Corrosion proof system, corrosion proof monitoring system and construction method thereof
A corrosion protection system using a water-containing fluid with fine cellulose fibers and a conductive base metal addresses localized corrosion in complex steel structures, providing effective protection and monitoring without disassembly, thus extending the lifespan and reducing maintenance costs.
Patent Information
- Application Number
- JP2023043948
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing corrosion protection methods for complex-shaped steel structures, such as bridges and plant equipment, are ineffective in preventing localized and rapid corrosion in areas like splicing plates due to differential ventilation, requiring large-scale replacement work and high costs, and existing sacrificial anode methods are difficult to implement without disassembling the structure.
A corrosion protection system using a water-containing fluid with fine cellulose fibers and a base metal with lower natural potential than steel, joined conductively, to supply base metal ions and electrons to the steel surface, creating a sacrificial corrosion protection effect without disassembly, and an RFID tag for monitoring wear.
The system effectively prevents corrosion in complex-shaped steel structures by maintaining a stable potential difference and can be monitored for wear without disassembly, extending the lifespan of structures and reducing maintenance costs.
Smart Images

Figure 2024133923000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a corrosion prevention system, a corrosion prevention monitoring system, and a method for constructing the same. [Background technology]
[0002] Many steel structures, including bridges, were constructed during the period of high economic growth in the 1970s, and are approaching the milestone of their 50-year lifespan. In particular, of the 700,000 bridges in Japan, 43% will be over 50 years old by 2023, and 67% by 2033. Reconstructing all of these bridges at the end of their lifespan is virtually impossible in terms of the impact on lifelines, particularly transportation, and the budget it would require.
[0003] In response to this, the Ministry of Land, Infrastructure, Transport and Tourism is recommending asset management centered on preventive maintenance based on regular inspections and the results, rather than the conventional method of post-mortem maintenance, in an effort to avoid the chaos that would accompany rebuilding. Asset management centered on preventive maintenance is also recommended for structures prone to corrosion, such as plant equipment, which is often installed in coastal areas. In particular, for steel structures, the main preventive maintenance measure is to prevent deterioration due to corrosion, and painting is the main method used for this.
[0004] For example, Patent Document 1 discloses a coating method characterized by coating a surface to be coated with a zinc-rich coating material (I) containing an epoxy resin binder and zinc dust as main components, and then coating a coating composition (III) containing an acrylic resin (A), an epoxy resin (B) having at least two epoxy groups in one molecule, and an amine curing agent (C) which may contain aminosilane.
[0005] Patent Document 2 discloses a corrosion prevention method for protecting the surface of a steel structure from corrosion by covering it with titanium foil, the corrosion prevention method comprising a coating step of applying paint to the surface of the steel material constituting the steel structure to form a paint layer, a coating step of coating the surface of the paint layer with the titanium foil except for the areas above the weld bead portions of the steel material, and an application step of applying titanium tape to the surface of the paint layer that is not covered with the titanium foil.
[0006] Furthermore, corrosion protection for the complex shapes of steel structures includes crevice protection. It is difficult to fundamentally solve the problem of crevice protection using anticorrosive paint. Sacrificial corrosion protection technology can be considered as a method to fundamentally solve the problem of crevice corrosion. Among sacrificial corrosion protection technologies, the sacrificial anode method can only function in seawater or soil containing moisture, so in recent years, sacrificial corrosion protection technology in the atmosphere has been devised and used as a countermeasure.
[0007] For example, Patent Document 3 discloses a corrosion prevention method in which, for a member to be protected whose surface has been oxidized to form a corrosion layer, a water-absorbent sheet made of an insulator and absorbing external moisture, and a sacrificial anode material made of a material that is less noble than the member to be protected and having a plurality of through holes formed therein that connect the outside to the water-absorbent sheet are placed between the corrosion layer and the sacrificial anode material, and a pair of terminals respectively placed on the member to be protected from corrosion and the sacrificial anode material are electrically connected, external moisture is supplied to the water-absorbent sheet via the plurality of through holes, the moisture absorbed by the water-absorbent sheet forms a corrosion circuit, and electrons that conduct the corrosion circuit from the sacrificial anode material to the member to be protected reduce the corrosion layer and convert it into a conversion layer that is stable against corrosion.
[0008] Patent Document 4 discloses an electrochemical protection structure for a reinforced concrete structure, which has a water-retaining layer provided on the concrete surface of the reinforced concrete structure and a galvanic anode provided in contact with the water-retaining layer, the galvanic anode and the reinforcing bars of the reinforced concrete structure being electrically connected so that an anticorrosive current flows from the galvanic anode to the reinforcing bars via the water-retaining layer, and the water-retaining layer is formed by retaining an electrolyte aqueous solution containing a deliquescent salt in a water-absorbent composed of hydrophilic fibers.
[0009] Patent Document 5 discloses a corrosion prevention structure for steel materials constituting a steel structure, a conductive adhesive applied to the surface of the steel material, a magnesium plate fixedly attached to the steel material with the conductive adhesive interposed therebetween, a plain woven fabric of polyester fibers having a gauze-like mesh structure covering the magnesium plate and arranged over an area wider than the surface area of the magnesium plate, and a bitumen-based cover further layered on the fabric, in which the flexible fabric and cover sandwiching the conductive adhesive and the magnesium plate and arranged on the surface are fixed to the steel material, the fabric carries magnesium ions generated from the magnesium plate, and the carried fabric is overlapped on the surface of the steel material, and the corrosion prevention structure is characterized in that the surface of the steel material is passivated and protected from corrosion over an area wider than the surface area of the magnesium plate and over the overlapped area.
[0010] Patent Document 6 describes a corrosion protection structure for a steel structure, the corrosion protection structure for the steel material comprising a steel material constituting the steel structure, a conductive adhesive applied to at least a part of the surface of the steel material, a single or multiple magnesium plates fixedly attached to the steel material with the conductive adhesive sandwiched therebetween, a flexible polyester fibrous substrate, and a bitumen-based cover. In the case of the single magnesium plate, the fibrous substrate covers the magnesium plate and is disposed on the surface over an area wider than the surface area of the magnesium plate, and in the case of the multiple magnesium plates, the fibrous substrate connects between multiple magnesium plates, covers the surface, and is disposed on the surface over an area wider than the surface area of the magnesium plates and the entire surface area of the connected portions, the cover is further disposed on the fibrous substrate in the case of the single magnesium plate or the fibrous substrate in the case of the multiple magnesium plates, and the single magnesium plate or the multiple magnesium plates is fixedly attached to the steel material with the conductive adhesive sandwiched therebetween. a fibrous substrate in the single case or a fibrous substrate in the multiple cases provided on the surface with a magnesium plate and the conductive adhesive sandwiched therebetween, and the cover is fixed to the steel material, the fibrous substrate in the single case or the fibrous substrate in the multiple cases carrying and supplying magnesium ions generated from the magnesium plate and electrons associated with ionization, and the fibrous substrate carrying and supplying is superimposed on at least a portion of the surface of the steel material, and the natural potential of the steel material is maintained at a corrosion prevention potential over the superimposed surface area by the fibrous substrate in the single case or the fibrous substrate in the multiple cases, thereby protecting at least one of the following areas of the steel structure that deform due to temperature or external force, areas of gaps where the steel structure is joined, and areas of the surface that have a unique shape where the magnesium plate cannot be placed. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] JP 2005-074272 A [Patent Document 2] JP 2011-206754 A [Patent Document 3] JP 2016-040403 A [Patent Document 4] JP 2016-169407 A [Patent Document 5] Patent Publication No. 2021-055147 [Patent Document 6] Patent Publication No. 2021-055148 Summary of the Invention [Problem to be solved by the invention]
[0012] Corrosion that occurs on ordinary steel surfaces exposed to the atmosphere occurs all over the surface, not in a fixed area. Therefore, because the corrosion rate is slow and easy to see, it is possible to maintain the strength of the steel for a long period of time by making an appropriate painting plan, completely scraping off the rust, and repainting. For example, in areas where rust can be easily removed from flat surfaces such as main girders, it is customary to remove the rust and paint them with inexpensive anti-corrosion paint.
[0013] On the other hand, in areas where rust is difficult to remove due to complex shapes such as the corners and supports of steel materials in bridges and plant facilities, even if anticorrosive paint is applied as a corrosion prevention measure, some of the remaining rust will cause corrosion to progress. This type of rust is unstable rust consisting of metal oxides containing trivalent Fe ions such as hematite or their hydrates.
[0014] For example, splice plates are an example of a part where rust is difficult to remove. Splice plates are plates made of steel that are used on-site to join the joints of steel materials that have been divided for transportation, etc. in bridges, etc., and are fastened with high-strength bolts, etc. Although the splice plates are firmly fastened with high-strength bolts, etc., tiny gaps are formed between the steel materials due to strain, etc. When moisture such as rainwater or salt water penetrates into the gaps, a difference in the amount of dissolved oxygen occurs between the inside and outside moisture, causing a concentration cell effect due to oxygen, and causing severe corrosion in those areas (this corrosion is called differential aeration corrosion). The rust that occurs due to corrosion collects and accumulates at the entrance, accelerating the deformation of the splice plate and inviting strength risks such as deformation of the bolts.
[0015] It is impossible to remove the rust from the gaps in the splice plate unless the splice plate itself is removed. For this reason, considering the impact of the bridge being closed to traffic due to the removal of the splice plate and the creation of a replacement splice part (bypass construction method), it is not easy to remove the rust from the splice plate, and the corrosion tends to be left unattended. Corrosion that is left unattended progresses at a faster rate than general general corrosion. This type of corrosion also causes further deformation of the splice plate, which makes it necessary to replace the splice plate, and ultimately requires large-scale replacement work and the associated response and costs such as road closures. As mentioned above, it is now impossible to replace bridges in 50 years, so in order to aim for longer-term use of bridges, a new method of dealing with this type of partial and rapidly progressing corrosion factor is required.
[0016] However, for example, in Patent Document 1, when repairing gaps in existing facilities using anticorrosive paint, it was necessary to dismantle the constituent facilities. In addition, the anticorrosive paint had a problem that the thickness of the coating film at the edge of the steel material became thin, and corrosion spread from the part where the coating film became thin.
[0017] In Patent Document 2, in order to check the corrosion protection status, it was necessary to peel off the titanium foil because it was not possible to check through it. In addition, since titanium is a noble metal compared to steel, there was a fundamental problem that corrosion of the steel material was likely to occur at the joint between the titanium foil and the steel material. In addition, there was also a problem that in order to prevent such corrosion, it was necessary to apply a thick anticorrosive paint.
[0018] In Patent Documents 3 to 6, the water absorbent sheet and the metal that is less noble than the steel must be shaped to fit the shape of the corrosion-protected material (object of corrosion protection) such as steel, which makes it difficult to protect structures and gaps with complex shapes. Also, in Patent Documents 3 to 6, the corrosion-protecting material must be in close contact with the surface of the steel to be protected via a medium such as a conductive adhesive or paper, and in order to protect against aerial differential corrosion by sacrificial protection in the atmosphere, it is necessary to disassemble the object to be protected, for example, a splice plate, and insert the corrosion-protecting material into the gap.
[0019] Therefore, an object of the present invention is to provide a system that can easily make a steel structure having a corrosion prevention effect, even if the steel structure has a complex shape and is a corrosion-resistant material. [Means for solving the problem]
[0020] The operating principle of the sacrificial anode method is that the electrophoresis of ions contained in seawater or electrolyte allows the transfer of electrons, and by passing an electric current between the object to be protected such as steel and the protective material, the potential of the metal surface is changed (called polarization), and the surface potential of the steel is changed from the potential at which corrosion begins (called the corrosion potential or natural potential) to a potential range where corrosion does not occur (called the corrosion protection potential), thereby realizing corrosion protection. For this reason, ions can easily flow in seawater or in soil that contains moisture, making corrosion protection possible.
[0021] On the other hand, in the principle of atmospheric sacrificial protection in the atmosphere where it is difficult to retain an electrolyte, the operating range is limited to the area where the object to be protected and the protected material are in close proximity, ensuring the range of ion movement and achieving corrosion protection. However, if the difference between the potential (equilibrium potential) specific to the protected material and the potential specific to the steel material is large enough, it is possible to achieve corrosion protection even on distant steel materials as long as an electrolyte is secured between the steel material and the protected material.
[0022] In the case of crevice corrosion, corrosion occurs precisely because of the water retention effect of the gap, so by taking measures to ensure that there is electrolyte from the protection material to the entrance of the gap, it is possible to ensure that water is retained from the protection material to the target of corrosion protection in the gap.
[0023] As a result of extensive research into the corrosion protection of steel materials with complex shapes, the inventors discovered that in a corrosion protection system for steel, steel is joined to a base metal having a lower natural potential than the steel in a manner that allows them to be electrically conductive, and an aqueous fluid containing fine cellulose fibers is brought into contact with the steel surface and the base metal surface.The aqueous fluid easily enters the gaps in the steel material with complex shapes as a carrier for supplying base metal ions generated by ionization of the base metal between the base metal and the steel material to the steel surface, and further, electrons generated by ionization of the base metal are supplied from the base metal to the joined steel material in an electrically conductive manner, and as a result, the corrosion protection system for steel materials with complex shapes thus constructed exhibits good corrosion protection effects, thereby completing the present invention.
[0024] That is, the gist of the present invention is as follows. (1) A corrosion protection system for steel comprising a steel material, a base metal having a lower natural potential than the steel material, fine cellulose fibers having an average fiber width of 1 nm or more and 1,000 nm or less, and a hydrous fluid containing an electrolyte, in which the steel material and the base metal are joined in an electrically conductive manner, the hydrous fluid is in contact with the steel material surface and the base metal surface, and supplies base metal ions generated from the base metal surface to the steel material surface. (2) A corrosion protection system for steel as described in (1), in which the content of fine cellulose fibers in the aqueous fluid is 1 mass% or more relative to the total mass of the aqueous fluid. (3) A corrosion protection system for steel as described in (1) or (2), in which the steel surface is a steel surface in a gap between steel members. (4) A corrosion protection system for steel according to any one of (1) to (3), in which the fine cellulose fibers contain anion-modified fine cellulose fibers in an amount of 0.1 mass% to 50 mass% based on the total mass of solids in the aqueous fluid, the anion-modified fine cellulose fibers have an average fiber width of 1 nm to 1000 nm, and the amount of anion-modified groups introduced into the anion-modified fine cellulose fibers is 0.3 mmol / g to 4.0 mmol / g. (5) A corrosion protection system for steel materials according to any one of (1) to (4), in which the water-containing fluid contains one or more electrolytes in an amount of 1.0 mass% or more relative to the total mass of solids in the water-containing fluid. (6) A corrosion protection system for steel as described in (5) above, in which at least one of the electrolytes functions as a reducing agent. (7) The corrosion protection system for steel materials according to (4), wherein the anion-modified fine cellulose fibers are sulfate-esterified fine cellulose fibers having the substituent group according to formula (1). [ka] (In the formula, n is an integer of 1 to 3, and M n+ is an n-valent cation, and the wavy lines are the sites of attachment to other atoms.) (8) A corrosion protection system for steel materials according to any one of (1) to (7), in which the water-containing fluid further contains fibers having a fiber diameter of 5 μm or more and 300 μm or less. (9) A corrosion protection system for steel material described in any one of (1) to (8), further comprising an exterior material applied to the surface of the steel material so as to cover the base metal and the water-containing fluid. (10) A corrosion prevention monitoring system comprising a corrosion prevention system for steel material described in any one of (1) to (9) and an RFID tag having a tamper function, wherein the RFID tag is electrically connected to both the steel material and the base metal in the corrosion prevention system for steel material, and the depletion and peeling of the base metal are read by an RFID reader. (11) The corrosion protection system or corrosion protection monitoring system for a steel material according to any one of (1) to (10), wherein the water-containing fluid is in a dry state. (12) A water-containing fluid for use in the corrosion prevention system or corrosion prevention monitoring system for a steel material according to any one of (1) to (10), comprising water, fine cellulose fibers, and an electrolyte. (13) A dry body for use in the corrosion prevention system or corrosion prevention monitoring system for steel materials according to (11), comprising fine cellulose fibers and an electrolyte. (14) A method for constructing a corrosion protection system or corrosion protection monitoring system for a steel material described in any one of (1) to (11), comprising joining a rusted steel material and a base metal having a lower natural potential than the steel material in an electrically conductive manner, and arranging an aqueous fluid so as to be in contact with the steel material surface and the base metal surface and so as to supply base metal ions generated from the base metal surface to the steel material surface, wherein the rust is not removed. Effect of the Invention
[0025] The present invention provides a system that can easily make a steel structure that is corrosion-resistant even if the steel structure has a complex shape and is a corrosion-resistant material. [Brief description of the drawings]
[0026] [Figure 1] FIG. 1 is a diagram showing a schematic example of an arrangement in which fibers 6 are sandwiched between water-containing fluid 3 on the surface of a steel material 1 or a base metal 2. [Diagram 2] FIG. 1 is a diagram illustrating an embodiment of the present invention. [Diagram 3] FIG. 1 is a diagram showing a typical example in which the anticorrosive effect is lost due to the water-containing fluid 3 not containing fine cellulose fibers. [Figure 4] FIG. 1 is a diagram illustrating an embodiment of the present invention. [Diagram 5] FIG. 1 is a diagram illustrating an embodiment of the present invention. [Figure 6]FIG. 1 is a diagram illustrating an embodiment of the present invention. [Figure 7] FIG. 1 is a diagram illustrating an embodiment of the present invention. [Figure 8] FIG. 1 is a diagram illustrating an embodiment of the present invention. [Figure 9] FIG. 1 is a diagram illustrating an embodiment of the present invention. [Figure 10] FIG. 1 is a diagram illustrating an embodiment of the present invention. [Figure 11] FIG. 1 is a diagram illustrating an embodiment of the present invention. [Figure 12] FIG. 1 is a diagram illustrating an embodiment of the present invention. [Figure 13] FIG. 1 is a schematic diagram of a steel-magnesium test specimen or a steel-zinc test specimen. [Figure 14] FIG. 2 is a schematic diagram showing the arrangement of a water-containing fluid 3 and a sterile gauze 6 on a steel-magnesium test piece or a steel-zinc test piece. [Figure 15] FIG. 2 is a schematic diagram showing a test specimen for RFID monitoring. [Figure 16] 2 is a diagram showing a schematic view of the front surface, cross section, and back surface to be brought into contact with a steel plate 1 of a magnesium alloy plate 2 in a test specimen for RFID monitoring. FIG. [Figure 17] FIG. 2 is a diagram showing dimensions of each part of a test specimen used in a corrosion confirmation experiment. [Figure 18] FIG. 2 is a diagram showing a schematic appearance of a test specimen in a corrosion confirmation experiment. [Figure 19] FIG. 13 is a diagram showing a schematic diagram of a state in which a gap is secured by plastic tape in a test specimen in a corrosion confirmation experiment. [Figure 20] FIG. 1 is a schematic diagram showing how an acrylic plate is placed on plastic tape attached to a test specimen in a corrosion confirmation experiment, and the four corners of the acrylic plate are clamped with a vice. [Figure 21] FIG. 1 is a schematic diagram showing the connection of each channel (CH) of a test specimen to a data logger in a corrosion confirmation experiment. [Figure 22] This is a photograph taken during a corrosion confirmation experiment. [Diagram 23] 1 is a graph showing changes in current value with time for steel and magnesium alloy in a corrosion confirmation experiment. [Figure 24] 1 is a graph showing changes in current value over time for steel and magnesium alloy in the presence or absence of sodium sulfite as an electrolyte in a corrosion confirmation experiment. [Diagram 25] 13 is a photograph showing the corrosion prevention state inside a gap in a corrosion confirmation experiment. [Figure 26] 1 is a graph showing the change in current value over time for a steel material when the corrosion protection system of the present invention is not used. [Figure 27] This is an exploded view of an example of an RFID tag, excerpted from Patent Application No. 2021-176544. [Figure 28] This is an oblique view of an example of an RFID tag, excerpted from Patent Application No. 2021-176544. [Figure 29] This is a schematic diagram of a continuity determination device, excerpted from Patent Application No. 2021-176544. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] Preferred embodiments of the present invention will now be described in detail. In this specification, the features of the present invention will be described with reference to the drawings as appropriate. In the drawings, the dimensions and shapes of each part are exaggerated for clarity, and the actual dimensions and shapes are not accurately depicted. Therefore, the technical scope of the present invention is not limited to the dimensions and shapes of each part shown in these drawings. The corrosion prevention system, corrosion prevention monitoring system, and construction method thereof of the present invention are not limited to the following embodiments, and can be implemented in various forms with modifications and improvements that can be made by those skilled in the art within the scope of the gist of the present invention.
[0028] The present invention relates to a corrosion protection system for steel comprising a steel material, a base metal having a lower natural potential than the steel material, and a hydrous fluid containing fine cellulose fibers having an average fiber width of 1 nm or more and 1000 nm or less, and an electrolyte, wherein the steel material and the base metal are joined in an electrically conductive manner, the hydrous fluid is in contact with the steel material surface and the base metal surface, and supplies base metal ions generated from the base metal surface to the steel material surface.
[0029] The term "steel material" refers to steel processed into a plate, bar, tube, or the like for use as a material for civil engineering, construction, machinery, or the like. The steel material may be one or a combination of two or more. The steel material is preferably a combination of two or more steel materials having a gap between the two steel materials, such as a splice plate, a flange, or a bolt.
[0030] The steel material may have rust on the surface of the steel material.
[0031] Even if the steel material has rust on its surface, the corrosion prevention system of the present invention can be constructed without removing the rust, and the corrosion prevention system of the present invention can suppress further spread of the rust.
[0032] Examples of base metals having a lower natural potential than steel include base metals known in the art, such as magnesium, magnesium alloys, zinc, zinc alloys, aluminum, and aluminum alloys.
[0033] For example, the equilibrium potential of magnesium alloys is lower than that of steel. Therefore, by bonding magnesium alloys and steel with a conductive adhesive (conductive adhesives known in the art, such as conductive adhesives based on at least one of the group consisting of silicone, epoxy, phenol, acrylic, ene, urea, melamine, isocyanate, and chloroprene rubber, which are cured and bonded under at least one condition of the group consisting of heat, anaerobic conditions, moisture, light absorption, and pressure sensitivity, or conductive adhesives containing hot melt resins), it is possible to supply anticorrosive current, that is, electrons generated when base metals are ionized, to the steel when a water-containing fluid penetrates, and it is possible to perform sacrificial corrosion protection. This makes it possible to reverse the anode part in the gap of the steel to the cathode part, and as long as the magnesium alloy is sound, it will not corrode.
[0034] The steel material and the base metal, which has a lower natural potential than the steel material, are joined in an electrically conductive manner. Here, "joined in an electrically conductive manner" includes joining methods known in the art. Examples of such joining methods include joining via a conductive adhesive, welding, soldering, riveting, and the like. When welding is used for joining, care must be taken because it may cause galvanic corrosion.
[0035] In the present invention, the corrosion protection potential of a steel material is generally −0.77 V vs. SCE or less, but it is preferable to lower the cathodic potential by 0.3 V or more from the inherent natural potential of the steel material.
[0036] The water-containing fluid means a continuous body in which no shear stress occurs in a stationary state (i.e., has fluidity). The water-containing fluid includes water, fine cellulose fibers, and an electrolyte.
[0037] Since the aqueous fluid contains water, fine cellulose fibers, and electrolytes, the fine cellulose fibers retain moisture when moisture penetrates and act as a medium for the electrolyte in the aqueous fluid, thereby supplying base metal ions generated from the steel and base metal surfaces to the steel surface.
[0038] Fine cellulose fiber is a type of fiber in which glucose is bonded via β-1,4-glycosidic bonds (C6H 10 O5) n It is a material with a structure in which fibers made of polysaccharides represented by the formula (I) are finely untangled to an average fiber width in the range of 1 nm to 1000 nm, and is sometimes called cellulose nanofiber (CNF) or cellulose nanocrystal (CNC).
[0039] Examples of the fine cellulose fibers include mechanically defibrated fine cellulose fibers, non-anion-modified fine cellulose fibers, and anion-modified fine cellulose fibers.
[0040] Anion-modified fine cellulose fibers are fibers composed of cellulose in which some of the OH groups of the glucose units have been modified to anions, i.e., cellulose in which the OH groups have been esterified or otherwise modified to introduce an anion-modified group having a negative charge, or cellulose in which an anion-modified group has been introduced by oxidizing the methylene to which the 6-OH group is bonded. Examples of anion-modified fine cellulose fibers include, but are not limited to, sulfate esterified fine cellulose fibers, TEMPO oxidized fine cellulose fibers, phosphate esterified fine cellulose fibers, phosphite esterified fine cellulose fibers, and xanthate esterified fine cellulose fibers.
[0041] For example, the anion-modified fine cellulose fiber may be one represented by the formula (1): [ka] (In the formula, n is an integer of 1 to 3, and M n+ is an n-valent cation, and the wavy line is the bond to another atom (the bond to the carbon atom that previously held the OH group of the glucose unit). Examples of such fibers include sulfated fine cellulose fibers (also called sulfated cellulose nanofibers) having high hydration properties and having the substituents described in 1. In sulfated fine cellulose fibers, sulfate ester groups are usually introduced by substituting a portion of the OH groups in the cellulose constituting the fibers with sulfate ester groups represented by general formula (1). Sulfated fine cellulose fibers can be produced, for example, by sulfate esterifying and defibrating raw pulp.
[0042] Here, M n+ Examples of the cations include hydrogen ions, metal ions, and ammonium ions. When n is 2 or 3, M n+ 2 or 3 -OSO3 - It forms an ionic bond with
[0043] Examples of the metal ion include an alkali metal ion, an alkaline earth metal ion, a transition metal ion, and other metal ions.
[0044] Here, the alkali metal ion is lithium ion (Li + ), sodium ion (Na + ), potassium ion (K + ), rubidium ion (Rb + ), Cesium ion (Cs + ) and the like. Examples of alkaline earth metal ions include calcium ions (Ca 2+ ), strontium ion (Sr 2+ ) Transition metal ions include iron ions, nickel ions, chromium ions, palladium ions, copper ions, and silver ions. Other metal ions include beryllium ions, magnesium ions, zinc ions, and aluminum ions.
[0045] The ammonium ion is NH4 + Not only NH4 + Examples of ammonium ions include those derived from various amines in which one or more hydrogen atoms are replaced by organic groups. For example, NH+ , quaternary ammonium cation, alkanolamine ion, pyridinium ion, imidazolinium ion, etc.
[0046] M n+ From the viewpoint of processability in each application of the anion-modified fine cellulose fiber, hydrogen ions, sodium ions, potassium ions, calcium ions, or quaternary ammonium cations are preferred, and sodium ions (Na + It is particularly preferable that M of the anion-modifying group represented by the above general formula (1) is n+ The number of types may be one or more.
[0047] The anion-modified fine cellulose fiber of the present invention may have other substituents in addition to the sulfate ester group represented by the general formula (1). Here, when the anion-modified fine cellulose fiber has a group other than the sulfate ester group represented by the general formula (1), i.e., other substituents, the other substituents are usually substituted with at least one of the OH groups in the cellulose constituting the fine cellulose fiber. Examples of the other substituents include, but are not limited to, anionic substituents and their salts, ester groups, ether groups, acyl groups, aldehyde groups, alkyl groups, alkylene groups, aryl groups, and combinations of two or more of these. When the other substituents are a combination of two or more types, the content ratio of each of the substituents is not limited. As the other substituents, among them, anionic substituents and their salts, or acyl groups are preferred from the viewpoint of nano-dispersibility. As the anionic substituents and their salts, particularly preferred are carboxy groups, phosphate groups, phosphite groups, and xanthate groups. When the anionic substituent is in the form of a salt, sodium salts, potassium salts, and calcium salts are particularly preferred from the viewpoint of nano-dispersibility. Furthermore, as a particularly preferred acyl group, an acetyl group is preferred from the viewpoint of nano-dispersibility.
[0048] Even if anion-modified fine cellulose fibers are dried, their water-retaining properties (gel-like state) can be restored by adding water.
[0049] The average fiber width of the anion-modified fine cellulose fiber is not limited, but is usually from 1 nm to 1000 nm, preferably from 1 nm to 100 nm, and more preferably from 2 nm to 10 nm.
[0050] The average fiber length of the anionically modified fine cellulose fibers is not limited, but is usually from 0.1 μm to 6 μm, and preferably from 0.1 μm to 2 μm.
[0051] The average fiber width and the average fiber length can be measured by, for example, using an atomic force microscope (SPM-9700HT, manufactured by Shimadzu Corporation) to measure the fiber width (fiber diameter (equivalent circle diameter)) and fiber length of 50 arbitrarily selected fibers and calculating the arithmetic mean value. The average fiber width and the average fiber length can be set to a desired range by adjusting the concentration of the reagent such as sulfuric acid, the amount of pulp in the reaction solution, and the reaction time.
[0052] When the anion-modified fine cellulose fibers have an average fiber width and an average fiber length within the above-mentioned ranges, the anion-modified fine cellulose fibers can fill the surface of the steel material to be protected from corrosion with an appropriate amount of moisture without absorbing or retaining excessive moisture, and even if they are dried, they can reversibly return to a water-containing fluid by absorbing water again, and can exert a coating corrosion protection effect when dried to form a dry film.
[0053] In the anion-modified fine cellulose fiber, the amount of anion-modified group introduced is not limited, but is usually 0.3 mmol / g or more and 4.0 mmol / g or less, preferably 0.3 mmol / g or more and 3.0 mmol / g or less, more preferably 0.4 mmol / g or more and 2.5 mmol / g or less, and even more preferably 0.8 mmol / g or more and 2.0 mmol / g or less. The amount of anion-modified group introduced in the anion-modified fine cellulose fiber is expressed as the anion-modified group content (mmol) per 1 g of the anion-modified fine cellulose fiber. The amount of anion-modified group introduced can be set to any appropriate value within the above range depending on the application, etc.
[0054] By having the amount of anion-modifying group introduced within the above range, high water dispersibility can be obtained after drying.
[0055] Examples of non-anion-modified fine cellulose fibers include mechanically defibrated cellulose nanofibers and mechanically defibrated cellulose microfibers.
[0056] Non-anionically modified fine cellulose fibers do not change in viscosity due to salt or alkali, and can be applied in a gel state. Therefore, non-anionically modified fine cellulose fibers are highly adaptable to complex shapes up to the entrance of gaps, and are easier to maintain continuity than, for example, paper. In addition, non-anionically modified fine cellulose fibers are made of the same fibrous material as paper and have water retention properties.
[0057] The material properties of non-anionically modified fine cellulose fibers include an average fiber width and average fiber length equivalent to those of anionically modified fine cellulose fibers, relatively excellent chemical resistance, and being less expensive than chemically modified fibers such as anionically modified fine cellulose fibers, but having reduced water dispersibility after drying.
[0058] The cellulose fibers may be a mixture of non-anionically modified fine cellulose fibers and anionically modified fine cellulose fibers, for example, sulfated fine cellulose fibers.
[0059] By using a mixture of non-anionically modified fine cellulose fibers and sulfated fine cellulose fibers as the cellulose fibers, the electrostatic repulsion of the sulfate ester groups of the sulfated fine cellulose fibers suppresses the decrease in water retention caused by hydrogen bonds that occur when the non-anionically modified fine cellulose fibers are dried.Furthermore, the non-anionically modified fine cellulose fibers can suppress the decrease in viscosity (sol formation) of the sulfated fine cellulose fibers caused by salt and alkali (alkalization with base metal hydroxides (pH 10.5 or so)).Therefore, by mixing the two, the disadvantages of each can be compensated for, and it is possible to achieve reproducibility of hydration when drying and maintenance of a gel state in the presence of alkali and salt.
[0060] In addition, the viscosity of the mixture can be freely adjusted by changing the ratio, and for example, by adjusting the mixture ratio to lower the viscosity, it becomes possible to spread the fine cellulose fibers to the inside of narrower gaps. In addition, since the fine cellulose fibers have an oxygen barrier function, the difference in oxygen concentration between the entrance and the inner part of the gap can be reduced, and the anticorrosive effect of the base metal anode can be transmitted to a deeper part.
[0061] When a mixture of non-anionically modified fine cellulose fibers and anionically modified fine cellulose fibers is used as the cellulose fibers, the mass ratio of the non-anionically modified fine cellulose fibers to the anionically modified fine cellulose fibers (non-anionically modified fine cellulose fibers:anionically modified fine cellulose fibers) depends on the properties of the intended mixture, such as the viscosity, and is not limited, but is usually 1:0.01 to 1:100, preferably 1:0.1 to 1:10.
[0062] The content of the fine cellulose fibers is not limited, but is usually 0.1% by mass to 50% by mass, preferably 1% by mass to 5% by mass, based on the total mass of the solid contents in the aqueous fluid.
[0063] By adjusting the content of fine cellulose fibers, it is possible to make the viscosity of the aqueous fluid suitable for application to complex shaped parts and gaps to be protected from corrosion.
[0064] The electrolyte is a compound different from the fine cellulose fiber, and is not limited thereto, but is preferably water-soluble, and more preferably also acts as a reducing agent, or is used in combination with a substance that acts as a reducing agent as part of the electrolyte. For example, the electrolyte may be one or more selected from the group consisting of water-soluble metal salts, ammonium salts, and ionic liquids. In addition, the anion-modified fine cellulose fiber also exhibits the function of an electrolyte because the anion-modified group is ionized as an anion.
[0065] The metal salt is not particularly limited, but may be one or more selected from the group consisting of alkali metal elements and alkaline earth metal elements as the cation. Specific examples of the metal salt include sodium chloride (table salt), potassium chloride, calcium chloride, sulfates, carboxylates, borates, and phosphates.
[0066] The ammonium salt is not particularly limited, but is represented by NH4X (wherein X is a monovalent base) or NR4X (wherein R is each independently a hydrogen atom or an alkyl group, and X is a monovalent base). X is preferably, for example, a halogen ion, a sulfate ion, an acetate ion, a nitrate ion, or a hydroxide ion from the viewpoint of dispersibility. Each R is independently an alkyl group having 1 to 4 carbon atoms. Examples of the ammonium salt include ammonium sulfate, ammonium acetate, ammonium formate, tetramethylammonium chloride, tetraethylammonium chloride, and tetraethylammonium hydroxide.
[0067] The ionic liquid is not particularly limited, but examples thereof include imidazolium-based ionic liquids, aromatic ionic liquids, pyrrolidinium-based ionic liquids, ammonium-based ionic liquids, piperidinium-based ionic liquids, quaternary phosphonium-based ionic liquids, etc. In addition to functioning as an electrolyte, ionic liquids also have antifreeze functions and dissolve cellulose-based compounds.
[0068] The imidazolium ionic liquid is not particularly limited, but examples thereof include hexyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide (C1C6Im-NTf2) and 1-butyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide (C1C4Im-NTf2).
[0069] The aromatic ionic liquid is not particularly limited, but examples thereof include diphenylmethane diisocyanate bis(trifluoromethanesulfonyl)imide (MDI-TFSI).
[0070] The ammonium-based ionic liquid is not particularly limited, but examples thereof include N,N-diethyl-N-(2-methoxyethyl)ammonium tetrafluoroborate (DEME-BF4), trimethylpropylammonium bis(trifluoromethanesulfonyl)imide (TMPA-(CF3SO2)2N), and the like.
[0071] Reducing electrolytes include sodium sulfite, sodium thiosulfate, iron(II) sulfate hydrazine, and gallic acid.
[0072] By including an electrolyte in the water-containing fluid, the base metal ions can be transferred more smoothly from the base metal to the steel material.
[0073] Furthermore, by making the water-containing fluid contain an electrolyte that also acts as a reducing agent, oxygen in the water-containing fluid can be reduced, thereby decreasing the oxygen concentration in the water-containing fluid.
[0074] Furthermore, if the aqueous fluid contains sodium sulfite, the oxygen concentration in the gap will decrease significantly, and if the corrosion-preventing effect of the base metal disappears, the potential difference between the oxygen concentration cell formed between the gap and the outside will also increase, which may accelerate corrosion in the gap. Therefore, the base metal must be replaced immediately after it is consumed.
[0075] The content of the electrolyte is not limited, but is usually 0.1% by mass or more, preferably 1% by mass or more, based on the total mass of the solid content in the water-containing fluid. The upper limit of the content of the electrolyte is not limited, but is usually 85% by mass, preferably 80% by mass. Therefore, the content of the electrolyte is not limited, but is usually 0.1% by mass or more and 85% by mass or less, preferably 1% by mass or more and 80% by mass or less, for example 45% by mass or more and 79% by mass or less, based on the total mass of the solid content in the water-containing fluid.
[0076] In addition, since the water-containing fluid of the present invention contains electrolytes, it may have a freezing point below 0°C due to freezing point depression, but it may also contain an antifreeze agent to further prevent freezing when used in a low-temperature environment.
[0077] The antifreezing agent is not particularly limited as long as it lowers the freezing point of water, and examples thereof include one or more selected from the group consisting of glycol-based compounds and highly polar amphipathic solvents. Examples of glycol-based compounds include, but are not limited to, ethylene glycol, diethylene glycol, and propylene glycol. Examples of highly polar amphipathic solvents include, but are not limited to, dimethyl sulfoxide, N-methylpyrrolidone, dimethylformamide, N,N-dimethylacetamide, methanol, ethanol, 2-propanol, and glycerin.
[0078] The content of the antifreeze agent can be selected arbitrarily depending on the usage environment, and is not limited, but is usually 0.1 mass% or more and 85 mass% or less, preferably 1 mass% or more and 80 mass% or less, for example 5 mass% or more and 50 mass% or less, relative to the total mass of solids in the water-containing fluid.
[0079] The solid content of the water-containing fluid is not limited, but is usually from 1% to 50%, preferably from 2% to 15%.
[0080] The corrosion protection system of the present invention may further include fibers for carrying aqueous fluids other than fine cellulose fibers (in this specification, etc., they may be simply referred to as "fibers" in contrast to "fine cellulose fibers"), such as cellulose fibers such as pulp, resin fibers, and entangled forms of these fibers, such as gauze, cotton, nonwoven fabric, and resin nets.
[0081] The average fiber diameter of the fibers is not limited, but is usually from 5 μm to 300 μm, preferably from 10 μm to 200 μm.
[0082] In the present invention, the fine cellulose fibers provide an environment in which ions can smoothly migrate in the aqueous fluid. Since the fine cellulose fibers dry over time, it is preferable that the fine cellulose fibers cover the entire surface of the entrance of the gap between the base metal, for example, the magnesium alloy, as much as possible when the fine cellulose fibers are dried. By including fibers for carrying an aqueous fluid in the corrosion protection system of the present invention, it is possible to alleviate the shrinkage characteristic derived from the bond caused by the drying of the fine cellulose fibers, and to suppress the occurrence of peeling and cracking of the cellulose fibers during the drying process. Note that the fibers only need to be able to carry the aqueous fluid, and the effect can be achieved by arranging them near the entrance of the gap, without needing to be inserted deep into the gap of a steel material having a complex shape.
[0083] The corrosion prevention system of the present invention preferably has a structure in which fibers 6 such as cotton gauze are sandwiched between water-containing fluid 3 on the surface of a steel material 1 or a base metal 2 as shown in FIG.
[0084] As shown in Figure 1, the corrosion prevention system of the present invention has a structure in which fibers 6 such as cotton gauze are sandwiched between aqueous fluid 3 on the surface of steel 1 or base metal 2, thereby making it possible to further suppress peeling and cracking of the aqueous fluid containing fine cellulose fibers or its dried body during the drying process.
[0085] When the corrosion protection system of the present invention includes fibers, it may further include water wicking and evaporation paper.
[0086] The corrosion prevention system of the present invention includes water-absorbing and evaporating paper, which can prevent peeling caused by the drying of the water-containing fluid.
[0087] The corrosion protection system of the present invention may further include an exterior material applied to the steel surface so as to cover the base metal and the water-containing fluid.
[0088] The exterior material is not limited, but is preferably made of a material that is excellent in weather resistance and waterproofing, for example, a material that is impermeable to air and ultraviolet rays. Examples of the exterior material include a mixture of bitumen (asphalt) and rubber, and a petrolatum-based sheet.
[0089] The exterior material can be installed, for example, by a waterproof adhesive (adhesives known in the art, for example, adhesives based on at least one of the group consisting of silicone, epoxy, phenol, acrylic, ene, urea, melamine, isocyanate, and chloroprene rubber, which cure and bond under at least one condition of the group consisting of heat, anaerobic conditions, moisture, light absorption, and pressure sensitivity, or adhesives containing hot melt resins) so as to cover the base metal and water-containing fluid on the steel surface where the gap exists, or by a physical method such as bolt fastening. The exterior material can play a role in preventing the intrusion of moisture from the outside world. Furthermore, even if the exterior material and adhesive deteriorate over time and moisture infiltrates, the moisture can be trapped inside the corrosion protection system to maintain the corrosion protection circuit.
[0090] Therefore, the present invention also relates to a corrosion prevention system in which, when the applied fine cellulose fibers have dried, in the environment surrounding the gap, the applied portion is covered with an exterior material provided to prevent the intrusion of moisture from the outside, and the exterior material is fixed to the steel material by a physical method such as a highly waterproof adhesive or bolting, and in the second step, even if the exterior material and adhesive deteriorate over time and moisture infiltrates, the moisture can be trapped inside and the corrosion prevention circuit can be maintained.
[0091] Because the corrosion prevention system of the present invention includes an exterior material, it is possible to suppress self-corrosion that occurs when base metals such as magnesium are exposed to the atmosphere, and further, it is possible to prevent moisture from reaching gaps. Even if moisture begins to penetrate due to deterioration or the like, the corrosion prevention circuit can be maintained by trapping the moisture within the exterior material, and in addition, the effect of diluting the oxygen supply by isolating it from the atmosphere can be obtained.
[0092] The corrosion protection system of the present invention may further comprise an RFID tag.
[0093] Here, the RFID tag will be described with reference to Figs. 27 to 29. Fig. 27 is an exploded view of an example of an RFID tag. Fig. 28 is a perspective view of an example of an RFID tag. Fig. 29 is a diagram showing a schematic diagram of a continuity determination device. The RFID tag 10 includes a block-shaped base substrate 16 long in one direction, an antenna substrate 17 arranged in a state of being overlapped on a first surface 23 of the base substrate 16, an IC chip module 20 located between the base substrate 16 and the antenna substrate 17 and having a first electrode 18 and a second electrode 19 on a surface facing the base substrate 16, a first detection terminal 21 electrically connected to the first electrode 18 of the IC chip module 20, and a second detection terminal 22 electrically connected to the second electrode 19 of the IC chip module 20, the first detection terminal 21 and the second detection terminal 22 being electrically connected to a base metal 2 and a steel material 1, respectively, and the antenna substrate 17 transmits a detection result of the presence or absence of continuity between two metal bodies by radio waves.
[0094] Such an RFID tag 10 can transmit the detection result of the presence or absence of continuity in a non-contact manner via radio waves.
[0095] The following configuration is desirable as an embodiment of the RFID tag 10. The base substrate 16 is made of an insulating material and has a second surface 24 on the opposite side to the first surface 23, the second surface 24 being spaced apart from the first surface 23 by a predetermined distance or more, and the RFID tag 10 is attached to the steel material 1 with the second surface 24 serving as an attachment surface.
[0096] If the distance between the steel material 1 and the IC chip module 20 becomes less than a predetermined distance, the IC chip module 20 may be affected by disturbances, which may reduce the accuracy of detection. If the distance between the first surface 23 and the second surface 24 is set to a predetermined distance or more, the steel material 1 and the IC chip module 20 are separated by the predetermined distance or more, which reduces the influence of disturbances and makes it possible to more accurately detect the presence or absence of continuity.
[0097] The RFID tag 10 is provided with a clip 25 that holds the antenna substrate 17 against the base substrate 16, and the first detection terminal 21 and the second detection terminal 22 maintain contact with the first electrode 18 and the second electrode 19 due to the elastic force of the clip 25, thereby maintaining electrical connection with the electrodes 18 and 19.
[0098] Each terminal 21, 22 and each electrode 18, 19 are held in contact with each other by being pressed by clip 25, and an electrical connection is maintained. Since terminals 21, 22 are not fixed to electrodes 18, 19, even if the electrodes 18, 19 and terminals 21, 22 are misaligned due to temperature changes and differences in linear expansion coefficients, the connection parts are not damaged and a good connection state can be maintained. This makes it possible to make RFID tag 10 resistant to temperature changes.
[0099] The continuity determination device 26 includes an RFID tag 10 and an RFID reader 11 that reads the detection result from the RFID tag 10 in a non-contact manner. In this manner, the detection result of the RFID tag 10 can be received by using the RFID reader 11 in a non-contact manner.
[0100] The presence or absence of conductivity can be used to determine whether the effect of sacrificial protection is being maintained.
[0101] The RFID reader 11 includes an RFID reader side antenna that transmits and receives radio waves between the RFID tag 10 and the RFID tag 10, and a control unit. The RFID tag 10 is a passive type that receives power from the received radio waves, detects the conductivity state, and transmits the detection results. The control unit may automatically adjust the level of the radio waves output to the RFID tag 10 so that the RFID reader side antenna can receive the detection results transmitted by the RFID tag 10.
[0102] In this way, the RFID reader 11 can receive the detection result of the RFID tag 10 more reliably.
[0103] The control unit may increase the level of the radio waves to be output when the RFID reader antenna cannot receive the detection result transmitted by the RFID tag 10. When the power supplied from the RFID reader 11 to the RFID tag 10 increases due to the increase in the radio wave level, the level of the radio waves transmitted from the RFID tag 10 to the RFID reader 11 also increases. This allows the RFID reader 11 to receive the radio waves from the RFID tag 10 more reliably.
[0104] The detection result is a close signal detected when there is continuity between the first detection terminal 21 and the second detection terminal 22, or an open signal detected when there is no continuity, and the control unit may determine the presence or absence of continuity based on the order and number of the open signals and close signals received.
[0105] The detection result may contain an error that indicates a result different from the actual continuity state. By determining the presence or absence of continuity based on the sequence and number of open and close signals received by the RFID reader 11, the influence of the error can be eliminated and the presence or absence of continuity can be determined more accurately.
[0106] The control unit may determine that there is no electrical continuity between the first detection terminal 21 and the second detection terminal 22 if the open signal is received one or more times before receiving the close signal multiple times, and may determine that there is electrical continuity between the first detection terminal 21 and the second detection terminal 22 if the close signal is received multiple times before receiving the open signal one or more times.
[0107] In this way, at least the first detected close signal is not used to determine whether or not there is continuity, so even if the first close signal is an error, it will not have an effect on the determination result. An accurate determination can be made based on the second and subsequent close signals.
[0108] In one embodiment of the RFID tag 10, the RFID tag 10 has an IC chip with a tamper function mounted on a ceramic tag, and emits a flag signal in response to a request from the RFID reader 11 when the metal material made of the base metal 2 peels off or wears off. Here, the tamper function is a function that detects a break in the lead wire 27 connected to the tag when the RFID tag 10 or the like is illegally opened and sets a flag. The tamper function was developed to detect breaks, and if the lead wire 27 is connected to metal, it will malfunction because of the electrostatic capacitance of the metal, but a program filter is applied to prevent the effect of the electrostatic capacitance through statistical processing. In addition, the RFID tag 10 is made of ceramic that is resistant to temperature changes, and is designed to maintain a long life (20 years or more) without being affected by changes in outdoor temperature. In addition, the RFID tag 10 tends to be disturbed by metals, making it impossible to read or the reading distance shortening, but it is also designed to prevent disturbance, and has a reading distance of about 4 m to 10 m even when covered with an exterior material. In particular, hydroxides that are by-products of metallic materials made of base metals 2, for example magnesium hydroxide that is a by-product of magnesium, are insulators, so when the entire base metal 2 is worn out and replaced with a hydroxide of the base metal 2, for example magnesium hydroxide, it becomes possible to instantly and remotely read the wear state with the RFID reader 11 while still covered with the exterior material. By using this RFID tag 10, it is possible to grasp the internal wear state remotely without removing the exterior material at close range, and it is possible to grasp the speed of wear due to differences in the environment that cannot be confirmed from the outside, so it is possible to operate it without worrying about the adverse effects. Furthermore, the RFID tag 10 is a passive type that does not use a power source, so there is no need to bother with battery replacement during use.
[0109] Figures 27 to 29 and the description of the RFID tag are excerpted from Patent Application No. 2021-176544.
[0110] Sacrificial protection is a method of exerting a corrosion protection function by consuming the base metal material of the steel material to be protected. Therefore, when the base metal material is completely consumed, the corrosion protection function is lost. In addition, when the conductive adhesive that electrically connects the base metal material and the steel material to be protected is peeled off, the corrosion protection function is lost.
[0111] In this case, it is possible to expect an anti-corrosion effect from the passive film in the gap, due to the adhesion of hydroxides derived from the metallic material made of base metals (magnesium hydroxide if a magnesium alloy is used as the base metal), etc., but this effect will be destroyed by the inflow of chloride ions from salts in the antifreeze, and there is a high possibility that corrosion will proceed as before.
[0112] For this reason, monitoring the wear and peeling of metallic materials made of base metals is important for maintaining the corrosion protection system. In addition, the technical application area of the present invention is the corrosion protection of bridges and plant facilities, which requires long-term monitoring, so a method that does not use a power source is preferable.
[0113] Therefore, by providing the corrosion prevention system of the present invention with a passive RFID tag that does not use a power source, the corrosion prevention system of the present invention can be used as a corrosion prevention monitoring system.
[0114] In the corrosion prevention system or corrosion prevention monitoring system of the present invention, the water-containing fluid may be dry.
[0115] When the aqueous fluid dries, a coating is formed based on the fine cellulose fibers contained in the aqueous fluid. This coating exerts an oxygen gas barrier effect, reducing the difference in oxygen concentration between the entrance and gap of the steel material, thereby suppressing corrosion of the steel material.
[0116] The present invention also relates to a water-containing fluid for use in the above-described corrosion protection system for steel or corrosion protection monitoring system.
[0117] The aqueous fluid of the present invention contains water, fine cellulose fibers, and an electrolyte, and the materials contained in the aqueous fluid are as described above.
[0118] The content and solid content of each material in the water-containing fluid of the present invention are as described above.
[0119] The viscosity of the water-containing fluid of the present invention is not limited as long as it has fluidity. The viscosity of the water-containing fluid of the present invention can be freely adjusted, but is usually 1 mPa·s to 100,000 mPa·s, preferably 10 mPa·s to 10,000 mPa·s, under the conditions in which the water-containing fluid is used, for example, at atmospheric pressure and at a temperature usually between -10°C and 65°C, for example between 0°C and 60°C. The water-containing fluid of the present invention is preferably in a gel state.
[0120] The water-containing fluid of the present invention has the role of propagating the anticorrosive current of the sacrificial protection system and protecting the area to which the anticorrosive current has propagated. Furthermore, the water-containing fluid of the present invention can effectively propagate the anticorrosive current by further containing an electrolyte. The water-containing fluid of the present invention makes it possible to apply the sacrificial protection system to parts with complex shapes or gaps, compared to a water-containing sheet using a paper sheet or the like.
[0121] By configuring the water-containing fluid of the present invention as described above, the water-containing fluid can easily penetrate into gaps in steel materials, making it possible to construct a corrosion prevention system or corrosion prevention monitoring system for steel materials of the present invention.
[0122] The present invention also relates to a dried body of the water-containing fluid for use in the above-described corrosion protection system for steel or the corrosion protection monitoring system.
[0123] The dried body of the hydrous fluid of the present invention is the hydrous fluid of the present invention dried, and contains fine cellulose fibers and an electrolyte. The dried body of the hydrous fluid of the present invention is a dry composition containing components that do not volatilize when dried, such as an electrolyte. The dried body of the hydrous fluid of the present invention is a coating formed of fine cellulose fibers, which exhibits an oxygen gas barrier effect and is intended to inhibit corrosion of steel materials, and can be present, for example, in gaps in steel materials that are corrosion-resistant materials having complex shapes that the hydrous fluid can reach.
[0124] The thickness of the dried water-containing fluid of the present invention is not limited, and is usually from 1 μm to 50 mm, preferably from 5 μm to 10 mm.
[0125] When the thickness of the dried body of the water-containing fluid of the present invention is within the above range, a sufficient oxygen gas barrier effect is exhibited, and corrosion of steel materials can be suppressed.
[0126] The present invention also relates to a method for constructing the above-described corrosion protection system or corrosion protection monitoring system for steel materials.
[0127] The method of the present invention includes the steps of joining a steel material and a base metal having a lower natural potential than the steel material in an electrically conductive manner, and arranging an aqueous fluid so as to be in contact with the steel material surface and the base metal surface and so as to supply base metal ions generated from the base metal surface to the steel material surface.
[0128] The method of disposing the water-containing fluid is not limited. The water-containing fluid is preferably introduced so as to be distributed evenly in the gaps between the steel materials. The water-containing fluid can be introduced, for example, by injection using a caulking injector, caulking gun, or syringe under normal pressure, low pressure, high pressure, or any other pressure condition, and within any temperature range in which water is in a liquid state.
[0129] In the method of the present invention, rust may be present on the steel material, and even if rust is present on the steel material, there is no need to remove the rust.
[0130] The method of the present invention can be carried out on steel materials having rust, such as splice plates, without disassembling the splice plates. This is because, in the method of the present invention, the aqueous fluid easily penetrates into the gaps in the steel material, so that base metal ions generated from the base metal surface can be supplied to the steel material surface, and the surface potential of the steel material can be set to a corrosion protection potential, thereby constructing a corrosion protection system or corrosion protection monitoring system for the steel material. Therefore, by using the present invention on steel materials having rust, further spread of rust can be suppressed. Therefore, the corrosion protection system or corrosion protection monitoring system of the present invention can prevent further corrosion due to rust and extend the life of steel materials, for example, even in steel materials that exist in an environment exposed to sunlight, wind and rain at atmospheric pressure and at temperatures usually between -10°C and 65°C, for example between 0°C and 60°C.
[0131] FIG. 2 shows one embodiment of the present invention.
[0132] The corrosion prevention system of one embodiment of the present invention shown in Fig. 2 includes a steel material 1, a base metal 2 having a lower natural potential than the steel material 1, and an aqueous fluid 3 containing fine cellulose fibers. An existing rust layer S' is formed on the steel material 1. The steel material 1 and the base metal 2 are joined in an electrically conductive manner (conductive adhesive 4). The aqueous fluid 3 is in contact with the surface of the steel material 1 and the surface of the base metal 2 in the gaps in the steel material 1 and around the base metal 2, and is arranged so as to supply base metal ions generated from the surface of the base metal 2 to the surface of the steel material 1 as shown by the arrows in Fig. 2.
[0133] In addition, when the water-containing fluid 3 does not contain fine cellulose fibers, as shown in Fig. 3, the water-containing fluid 3 may be in contact with each of the steel material 1 surface and the base metal 2 surface, but may not be arranged to supply base metal ions generated from the base metal 2 surface to the steel material 1 surface, as shown by the arrow in Fig. 3. In this case, it is not possible to pass an electric current between the steel material 1 and the base metal 2, and as a result, the corrosion prevention effect cannot be exhibited, and rust S is formed. Therefore, the fine cellulose fibers contained in the water-containing fluid 3 have the role of connecting the base metal 2 surface and the steel material 1 surface without interruption so that the surface of the steel material 1 can be smoothly supplied with base metal ions generated from the base metal 2 surface by moderately wetting the surface of the steel material 1.
[0134] FIG. 4 shows another embodiment of the present invention.
[0135] The corrosion prevention system according to one embodiment of the present invention shown in FIG. 4 includes a steel material 1, two base metals 2 having a lower natural potential than the steel material 1, and a water-containing fluid 3 containing fine cellulose fibers. An existing rust layer S' is formed on the steel material 1. The steel material 1 and the base metal 2 are joined in an electrically conductive manner (conductive adhesive 4). The water-containing fluid 3 is arranged in the gaps of the steel material 1 and around the two base metals 2, in contact with the steel material 1 surface and the two base metals 2 surfaces, and is arranged so as to supply base metal ions generated from the two base metals 2 surfaces to the upper and lower steel material 1 surfaces where the base metals are joined. The fine cellulose fibers contained in the water-containing fluid 3 have an oxygen gas barrier function that blocks oxygen in the atmosphere.
[0136] FIG. 5 shows another embodiment of the present invention.
[0137] The corrosion prevention system according to one embodiment of the present invention shown in FIG. 5 includes a steel material 1, two base metals 2 having a lower natural potential than the steel material 1, a water-containing fluid 3 containing fine cellulose fibers, and an exterior material 5. An existing rust layer S' is formed on the steel material 1. The steel material 1 and the base metal 2 are joined in an electrically conductive form (conductive adhesive 4). The water-containing fluid 3 is arranged in the gaps of the steel material 1 and around the two base metals 2 so as to contact the steel material 1 surface and the two base metals 2 surfaces and to supply base metal ions generated from the two base metals 2 surfaces to the upper and lower steel material 1 surfaces where the base metals are joined. The exterior material 5 is stretched on the surface of the steel material 1 so as to cover the two base metals 2 and the water-containing fluid 3. The exterior material 5 has an oxygen gas barrier function that blocks oxygen in the atmosphere, similar to the fine cellulose fibers contained in the water-containing fluid 3, and also has a role of trapping moisture inside.
[0138] FIG. 6 shows another embodiment of the present invention.
[0139] The corrosion prevention system of one embodiment of the present invention shown in Fig. 6 includes a steel material 1, three base metals 2 having a lower natural potential than the steel material 1 bonded onto the steel material 1, an anchor bolt 28 embedded in a bolt through hole of the steel material 1, a nut portion 29 fastened to the anchor bolt 28, the base metals 2 surrounding the side of the nut portion 29, a washer 31 installed in the lower portion of the nut portion 29, i.e., between the nut portion 29 and the steel material 1, a water-containing fluid 3 containing fine cellulose fibers, and an exterior material 5. The steel material 1 and the three base metals 2 bonded onto the steel material 1, and the nut portion 29 and the base metals 2 surrounding the side of the nut portion 29 are bonded in an electrically conductive manner (conductive adhesive 4). The water-containing fluid 3 is in contact with the gaps and surface (surroundings) of the steel material 1, the surfaces of the three base metals 2 joined on the steel material 1, the surface of the anchor bolt 28, the surface of the nut part 29 and the washer 31, the surface of the base metal 2 surrounding the side of the nut part 29, the minute gap 30 that may be formed between the anchor bolt 28 and the nut part 29, the minute gap 30 that may be formed between the nut part 29 and the washer 31 and the steel material 1, and the minute gap 30 that may be formed between the steel material 1 and the anchor bolt 28, and is arranged so as to supply base metal ions generated from the three base metals 2 joined on the steel material 1 and the surface of the base metal 2 surrounding the side of the nut part 29 to the surface of the steel material 1, the surface of the nut part 29 and the washer 31, and the surface of the anchor bolt 28. The exterior material 5 is stretched over the surface of the steel material 1 so as to cover the three base metals 2 joined on the steel material 1, the anchor bolt 28, the nut part 29 and the washer 31, the base metal 2 surrounding the side of the nut part 29, and the water-containing fluid 3. 6, the minute gap 30 is depicted as if it were visible for the sake of convenience, but the minute gap 30 is not usually a gap visible to the naked eye, but a gap through which the water-containing fluid 3 can pass, and refers to a minute gap that can be unavoidably formed during construction. Here, the water-containing fluid 3 becomes a seal at the boundary between the steel material 1 (particularly the base plate), particularly the lower part of the steel material 1, and the anchor bolt 28 due to their close contact, and is not discharged from the corrosion prevention system of the present invention.Furthermore, in order to reliably transmit the water-containing fluid in the minute gap 30 to the surface of the lower part of the anchor bolt 28, a cut is made in the washer 31 installed in the lower part of the nut part 29 to a degree that does not affect its function, thereby making it possible to more reliably maintain the continuity of the water-containing fluid 3. Also, the lower part of Fig. 6 (i.e., a member that may be joined to the lower part of the steel material 1 by the anchor bolt 28, such as mortar) is omitted. Furthermore, the exterior material 5, like the fine cellulose fibers contained in the water-containing fluid 3, has an oxygen gas barrier function that blocks oxygen in the atmosphere, and also has the role of trapping moisture inside.
[0140] Figure 7 shows a schematic diagram of the internal state of the exterior material of the corrosion protection system of one embodiment of the present invention shown in Figure 6. Figure 7 shows how, even if moisture W penetrates into the corrosion protection system from the outside, the moisture W can be confined inside the corrosion protection system to maintain the corrosion protection circuit.
[0141] FIG. 8 shows another embodiment of the present invention.
[0142] The corrosion prevention system of one embodiment of the present invention shown in Fig. 8 includes a steel material 1, two base metals 2 having a lower natural potential than the steel material 1, and an aqueous fluid 3 containing fine cellulose fibers. The steel material 1 and the base metals 2 are joined in an electrically conductive manner (conductive adhesive 4). The aqueous fluid 3 is arranged in the gaps in the steel material 1 and around the two base metals 2 as well as around the steel material 1, in contact with the surface of the steel material 1 and the surfaces of the two base metals 2, and is arranged to supply base metal ions generated from the surfaces of the two base metals 2 to the upper and lower surfaces of the steel material 1 where the respective base metals are joined.
[0143] FIG. 9 shows another embodiment of the present invention.
[0144] The corrosion prevention system according to one embodiment of the present invention shown in FIG. 9 includes a steel material 1, two base metals 2 having a lower natural potential than the steel material 1, a water-containing fluid 3 containing fine cellulose fibers, and fibers 6. The steel material 1 and the two base metals 2 are joined in an electrically conductive form (conductive adhesive 4). The water-containing fluid 3 is arranged so as to contact the steel material 1 surface and the two base metals 2 surfaces not only in the gaps of the steel material 1 and around the two base metals 2 but also around the steel material 1, and to supply base metal ions generated from the two base metals 2 surfaces to the upper and lower steel material 1 surfaces where the base metals are joined. The fibers 6 are arranged so as to be inserted into the gaps of the steel material 1. By inserting the fibers 6 into the gaps of the steel material 1, it is possible to prevent the water-containing fluid 3 from being interrupted as shown in FIG. 3.
[0145] FIG. 10 shows another embodiment of the present invention.
[0146] The corrosion prevention system according to one embodiment of the present invention shown in FIG. 10 includes a steel material 1, two base metals 2 having a lower natural potential than the steel material 1, a water-containing fluid 3 containing fine cellulose fibers, and two fibers 6. The steel material 1 and the base metal 2 are joined in an electrically conductive form (conductive adhesive 4). The water-containing fluid 3 is arranged so as to contact the steel material 1 surface and the two base metals 2 surfaces not only in the gaps of the steel material 1 and around the two base metals 2 but also around the steel material 1, and to supply base metal ions generated from the two base metals 2 surfaces to the upper and lower steel material 1 surfaces where the respective base metals are joined. One of the two fibers 6 is arranged so as to be inserted into the gaps of the steel material 1. By using two fibers 6, it is possible to more effectively prevent the water-containing fluid 3 from being interrupted as shown in FIG. 3.
[0147] FIG. 11 shows another embodiment of the present invention.
[0148] The corrosion prevention system according to one embodiment of the present invention shown in FIG. 11 includes a steel material 1, two base metals 2 having a lower natural potential than the steel material 1, a water-containing fluid 3 containing fine cellulose fibers, two fibers 6, and water-absorbing and evaporative paper 7. The steel material 1 and the base metal 2 are joined in an electrically conductive form (conductive adhesive 4). The water-containing fluid 3 is arranged so as to contact the surface of the steel material 1 and the surfaces of the two base metals 2 not only in the gaps of the steel material 1 and around the two base metals 2 but also around the steel material 1, and to supply base metal ions generated from the surfaces of the two base metals 2 to the upper and lower steel material 1 surfaces where the respective base metals are joined. One of the two fibers 6 is arranged so as to be inserted into the gaps of the steel material 1. The water-absorbing and evaporative paper 7 is arranged on the fibers 6 between the steel material 1 and the base metals 2. The arrangement of the water-absorbing and evaporative paper 7 can prevent peeling due to drying of the water-containing fluid 3.
[0149] FIG. 12 shows another embodiment of the present invention.
[0150] The corrosion prevention system according to one embodiment of the present invention shown in FIG. 12 includes a steel material 1, two base metals 2 having a lower natural potential than the steel material 1, a water-containing fluid 3 containing fine cellulose fibers, two fibers 6, and water-absorbing and evaporative paper 7. The steel material 1 and the base metal 2 are joined in an electrically conductive form (conductive adhesive 4). The water-containing fluid 3 is arranged not only around the gaps in the steel material 1 and the two base metals 2, but also around the steel material 1 and on the two fibers 6, in contact with the steel material 1 surface and the two base metals 2 surfaces, and is arranged to supply base metal ions generated from the two base metals 2 surfaces to the upper and lower steel material 1 surfaces where the respective base metals are joined. One of the two fibers 6 is arranged to be inserted into the gaps in the steel material 1. The water-absorbing and evaporative paper 7 is arranged on the fibers 6 between the steel material 1 and the base metals 2, and the water-containing fluid 3 is arranged to cover the water-absorbing and evaporative paper 7, so that peeling due to drying of the water-containing fluid 3 can be further prevented. EXAMPLES
[0151] The present invention will be described in more detail below using examples, but the technical scope of the present invention is not limited to these examples.
[0152] <Method for producing highly substituted sulfated CNF (cellulose nanofiber) as fine cellulose fiber> 90 g of dimethyl sulfoxide (DMSO), 10 g of acetic anhydride (concentration in defibration solution: 9.8% by mass), and 2.0 g of sulfuric acid (concentration in defibration solution: 2.0% by mass) were placed in a 300 ml sample bottle and stirred for approximately 30 seconds using a magnetic stirrer at room temperature of 23°C to prepare a defibration solution.
[0153] Next, 3.0 g of softwood kraft pulp NBKP (manufactured by Nippon Paper Industries Co., Ltd.) was added to the defibrated solution and stirred for an additional 2 hours at room temperature of 23°C to carry out a sulfate esterification reaction. After stirring, 150 ml of distilled water was added to the cellulose-containing defibrated solution to stop the reaction, and then a 5% by mass aqueous solution of sodium hydroxide was added until the pH reached 7 to neutralize the reaction solution. The supernatant was then removed by centrifugation.
[0154] An additional 1350 ml of distilled water was added and stirred until uniformly dispersed, after which the supernatant was removed by centrifugation. The same procedure was repeated for a total of three washes. After washing by centrifugation, distilled water was added and the total weight was diluted to 300 g.
[0155] Next, the mixture was stirred for 3 minutes using a mixer (G5200, manufactured by Biolomix) to obtain a uniform aqueous dispersion of cellulose nanofibers having sulfate ester groups (sulfate-esterified CNF) with a concentration of 1% by mass.
[0156] The aqueous dispersion of sulfated CNF was dried for 24 hours at room temperature of 23°C to obtain solid sulfated CNF. The sulfate ester group was quantified using an infrared spectrometer (Nicolet iS 5N FT-IR, Thermo Fisher Science) and an organic elemental analyzer (EA-3100, JASCO), and the degree of sulfate ester group substitution per glucose unit of cellulose was found to be 3.5 mmol / g.
[0157] <Method for producing low-substitution sulfate esterified CNF (cellulose nanofiber) as fine cellulose fiber> 90 g of dimethyl sulfoxide (DMSO), 10 g of acetic anhydride (concentration in defibration solution: 9.9% by mass), and 1.0 g of sulfuric acid (concentration in defibration solution: 1.0% by mass) were placed in a 300 ml sample bottle and stirred for approximately 30 seconds using a magnetic stirrer at room temperature of 23°C to prepare a defibration solution.
[0158] Next, 3.0 g of softwood kraft pulp NBKP (manufactured by Nippon Paper Industries Co., Ltd.) was added to the defibrated solution and stirred for an additional 2 hours at room temperature of 23°C to carry out a sulfate esterification reaction. After stirring, 150 ml of distilled water was added to the cellulose-containing defibrated solution to stop the reaction, and then a 5% by mass aqueous solution of sodium hydroxide was added until the pH reached 7 to neutralize the reaction solution. The supernatant was then removed by centrifugation.
[0159] An additional 1350 ml of distilled water was added and stirred until uniformly dispersed, after which the supernatant was removed by centrifugation. The same procedure was repeated for a total of three washes. After washing by centrifugation, distilled water was added and the total weight was diluted to 300 g.
[0160] Next, the mixture was stirred for 3 minutes using a mixer (G5200, manufactured by Biolomix) to obtain a uniform aqueous dispersion of cellulose nanofibers having sulfate ester groups (sulfate-esterified CNF) with a concentration of 1% by mass.
[0161] The aqueous dispersion of sulfated CNF was dried for 24 hours at room temperature of 23°C to obtain solid sulfated CNF. The sulfate ester group was quantified using an infrared spectrometer (Nicolet iS 5N FT-IR, Thermo Fisher Science) and an organic elemental analyzer (EA-3100, JASCO), and the degree of sulfate ester group substitution per glucose unit of cellulose was found to be 1.6 mmol / g.
[0162] <How to prepare steel-magnesium test specimens> As shown in Figure 13, 1 g of conductive adhesive (SX-ECA-48, manufactured by Cemedine) 4 was applied to a steel plate 1, a magnesium alloy plate (AZ91) was attached as a base metal 2, and the plate was heated in an oven at 80°C for 1 hour to harden the adhesive, and then cooled to room temperature. Next, the steel plate 1, which had a hole 8 for measuring the electric potential, was placed against a support 9 to obtain a steel-magnesium test specimen with a complex gap and support shape. This test specimen was designed to reproduce gaps and complex shapes, allowing simultaneous testing.
[0163] <How to prepare steel-zinc test specimens> As shown in Figure 13, 1g of conductive adhesive (SX-ECA-48, manufactured by Cemedine) 4 was applied to a steel plate 1, a zinc plate (zinc purity 99% or more) was attached as a base metal 2, and the plate was heated in an oven at 80°C for 1 hour to harden the adhesive, and then cooled to room temperature. Next, the steel plate 1, which had holes 8 for measuring electric potential, was placed against a support to obtain a steel-zinc test specimen with complex shapes for the gap and support. This test specimen was designed to reproduce gaps and complex shapes, allowing simultaneous testing.
[0164] <Method for producing composition containing fine cellulose fibers and evaluation test method> [Example 1] 0.12 g of salt was added to 100 g of an aqueous dispersion containing sulfated cellulose nanofibers with a high degree of substitution (3.5 mmol / g) at a concentration of 1% by mass, and after complete dissolution, 24.88 g of mechanically defibrated cellulose nanofibers BiNFIs (solid content concentration 10% by mass, manufactured by Sugino Machine) was added and mixed for 5 minutes with a planetary mixer to obtain sample No. 1. 20 g of sample No. 1 was applied to a steel-magnesium test specimen having the structure shown in Figure 13, and the corrosion protection potential, magnesium wear, and corrosion protection potential after repeated drying and hydration were measured.
[0165] [Example 2] 0.15g of salt was added to 100g of an aqueous dispersion containing 1% by mass of sulfated cellulose nanofiber with a high degree of substitution (3.5mmol / g), and after complete dissolution, 49.85g of mechanically defibrated cellulose nanofiber BiNFis (WFo-10010, solids concentration 10% by mass, manufactured by Sugino Machine) was added and mixed for 5 minutes with a planetary mixer to obtain sample No. 2. 20g of sample No. 2 was applied to a steel-magnesium test specimen having the structure shown in Figure 13, and the corrosion protection potential, magnesium wear, and corrosion protection potential after repeated drying and hydration were measured.
[0166] [Example 3] 0.15 g of salt was added to 100 g of 1 mass% TEMPO oxidized CNF aqueous dispersion (manufactured by Nippon Paper Industries Co., Ltd.), and after complete dissolution, 49.85 g of mechanically defibrated cellulose nanofiber BiNFis (WFo-10010, solids concentration 10 mass%, manufactured by Sugino Machine Co., Ltd.) was added and mixed for 5 minutes with a planetary mixer to obtain sample No. 3. 20 g of sample No. 3 was applied to a steel-magnesium test specimen having the structure shown in Figure 13, and the corrosion protection potential, magnesium wear, and corrosion protection potential after repeated drying and hydration were measured.
[0167] [Example 4] 0.15g of salt was added to 100g of an aqueous dispersion containing 1% by mass of sulfated cellulose nanofiber with a high degree of substitution (3.5mmol / g), and after complete dissolution, 49.85g of mechanically defibrated cellulose nanofiber BiNFis (WFo-10010, solids concentration 10% by mass, manufactured by Sugino Machine Co., Ltd.) was added and mixed for 5 minutes with a planetary mixer to obtain sample No. 4. 20g of sample No. 4 was applied to a steel-zinc test specimen having the structure shown in Figure 13, and the corrosion protection potential, zinc wear, and corrosion protection potential after repeated drying and hydration were measured.
[0168] [Example 5] 50g of pure water was added to 50g of aqueous dispersion containing 1% by mass of sulfated cellulose nanofiber with a high degree of substitution (3.5mmol / g), to obtain 100g of sulfated CNF dispersion with a concentration of 0.5% by mass. 0.15g of salt was further added and completely dissolved, after which 49.85g of mechanically defibrated cellulose nanofiber BiNFis (WFo-10010, solid content concentration 10% by mass, manufactured by Sugino Machine Co., Ltd.) was added and mixed for 5 minutes with a planetary mixer to obtain sample No. 5. 20g of sample No. 5 was applied to a steel-zinc test specimen having the structure shown in Figure 13, and the corrosion protection potential, zinc wear, and corrosion protection potential after repeated drying and hydration were measured.
[0169] [Example 6] 5g of sodium chloride was added to 95g of an aqueous dispersion containing 1% by mass of sulfated cellulose nanofiber with a high degree of substitution (3.5mmol / g), and completely dissolved, after which 50g of mechanically defibrated cellulose nanofiber BiNFis (WFo-10010, solids concentration 10% by mass, manufactured by Sugino Machine) was added and mixed for 5 minutes with a planetary mixer to obtain sample No. 6. 20g of sample No. 6 was applied to a steel-magnesium test specimen having the structure shown in Figure 13, and the corrosion protection potential, magnesium wear, and corrosion protection potential after repeated drying and hydration were measured.
[0170] [Example 7] 5g of sodium sulfite (Wako Pure Chemical Industries, Ltd.) was added to 95g of an aqueous dispersion containing 1% by mass of sulfated cellulose nanofiber with a high degree of substitution (3.5mmol / g), and completely dissolved, after which 50g of mechanically defibrated cellulose nanofiber BiNFis (WFo-10010, solids concentration 10% by mass, Sugino Machine Co., Ltd.) was added and mixed for 5 minutes with a planetary mixer to obtain sample No. 7. 20g of sample No. 7 was applied to a steel-magnesium test specimen having the structure shown in Figure 13, and the corrosion protection potential, magnesium wear, and corrosion protection potential after repeated drying and hydration were measured.
[0171] [Example 8] To 85 g of an aqueous dispersion containing sulfated cellulose nanofibers with a high degree of substitution (3.5 mmol / g) at a concentration of 1% by mass, 15 g of sodium sulfite (Wako Pure Chemical Industries, Ltd.) was added and completely dissolved, after which 50 g of mechanically defibrated cellulose nanofibers BiNFis (WFo-10010, solids concentration 10% by mass, Sugino Machine Co., Ltd.) was added and mixed for 5 minutes with a planetary mixer to obtain sample No. 8. 20 g of sample No. 8 was applied to a steel-magnesium test specimen having the structure shown in Figure 13, and the corrosion protection potential, magnesium wear, and corrosion protection potential after repeated drying and hydration were measured.
[0172] [Example 9] 15g of sodium sulfite (Wako Pure Chemical Industries, Ltd.) was added to 85g of an aqueous dispersion containing 1% by mass of sulfated cellulose nanofiber with a low degree of substitution (1.6mmol / g), and after complete dissolution, 50g of mechanically defibrated cellulose nanofiber BiNFis (WFo-10010, solids concentration 10% by mass, Sugino Machine Co., Ltd.) was added and mixed for 5 minutes with a planetary mixer to obtain sample No. 9. 20g of sample No. 9 was applied to a steel-magnesium test specimen having the structure shown in Figure 13, and the corrosion protection potential, magnesium wear, and corrosion protection potential after repeated drying and hydration were measured.
[0173] [Example 10] As shown in Fig. 14, 10 g of sample No. 8 obtained in Example 8 was applied to a steel-magnesium test piece having the structure shown in Fig. 13, and then sterile gauze (Suzuran Co., Ltd., 12PLY) was placed as fiber 6 to cover the exposed top surface of the applied sample No. 8 and the interface between the bottom steel plate and the magnesium alloy, and 10 g of sample No. 8 was further applied on the sterile gauze. Thereafter, the corrosion protection potential, magnesium wear, and corrosion protection potential after repeated drying and hydration were measured.
[0174] [Example 11] To 95 g of an aqueous dispersion containing 1 mass% sulfated cellulose nanofibers with a high degree of substitution (3.5 mmol / g), 5 g of EMI-TFSI (1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide) (Merck) was added as an ionic liquid and completely dissolved, and then 50 g of mechanically defibrated cellulose nanofibers BiNFis (WFo-10010, solid content concentration 10 mass%, Sugino Machine) was added and mixed for 5 minutes with a planetary mixer to obtain sample No. 10. 20 g of sample No. 10 was applied to a steel-magnesium test specimen having the structure shown in Figure 13, and the corrosion protection potential, magnesium wear, and corrosion protection potential after repeated drying and hydration were measured.
[0175] [Example 12] To 85 g of an aqueous dispersion containing 1 mass% sulfated cellulose nanofibers with a high degree of substitution (3.5 mmol / g), 7.5 g of sodium sulfite (Wako Pure Chemical Industries, Ltd.) was added and completely dissolved, and then 50 g of mechanically defibrated cellulose nanofibers BiNFis (WFo-10010, solids concentration 10 mass%, Sugino Machine Co., Ltd.) and 7.5 g of ethylene glycol were added and mixed for 5 minutes with a planetary mixer to obtain sample No. 11. 20 g of sample No. 11 was applied to a steel-magnesium test specimen having the structure shown in Figure 13, and the corrosion protection potential, magnesium wear, and corrosion protection potential after repeated drying and hydration were measured.
[0176] [Comparative Example 1] 50 g of mechanically defibrated cellulose nanofiber BiNFis (WFo-10010, solids concentration 10 mass%, manufactured by Sugino Machine) was added to 100 g of pure water and mixed for 5 minutes with a planetary mixer to obtain sample No. 12. 20 g of sample No. 12 was applied to a steel-magnesium test specimen having the structure shown in Figure 13, and the corrosion protection potential, magnesium wear, and corrosion protection potential after repeated drying and hydration were measured.
[0177] [Comparative Example 2] 3.5g of water-absorbing polymer (sodium polyacrylate, commercially available product) and 0.1g of salt were added to 100g of pure water and mixed for 5 minutes with a planetary mixer to obtain sample No. 13. 20g of sample No. 13 was applied to a steel-magnesium test piece having the structure shown in Figure 13, and the corrosion protection potential, magnesium wear, and corrosion protection potential after repeated drying and hydration were measured.
[0178] Table 1 shows the evaluation results of [Example 1] to [Example 12] and [Comparative Example 1] to [Comparative Example 2].
[0179] For the evaluation in Table 1, the positive electrode was connected to a base metal plate, and the negative electrode was connected to the sample through a hole in the steel plate via a saturated copper sulfate electrode, and the potential difference was measured to evaluate whether corrosion protection was achieved. For the initial corrosion protection potential, -1000mV vs. CSE or less was rated as ◯, -1000mV vs. CSE or more but less than -100mV vs. CSE was △, and -100mV vs. CSE or more was ×.
[0180] Regarding the reproduction of the corrosion protection potential after drying / water addition, the potential difference was measured by connecting in the same manner as the initial corrosion protection potential, and -1000mV vs. CSE or less was marked as ◯, -1000mV vs. CSE or more and less than -100mV vs. CSE was marked as △, and -100mV vs. CSE or more was marked as ×. Furthermore, when the sample was not peeled off at all from each test piece, that is, when there was no interruption of the electrical circuit, it was marked as ◎. Note that even after the drying process, the ionic liquid remained in liquid form in the sample of Example 11, and ethylene glycol remained in liquid form in the sample of Example 12, but the evaluation was performed as it was.
[0181] Finally, to evaluate the inhibition of base metal depletion, the mass loss of base metal per unit area was measured 24 hours after the sample was applied, and a mark of ◯ was given when the mass loss was less than 0.1%, and a mark of △ was given when the mass loss was less than 1%.
[0182] [Table 1]
[0183] In Example 10, experiments were conducted in which (i) Sample No. 8 was placed only on one side of the sterilized gauze, and (ii) the sterilized gauze was changed to a polyester net. In both (i) and (ii), the effect of suppressing peeling and cracking was observed, but Example 10 had the best effect.
[0184] <Method for Producing Test Specimen for RFID Monitoring> As shown in Fig. 15, 1 g of a conductive adhesive (SX-ECA-48, manufactured by Cemedine) 4 was applied to the steel plate 1, and two through-holes were provided in the grooves formed in a rib shape at the bottom so that the conductive wire did not contact the steel plate 1. A magnesium alloy plate (AZ91) (Fig. 16) as the base metal 2 was pasted through the through-holes and the conductive wire was tied, and the adhesive 4 was cured at room temperature. Subsequently, the conductive wire was fixed to the bottom steel plate 1 using a fixing tape (Kapton tape). Subsequently, the conductive wire was coupled to an RFID tag (manufactured by Eagle Co., Ltd.) 10.
[0185] As the test specimen for RFID monitoring, as the base metal 2, three types of magnesium alloy plates, an uncorroded magnesium alloy plate (A in Fig. 15), a magnesium alloy plate corroded halfway (B in Fig. 15), and a completely corroded magnesium alloy plate (C in Fig. 15) (the RFID monitoring test specimens with intermediate corrosion and complete corrosion were prepared as follows) were adhered to the steel plate 1 with the conductive adhesive 4 by the above method, and further, a total of four specimens were prepared, including one in which the magnesium alloy plate was simply placed on the steel plate without using the conductive adhesive (D in Fig. 15).
[0186] · Corrosion treatment of magnesium alloy plate The magnesium alloy plate was fixed to the steel plate with a clip so that electrical conduction occurred between the metals, and corrosion treatment was performed by immersing and leaving it for 24 hours and 96 hours in an environment of 5 mass% brine, thereby obtaining RFID monitoring test specimens with intermediate corrosion (B in Fig. 15) and complete corrosion (C in Fig. 15).
[0187] · RFID monitoring An RFID monitoring evaluation was performed by reading the state of an RFID monitoring specimen (A in FIG. 15) in which a magnesium alloy plate as a base metal 2 not yet subjected to corrosion treatment was bonded to a steel plate 1 with a conductive adhesive 4 using an RFID reader (manufactured by DENSO WAVE Inc.) 11. As a result, the RFID monitoring specimen (A in FIG. 15) was determined to be in a "conductive state." Therefore, it was confirmed that the magnesium alloy of the base metal 2 of the RFID monitoring specimen (A in FIG. 15) had not fallen off or been completely consumed, and was contributing to the anti-corrosion function.
[0188] Next, an RFID monitoring evaluation was performed by reading the state of the RFID monitoring test specimen (B in FIG. 15) 24 hours after the corrosion treatment using an RFID reader (manufactured by DENSO WAVE Inc.) 11. As a result, the RFID monitoring test specimen (A in FIG. 15) was determined to be in a "conductive state."
[0189] When the steel plate 1 of the RFID monitoring test specimen (B in FIG. 15) that had become conductive was checked, no falling off of the magnesium alloy of the base metal 2 was observed, and only slight attrition was observed.
[0190] Meanwhile, an RFID monitoring evaluation was performed by reading the condition of the RFID monitoring test specimen (C in Fig. 15) 96 hours after the corrosion treatment with an RFID reader (manufactured by DENSO WAVE Inc.) 11. As a result, the RFID monitoring test specimen (C in Fig. 15) was judged to be in a "non-conductive state." When the steel plate 1 of the RFID monitoring test specimen (C in Fig. 15) that had become non-conductive was checked, it was confirmed that the magnesium alloy as the base metal 2 had been significantly depleted and the sacrificial corrosion protection function could not be fully exerted.
[0191] In addition, when an RFID monitoring evaluation was performed by reading the state of the RFID monitoring test specimen (D in Fig. 15) in which the magnesium alloy plate as the base metal 2 was simply placed stationary using an RFID reader (made by DENSO WAVE Inc.) 11, it was determined to be in a "no conduction state." This confirmed that even in the state in which the steel plate 1 and the magnesium alloy as the base metal 2 were peeled off, the sacrificial corrosion protection function could not be fully exerted.
[0192] <Corrosion verification experiment> In this experiment, a method was adopted to grasp the planar distribution of corroded and protected areas over time by actually measuring the magnitude and direction of the current associated with corrosion protection (the direction of current flowing in and out of the electrodes) (commonly known as the coupling current method).
[0193] The test specimen was constructed as shown in Figs. 17-20. First, a plurality of steel materials 1 serving as electrodes were penetrated into the resin 12, which was an insulator, and CH1 and CH2 were protruded from the outer surface (Figs. 17 and 18). Next, a plastic tape 13 having a thickness of 1 mm was placed around the outer periphery of CH3 and after, so as to surround it in three directions (surrounding CHs after CH3) (Fig. 19). Then, an acrylic plate 14 was placed on top of the plastic tape 13, and the four corners of the acrylic plate 14 were clamped with a vice to reproduce the gap (Fig. 20). Next, a magnesium alloy 2 (12 mm x 15 mm x 2 mm) was attached to the electrodes of CH1 and CH2 using a conductive adhesive (Fig. 20), and the water-containing fluid of sample No. 8 was applied from its top surface to the inside of the gap. In the test specimen thus constructed, the magnitude and direction of the current when the magnesium alloy 2 attached to CH1 and CH2 was used to protect the electrode surface (steel material 1) inside the gap was measured by connecting the electrode part of each CH to a 32CH data logger 15 with a lead wire and simultaneously shorting it (short-circuiting enables corrosion protection) (Fig. 21), and scanning each electrode every 10 seconds. Fig. 22 shows a photograph of the corrosion confirmation experiment.
[0194] Figure 23 shows the measurement results of the current value of the steel material and magnesium alloy when the corrosion protection system was applied to the test specimen. The magnesium alloy corrodes by performing corrosion protection (negative (-) current value: corrosion current). In the steel material, a current value of the same magnitude but in the opposite direction to that of the magnesium alloy is measured according to the law of conservation of charge (positive (+) current value: corrosion protection current). At the beginning of the measurement, the current value continues to decrease because a large amount of oxygen contained in the water-containing fluid is consumed inside the gap due to corrosion protection, but when the oxygen inside the gap is consumed, the current value settles at around 0. If water is injected during the measurement, the injected water does not contain as much oxygen as the initial water-containing fluid, so the rising current value is small and the current value reaches around 0 quickly. This suggests that the magnesium alloy does not wear out early but can be maintained for a relatively long life. In the case of the corrosion confirmation experiment, the life of the magnesium alloy was calculated to be more than 50 years from the current value.
[0195] Next, in order to confirm the effect of sodium sulfite (Na2SO3) as an electrolyte, an experiment was carried out in the same manner as the above corrosion confirmation test, except that sodium sulfite was omitted from the aqueous fluid as an electrolyte.
[0196] The results are shown in Figure 24. The graphs for steel + Na2SO3 and Mg alloy + Na2SO3 in Figure 24 are reprints of the graphs in Figure 23. Figure 24 shows that in the case of a water-containing fluid that does not contain sodium sulfite, the current value is large both initially and when water is poured in, and the decay rate from the initial current value is also slow, and therefore the life of the magnesium alloy is shortened.
[0197] Figure 25 shows photographs that show the difference in corrosion conditions inside a crevice when the corrosion prevention system of the present invention is applied and when it is not applied, one week after 0.1 mass % salt water is injected into the crevice.
[0198] From FIG. 25, it is clear that the corrosion prevention system of the present invention can effectively prevent corrosion inside gaps.
[0199] FIG. 26 is a graph showing the change in current value versus time for a steel material when the corrosion prevention system of the present invention is not used.
[0200] From Figure 26, it can be seen that when the corrosion protection system of the present invention is not used, the current value does not converge as it does when the corrosion protection system of the present invention is used, and therefore corrosion of the steel continues unless the moisture evaporates. [Explanation of symbols]
[0201] 1. Steel material (steel plate) 2. Base metals (magnesium alloy plate, zinc plate, aluminum alloy plate) 3. Hydrous fluid 4.Conductive adhesive 5. Exterior materials 6. Fiber (gauze) 7. Water-absorbing and evaporative paper 8. Hole for potential measurement 9. Prop 10. RFID tags 11. RFID Reader 12. Resin 13. Plastic Tape 14. Acrylic board 15.32CH data logger 16. Base substrate 17.Antenna board 18.First electrode 19.Second electrode 20. IC chip module 21. First detection terminal 22. Second detection terminal 23. First side of the base board 24. Second side of the base board 25. Clip 26.Continuity determination device 27. Lead Wire 28. Anchor bolts 29. Nut part 30. Small gaps 31. Washer S. Rust S'. Existing rust layer
Claims
1. A corrosion protection system for steel comprising a steel material, a base metal having a lower natural potential than the steel material, fine cellulose fibers having an average fiber width of 1 nm or more and 1000 nm or less, and a hydrous fluid containing an electrolyte, wherein the steel material and the base metal are joined in an electrically conductive manner, the hydrous fluid is in contact with the steel material surface and the base metal surface, and supplies base metal ions generated from the base metal surface to the steel material surface.
2. The corrosion protection system for steel materials according to claim 1 , wherein the content of the fine cellulose fibers in the aqueous fluid is 1 mass % or more with respect to the total mass of the aqueous fluid.
3. The corrosion protection system for steel materials according to claim 1 or 2, wherein the steel material surface is a steel material surface in a gap between steel materials.
4. 3. The corrosion protection system for steel material according to claim 1 or 2, wherein the fine cellulose fibers contain anion-modified fine cellulose fibers in an amount of 0.1 mass% or more and 50 mass% or less of anion-modified fine cellulose fibers relative to the total mass of solids in the aqueous fluid, the average fiber width of the anion-modified fine cellulose fibers is 1 nm or more and 1000 nm or less, and the amount of anion-modified group introduced into the anion-modified fine cellulose fibers is 0.3 mmol / g or more and 4.0 mmol / g or less.
5. 3. The corrosion protection system for steel according to claim 1 or 2, wherein the aqueous fluid contains at least one electrolyte in an amount of 1.0 mass % or more relative to the total mass of solids in the aqueous fluid.
6. The corrosion protection system for steel according to claim 5 , wherein at least one of the electrolytes functions as a reducing agent.
7. 5. The corrosion protection system for steel according to claim 4, wherein the anion-modified fine cellulose fibers are sulfate-esterified fine cellulose fibers having the substituent group represented by formula (1). [Formula 1] (wherein n is an integer from 1 to 3; M n+ is an n-valent cation, and the wavy lines are the bonding sites to other atoms.)
8. The corrosion protection system for steel materials according to claim 1 or 2, wherein the water-containing fluid further contains fibers having a fiber diameter of 5 μm or more and 300 μm or less.
9. The corrosion protection system for steel according to claim 1 or 2, further comprising an exterior material stretched over a surface of the steel so as to cover the base metal and the water-containing fluid.
10. A corrosion protection monitoring system comprising the corrosion protection system for steel material described in claim 1 and an RFID tag having a tamper function, wherein the RFID tag is electrically connected to both the steel material and the base metal in the corrosion protection system for steel material, and the depletion and peeling of the base metal are read by an RFID reader.
11. 11. The corrosion protection system or corrosion protection monitoring system for steel materials according to claim 1 or 10, wherein the water-containing fluid is in a dry state.
12. 11. A water-containing fluid for use in the corrosion protection system or corrosion protection monitoring system for steel materials according to claim 1 or 10, comprising water, fine cellulose fibers, and an electrolyte.
13. A dry body for use in a corrosion prevention system or a corrosion prevention monitoring system for a steel material according to claim 11, comprising fine cellulose fibers and an electrolyte.
14. A method for constructing a corrosion protection system or corrosion protection monitoring system for steel as described in claim 1 or 10, comprising joining a rust-bearing steel material and a base metal having a lower natural potential than the steel material in an electrically conductive manner, and arranging an aqueous fluid so as to be in contact with the steel material surface and the base metal surface and so as to supply base metal ions generated from the base metal surface to the steel material surface, wherein the rust is not removed.
Citation Information
Patent Citations
Coating method
JP2005074272A
Corrosion control method
JP2011206754A
Anticorrosion method and anticorrosion device
JP2016040403A
Electric protection structure of reinforced concrete structure
JP2016169407A
Corrosion proof structure of steel structure and installation method thereof
JP2021055147A