Material set for manufacturing fiber-reinforced composite material, method for manufacturing fiber-reinforced composite material, and fiber-reinforced composite material
A material set with a base resin and sizing agent combination minimizes thermal decomposition, enhancing the bending strength of fiber-reinforced composites by reducing voids, achieving high mechanical strength.
Patent Information
- Application Number
- JP2023044243
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The thermal decomposition of sizing agents during the impregnation process in fiber-reinforced composite materials leads to voids, reducing the bending strength of the composite due to meandering and volatile matter generation.
A material set comprising a base resin with an amide group and a sizing agent with a phenolic hydroxyl group, where the weight loss rate of the sizing agent is 25% by weight or less, is used to minimize thermal decomposition, ensuring high bending strength.
The material set enhances the bending strength of the fiber-reinforced composite material by reducing voids, achieving strengths of 500 MPa or more with glass fibers and 1600 MPa or more with other fibers.
Smart Images

Figure 2024134123000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a material set for producing a fiber-reinforced composite material. The present invention also relates to a method for producing a fiber-reinforced composite material using the material set. The present invention also relates to a fiber-reinforced composite material. [Background technology]
[0002] Fiber-reinforced composites in which a matrix resin is reinforced with reinforcing fibers such as carbon fibers are known. Fiber-reinforced composites have the advantages of being lightweight yet excellent in strength, rigidity, and dimensional stability. For this reason, fiber-reinforced composites are used in a variety of applications, such as vehicles such as automobiles and aircraft, office equipment, IC trays, notebook computer housings, waterstops, and wind turbine blades, and the demand for them is increasing year by year.
[0003] Fiber-reinforced composite materials are produced by impregnating the spaces between fibers of a fiber bundle with a matrix resin (base resin). In addition, fiber bundles to which a sizing agent is attached may be used as the fiber bundle (for example, Patent Documents 1 and 2 below). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2014-162999 A [Patent Document 2] JP 2003-165849 A Summary of the Invention [Problem to be solved by the invention]
[0005] The temperature (impregnation temperature) at which the matrix resin is impregnated into the interfiber spaces of the fiber bundle is relatively high. Therefore, the sizing agent may thermally decompose during the impregnation process. When the sizing agent thermally decomposes, the fiber bundle may become meandering, or volatile substances may be generated as thermal decomposition products, which may lead to the existence of voids in the resulting fiber-reinforced composite material. In fiber-reinforced composite materials with voids, the bending strength of the fiber-reinforced composite material decreases due to these voids.
[0006] An object of the present invention is to provide a material set for producing a fiber-reinforced composite material, which can increase the bending strength of the resulting fiber-reinforced composite material. Another object of the present invention is to provide a method for producing a fiber-reinforced composite material using the material set for producing a fiber-reinforced composite material. Another object of the present invention is to provide a fiber-reinforced composite material having high bending strength. [Means for solving the problem]
[0007] This specification discloses the following material set for manufacturing a fiber-reinforced composite material, a manufacturing method for a fiber-reinforced composite material, and a fiber-reinforced composite material.
[0008] Item 1. A material set for producing a fiber-reinforced composite material, the material set being a base resin, a fiber bundle, and a sizing agent, the base resin having an amide group, the sizing agent having a phenolic hydroxyl group, and the combination of the base resin and the sizing agent being such that the weight loss rate of the sizing agent measured by the following measurement method is 25% by weight or less.
[0009] Method for measuring the weight loss rate of the sizing agent: The melting temperature of the base resin is defined as T°C. The sizing agent is heated from 30°C to (T+50)°C at a heating rate of 10°C / min in an air atmosphere, and the weight of the sizing agent at each temperature is measured. The weight of the sizing agent at 30°C is defined as W0, an arbitrary temperature between 30°C and (T+50)°C is defined as t, and the weight of the sizing agent at t°C is defined as W0. t Then, the formula is: W0-W tThe weight of the sizing agent at the temperature at which the weight loss of the sizing agent is maximum is defined as W1. The weight loss rate of the sizing agent is calculated from W0 and W1 by the following formula (1).
[0010] Weight reduction rate of sizing agent (wt%) = [(W0-W1) / W0] × 100 (1)
[0011] Item 2. The material set for manufacturing fiber-reinforced composite materials according to item 1, wherein the melting temperature of the base resin is 260°C or higher.
[0012] Item 3. The material set for producing a fiber-reinforced composite material according to item 1 or 2, wherein the fibers of the fiber bundles are carbon fibers.
[0013] Item 4. The material set for producing a fiber-reinforced composite material according to any one of Items 1 to 3, which is a material set including the base resin, the fiber bundles, the sizing agent, and a filler.
[0014] Item 5. The material set for producing a fiber-reinforced composite material according to any one of Items 1 to 4, wherein the base resin is a thermoplastic resin.
[0015] Item 6. The material set for producing a fiber-reinforced composite material according to any one of Items 1 to 5, wherein the base resin is a polyamide resin.
[0016] Item 7. The material set for producing a fiber-reinforced composite material according to any one of Items 1 to 6, wherein the base resin is a semi-aromatic polyamide resin.
[0017] Item 8. A method for producing a fiber-reinforced composite material using the material set for producing a fiber-reinforced composite material according to any one of items 1 to 7, comprising an impregnation step of impregnating the inter-fiber portions of the fiber bundle to which the sizing agent is attached with the matrix resin.
[0018] Item 9. A fiber-reinforced composite material, in which the base resin is impregnated into the inter-fiber portions of the fiber bundle to which the sizing agent is attached, using the material set for manufacturing a fiber-reinforced composite material according to any one of items 1 to 7.
[0019] Item 10. A fiber-reinforced composite material comprising a matrix resin, a fiber bundle, and a sizing agent, wherein the matrix resin has an amide group, the sizing agent is attached to the outer surface of the fiber bundle, and the sizing agent has a phenolic hydroxyl group. When the fiber bundle is a glass fiber, the bending strength of the fiber-reinforced composite material measured in accordance with JIS K7017 is 500 MPa or more, and when the fiber bundle is a fiber other than glass fiber, the bending strength of the fiber-reinforced composite material measured in accordance with JIS K7074 is 1600 MPa or more. A fiber-reinforced composite material. Effect of the Invention
[0020] The material set for producing a fiber-reinforced composite material according to the present invention is a material set for producing a fiber-reinforced composite material. The material set according to the present invention is a material set of a base resin, a fiber bundle, and a sizing agent. In the material set according to the present invention, the base resin has an amide group, and the sizing agent has a phenolic hydroxyl group. In the material set according to the present invention, the combination of the base resin and the sizing agent is a combination in which the weight loss rate of the sizing agent measured by a specific measurement method is 25% by weight or less. Since the material set according to the present invention is provided with the above configuration, the bending strength of the obtained fiber-reinforced composite material can be increased.
[0021] The fiber reinforced composite material according to the present invention includes a matrix resin, a fiber bundle, and a sizing agent. In the fiber reinforced composite material according to the present invention, the matrix resin has an amide group, and the sizing agent is attached to the outer surface of the fiber of the fiber bundle, and the sizing agent has a phenolic hydroxyl group. In the fiber reinforced composite material according to the present invention, when the fiber of the fiber bundle is a glass fiber, the bending strength of the fiber reinforced composite material measured according to JIS K7017 is 500 MPa or more, and when the fiber of the fiber bundle is a fiber other than glass fiber, the bending strength of the fiber reinforced composite material measured according to JIS K7074 is 1600 MPa or more. Since the fiber reinforced composite material according to the present invention has the above configuration, it has a high bending strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] The present invention will be described in detail below.
[0023] (Fiber-reinforced composite manufacturing material set) A material set for producing a fiber-reinforced composite material according to the present invention (hereinafter sometimes abbreviated as "material set") is a material set for producing a fiber-reinforced composite material.
[0024] The material set according to the present invention is a material set of a base resin, a fiber bundle, and a sizing agent. The material set according to the present invention has a base resin (first material), a fiber bundle (second material), and a sizing agent (third material). The material set according to the present invention is a combination of a base resin, a fiber bundle, and a sizing agent.
[0025] In the material set according to the present invention, the base resin has an amide group, and the sizing agent has a phenolic hydroxyl group.
[0026] In the material set according to the present invention, the combination of the base resin and the sizing agent is such that the weight loss rate of the sizing agent measured by the following measurement method is 25% by weight or less.
[0027] Method for measuring the weight loss rate of the sizing agent: The melting temperature of the base resin is defined as T°C. The sizing agent is heated from 30°C to (T+50)°C at a heating rate of 10°C / min in an air atmosphere, and the weight of the sizing agent at each temperature is measured. The weight of the sizing agent at 30°C is defined as W0, any temperature between 30°C and (T+50)°C is defined as t, and the weight of the sizing agent at t°C is defined as W0. t Then, the formula is: W0-W t The weight of the sizing agent at the temperature at which the weight loss of the sizing agent is maximum is defined as W1. The weight loss rate of the sizing agent is calculated from the above W0 and W1 by the following formula (1).
[0028] Weight reduction rate of sizing agent (wt%) = [(W0-W1) / W0] × 100 (1)
[0029] The material set according to the present invention has the above-mentioned configuration, and therefore the bending strength of the resulting fiber-reinforced composite material can be increased. In the material set according to the present invention, the combination of the base resin and the sizing agent is such that the weight loss rate of the sizing agent is 25% by weight or less, and therefore the sizing agent is unlikely to be thermally decomposed in the impregnation step during the manufacture of the fiber-reinforced composite material. Therefore, a fiber-reinforced composite material with few voids can be obtained well, and therefore a fiber-reinforced composite material with high bending strength can be obtained well.
[0030] The weight loss rate of the sizing agent will now be described in more detail.
[0031] First, the melting temperature (T) of the base resin is measured. The melting temperature (T) of the base resin can be measured by a differential scanning calorimeter (DSC).
[0032] In addition, the sizing agent to be used as a measurement sample is heated at 200°C for 2 hours or more to thoroughly dry it, and then cooled to 30°C. The dried sizing agent is left to stand in an environment of 30°C for 1 hour or more. The sizing agent to be used as a measurement sample may be obtained by separately preparing the same type of sizing agent as the sizing agent attached to the fiber bundle, or by collecting the sizing agent attached to the fiber bundle. Next, the sizing agent is weighed in an aluminum container, and the weight (W0) of the sizing agent at 30°C is taken as the weight. The weight (W0) of the sizing agent at 30°C can be, for example, 10 mg. Next, the aluminum container on which the sizing agent is placed is placed, for example, in a thermogravimetric analyzer (TGA device), and heated from 30°C to (T+50)°C at a heating rate of 10°C / min. The weight of the sizing agent at each temperature is measured, and the weight of the sizing agent at the sizing agent temperature t°C is taken as W t t is any temperature between 30°C and (T+50)°C. Also, the formula: W0-W t The weight loss of the sizing agent is calculated by the value expressed by the formula: t The formula is W0-W t The weight of the sizing agent at the temperature at which the weight loss of the sizing agent represented by the above formula is maximum is defined as W1.
[0033] The weight loss rate of the sizing agent is calculated from W0 and W1 by the above formula (1).
[0034] In order to exert the effects of the present invention, the weight loss rate of the sizing agent is 25% by weight or less.
[0035] The weight loss rate of the sizing agent is preferably 20% by weight or less, more preferably 15% by weight or less. When the weight loss rate of the sizing agent is equal to or less than the upper limit, the effect of the present invention can be more effectively exhibited. The weight loss rate of the sizing agent may be 0.1% by weight or more, or 1% by weight or more.
[0036] The material set according to the present invention will be further described below.
[0037] <Base resin> The material set includes a base resin. The base resin includes an amide group. Only one type of base resin may be used, or two or more types of base resins may be used in combination.
[0038] The base resin preferably has a structural unit having an amide group, and more preferably has a structural unit having an amide group as a repeating structural unit, in which case the effects of the present invention can be more effectively exhibited.
[0039] The type of the base resin is not particularly limited as long as it has an amide group, and examples of the base resin include thermoplastic resins and thermosetting resins.
[0040] The matrix resin is preferably a thermoplastic resin. Since the melting temperature of a thermoplastic resin is high, when a thermoplastic resin is used as the matrix resin, the sizing agent is easily thermally decomposed in the impregnation step during the production of a fiber reinforced composite material. However, since the matrix resin and the sizing agent are a specific combination in the present invention, the effects of the present invention can be achieved even if the matrix resin is a thermoplastic resin.
[0041] Examples of the thermoplastic resin (the thermoplastic resin having an amide group) include polyamide resin, polyimide resin, and polyamideimide resin.
[0042] Examples of the polyamide resin include aliphatic polyamide resin, semi-aromatic polyamide resin, and fully aromatic polyamide resin. The aliphatic polyamide resin is a polyamide resin that does not have an aromatic ring. The semi-aromatic polyamide resin is a polyamide resin in which one of the monomer dicarboxylic acid and the monomer diamine is an aromatic compound. The fully aromatic polyamide resin is a polyamide resin in which both the monomer dicarboxylic acid and the monomer diamine are aromatic compounds. Examples of the dicarboxylic acid include terephthalic acid. Examples of the diamine include hexamethylenediamine.
[0043] Examples of the aliphatic polyamide resin include polyamide-6, polyamide-6,6, polyamide-6,12, polyamide-11, polyamide-12, and polyamide-4,6.
[0044] Examples of the semi-aromatic polyamide resin include polyphthalamide and polymetaxylylene adipamide.
[0045] The wholly aromatic polyamide resin may, for example, be poly-p-phenylene terephthalamide.
[0046] The matrix resin is preferably a polyamide resin, and more preferably a semi-aromatic polyamide resin. In this case, the effects of the present invention can be more effectively exhibited. In addition, the heat resistance of the obtained fiber-reinforced composite material can be further improved and the water absorption can be further reduced. Since the melting temperature of polyamide resin (particularly semi-aromatic polyamide resin) is high, when polyamide resin is simply used as the matrix resin, the sizing agent is easily thermally decomposed in the impregnation step during the production of the fiber-reinforced composite material. In contrast, in the present invention, the matrix resin and the sizing agent are a specific combination, so that the effects of the present invention can be exhibited even if the matrix resin is a polyamide resin.
[0047] The melting temperature (T) of the matrix resin is preferably 260° C. or higher, preferably 350° C. or lower, and more preferably 330° C. or lower. When the melting temperature (T) of the matrix resin is equal to or higher than the lower limit, the matrix resin can be melted well and impregnated well into the fiber bundle, so that the bending strength of the obtained fiber reinforced composite material can be further increased. When the melting temperature (T) of the matrix resin is equal to or lower than the upper limit, there is no need to excessively increase the impregnation temperature during the production of the fiber reinforced composite material, so that the effects of the present invention can be more effectively exhibited.
[0048] The base resin may be in the form of a sheet or particles, or may be in a form other than these.
[0049] When the base resin is particulate, the average particle size of the particulate base resin is usually larger than the average particle size of the filler described below. The average particle size of the particulate base resin is preferably 0.1 μm or more, more preferably 1 μm or more, even more preferably 5 μm or more, and preferably 50 μm or less, more preferably 30 μm or less, even more preferably 20 μm or less.
[0050] The average particle size of the particulate base resin is determined from an electron microscope photograph using image analysis software (for example, "WinROOF" manufactured by Mitani Shoji Co., Ltd.).
[0051] The average particle size of the particulate base resin is the number average particle size, which is the arithmetic mean value of the particle sizes of the base resin. The particle size means the diameter of the equivalent circle of the base resin.
[0052] The average particle size of the particulate base resin is preferably determined from 100 or more base resin particles. If there are not 100 or more base resin particles in the obtained electron microscope photograph, it is preferable to photograph a new region with the electron microscope until the number of base resin particles reaches 100 or more.
[0053] <Fiber bundle> The material set includes fiber bundles. The fiber bundles may be of one type or of two or more types in combination.
[0054] The form of the fiber bundle may be unidirectional continuous fiber (UD), woven fabric, knitted fabric, etc. The knitted fabric may be NCF (non-crimp fabric), etc.
[0055] From the viewpoint of further increasing the strength of the obtained fiber-reinforced composite material, the form of the fiber bundle is preferably a unidirectional continuous fiber, a knitted fabric or a woven fabric, and more preferably a unidirectional continuous fiber. The fiber bundle may be a fiber bundle in which a plurality of fiber bundles are laminated in the thickness direction.
[0056] The fiber bundle includes a plurality of fibers. The fibers may be of one type or of two or more types in combination.
[0057] Examples of the fibers include carbon fibers, glass fibers, ceramic fibers, metal fibers, silicon carbide fibers, and aramid fibers.
[0058] From the viewpoint of further increasing the bending strength and compressive strength of the resulting fiber-reinforced composite material, it is preferable that the fibers include carbon fibers, glass fibers, or aramid fibers.
[0059] From the viewpoint of reducing the weight of the resulting fiber-reinforced composite material and further increasing the mechanical strength of the resulting fiber-reinforced composite material, the above-mentioned fiber is preferably carbon fiber or aramid fiber, and more preferably carbon fiber.
[0060] From the viewpoint of reducing the production costs of the fiber-reinforced composite material, the fibers are preferably glass fibers.
[0061] Examples of the carbon fiber include PAN-based carbon fiber and PITCH-based carbon fiber.
[0062] The fibers are preferably continuous fibers, such as unidirectional continuous fibers (UD; Unidirectional fibers) and fibers contained in woven fabrics, which exist continuously in the cross-sectional direction.
[0063] <Sizing agent> The material set has a sizing agent. In the material set, the sizing agent may be attached to the outer surface of the fibers of the fiber bundle. That is, in the material set, the fiber bundle and the sizing agent may be in a state of a sizing-agent-attached fiber bundle in which the sizing agent is attached to the outer surface of the fibers of the fiber bundle. In the material set, the sizing agent may be the sizing agent before being attached to the outer surface of the fibers of the fiber bundle. The sizing agent has a phenolic hydroxyl group. The phenolic hydroxyl group is a hydroxyl group (OH group) directly bonded to a carbon atom constituting an aromatic ring. Only one type of the sizing agent may be used, or two or more types may be used in combination.
[0064] Furthermore, by using the sizing agent (a sizing agent having a phenolic hydroxyl group), even if the base resin is the semi-aromatic polyamide resin, the adhesion between the sizing agent and the base resin can be increased, and the bending strength of the resulting fiber-reinforced composite can be further increased.
[0065] Examples of the sizing agent (a sizing agent having a phenolic hydroxyl group) include phenolic resins.
[0066] The molecular weight of the sizing agent is preferably 100 or more, more preferably 1000 or more, and is preferably 1,000,000 or less, more preferably 100,000 or less.
[0067] The molecular weight of the sizing agent means the molecular weight that can be calculated from the structural formula when the sizing agent is not a polymer and when the structural formula of the sizing agent can be specified. When the sizing agent is a polymer, the molecular weight of the sizing agent means the weight average molecular weight.
[0068] In the fiber bundle with sizing agent, the content of the sizing agent (the amount of sizing agent adhering to the fibers) in the total of 100% by weight of the fibers of the fiber bundle and the sizing agent is preferably 0.1% by weight or more, more preferably 0.5% by weight or more, even more preferably 1.0% by weight or more, preferably 7.0% by weight or less, more preferably 5.0% by weight or less, and even more preferably 3.0% by weight or less.
[0069] <Filler> The material set preferably includes a filler. That is, the material set preferably includes the base resin (first material), the fiber bundle (second material), the sizing agent (third material), and the filler (fourth material). In the material set, the filler may be a filler disposed between the fibers of the fiber bundle. In the material set, the filler may be a filler before being disposed between the fibers of the fiber bundle. By using the filler, a spread fiber bundle (a fiber bundle spread by a filler) can be obtained. By using the spread fiber bundle, the impregnation of the base resin can be further improved. Only one type of the filler may be used, or two or more types may be used in combination.
[0070] The filler may be organic particles (organic filler) or inorganic particles (inorganic filler).
[0071] Examples of the organic particles include thermosetting resin particles such as epoxy resin particles, phenol resin particles, melamine resin particles, urea resin particles, unsaturated polyester resin particles, and oxazine resin particles; divinylbenzene resin particles; polyolefin resin particles; polybutylene terephthalate resin particles; polyethylene terephthalate resin particles; acrylic resin particles; polycarbonate resin particles, etc. The material of the organic particles may be the same as that of the base resin.
[0072] Examples of the inorganic particles include silica particles, metal particles, carbon particles, talc particles, and calcium carbonate particles. Examples of the metal particles include alumina particles, titanium oxide particles, ferrite particles, iron particles, and copper particles. Examples of the carbon particles include amorphous carbon particles and graphite particles.
[0073] The filler is preferably oxazine resin particles, divinylbenzene resin particles, resin particles of a resin having an amide group, silica particles, carbon particles, calcium carbonate particles, or talc particles, and more preferably oxazine resin particles, divinylbenzene resin particles, resin particles of a resin having an amide group, silica particles, or carbon particles. The resin having an amide group is preferably the same resin as the matrix resin. In this case, the open state of the spread fiber bundles is well maintained, so that the impregnation of the matrix resin can be further improved, and therefore various physical properties such as the compressive strength of the obtained fiber reinforced composite can be improved in a well-balanced manner.
[0074] The shape of the filler is not particularly limited. The shape of the filler may be spherical, or may be a shape other than a spherical shape, such as flat, scaly, needle-like, or cubic. The shape of the filler is preferably spherical.
[0075] The average particle size of the filler is preferably 0.1 μm or more, more preferably 0.5 μm or more, even more preferably 1 μm or more, and preferably 10 μm or less, more preferably 7 μm or less, and even more preferably 5 μm or less. When the average particle size is equal to or more than the lower limit and equal to or less than the upper limit, the fiber bundles are well maintained in an open state, so that the impregnation with the matrix resin can be further improved, and therefore various physical properties such as the compressive strength of the obtained fiber reinforced composite can be improved in a well-balanced manner.
[0076] The average particle size of the filler is determined from an electron microscope photograph using image analysis software (e.g., "WinROOF" manufactured by Mitani Shoji Co., Ltd.). Alternatively, it may be determined from an electron microscope photograph of a cross section of the obtained fiber-reinforced composite material using image analysis software (e.g., "WinROOF" manufactured by Mitani Shoji Co., Ltd.).
[0077] The average particle size of the filler is a number average particle size, which is an arithmetic mean value of the particle sizes of the filler. The particle size means the equivalent circle diameter of the filler.
[0078] The average particle size of the filler is preferably determined from 100 or more fillers. If there are not 100 or more fillers in the obtained electron microscope photograph, it is preferable to photograph a new region with the electron microscope until the number of fillers becomes 100 or more.
[0079] In the spread fiber bundle, the content of the filler is preferably 0.1 part by weight or more, more preferably 0.5 part by weight or more, preferably 10 parts by weight or less, more preferably 5.0 parts by weight or less, and even more preferably 2.0 parts by weight or less, relative to 100 parts by weight of the total of the fibers of the fiber bundle and the sizing agent. When the content of the filler is equal to or more than the lower limit and equal to or less than the upper limit, the spread state of the fiber bundle is well maintained, so that the impregnation with the matrix resin can be further improved, and therefore various physical properties such as the compressive strength of the obtained fiber reinforced composite can be improved in a well-balanced manner.
[0080] <Other ingredients (other materials)> The material set may contain other components (other materials) different from the four types of the base resin, the fiber bundles, the sizing agent, and the filler.
[0081] (Method of manufacturing fiber-reinforced composite materials) A fiber-reinforced composite material can be manufactured using the above-mentioned material set. The manufacturing method of the fiber-reinforced composite material according to the present invention includes an impregnation step of impregnating the inter-fiber portions of the fiber bundle to which the sizing agent is attached (fiber bundle with sizing agent) with the matrix resin. The manufacturing method of the fiber-reinforced composite material preferably includes a step of obtaining the fiber bundle to which the sizing agent is attached (fiber bundle with sizing agent) prior to the impregnation step.
[0082] The fiber bundle with a sizing agent can be obtained, for example, by contacting the fiber bundle with the sizing agent. Note that, as the fiber bundle with a sizing agent, a commercially available fiber bundle with a sizing agent attached thereto may be used.
[0083] The fiber bundle with a sizing agent is preferably a spread fiber bundle. The spread fiber bundle can be obtained, for example, by spreading a fiber bundle with a filler. That is, the spread fiber bundle is, for example, a fiber bundle spread with a filler.
[0084] Examples of a method for obtaining the above-mentioned spread fiber bundle (fiber bundle spread by a filler) include the following method (i), (ii), or (iii).
[0085] (i) A method in which a liquid containing a sizing agent and a filler is brought into contact with a fiber bundle to adhere the filler to the outer surface of the fibers of the fiber bundle.
[0086] (ii) A method in which the fiber bundle is brought into contact with a sizing agent and then further brought into contact with a liquid containing a filler, thereby adhering the filler to the outer surface of the fibers of the fiber bundle.
[0087] (iii) A method in which a fiber bundle having a sizing agent attached thereto (fiber bundle with sizing agent) is prepared, and this fiber bundle with sizing agent is brought into contact with a liquid containing a filler to adhere the filler to the outer surface of the fibers of the fiber bundle.
[0088] The method for bringing the fiber bundle into contact with the liquid containing the filler includes spraying, coating, immersion, and the like.
[0089] By rotating or vibrating the fiber bundle in contact with the filler, or handling it with a roller or the like, the liquid containing the filler spreads over the fiber surface, and the filler penetrates between the fibers, resulting in an opened fiber bundle (a fiber bundle opened by the filler).
[0090] From the viewpoint of increasing the wetting and spreading property of the filler-containing liquid on the fiber surface, the filler-containing liquid preferably contains an organic solvent. The organic solvent is not particularly limited. From the viewpoint of workability, the organic solvent preferably contains methanol, ethanol, propanol, tetrahydrofuran, or acetone. The filler-containing liquid may contain water.
[0091] After contacting the fiber bundle with a liquid containing a filler, the fiber bundle can be heated or dried to remove the solvent (organic solvent, water, etc.), thereby obtaining a spread fiber bundle (fiber bundle spread by the filler).
[0092] When a particulate matrix resin is used as the matrix resin, a fiber bundle to which both the sizing agent and the particulate matrix resin are attached (fiber bundle with sizing agent and matrix resin) may be obtained in the step of obtaining the fiber bundle to which the sizing agent is attached (fiber bundle with sizing agent). The fiber bundle with sizing agent and matrix resin can be obtained, for example, by the following method (1) or (2). (1) A method of adding particulate matrix resin to a liquid containing a sizing agent or a liquid containing a sizing agent and a filler, and bringing the obtained liquid into contact with the fiber bundle. (2) A method of bringing a fiber bundle with sizing agent, which may be a spread fiber bundle, into contact with particulate matrix resin.
[0093] In the impregnation step, the method of impregnating the interfiber portions of the fiber bundle with the sizing agent with the matrix resin is not particularly limited. Examples of the method of impregnating the interfiber portions of the fiber bundle with the sizing agent include the following methods (1) and (2). (1) A method in which the molten matrix resin is extruded into a film using a sheet die or the like, laminated on the fiber bundle with the sizing agent, and then compressed while being heated to impregnate the interfiber portions of the fiber bundle with the matrix resin. (2) A method in which the fiber bundle with the sizing agent and matrix resin is compressed while being heated to impregnate the interfiber portions of the fiber bundle with the matrix resin.
[0094] The melting temperature of the matrix resin is designated as T° C. The impregnation temperature in the impregnation step is preferably at least (T+5)° C., more preferably at least (T+10)° C., and preferably at most (T+50)° C., and more preferably at most (T+40)° C. When the impregnation temperature is at least the lower limit and at most the upper limit, thermal decomposition of the sizing agent can be effectively suppressed, and a fiber-reinforced composite material having high bending strength can be satisfactorily obtained.
[0095] (Fiber reinforced composite materials) The fiber-reinforced composite material can be obtained by impregnating the inter-fiber portions of the fiber bundle to which the sizing agent is attached (fiber bundle with sizing agent) with the base resin using the material set.
[0096] The fiber reinforced composite material includes the matrix resin, the fiber bundle, and the sizing agent. In the fiber reinforced composite material, the matrix resin preferably has an amide group. In the fiber reinforced composite material, the sizing agent preferably adheres to the outer surface of the fibers of the fiber bundle. In the fiber reinforced composite material, the sizing agent preferably has a phenolic hydroxyl group.
[0097] The fiber reinforced composite preferably includes the filler. The filler is preferably disposed between the fibers of the fiber bundle. The filler is preferably disposed on the outer peripheral surface of the fiber. The filler may be disposed on the outer peripheral surface of the fiber via a sizing agent. As described above, the filler is preferably oxazine resin particles, divinylbenzene resin particles, resin particles of a resin having an amide group, silica particles, carbon particles, calcium carbonate particles, or talc particles, and more preferably oxazine resin particles, divinylbenzene resin particles, resin particles of a resin having an amide group, silica particles, or carbon particles.
[0098] In 100% by volume of the fiber reinforced composite material, the content of the matrix resin is preferably 30% by volume or more, more preferably 40% by volume or more, and preferably 80% by volume or less, and more preferably 60% by volume or less. When the content of the matrix resin is equal to or more than the lower limit and equal to or less than the upper limit, the mechanical strength of the fiber reinforced composite material can be further increased.
[0099] When the fiber reinforced composite material contains glass fibers, the flexural strength of the fiber reinforced composite material measured in accordance with JIS K7017 is preferably 500 MPa or more, and more preferably 550 MPa or more.
[0100] In the above fiber reinforced composite material, when the above fibers are fibers other than glass fibers, the bending strength of the fiber reinforced composite material measured in accordance with JIS K7074 is preferably 1600 MPa or more, and more preferably 1650 MPa or more.
[0101] The flexural strength of the above fiber reinforced composite material is measured at 23°C.
[0102] The present invention will be specifically described below by way of examples and comparative examples, but the present invention is not limited to the following examples.
[0103] The following materials were prepared:
[0104] (Base resin) Polyphthalamide resin (Kuraray's "PA9T" in particulate form, resin with amide groups, melting temperature (T): 306°C, average particle size (D50): 34μm)
[0105] The melting temperature (T) of the base resin was measured by a differential scanning calorimeter (DSC).
[0106] (Fiber bundle) Carbon fiber bundle (HEXCEL "AS4D")
[0107] (Sizing agent having a phenolic hydroxyl group) Phenolic resin 1 (Takemoto Oil Co., Ltd. "Delion F-5919", aqueous dispersion with a solid content of 30% by weight) Phenol resin 2 (Konishi Chemical's "WSR-SP82", an aqueous solution with a solids concentration of 32% by weight) Epoxy resin (Takemoto Oil & Fat Co., Ltd. "Delion F-5918", aqueous dispersion with a solid content of 47% by weight, containing phenolic hydroxyl groups derived from the starting material during synthesis)
[0108] (Sizing agent without phenolic hydroxyl group) Polyetherimide resin (MICHELMAN "HP-1632", aqueous dispersion with a solid content of 11% by weight) Urethane resin (Takemoto Oil Co., Ltd.'s "Delion F-5886", aqueous dispersion with a solid content of 50% by weight)
[0109] (Filler) Silica particles (AGC Si-Tech "L-31")
[0110] As the material sets, material sets A to E were obtained by combining the following materials.
[0111] <Material set A> Base resin: Polyphthalamide resin (particulate) Fiber bundle: Carbon fiber bundle Sizing agent: Phenolic resin 1 Filler: Silica particles
[0112] <Material set B> Base resin: Polyphthalamide resin (particulate) Fiber bundle: Carbon fiber bundle Sizing agent: Phenolic resin 2 Filler: Silica particles
[0113] <Material Set C> Base resin: Polyphthalamide resin (particulate) Fiber bundle: Carbon fiber bundle Sizing agent: Polyetherimide resin Filler: Silica particles
[0114] <Material Set D> Base resin: Polyphthalamide resin (particulate) Fiber bundle: Carbon fiber bundle Sizing agent: urethane resin Filler: Silica particles
[0115] <Material Set E> Base resin: Polyphthalamide resin (particulate) Fiber bundle: Carbon fiber bundle Sizing agent: Epoxy resin Filler: Silica particles
[0116] (Examples 1 and 2 and Comparative Examples 1 to 3) (1) Material set: The material set described in Table 1 was used.
[0117] (2) Measurement of weight loss rate of sizing agent: The sizing agent to be measured was heated at 200°C for 2 hours or more to thoroughly dry it, and then cooled to 30°C. The dried sizing agent was left to stand in an environment of 30°C for 1 hour or more. The sizing agent was then weighed in an aluminum container, and the weight of the sizing agent at 30°C (W0) was recorded. The aluminum container on which the sizing agent was placed was then placed in a thermogravimetric measuring device (TGA device, Hitachi "STA7300"), and heated from 30°C to (T+50)°C at a heating rate of 10°C / min, and the weight of the sizing agent at each temperature was measured. Note that any temperature between 30°C and (T+50)°C was defined as t, and the weight of the sizing agent at temperature t°C was recorded as W t Then, the formula is: W0-W t The weight loss of the sizing agent is calculated by the formula: W0-W t The weight of the sizing agent at the temperature at which the weight loss of the sizing agent, expressed as: was maximum, was designated as W1. The weight loss rate of the sizing agent was calculated from the above W0 and W1 according to the following formula (1).
[0118] Weight reduction rate of sizing agent (wt%) = [(W0-W1) / W0] × 100 (1)
[0119] The results of the weight loss rate of the sizing agent are shown in Table 1 below.
[0120] (3) Preparation of fiber-reinforced composites: A mixture was obtained by mixing 60 parts by weight of ethanol, 37 parts by weight of distilled water, and a sizing agent (commercially available). The sizing agent (commercially available) was mixed with ethanol and distilled water so that the concentration (solid content concentration) of the sizing agent in the resulting mixture was 1% by weight. 0.5 parts by weight of filler and 6 parts by weight of particulate base resin were added to the resulting mixture to obtain a fiber-opening liquid. Next, the carbon fiber bundle was immersed in the fiber-opening liquid, and then excess liquid was removed. Next, the fiber bundle was heated at 300°C for 2 minutes and dried to obtain a fiber bundle with the sizing agent attached thereto (fiber bundle with sizing agent and base resin).
[0121] The fiber bundle with the sizing agent attached was heated to 340°C and compressed at a pressure of 3 MPa for 15 minutes to impregnate the spaces between the fibers of the fiber bundle with the matrix resin. In this way, a fiber reinforced composite material with a length of 200 mm, a width of 50 mm, and a thickness of 2 mm was obtained. The fiber volume content (Vf) of the fiber reinforced composite material was 55% by volume.
[0122] (Reference example A) A commonly used fiber-reinforced composite material with an epoxy resin matrix (produced by combining Mitsubishi Chemical Corporation's "TR350C075S" and "TR350C150S") was prepared as a reference fiber-reinforced composite material for bending strength. The fiber volume fraction (Vf) of the fiber-reinforced composite material was 67% by volume.
[0123] (evaluation) (1) Bending strength of fiber-reinforced composite materials The bending strength of the obtained fiber reinforced composite material was measured at 23°C in accordance with JIS K7074. The test was repeated three times, and the average value of the bending strengths obtained in the three tests was regarded as the bending strength of the fiber reinforced composite material. The bending strength of the fiber reinforced composite material was evaluated according to the following criteria.
[0124] <Criteria for determining bending strength of fiber-reinforced composite materials> 〇: Bending strength is 1660MPa or more (90% or more of the bending strength of Reference Example A) ×: Bending strength is less than 1660 MPa (less than 90% of the bending strength of Reference Example A)
[0125] The configuration and results are shown in Table 1 below.
[0126] [Table 1]
Claims
1. A material set for manufacturing a fiber-reinforced composite material, comprising: A material set including a base resin, a fiber bundle, and a sizing agent, The matrix resin has an amide group, The sizing agent has a phenolic hydroxyl group, A material set for manufacturing a fiber-reinforced composite material, wherein the combination of the base resin and the sizing agent is such that the weight loss rate of the sizing agent measured by the following measurement method is 25% by weight or less. Method for measuring the weight loss rate of the sizing agent: The melting temperature of the base resin is defined as T°C. The sizing agent is heated from 30°C to (T+50)°C at a temperature increase rate of 10°C / min in an air atmosphere, and the weight of the sizing agent at each temperature is measured. The weight of the sizing agent at 30°C is defined as W 0 Let t be any temperature between 30°C and (T+50)°C, and let W be the weight of the sizing agent at t°C. t And the formula: W 0 -W t The weight of the sizing agent at the temperature at which the weight loss of the sizing agent is maximum is represented by W 1 The above W 0 and the above W 1 From this, the weight loss rate of the sizing agent is calculated according to the following formula (1). Weight reduction rate of sizing agent (wt%) = [(W 0 -W 1 ) / W 0 ] × 100 ... (1)
2. The material set for manufacturing a fiber-reinforced composite material according to claim 1 , wherein the melting temperature of the base resin is 260° C. or higher.
3. The material set for manufacturing a fiber-reinforced composite material according to claim 1 or 2, wherein the fibers of the fiber bundles are carbon fibers.
4. The material set for producing a fiber-reinforced composite material according to claim 1 or 2, which is a material set including the base resin, the fiber bundles, the sizing agent, and a filler.
5. The material set for manufacturing a fiber-reinforced composite material according to claim 1 or 2, wherein the base resin is a thermoplastic resin.
6. The material set for manufacturing a fiber-reinforced composite material according to claim 1 or 2, wherein the base resin is a polyamide resin.
7. The material set for manufacturing a fiber-reinforced composite material according to claim 1 or 2, wherein the matrix resin is a semi-aromatic polyamide resin.
8. A method for producing a fiber-reinforced composite material using the material set for producing a fiber-reinforced composite material according to claim 1 or 2, comprising the steps of: A method for producing a fiber-reinforced composite material, comprising: an impregnation step of impregnating the inter-fiber portions of the fiber bundle to which the sizing agent is attached with the matrix resin.
9. A fiber-reinforced composite material, comprising: a fiber bundle having a sizing agent attached thereto; and a fiber bundle having a sizing agent attached thereto; and a fiber bundle having a sizing agent attached thereto; and a fiber bundle having a sizing agent attached thereto;
10. A fiber-reinforced composite material, The composite material includes a matrix resin, a fiber bundle, and a sizing agent, The matrix resin has an amide group, the sizing agent is deposited on an outer surface of the fibers of the fiber bundle; The sizing agent has a phenolic hydroxyl group, When the fibers of the fiber bundles are glass fibers, the bending strength of the fiber-reinforced composite material measured in accordance with JIS K7017 is 500 MPa or more, When the fibers of the fiber bundles are fibers other than glass fibers, the fiber reinforced composite material has a bending strength of 1600 MPa or more as measured in accordance with JIS K7074.
Citation Information
Patent Citations
Carbon fiber chopped strand and method for producing the same
JP2003165849A
Carbon fiber bundle and carbon-fiber-reinforced composite material using the same
JP2014162999A