Cellulose nanofiber, and method for manufacturing composite body of the same
By processing cotton with a grinder at specific settings and forming a composite with an epoxy resin layer, the challenges of defibrating cotton and aggregating CNF are overcome, resulting in high-strength cellulose nanofibers with improved resin composition strength.
Patent Information
- Application Number
- JP2023044402
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
AI Technical Summary
Cotton fibers are difficult to defibrate, leading to high production costs and aggregation issues of cellulose nanofibers (CNF) due to their hydrophilicity and hydrogen bonding, making it challenging to combine them with hydrophobic polymers effectively.
A method involving the use of a grinder with specific concentration and clearance to process cotton to a certain size, followed by a composite formation with an epoxy resin layer without chemical modification, to produce high-strength CNF.
This approach enables the production of high-strength CNF at low cost and improves the strength of resin compositions by preventing aggregation and enhancing hydrophobicity.
Smart Images

Figure 2024134208000001 
Figure 2024134208000002 
Figure 2024134208000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing cellulose nanofibers and composites thereof. [Background technology]
[0002] Cellulose is the main component of plant cell walls and plant fibers, a natural polymer in which many β-glucose molecules are polymerized in a linear chain via glycosidic bonds, and is a component with a small environmental impact. Cellulose fibers are structured such that single cellulose nanofibers (single CNFs) with a basic unit width of 3 nm to 4 nm are bundled to form cellulose nanofibers (CNFs) with a basic unit width of 10 nm to 20 nm in the cell wall, which are further bundled to a thickness of several tens of μm (Non-Patent Document 1).
[0003] In recent years, it has become clear that CNFs have excellent properties, such as high elastic modulus, high strength, low coefficient of linear expansion, and gas barrier properties. In addition, because they are lighter than glass fiber, carbon fiber, and inorganic fillers, research and development is being conducted into a variety of applications for CNFs, such as resin reinforcement, paint additives, films, and thickeners.
[0004] The raw materials for CNF are generally pulps derived from broadleaf and coniferous trees that have a high hemicellulose content and are easy to defibrate (Non-Patent Document 2). The raw materials for CNF are non-wood pulps with their own characteristics, such as fast-growing kenaf, bagasse (a sugarcane residue), low-cost rice straw, and abaca, which has long fibers and can be used to make high-strength paper.
[0005] Cotton linter pulp has low hemicellulose and lignin content and can be used to produce high-quality CNF. Cotton linter pulp generally has the problem that it is expensive and difficult to defibrate and produce CNF.
[0006] Cotton is a material that has longer fibers than cotton linters and is expected to have higher strength. Cotton generally has the problem of being more difficult to defibrate than cotton linter pulp.
[0007] However, if cotton could be defibrated reproducibly, it would be possible to produce high-strength CNF at low cost, for example, by using scraps from manufacturing or recycled materials.
[0008] CNF manufacturing methods include (i) mechanical fiber defibration using a high-pressure dispersion device or grinder, (ii) chemically hydrophilizing pulp with a cationizing agent and then mechanical fiber defibration using a kneader, etc., and (iii) partially oxidizing the pulp using a TEMPO catalyst, etc. to facilitate chemical fiber defibration. Of the various CNF manufacturing methods, the mechanical fiber defibration process using a grinder is suitable for mass production in terms of raw material selectivity and cost.
[0009] Incidentally, CNF is rarely used alone, but is generally used in combination with organic components, organic solvents, etc.
[0010] The cellulose that makes up CNF has many hydroxyl groups on the glucose molecules, which means that hydrogen bonds between the hydroxyl groups are likely to occur, which results in the problem that the CNFs tend to aggregate. Another problem is that cellulose has many hydroxyl groups on its surface, which makes it extremely hydrophilic and therefore lacks affinity with hydrophobic organic solvents.
[0011] That is, CNF exists stably in water, but in general, when the water content is high, it is difficult to composite (especially melt-knead) with hydrophobic polymers, hydrolyzable polymers, etc. On the other hand, when CNF dries, it aggregates and becomes a residue in the polymer, which reduces the properties of CNF, making it difficult to exert the properties of CNF in the polymer (Non-Patent Document 3).
[0012] In order to solve such problems, methods for hydrophobizing CNF have been studied. The method for hydrophobizing CNF generally involves a chemical method of substituting the hydroxyl groups of CNF with hydrophobic substituents. This method is generally costly and only partially substitutes the hydroxyl groups, so there is a problem that aggregation due to hydrogen bonds cannot be suppressed.
[0013] These problems are particularly pronounced in CNF compared to ordinary cellulose fibers, because CNF has a large number of hydroxyl groups exposed on its surface relative to its solid weight. [Prior art documents] [Non-patent literature]
[0014] [Non-Patent Document 1] Hiroyuki Yano. "Production and Use of Cellulose Nanofibers." Journal of Functional Paper Research 49, 15-20 (2010) [Non-Patent Document 2] Akira Isogai. "Cellulose nanofiber." Surface Technology 71.6, 389-395 (2020) [Non-Patent Document 3] Tomohiro Hase. "Characteristics and Applications of Cellulose Nanofiber Reinforced Rubber Materials." Journal of the Society of Rubber Science and Technology of Japan 90.2, 30-35 (2017) Summary of the Invention [Problem to be solved by the invention]
[0015] The objective of the present invention is to defibrate cotton, which is difficult to defibrate, and produce high-strength cellulose nanofibers (CNF) at low cost.
[0016] The present invention aims to provide a composite that can improve the strength of a resin composition by hydrophobizing cellulose instead of substituting the hydroxyl groups of cellulose with hydrophobic substituents. [Means for solving the problem]
[0017] The inventors have discovered that high-strength cellulose nanofibers (CNFs) can be produced by processing cotton ground to a certain size using a grinder with a certain concentration and a certain range of clearance.
[0018] The present inventors have also discovered that by providing an epoxy resin layer on the surface of cellulose, it is possible to produce a composite having performance equal to or greater than that of conventional resin-reinforced composites, without chemically modifying the cellulose.
[0019] Based on this finding, the inventors have conducted further research and have completed the present invention.
[0020] That is, the present invention provides the following complex:
[0021] The present invention encompasses the following cellulose nanofibers (CNFs) and composites of CNFs and water-insoluble substances.
[0022] Section 1. A method for producing cellulose nanofibers, comprising the steps of: (1) mixing ground cotton fabric with water and adjusting the content of ground cotton fabric to 0.1% by weight to 4% by weight based on the total weight of the mixture; and (2) subjecting the mixture obtained in step (1) to a grinding process; The size of the ground cotton fabric is 400 mesh to 5 mm mesh or less, The manufacturing method, wherein the grinder has a clearance of 100 μm or less.
[0023] Section 2. 2. The method according to claim 1, wherein the mixture contains 90% by weight or more of water.
[0024] The method for producing the same according to item 1.
[0025] Section 3. 2. The method according to claim 1, wherein the cotton fabric is a recycled product of scraps from cotton manufacturing or a recycled product of used clothing.
[0026] Section 4. A method for producing cellulose nanofibers, comprising the steps of: (1) mixing ground cotton fabric with water and subjecting the mixture to a grinding process; and (2) A manufacturing method comprising the step of filtering the mixture that has been ground after step (1) to produce a slurry containing 6% or more by weight of cellulose nanofibers based on the total weight of the mixture.
[0027] Section 5. A method for producing cellulose nanofibers, comprising the steps of: (1) mixing ground cotton fabric with water and subjecting the mixture to a grinding process; and (3) A manufacturing method including a step of centrifuging or pressurizing the grinder-treated mixture after step (1) to produce a slurry containing 10% by weight or more of cellulose nanofibers based on the total weight of the mixture.
[0028] Section 6. A method for producing cellulose nanofibers, comprising the steps of: (1) A process for mixing ground cotton fabric with water and subjecting the mixture to a grinding process; (2) After step (1), the mixture treated with the grinder is filtered to produce a slurry containing 6% by weight or more of cellulose nanofibers based on the total weight of the mixture; and (3) A manufacturing method including a step of centrifuging or pressurizing the filtered slurry after step (2) to produce a slurry containing 10% by weight or more of cellulose nanofibers based on the weight of the total mixture.
[0029] Section 7. A method for producing a composite of cellulose nanofibers and a water-insoluble substance, comprising the steps of: (1) A process for mixing ground cotton fabric with water and subjecting the mixture to a grinding process; (2) after step (1), removing water from the mixture treated with the grinder and adjusting the solid content in the mixture to 10% by weight or more; and (3) A production method comprising the step of adding a water-insoluble substance and a water-soluble organic solvent to the mixture having a solid content adjusted to 10% by weight or more after the step (2).
[0030] Section 8. Furthermore, Item 10. The method for producing a cellulose nanofiber according to item 9, further comprising the steps of: (4) heating and reducing pressure to the mixture to which the water-insoluble substance and the water-soluble organic solvent have been added after step (3), removing water from the mixture, and adjusting the content of cellulose nanofibers to 20% by weight or more based on the total weight of the mixture.
[0031] Section 9. Item 9. The method according to item 7 or 8, wherein the boiling point of the water-soluble organic solvent is 110° C. or higher.
[0032] Section 10. Item 9. The method according to item 7 or 8, wherein the water-insoluble substance is an epoxy compound. Effect of the Invention
[0033] This invention makes it possible to produce high-strength cellulose nanofibers (CNF) by processing cotton ground to a certain size using a grinder with a certain concentration and a certain range of clearance.
[0034] The present invention can also provide a composite material capable of improving the strength of a resin composition without chemically modifying the cellulose surface. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0035] The present invention will be described in detail below.
[0036] The embodiments of the present invention are intended to provide a better understanding of the gist of the invention, and unless otherwise specified, do not limit the content of the invention.
[0037] In this specification, the terms "comprise" and "containing" are concepts which encompass all of "comprise," "consist essentially of," and "consist only of."
[0038] In this specification, when a numerical range is indicated as "A to B," it means "A or more and B or less."
[0039] In this specification, the designations parts, % etc. are generally used.
[0040] In this specification, unless otherwise specified, all parts by mass or % by mass (wt%) are used.
[0041] [1] Manufacturing method of cellulose nanofiber (CNF) The method for producing cellulose nanofiber (CNF) of the present invention is as follows: (1) mixing ground cotton fabric with water and adjusting the content of ground cotton fabric to 0.1% by weight to 4% by weight based on the total weight of the mixture; and (2) subjecting the mixture obtained in step (1) to a grinding process.
[0042] In the method for producing CNF, the mixture preferably contains 90% or more by weight of water.
[0043] In the method for producing CNF, the size of the ground cotton fabric is preferably 400 mesh to 5 mm mesh or less.
[0044] In the method for producing CNF, the cotton fabric is preferably a recycled product made from scraps from cotton manufacturing or recycled material from used clothing.
[0045] In the method for producing CNF, the grinder clearance is 100 μm or less, preferably 80 μm or less.
[0046] According to the CNF manufacturing method of the present invention, high-strength CNF can be produced by processing cotton ground to a certain size using a grinder with a certain concentration and a certain range of clearance.
[0047] The method for producing cellulose nanofiber (CNF) of the present invention is as follows: (1) mixing ground cotton fabric with water and subjecting the mixture to a grinding process; and (2) After step (1), the mixture that has been ground is filtered to produce a slurry containing 6% or more by weight of CNF based on the total weight of the mixture.
[0048] The method for producing cellulose nanofiber (CNF) of the present invention is as follows: (1) mixing ground cotton fabric with water and subjecting the mixture to a grinding process; and (3) After step (1), the grinder-treated mixture is centrifuged or pressurized to produce a slurry containing 10% by weight or more of CNF based on the total weight of the mixture.
[0049] The method for producing cellulose nanofiber (CNF) of the present invention is as follows: (1) a process for mixing ground cotton fabric with water and subjecting the mixture to a grinding process; (2) After step (1), the mixture treated with the grinder is filtered to produce a slurry containing 6% by weight or more of CNF based on the total weight of the mixture; and (3) After step (2), the filtered slurry is centrifuged or pressurized to produce a slurry containing 10% by weight or more of CNF based on the weight of the total mixture.
[0050] According to the CNF manufacturing method of the present invention, high-strength CNF can be produced by processing cotton ground to a certain size using a grinder with a certain concentration and a certain range of clearance.
[0051] [1-1] Cellulose As for the cellulose, cotton is preferably used, since it is expected to have strength superior to that of broad-leaved trees (eucalyptus, poplar, etc.), coniferous trees (pine, fir, cedar, cypress, etc.), and herbaceous plants (straw, bagasse, reed, kenaf, abaca, sisal, etc.).
[0052] From the viewpoint of lower cost than cotton linter pulp, the cellulose used is preferably a recycled product of scraps from cotton manufacturing or cotton derived from recycled clothing.
[0053] The cellulose may be at least one type of cellulose selected from the group consisting of the above-mentioned celluloses (broadleaf trees, coniferous trees, herbaceous plants, etc.), and these celluloses may be used alone or in combination (blend) of two or more types depending on the purpose.
[0054] The cellulose of the raw material to be mixed with cotton is determined based on the hemicellulose and lignin contents in the cellulose.
[0055] The higher the hemicellulose content in cellulose, the easier it is to defibrate during the production of cellulose nanofibers (CNFs).The higher the hemicellulose content in cellulose, the lower the elastic modulus of the resulting resin composition tends to be during the production of a composite.
[0056] The higher the lignin content in cellulose, the more difficult it is to defibrate during CNF production, and the more discoloration occurs due to heating.The higher the lignin content in cellulose, the more phenolic hydroxyl groups there are, so the more likely it is to react with aromatic epoxies, etc., during composite production, resulting in the desired crosslinking reaction.
[0057] The ratio of pure cellulose components in the raw cellulose to be mixed with cotton is appropriately set according to the intended use.
[0058] When CNF is used for the purpose of resin reinforcement, the ratio of the pure cellulose component is preferably 70% by mass or more, more preferably 80% by mass or more, based on 100% by mass of cellulose in order to effectively utilize the strength characteristics of the cellulose component. The upper limit of the ratio of the pure cellulose component can preferably be set to 100% by mass of cellulose.
[0059] The cellulose ratio is the ratio of pure cellulose components in which β-glucose molecules are polymerized in a linear chain via glycosidic bonds to the total mass of cellulose (100% by mass).
[0060] The degree of polymerization of the pure cellulose component contained in the raw cellulose to be mixed with cotton is appropriately set depending on the application of the composite.
[0061] The lower the degree of polymerization of the cellulose component, the easier the cellulose tends to be defibrated, whereas the higher the degree of polymerization of the cellulose component contained in the cellulose, the higher the elastic modulus of the resulting composite or composition.
[0062] In order to obtain a resin composition having high strength, the cellulose used is preferably a cellulose component having a degree of polymerization of 500 or more, more preferably a cellulose component having a degree of polymerization of 600 or more. The upper limit of the degree of polymerization of the cellulose component is not particularly limited, and is preferably about 100,000.
[0063] The cellulose raw material to be mixed with cotton tends to be more easily defibrated when the crystallinity of the pure cellulose component contained in the cellulose is low, whereas the cellulose can have a high elastic modulus when the crystallinity of the pure cellulose component contained in the cellulose is high.
[0064] In order to obtain a high-strength composition, the crystallinity of the pure cellulose component contained in the cellulose is preferably 60% or more, more preferably 70% or more. The upper limit of the crystallinity of the cellulose is not particularly limited, and is preferably 99%, more preferably 98%.
[0065] The crystal structure of the cellulose component may be type I, type II, type III, or type IV. Among them, from the viewpoint of reinforcing the resin, the cellulose component preferably has a type I crystal structure, which has a high elastic modulus and the like.
[0066] Size of cotton fabric grinds The ground cotton fabric is preferably between 400 mesh and 5 mm mesh.
[0067] When the mesh size of cotton fabric is coarse, the raw material may clog the grinder during defibration, and defibration may not be sufficient. When the mesh size of cotton is fine, it is costly to grind the raw material, and the fibers may be too short, which may weaken the reinforcing properties when compounded with resin or rubber. In addition, the material may be discharged with a short residence time in the grinder, and defibration may not be sufficient.
[0068] The mesh size of the ground cotton fabric is at least 400 mesh (a fine sieve with 400 openings per inch) and not more than 5 mm mesh (5 mm openings), preferably at least 100 mesh and not more than 2 mm mesh, and more preferably at least 80 mesh and not more than 2 mm mesh.
[0069] [1-2] Method for refining cellulose The method for finely pulverizing cellulose uses a grinder, which is a physical fiberization method that has a wide range of options for raw material components, sizes, and shapes and has high fiberization efficiency.
[0070] In the physical fiber defibration method, the diameter of the nanofibers is generally 10 nm to 1,000 nm.
[0071] In addition to the grinder, other fiber-disintegration methods may be used in combination.
[0072] The other defibration methods used in combination are preferably physical methods such as a high-pressure homogenizer method, an underwater collision method, a grinder method, a ball mill method, a biaxial kneading method, etc. By using other physical defibration methods in combination, the uniformity of defibration can be increased.
[0073] The other defibration method used in combination is preferably a chemical defibration method using a TEMPO catalyst, phosphoric acid, a dibasic acid, sulfuric acid, hydrochloric acid, etc. By using a chemical method in combination, it is possible to obtain even thinner cellulose nanofibers (CNF) with a diameter of 3 nm to 10 nm.
[0074] The smaller the diameter and the larger the aspect ratio of CNF, the higher the physical properties such as strength of the resin composition obtained during the production of the composite can be expected. However, the smaller the diameter and the larger the aspect ratio of CNF, the higher the viscosity during the production of the composite, which may reduce the production efficiency or cause aggregation, making it impossible to achieve high strength.
[0075] The solvent used for defibrating cellulose is preferably water-based. Because cellulose is hydrophilic and contains many hydroxyl groups, defibration efficiency is high when water is used as the solvent for defibrating cellulose. The content of water in the solvent for defibrating cellulose is preferably 80% by weight or more, more preferably 90% by weight or more.
[0076] In order to prevent the cellulose from drying out during defibration, the solvent used when cellulose is defibrated is preferably a hydrophilic solvent such as a glycerin-based or glycol-based solvent that contains a hydroxyl group and has a boiling point of more than 100°C, more preferably a solvent with a boiling point of 110°C or higher.
[0077] In order to facilitate removal of the solvent after defibration, it is preferable to add a solvent that is water-soluble and has a boiling point of 100° C. or less, such as alcohol or acetone, when cellulose is defibrated.
[0078] A water-soluble solvent is preferably added as a solvent for defibrating cellulose, for the purpose of compounding with an organic substance that is not soluble in pure water during or after defibration. The boiling point of the water-soluble solvent is not particularly limited. When water is to be removed after compounding, a water-soluble solvent having a boiling point higher than 100°C is preferably used. When the solvent is to be quickly removed after compounding, a water-soluble solvent having a boiling point of 100°C or less is preferably used.
[0079] The cellulose concentration (content of ground cotton fabric) is adjusted to 0.1 to 4.0% by weight (4% by weight) based on the total weight (total mixture of ground cotton fabric and water), preferably 0.5 to 3.6% by weight, and more preferably 1.0 to 3.4% by weight.
[0080] If the cellulose concentration is less than 0.1% by weight, the production efficiency of CNF tends to be poor.If the cellulose concentration is more than 4.0% by weight, the raw material may clog the grinder, and mainly only water may be discharged, which may further increase the cellulose concentration and prevent cellulose defibration.
[0081] grinder In the method for producing CNF, the grinder clearance is 100 μm or less, preferably 80 μm or less, and more preferably 1 μm to 70 μm. If the grinder clearance is more than 100 μm, cotton, which is generally difficult to defibrate, tends not to be sufficiently defibrated.
[0082] In order to defibrate cellulose in fewer cycles, it is preferable to narrow the clearance of the grinder. If the clearance of the grinder is narrow, defibration is sufficient, but if it is too narrow, the discharge amount per hour is small, and there is a risk that the grinder will become clogged, causing the device to stop, or only water will be discharged. If the clearance of the grinder is widened, the discharge amount per hour will increase, but if it is too wide, there is a risk that defibration is not sufficient.
[0083] The clearance of the grinder is more preferably 5 μm to 50 μm, and further preferably 10 μm to 40 μm.
[0084] [1-3] Post-fine processing The finely divided cellulose can be used as it is in the form of an aqueous dispersion.
[0085] When the finely divided cellulose is to be composited with other materials, particularly with water-insoluble substances, it is preferable to remove the solvent such as water.
[0086] In the CNF manufacturing method, the water can be easily removed by, for example, filtering the grinder-treated mixture (a mixture of ground cotton fabric and water). By simply filtering the grinder-treated mixture under its own weight, the CNF concentration can be increased to 6% by weight or more (i.e., a slurry containing 6% by weight or more can be produced) without using energy.
[0087] In the CNF manufacturing method, the grinder-processed mixture can be centrifuged or pressurized to increase the CNF concentration to 10% by weight or more (i.e., a slurry containing 10% by weight or more of CNF can be produced).
[0088] When the solvent contained in the mixture treated with a grinder is removed, the labor required for removing the solvent and the labor required for dissolving during compounding are increased. The more the solvent contained in the mixture treated with a grinder is removed, the easier it becomes to compound with a water-insoluble substance.
[0089] After the grinder-treated mixture has been removed of the solvent, the CNF concentration is preferably 6% by weight to 40% by weight, and more preferably 10% by weight to 30% by weight.
[0090] The CNF manufacturing method of the present invention can produce high-strength CNF by processing cotton ground to a certain size using a grinder with a certain concentration and a certain range of clearance.
[0091] [2] Manufacturing method for composite of cellulose nanofiber (CNF) and water-insoluble substance The method for producing a composite of cellulose nanofiber (CNF) and a water-insoluble substance of the present invention is as follows: (1) a process for mixing ground cotton fabric with water and subjecting the mixture to a grinding process; (2) after step (1), removing water from the mixture treated with the grinder and adjusting the solid content in the mixture to 10% by weight or more; and (3) After step (2), the method includes a step of adding a water-insoluble substance and a water-soluble organic solvent to the mixture whose solid content has been adjusted to 10% by weight or more.
[0092] The manufacturing method of the composite of CNF and water-insoluble substance is as follows: Preferably, further comprising: (4) After step (3), the mixture to which the water-insoluble substance and the water-soluble organic solvent have been added is heated and reduced pressure to remove water from the mixture and adjust the CNF content to 20% by weight or more based on the total weight of the mixture.
[0093] In the method for producing a composite of CNF and a water-insoluble substance, the boiling point of the water-soluble organic solvent is preferably 110°C or higher.
[0094] In the method for producing a composite of CNF and a water-insoluble substance, the water-insoluble substance is preferably an epoxy compound.
[0095] The manufacturing method of the present invention for producing a composite of CNF and a water-insoluble substance makes it possible to provide a composite that can improve the strength of a resin composition without chemically modifying the cellulose surface.
[0096] [2-1] Complexation with water-insoluble substances In a method for producing cellulose nanofibers (CNF), a composite can be produced by coating part or all of the cellulose surface of a grinder-processed mixture (a mixture of ground cotton fabric and water) with a water-insoluble substance in order to prevent the CNF from agglomerating and to impart hydrophobicity.
[0097] water insoluble substances The water-insoluble substance to be coated is preferably an epoxy compound having two or more epoxy groups per molecule, in order to react with both the cellulose and the resin during kneading to form a crosslinked structure, and the water-insoluble substance to be coated is preferably an epoxy compound having one epoxy group per molecule, in order to make the substance hydrophobic while avoiding the crosslinked structure.
[0098] The epoxy compound is preferably selected from those having an aliphatic structure or an aromatic structure. In order to improve the elastic modulus and heat resistance of the resulting resin composition, the epoxy compound is preferably an epoxy compound having a molecular weight of 350 or less, more preferably an epoxy compound having a molecular weight of 300 or less. The lower limit of the molecular weight of the epoxy compound is not particularly limited, and preferably an epoxy compound having a molecular weight of 100 or more is used.
[0099] When the composite is used in combination with a polyolefin resin that does not have a reactive group with epoxy, such as polyethylene (PE) or polypropylene (PP), from the viewpoint of making the composite more hydrophobic, it is preferable to use an epoxy compound having an aromatic ring structure or an epoxy compound that does not have an ether structure other than a glycidyl ether group.
[0100] By using an epoxy compound in which the aromatic ring has an aliphatic substituent in the composite, it is possible to obtain the effect of further increasing the hydrophobicity of the composite or imparting flexibility to the composite.Preferably, the epoxy compound used is o-cresyl glycidyl ether (glycidyl ether of o-cresol), p-tolyl glycidyl ether, m,p-cresyl glycidyl ether, p-tert-butylphenyl glycidyl ether, or the like.
[0101] The epoxy compound used in the composite preferably has both groups represented by the following general formulas (1) and (2), thereby making it possible to obtain the effect of controlling the hydrophobicity and flexibility of the composite. The epoxy compound used is preferably an epoxy compound having a glycidyl ether structure.
[0102] [ka]
[0103] [ka]
[0104] In general formula (2), R 1 , R 2 , and R 3 R preferably each independently represents any substituent or a hydrogen atom. 1 , R 2 , and R 3 More preferably, each independently represents a substituent selected from the group consisting of an alkyl group, an alkenyl group, a cycloalkyl group, an aryl group, and derivatives thereof, or a hydrogen atom.
[0105] The epoxy compound preferably has an ether structure, and an epoxy compound having only the ether structure represented by general formula (1) is used as the ether structure. The epoxy compound having only the ether structure represented by general formula (1) can further increase the hydrophobicity of the composite.
[0106] The compound having one epoxy group can be widely used among known compounds. The compound having one epoxy group is preferably an aliphatic alcohol-based epoxy compound, an epoxidized vegetable oil, an epoxidized rubber, an aromatic phenol-based epoxy compound, or the like.
[0107] The aliphatic alcohol-based epoxy compound is preferably a glycidyl ether of butanol (C4) to stearyl alcohol (C18). By using a glycidyl ether of butanol (C4) to stearyl alcohol (C18), the molecular weight of the epoxy compound is such that the elastic modulus and heat resistance of the resulting resin composition (composite) are good, the volatilization of the epoxy compound during the production of the composite can be suppressed, and the composite exerts an excellent hydrophobic effect.
[0108] The aliphatic alcohol-based epoxy compound is preferably a compound having a branched chain, such as glycidyl ether of ethylhexanol (C8).
[0109] As the aliphatic alcohol-based epoxy compound, it is more preferable to use a glycidyl ether having a carbon number of C4 to C18.
[0110] The general name for epoxidized vegetable oil is vegetable oil having epoxy groups obtained by oxidizing the double bonds of vegetable oils containing unsaturated fatty acids. The epoxidized vegetable oil preferably used is epoxidized soybean oil, epoxidized linseed oil, or the like.
[0111] The epoxidized rubber used is preferably epoxidized polybutadiene, epoxidized SEBS, epoxidized SBS, epoxidized natural rubber, or the like.
[0112] As the aromatic phenol-based epoxy compound, an aromatic phenol-based glycidyl ether is preferably used. As the aromatic phenol-based epoxy compound, a glycidyl ether of phenol, a glycidyl ether of its substituted derivative (cresol, t-butylphenol), a glycidyl ether of orthophenylphenol, a glycidyl ether of naphthol, a glycidyl ether of a fluorene derivative, or the like is more preferably used.
[0113] As the aromatic phenol-based epoxy compound, from the viewpoints of heat resistance, compatibility with resin, and elastic modulus, a glycidyl ether of a fluorene derivative is preferably used.
[0114] The content of the epoxy compound in the composite is preferably 2 to 100 parts by mass, and more preferably 5 to 75 parts by mass, per 100 parts by mass of cellulose nanofiber (CNF) (solid content equivalent). By adjusting the content of the epoxy compound in the composite, it is possible to prevent aggregation of CNF in the composite and to obtain the effect of hydrophobizing the CNF.
[0115] The thickness of the epoxy resin layer is not particularly limited, and is preferably 1 nm to 1,000 nm.
[0116] The epoxy resin layer preferably contains, in addition to the epoxy compound, a curing agent for the epoxy resin, a cure accelerator, an inorganic metal oxide, a carbon material, and the like, depending on the intended use of the composite and the resin composition.
[0117] The water-insoluble coating material is not limited to epoxy compounds.
[0118] The water-insoluble substance to be coated is not particularly limited, and is used for the purpose of making the surface hydrophobic, and preferably, a component having a functional group capable of chemically reacting with cellulose is used. The water-insoluble substance to be coated is preferably an isocyanate compound, an acid anhydride compound, or a compound having a carboxylic acid.
[0119] The non-water-soluble coating material can be any material that is not expected to chemically react with cellulose nanofiber (CNF).
[0120] The water-insoluble coating material is preferably a compound having a nitrogen atom and a hydrogen atom (an amine compound capable of forming hydrogen bonds with cellulose), a compound having an oxygen atom and a hydrogen atom (a compound having an alcoholic hydroxyl group, a phenolic hydroxyl group, etc.), a compound having a fluorine atom or a chlorine atom, etc., for the purpose of preventing aggregation of CNF while coating the surface with a hydrophobic material.
[0121] The water-insoluble coating material does not need to have a reactive functional group in order to prevent the CNF from agglomerating. The water-insoluble coating material may be an emulsion of oil or resin in order to prevent the CNF from agglomerating.
[0122] The water-insoluble substance may be at least one selected from the group consisting of the water-insoluble substances described above. These water-insoluble substances may be used alone or in combination (blend) of two or more types depending on the purpose.
[0123] Water-soluble organic solvent A water-insoluble compound is dissolved or dispersed in an organic solvent (preferably a water-soluble organic solvent) and then mixed with wet cellulose nanofibers (CNF) to obtain a composite.
[0124] The mixture containing CNF, an organic solvent (a water-soluble organic solvent), water, and a water-insoluble compound can be used as is. Preferably, a part or all of the solvent is removed from the mixture containing CNF, an organic solvent (a water-soluble organic solvent), water, and a water-insoluble compound depending on the purpose.
[0125] In the composite, a part of the solvent may be left in order to improve the dispersibility of the CNF in the thermoplastic resin or the thermosetting resin. In the composite, the content ratio of the CNF in the total weight is preferably 10% by weight or more, more preferably 20% by weight or more, even more preferably 25% by weight or more, and particularly preferably 30% by weight or more, from the viewpoint of ease of removing the solvent.
[0126] From the viewpoint of kneading and mixing in a device that cannot remove the solvent, and from the viewpoint of the degree of freedom of blending, such as mixing with non-hydrophilic substances, all or most of the solvent may be removed. In the composite, the content ratio of CNF in the total weight is preferably 80% by weight or more, more preferably 90% by weight or more, and even more preferably 95% by weight or more, from the viewpoint of ease of removing the solvent.
[0127] The organic solvent may be a wide variety of known organic solvents. The organic solvent is preferably a water-soluble organic solvent. In order to prevent the aggregation of cellulose while removing water when obtaining a resin composition, the organic solvent is preferably an organic solvent having a boiling point of 110° C. or more. In order to easily remove the organic solvent, the organic solvent is preferably an organic solvent having a boiling point of 250° C. or less.
[0128] When kneading with a hydrolyzable resin while containing an organic solvent, it is preferable to use an organic solvent that does not have a hydroxyl group in order to avoid alcoholysis when kneading with a hydrolyzable resin.
[0129] The organic solvent is preferably a water-soluble organic solvent, and preferably an amphiphilic organic solvent such as an alcohol, ketone, glycol, lactone, lactam, amide, sulfoxide, or ether having affinity for both water and epoxy is used.
[0130] Considering that the composition will be kneaded with the solvent remaining in the composition, it is preferable to use an organic solvent such as a ketone-based organic solvent, a glycol-based organic solvent having etherified terminals and no hydroxyl groups, a lactone-based organic solvent, a lactam-based organic solvent, an amide-based organic solvent, or a sulfoxide-based organic solvent.
[0131] The organic solvent may be at least one selected from the group consisting of the above organic solvents. These organic solvents may be used alone or in combination (blend) of two or more depending on the purpose.
[0132] Complex The composite can be used by mixing with thermoplastic resins, thermosetting resins, photocurable resins, rubbers, elastomers, etc.
[0133] Cellulose has polarity even when it forms a complex. The resin to be mixed has compatibility with the excess epoxy. The resin to be mixed is not particularly limited, and preferably, a polyester resin, a polyamide resin, a polycarbonate resin, or the like is used.
[0134] The composite has epoxy on its surface and is in a low polarity state as a composite. The resin to be mixed is preferably a low polarity resin such as polyolefins such as polyethylene (PE) and polypropylene (PP), polystyrene (PS), ABS resin, SEBS resin, SBS resin, AS resin, or other polystyrene-based resins.
[0135] From the viewpoint of environmental friendliness, it is preferable to increase the biomass ratio of the resin to be mixed, and biomass plastics, microbially produced plastics, etc. are used.
[0136] The resin may be at least one resin selected from the group consisting of the above-mentioned resins. These resins may be used alone or in combination (blend) of two or more types depending on the purpose.
[0137] The composite preferably uses rubber, thermoplastic elastomers, and the like, because they take advantage of the high elastic modulus of cellulose.
[0138] The rubber to be used is preferably a diene rubber, an olefin rubber, an acrylic rubber, a butyl rubber, an epichlorohydrin rubber, a silicone rubber, a polysulfide rubber, a fluororubber, etc. From the viewpoint of compatibility, the rubber to be used is preferably a diene rubber, an olefin rubber, etc.
[0139] As the diene rubber, preferably, styrene-butadiene rubber, isoprene rubber, butadiene rubber, chloroprene rubber, acrylonitrile-butadiene rubber, or the like is used.
[0140] As the olefin-based rubber, preferably, ethylene-propylene rubber, ethylene-propylene-diene rubber, or the like is used.
[0141] The rubber used may be at least one type of rubber selected from the group consisting of the above rubbers. These rubbers may be used alone or in combination (blended) of two or more types depending on the purpose.
[0142] The thermoplastic elastomer is preferably a styrene-based, olefin-based, ester-based, urethane-based, amide-based, polyvinyl chloride-based, or fluorine-based thermoplastic elastomer. From the viewpoint of compatibility, the thermoplastic elastomer is preferably an olefin-based, ester-based, or amide-based thermoplastic elastomer.
[0143] The thermoplastic elastomer is preferably one having a polyethylene structure, a polypropylene structure, a butadiene structure, a polyethylene terephthalate structure, a polyamide 6 structure, a polyamide 66 structure, a polyamide 11 structure, or a polyamide 12 structure, and may contain a styrene structure, which is a different system, while having an olefin structure or a diene structure, such as a styrene-ethylene-butylene-styrene copolymer, a styrene-butadiene-styrene copolymer, or a styrene-butylene-butadiene-styrene copolymer.
[0144] The thermoplastic elastomer may be at least one type of thermoplastic elastomer selected from the group consisting of the above-mentioned thermoplastic elastomers. These thermoplastic elastomers may be used alone or in combination (blended) in two or more types depending on the purpose.
[0145] The composite preferably uses polylactic acid, polyamide 4, polyamide 11, polybutylene succinate, polyhydroxybutyrate, etc. The composite preferably uses PE, PP, and copolymers having the same structure (random polymer, block polymer).
[0146] The method for producing a composite of CNF and a water-insoluble substance of the present invention can produce a composite that can improve the strength of the resin composition without chemically modifying the cellulose surface. EXAMPLES
[0147] The present invention will be specifically described below with reference to examples.
[0148] The present invention is not limited to the following specific examples.
[0149] Example 1 Clothing scraps were crushed through a 5 mm mesh and mixed with 500 g of cotton fabric to make a total weight of 20 kg. The content ratio of crushed cotton fabric to the total weight of the mixture was adjusted to 2.5% by weight (500 g / 20 kg).
[0150] The mixture was then defibrated by three passes using a grinder (clearance 20 μm) to obtain an aqueous dispersion containing cellulose nanofibers (CNF).
[0151] (Clothing scraps before defibration)
[0152] [ka]
[0153] (After defibration)
[0154] [ka]
[0155] Example 2 Defibration was performed in the same manner as in Example 1, except that cotton woven fabric made from clothing scraps crushed using a 2 mm mesh was used and the number of passes was changed to one pass.
[0156] Next, 800 g of the CNF aqueous dispersion was filtered to obtain 100 g of a water-wetted body containing 20 g (20 wt%) of solids. Next, 200 g of diethylene glycol dimethyl ether and 10 g of phenoxyethanol fluorenediglycidyl ether (50 parts by mass of epoxy compound per 100 parts by mass of CNF) were added to this water-wetted body, and the mixture was stirred and then decompressed at 80° C. to obtain about 100 g of a composite wetted with diethylene glycol dimethyl ether.
[0157] Thereafter, 100 g of the composite and 170 g of polylactic acid (TE-2000 manufactured by Unitika) were melt-kneaded at 190° C. using a twin-screw extruder (manufactured by Technovel, 15 mmφ, L / D=30) to obtain 150 g of a resin composition.
[0158] The resin composition thus obtained was dried at 80°C for 24 hours, and then molded into a dumbbell test piece having a length of 75 mm, a parallel part width of 5 mm, a parallel part length of 35 mm, and a thickness of 2 mm using an injection molding machine (Shinko Selvick, C,MOBILE-0813). A tensile test was performed on this test piece using a universal material testing machine (Instron 5567) at an ambient temperature of 23°C, a tensile speed of 10 mm / min, and n=5, and the tensile strength was calculated.
[0159] The tensile strength of the test piece was 83.8 MPa.
[0160] [ka]
[0161] Comparative Example 1 The experiment was carried out in the same manner as in Example 2, except that the raw cotton woven fabric was changed to a 10 mm mesh.
[0162] The mesh size of the cotton fabric was coarse, and an aqueous dispersion containing CNF was obtained in the initial stage of defibration, but the cotton clogged the grinder, making it impossible to discharge and defibrate stably.
[0163] [ka]
[0164] Example 3 The experiment was carried out in the same manner as in Example 2, except that the raw cotton fabric was changed to 20 mesh.
[0165] An aqueous dispersion containing CNF was obtained.
[0166] The tensile strength of the test piece was 75.7 MPa.
[0167] [ka]
[0168] Example 4 The experiment was carried out in the same manner as in Example 1, except that the raw cotton fabric was changed to 80 mesh.
[0169] As a result, an aqueous dispersion containing CNF was obtained, with some fibers measuring 500nm to 1,000nm in diameter also being observed.
[0170] [ka]
[0171] Example 5 An experiment was carried out in the same manner as in Example 1, except that the grinder clearance was changed to 80 μm.
[0172] As a result, an aqueous dispersion containing CNF was obtained. Many fibers with diameters of 500nm to 1,000nm were observed. If the clearance was made wider than this, it is thought that fibers with diameters of 1,000nm or more would be mixed in.
[0173] [ka]
[0174] Comparative Example 2 An experiment was carried out in the same manner as in Example 1, except that the grinder clearance was changed to 120 μm.
[0175] As a result, although some fiber cleavage and some nanofiberization were observed, the cotton was hardly defibrated.
[0176] [ka]
[0177] Comparative Example 3 The experiment was carried out in the same manner as in Example 3, except that the raw cotton fabric was changed to absorbent cotton.
[0178] As a result, the absorbent cotton became clogged inside the grinder and could not be discharged or defibrated.
[0179] Comparative Example 4 The experiment was carried out in the same manner as in Example 3, except that the concentration of the raw cotton fabric was 4.1% by weight.
[0180] As a result, the water was discharged, but almost no CNF was discharged, and the cotton became concentrated in the grinder, making it impossible to defibrate it stably.
[0181] Comparative Example 5 The experiment was carried out in the same manner as in Example 2, except that the raw cotton fabric was changed to Cellulose Powder KC Flock 50GK.
[0182] As a result, nanofibers of nano to submicron size were obtained. The tensile strength of the test piece was 62 MPa. The tensile strength of the test piece was lower than that of the CNF made from cotton fabric.
[0183] [ka]
[0184] Comparative Example 6 The experiment was carried out in the same manner as in Example 2, except that the raw cotton fabric was changed to hardwood pulp.
[0185] As a result, CNF was obtained. The tensile strength of the test piece was 65 MPa. The tensile strength of the test piece was lower than that of the CNF made from cotton fabric.
[0186] [ka]
[0187] Comparative Example 7 The experiment was carried out in the same manner as in Example 2, except that the raw cotton fabric was changed to abaca pulp.
[0188] As a result, CNF was obtained. The tensile strength of the test piece was 64 MPa. The tensile strength of the test piece was lower than that of the CNF made from cotton fabric.
[0189] [ka]
[0190] Comparative Example 8 The experiment was carried out in the same manner as in Example 2, except that the raw cotton fabric was changed to kenaf pulp.
[0191] As a result, CNF was obtained. The tensile strength of the test piece was 63 MPa. The tensile strength of the test piece was lower than that of the CNF made from cotton fabric.
[0192] [ka]
[0193] Comparative Example 9 The experiment was carried out in the same manner as in Example 2, except that the raw cotton fabric was changed to bagasse pulp.
[0194] As a result, CNF was obtained. The tensile strength of the test piece was 69 MPa. The tensile strength of the test piece was lower than that of the CNF made from cotton fabric.
[0195] [ka]
[0196] As shown in the examples, cotton fabric was successfully defibrated by grinding it with a constant concentration and constant clearance. As shown in the examples, when the CNF obtained by defibrating cotton was composited with resin, a composite resin with higher strength was obtained compared to CNF from other cellulose sources.
[0197] [Industrial Applicability] This invention makes it possible to produce high-strength cellulose nanofibers (CNF) by processing cotton ground to a certain size in a grinder with a certain concentration and a certain range of clearance.
[0198] The present invention also makes it possible to produce a composite that can improve the strength of a resin composition without chemically modifying the cellulose surface.
Claims
1. A method for producing cellulose nanofibers, comprising the steps of: (1) mixing ground cotton fabric with water and adjusting the content of ground cotton fabric to 0.1% to 4% by weight based on the total weight of the mixture; and (2) subjecting the mixture obtained in step (1) to a grinding process; The size of the ground cotton fabric is 400 mesh to 5 mm mesh or less; The manufacturing method, wherein the grinder has a clearance of 100 μm or less.
2. The method according to claim 1 , wherein the mixture contains 90% by weight or more of water.
3. The method according to claim 1, wherein the cotton fabric is a recycled product of scraps from cotton manufacturing or a recycled product of used clothing.
4. A method for producing cellulose nanofibers, comprising the steps of: (1) mixing ground cotton fabric with water and subjecting the mixture to a grinding process; and (2) After step (1), the mixture that has been subjected to the grinding process is filtered to produce a slurry containing 6% or more by weight of cellulose nanofibers based on the total weight of the mixture.
5. A method for producing cellulose nanofibers, comprising the steps of: (1) mixing ground cotton fabric with water and subjecting the mixture to a grinding process; and (3) A manufacturing method including a step of centrifuging or pressurizing the grinder-treated mixture after step (1) to produce a slurry containing 10% by weight or more of cellulose nanofibers based on the total weight of the mixture.
6. A method for producing cellulose nanofibers, comprising the steps of: (1) A process for mixing ground cotton fabric with water and subjecting the mixture to a grinding process; (2) After step (1), the mixture treated with the grinder is filtered to produce a slurry containing 6% by weight or more of cellulose nanofibers based on the total weight of the mixture; and (3) A manufacturing method including a step of centrifuging or pressurizing the filtered slurry after step (2) to produce a slurry containing 10% by weight or more of cellulose nanofibers based on the weight of the total mixture.
7. A method for producing a composite of cellulose nanofibers and a water-insoluble substance, comprising the steps of: (1) A process for mixing ground cotton fabric with water and subjecting the mixture to a grinding process; (2) after step (1), removing water from the mixture treated with the grinder and adjusting the solid content in the mixture to 10% by weight or more; and (3) A production method including the step of adding a water-insoluble substance and a water-soluble organic solvent to the mixture having a solid content of 10% by weight or more after the step (2).
8. Furthermore, The manufacturing method according to claim 9, further comprising the step of (4) heating and reducing the pressure of the mixture to which the water-insoluble substance and the water-soluble organic solvent have been added after step (3), removing water from the mixture, and adjusting the content of cellulose nanofibers to 20% by weight or more based on the total weight of the mixture.
9. 9. The method according to claim 7, wherein the water-soluble organic solvent has a boiling point of 110° C. or higher.
10. 9. The method according to claim 7, wherein the water-insoluble substance is an epoxy compound.