Two-pack type aqueous coating material

A two-component water-based coating material with specific resin and silane compound ratios addresses adhesion issues in water-based coatings, ensuring strong bonding and durability on diverse substrates and coatings.

JP2024133371AActive Publication Date: 2024-10-01BEKKU KK
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024117613
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-09-06
Filing Date
2024-07-23
Publication Date
2024-10-01
Estimated Expiration
2040-08-31

AI Technical Summary

Technical Problem

Water-based undercoating materials often exhibit poorer adhesion compared to solvent-based materials, particularly when applied to exterior building materials requiring high weather resistance and stain resistance, making it difficult to achieve sufficient adhesion with existing water-based coatings.

Method used

A two-component water-based coating material is developed, comprising a base material containing an epoxy resin emulsion and a curing agent made of an amino group-containing resin and an amino group-containing silane compound, with specific weight ratios and combinations of epoxy resin emulsion and acrylic resin emulsion to enhance adhesion.

Benefits of technology

The coating material demonstrates excellent adhesion to various substrates and coatings, including those with existing coatings, while maintaining stability and pot life, and forms films with improved water resistance and appearance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133371000001
    Figure 2024133371000001
  • Figure 2024133371000002
    Figure 2024133371000002
  • Figure 2024133371000003
    Figure 2024133371000003
Patent Text Reader

Abstract

To provide a two-pack type aqueous coating material which is composed of a curing agent for an aqueous epoxy resin exhibiting excellent adhesion to various base materials and a coating film, and a main agent containing an aqueous epoxy resin.SOLUTION: A two-pack type aqueous coating material is composed of a curing agent for an aqueous epoxy resin, and a main agent containing an aqueous epoxy resin, wherein the curing agent contains an amino group-containing resin, and an amino group-containing silane compound, a mixture ratio (solid content weight ratio) of the amino group-containing resin and the amino group-containing silane compound is 5:95 to 90:10, and the main agent contains epoxy resin emulsion and epoxy group-containing acrylic resin emulsion, as an aqueous epoxy resin.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention is a novel Two-component water-based coating material This is regarding. [Background technology]

[0002] In painting interior and exterior walls and floors of buildings, various undercoat materials are selected and used in consideration of adhesion to the substrate. Conventionally, such undercoat materials have been mainly solvent-based, but recently, water-based undercoat materials have been adopted in consideration of the environment, safety, etc. For example, Patent Document 1 describes a two-liquid reactive curing water-based paint composition for undercoat paint, which is composed of a base agent containing an epoxy resin emulsion and a curing agent containing an amine resin.

[0003] However, water-based undercoat materials may have poorer adhesion than solvent-based undercoat materials. In particular, in recent years, exterior building materials used on exterior wall surfaces are provided with various coating films having functionality such as high weather resistance and stain resistance. In the repair of such coating films, water-based undercoat materials may not be able to provide sufficient adhesion, and solvent-based undercoat materials are currently widely used. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2018-53028 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention has been made in consideration of the above problems, and has an object to provide an aqueous coating material that can ensure sufficient adhesion to various substrates and coating films. [Means for solving the problem]

[0006] As a result of extensive research into such problems, the present inventors、 An amino group-containing resin and an amino group-containing silane compound are mixed in a specific weight ratio. For water-based epoxy resin Hardener A two-component water-based coating material consisting of a base material containing an epoxy resin emulsion and an epoxy-containing acrylic resin emulsion. We have discovered and completed the present invention.

[0007] That is, the present invention has the following features. 1. Hardener for water-based epoxy resin A two-component water-based coating material consisting of a base material containing water-based epoxy resin. And, The curing agent is The composition includes an amino group-containing resin and an amino group-containing silane compound, The amino group-containing resin is a polyamine resin (excluding amino group-containing silane compounds), The amino group-containing silane compound is a compound having an amino group and an alkoxysilyl group, The mixing ratio (solid weight ratio) of the amino group-containing resin to the amino group-containing silane compound is 5:95 to 90:10. the law of nature, The base material contains an epoxy resin emulsion and an epoxy group-containing acrylic resin emulsion as an aqueous epoxy resin. Characterized by Two-component water-based coating material . 2. 2. The two-component water-based coating material according to 1, wherein the mixing ratio (solids weight ratio) of the epoxy resin emulsion to the epoxy group-containing acrylic resin emulsion is 5:95 to 80:20. Effect of the Invention

[0008] The present invention A two-liquid water-based coating material consisting of a hardener for water-based epoxy resin and a base material containing water-based epoxy resin, It exhibits excellent adhesion to a variety of substrates and coatings. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] (hardening agent) The curing agent of the present invention is mixed with a resin composition (hereinafter, also simply referred to as the "main agent") containing an aqueous epoxy resin (A), and contains an amino group-containing resin (B) and an amino group-containing silane compound (M).

[0010] The amino group-containing resin (B) of the present invention (hereinafter, simply referred to as "(B) component") reacts with the aqueous epoxy resin (A) to form a coating. As such (B) component, for example, a polyamine resin containing two or more amino groups in one molecule can be used, and examples thereof include aliphatic polyamines, alicyclic polyamines, aromatic polyamines, heterocyclic amines, and modified polyamine resins obtained by modifying the amino groups of these polyamine resins. In addition, known methods can be used to modify the above polyamine resins, and examples thereof include amidation of amino groups, Mannich reaction of amino groups with carbonyl compounds, addition reaction of amino groups with epoxy groups, and addition reaction of amino groups with styrene. In addition, as (B) component, aliphatic polyamides, alicyclic polyamides, aromatic polyamides, aliphatic polyamidoamines, alicyclic polyamidoamines, aromatic polyamidoamines, etc. can also be used. These can be used alone or in combination of two or more.

[0011] In the present invention, it is preferable that the (B) component contains at least one selected from, for example, aliphatic polyamines and modified aliphatic polyamines. This improves adhesion and adhesion to substrates and coatings when mixed with a base material containing an aqueous epoxy resin. Examples of aliphatic polyamines include chain aliphatic polyamines such as diethylenetriamine, triethylenetetraamine, tetraethylenepentamine, dipropylenediamine, diethylaminopropylamine, and hexamethylenediamine; cyclic aliphatic polyamines such as N-aminoethylpiperazine, bis(4-amino-3-methylcyclohexyl)methane, menthenediamine, isophoronediamine, 4,4'-diaminodicyclohexylmethane, 3,9-bis(3-aminopropyl)-2,4,8,10-tetraoxaspiro[5.5]undecane (spiroacetaldiamine), norbornanediamine, tricyclodecanediamine, and 1,3-bisaminomethylcyclohexane; and aliphatic aromatic amines such as metaxylenediamine. In the present invention, it is particularly preferable that the monomer contains at least one selected from meta-xylylenediamine and a styrene addition reaction product of meta-xylylenediamine.

[0012] The embodiment of the (B) component is not particularly limited, but a water-soluble resin that can be dissolved in an aqueous medium, or a water-dispersed resin that can be dispersed in an aqueous medium, can be used. In the present invention, it is preferable that the (B) component contains a water-soluble resin. In this case, the storage stability is excellent and the activity of the amino group-containing silane compound (M) can be increased. In addition, when mixed with the main agent, the reactivity with the aqueous epoxy resin is increased, and the adhesion and adhesion to the substrate and the coating film are further improved, and a coating film with excellent water resistance and coating film appearance can be formed. The (B) component may be a solvent-free type (solid content 100% by weight) or may be one in which the (B) component is dissolved or dispersed in an aqueous medium in advance. The solid content of the (B) component is preferably 50% by weight or more (more preferably 55% by weight or more, and even more preferably 60% by weight or more). The upper limit of the solid content of the (B) component is 100% by weight or less. When this range is satisfied, the effects of the present invention can be fully exhibited. The aqueous medium is a medium that mainly contains water, and may contain water-soluble solvents such as lower alcohols, polyhydric alcohols, ether compounds, ester compounds, and alkylene oxide-containing compounds, as necessary.

[0013] In addition, the active hydrogen equivalent y of the component (B) is b is preferably 10 to 1000 (more preferably 50 to 800, and further preferably 80 to 600). b " is the number of grams of resin solids containing 1 gram equivalent of active hydrogen groups [g / eq], and is the value obtained by dividing the weight average molecular weight of the amino group-containing resin by the number of hydrogen atoms of the amino group per molecule. In the present invention, "α to β" is synonymous with "α or more and β or less."

[0014] As the amino group-containing silane compound (M) (hereinafter also simply referred to as "component (M)"), a compound having an amino group and an alkoxysilyl group, or a compound having an amino group and a cyclic siloxane, etc., can be used. These can be used alone or in combination of two or more.

[0015] Examples of the compound having an amino group and an alkoxysilyl group include an amino group-containing silane coupling agent, a hydrolyzed oligomer thereof, and a polymer having an alkoxysilyl group and an amino group. Specific examples of the amino group-containing silane coupling agent include: γ-Aminopropyltrimethoxysilane, γ-Aminopropyltriethoxysilane, γ-Aminopropyltriisopropoxysilane, γ-Aminopropylmethyldimethoxysilane, γ-Aminopropylmethyldiethoxysilane, N-β(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β(aminoethyl)-γ-aminopropylmethyldimethoxysilane, N-β(aminoethyl)-γ-aminopropyltriethoxysilane, N-β(aminoethyl)-γ-aminopropylmethyldiethoxysilane, N-β(aminoethyl) )-γ-aminopropyltriisopropoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, γ-ureidopropyltrimethoxysilane, γ-anilinopropyltrimethoxysilane, γ-ureidopropyltrimethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, N-vinylbenzyl-γ-aminopropyltriethoxysilane, N-β(aminoethyl)-8-aminooctyltrimethoxysilane, γ-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, and the like.

[0016] As the hydrolysis oligomer of the amino group-containing silane coupling agent, those having an alkoxysilyl group and an amino group can be used. As such component (M), those in which some or all of the alkoxysilyl groups have been converted to silanol groups can also be used.

[0017] In particular, in the present invention, as the component (M), an amino group-containing silane coupling agent is preferred, such as one or more selected from γ-aminopropylmethyldimethoxysilane, γ-aminopropylmethyldiethoxysilane, N-β(aminoethyl)-γ-aminopropylmethyldimethoxysilane, and N-β(aminoethyl)-γ-aminopropylmethyldiethoxysilane. When these are used, the adhesion to the substrate and the coating film is improved.

[0018] In addition, the above component (M) has an active hydrogen equivalent y m However, the active hydrogen equivalent y is preferably 10 to 500 (more preferably 20 to 400, and further preferably 30 to 300). m " is the number of grams [g / eq] of an amino group-containing silane compound containing 1 gram equivalent of active hydrogen groups, and is the value obtained by dividing the weight average molecular weight of the amino group-containing silane compound by the number of hydrogen atoms of the amino group per molecule.

[0019] The curing agent of the present invention is characterized in that it contains the above-mentioned (B) component and the above-mentioned (M) component in a solids weight ratio of (B) component:(M) component=5:95 to 90:10 (preferably 10:90 to 60:40, more preferably 12:88 to 50:50, and even more preferably 15:85 to 45:55).When such a range is satisfied, the curing agent has excellent storage stability, and when mixed with the base material, it can fully exhibit adhesion and adhesion to the substrate and coating film.

[0020] The curing agent of the present invention contains the above-mentioned (B) component and the above-mentioned (M) component, and the solid content is preferably 10% by weight or more (more preferably 15% by weight or more, and even more preferably 20% by weight or more). The upper limit of the solid content is 100% by weight or less. When this range is satisfied, the effects of the present invention can be fully exhibited. The solid content can be adjusted by mixing the above-mentioned aqueous medium. Specifically, the aqueous medium in the curing agent may be one mixed during the production of the curing agent, or may be one contained as a medium such as the above-mentioned (B) component or the above-mentioned (M) component. When water is contained as the aqueous medium, the water content in the curing agent is preferably 30% by weight or less (more preferably 20% by weight or less, and even more preferably 10% by weight or less), and an embodiment that does not substantially contain water is also suitable. When this range is satisfied, the storage stability of the curing agent can be fully exhibited, and the activity of the above-mentioned (M) component can be increased, and when mixed with the main agent, the adhesion development and adhesion to the substrate and the coating film can be further improved.

[0021] It is preferable to mix a curing accelerator (O) (hereinafter, also referred to simply as "component (O)") with the curing agent of the present invention. Examples of component (O) include various aromatic carboxylic acids such as benzoic acid, salicylic acid, trihydroxybenzoic acid, phthalic acid, cinnamic acid, and benzenehexacarboxylic acid; tertiary amines such as trimethylamine, ethyldimethylamine, propyldimethylamine, N,N'-dimethylpiperazine, pyridine, picoline, 1,8-diazabiscyclo(5,4,0)undecene-1 (DBU), benzyldimethylamine, 2-(dimethylaminomethyl)phenol (DMP-10), and 2,4,6-tris(dimethylaminomethyl)phenol (DMP-30); hydroxyamines such as hydroxylamine and phenoxyamine; Examples of the (B) component include silamines, imidazole, 1-methylimidazole, 2-methylimidazole, 4(5)-methylimidazole, 2-ethyl-4-methylimidazole, 2-ethylimidazole, 2-phenylimidazole, and other imidazoles; amines other than the (M) component; phenols such as phenol novolac, o-cresol novolac, p-cresol novolac, t-butylphenol novolac, and dicyclopentadiene cresol; and organometallic compounds such as tin octylate, dibutyltin dilaurate, dibutyltin diacetate, organotitanate, and sodium acetate. These can be used alone or in combination of two or more. Among these (O) components, aromatic carboxylic acids are particularly preferred.

[0022] The amount of the (O) component mixed is preferably 0.01 to 10 parts by weight (preferably 0.02 to 8 parts by weight) based on 100 parts by weight of the total (solid content) of the (B) and (M) components. In this range, the reactivity with the water-based epoxy resin is increased, and the adhesion and adhesion to the substrate and coating film are further improved, and a coating film excellent in water resistance and coating film appearance can be formed.

[0023] <Water-based coating material> The above curing agent is used as a curing agent for the aqueous epoxy resin (A). In the present invention, it is preferable to use the above curing agent as a two-liquid aqueous coating material consisting of a base material containing the aqueous epoxy resin (A).

[0024] (Main ingredient) The base material of the present invention is characterized by containing an aqueous epoxy resin (A). In the present invention, the aqueous epoxy resin (A) (hereinafter, also simply referred to as "component (A)") is an aqueous resin component containing an epoxy group, and for example, (A1) an epoxy resin dissolved or dispersed in an aqueous medium (hereinafter also referred to simply as "component (A1)"); (A2) a monomer obtained by emulsion polymerization of a monomer group including an epoxy group-containing monomer (hereinafter, also referred to simply as “component (A2)”), These may be used in combination. In the present invention, a resin having both an epoxy group and an amino group may be treated as a resin containing a relatively large number of epoxy groups in one molecule as component (A) and as a resin containing a relatively large number of amino groups in one molecule as component (B).

[0025] Examples of the (A1) component include water-soluble epoxy resins and aqueous epoxy resin dispersions. In the present invention, the (A1) component preferably contains an aqueous epoxy resin dispersion (epoxy resin emulsion) in which an epoxy resin is dispersed or emulsified in an aqueous medium. When dispersing an epoxy resin in an aqueous medium, an emulsifier or the like can be used as necessary. The aqueous medium is a medium that mainly contains water, and may contain water-soluble solvents such as lower alcohols, polyhydric alcohols, ether compounds, ester compounds, and alkylene oxide-containing compounds as necessary.

[0026] The epoxy resin of the component (A1) may be any epoxy resin that can be dissolved or dispersed in an aqueous medium, and may be either a solid epoxy resin and / or a liquid epoxy resin. For example, a resin containing at least one epoxy group, preferably at least two epoxy groups in the molecule, may be used, and examples of such an epoxy resin include aromatic epoxy resins, aliphatic epoxy resins, alicyclic epoxy resins, polybutadiene resins having epoxy groups, and polyurethane resins having epoxy groups. In the present invention, aromatic epoxy resins are preferred, and examples of such resins include bisphenol A type epoxy resins, bisphenol AD ​​type epoxy resins, bisphenol F type epoxy resins, and novolac type epoxy resins. Among these, at least one selected from bisphenol A type epoxy resins, bisphenol AD ​​type epoxy resins, and bisphenol F type epoxy resins are particularly preferred. Furthermore, the epoxy resin may be one whose molecular weight has been increased as necessary, a fatty acid-modified epoxy resin obtained by reacting a fatty acid, or one obtained by making an amine-added epoxy resin (amine-modified epoxy resin) obtained by addition reaction of an amino group-containing compound water-soluble, or the like. These can be used alone or in combination of two or more. Note that solid epoxy resins are those that are solid at room temperature (23°C), and liquid epoxy resins are those that are liquid at room temperature (23°C).

[0027] In the present invention, the component (A1) preferably contains a solid epoxy resin (a1) as an essential component. Such an embodiment includes an embodiment containing only the solid epoxy resin (a1) and an embodiment containing the solid epoxy resin (a1) and the liquid epoxy resin (a2). This allows the effects of the present invention to be fully achieved. When the solid epoxy resin (a1) and the liquid epoxy resin (a2) are mixed, the mixing ratio (solids weight ratio) is preferably 100:0 to 5:95 (more preferably 100:0 to 10:90), depending on the epoxy equivalent of each epoxy resin.

[0028] The method for preparing the epoxy resin water dispersion (epoxy resin emulsion) is not particularly limited, but for example, a method of mixing a solid epoxy resin and / or a liquid epoxy resin with an emulsifier as necessary to prepare a resin solution, and then mixing it with an aqueous medium (containing an emulsifier as necessary) to emulsify it, etc. can be mentioned. In addition, during the above preparation, heating can be performed as necessary. In the present invention, when a solid epoxy resin and a liquid epoxy resin are used in combination, it is preferable to prepare aqueous dispersions of the solid epoxy resin and the liquid epoxy resin, and then mix them for use. The resin solid content of the epoxy resin water dispersion is not particularly limited, but is preferably 10 to 80% by weight (more preferably 20 to 70% by weight).

[0029] As the emulsifier, for example, anionic surfactants, nonionic surfactants, etc. can be used either alone or in combination. Examples of the anionic surfactant include alkali metal sulfonates such as sodium dodecylbenzenesulfonate, sodium laurylnaphthalenesulfonate, and sodium stearyl diphenyl ether disulfonate; and alkali metal sulfates such as sodium lauryl sulfate, polyoxyethylene lauryl ether sodium sulfate, and polyoxyethylene octylphenyl ether sodium sulfate. Examples of nonionic surfactants include polyoxyethylene lauryl ether, polyoxyethylene oleyl ether, polyoxyethylene octylphenyl ether, polyoxyethylene nonylphenyl ether, and oxyethylene-oxypropylene block copolymers. The amount of the emulsifier to be added is preferably within the range of 0.1 to 15% by weight (more preferably 0.1 to 10% by weight, and even more preferably 0.5 to 5% by weight) based on the resin solid content.

[0030] The average particle size of the epoxy resin water dispersion of the component (A1) of the present invention is not particularly limited, but is preferably 100 to 1000 nm (more preferably 150 to 900 nm, and even more preferably 200 to 800 nm). If the average particle size is within such a range, advantageous effects can be obtained in terms of sealing properties, efflorescence resistance, whitening resistance, etc. The average particle size referred to here is a value measured by a dynamic light scattering method.

[0031] The component (A1) of the present invention has an epoxy equivalent x a However, the epoxy equivalent x is preferably 100 to 3000 (more preferably 110 to 2000, and further preferably 120 to 1500). a " is the number of grams of resin solids containing 1 gram equivalent of epoxy groups [g / eq], and is the value obtained by dividing the weight average molecular weight of the epoxy resin by the number of epoxy groups per molecule.

[0032] In addition, the above component (A1) has an epoxy equivalent x a It is also possible to use a mixture of particles having different sizes and average particle sizes.

[0033] The component (A2) preferably contains, as a monomer group containing an epoxy group-containing monomer, a (meth)acrylic acid alkyl ester, an aromatic monomer, etc., and more preferably contains a (meth)acrylic acid alkyl ester as the resin skeleton (main component). Polymers of a monomer group containing an epoxy group-containing monomer and an alkyl (meth)acrylate ester; Polymers of a monomer group including epoxy group-containing monomers, (meth)acrylic acid alkyl esters and aromatic monomers; As the component (A2), an emulsion of such a polymer (also called an "epoxy group-containing acrylic resin emulsion") is preferable.

[0034] Examples of epoxy group-containing monomers include glycidyl (meth)acrylate, diglycidyl fumarate, 3,4-epoxycyclohexyl (meth)acrylate, 3,4-epoxyvinylcyclohexane, allyl glycidyl ether, ε-caprolactone-modified glycidyl (meth)acrylate, β-methylglycidyl (meth)acrylate, etc. These can be used alone or in combination of two or more. In the present invention, the content of the epoxy group-containing monomer is preferably 0.5 to 50% by weight (more preferably 1 to 30% by weight) in the total monomers constituting the component (A2). This allows the effects of the present invention to be fully exhibited.

[0035] The (meth)acrylic acid alkyl ester and aromatic monomer can be the main components of the resin skeleton. In the present invention, the acrylic acid alkyl ester and the methacrylic acid alkyl ester are collectively referred to as the (meth)acrylic acid alkyl ester. The monomer is a general term for a compound having a polymerizable unsaturated double bond.

[0036] Specific examples of (meth)acrylic acid alkyl esters include, for example, methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, isobutyl (meth)acrylate, n-amyl (meth)acrylate, isoamyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, octadecyl (meth)acrylate, cyclohexyl (meth)acrylate, etc. These can be used alone or in combination of two or more.

[0037] The aromatic monomer is a compound having an aromatic ring and a polymerizable unsaturated double bond, and specific examples thereof include styrene, 2-methylstyrene, vinyltoluene, t-butylstyrene, chlorostyrene, vinylanisole, vinylnaphthalene, divinylbenzene, phenyl(meth)acrylate, benzyl(meth)acrylate, etc. These can be used alone or in combination of two or more.

[0038] In the component (A2), other monomers copolymerizable with the above components can also be used within the range that does not impair the effects of the present invention. Examples of such monomers include Nitrile group-containing monomers such as (meth)acrylonitrile, vinylidene cyanide, and α-cyanoethyl (meth)acrylate; Amide group-containing monomers such as maleic acid amide, (meth)acrylamide, N-monoalkyl (meth)acrylamide, N,N-dialkyl (meth)acrylamide, 2-(dimethylamino)ethyl (methacrylate), N-[3-(dimethylamino)propyl] (meth)acrylamide, and vinylamide; Carbonyl group-containing monomers such as acrolein, diacetone (meth)acrylamide, vinyl methyl ketone, vinyl ethyl ketone, and vinyl butyl ketone;

[0039] Carboxyl group-containing monomers such as (meth)acrylic acid, crotonic acid, maleic acid, itaconic acid, fumaric acid, isocrotonic acid, and salicylic acid; Alkoxysilyl group-containing monomers, such as 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropylmethyldiethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, and vinyltriisopropoxysilane; Amino group-containing monomers such as aminomethyl acrylate, aminoethyl acrylate, aminopropyl (meth)acrylate, amino-n-butyl (meth)acrylate, butylvinylbenzylamine, vinylphenylamine, p-aminostyrene, N-methylaminoethyl (meth)acrylate, and Nt-butylaminoethyl (meth)acrylate; Hydroxyl group-containing monomers such as hydroxypropyl (meth)acrylate, ethylene glycol mono(meth)acrylate, and glycerol mono(meth)acrylate; vinylidene halide monomers such as vinylidene fluoride; Ethylene, propylene, isoprene, butadiene, vinyl ethers, vinyl ketones, silicone macromers; etc.

[0040] The (A2) component can be produced by emulsion polymerization of a monomer group obtained by appropriately mixing the above monomers. Any known method can be used as the polymerization method, and in addition to normal emulsion polymerization, soap-free emulsion polymerization, feed emulsion polymerization, seed emulsion polymerization, multi-stage emulsion polymerization, etc. can also be used. During polymerization, for example, emulsifiers, initiators, dispersants, polymerization inhibitors, polymerization retarders, buffers, chain transfer agents, pH adjusters, etc. can be used.

[0041] As the emulsifier, various surfactants that can be used in emulsion polymerization can be used, and these may be reactive types (reactive surfactants) having polymerizable unsaturated double bonds. As the emulsifier, for example, anionic surfactants, nonionic surfactants, etc. can be used alone or in combination. Specifically, for example, they can be appropriately selected from those described in the above component (A).

[0042] The glass transition temperature of the component (A2) can be adjusted by selecting the type of monomer, the mixing ratio, etc. The glass transition temperature may be appropriately set in consideration of the final required performance, etc., and is preferably about -50 to 80°C (more preferably about -40 to 60°C). The glass transition temperature can be calculated by the Fox formula.

[0043] The average particle size of the component (A2) is not particularly limited, but is preferably 300 nm or less (more preferably 20 to 250 nm, and even more preferably 30 to 200 nm). If the average particle size is within this range, advantageous effects can be obtained in terms of impregnation reinforcement, sealing properties, efflorescence resistance, whitening resistance, etc. The average particle size referred to here is a value measured by dynamic light scattering.

[0044] The component (A2) may be a mixture of two or more types having different resin compositions, glass transition temperatures, average particle sizes, etc.

[0045] In the present invention, the embodiment of the (A) component includes an embodiment of the (A1) component only, an embodiment of the (A2) component only, and an embodiment containing the (A1) component and the (A2) component. In particular, in the present invention, it is preferable to contain the (A1) component and the (A2) component in combination. This can ensure even better adhesion, water resistance, etc. to various substrates and coating films when the curing agent is used.

[0046] The mixing ratio (weight ratio of solid contents) of the above-mentioned (A1) component and (A2) component is preferably (A1):(A2)=5:95 to 80:20 (more preferably 10:90 to 60:40, further preferably 12:88 to 50:50, particularly preferably 15:85 to 45:55). In such a case, excellent adhesion to various substrates and coating films can be exhibited, and in particular, adhesion to existing coating films and top coating films can be enhanced. Furthermore, a coating film excellent in water resistance and coating film appearance can be formed.

[0047] The base material of the present invention may further contain a silane compound (N) (hereinafter, simply referred to as "component (N)") other than the amino group-containing silane compound (M). Such component (N) may be any compound having an alkoxysilyl group, and in the present invention, a glycidyl group-containing silane compound (N1) and / or an alkoxysilane compound (N2) are preferred.

[0048] As the glycidyl group-containing silane compound (N1) (hereinafter also simply referred to as "component (N1)"), a compound having a glycidyl group (epoxy group) and an alkoxysilyl group, or a compound having a glycidyl group and a cyclic siloxane, etc., can be used. These can be used alone or in combination of two or more.

[0049] Examples of the compound having a glycidyl group (epoxy group) and an alkoxysilyl group include a glycidyl group-containing silane coupling agent and a hydrolyzed oligomer thereof.

[0050] Specifically, examples of the glycidyl group-containing silane coupling agent include glycidoxymethyltrimethoxysilane, glycidoxymethyltriethoxysilane, β-glycidoxyethyltrimethoxysilane, β-glycidoxyethyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, γ-glycidoxypropyldimethylmethoxysilane, γ-glycidoxypropyl(ethyl)dimethoxysilane, β-3,4-epoxycyclohexylethyltrimethoxysilane, β-3,4-epoxycyclohexylethyltriethoxysilane, 8-glycidoxyoctyltrimethoxysilane, 8-glycidoxyoctylmethyldimethoxysilane, 8-glycidoxyoctylmethyldiethoxysilane, and the like. Preferably, the glycidyl group-containing silane coupling agent has an epoxy equivalent of x n1 The epoxy equivalent x is preferably 10 to 1000 (more preferably 50 to 500). n1 " is the number of grams of a silane compound containing 1 gram equivalent of an epoxy group [g / eq], and is the value obtained by dividing the weight average molecular weight of a glycidyl group-containing silane compound by the number of epoxy groups per molecule.

[0051] The hydrolysis oligomer of the glycidyl group-containing silane coupling agent has an alkoxysilyl group and a glycidyl group, and preferably has an alkoxy group content of 10 to 80 wt % (more preferably 20 to 75 wt %) and an epoxy equivalent x n1 The (N1) component may have two or more types of alkoxysilyl groups, or may have all or some of the alkoxysilyl groups in a silanol group state.

[0052] The compound having a glycidyl group and a cyclic siloxane is a silicone oligomer having only a glycidyl group as a reactive functional group, and preferably has an epoxy equivalent of x n1 is 100 to 500 (more preferably 150 to 400).

[0053] In particular, in the present invention, as the above-mentioned (N1) component, a glycidyl group-containing silane coupling agent is preferred, for example, one or more selected from glycidoxymethyltrimethoxysilane, glycidoxymethyltriethoxysilane, β-glycidoxyethyltrimethoxysilane, β-glycidoxyethyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, β-3,4-epoxycyclohexylethyltrimethoxysilane, and β-3,4-epoxycyclohexylethyltriethoxysilane are preferred, and an embodiment including one or more selected from β-3,4-epoxycyclohexylethyltrimethoxysilane and β-3,4-epoxycyclohexylethyltriethoxysilane is more preferred. When these are used, the adhesion development and adhesion to the substrate and coating film are further improved. Furthermore, the stability and usable time of the aqueous coating material can be increased.

[0054] In the case where the base agent of the present invention contains the above-mentioned components in addition to the above-mentioned components (N1), the mixing ratio of the above-mentioned (N1) component is preferably 0.5 to 20 parts by weight (more preferably 1 to 15 parts by weight) per 100 parts by weight of the solid content of the above-mentioned (A) component. In such a case, the adhesion to the substrate and the coating film is enhanced, and the adhesion is further improved. Furthermore, the stability and usable life of the aqueous coating material can be increased.

[0055] As the alkoxysilane compound (N2) (hereinafter also simply referred to as "(N2) component"), alkoxysilane and its hydrolysis condensate can be used. These can be used alone or in combination of two or more. By using such an (N2) component, the adhesion to the substrate can be further improved.

[0056] Examples of such component (N2) include tetrafunctional alkoxysilane compounds such as tetraethoxysilane, tetramethoxysilane, tetra-n-propoxysilane, tetraisopropoxysilane, tetraisobutoxysilane, tetra-sec-butoxysilane, tetra-t-butoxysilane, and tetraphenoxysilane;

[0057] trifunctional alkylalkoxysilane compounds such as methyltrimethoxysilane, methyltriethoxysilane, methyltrippropoxysilane, methyltributoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, ethyltrippropoxysilane, ethyltributoxysilane, propyltrimethoxysilane, propyltriethoxysilane, propyltrippropoxysilane, propyltributoxysilane, butyltrimethoxysilane, butyltriethoxysilane, butyltrippropoxysilane, butyltributoxysilane, hexyltrimethoxysilane, hexyltriethoxysilane, decyltrimethoxysilane, trifluoropropyltrimethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, and phenyltributoxysilane;

[0058] bifunctional alkylalkoxysilane compounds such as dimethyldimethoxysilane, dimethyldiethoxysilane, dimethyldibutoxysilane, diethyldimethoxysilane, diethyldiethoxysilane, diethyldibutoxysilane, diethyldipropoxysilane, dipropyldimethoxysilane, dipropyldiethoxysilane, dibutyldimethoxysilane, dibutyldiethoxysilane, diphenyldimethoxysilane, diphenyldiethoxysilane, diphenyldibutoxysilane, dimethoxymethylphenylsilane, and methylphenyldiethoxysilane; These may be used alone or in combination of two or more.

[0059] In the present invention, the (N2) component preferably contains a trifunctional alkylalkoxysilane compound and / or a bifunctional alkylalkoxysilane compound. Furthermore, it is preferable to contain one containing a phenyl group. Examples of such (N2) components include phenyltrimethoxysilane, dimethoxymethylphenylsilane, diphenyldimethoxysilane, phenyltriethoxysilane, diphenyldiethoxysilane, phenyltributoxysilane, and diphenyldibutoxysilane. When these are used, the curing property of the formed coating film is increased, and the adhesion and adhesion to the substrate and coating film are further improved. In particular, it can exhibit excellent effects in improving the adhesion and adhesion to the substrate having an existing coating film.

[0060] In the case where the base agent of the present invention contains the above-mentioned components in addition to the above-mentioned components (N2), the mixing ratio of the above-mentioned component (N2) is preferably 0.3 to 20 parts by weight (more preferably 0.5 to 18 parts by weight, and even more preferably 2 to 15 parts by weight) per 100 parts by weight of the solid content of the above-mentioned component (A). In such a case, the above-mentioned effects can be fully exhibited.

[0061] In the aqueous coating material of the present invention, the base agent and the curing agent are preferably mixed so that the base agent:curing agent (solid weight ratio) is 100:5-100 (more preferably 100:8-80, and even more preferably 100:10-50). In such a case, the adhesion and adhesion of the aqueous coating material to the substrate and coating film are improved. Furthermore, the stability and usable life of the aqueous coating material can be increased.

[0062] When the mixing ratio of the base agent to the curing agent is the above ratio, the amount of the (B) component can be set to preferably 1 to 50 parts by weight (more preferably 1.2 to 40 parts by weight, and even more preferably 1.5 to 30 parts by weight) in terms of solid content per 100 parts by weight of the (A) component solid content. Furthermore, the amount of the (M) component can be set to preferably 3 to 85 parts by weight (more preferably 4 to 70 parts by weight, and even more preferably 5 to 50 parts by weight) per 100 parts by weight of the solid content of the (A) component.

[0063] In addition, when the base agent contains the component (A1) as the component (A) in the base agent, the mixing ratio of the base agent and the curing agent is determined based on the epoxy equivalent of the component (A1) in the base agent ([X A1 ]; solid content equivalent) and the active hydrogen equivalent of component (B) in the curing agent ([Y B ] (solid content equivalent) ratio [X A1 / Y B ] can be set to be preferably 0.5 to 5 (more preferably 0.6 to 4, further preferably 0.7 to 3, and particularly preferably 0.8 to 2.5).

[0064] Furthermore, the epoxy equivalent of the (A1) component in the base resin ([X A1 ]: solid content equivalent) and the active hydrogen equivalent of component (B) in the hardener ([Y B ]; solid content equivalent) and the active hydrogen equivalent of component (M) ([Y M ] (solid content equivalent) ratio [X A1 / (Y B +Y M)] can be set to be preferably 0.1 to 3 (more preferably 0.12 to 2, and even more preferably 0.15 to 1). In such a case, the adhesion and adhesion of the aqueous coating material to the substrate and coating film are improved. Furthermore, the stability and usable life of the aqueous coating material can be increased.

[0065] In addition, the above X A1 , the above Y B is determined from the blending parts at the time of mixing, and specifically, the above [X A1 ] is the amount of component (A1) contained in the base resin (parts by weight of solid content) multiplied by the epoxy equivalent of component (A1) x a In addition, the above [Y B is the amount of component (B) contained in the curing agent (parts by weight of solid content) expressed as the active hydrogen equivalent y b Furthermore, the value is the value divided by the above [Y M ] is the amount of component (M) contained in the curing agent (parts by weight of solid content) expressed as the active hydrogen equivalent y m This is the value divided by .

[0066] In addition to the above-mentioned components, the aqueous coating material of the present invention may contain color pigments, extender pigments, rust-preventive pigments, pH regulators, plasticizers, preservatives, antifungal agents, antialgae agents, defoamers, leveling agents, dispersants, antisettling agents, antisagging agents, thickeners (thixotropic regulators), film-forming assistants, matting agents, crosslinking agents, catalysts, curing accelerators, adhesion agents, ultraviolet absorbers, light stabilizers, etc., as necessary, within the range in which the effects of the present invention are not impaired. The pH of the aqueous coating material of the present invention is preferably 3 to 12 (more preferably 4 to 11). In the present invention, it is preferable that the pH of the aqueous coating material satisfies the above.

[0067] In the aqueous coating material of the present invention, it is preferable to mix a catalyst (P) (hereinafter, simply referred to as "component (P)") into the main agent. Component (P) promotes, for example, the reaction between the glycidyl group (epoxy group) and the amino group in the aqueous coating material, or the hydrolysis and condensation of the alkoxysilyl group, and can further improve adhesion to substrates, particularly to substrates having an existing coating film.

[0068] As the component (P), one or more of the compounds described above as the component (O) can be used. Among these, organotin compounds such as tin octoate, dibutyltin dilaurate, and dibutyltin diacetate are particularly suitable for use as the component (P).

[0069] The mixing amount of the above component (P) is preferably 0.01 to 10 parts by weight (more preferably 0.02 to 8 parts by weight) per 100 parts by weight of the component (A) (solid content). Within such a range, the effects of the present invention can be enhanced.

[0070] The aqueous coating material of the present invention can be various, such as colored or uncolored, or opaque or transparent. In the present invention, it can be preferably used as a clear aqueous coating material having transparency. The aqueous coating material of the present invention preferably has a solid content of 5 to 60% by weight (more preferably 6 to 50% by weight, and even more preferably 7 to 45% by weight). The solid content can be adjusted by mixing the above-mentioned aqueous medium. When it is within such a range, it is possible to achieve excellent coating workability and further improve adhesion to various substrates and coating films.

[0071] The aqueous coating material of the present invention is preferably used as an undercoat material for painting interior and exterior wall surfaces and floor surfaces. For example, it is preferably used as an undercoat material applied to substrates such as mortar, concrete, ceramic siding boards, ceramic siding boards, metal siding boards, extrusion molding boards, slate boards, calcium silicate boards, ALC boards, metals, wood, glass, ceramics, synthetic resins, etc., or substrates such as a wide variety of existing coating films formed on such substrates (substrate surfaces). In addition, the shape of such substrates (substrates and existing coating films) can be smooth (flat), or have various uneven patterns (for example, stone-like, brick / tile-like, wood-grain-like, border-like, plaster-like, spray-applied, etc.). Furthermore, it can also be applied to substrates including sealing joints.

[0072] In particular, the aqueous coating material of the present invention is suitable as an undercoat material for repairing a substrate, and can be suitably used as an undercoat material, for example, when repairing a siding board having an existing coating film.

[0073] The existing coating film is a coating film that has already been applied on the substrate by on-site painting or factory painting (line painting), and examples thereof include at least one coating film selected from organic coating films, inorganic coating films, and organic-inorganic composite coating films. Examples of the existing coating film include colored coating films (enamel coating films, printed coating films, etc.), clear coating films, and laminated coating films thereof, and are coating films formed by applying and curing various coating materials to the substrate. Such coating materials may be any of room temperature drying type, room temperature curing type, bake curing type, ultraviolet (UV) curing type, electron beam curing type, etc.

[0074] Examples of binders for such coating materials include organic binders such as acrylic resin, polyurethane resin, epoxy resin, fluororesin, alkyd resin, and polyester resin; inorganic binders such as silicone resin, alkoxysilane, colloidal silica, and silicate; and organic-inorganic composite binders such as acrylic silicone resin.

[0075] The present invention is particularly suitable when the existing coating film is one or more selected from inorganic coating films (coating films containing the above-mentioned inorganic binder), organic-inorganic composite coating films (coating films containing the above-mentioned organic-inorganic composite binder), fluororesin coating films (coating films containing the above-mentioned fluororesin), etc., and can further be suitably applied to clear coating films thereof. Such existing coating films may contain photocatalytic titanium oxide, etc.

[0076] Specific examples of coating materials include weather-resistant topcoat paints for architecture (JIS K5658:2010), weather-resistant paints for steel structures (JIS K5659:2008), glossy synthetic resin emulsion paints (JIS K5660:2008), fire-retardant paints for architecture (JIS K5661:1970), synthetic resin emulsion paints (JIS K5663:2008), road marking paints (JIS K5665:2011), multicolored pattern paints (JIS K5667:2003), synthetic resin emulsion pattern paints (JIS K5668:2010), acrylic resin-based non-aqueous dispersion paints (JIS K5670:2008), lead- and chromium-free rust-preventive paints (JIS K5674:2008), high solar reflectance paints for roofs (JIS K5675:2011), and floor paints for buildings (JIS K5970:2008), architectural coating waterproofing materials (JIS A6021:2011), architectural finishing coating materials (JIS A6909:2014), etc.

[0077] In the application of the aqueous coating material of the present invention, various methods can be used, such as brush application, roller application, spray application, etc. Furthermore, when applying in a factory, in addition to the above, a roll coater, a flow coater, etc. can also be used for application.

[0078] The amount of the aqueous coating material applied is preferably 0.05 to 0.5 kg / m 2 (More preferably 0.07 to 0.3 kg / m 2 ) The number of coats of the aqueous coating material may be appropriately determined depending on the condition of the substrate, but is preferably 1 to 2 coats. The drying time of the aqueous coating material is preferably 1 hour or more and 1 week or less. The drying temperature is preferably -10°C or more and 50°C or less, more preferably -5°C or more and 40°C or less. The aqueous coating material of the present invention is preferably a room temperature curing type.

[0079] The coating film formed by the aqueous coating material of the present invention has excellent adhesion to a wide variety of topcoat materials. The topcoat material is not particularly limited as long as it is generally used for painting buildings, and the binder may be, for example, an organic binder such as acrylic resin, polyurethane resin, epoxy resin, fluororesin, alkyd resin, or polyester resin, or an inorganic binder such as silicon resin, alkoxysilane, colloidal silica, or silicate, or an organic-inorganic composite binder such as acrylic silicon resin. In particular, in the present invention, the adhesiveness with the topcoat material containing one or more selected from the organic binder and the organic-inorganic composite binder can be fully exhibited.

[0080] Specific topcoat materials include, for example, weather-resistant topcoat paint for architecture (JIS K5658:2010), weather-resistant paint for steel structures (JIS K5659:2008), glossy synthetic resin emulsion paint (JIS K5660:2008), fireproof paint for architecture (JIS K5661:1970), synthetic resin emulsion paint (JIS K5663:2008), paint for road markings (JIS K5665:2011), multicolored pattern paint (JIS K5667:2003), synthetic resin emulsion pattern paint (JIS K5668:2010), acrylic resin-based non-aqueous dispersion paint (JIS K5670:2008), lead- and chromium-free rust-preventive paint (JIS K5674:2008), high solar reflectance paint for roofs (JIS K5675:2011), floor paint for buildings (JIS K5970:2008), architectural coating waterproofing materials (JIS A6021:2011), architectural finishing coating materials (JIS A6909:2014), etc.

[0081] The method of applying the topcoat material is not particularly limited and can be applied by a known method, for example, brush coating, trowel coating, spray coating, roller coating, roll coater, flow coater, etc. In other words, each topcoat material can be applied based on the normal process with the optimal coating specifications for each topcoat material. EXAMPLES

[0082] The following examples and comparative examples will clarify the features of the present invention.

[0083] <Preparation of hardeners 1 to 11> The amino group-containing resin (B) and the amino group-containing silane compound (M) were mixed in the mixing ratios shown in Table 1 to prepare curing agents 1 to 11. The following raw materials were used:

[0084] (B) Amino group-containing resin (B-1) Polyamine resin [water-soluble type, containing modified aliphatic polyamine and meta-xylylenediamine, solid content 80% by weight (solvent: water, water content 20% by weight), active hydrogen equivalent y b :147] (B-2) Polyamine resin [water-dispersible, containing modified aliphatic polyamine and meta-xylenediamine, solid content 60% by weight (solvent: water, water content 40% by weight), active hydrogen equivalent y b :160] (B-3) Polyamine resin [water-soluble, styrene addition reaction product of meta-xylenediamine, solid content 100% by weight, active hydrogen equivalent y b :103]

[0085] (M) Amino group-containing silane compound [N-β(aminoethyl)-γ-aminopropylmethyldimethoxysilane, active hydrogen equivalent y m :103]

[0086] [Table 1]

[0087] <Production of main components 1 to 20> The water-based epoxy resin (A), (N1) glycidyl group-containing silane compound, (N2) alkoxysilane compound, (P) catalyst, additives, and water were mixed in the mixing ratios shown in Tables 2 and 3 to prepare main components 1 to 20. The following raw materials were used:

[0088] (A) Water-based epoxy resin (A1) Water-based epoxy resin [bisphenol A type epoxy resin (solid type) water dispersion, solid content 46% by weight, epoxy equivalent x a 508] (A2-1) Epoxy group-containing acrylic resin emulsion [styrene / 2-ethylhexyl acrylate / glycidyl methacrylate copolymer, solid content: 33% by weight, glycidyl methacrylate content: 9% by weight, average particle size: 70 nm] (A2-2) Epoxy group-containing acrylic resin emulsion [styrene / 2-ethylhexyl acrylate / glycidyl methacrylate copolymer, solid content: 33% by weight, glycidyl methacrylate content: 9% by weight, average particle size: 150 nm]

[0089] (N1) Glycidyl group-containing silane compound [β-3,4-epoxycyclohexylethyltrimethoxysilane, epoxy equivalent x n1 :246] (N2-1) Alkylalkoxysilane compound [Phenyltrimethoxysilane] (N2-2) Alkylalkoxysilane compound [Dimethoxymethylphenylsilane] (P) Catalyst [organotin compound dispersion, solid content: 10% by weight] Additives: Antifoaming agents, thickeners, film-forming agents, etc.

[0090] [Table 2]

[0091] Example 1 The following evaluations were carried out using an aqueous coating material (clear type aqueous coating material) prepared by mixing the base agent 1 (337.4 parts by weight) shown in Table 2 and the hardener 1 (100 parts by weight) shown in Table 1. <Pot life> After mixing the base resin and the hardener, the time until the fluidity was lost was measured. The evaluation criteria are as follows. The results are shown in Table 3. A: 240 minutes or more B: 120 minutes or more and less than 240 minutes C: 30 minutes or more but less than 120 minutes D: Less than 30 minutes

[0092] <Adhesion Evaluation 1> Test specimen [I] On the siding board with an inorganic clear coating formed as the existing coating, a water-based coating material (clear type water-based coating material) obtained by mixing the base agent and hardener in the combination shown in Table 3 was applied at an amount of 0.1 kg / m. 2 The mixture was applied immediately after mixing so that the composition satisfies the above requirements, and then dried for 4 hours under standard conditions (air temperature 23°C, relative humidity 50%). Then, a water-based topcoat material (acrylic silicone resin emulsion paint) was applied at a rate of 0.1 kg / m. 2 The paint was applied so that the above formula was obtained, and then dried for one day in a 50°C environment to prepare test specimen [I].

[0093] The adhesion of the prepared specimen [I] was evaluated by the cross-cut tape method according to JIS K 5600-5-6. The results are shown in Table 3. The evaluation criteria are as follows: AA: Defect area is less than 5% A: The area of ​​the defect is 5% or more but less than 10% AB: Defect area is 10% or more but less than 25% B: Defect area is 25% or more but less than 40% C: Defective area is 40% or more but less than 55% D: Defective area is 55% or more

[0094] <Adhesion evaluation 2> Test specimen [II] Except for using hardeners 1 to 11 stored at 50°C for 7 days as hardeners, the water-based coating material and water-based topcoat material were applied and dried in the same manner as for test specimen [I] to prepare test specimen [II]. The adhesion of the prepared specimen [II] was evaluated in the same manner as for the above specimen [I]. The results are shown in Table 3.

[0095] (Examples 2 to 8, Comparative Examples 1 to 3) Water-based coating materials (clear water-based coating materials) were prepared by mixing the main agent (each total part by weight) shown in Table 2 with the curing agents 2 to 11 (each total part by weight) shown in Table 1, and pot life and adhesion evaluations 1 and 2 were carried out in the same manner as described above. The combinations of the main agent and the curing agent are shown in Table 3. For example, in Example 2, the main agent 1 (337.4 parts by weight) and the curing agent 2 (75 parts by weight) were mixed.

[0096] Examples 1 to 8 had good adhesion to the substrate and topcoat material. Moreover, Examples 2 to 4 and Example 8 had good adhesion even after storage of the curing agent. On the other hand, in Comparative Examples 1 to 3, the adhesion to the substrate was insufficient.

[0097] <Adhesion Evaluation 3> Next, for Examples 3 and 8, the following specimens [III], [IV], [V], and [VI] were prepared and the adhesion was evaluated in the same manner as for the above specimen [I]. The results are shown in Table 3.

[0098] Test specimens [III]~[V] A water-based coating material was applied at a rate of 0.1 kg / m on a siding board that had an inorganic clear coating as the existing coating. 2 The mixture was applied immediately after mixing so that the composition satisfies the above requirements, and then dried for 4 hours under standard conditions (air temperature 23°C, relative humidity 50%). Then, a water-based topcoat material (acrylic silicone resin emulsion paint) was applied at a rate of 0.1 kg / m. 2 The coating was applied as shown in the figure, and specimens [III], [IV], and [V] were prepared by drying for one day, four days, and seven days under standard conditions, respectively.

[0099] Test specimen [VI] A water-based coating material was applied at a rate of 0.1 kg / m on a siding board that had an inorganic clear coating as the existing coating. 2 The mixture was applied immediately after mixing, dried for 7 days in a 50°C environment, and then a water-based topcoat (acrylic silicone resin emulsion paint) was applied at a rate of 0.1 kg / m. 2 The paint was applied as shown in the figure and dried for one day under standard conditions to prepare test specimen [VI].

[0100] In Examples 3 and 8, good adhesion was observed.

[0101] [Table 3]

[0102] (Examples 9 to 27) Using aqueous coating materials (clear aqueous coating materials) prepared by mixing each of the main agents (total parts by weight) shown in Table 2 with hardener 3 (50 parts by weight), pot life and adhesion evaluations 1 to 3 were carried out in the same manner as above. The combinations of main agents and hardeners and the results are shown in Table 4. (Examples 28 to 46) Using aqueous coating materials (clear aqueous coating materials) prepared by mixing each of the main agents (total parts by weight) shown in Table 2 with hardener 8 (25 parts by weight), pot life and adhesion evaluations 1 to 3 were carried out in the same manner as above. The combinations of main agents and hardeners and the results are shown in Table 5.

[0103] In Examples 9 to 46, the adhesiveness was good with the substrate and the topcoat material. In particular, in Examples 15, 17, 19 to 26, 34, 36, and 38 to 45, all were rated A or higher and had sufficient adhesiveness. Therefore, a water resistance evaluation was carried out on these.

[0104] <Water resistance evaluation> The existing coating was prepared by mixing the base agent and hardener on a black acrylic plate (150mm x 200mm x 3mm) and applying the water-based coating material to a thickness of 0.15mm immediately after mixing, and then drying for one day under standard conditions (air temperature 23℃, relative humidity 50%) to prepare test specimens [VII]. Each test specimen was immersed in water at 20℃ for 24 hours, then removed and dried (23℃, 3 hours), and the condition of the coating was visually observed and evaluated for swelling, peeling, whitening, etc. The evaluation criteria were a six-level scale (AA>A>AB>B>C>D), with "AA" being almost no abnormality and "D" being abnormality. The results are shown in Tables 4 and 5.

[0105]

Table 4

[0106]

Table 5

Claims

1. A two-component water-based coating material comprising a curing agent for water-based epoxy resin and a base material containing water-based epoxy resin, The curing agent includes an amino group-containing resin and an amino group-containing silane compound, The amino group-containing resin is a polyamine resin (excluding amino group-containing silane compounds), the amino group-containing silane compound is a compound having an amino group and an alkoxysilyl group, the mixing ratio (solids weight ratio) of the amino group-containing resin to the amino group-containing silane compound is 5:95 to 90:10, The above-mentioned base material is a two-liquid type water-based coating material characterized in that it contains, as water-based epoxy resins, an epoxy resin emulsion and an epoxy group-containing acrylic resin emulsion.

2. A two-component water-based coating material as described in claim 1, characterized in that the mixing ratio (solid weight ratio) of the epoxy resin emulsion to the epoxy group-containing acrylic resin emulsion is 5:95 to 80:20.

Citation Information

Patent Citations

  • Aqueous coating material

    JP2018065998A

  • Two liquid reaction-curable aqueous coating composition for primer, and multilayer film forming method using the same and coated body