Oxidation prevention cover and heating treatment method

The use of a porous carbon material cover for non-oxide heat treatment addresses coating complexities and inert gas requirements, ensuring efficient and cost-effective oxidation prevention during heat treatment.

JP2024133985APending Publication Date: 2024-10-03TOMOEGAWA CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023044039
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional methods for heat-treating non-oxide materials face challenges in coating complex structures with carbonaceous membranes, risk of carbon fiber mixing, and require inert gas atmospheres, which are costly and time-consuming.

Method used

An oxidation-preventing cover made of porous carbon material with specific properties is used to cover non-oxide objects during heat treatment, allowing air permeability and preventing oxidation without inert gases.

Benefits of technology

Enables simple and effective heat treatment of non-oxide materials by maintaining low oxygen concentrations within the treatment environment, reducing costs and time, and avoiding carbon fiber mixing issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133985000001_ABST
    Figure 2024133985000001_ABST
Patent Text Reader

Abstract

To provide an oxidation prevention cover and a heating treatment method which easily enable the heating treatment of a non-oxide without requiring use of an inert gas.SOLUTION: There is provided an oxidation prevention cover 12 for preventing oxidation of a non-oxide when a non-oxide-containing object 11 is subjected to heating treatment. The oxidation prevention cover 12 is made of a porous carbon material 13 having gas permeability at least in a thickness direction and can cover a circumference of the object 11 during the heat treatment of the object 11, and the porous carbon material 13 has a specific surface area of 0.05 m2 / g or more, a carbon purity of 95 wt% or more and density uniformity with a standard deviation of bulk density of 0.1 g / cm3 or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an oxidation-preventing cover and a heat treatment method. [Background technology]

[0002] When heat-treating an object, oxygen in the air can cause the object to deteriorate. However, when heat-treating an object under an atmosphere using an inert gas such as nitrogen, the inert gas and equipment such as an atmospheric furnace that uses the gas are required, which incurs significant costs.

[0003] For example, Patent Document 1 describes a method in which a non-oxide or a refractory material containing a non-oxide as part of its composition is coated with a carbonaceous film in advance and then fired. Examples of the carbonaceous film include woven fabric, non-woven fabric, and film, and examples of the coating method include adhesion or wrapping. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 5-17238 Summary of the Invention [Problem to be solved by the invention]

[0005] In the conventional technology, the method of coating an object by attaching or wrapping a carbonaceous film has problems such as difficulty in coating complex structures, the risk of carbon fibers constituting the carbonaceous film being mixed into non-oxides, and the laborious task of removing the carbonaceous film after heat treatment.

[0006] An object of the present invention is to provide an oxidation-preventing cover and a heat treatment method that enable heat treatment of non-oxides easily without using an inert gas. [Means for solving the problem]

[0007] A first aspect is an oxidation prevention cover for preventing oxidation of a non-oxide when a target containing a non-oxide is heat-treated, the oxidation prevention cover being made of a porous carbon material having air permeability at least in a thickness direction and capable of covering a periphery of the target during heat treatment of the target, the porous carbon material having a specific surface area of ​​0.05 m 2 / g or more, carbon purity is 95wt% or more, and density uniformity is 0.1g / cm as the standard deviation of bulk density. 3 The present invention is characterized in that:

[0008] In a second aspect, in the first aspect, the porous carbon material has an air permeability of 0.1 to 50 cm 3 / cm 2 s, observation area 360μm 2 The total length of the boundary between carbon and voids observed on the cut surface is 30 μm or more, and the porosity is 20 to 80%. A third aspect is characterized in that in the first or second aspect, the porous carbon material is made of carbon particles or carbon fibers, and the carbon particles or carbon fibers are bound together. A fourth aspect is any one of the first to third aspects, characterized in that the oxidation prevention cover has a concave internal space capable of accommodating the object.

[0009] A fifth aspect is a heat treatment method for heat treating an object using an anti-oxidation cover of any one of claims 1 to 4, characterized in that the anti-oxidation cover is positioned so as not to come into contact with the object during heat treatment of the object. A sixth aspect is a heat treatment method for heat-treating an object using an anti-oxidation cover of any one of claims 1 to 4, characterized in that a recess capable of accommodating the object is formed, the object is filled into the recess, and then the object is heat-treated.

[0010] A seventh aspect is characterized in that the object is heat-treated in the atmosphere using any one of the oxidation-preventing covers from the first to fourth aspects. The eighth aspect is any one of the fifth to seventh aspects, characterized in that the object is a solid or paste-like object, and the heat treatment is firing or sintering. Effect of the Invention

[0011] According to the present invention, it is possible to provide an oxidation-preventing cover and a heat treatment method that enable heat treatment of non-oxides simply and easily without using an inert gas. [Brief description of the drawings]

[0012] [Figure 1] 1A to 1C are explanatory diagrams showing an oxidation prevention cover and a heat treatment method according to an embodiment. [Diagram 2] FIG. 2 is an explanatory diagram showing an oxidation prevention cover and a heat treatment method according to Example 1. [Diagram 3] FIG. 11 is an explanatory diagram showing an oxidation prevention cover and a heat treatment method according to Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, the present invention will be described based on preferred embodiments.

[0014] An example of an oxidation-preventing cover and a heat treatment method according to the embodiment is shown in Fig. 1. The oxidation-preventing cover 12 according to the embodiment is used to prevent oxidation of non-oxides when a target object 11 containing non-oxides is heat-treated.

[0015] The oxidation-preventive cover 12 is made of a porous carbon material 13 that is air permeable at least in the thickness direction, and is capable of covering the periphery of the object 11 during heat treatment of the object 11. The object 11 is accommodated in an internal space 15 defined by the oxidation-preventive cover 12. The oxidation-preventive cover 12 preferably has a concave internal space 15 capable of accommodating the object 11.

[0016] The method of heat treatment is not particularly limited, and can be performed, for example, by placing the object 11 and the oxidation-preventing cover 12 in a heat treatment device 10 such as an oven. A heat treatment atmosphere is formed in the heat treatment device 10. As shown in Figs. 2 and 3 described later, it is also possible to perform heat treatment by directly applying a heat source 19 such as a burner or plasma to the oxidation-preventing cover 12 containing the object 11.

[0017] The object 11 is not particularly limited as long as it contains a non-oxide, and may be an inorganic or organic substance. Examples of components contained in the object 11 include metals, inorganic compounds, organic compounds, and mixtures containing two or more of these.

[0018] When the target object 11 includes a metal, examples of the metal include base metals and precious metals, and it is preferable that the target object 11 includes a metal that is stable in air at room temperature and oxidizes in air at high temperatures. Specific examples include, but are not limited to, copper (Cu), iron (Fe), nickel (Ni), chromium (Cr), zirconium (Zr), titanium (Ti), magnesium (Mg), silver (Ag), zinc (Zn), tin (Sn), aluminum (Al), or an alloy containing one or more of these metals.

[0019] The object 11 may be composed of only non-oxides, or may be a mixture of non-oxides and oxides. 2 O), metal oxides, etc. Non-metallic non-oxides include halides such as chlorides, nitrides, carbides, sulfides, borates, carbonates, nitrates, silicates, phosphates, sulfates, etc. Non-oxide types include metals such as copper, zinc, silver, aluminum, and stainless steel (SUS), and ceramics such as silicon nitride.

[0020] The oxidation-preventing cover 12 is used to prevent an oxidation reaction of non-oxides contained in the object 11 during heat treatment. The oxidation reaction of the object 11 may be a reaction in which a non-oxide becomes an oxide, or a reaction in which a non-oxide reacts with oxygen to produce another non-oxide.

[0021] The shape of the object 11 is not particularly limited, and examples of the shape include powder, fiber, sphere, plate, column, flake, lump, and a mixture of two or more of these. The object 11 is preferably a solid, but the object 11 may contain a liquid and / or gas. Examples of the liquid that may be contained in the object 11 include water, an organic solvent, and the like.

[0022] The object 11 may be a solid or a paste, and the solid or paste-like object 11 may contain liquid and / or gas. For example, a liquid may be added to the powder and / or granules of the object 11 to make it into a paste, and the paste may be molded into a desired shape like clay. The object 11 may be molded and then housed in the oxidation-preventive cover 12, or the object 11 may be molded into the shape of the recess 17 by filling the recess 17 of the oxidation-preventive cover 12 with the object 11.

[0023] The heat treatment may be intended to cause a change in the object 11. The change in the object 11 may be a chemical change or a physical change, such as calcination, sintering, drying, thermal curing, thermal decomposition, crosslinking, condensation, etc. The purpose of the heat treatment may include at least calcination or sintering, during which drying, thermal decomposition, etc. may occur. Although an oxidation reaction of the object 11 should be suppressed, other chemical reactions can be the purpose of the heat treatment as desired.

[0024] Since the porous carbon material 13 has voids 14, atmospheric gas can flow between the internal space 15 and the external space 16 of the oxidation prevention cover 12. The flow direction of the atmospheric gas is not particularly limited, and may be a direction from the internal space 15 to the external space 16, or a direction from the external space 16 to the internal space 15. The flow direction may be determined spontaneously depending on a pressure difference, convection, or the like, or may be artificially controlled by using a blower such as a fan.

[0025] The object 11 may be heat-treated in the atmosphere. When the oxidation-preventive cover 12 housing the object 11 is directly heated, outside air may be present in the external space 16. When the external space 16 is a closed space, it may be filled with outside air before being closed. Outside air may be allowed to circulate through the external space 16 during the heat treatment.

[0026] When the heat treatment atmosphere of the heat treatment apparatus 10 has a certain range surrounded by a housing or the like, the external space 16 is a region of the heat treatment atmosphere that is partitioned from the internal space 15 via the oxidation-preventive cover 12. It is also possible to perform heat treatment in a state where the oxidation-preventive cover 12 containing the object 11 is not surrounded by a housing or the like. In this case, the external space 16 refers to the space around the oxidation-preventive cover 12.

[0027] The atmospheric gas in the external space 16 may include air. For example, the external space 16 may include oxygen (O 2 ), nitrogen (N 2 The atmospheric gas in the external space 16 may contain oxygen (O2), argon (Ar), etc. The normal composition of the atmosphere is, for example, about 21% oxygen, about 78% nitrogen, and about 1% argon, but the composition of the atmospheric gas in the external space 16 may be different from the composition of the atmosphere. The oxygen concentration in the external space 16 may be, for example, 10 to 25% by volume.

[0028] The oxidation-preventive cover 12 may cover the entire periphery of the object 11, or may cover only a portion of the periphery of the object 11. In the area of ​​the object 11 that is not covered by the oxidation-preventive cover 12, the object 11 is preferably covered by an airtight partition such as the installation surface 18.

[0029] The shape of the oxidation prevention cover 12 is not particularly limited, but may have a recess 17 capable of accommodating the target object 11. The number of recesses 17 is not particularly limited, and may be one or more. When the target object 11 is placed on a predetermined installation surface 18, the oxidation prevention cover 12 may come into contact with the installation surface 18 to partition the internal space 15 from the external space 16.

[0030] The installation surface 18 of the object 11 may be part of a wall surface, a floor surface, or the like of the heat treatment device 10, or may be part of a substrate or the like that is separable from the heat treatment device 10. When the oxidation-preventing cover 12 housing the object 11 is directly heated from the heat source 19, the upper side of the installation surface 18 may be open to the outside air, although not particularly shown. When the oxidation-preventing cover 12 contacts the installation surface 18, it is not necessary to place the oxidation-preventing cover 12 between the object 11 and the installation surface 18.

[0031] It is preferable that the pressure difference between the internal space 15 and the external space 16 is small. If the pressure in the internal space 15 is too high compared to the pressure in the external space 16, the pressure in the internal space 15 may cause the oxidation prevention cover 12 to come off from the periphery of the target object 11. If the pressure in the internal space 15 is too low compared to the pressure in the external space 16, a large amount of oxygen-containing gas may flow in from the external space 16, causing the oxygen concentration in the internal space 15 to increase.

[0032] When the oxidation-preventing cover 12 comes into contact with oxygen during the heat treatment, a carbon oxidation reaction occurs, and the carbon material in the oxidation-preventing cover 12 is oxidized to produce carbon dioxide (CO 2 ) is generated. As a result, the oxygen concentration in the atmosphere around the oxidation-preventing cover 12 decreases. By installing the oxidation-preventing cover 12 around the object 11, the oxygen concentration in the internal space 15 during the heat treatment can be reduced. As a result, the oxidation of the object 11 during the heat treatment can be prevented.

[0033] The temperature at which carbon reacts with oxygen is, for example, about 450° C. or higher. A catalyst may be impregnated or supported in the porous carbon material 13 of the oxidation-resistant cover 12 to reduce the temperature at which carbon reacts with oxygen.

[0034] In the heat treatment using the oxidation-preventing cover 12 of the embodiment, it is preferable that the temperature reaches the temperature range where carbon reacts with oxygen at least in a part of the time period. In the pre-treatment or post-treatment of the heat treatment, treatment such as preheating, drying, and cooling may be performed in a temperature range lower than the temperature where carbon reacts with oxygen.

[0035] The oxidation reaction of carbon can occur anywhere in the gap 14 of the oxidation prevention cover 12, on the internal space 15 side, or on the external space 16 side. Since the volume of the internal space 15 is limited, when the oxygen contained in the internal space 15 is consumed, the oxygen concentration in the internal space 15 can be made substantially zero or close to zero. It is preferable that the volume of the internal space 15 is as small as possible as long as it can accommodate the target object 11.

[0036] The oxidation prevention cover 12 of the embodiment has air permeability because it is formed from the porous carbon material 13. The air permeability of the oxidation prevention cover 12 allows hot air from the external space 16 to flow into the internal space 15. In addition, even if gas is generated or expands in the internal space 15 during the heat treatment of the target object 11, an increase in the pressure in the internal space 15 can be suppressed.

[0037] The porous carbon material 13 may be an aggregate formed from carbon fragments such as carbon particles and / or carbon fibers, or may be a porous aggregate of carbon material. When the carbon fragments are carbon fibers, they may be short or long fibers. For example, the porous carbon material 13 may be in the form of a woven fabric, a nonwoven fabric, or the like.

[0038] When the aspect ratio of a carbon fragment is the ratio of the large diameter to the small diameter, the aspect ratio of a carbon particle is 3 or less, and the aspect ratio of a carbon fiber is greater than 3. In this case, the smallest value of the distance between two parallel lines tangent to the outline of the carbon fragment that can be observed from a direction perpendicular to the horizontal plane when the carbon fragment is placed most stably on a horizontal plane is taken as the smallest value, and the largest value as the large diameter.

[0039] The size of the carbon fragments is not particularly limited, but examples of the particle size include a particle size of about 0.1 to 50 μm or about 1 to 10 μm. Coarse particles having a larger particle size and fine particles having a smaller particle size may be included. If necessary, the particle size distribution of the carbon fragments as the raw material may be adjusted by sieving or the like. Carbon fragments having a larger particle size and carbon fragments having a smaller particle size may be mixed to adjust the particle size distribution to have two or more peaks, or may be adjusted to have one peak.

[0040] The method for producing the porous carbon material 13 is not particularly limited, and examples thereof include the above-mentioned method of binding carbon fragments and a method of carbonizing an aggregate of organic fragments. The organic fragments are not particularly limited, and may be synthetic materials such as synthetic resin particles and synthetic fibers, or natural materials such as sawdust and rice husks. Even without using carbon fragments, the porous carbon material 13 can be obtained by, for example, a method of carbonizing an organic foam containing open cells.

[0041] The mechanism by which heat moves from the outside of the oxidation-preventing cover 12 to the object 11 is not particularly limited, and may be heat conduction, convection, radiation, or a combination of these. For example, heat may be released toward the internal space 15 by energy obtained by absorbing infrared rays on the outer surface of the oxidation-preventing cover 12.

[0042] Examples of outgassing that may be emitted from the object 11 in the internal space 15 include water vapor, carbon dioxide, solvent vapor, and the like, but are not limited thereto. Depending on the components contained in the object 11, hydrogen (H 2 ), ammonia (NH 3 ), hydrogen sulfide (H 2 S), sulfur dioxide (SO 2 ) or any other gas may be generated.

[0043] Even if outgassing is not generated in the internal space 15, as described above, the target object 11 can be heated more efficiently by the ambient gas heated as hot air flowing from the external space 16 into the internal space 15.

[0044] The oxidation reaction of carbon is likely to occur inside the voids 14 of the oxidation-preventive cover 12 because the surface area of ​​the porous carbon material 13 facing the voids 14 is large compared to the volume of the voids 14. When the atmospheric gas in the external space 16 flows into the internal space 15 through the voids 14, it is preferable that the oxygen in the atmospheric gas reacts with carbon so that the oxygen concentration becomes substantially zero or approaches zero.

[0045] The specific surface area of ​​the porous carbon material 13 is 0.05 m 2 / g or more is preferable, and 0.3m 2 / g or more is more preferable, and 0.9m 2 / g or more is more preferable.

[0046] The method for measuring the specific surface area is not particularly limited, but examples thereof include gas adsorption measurement.

[0047] The larger the specific surface area, the better the effect, provided that the air permeability of the porous carbon material 13 is not impaired. By using carbon particles having a smaller particle size or carbon fibers having a smaller fiber diameter as the material, it is possible to obtain a porous carbon material 13 having an even larger specific surface area.

[0048] The carbon purity of the porous carbon material 13 is preferably 95 wt % or more, more preferably 99% or more, and even more preferably 99.9% or more.

[0049] The carbon purity can be measured, for example, by the following method. (1) A sample of the porous carbon material is prepared and weighed. (2) The sample is combusted and the carbon dioxide produced is quantitatively analyzed using gas chromatography. (3) CO obtained from the analysis results 2 Based on the amount of substance, the mass of carbon contained in the burned sample (i.e., the mass of pure carbon) is calculated. (4) The ratio (percentage) of the "mass of pure carbon" to the "sample mass before combustion" is defined as the "carbon purity (wt%)" and this value is evaluated.

[0050] The density uniformity of the porous carbon material 13 is 0.1 g / cm as the standard deviation of the bulk density. 3 Less than 0.08 g / cm is preferred. 3 Less than 0.05 g / cm is more preferable. 3 Even more preferred is the following:

[0051] The density uniformity can be measured, for example, by the following method. (1) Prepare one sample of a porous carbon material and cut out n pieces of equal volume (hereinafter, the sample cut into n pieces will be referred to as "small pieces"). (2) Weigh each piece and calculate the bulk density of each piece by “mass / volume.” (3) From the bulk density value of each small piece obtained, the degree of variation (standard deviation σ) of the small piece sample is calculated. (4) The obtained standard deviation σ is evaluated as the “density uniformity” of the sample.

[0052] The number n of small pieces in the evaluation of density uniformity may be, for example, n = 10. Furthermore, the calculation of the standard deviation can be performed based on JIS Z8103:2019 (measurement terminology).

[0053] The air permeability of the porous carbon material 13 is 0.1 to 50 cm 3 / cm 2 s is preferred, 1-10cm 3 / cm 2 s is more preferable, 3-5cm 3 / cm 2 ·s is even more preferred.

[0054] If the air permeability is less than the lower limit of the above-mentioned range, there is a risk that the temperature rise in the internal space 15 is hindered or that the internal pressure is increased. If the air permeability is more than the upper limit of the above-mentioned range, the oxygen in the gas flowing in from the external space 16 is not sufficiently removed, which may result in oxidation of the target object 11.

[0055] The method for measuring the air permeability is not particularly limited, but may be, for example, Method A (Fragile method) of JIS L 1096 (Fabric testing methods for woven and knitted fabrics).

[0056] The porous carbon material 13 has an observation area of ​​360 μm 2 The sum of the lengths of the boundary lines between carbon and voids observed on the cut surface (hereinafter sometimes referred to as "boundary line length per observed area") is preferably 30 μm or more, more preferably 100 μm or more, and even more preferably 360 μm or more.

[0057] If the "border line length per observation area" is less than the above-mentioned lower limit, the specific surface area of ​​the porous carbon material 13 becomes too small, and oxygen in the gas flowing in from the external space 16 is not sufficiently removed, which may result in oxidation of the object 11.

[0058] The "boundary line length per observation area" is preferably measured by observing a cut surface of the porous carbon material 13 with a scanning electron microscope (SEM) and analyzing the image obtained. Specifically, an observation area of ​​a predetermined area is extracted to separate the carbon area and the void area, the boundary between the carbon area and the void area is identified, and the lengths of the boundary lines included in the observation area are totaled to obtain the measurement. In the above-mentioned numerical range, the area of ​​the observation area is set to 360 μm 2 It states that:

[0059] A method for extracting the observation area from the image of the cut surface is preferably a random method. For example, multiple observation areas may be extracted from the image, and the average length of the boundary lines included in each observation area may be used as the numerical value of the "boundary line length per observation area." Observation areas may be extracted from multiple locations corresponding to each part of the oxidation-preventing cover 12.

[0060] It is preferable to obtain an average "boundary line length per observation area" value by cutting a sample of the oxidation-resistant cover 12 so as to obtain a cross-sectional area that is sufficiently larger than the area of ​​the observation area, and appropriately sampling the observation area within the cross-sectional area.

[0061] The shape of the observation region is not particularly limited, and may be, for example, a square, a circle, or a rectangle, for example, 18 μm × 20 μm. 2 If different, the area of ​​the observation region is A (μm 2 ), and the length of the boundary line is B (μm), it can be calculated as "boundary line length per observation area" = (B / A) × 360.

[0062] The steps of separating the carbon region and the void region from the observation area, identifying the boundary between the carbon region and the void region, and adding up the length of the boundary lines included in the observation area can be performed by known methods for image analysis of cut surfaces.

[0063] When the porous carbon material 13 is composed of an aggregate of carbon fragments such as carbon particles and / or carbon fibers, the carbon region includes a region that is a cross section of the carbon fragments, a region where the carbon fragments are in contact or bonded together, a region where no void is recognized between overlapping carbon fragments, etc. The void region is a region other than the carbon region. The carbon region and the void region can be distinguished by, for example, a binarization process.

[0064] As a specific example, low brightness pixels in an image may be carbon regions, and high brightness pixels may be void regions. The brightness threshold used to distinguish between carbon regions and void regions can be set appropriately. Since normal carbon exhibits a low brightness color such as black, it is easy to distinguish between carbon regions and void regions even in observation in the visible light region. The wavelength of light used to capture the image is not limited to all or a part of the visible light region, and may include the infrared light region and the ultraviolet light region.

[0065] A region in an image where many consecutive pixels that are considered to be carbon regions exist may be considered a carbon region, and a region where many consecutive pixels that are considered to be void regions exist may be considered a void region. A region consisting of a small number of pixels may be included in a surrounding region as noise. For example, a minute carbon region may be included in a surrounding void region, or a minute void region may be included in a surrounding carbon region. The number of pixels and the shape of the region used to distinguish a minute region can be set appropriately.

[0066] For example, when the porous carbon material 13 is made of carbon particles, the larger the diameter of the carbon particles, the smaller the numerical value of the "boundary line length per observation area" tends to be, and the smaller the diameter of the carbon particles, the larger the numerical value of the "boundary line length per observation area" tends to be.

[0067] For example, if we assume that the circular cross-sections of spherical carbon particles are closely packed in a hexagonal lattice, the specific surface area S (m 2 / g) is the density ρ(g / cm 3 ) and from the ratio of the surface area to the mass of a sphere with diameter D (μm), S = 6 / (D × ρ).

[0068] In addition, the "boundary length per observation area" is the area of ​​the observation area A = √3 × D in a unit lattice of two circular cross sections when the circular cross sections with diameter D (μm) are arranged in a close-packed manner. 2 Since the boundary line length B = 2πD, the "boundary line length per observation area" can be calculated as ≒ 1305 / D. In an actual cut surface, the particle shape is not necessarily spherical, so the boundary line length may be greater. Conversely, even if the particle shape is spherical, a great circle (a cut surface that includes the center of a sphere) does not necessarily appear on the cut surface, so the boundary line length may be smaller.

[0069] Similarly, when the porous carbon material 13 is made of carbon fiber, the larger the diameter or length of the carbon fiber, the smaller the numerical value of the "boundary line length per observation area" tends to be, and the smaller the diameter or length of the carbon fiber, the larger the numerical value of the "boundary line length per observation area" tends to be.

[0070] For example, if we assume that the circular cross sections of cylindrical carbon fibers (planes perpendicular to the length of the carbon fibers) are closely packed, the specific surface area S (m 2 / g) is the density ρ(g / cm 3 ), the ratio of the surface area to the mass of a cylinder with diameter D (μm) is given as S = 4 / (D × ρ). As with the spherical carbon particles mentioned above, the "boundary length per observation area" can be calculated as a formula that is inversely proportional to the diameter D.

[0071] As shown in the above example, since the specific surface area and the "boundary line length per observation area" are both expressed by equations that are inversely proportional to the diameter D, the magnitude relationship of the specific surface area can be inferred from the value of the "boundary line length per observation area."

[0072] More generally, in a collection of carbon fragments of arbitrary dimensions, not necessarily uniform, when the specific surface area and "boundary line length per observation area" are each of predetermined values, it is possible to consider the case in which the dimensions of all the carbon fragments are equally enlarged or reduced by a factor k in the three axes directions x, y, and z (dimensional change ratio k).

[0073] For the above dimensional change ratio k, the surface area is k 2 times, mass is k 3 Since the specific surface area is 1 / k times larger, the area of ​​the observation region is k 2 Since the specific surface area is multiplied by 1 / k and the boundary line length is k times larger, the "boundary line length per observation area" is 1 / k. Since both the specific surface area and the "boundary line length per observation area" are inversely proportional to the dimensional change ratio k, the magnitude relationship of the specific surface area can be inferred from the value of the "boundary line length per observation area."

[0074] The porosity of the porous carbon material 13 is preferably 20 to 80%, more preferably 35 to 65%, and even more preferably 40 to 60%. If the porosity is less than the lower limit, gas will not easily move between the internal space 15 and the external space 16, which may hinder an increase in temperature of the internal space 15 or may cause an increase in internal pressure due to gas generated from the object 11. If the porosity is more than the upper limit, it may become difficult to maintain the shape of the porous carbon material 13.

[0075] The porosity of the porous carbon material 13 is expressed as follows: the volume of the entire porous carbon material 13 including the voids 14 is V, and the volume of the voids 14 is v 1 , the volume excluding the void 14 is v 2 =Vv 1 Then, v 1 It is expressed as / V. When expressed as a percentage, (v 1The porosity (%) can be calculated by multiplying the void volume by 100 (%).

[0076] The method for measuring the volume V of the entire porous carbon material 13 is not particularly limited, but examples include a method of calculating from the general shape of the porous carbon material 13, a method of measuring the volume of a sample that blocks the voids 14, and a method of immersing the sample in a liquid such as mercury that does not easily enter the voids 14.

[0077] When the true density ρ of the porous carbon material 13 is known, the volume (v ) excluding the voids 14 can be calculated based on the ratio of the mass M of the porous carbon material 13 to the true density ρ. 2 =Vv 1 ) can be obtained. Vv 1 =M / ρ, the porosity (v 1 / V) = 1-M / (V × ρ).

[0078] When the object 11 is heat-treated using the oxidation-preventive cover 12 of the embodiment, for example, an oxidation-preventive cover 12A may be placed around the object 11 placed on a mounting surface 18, as illustrated in Fig. 2. The object 11 may be heated by directly applying a heat source 19 such as a burner or plasma to the oxidation-preventive cover 12A housing the object 11, as shown in Fig. 2, or by using a heat treatment device 10, as shown in Fig. 1.

[0079] The oxidation-preventing cover 12A may be disposed so as not to come into contact with the object 11 during the heat treatment of the object 11. In this case, the recess 17 of the oxidation-preventing cover 12A forms an internal space 15. It is preferable that the oxidation-preventing cover 12A is a rigid molded body having a strength capable of standing on the installation surface 18 by itself.

[0080] 3, a recess 17 capable of accommodating the object 11 may be formed in the oxidation-preventive cover 12B, the recess 17 may be filled with the object 11, and then the object 11 may be heat-treated. In this case, the process may include, in this order, (1) a step of manufacturing the oxidation-preventive cover 12B having the recess 17, (2) a step of filling the recess 17 with the object 11, (3) a step of placing the oxidation-preventive cover 12B filled with the object 11 on the installation surface 18, and (4) a step of heating the object 11 on the installation surface 18 via the oxidation-preventive cover 12B.

[0081] 1 to 3, the anti-oxidation covers 12, 12A, and 12B are given different reference numerals due to differences in their shapes, but details regarding the anti-oxidation covers 12A and 12B in Fig. 2 and Fig. 3 can be similar to those described for the anti-oxidation cover 12 with reference to Fig. 1. For this reason, descriptions of the anti-oxidation covers 12A and 12B that overlap with those of the anti-oxidation cover 12 may be omitted. Also, illustration of the gap 14 is omitted in Fig. 2 and Fig. 3.

[0082] When carbon fragments or organic fragments are bound in producing the porous carbon material 13, a carbonizable resin or the like may be used as a binder. When producing a thin sheet-like porous carbon material 13, a slurry containing carbon fragments or organic fragments may be applied and then dried. The slurry containing carbon fragments or organic fragments is formed into a desired shape, dried, and then carbonized, whereby the porous carbon material 13 can be produced in a desired shape.

[0083] Methods for forming the recesses 17 in the oxidation prevention covers 12, 12A, 12B include a method of cutting the porous carbon material 13 by machining or the like to form a groove-like, tank-like or other shape, a method of pouring a slurry consisting of carbon particles, a binder component, and a solvent into a mold having a shape with the recesses 17, drying the solvent, and then carbonizing the binder component to bond the material, and a method of carbonizing a molded product of an organic material formed into a shape with the recesses 17.

[0084] 2, a method is preferable in which a mold that fits the shape of the oxidation-preventive cover 12A is made and a material is molded to fit the shape of the mold in order to obtain a large recess 17. In addition, since it is sufficient that the internal space 15 is larger than the target object 11, the recess 17 may be formed by combining porous carbon materials 13 having a predetermined shape such as a plate or sheet into a box shape.

[0085] In the oxidation prevention cover 12B of specific example 2 shown in FIG. 3, since the recesses 17 can be small, a method of forming the recesses 17 by cutting the surface of the porous carbon material 13 having a predetermined shape such as a plate or a column is preferable.

[0086] The present invention has been described above based on a preferred embodiment, but the present invention is not limited to the above-mentioned embodiment, and various modifications are possible without departing from the gist of the present invention. EXAMPLES

[0087] Examples of the present invention will be described below, but the present invention is not limited to these examples.

[0088] (How to make an oxidation prevention cover) A non-porous carbon material was used in Comparative Example 1, and a mesh-like carbon material was used in Comparative Example 2. In the other comparative examples, the carbon particles or carbon fibers shown in Table 1 or Table 2 were used as the carbon material, and were bound and carbonized by the method shown below to produce an oxidation-resistant cover.

[0089] Polyimide varnish was prepared as a binder for carbon particles or carbon fibers, and cyclohexanone was prepared as a solvent. The carbon material, binder, and solvent were mixed in a ratio of 3:1:1 to prepare a slurry. The slurry was poured into a silicone mold to prepare a block body, or a sheet body was prepared by coating and then dried. The dried block body or sheet body was placed in an oven in a vacuum or nitrogen atmosphere, heated to 1000°C in 2 to 3 hours, and held at 1000°C for 1 hour to carbonize the polyimide. Furthermore, a space to store non-oxides was formed in the carbonized block body by grinding.

[0090] (Non-oxide calcination method) The cavity of the block was either coated or filled with a non-oxide, or covered with a sheet, and then placed in an oven. Copper paste with a thickness of 1 mm or less was used as the non-oxide, and the copper paste was fired at 430°C or higher for 30 minutes.

[0091] (Method of measuring air permeability) The air permeability was measured by the A method (Fragile method) of JIS L 1096 (Fabric testing method for woven and knitted fabrics). Air was sucked in so that the internal pressure was 125 Pa, and the air flow rate resulting from the difference with the external pressure (atmospheric pressure) was measured. The air hole size was selected to be 40 mm in diameter.

[0092] (Method of measuring void ratio) The porosity was measured by the following procedures (1) to (3). (1) The dimensions of the sample were measured, and the volume V was calculated. (2) The mass M of the sample is calculated based on the true density ρ of graphite (2.2 g / m 3 ) to obtain the volume of the sample excluding voids, v 2 was calculated. (3) V and v 2 Since the difference is the volume of the void only, the porosity (%) of the sample is 100 × (Vv 2 ) / V.

[0093] (Method of measuring specific surface area) The specific surface area was measured by the following procedures (1) to (3). (1) The sample was placed in a sample tube for gas adsorption measurement and pretreated at 300°C / 3 hours under reduced pressure using a pretreatment device (BELPREP-vacIII [Microtrack-Bel Co., Ltd.]). (2) After pretreatment, the mass of the sample was measured, and adsorption measurements were performed under the following conditions using an analytical device (BELSORP-maxII [Microtrack BEL Co., Ltd.]). Sample tube: Large capacity sample tube (5.0 cm 3 , φ9mm) Sample size: 0.05-0.7g Adsorbate: Krypton Adsorption temperature: 77.360K Dead volume measurement: before or after adsorption measurement Saturated vapor pressure: Actual measurement (3) The specific surface area was calculated from the adsorption amount by the BET method.

[0094] (Method of measuring boundary line length per observation area) The "border line length per observation area" was measured according to the following steps (1) to (4). (1) The sample was cut at any location where the cut surface could be observed sufficiently, and the cut surface was observed with a scanning electron microscope (SEM) at a magnification of 3000 to obtain an image of the cut surface of the sample (hereinafter referred to as the image). (2) In the obtained image, the area is 360 μm 2 Observation areas consisting of rectangles of (18 μm × 20 μm) were randomly extracted and observed. The carbon regions in the observation areas were colored using image processing software (Paint Shop pro V4.20J) to obtain binarized images. (3) The perimeter of the colored area in the obtained binarized image was measured using image processing software (WinROOF V3.0), and the sum of the perimeters was calculated. (4) The above steps (1) to (3) were performed at 10 different points on the sample, and the average of the obtained total sums was defined as the boundary line length per observation area.

[0095] (Method of measuring carbon purity) The carbon purity was measured by the following procedures (1) to (4). (1) The sample was weighed to determine the mass. (2) The weighed sample was combusted and the carbon dioxide generated was quantitatively analyzed using gas chromatography. (3) CO obtained from the analysis results 2 Based on the amount of substance, the mass of carbon contained in the combusted sample (i.e., the mass of pure carbon) was calculated. (4) The ratio (percentage) of the "mass of pure carbon" to the "mass of the sample before combustion" was calculated, and this value was taken as the carbon purity (wt%).

[0096] (Method for Measuring Density Uniformity) The density uniformity was measured by the following procedures (1) to (3). (1) Ten samples were cut out so as to have equal arbitrary volumes (hereinafter, the samples cut into ten pieces are referred to as "small pieces"). (2) Each small piece was weighed, and the bulk density was calculated from "mass / volume" for each small piece. (3) From the values of the bulk density of each obtained small piece, the degree of variation (standard deviation σ) of the small piece sample was determined, and this value was taken as the density uniformity.

[0097] (Method for Evaluating Mass Increase X) After firing the non-oxide, in order to confirm the mass increase due to oxidation, the mass before and after firing was measured, and the oxidation prevention performance of the oxidation prevention cover was evaluated by observing the mass increase due to oxidation. Let the mass before firing be m 1 , and the mass after firing be m 2 . Using the following formula, the mass increase X (wt%) was obtained, and the fraction less than the decimal point (less than 1 wt%) was rounded down. X = (m 2 - m 1 ) / m 1 × 100 (wt%)

[0098] The evaluation of the mass increase was "◎" when X ≤ 4, "○" when 4 < X ≤ 10, and "×" when 10 < X.

[0099] (Method for Evaluating Cover Surface State) The surface state of the oxidation prevention cover after being used for firing was observed, and the presence or absence of cracks or the like due to an increase in the internal pressure of the cover was confirmed. Specifically, the surface of the oxidation prevention cover body after firing was observed with a microscope or the like, and it was evaluated as "◎" if there were no cracks, "○" if cracks could be confirmed but the original shape was maintained, and "×" if the cover was broken and the original shape was not maintained.

[0100] (Comprehensive Evaluation) If the evaluations of the mass increase and the cover surface condition were both "◎", the overall evaluation was also "◎". If at least one was "○" and neither was "×", the overall evaluation was "○". If at least one was "×", the overall evaluation was "×".

[0101] The above results are shown in Tables 1 and 2.

[0102] In the column "Carbon material structure," porous is indicated as "P" and non-porous is indicated as "NP." In Examples 10 to 11 and Comparative Example 5, carbon particles having a wide particle size distribution were used as the material. In Example 12, carbon fibers were used as the material, and the particle size was set to a fiber diameter (D) of 1 μm and a fiber length (L) of 10 μm.

[0103] [Table 1]

[0104] [Table 2]

[0105] In Examples 1 to 12, the overall evaluation was "◎" or "◯". In Comparative Examples 1 to 5, the overall evaluation was "x". [Explanation of symbols]

[0106] 10...heat treatment device, 11...object, 12, 12A, 12B...oxidation prevention cover, 13...porous carbon material, 14...gap, 15...internal space, 16...external space, 17...recess, 18...installation surface, 19...heat source.

Claims

1. An oxidation prevention cover for preventing oxidation of a non-oxide when an object containing the non-oxide is heat-treated, the oxidation prevention cover is made of a porous carbon material that is breathable at least in a thickness direction and is capable of covering the periphery of the object during heat treatment of the object; The porous carbon material has a specific surface area of ​​0.05 m 2 / g or more, carbon purity of 95 wt% or more, density uniformity of 0.1 g / cm as standard deviation of bulk density 3 An oxidation-preventing cover characterized by:

2. The porous carbon material has an air permeability of 0.1 to 50 cm 3 / cm 2 s, observation area 360 μm 2 2. The oxidation-preventing cover according to claim 1, wherein the sum of the lengths of the boundaries between the carbon and the voids observed on the cut surface is 30 μm or more, and the void ratio is 20 to 80%.

3. 2. The oxidation-preventing cover according to claim 1, wherein the porous carbon material is made of carbon particles or carbon fibers, and the carbon particles or carbon fibers are bound together.

4. The oxidation-preventing cover according to claim 1 , wherein the oxidation-preventing cover has a concave internal space capable of accommodating the object.

5. A heat treatment method for heat treating an object using the oxidation-preventing cover according to claim 1, comprising: A heat treatment method, characterized in that the oxidation prevention cover is arranged so as not to come into contact with the object during the heat treatment of the object.

6. A heat treatment method for heat treating an object using the oxidation-preventing cover according to claim 1, comprising: A heat treatment method comprising forming a recess capable of accommodating the object, filling the object into the recess, and then heat treating the object.

7. A heat treatment method, comprising heat treating the object in the atmosphere using the oxidation-preventing cover according to claim 1.

8. 8. The heat treatment method according to claim 5, wherein the object is a solid or a paste, and the heat treatment is firing or sintering.

Citation Information

Patent Citations

  • Non-oxidative firing method

    JP1993017238A