass composition contains SiO2 in the range of 52.0 to 56.0 mass%, Al2O3 in the range of 12.0 to 16.0 mass%, MgO and CaO in total in the range of 20.0 to 25.0 mass%, and B2O3 in the range of 5.0 to 10.0 mass%.
[0038] The high-strength, high-elasticity glass composition contains SiO2 in the range of 60.0 to 70.0 mass%, Al2O3 in the range of 20.0 to 30.0 mass%, MgO in the range of 5.0 to 15.0 mass%, Fe2O3 in the range of 0 to 1.5 mass%, and Na2O, K2O, and Li2O in a total range of 0 to 0.2 mass%.
[0039] The high elastic modulus, easily manufacturable glass composition contains SiO2 in the range of 57.0 to 60.0 mass%, Al2O3 in the range of 17.5 to 20.0 mass%, MgO in the range of 8.5 to 12.0 mass%, CaO in the range of 10.0 to 13.0 mass%, and B2O3 in the range of 0.5 to 1.5 mass%, and contains SiO2, Al2O3, MgO, and CaO in a total amount of 98.0 mass% or more.
[0040] The low dielectric constant and low dielectric tangent glass composition includes SiO2 in the range of 48.0 to 62.0 mass%, B2O3 in the range of 17.0 to 26.0 mass%, Al2O3 in the range of 9.0 to 18.0 mass%, CaO in the range of 0.1 to 9.0 mass%, MgO in the range of 0 to 6.0 mass%, Na2O, K2O, and Li2O in a total range of 0.05 to 0.5 mass%, TiO2 in the range of 0 to 5.0 mass%, SrO in the range of 0 to 6.0 mass%, F2 and Cl2 in a total range of 0 to 3.0 mass%, and P2O5 in the range of 0 to 6.0 mass%.
[0041] In one embodiment of the present disclosure, the content of glass frits other than commercial waste glass in the glass frit may be, for example, less than 50 mass%, less than 45 mass%, less than 40 mass%, less than 35 mass%, less than 30 mass%, less than 26 mass%, 25 mass% or less, less than 24 mass%, less than 20 mass%, less than 15 mass%, less than 10 mass%, less than 5 mass%, less than 2 mass%, or less than 1 mass%, and in a preferred embodiment, may be 0 mass%. That is, in a preferred embodiment, the glass frit may not contain glass frits other than commercial waste glass.
[0042] In one embodiment of the present disclosure, the glass raw materials as a whole have a glass composition in which SiO2 is 61.0 to 69.0 mass%, Al2O3 is 1.0 to 7.0 mass%, B2O3 is 1.0 to 5.0 mass%, the total of CaO and MgO is 7.3 to 15.0 mass%, the total of BaO and SrO is 2.8 to 7.0 mass%, and the total of Na2O and K2O (R2O) is 12.0 to 17.5 mass%. In a preferred embodiment of the present disclosure, the glass frit has a glass composition in which SiO2 is 63.5 to 66.5 mass%, Al2O3 is 1.5 to 3.5 mass%, B2O3 is 3.0 to 4.5 mass%, the sum of CaO and MgO is 7.5 to 10.0 mass%, the sum of BaO and SrO is 3.5 to 5.5 mass%, and the sum of Na2O and K2O (R2O) is 15.0 to 17.3 mass%. The glass frit, the long glass fiber obtained by melting and spinning the glass frit, and the glass monofilament constituting the long glass fiber have substantially the same glass composition.
[0043] The glass fiber reinforced resin composition according to the present disclosure contains, as a reinforcing material, a long glass fiber or a glass fiber material which is a cut or crushed product thereof. In the present disclosure, the long glass fiber (also called a glass fiber bundle or glass strand) means a glass fiber which is in a state of having a length of at least 1000 m or more in the manufacturing process, and is composed of one glass monofilament or a bundle of multiple glass monofilaments. Such a long glass fiber is prepared, for example, by a procedure in which molten glass is made to flow down through a platinum nozzle called a bushing and stretched, and is continuously fiberized (spinning), and an operation of bundling as necessary. The long glass fiber according to the present disclosure is clearly distinguished from short glass fibers such as glass wool, which are glass fibers prepared without spinning.
[0044] The fiber diameter of the glass monofilament in the long glass fiber according to the present disclosure is, for example, in the range of 3.0 to 100.0 μm, preferably in the range of 4.0 to 70.0 μm, more preferably in the range of 5.0 to 50.0 μm, even more preferably in the range of 6.5 to 40.0 μm, particularly preferably in the range of 7.0 to 30.0 μm, and most preferably in the range of 10.5 to 16.0 μm.
[0045] The glass fiber material according to the present disclosure may be unprocessed long glass fibers, or may be cut or crushed long glass fibers that have been appropriately processed. Such glass fiber materials may be, for example, chopped strands, rovings, or cut fibers.
[0046] The number of glass monofilaments (bundled number) constituting the long glass fiber according to the present disclosure and the length of the glass fiber material can be appropriately selected according to the form of the glass fiber material. For example, when the glass fiber material is a chopped strand, the number of glass monofilaments (bundled number) constituting it may be preferably 1 to 20,000, more preferably 50 to 10,000, and even more preferably 200 to 8,000, and in this case, the chopped strand may be cut to a length of preferably 1.0 to 100.0 mm, more preferably 1.2 to 51.0 mm, even more preferably 1.5 to 30.0 mm, particularly preferably 2.0 to 15.0 mm, and most preferably 2.3 to 7.8 mm. When the glass fiber material is a roving, the number of glass monofilaments (bundled number) constituting it may be, for example, 10 to 30,000, and the long glass fiber is not cut in the preparation thereof. Furthermore, when the glass fiber material is cut fiber, the number of glass monofilaments (bundled number) constituting it may be, for example, 1 to 20,000, and in this case, the cut fiber may be pulverized to a length of 0.001 to 0.900 mm by a known method such as a ball mill or a Henschel mixer.
[0047] The glass fiber material according to one embodiment of the present disclosure may be coated with a sizing agent. The sizing agent may be, for example, a sizing agent containing at least one selected from the group consisting of a silane coupling agent, a urethane resin, and an epoxy resin, a sizing agent containing a silane coupling agent and a urethane resin, or a sizing agent containing a silane coupling agent, a urethane resin, and an epoxy resin. In addition, the glass fiber material according to one embodiment of the present disclosure may be coated with a silane coupling agent and a urethane resin, for example, an aminosilane and a urethane resin.
[0048] Examples of the silane coupling agent include aminosilane, chlorosilane, epoxysilane, mercaptosilane, vinylsilane, and acrylicsilane. The above-mentioned silane coupling agent may be used alone or in combination of two or more of these compounds. Examples of the aminosilane include γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-N'-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, and γ-anilinopropyltrimethoxysilane. Examples of the chlorosilane include γ-chloropropyltrimethoxysilane. Examples of the epoxysilane include γ-glycidoxypropyltrimethoxysilane and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane. Examples of the mercaptosilane include γ-mercaptotrimethoxysilane. Examples of vinyl silanes include vinyl trimethoxy silane, N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyl trimethoxy silane, etc. Examples of acryl silanes include γ-methacryloxypropyl trimethoxy silane, etc.
[0049] Examples of the urethane resin include polyether-based urethane resin and polyester-based urethane resin.
[0050] Examples of epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol A novolac type epoxy resins, bisphenol F novolac type epoxy resins, biphenyl type bifunctional epoxy resins, biphenyl modified novolac type epoxy resins, naphthol-cresol co-condensed novolac type epoxy resins, naphthol-phenol co-condensed novolac type epoxy resins, dicyclopentadiene-phenol addition reaction type epoxy resins, triphenylmethane type epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, tetraphenylethane type epoxy resins, and naphthol novolac type epoxy resins.
[0051] In the glass fiber reinforced resin composition according to one embodiment of the present disclosure, the ratio (T / S) of the liquidus temperature T (°C) of the glass forming the long glass fiber to the tensile strength S (GPa) of the glass monofilament constituting the long glass fiber at 23°C and a pulling speed of 5 mm / min is 361.5 to 457.0. In the glass fiber reinforced resin composition according to another embodiment, the T / S may be 375.0 to 445.0, 385.0 to 435.0, 390.0 to 430.0, or 391.7 to 428.6.
[0052] When the T / S of the glass monofilament constituting the long glass fiber is within the above range, the efficiency of increasing the strength of the molded product relative to the strength of the monofilament is high when the glass fiber reinforced resin composition is used to produce a molded product. The properties of the long glass fiber that mainly contribute to the mechanical strength of the glass fiber reinforced resin composition include the mechanical strength of the glass fiber itself and the efficiency of increasing the mechanical strength of the glass fiber reinforced resin molded product when used as a reinforcing material. In the glass fiber reinforced resin molded product produced according to the above production method, the efficiency of increasing the mechanical strength of the glass fiber reinforced resin molded product is high because the long glass fiber satisfies the above properties. More specifically, the above-mentioned reinforcement efficiency of the glass fiber reinforced resin molded product exceeds 1. That is, the reinforcement efficiency is improved compared to when E glass is used.
[0053] In addition, when the T / S of the glass monofilaments constituting the long glass fibers is within the above range, the amount of CO2 emissions in the production of the glass fiber reinforced resin composition can be reduced. Furthermore, in the glass fiber reinforced resin composition according to the present disclosure, waste glass is used as a raw material, and the T / S of the glass monofilaments constituting the long glass fibers is within the above range, so that the environmental load in the production is reduced.
[0054] The tensile strength S (GPa) of the glass monofilament according to the present disclosure at 23° C. and a pulling speed of 5 mm / min is a value that can be calculated by dividing the actual maximum load value of the glass monofilament measured according to a method normally performed by a person skilled in the art by the fiber cross-sectional area. That is, the maximum load value of the glass monofilament is W (N), and the fiber cross-sectional area is A (mm 2 ), then S = (W / A) / 1000.
[0055] The actual measured value of the maximum load value W used to calculate the tensile strength S of the glass monofilament may be, for example, a maximum load value measured by a tensile tester as a method normally performed by a person skilled in the art. A more specific example may be the maximum load value at break obtained by fixing (bonding) a glass monofilament in a state free of deterioration due to contact or friction to a support (e.g., a mount) having a hole in the center so that the glass monofilament passes through the hole when viewed from the front, holding one point in the area through which the glass monofilament passes with a gripper of a tensile tester, and then performing a tensile test at a temperature condition of 23°C and a crosshead speed of 5 mm / min.
[0056] The fiber cross-sectional area S used in calculating the tensile strength S of the glass monofilament may be a fiber cross-sectional area calculated from the fiber diameter measured by observation using a scanning electron microscope, for example, as a method normally performed by a person skilled in the art. The fiber cross-sectional area may be a measured value for each glass monofilament subjected to measurement in the above-mentioned tensile tester, or may be a fiber cross-sectional area calculated from the average value (number average value, number average fiber diameter) of measured fiber diameters for glass monofilaments prepared in the same manner as the glass monofilament subjected to measurement in the above-mentioned tensile tester.
[0057] The liquidus temperature T (°C) used in calculating the above ratio (T / S) may be, for example, an estimated value predicted based on the glass composition of the glass monofilament, or may be an actually measured value of the liquidus temperature T. From the viewpoint of ease of measurement, in a preferred embodiment, the liquidus temperature T may be an estimated value predicted based on the glass composition of the glass monofilament.
[0058] The glass composition of the glass monofilament used to predict the liquidus temperature T can be measured by a method that is usually performed by a person skilled in the art. For example, the light element Li can be measured using an ICP emission spectrometer, and other elements can be measured using a wavelength dispersive X-ray fluorescence analyzer. As a more specific measurement method, the glass fiber is first placed in a platinum crucible and melted in an electric furnace at a temperature of 1550 ° C. for 6 hours while stirring to obtain a homogeneous molten glass. Next, the obtained molten glass is poured onto a carbon plate to produce glass cullet, which is then crushed and powdered to obtain glass powder. For the light element Li, the obtained glass powder is thermally decomposed with acid and then quantitatively analyzed using an ICP emission spectrometer. For other elements, the glass powder is molded into a disk shape using a press machine and then quantitatively analyzed using a wavelength dispersive X-ray fluorescence analyzer. The results of these quantitative analyses are converted into oxides to calculate the content and total amount of each component, and the content of each component in the glass composition can be obtained from these values.
[0059] The liquidus temperature T based on the glass composition can be predicted using software commonly used by those skilled in the art, for example, INTERGLAD Ver. 8.
[0060] The actual value of the liquidus temperature T can be measured by a method commonly used by those skilled in the art, for example, using a temperature gradient furnace or a differential scanning calorimeter (DSC).
[0061] A person skilled in the art can adjust the ratio (T / S) to be within the above range by appropriately adjusting the glass composition of the glass monofilament, and can adjust the glass composition of the glass monofilament by, for example, appropriately adjusting the glass composition of the glass raw material used to prepare the glass monofilament. More specifically, as described above, the liquidus temperature T based on the glass composition can be predicted using software that is commonly used by a person skilled in the art. First, using such software, a plurality of glass compositions are estimated, which have a liquidus temperature T suitable for setting the ratio (T / S) within the above range. Then, a glass monofilament that actually satisfies such a glass composition is actually prepared, the tensile strength S is measured, and a glass composition that sets the ratio (T / S) within the above range is selected. Alternatively, if no glass composition having the ratio (T / S) within the above range is found, a glass composition having an increased or decreased tensile strength S can be found based on known knowledge about the relationship between glass composition and tensile strength by searching for glass compositions having a ratio (T / S) close to the above range among the candidates, while confirming that the liquidus temperature T is not significantly changed using software capable of predicting the liquidus temperature T. The tensile strength of the glass monofilament can also be predicted using software commonly used by those skilled in the art, for example, INTERGLAD Ver. 8, and in the above-mentioned glass composition search process, the prediction of the tensile strength of the glass monofilament may be used instead of measuring the tensile strength of the glass monofilament.
[0062] In the production of the glass fiber reinforced resin composition according to the present disclosure, in order to set the ratio (T / S) within the above range, the glass composition in the glass raw materials can be appropriately adjusted, for example, by appropriately adjusting the types of waste glass and other glass raw materials contained in the glass raw materials and the content ratios of these glass raw materials.
[0063] In the production of the glass fiber reinforced resin composition according to an embodiment of the present disclosure, the above ratio (T / S) can be adjusted to 361.5 to 457.0 by, for example, adjusting the glass composition of the glass raw material so that SiO2 is 61.0 to 69.0 mass%, Al2O3 is 1.0 to 7.0 mass%, B2O3 is 1.0 to 5.0 mass%, the total of CaO and MgO is 7.3 to 15.0 mass%, the total of BaO and SrO is 2.8 to 7.0 mass%, and the total of Na2O and K2O (R2O) is 10.5 to 17.5 mass%. Such a glass composition can be achieved, for example, by using a glass raw material consisting of waste glass in a market exceeding a predetermined ratio and a glass raw material satisfying the E-glass composition.
[0064] In the glass fiber reinforced resin composition according to a preferred embodiment of the present disclosure, the ratio (T / S) is 410.2 to 447.0. In the glass fiber reinforced resin composition according to another preferred embodiment, the ratio (T / S) may be 415.0 to 440.0, 420.0 to 435.0, or 425.0 to 430.0. When the ratio (T / S) is within the above range, the reinforcement efficiency of the glass fiber reinforced resin molded product is increased, and the reinforcement efficiency is further improved compared to when E glass is used. In addition, when the ratio (T / S) of the glass monofilament constituting the long glass fiber is within the above range, the CO2 emissions in the production of the glass fiber reinforced resin composition can be further reduced. Furthermore, in the glass fiber reinforced resin composition according to the present disclosure, waste glass is used as a raw material, and the ratio (T / S) of the glass monofilament constituting the long glass fiber is within the above range, so that the environmental load in the production is further reduced.
[0065] In the production of a glass fiber reinforced resin composition according to a preferred embodiment of the present disclosure, the above ratio (T / S) can be adjusted to 410.2 to 447.0 by, for example, adjusting the glass composition of the glass raw material so that SiO2 is 63.5 to 66.5 mass%, Al2O3 is 1.5 to 3.5 mass%, B2O3 is 3.0 to 4.5 mass%, the total of CaO and MgO is 7.5 to 10.0 mass%, the total of BaO and SrO is 3.5 to 5.5 mass%, and the total of Na2O and K2O (R2O) is 15.0 to 17.3 mass%. Such a glass composition can be achieved by using a glass raw material made of, for example, waste glass from the market.
[0066] In one embodiment of the present disclosure, the tensile strength S of the glass monofilament constituting the long glass fiber at 23° C. and a pulling speed of 5 mm / min is, for example, in the range of 1.5 to 5.5 GPa, preferably in the range of 1.7 to 3.4 GPa, more preferably in the range of 1.9 to 3.0 GPa, even more preferably in the range of 2.0 to 2.9 GPa, and particularly preferably in the range of 2.1 to 2.8 GPa.
[0067] In one embodiment of the present disclosure, the liquidus temperature T of the glass forming the long glass fiber is, for example, in the range of 750 to 1500°C, preferably in the range of 800 to 1200°C, more preferably in the range of 850 to 1050°C, further preferably in the range of 880 to 1000°C, and particularly preferably in the range of 900 to 990°C.
[0068] The long glass fiber composed of the glass monofilament satisfying the above-mentioned ratio (T / S) as explained above can be prepared by a step of obtaining a melt of a glass raw material containing more than 50 mass% of commercial waste glass (melting step) and a step of spinning the melt obtained in the melting step (spinning step). The long glass fiber or a glass fiber material which is a cut or crushed product thereof can be obtained by cutting the long glass fiber obtained in the spinning step as necessary to obtain chopped strands or crushing it to obtain cut fibers.
[0069] In the melting step, a melt of glass raw materials containing more than 50% by mass of waste glass is obtained. When the glass raw materials are made of waste glass, the melt can be obtained by melting the waste glass. When the glass raw materials are made of waste glass and other glasses, the melt can be obtained by melting a mixture of waste glass and other glasses, or by mixing a liquid obtained by melting waste glass and a liquid obtained by melting other glasses. In one embodiment, the melting step can also be performed by melting a mixture of waste glass and other glasses at, for example, 1400°C to 1550°C, and then cooling the mixture once (preparation step), to obtain glass cullet, which is obtained by melting the mixture again.
[0070] The melting of glass raw materials in the melting step can be carried out, for example, by supplying glass raw materials (glass batch) to a melting furnace and heating them under high-temperature conditions (for example, 1000° C. to 1200° C.) at which glass melts.
[0071] In the spinning step, the molten material (molten glass) obtained in the melting step is spun to obtain a long glass fiber. The method is not particularly limited as long as it is a method normally used by those skilled in the art, and for example, the molten glass in a melting furnace is drawn out from 1 to 30,000 nozzle tips of a platinum bushing controlled at a predetermined temperature, and then quenched to form a glass monofilament.
[0072] In the spinning step, a sizing agent or binder may be applied to the glass monofilament. This makes it possible to obtain a long glass fiber in which a plurality of glass monofilaments are bundled. The application of the sizing agent or binder to the glass monofilament can be carried out, for example, by providing an applicator between the nozzle tip and the winding device and supplying the sizing agent or binder from the applicator. As a result, the long glass fiber recovered by the winding device is coated with the sizing agent or binder, and a long glass fiber containing a fiber in which a plurality of glass monofilaments are bundled is obtained on the tube of the winding device. Note that by making the nozzle tip have a non-circular shape and a protrusion or a notch for quenching the molten glass, and controlling the temperature conditions, a long glass fiber composed of glass filaments having a flat cross-sectional shape can be obtained.
[0073] In the spinning step, when a sizing agent or binder is applied to the glass monofilament, the amount thereof may be, for example, 0.1 to 5.0 parts by mass, 0.3 to 3.0 parts by mass, or 0.5 to 1.0 parts by mass per 100 parts by mass of the glass raw material.
[0074] As the resin in the glass fiber reinforced resin composition according to the present disclosure, those generally used by those skilled in the art can be used. Examples of such resins include thermoplastic resins and thermosetting resins, but from the viewpoint of the recyclability of the resin itself, it is preferable to use a thermoplastic resin. Examples of thermoplastic resins include polyethylene, polypropylene, polystyrene, styrene / maleic anhydride resin, styrene / maleimide resin, polyacrylonitrile, acrylonitrile / styrene (AS) resin, acrylonitrile / butadiene / styrene (ABS) resin, chlorinated polyethylene / acrylonitrile / styrene (ACS) resin, acrylonitrile / ethylene / styrene (AES) resin, acrylonitrile / styrene / methyl acrylate (ASA) resin, styrene / acrylonitrile (SAN) resin, (meth)acrylic resin, polyvinyl chloride (PVC), polyvinylidene chloride (PVDC), polyamide, polyacetal, polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polytrimethylene terephthalate (PTT), polycarbonate, etc. Examples of the resin include polyaryletherketone, polyarylene sulfide, polyethersulfone (PES), polyphenylsulfone (PPSU), polyphenylene ether (PPE), modified polyphenylene ether (m-PPE), polyaryletherketone, liquid crystal polymer (LCP), fluororesin, polyetherimide (PEI), polyarylate (PAR), polysulfone (PSF), polyamideimide (PAI), polyaminobismaleimide (PABM), thermoplastic polyimide (TPI), polyethylene naphthalate (PEN), ethylene / vinyl acetate (EVA) resin, ionomer (IO) resin, polybutadiene, styrene / butadiene resin, polybutylene, polymethylpentene, olefin / vinyl alcohol resin, cyclic olefin resin, cellulose resin, polylactic acid, etc. In addition, (meth)acrylic means acrylic or methacrylic.
[0075] Examples of the polyethylene include high density polyethylene (HDPE), medium density polyethylene, low density polyethylene (LDPE), linear low density polyethylene (LLDPE), and ultra-high molecular weight polyethylene.
[0076] Examples of the polypropylene include isotactic polypropylene, atactic polypropylene, syndiotactic polypropylene, and mixtures thereof.
[0077] Examples of the polystyrene include general-purpose polystyrene (GPPS), which is an atactic polystyrene having an atactic structure, high impact polystyrene (HIPS), which is GPPS with a rubber component added, and syndiotactic polystyrene having a syndiotactic structure.
[0078] Examples of the (meth)acrylic resin include a homopolymer of one of acrylic acid, methacrylic acid, styrene, methyl acrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, butyl methacrylate, and a fatty acid vinyl ester, or a copolymer of two or more of them.
[0079] Examples of the polyvinyl chloride include a vinyl chloride homopolymer polymerized by a conventionally known method such as emulsion polymerization, suspension polymerization, microsuspension polymerization, or bulk polymerization; a copolymer of a vinyl chloride monomer with a copolymerizable monomer; and a graft copolymer in which a vinyl chloride monomer is graft-polymerized onto a polymer.
[0080] Examples of the polyamides include polycaproamide (polyamide 6), polyhexamethylene adipamide (polyamide 66), polytetramethylene adipamide (polyamide 46), polytetramethylene sebacamide (polyamide 410), polypentamethylene adipamide (polyamide 56), polypentamethylene sebacamide (polyamide 510), polyhexamethylene sebacamide (polyamide 610), polyhexamethylene dodecamide (polyamide 612), polydecamethylene adipamide (polyamide 106), polyde Camethylene sebacamide (Polyamide 1010), Polydecamethylene dodecamide (Polyamide 1012), Polyundecane amide (Polyamide 11), Polyundecamethylene adipamide (Polyamide 116), Polydodecanamide (Polyamide 12), Polyxylene adipamide (Polyamide XD6), Polyxylene sebacamide (Polyamide XD10), Polymeta-xylylene adipamide (Polyamide MXD6), Polypara-xylylene adipamide (Polyamide PXD6), Polytetramethylene terephthalamide (Po Polyamide 4T), Polypentamethylene terephthalamide (Polyamide 5T), Polyhexamethylene terephthalamide (Polyamide 6T), Polyhexamethylene isophthalamide (Polyamide 6I), Polynonamethylene terephthalamide (Polyamide 9T), Polydecamethylene terephthalamide (Polyamide 10T), Polyundecamethylene terephthalamide (Polyamide 11T), Polydodecamethylene terephthalamide (Polyamide 12T), Polytetramethylene isophthalamide (Polyamide 4I), Poly Examples of the copolymer include one or more of the components such as bis(3-methyl-4-aminohexyl)methane terephthalamide (polyamide PACMT), polybis(3-methyl-4-aminohexyl)methane isophthalamide (polyamide PACMI), polybis(3-methyl-4-aminohexyl)methanendodecamide (polyamide PACM12), polybis(3-methyl-4-aminohexyl)methane tetradecamide (polyamide PACM14), and a copolymer of these or a mixture of these components.
[0081] Examples of the polyacetal include homopolymers having oxymethylene units as the main repeating units, and copolymers mainly composed of oxymethylene units and containing oxyalkylene units having 2 to 8 adjacent carbon atoms in the main chain.
[0082] The polyethylene terephthalate may be, for example, a polymer obtained by polycondensing terephthalic acid or a derivative thereof with ethylene glycol.
[0083] The polybutylene terephthalate may be, for example, a polymer obtained by polycondensing terephthalic acid or a derivative thereof with 1,4-butanediol.
[0084] The polytrimethylene terephthalate may be, for example, a polymer obtained by polycondensing terephthalic acid or a derivative thereof with 1,3-propanediol.
[0085] Examples of the polycarbonate include a polymer obtained by a transesterification method in which a dihydroxydiaryl compound is reacted with a carbonate ester such as diphenyl carbonate in a molten state, and a polymer obtained by a phosgene method in which a dihydroxyaryl compound is reacted with phosgene.
[0086] Examples of the polyarylene sulfide include linear polyphenylene sulfide, crosslinked polyphenylene sulfide which has been polymerized and then cured, polyphenylene sulfide sulfone, polyphenylene sulfide ether, and polyphenylene sulfide ketone.
[0087] Examples of the modified polyphenylene ether include a polymer alloy of poly(2,6-dimethyl-1,4-phenylene) ether and polystyrene, a polymer alloy of poly(2,6-dimethyl-1,4-phenylene) ether and a styrene / butadiene copolymer, a polymer alloy of poly(2,6-dimethyl-1,4-phenylene) ether and a styrene / maleic anhydride copolymer, a polymer alloy of poly(2,6-dimethyl-1,4-phenylene) ether and a polyamide, and a polymer alloy of poly(2,6-dimethyl-1,4-phenylene) ether and a styrene / butadiene / acrylonitrile copolymer.
[0088] Examples of the polyaryletherketone include polyetherketone (PEK), polyetheretherketone (PEEK), polyetherketoneketone (PEKK), and polyetheretherketoneketone (PEEKK).
[0089] Examples of the liquid crystal polymer (LCP) include thermotropic liquid crystal polyesters, such as (co)polymers composed of one or more structural units selected from aromatic hydroxycarbonyl units, aromatic dihydroxy units, aromatic dicarbonyl units, aliphatic dihydroxy units, aliphatic dicarbonyl units, and the like.
[0090] Examples of the fluororesin include polytetrafluoroethylene (PTFE), perfluoroalkoxy resin (PFA), fluorinated ethylene propylene resin (FEP), fluorinated ethylene tetrafluoroethylene resin (ETFE), polyvinyl fluoride (PVF), polyvinylidene fluoride (PVDF), polychlorotrifluoroethylene (PCTFE), ethylene / chlorotrifluoroethylene resin (ECTFE), and the like.
[0091] The ionomer (IO) resin may be a copolymer of an olefin or styrene with an unsaturated carboxylic acid, in which a portion of the carboxyl groups is neutralized with a metal ion.
[0092] Examples of the olefin / vinyl alcohol resin include an ethylene / vinyl alcohol copolymer, a propylene / vinyl alcohol copolymer, a saponified ethylene / vinyl acetate copolymer, and a saponified propylene / vinyl acetate copolymer.
[0093] Examples of the cyclic olefin resin include monocyclic compounds such as cyclohexene, polycyclic compounds such as tetracyclopentadiene, and polymers of cyclic olefin monomers.
[0094] Examples of the polylactic acid include poly-L-lactic acid, which is a homopolymer of the L-form, poly-D-lactic acid, which is a homopolymer of the D-form, and stereocomplex polylactic acid, which is a mixture thereof.
[0095] Examples of the cellulose resin include methyl cellulose, ethyl cellulose, hydroxy cellulose, hydroxy methyl cellulose, hydroxy ethyl cellulose, hydroxy ethyl methyl cellulose, hydroxy propyl methyl cellulose, cellulose acetate, cellulose propionate, and cellulose butyrate.
[0096] Examples of the thermosetting resin include unsaturated polyester resin, vinyl ester resin, epoxy (EP) resin, melamine (MF) resin, phenolic resin (PF), urethane resin (PU), polyisocyanate, polyisocyanurate, polyimide (PI), urea (UF) resin, silicone (SI) resin, furan (FR) resin, benzoguanamine (BR) resin, alkyd resin, xylene resin, bismaleimide triazine (BT) resin, and diallyl phthalate resin (PDAP).
[0097] The intrinsic viscosity of the resin in the glass fiber reinforced resin composition according to the present disclosure may be, for example, 0.3 dl / g or more, 0.5 dl / g or more, or 0.6 dl / g or more, and may be 1.5 dl / g or less, 1.3 dl / g or less, or 1.0 dl / g or less, and these values can be freely combined. A specific example is 0.3 to 1.5 dl / g or 0.5 to 1.3 dl / g, and preferably 0.6 to 1.0 dl / g.
[0098] The intrinsic viscosity (intrinsic viscosity) of the resin in the glass fiber reinforced resin composition may be a value calculated based on the viscosity measured, for example, by a solution viscometer, as a method normally performed by those skilled in the art. The intrinsic viscosity of the resin in the glass fiber reinforced resin composition may be, for example, the intrinsic viscosity measured at 30°C in a mixed solvent of phenol / 1,1,2,2-tetrachloroethane (mass ratio 1 / 1).
[0099] The resin in the glass fiber reinforced resin composition according to the present disclosure may be preferably at least one selected from the group consisting of polybutylene terephthalate, polyethylene terephthalate, polycarbonate, and polyphenylene sulfide, more preferably polybutylene terephthalate, polyethylene terephthalate, polycarbonate, or polyphenylene sulfide, and a specific example may be polybutylene terephthalate.
[0100] The content of the glass fiber material (reinforcing material) in the glass fiber reinforced resin composition according to the present disclosure may be, for example, 10.0 mass% or more, 15.0 mass% or more, 20.0 mass% or more, or 25.0 mass% or more, based on the total amount of the glass fiber reinforced resin composition, and may be 50.0 mass% or less, 45.0 mass% or less, 40.0 mass% or less, or 35.0 mass% or less, and these numerical values can be freely combined. A specific example is 10.0 mass% to 50.0 mass%, and preferably 20.0 mass% to 40.0 mass%.
[0101] The content ratio of resin to glass fiber material (reinforcing material) in the glass fiber reinforced resin composition according to the present disclosure may be, for example, 9.0:1.0 to 5.0:5.0, 8.5:1.5 to 5.5:4.5, 8.0:2.0 to 6.0:4.0, or 7.5:2.5 to 6.5:3.5 on a mass basis.
[0102] The glass fiber reinforced resin composition according to the present disclosure can be obtained by mixing the above-described glass fiber material and resin (mixing step). The mixing method in the mixing step is not particularly limited as long as it is a method capable of mixing the glass fiber material and the resin, and can be performed by a method normally performed by a person skilled in the art, for example, kneading, and the kneading can be performed using, for example, a twin-screw kneader.
[0103] The glass fiber reinforced resin composition according to the present disclosure may further contain various additives in addition to the glass fiber material and the resin. Examples of the various additives include flame retardants, colorants, release agents, antioxidants, UV absorbers, antistatic agents, nucleating agents, plasticizers, fillers, modifiers, etc. These additives may be incorporated into the glass fiber reinforced resin composition by, for example, mixing with the glass fiber material and the resin in a mixing step.
[0104] Examples of flame retardants include phosphorus-based flame retardants such as non-halogen phosphate esters, halogen-containing phosphate esters, non-halogen condensed phosphate esters, halogen-containing condensed phosphate esters, polyphosphates, and red phosphorus; bromine-based flame retardants such as TBA (tetrabromobisphenol A), DBDPO (decabromodiphenyl ether), OCTA (octabromodiphenyl oxide), and TBP (tribromophenol); and inorganic flame retardants such as aluminum hydroxide, antimony trioxide, tin oxide, tin hydroxide, molybdenum oxide, antimony pentoxide, and magnesium hydroxide.
[0105] Examples of the colorant include titanium oxide, zinc oxide, zinc sulfide, and carbon black.
[0106] Examples of the release agent include magnesium stearate, talc stearate, metal soap, polyethylene wax, ethylene bisstearinamide, EDA (ethylene diamine), EBA (ethylene bisstearic acid amide), lithium stearate, and metal salts of higher fatty acids.
[0107] Examples of the antioxidant include phenol-based antioxidants, amine-based antioxidants, sulfur-based antioxidants, and phosphorus-based antioxidants.
[0108] Examples of the ultraviolet absorbing agent include salicylate-based ultraviolet absorbing agents, benzophenone-based ultraviolet absorbing agents, benzotriazole-based ultraviolet absorbing agents, cyanoacrylate-based ultraviolet absorbing agents, nickel chelate-based ultraviolet absorbing agents, and hindered amine-based ultraviolet absorbing agents.
[0109] Examples of the antistatic agent include anionic surfactants, cationic surfactants, nonionic surfactants, and amphoteric surfactants.
[0110] Examples of the nucleating agent include talc, dibenzylidene sorbitol, and a β-crystal nucleating agent.
[0111] Examples of the plasticizer include phthalic acid plasticizers (DOP (dioctyl phthalate), DBP (dibutyl phthalate), DHP (diheptyl phthalate), DIDP (diisodecyl phthalate), DINP (diisononyl phthalate)), fatty acid plasticizers, phosphoric acid plasticizers (TCP (tricresyl phosphate), TMP (trimethyl phosphate), TEP (triethyl phosphate), etc.), adipic acid plasticizers (DOA (dioctyl adipate), DINA (diisononyl adipate), DIDA (diisodecyl adipate)), polyester plasticizers, and epoxy plasticizers.
[0112] Examples of the filler include talc, mica, glass flakes, glass beads, calcium carbonate, and the like.
[0113] Examples of the modifier include polybutadiene, styrene-butadiene copolymer, styrene-butadiene-styrene block copolymer, acrylonitrile-butadiene-styrene copolymer, methyl methacrylate-butadiene-styrene copolymer, methyl methacrylate-acrylonitrile-butadiene-styrene copolymer, methyl methacrylate-butadiene copolymer, acrylonitrile-styrene-acrylic rubber copolymer, acrylonitrile-ethylene propylene rubber-styrene copolymer, methyl methacrylate-acrylic rubber copolymer, methyl methacrylate-acrylic rubber-styrene copolymer, methyl methacrylate-acrylic-butadiene rubber copolymer, methyl methacrylate-acrylic-butadiene rubber copolymer, methyl methacrylate-acrylic-butadiene rubber-styrene copolymer, methyl methacrylate-(acrylic-silicone IPN rubber) copolymer, and natural rubber.
[0114] Another embodiment of the present disclosure may be a method for producing a glass fiber reinforced resin composition according to an embodiment of the present disclosure, the method including a mixing step. The method may include a spinning step and a mixing step in this order, a melting step, a spinning step and a mixing step in this order, or a preparation step, a melting step, a spinning step and a mixing step in this order.
[0115] Another embodiment of the present disclosure is a glass fiber reinforced resin molded product (a glass fiber reinforced resin molded product formed from a glass fiber reinforced resin composition) consisting of a molded product of the glass fiber reinforced resin composition according to one embodiment of the present disclosure. That is, the glass fiber reinforced resin molded product according to another embodiment of the present disclosure is obtained by molding the glass fiber reinforced resin composition according to one embodiment of the present disclosure (molding step). Yet another embodiment of the present disclosure may be a method for producing a glass fiber reinforced resin molded product, which includes molding the glass fiber reinforced resin composition according to one embodiment of the present disclosure.
[0116] The molding method in the molding step is not particularly limited, and for example, the glass fiber reinforced resin can be injection compression molding, two-color molding, hollow molding, foam molding (including supercritical fluid foam molding), insert molding, in-mold coating molding, extrusion molding, sheet molding, thermoforming, rotational molding, lamination molding, press molding, blow molding, stamping molding, infusion, hand layup, spray-up, resin transfer molding, sheet molding compound method, bulk molding compound method, pultrusion method, filament winding method, etc. As a specific example of the molding step, a glass fiber reinforced resin molded product can be obtained by injection molding using pellets of glass fiber reinforced resin.
[0117] According to the present disclosure, it is possible to provide a glass fiber reinforced resin composition that can be used to form a glass fiber reinforced resin molded product having sufficiently high mechanical strength such as tensile strength, using city waste glass as a raw material, and suppressing CO2 emissions during production. According to the present disclosure, it is possible to provide a glass fiber reinforced resin composition that can be used to form a glass fiber reinforced resin molded product having sufficiently high reinforcement efficiency, using city waste glass as a raw material, and suppressing CO2 emissions during production. According to the present disclosure, it is possible to provide a glass fiber reinforced resin composition that can be used to form a glass fiber reinforced resin molded product having sufficiently high mechanical strength such as tensile strength, due to a sufficiently high reinforcement efficiency, using city waste glass as a raw material, and suppressing CO2 emissions during production.
[0118] In this disclosure, suppression of CO2 emissions may mean that the value equivalent to the physical volume-based emission intensity for "other non-metallic minerals" shown in No. 32, column code 62909 in the "Emissions intensity unit based on input-output tables" described in the "Emissions intensity unit database for calculating greenhouse gas emissions, etc. of organizations through the supply chain (Ver. 2.5)" is 0.050t-CO2eq / ton or less or 0.025t-CO2eq / ton or less.
[0119] In the present disclosure, a glass fiber reinforced resin molded product having sufficiently high mechanical strength may have a tensile strength of 90 MPa or more, 100 MPa or more, 110 MPa or more, 115 MPa or more, 116 MPa or more, 117 MPa or more, 118 MPa or more, 119 MPa or more, or 120 MPa or more in a static tensile test in accordance with Japanese Industrial Standards (JIS) K7161-1, 2:2014 conducted at a test temperature of 23°C. The phrase "the mechanical strength of the glass fiber reinforced resin molded product according to one embodiment of the present disclosure is sufficiently high" may mean that the measured mechanical strength is 0.65 times or more, 0.75 times or more, 0.80 times or more, 0.85 times or more, 0.90 times or more, 0.91 times or more, 0.92 times or more, or 0.95 times or more of the measured mechanical strength of a glass fiber reinforced resin molded product prepared in the exact same manner except that the glass fiber material contains, as the glass fiber material, a long glass fiber composed of a glass monofilament having an E-glass composition, or a glass fiber material that is cut or crushed thereof.
[0120] In the present disclosure, the reinforcement efficiency of a glass fiber reinforced resin molded product is sufficiently high, and may be more than 1.00, 1.10 or more, 1.20 or more, 1.25 or more, 1.27 or more, 1.30 or more, 1.35 or more, or 1.38 or more. The reinforcement efficiency of a glass fiber reinforced resin molded product is defined as a value expressed by X / Y, where X is the value obtained by dividing the tensile strength of a glass fiber reinforced resin molded product formed using the glass fiber reinforced resin composition to be evaluated by the tensile strength of a glass fiber reinforced resin molded product formed using a glass fiber reinforced resin composition containing long glass fibers satisfying the E-glass composition, and Y is the value obtained by dividing the tensile strength of a glass monofilament in a glass fiber material contained in the glass fiber reinforced resin composition to be evaluated by the tensile strength of a glass monofilament satisfying the E-glass composition (the tensile strengths are all measured at 23° C., the tensile strength of the glass monofilament is measured at a pulling speed of 5 mm / min, and the tensile strength of the glass fiber reinforced resin molded product is measured at a pulling speed of 2 mm / min). In other words, the higher the reinforcement efficiency of the glass fiber reinforced plastic molding, the higher the efficiency of increasing the mechanical strength of the glass fiber reinforced plastic molding relative to the mechanical strength of the glass monofilament, compared to a glass fiber reinforced plastic molding using E glass as the glass raw material. EXAMPLES
[0121] The present disclosure will be described more specifically below using examples, but the present disclosure is not limited to the following examples.
[0122] The glass composition in the following examples was measured as follows. First, glass fiber or recycled glass cullet was placed in a platinum crucible, and in an electric furnace, the glass fiber or recycled glass cullet was turned into molten glass without any residual melting in the range of 1200 to 1650 ° C., and the molten glass was melted while stirring for 6 hours at a temperature at which the molten glass could flow out of the platinum crucible when the platinum crucible containing the molten glass was tilted 60 ° upward from the horizontal direction to the opening surface, thereby obtaining a homogeneous molten glass. Next, the obtained molten glass was poured onto a carbon plate to produce glass cullet, which was then crushed and powdered to obtain glass powder. The light element Li was quantitatively analyzed using an ICP emission spectrometer after the obtained glass powder was thermally decomposed with acid. The other elements were quantitatively analyzed using a wavelength dispersive X-ray fluorescence analyzer after the glass powder was molded into a disk shape using a press machine. The results of these quantitative analyses were converted into oxides to calculate the content and total amount of each component, and the content of each component in the glass composition was obtained from these values.
[0123] The intrinsic viscosity of the polybutylene terephthalate resin used in the following examples was measured and calculated as follows. Pellets of polybutylene terephthalate resin were dissolved in a mixed solvent of phenol / 1,1,2,2-tetrachloroethane (mass ratio 1 / 1) by stirring at 110°C for 1 hour to a concentration of 1.00 g / dL. The solution was then cooled to 30°C. The number of seconds it took for the sample solution and the solvent alone to fall at 30°C was measured using a fully automatic solution viscometer, and the intrinsic viscosity was calculated according to the following formula. Intrinsic viscosity=((1+4KHηsp)0.5-1) / (2KHC) Here, ηsp=η / η0-1, η is the time for the sample solution to fall, η0 is the time for the solvent alone to fall, C is the concentration of the sample solution (g / dL), and KH is Huggins' constant. KH was set to 0.33. The unit is dL / g. The fully automatic solution viscometer used was a product of Shibayama Scientific Co., Ltd.
[0124] <Example 1> Glass bottles collected as municipal waste were washed and crushed to obtain recycled glass cullet having a particle size of 10 to 50 mm and a glass composition containing, relative to the total amount of glass components, 65.0 mass% SiO2, 2.0 mass% Al2O3, and 4.0 mass% B2O3, with a total content of CaO and MgO of 8.0 mass%, a total content of BaO and SrO of 4.0 mass%, and a total content of Na2O and K2O (R2O) of 17.0 mass% (preparation process).
[0125] The recycled glass cullet obtained in the preparation step was put into a platinum vessel equipped with 200 nozzle tips at the bottom, and the platinum vessel was heated to 1000°C to 1300°C to melt the glass cullet and obtain molten glass (melting step). Next, the molten glass was drawn out from the nozzle tips of the platinum vessel and wound around a winding device. The winding device was rotated to wind the molten glass at a rotation speed of 1000 rpm, and a sizing agent containing aminosilane and urethane resin was applied to the monofilament at a ratio of 0.8 mass% relative to the monofilament using an applicator provided between the nozzle tips and the winding device, thereby producing a long glass fiber with a number of monofilaments of 200 and a number average fiber diameter of 15 μm (spinning step). The glass composition of the obtained long glass fiber was measured, and the glass composition was substantially the same as the glass composition of the recycled glass cullet obtained in the preparation step.
[0126] The long glass fibers obtained in the spinning process were cut to 3 mm to obtain chopped strands. The chopped strands were then mixed with a polybutylene terephthalate resin having an intrinsic viscosity of 0.83 dl / g in a twin-screw kneader (manufactured by Shibaura Machine Co., Ltd., product name: TEM-26SS) at a screw rotation speed of 100 rpm to produce resin pellets (glass fiber reinforced resin pellets) having a glass content of 30.0 mass% (mixing process).
[0127] The glass fiber reinforced resin pellets obtained in the mixing process were injection molded using an injection molding machine (manufactured by Nissei Plastics Industrial Co., Ltd., product name: NEX80) at a mold temperature of 140°C and an injection temperature of 260°C to produce glass fiber reinforced resin molded products, which are dumbbell test pieces conforming to JIS K 7161-1:2014 (molding process).
[0128] <Example 2> 75 parts by mass of the recycled glass cullet prepared in the preparation step of Example 1 and 25 parts by mass of a mineral material having an E-glass composition (a mineral material having a glass composition containing 54.0% by mass of SiO2, 14.0% by mass of Al2O3, and 6.0% by mass of B2O3, with respect to the total amount of glass components, as a designed glass composition based on the components contained in each mineral designed for the production of glass fiber, with a total content of CaO and MgO of 24.0% by mass, a total content of BaO and SrO of 0.0% by mass, R2O of 1.0% by mass, and other components of 1.0% by mass) were mixed to obtain a glass raw material. The obtained glass raw material was placed in a platinum crucible, and the platinum crucible was held in an electric furnace at a temperature in the range of 1400 to 1550 ° C. for 4 hours, and the glass raw material was melted while being stirred, to obtain a homogeneous molten glass. The obtained molten glass was poured onto a carbon plate and cooled to obtain a lump-shaped glass cullet (preparation step).
[0129] The glass cullet obtained in the preparation step was put into a platinum vessel equipped with 200 nozzle tips at the bottom, and the platinum vessel was heated to 1000°C to 1300°C to melt the glass cullet and obtain molten glass (melting step). Next, the molten glass was drawn out from the nozzle tips of the platinum vessel and wound around a winding device. The winding device was rotated to wind the molten glass at a rotation speed of 1000 rpm, and a sizing agent containing a silane coupling agent and a film former was applied to the monofilament using an applicator provided between the nozzle tips and the winding device, thereby producing a long glass fiber having a number of monofilaments of 200 and a number average fiber diameter of 15 μm (spinning step). The glass composition of the obtained long glass fiber was measured and it was found to have a glass composition containing, relative to the total amount of glass components, 62.2 mass% SiO2, 5.0 mass% Al2O3, and 4.5 mass% B2O3, with a total content of CaO and MgO of 12.0 mass%, a total content of BaO and SrO of 3.0 mass%, R2O of 13.0 mass%, and 0.3 mass% of other components.
[0130] Using the long glass fibers obtained in the spinning process, a mixing process was carried out in the same manner as in Example 1 to obtain glass fiber reinforced resin pellets. In addition, using the obtained glass fiber reinforced resin pellets, a molding process was carried out in the same manner as in Example 1 to produce a glass fiber reinforced resin molded product.
[0131] <Comparative Example 1> As the glass raw material in the preparation step, a mineral material having an E glass composition (a mineral material having a glass composition containing 54.0 mass% SiO2, 14.0 mass% Al2O3, and 6.0 mass% B2O3 based on the components of each mineral designed for the production of glass fiber, with respect to the total amount of glass components, a total content of CaO and MgO of 24.0 mass%, a total content of BaO and SrO of 0.0 mass%, R2O of 1.0 mass%, and other components of 1.0 mass%) was used, and the preparation step, melting step, and spinning step were performed in the same manner as in Example 2 to obtain a long glass fiber, except that the heating temperature in the melting step was set to 1150 to 1450°C. When the glass composition of the obtained long glass fiber was measured, the glass composition was substantially the same as the glass composition of the mineral material designed for the production of glass fiber used in the preparation step.
[0132] Using the long glass fibers obtained in the spinning process, a mixing process was carried out in the same manner as in Example 1 to obtain glass fiber reinforced resin pellets. In addition, using the obtained glass fiber reinforced resin pellets, a molding process was carried out in the same manner as in Example 1 to produce a glass fiber reinforced resin molded product.
[0133] <Comparative Example 2> A mineral material having a glass composition containing 65.0 mass% SiO2 and 25.0 mass% Al2O3, with a total content of CaO and MgO of 10.0 mass%, and a total content of BaO and SrO of 0.0 mass%, based on the components of each mineral designed for the production of glass fiber, was used as a glass raw material, and a long glass fiber was obtained by carrying out the preparation step, melting step, and spinning step in the same manner as in Example 2, except that the heating temperature in the preparation step was 1550 to 1650°C and the heating temperature in the melting step was 1500 to 1650°C. The glass composition of the obtained long glass fiber was measured, and the glass composition was substantially the same as the glass composition of the mineral material designed for the production of glass fiber used in the preparation step.
[0134] Using the long glass fibers obtained in the spinning process, a mixing process was carried out in the same manner as in Example 1 to obtain glass fiber reinforced resin pellets. In addition, using the obtained glass fiber reinforced resin pellets, a molding process was carried out in the same manner as in Example 1 to produce a glass fiber reinforced resin molded product.
[0135] <Comparative Example 3> Based on the components of each mineral designed for the production of glass fiber, a designed glass composition was prepared based on the components of each mineral, and the glass composition contained 54.0 mass% SiO2, 12.0 mass% Al2O3, and 23.0 mass% B2O3 relative to the total amount of glass fiber, the total content of CaO and MgO was 8.0 mass%, the total content of BaO and SrO was 0.0 mass%, and other components were 3.0 mass%. A mineral material having such a glass composition was used as a glass raw material, and a preparation step, a melting step, and a spinning step were performed in the same manner as in Example 2 to obtain a long glass fiber, except that the heating temperature in the preparation step was 1450 to 1600°C and the heating temperature in the melting step was 1250 to 1550°C. The glass composition of the obtained long glass fiber was measured, and the glass composition was substantially the same as the glass composition contained in the mineral material designed for the production of glass fiber used in the preparation step.
[0136] Using the long glass fibers obtained in the spinning process, a mixing process was carried out in the same manner as in Example 1 to obtain glass fiber reinforced resin pellets. In addition, using the obtained glass fiber reinforced resin pellets, a molding process was carried out in the same manner as in Example 1 to produce a glass fiber reinforced resin molded product.
[0137] <Comparative Example 4> The recycled glass cullet obtained in the preparation step of Example 1 was melted, and the molten glass was made to flow out from a number of holes using a centrifugal fiberization device, to produce glass short fibers (glass wool) with a number average fiber diameter of 8 μm. The glass composition of the obtained glass wool was measured, and the glass composition was substantially the same as the glass composition of the recycled glass cullet obtained in the preparation step of Example 1. A sizing agent containing a silane coupling agent and a urethane resin was applied to the glass wool using a spray at a ratio of 0.8 mass% relative to the mass of the glass wool.
[0138] The glass wool to which a sizing agent was added was compressed and solidified, and polybutylene terephthalate resin having an intrinsic viscosity of 0.83 dl / g was kneaded in a twin-screw kneader (manufactured by Shibaura Machine Co., Ltd., product name: TEM-26SS) at a screw speed of 100 rpm to produce resin pellets (glass fiber reinforced resin pellets) with a glass content of 30.0 mass%. The glass fiber reinforced resin pellets were used to carry out a molding process similar to that of Example 1 to produce a glass fiber reinforced resin molded product.
[0139] <Measurement of tensile strength of continuous glass fiber monofilament> After the spinning process in Examples 1 to 3 and Comparative Examples 1 to 3, monofilaments were taken one by one from between the nozzle tip and the winding device. Also, monofilaments were taken one by one from the glass wool prepared in Comparative Example 4. From the monofilaments thus obtained, those that were not deteriorated due to contact or friction were selected, and at least 30 monofilaments were selected as measurement samples for each of the Examples and Comparative Examples.
[0140] First, the fiber diameters of at least 10 measurement samples for each of Examples 1 to 3 and Comparative Examples 1 to 4 were measured by observing them with a scanning electron microscope (manufactured by Hitachi High-Technologies Corporation, product name: S-3400N). Of the obtained measured values, the maximum two measured values and the minimum two measured values were excluded, and the number average of the remaining measured values was taken as the average fiber diameter. The cross-sectional shape was taken as a circle, and the fiber cross-sectional area was calculated.
[0141] Next, the measurement samples of Examples 1 to 3 and Comparative Examples 1 to 4 were bonded to a given mount with a rectangular hole with long sides of 25 mm and short sides of 10 mm in the center so that the fiber length in the hole was 25 mm to prepare a test piece. At a temperature condition of 23°C, the obtained test piece was set in the grip of a tensile tester (manufactured by A&D Co., Ltd., product name: Single column type tensile tester STB-1225S), and after cutting off the end of the mount, a tensile test was performed at a crosshead speed of 5 mm / min to measure the maximum load value at break. Note that test pieces in which threads came off or broke during the measurement were excluded.
[0142] The maximum load value thus obtained was divided by the fiber cross-sectional area to calculate the monofilament tensile strength S [GPa] at 23°C and a pulling speed of 5 mm / min. Of the valid values obtained, the maximum and minimum two measured values were excluded, and the arithmetic mean of the remaining calculated values was taken as the measured value of the monofilament tensile strength. The results are shown in Table 1.
[0143] <Measurement of tensile strength of glass fiber reinforced resin molded products> For the glass fiber reinforced resin molded products obtained in Examples 1 to 3 and Comparative Examples 1 to 4, a static tensile test was performed in accordance with Japanese Industrial Standards (JIS) K7161-1, 2:2014 using a precision universal testing machine (manufactured by Shimadzu Corporation, product name: precision universal testing machine AG-50kNXplus) at a test temperature of 23° C. to measure the tensile strength [MPa] of the glass fiber reinforced resin molded products. The results are shown in Table 1.
[0144] <Calculation of reinforcement efficiency of glass fiber reinforced plastic moldings> Based on the monofilament tensile strength and the tensile strength of the glass fiber reinforced resin molded product obtained above, the strengthening efficiency of the glass fiber reinforced resin molded product in each of Examples 1 to 3 and Comparative Examples 1 to 4 (the calculation target) was calculated. Specifically, X, which is the value obtained by dividing the tensile strength of the glass fiber reinforced resin molded product of the calculation target by the tensile strength of the glass fiber reinforced resin molded product of Comparative Example 1, and Y, which is the value obtained by dividing the monofilament tensile strength of the calculation target by the monofilament tensile strength of Comparative Example 1, were calculated respectively, and the strengthening efficiency of the glass fiber reinforced resin molded product of the calculation target was calculated as the value obtained by dividing X by Y (X / Y).
[0145] <Measurement of liquid phase temperature> First, the glass raw materials were mixed so that the glass composition after melting and solidification became the same as the glass composition of the glass long fibers or the glass composition of the glass wool in Examples 1 to 2 and Comparative Examples 1 to 4 shown in Table 1, and a glass batch was obtained. Next, the obtained glass batch was put into a platinum crucible, and this platinum crucible was held in an electric furnace for 4 hours under the temperature conditions in the range of 1200 to 1650 °C, where the glass batch of each example or comparative example melted completely into molten glass, and the molten glass could flow out of the platinum crucible when the platinum crucible containing the molten glass was tilted upward by 60° from the horizontal direction on the opening surface, and the glass batch was melted while being stirred to obtain a homogeneous molten glass. Next, the obtained molten glass was poured onto a carbon plate and cooled to obtain a块状 glass cullet. Then, the obtained glass cullet was crushed to obtain glass particles with a particle size of 0.5 to 1.5 mm. Then, 40 g of the obtained glass particles were put into a platinum boat of 180 mm × 20 mm × 15 mm, heated in a tubular electric furnace with a temperature gradient of 800 to 1500 °C for 8 hours or more, taken out from the tubular electric furnace, and observed with a polarizing microscope to identify the position where crystals (devitrification) derived from the glass began to precipitate. Next, the temperature in the tubular electric furnace was measured actually using a B thermocouple, and the temperature at the position where the crystals began to precipitate was obtained as the liquid phase temperature. The results are shown in Table 1.
[0146] <CO2 emission reduction rate> In the "Emissions Unit Database for Calculating Organizational Greenhouse Gas Emissions Throughout the Supply Chain (Ver.2.5)," the numerical value corresponding to the physical-volume-based emissions unit for No. 32, column code 62909 "Other non-metallic minerals" in the "Emissions Unit Database for Calculating Organizational Greenhouse Gas Emissions Throughout the Supply Chain (Ver.2.5)" was evaluated as "A" if it was in the range of 0 to 0.025 t-CO2eq / ton, "B" if it was in the range of 0.026 to 0.050 t-CO2eq / ton, and "C" if it was 0.051 t-CO2eq / ton or more. The results are shown in Table 1.
[0147] [Table 1]
[0148] According to the results shown in Table 1, the glass fiber reinforced plastic molded products according to Examples 1 and 2, which have a T / S of 361.5 to 457.0, have a high reinforcement efficiency and therefore a sufficiently high strength of the glass fiber reinforced plastic molded product, even though more than 50 mass% of waste glass from the market is used as a glass raw material, and such molded products could be manufactured while reducing CO2 emissions during production. Furthermore, according to the results shown in Table 1, the glass fiber reinforced plastic molded product according to Example 1, which has a T / S of 410.2 to 447.0, has a remarkably high reinforcement efficiency and therefore a sufficiently high strength of the glass fiber reinforced plastic molded product, even though more than 50 mass% of waste glass from the market is used as a glass raw material, and such molded products could be manufactured while reducing CO2 emissions during production.
Claims
1. The present invention comprises a glass fiber material, which is a long glass fiber or a cut or crushed product thereof, obtained by melting and spinning a glass raw material containing more than 50% by mass of waste glass in the market, and a resin; A glass fiber reinforced resin composition, in which the ratio (T / S) of the liquidus temperature T (°C) of glass forming the long glass fiber to the tensile strength S (GPa) of a glass monofilament constituting the long glass fiber at 23°C and a pulling speed of 5 mm / min is 361.5 to 457.
0.
2. The glass fiber reinforced resin composition according to claim 1, wherein the ratio (T / S) is 410.2 to 447.
0.
3. The glass raw material is SiO 2 is 63.5 to 66.5 mass %, and Al 2 O 3 is 1.5 to 3.5 mass %, B 2 O 3 is 3.0 to 4.5 mass%, the sum of CaO and MgO is 7.5 to 10.0 mass%, the sum of BaO and SrO is 3.5 to 5.5 mass%, and Na 2 O and K 2 The glass fiber reinforced resin composition according to claim 1, comprising a glass composition having a total O content of 15.0 to 17.3 mass%.
4. The glass fiber reinforced resin composition according to claim 1, wherein the content of the glass fiber material in the glass fiber reinforced resin composition is 10.0 to 50.0 mass% based on the total amount of the glass fiber reinforced resin composition.
5. 2. The glass fiber reinforced resin composition according to claim 1, wherein the glass fiber material is coated with an aminosilane and a urethane resin.
6. The glass fiber reinforced resin composition according to claim 1, wherein the resin has an intrinsic viscosity of 0.3 to 1.5 dl / g.
7. The glass fiber reinforced resin composition according to claim 1 , wherein the resin is at least one selected from the group consisting of polybutylene terephthalate, polyethylene terephthalate, polycarbonate, and polyphenylene sulfide.
Citation Information
Patent Citations
Glass composition for manufacturing inorganic fiber and its molding
JP2003267753A
Method for producing long glass fibers
WO2023276617A1
Cited By
Resin composition, pellet, molded article, method for improving appearance, and appearance improver
JP2026089452A
Glass composition for glass fiber and glass fiber
JP7817665B1
Glass chopped strand mats, glass fiber reinforced resin molded products, and automotive molded headliner materials.
JP7904516B1
Glass composition for glass fiber and glass fiber
WO2026014302A1
Resin-reinforcing glass fiber
WO2026014303A1