Ethylenic copolymer composition and applications thereof
The ethylene copolymer composition with specific ethylene, α-olefin, and non-conjugated polyene ratios, combined with a modified copolymer and transpolyoctenylene, addresses adhesion issues in conventional ethylene/α-olefin/nonconjugated polyene copolymers, enhancing lamination and mechanical strength for industrial materials.
Patent Information
- Application Number
- JP2023044741
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional ethylene/α-olefin/nonconjugated polyene copolymers face challenges in achieving sufficient adhesion to synthetic fibers, which hampers the lamination process and reduces the productivity of industrial materials.
An ethylene copolymer composition comprising specific ratios of ethylene, α-olefin, and non-conjugated polyene, along with a modified ethylene/α-olefin copolymer and transpolyoctenylene, enhances adhesion to fiber materials, facilitating improved lamination and mechanical strength.
The composition improves adhesion and mechanical strength, enabling faster production and better performance in applications such as hoses and belts.
Smart Images

Figure 2024134436000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a crosslinkable ethylene copolymer composition, a laminate using said composition and a layer containing a fiber material, and uses thereof. [Background technology]
[0002] Ethylene-α-olefin-non-conjugated polyene copolymers such as EPDM generally have excellent weather resistance, heat resistance, and ozone resistance, and are used in industrial materials such as automotive industrial parts, industrial rubber products, electrical insulating materials, civil engineering and construction materials, and rubberized fabrics. Conventional ethylene-α-olefin-non-conjugated polyene copolymers have the disadvantage of inferior adhesion to synthetic fibers compared to polar rubbers such as nitrile rubber, chloroprene rubber, and chlorosulfonated polyethylene. As a method to solve this drawback, it has been disclosed that an adhesive solution of a chlorosulfonated copolymer is used to improve the adhesion between ethylene-α-olefin-non-conjugated polyene copolymer and synthetic fibers (Patent Document 1). However, in today's world where environmental issues such as non-halogenation are a concern, it is difficult to say that such adhesive technology that utilizes the polarity of halogenation is optimal. Also, a conventional adhesive method is known in which synthetic fibers are treated with resorcinol-formaldehyde latex (RFL) and then embedded in rubber to crosslink and adhere. More specifically, a method is known in which isocyanates or isocyanuric acid derivatives are used in the RFL treatment. However, even if these methods are applied to rubbers that use ethylene-α-olefin-non-conjugated polyene copolymers, it is difficult to obtain sufficient adhesion. Also, in order to improve compression set resistance, it has been proposed to compound a sulfur-vulcanized ethylene propylene rubber compound in which zinc oxide made by compounding an ethylene-α-olefin-diene copolymer with trans-polyoctenylene rubber is compounded (Patent Document 2). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Special Publication No. 42-23632 [Patent Document 2] Patent No. 2528033 Summary of the Invention [Problem to be solved by the invention]
[0004] On the other hand, molded articles such as industrial materials are made by laminating or bonding a plurality of materials depending on the application, and the work process is one of the factors that reduce the productivity of industrial materials. An object of the present invention is to obtain an ethylene-based copolymer composition having improved adhesiveness, which can facilitate lamination of other materials, such as layers containing fibrous materials, and improve the productivity of molded articles. [Means for solving the problem]
[0005] The present invention relates to the following items [1] to
[11] . [1] An ethylene copolymer composition comprising the following components (A) and (B): (A): An ethylene-α-olefin-non-conjugated polyene copolymer containing ethylene [L], an α-olefin [M] having 4 to 20 carbon atoms, and a non-conjugated polyene [N], which satisfies the requirements (a-1) to (a-4) below. <Requirement (a-1)> The molar ratio [[L] / [M]] of the structural unit derived from ethylene [L] to the structural unit derived from an α-olefin [M] having 4 to 20 carbon atoms is 40 / 60 to 90 / 10. <Requirement (a-2)>: The content of the structural unit derived from the non-conjugated polyene [N] is 0.1 to 6.0 mol % with the total of the structural units [L], [M] and [N] being 100 mol %. <Requirement (a-3)> The Mooney viscosity at 125°C, ML(1+4)125°C, is 5 to 100. <Requirement (a-4)>: The B value represented by the following formula (i) is 1.20 or more. B value=([EX]+2[Y]) / [2×[E]×([X]+[Y])]···(i) [Here, [E], [X] and [Y] respectively represent the mole fractions of ethylene [L], α-olefin [M] having 4 to 20 carbon atoms, and non-conjugated polyene [N], and [EX] represents the dyad chain fraction of ethylene [L]-α-olefin [M] having 4 to 20 carbon atoms.] (B): A modified ethylene-α-olefin copolymer satisfying the following requirements (b-1) to (b-3). <Requirement (b-1)>: The content of structural units derived from ethylene is in the range of 15 to 85 mol % (provided that the total content of structural units derived from ethylene and the content of structural units derived from α-olefins is 100 mol %). <Requirement (b-2)>: The weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) is in the range of 1,000 to 100,000. <Requirement (b-3)>: A modified ethylene-α-olefin copolymer having a substituent derived from a compound having a carbon-carbon unsaturated bond, and the content of the moiety derived from the compound having a carbon-carbon unsaturated bond in the modified ethylene-α-olefin copolymer is in the range of 1 to 70 mass %. [2] Item [1]: The ethylene-based copolymer composition according to item [1], wherein the α-olefin [M] having 4 to 20 carbon atoms constituting the ethylene-α-olefin-non-conjugated polyene copolymer (A) is 1-butene. [3] The modified ethylene-α-olefin copolymer (B) satisfies the requirement (b-1) above, in which the ethylene structural unit content is in the range of 40 to 60 mol %, and the requirement (b-2) above, in which the weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) is in the range of 2,000 to 80,000; The ethylene-based copolymer composition according to item [1] or [2], wherein, in the requirement (b-3), the compound having a carbon-carbon unsaturated bond is one or more compounds selected from a vinyl aromatic compound, an unsaturated carboxylic acid, and an unsaturated carboxylic acid derivative, and the content of the moiety derived from the compound having a carbon-carbon unsaturated bond in the modified ethylene-α-olefin copolymer is in the range of 1 to 40 mass%. [4] The ethylene-based copolymer composition according to item [3], wherein the modified ethylene-α-olefin copolymer (B) satisfies requirement (b-3), the compound having a carbon-carbon unsaturated bond is a vinyl aromatic compound, and the content of the portion derived from the vinyl aromatic compound is in the range of 3 to 40 mass%. [5] The ethylene-based copolymer composition according to any one of items [1] to [4], comprising 0.5 to 100 parts by mass of the modified ethylene-α-olefin copolymer (B) per 100 parts by mass of the ethylene-α-olefin-non-conjugated polyene copolymer (A). [6] The ethylene copolymer composition according to any one of items [1] to [5], which contains a trans-polyoctenylene (C). [7] Item [6]. The ethylene-based copolymer composition according to item [6], comprising 0.5 to 50 parts by mass of trans-polyoctenylene (C) per 100 parts by mass of the ethylene-α-olefin-non-conjugated polyene copolymer (A). [8] A layer [I] made of the ethylene copolymer composition according to any one of items [1] to [7]; and a layer [II] containing a fibrous material. [9] Item [8] The laminate according to item [8], wherein the ethylene copolymer composition is crosslinked.
[10] The laminate according to item [8] or [9], wherein the fiber material of the layer [II] is canvas.
[11] An industrial belt comprising the laminate according to any one of items [8] to
[10] . Effect of the Invention
[0006] The ethylene copolymer composition of the present invention has improved adhesion to other materials, for example, layers containing fiber materials, when used to produce laminates, allowing the production rate to be increased. Furthermore, the laminate obtained by crosslinking has good mechanical strength and can be used for a wide range of applications, including hoses, belts, etc. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] <Ethylene-α-olefin-non-conjugated polyene copolymer (A)> The ethylene-α-olefin-non-conjugated polyene copolymer (A), which is the component (A) contained in the ethylene-based copolymer composition of the present invention and the ethylene-based copolymer composition forming the layer [I] of the laminate of the present invention, is an ethylene-α-olefin-non-conjugated polyene copolymer that contains a structural unit derived from ethylene [L], a structural unit derived from an α-olefin [M] having 4 to 20 carbon atoms, and a structural unit derived from a non-conjugated polyene [N] and satisfies the following requirements (a-1) to (a-4). Such a specific ethylene-α-olefin-non-conjugated polyene copolymer is also referred to as "ethylene-based copolymer (A)" and may be abbreviated as "ethylene-based copolymer (A)".
[0008] The α-olefin [M] having 4 to 20 carbon atoms and the non-conjugated polyene [N] may each be used alone or in combination of two or more. That is, the ethylene-α-olefin-non-conjugated polyene copolymer (A) according to the present invention contains a structural unit derived from ethylene [L], a structural unit derived from at least one kind of α-olefin [M] having 4 to 20 carbon atoms, and a structural unit derived from at least one kind of non-conjugated polyene [N]. The ethylene [L], the α-olefin [M], and the non-conjugated polyene [N] may be derived from biomass. <Requirement (a-1)> The molar ratio [[L] / [M]] of the structural unit derived from ethylene [L] to the structural unit derived from an α-olefin [M] is 40 / 60 to 90 / 10, <Requirement (a-2)> The content of the structural unit derived from the non-conjugated polyene [N] is 0.1 to 6.0 mol % based on 100 mol % of the total of the structural units of [L], [M] and [N], <Requirement (a-3)>: Mooney viscosity ML(1+4)125°C at 125°C is 5 to 100, <Requirement (a-4)>: The B value represented by the following formula (i) is 1.20 or more. B value=([EX]+2[Y]) / [2×[E]×([X]+[Y])]···(i) [Here, [E], [X] and [Y] respectively represent the mole fractions of ethylene [L], α-olefin [M] having 4 to 20 carbon atoms, and non-conjugated polyene [N], and [EX] represents the ethylene [L]-α-olefin [M] having 4 to 20 carbon atoms dyad chain fraction.]
[0009] Examples of the α-olefin [M] having 4 to 20 carbon atoms include 1-butene having 4 carbon atoms, which has a linear structure without side chains, through 1-nonene having 9 carbon atoms and 1-decene having 10 carbon atoms, 1-nonadecene having 19 carbon atoms, 1-eicosene having 20 carbon atoms, and 4-methyl-1-pentene, 9-methyl-1-decene, 11-methyl-1-dodecene, 12-ethyl-1-tetradecene, and the like having side chains.
[0010] These α-olefins [M] can be used alone or in combination of two or more. Among these, α-olefins having 4 to 10 carbon atoms are preferred, and 1-butene, 1-hexene, 1-octene, etc. are particularly preferred, with 1-butene being particularly preferred.
[0011] Specific examples of the non-conjugated polyene [N] include linear non-conjugated dienes such as 1,4-hexadiene, 1,6-octadiene, 2-methyl-1,5-hexadiene, 6-methyl-1,5-heptadiene, and 7-methyl-1,6-octadiene; cyclohexadiene, dicyclopentadiene, methyltetrahydroindene, 5-vinyl-2-norbornene, 5-ethylidene-2-norbornene, 5-methylene-2-norbornene, and 5-isopropylidene-2-norbornene. cyclic non-conjugated dienes such as norbornene and 6-chloromethyl-5-isopropenyl-2-norbornene; and trienes such as 2,3-diisopropylidene-5-norbornene, 2-ethylidene-3-isopropylidene-5-norbornene, 2-propenyl-2,5-norbornadiene, 1,3,7-octatriene, 1,4,9-decatriene, 4,8-dimethyl-1,4,8-decatriene, and 4-ethylidene-8-methyl-1,7-nonadiene.
[0012] These non-conjugated polyenes [N] can be used alone or in combination of two or more kinds. Among these, linear non-conjugated dienes such as 1,4-hexadiene, and cyclic non-conjugated dienes such as 5-ethylidene-2-norbornene, 5-ethylidene-2-norbornene, and 5-vinyl-2-norbornene are preferred, and among these, cyclic non-conjugated dienes are preferred, with 5-ethylidene-2-norbornene and 5-vinyl-2-norbornene being particularly preferred.
[0013] Examples of the ethylene copolymer (A) include the following: ethylene-1-butene-1,4-hexadiene copolymer, ethylene-1-pentene-1,4-hexadiene copolymer, ethylene-1-hexene-1,4-hexadiene copolymer, ethylene-1-heptene-1,4-hexadiene copolymer, ethylene-1-octene-1,4-hexadiene copolymer, ethylene-1-nonene-1,4-hexadiene copolymer, ethylene-1-decene-1,4-hexadiene copolymer, and ethylene-1-butene-1-octene-1,4-hexadiene copolymer. , ethylene-1-butene-5-ethylidene-2-norbornene copolymer, ethylene-1-pentene-5-ethylidene-2-norbornene copolymer, ethylene-1-hexene-5-ethylidene-2-norbornene copolymer, ethylene-1-heptene-5-ethylidene-2-norbornene copolymer, ethylene-1-octene-5-ethylidene-2-norbornene copolymer, ethylene-1-nonene-5-ethylidene-2-norbornene copolymer, ethylene-1-decene-5-ethylidene-2-norbornene copolymer Norbornene copolymer, ethylene-1-butene-1-octene-5-ethylidene-2-norbornene copolymer, ethylene-1-butene-5-ethylidene-2-norbornene-5-vinyl-2-norbornene copolymer, ethylene-1-pentene-5-ethylidene-2-norbornene-5-vinyl-2-norbornene copolymer, ethylene-1-hexene-5-ethylidene-2-norbornene-5-vinyl-2-norbornene copolymer, ethylene-1-heptene-5-ethylidene-2-norbornene-5-vinyl-2-norbornene copolymer Ethylene-1-octene-5-ethylidene-2-norbornene-5-vinyl-2-norbornene copolymer, Ethylene-1-nonene-5-ethylidene-2-norbornene-5-vinyl-2-norbornene copolymer, Ethylene-1-decene-5-ethylidene-2-norbornene-5-vinyl-2-norbornene copolymer, Ethylene-1-butene-1-octene-5-ethylidene-2-norbornene-5-vinyl-2-norbornene copolymer. The ethylene copolymer (A) may be used alone or in combination of two or more, as required.
[0014] The ethylene copolymer (A) according to the present invention satisfies the following (a-1) to (a-4). <Requirement (a-1)> The ethylene-based copolymer (A) has a molar ratio [[L] / [M]] of structural units derived from ethylene [L] to structural units derived from an α-olefin [M] having 4 to 20 carbon atoms of 40 / 60 to 90 / 10. The ethylene-based copolymer (A) having a molar ratio within the above range has an excellent balance between rubber elasticity at low temperatures and tensile strength at room temperature. The lower limit of [L] / [M] is preferably 45 / 55, more preferably 50 / 50, and particularly preferably 55 / 45. The upper limit of [L] / [M] is preferably 80 / 20, more preferably 75 / 25, and even more preferably 70 / 30.
[0015] <Requirement (a-2)> The ethylene copolymer (A) has a content of structural units derived from the non-conjugated polyene [N] of 0.1 to 6.0 mol % relative to 100 mol % of the total of the structural units derived from the [L], the structural units derived from the [M] and the structural units derived from the [N]. The ethylene copolymer (A) having this content in the above range has sufficient crosslinkability and flexibility. The lower limit of the content of the structural unit derived from [N] is preferably 0.5 mol %. The upper limit of the content of the structural unit derived from [N] is preferably 4.0 mol %, more preferably 3.5 mol %, and even more preferably 3.0 mol %. When the content of the structural unit derived from the non-conjugated polyene [N] is within the above range, an ethylene copolymer (A) having sufficient crosslinkability and flexibility can be obtained.
[0016] <Requirement (a-3)> The Mooney viscosity ML(1+4)125°C is in the range of 5-100, preferably 10-95, and particularly preferably 10-60. When the Mooney viscosity is within the above range, the ethylene-based copolymer (A) has good processability and flowability, and exhibits good post-treatment quality (ribbon handling properties) and excellent physical properties.
[0017] <Requirement (a-4)> The B value is 1.20 or more, preferably 1.20 to 1.80, and particularly preferably in the range of 1.22 to 1.40. An ethylene copolymer having a B value of less than 1.20 has a large compression set at low temperatures, and there is a risk that an ethylene copolymer having an excellent balance between rubber elasticity at low temperatures and tensile strength at room temperature cannot be obtained.
[0018] <Production method of ethylene-α-olefin-non-conjugated polyene copolymer (A)> The ethylene-α-olefin-non-conjugated polyene copolymer (A) according to the present invention can be obtained by various known production methods, for example, a conventionally known production method using a metallocene catalyst. As the metallocene catalyst and the production method using the catalyst, for example, the examples described in WO 2015 / 122415, particularly paragraphs
[0249] to
[0320] of the publication, can be adopted.
[0019] <Modified ethylene-α-olefin copolymer (B)> The ethylene-based copolymer composition of the present invention and the modified ethylene-α-olefin copolymer (B) (hereinafter sometimes abbreviated as "modified copolymer (B)"), which is the component (B) contained in the ethylene-based copolymer composition forming the layer [I] of the laminate of the present invention, are characterized by satisfying the following requirements (b-1) to (b-3):
[0020] <Requirement (b-1)> The content of structural units derived from ethylene (sometimes abbreviated as "ethylene content") is 15 to 85 mol % (wherein the total of the content of structural units derived from ethylene and the content of structural units derived from an α-olefin is 100 mol %). The ethylene content is 15 to 85 mol%, preferably 20 to 80 mol%, more preferably 30 to 70 mol%, and further preferably 40 to 60 mol%. If the ethylene content is too high or too low, the crystallinity becomes high, which may deteriorate the handleability when kneaded with the ethylene copolymer (A) or deteriorate the low-temperature flexibility of the obtained ethylene copolymer composition.
[0021] The ethylene content of the modified ethylene-α-olefin copolymer (B) is: 13 The measurement can be performed by C-NMR, and peaks can be identified and quantified, for example, according to the method described below and the method described in "Polymer Analysis Handbook" (published by Asakura Publishing, pp. 163-170).
[0022] The α-olefin constituting the modified ethylene-α-olefin copolymer (B) according to the present invention may be an α-olefin other than ethylene having 3 or more carbon atoms, and typical examples thereof include α-olefins having 3 to 20 carbon atoms such as propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-nonadecene, and 1-eicosene. These α-olefins may be used alone or in combination of two or more. The ethylene and α-olefins may include biomass-derived ethylene and α-olefins.
[0023] Among these α-olefins, α-olefins having 3 to 10 carbon atoms are preferred, propylene and 1-butene are more preferred, and propylene is even more preferred, from the viewpoints that crystallinity can be effectively reduced, a liquid copolymer can be obtained, and a composition and a molded article exhibiting the desired effects can be easily obtained.
[0024] The polymerization can also be carried out by allowing at least one other monomer selected from a polar group-containing monomer, a vinyl aromatic compound, and a cyclic olefin to coexist in the reaction system. The other monomer can be used in an amount of, for example, 20 parts by mass or less, preferably 10 parts by mass or less, based on 100 parts by mass in total of ethylene and an α-olefin having 3 to 20 carbon atoms.
[0025] Examples of polar group-containing monomers include α,β-unsaturated carboxylic acids such as acrylic acid, methacrylic acid, fumaric acid, and maleic anhydride, and metal salts thereof such as sodium salts, α,β-unsaturated carboxylic acid esters such as methyl acrylate, ethyl acrylate, n-propyl acrylate, methyl methacrylate, and ethyl methacrylate, vinyl esters such as vinyl acetate and vinyl propionate, and unsaturated glycidyls such as glycidyl acrylate and glycidyl methacrylate.
[0026] Examples of vinyl aromatic compounds include styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, o,p-dimethylstyrene, methoxystyrene, vinylbenzoic acid, methyl vinylbenzoate, vinylbenzyl acetate, hydroxystyrene, p-chlorostyrene, divinylbenzene, α-methylstyrene, and allylbenzene.
[0027] Examples of the cyclic olefin include cyclic olefins having 3 to 30 carbon atoms, preferably 3 to 20 carbon atoms, such as cyclopentene, cycloheptene, norbornene, 5-methyl-2-norbornene, 5-ethylidene-2-norbornene, 5-vinyl-2-norbornene, and tetracyclododecene.
[0028] <Requirement (b-2)> The weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) is in the range of 1,000 to 100,000. The Mw of the modified ethylene / α-olefin copolymer (B) according to the present invention is from 1,000 to 100,000, preferably from 1,500 to 90,000, and more preferably from 2,000 to 80,000.
[0029] When the weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) is within the above range, a good balance between processability when kneaded with the ethylene-based copolymer (A) and filler dispersibility in the resulting ethylene-based copolymer composition is obtained.
[0030] <Requirement (b-3)> The modified copolymer has a substituent derived from a compound having a carbon-carbon unsaturated bond, and the content of the moiety derived from the compound having a carbon-carbon unsaturated bond in the modified copolymer is in the range of 1 to 70 mass %. The modified ethylene-α-olefin copolymer (B) according to the present invention is a modified copolymer having a substituent derived from a compound having a carbon-carbon unsaturated bond. The graft position of the substituent is not particularly limited.
[0031] Examples of compounds having a carbon-carbon unsaturated bond include compounds having an aromatic ring, such as styrene and allylbenzene; compounds having an acid or acid-derived group, such as acid, acid anhydride, ester, amide and imide; compounds having an oxygen-containing group, such as alcohol, epoxy and ether; compounds having a nitrogen-containing group, such as amine, nitrile and isocyanate; compounds having a sulfur-containing group, such as sulfide, sulfoxide, sulfone and sulfonamide; and compounds having a silicon-containing group, such as vinyltrimethoxysilane.
[0032] Among these compounds having a carbon-carbon unsaturated bond, compounds having an aromatic ring, compounds having an acid or an acid derivative, and compounds having an oxygen-containing group are preferred, compounds having an aromatic ring, compounds having an acid or an acid derivative, and compounds having an alcoholic hydroxy group are more preferred, and compounds having an aromatic ring, unsaturated carboxylic acid, or unsaturated carboxylic acid derivative are even more preferred.
[0033] Examples of compounds having a carbon-carbon unsaturated bond and an aromatic ring include vinyl aromatic compounds in which a vinyl group is directly bonded to an aromatic ring, such as styrene, vinylnaphthalene, and vinylpyridine; compounds in which a vinyl group is not directly bonded to an aromatic ring, such as allylbenzene and allyl benzoate; and compounds having an ethynyl group, such as phenylacetylene. From the viewpoints of availability and reactivity in the graft reaction, vinyl aromatic compounds are preferred.
[0034] Examples of vinyl aromatic compounds include styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, o,p-dimethylstyrene, methoxystyrene, vinylbenzoic acid, methyl vinylbenzoate, vinylbenzyl acetate, hydroxystyrene, p-chlorostyrene, divinylbenzene, α-methylstyrene, vinylnaphthalene, vinylbiphenyl, vinylanthracene, vinyltriphenylene, vinylthiophene, and vinylpyridine. Among them, styrene is preferred from the viewpoint of availability and compatibility. These vinyl aromatic compounds may be used alone or in combination of two or more. The grafting position of the vinyl aromatic compound is not particularly limited.
[0035] When a vinyl aromatic compound is used as the compound having a carbon-carbon unsaturated bond, the content of the portion derived from the vinyl aromatic compound in the modified copolymer (B) is 1 to 70 mass%, preferably 2 to 60 mass%, more preferably 3 to 45 mass%. When the content of the portion derived from the vinyl aromatic compound is within the above range, the compatibility with the rubber (A), particularly the copolymer of the vinyl aromatic compound and the conjugated diene compound, is good, and a copolymer composition having a good balance of processability and filler dispersibility can be obtained.
[0036] The modified copolymer (B) according to the present invention is a modified copolymer (B) obtained by modifying, preferably graft-modifying, the unmodified ethylene-α-olefin copolymer (B') satisfying the above-mentioned requirement (b-1) with the above-mentioned compound having a carbon-carbon unsaturated bond.
[0037] <Trans polyoctenylene (C)> The trans-polyoctenylene (C), which is one of the components that may be contained in the ethylene-based copolymer composition of the present invention and the ethylene-based copolymer composition that forms the layer [I] of the laminate of the present invention, is a polymer of octenylene having a trans structure, and is mainly a metathesis polymer of cyclooctene having a trans double bond. The ethylene copolymer composition of the present invention contains the trans-polyoctenylene (C), and thus the compatibility with fibrous materials is improved, thereby improving the tackiness and the adhesiveness to fibrous materials. The trans-polyoctenylene (C) according to the present invention is manufactured and sold by Evonik Industries under the trade name VESTENAMER.
[0038] <Ethylene-based copolymer composition> The ethylene-based copolymer composition of the present invention and the ethylene-based copolymer composition forming the layer [I] of the laminate of the present invention are compositions containing an ethylene-based copolymer (A) and the above-mentioned modified copolymer (B), and preferably contain the above-mentioned modified copolymer (B) in an amount of 0.5 to 100 parts by mass, more preferably 1 to 70 parts by mass, and even more preferably 2 to 50 parts by mass per 100 parts by mass of the ethylene-based copolymer (A).
[0039] The ethylene-based copolymer composition of the present invention contains the ethylene-based copolymer (A) and the modified copolymer (B), and therefore has excellent adhesion to other materials, for example, layers containing fiber materials such as industrial belts, and molded articles and laminates obtained from the composition also have good mechanical properties.
[0040] The ethylene copolymer composition of the present invention may contain the trans polyoctenylene (C) in addition to the ethylene copolymer (A) and the modified copolymer (B). When the ethylene copolymer composition of the present invention contains the trans polyoctenylene (C), the amount thereof is in the range of 0.5 to 50 parts by mass, more preferably 10 to 30 parts by mass, and further preferably 2 to 10 parts by mass, per 100 parts by mass of the ethylene copolymer (A). The ethylene copolymer composition containing the trans-polyoctenylene (C) has good adhesion to other materials, for example, layers containing fibrous materials such as industrial belts, and a laminate obtained by crosslinking the composition has excellent adhesive strength with layers containing fibrous materials.
[0041] In addition to the ethylene copolymer (A), the modified copolymer (B), and the trans-polyoctenylene (C), the ethylene copolymer composition of the present invention may contain other components according to the desired purpose within the range that does not impair the effects of the present invention. The other components may contain at least one selected from, for example, a crosslinking agent, a crosslinking aid, a vulcanization accelerator, a vulcanization aid, a filler, a softener, an antiaging agent, a processing aid, an activator, a heat stabilizer, a weather stabilizer, an antistatic agent, a colorant, a lubricant, and a thickener. Each additive may be used alone or in combination of two or more.
[0042] <Crosslinking Agent, Crosslinking Coagent, Vulcanization Accelerator, and Vulcanization Coagent> Examples of the crosslinking agent include crosslinking agents generally used when crosslinking rubber, such as organic peroxides, phenolic resins, sulfur-based compounds, hydrosilicone-based compounds, amino resins, quinones or their derivatives, amine-based compounds, azo-based compounds, epoxy-based compounds, isocyanate-based compounds, etc. Among these, organic peroxides and sulfur-based compounds (hereinafter also referred to as "vulcanizing agents") are preferred.
[0043] Examples of organic peroxides include dicumyl peroxide (DCP), di-tert-butyl peroxide, 2,5-di-(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexyne-3, 1,3-bis(tert-butylperoxyisopropyl)benzene, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, n-butyl-4,4-bis(tert-butylperoxy)valerate, benzoyl peroxide, p-chlorobenzoyl peroxide, 2,4-dichlorobenzoyl peroxide, tert-butyl peroxybenzoate, ert-butylperoxyisopropyl carbonate, diacetyl peroxide, lauroyl peroxide, and tert-butylcumyl peroxide.
[0044] When an organic peroxide is used as a crosslinking agent, the amount of the organic peroxide in the copolymer composition is generally 0.1 to 20 parts by mass, preferably 0.2 to 15 parts by mass, and more preferably 0.5 to 10 parts by mass, based on 100 parts by mass of the ethylene copolymer (A). When the amount of the organic peroxide is within the above range, the ethylene copolymer composition exhibits excellent crosslinking properties without blooming on the surface of the obtained molded article, which is preferable.
[0045] When an organic peroxide is used as a crosslinking agent, it is preferable to use a crosslinking assistant in combination. Examples of the crosslinking assistant include sulfur; quinone dioxime crosslinking assistant such as p-quinone dioxime; acrylic crosslinking assistant such as ethylene glycol dimethacrylate and trimethylolpropane trimethacrylate; allyl crosslinking assistant such as diallyl phthalate and triallyl isocyanurate; maleimide crosslinking assistant; divinylbenzene; and metal oxides such as zinc oxide (e.g., ZnO#1 / zinc oxide type 2 (JIS standard (K-1410)), manufactured by Hakusui Tech Co., Ltd.), magnesium oxide, and activated zinc oxide (e.g., zinc oxide such as "META-Z102" (trade name; manufactured by Inoue Seki Kogyo Co., Ltd.)).
[0046] When a crosslinking aid is used, the amount of the crosslinking aid in the ethylene copolymer composition is usually 0.5 to 10 mol, preferably 0.5 to 7 mol, more preferably 1 to 6 mol, per mol of the organic peroxide.
[0047] Examples of sulfur-based compounds (vulcanizing agents) include sulfur, sulfur chloride, sulfur dichloride, morpholine disulfide, alkylphenol disulfide, tetramethylthiuram disulfide, and selenium dithiocarbamate.
[0048] When a sulfur-based compound is used as a crosslinking agent, the blending amount in the copolymer composition is usually 0.1 to 10 parts by mass, preferably 0.2 to 7.0 parts by mass, and more preferably 0.3 to 5.0 parts by mass, based on 100 parts by mass of the ethylene-based copolymer (A). When the blending amount of the sulfur-based compound is within the above range, there is no bloom on the surface of the obtained molded article, and the ethylene-based copolymer composition shows excellent crosslinking properties.
[0049] When a sulfur-based compound is used as the crosslinking agent, it is preferable to use a vulcanization accelerator in combination. Examples of the vulcanization accelerator include N-cyclohexyl-2-benzothiazole sulfenamide, N-oxydiethylene-2-benzothiazole sulfenamide, N,N'-diisopropyl-2-benzothiazole sulfenamide, 2-mercaptobenzothiazole (e.g., Suncerer M (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)), 2-(4-morpholinodithio)benzothiazole (e.g., Noccelaer MDB-P (trade name; manufactured by Ouchi Shinko Chemical Industry Co., Ltd.)), 2-(2,4-dinitrophenyl)mercaptobenzothiazole, 2-(2,6-dinitrophenyl)mercaptobenzothiazole, Thiazole-based vulcanization accelerators such as ethyl-4-morpholinothio)benzothiazole and dibenzothiazyl disulfide (for example, Sancerer DM (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)); guanidine-based vulcanization accelerators such as diphenyl guanidine, triphenyl guanidine, and diorthotolyl guanidine; aldehyde amine-based vulcanization accelerators such as acetaldehyde-aniline condensation product and butyraldehyde-aniline condensation product; imidazoline-based vulcanization accelerators such as 2-mercaptoimidazoline; tetramethylthiuram monosulfide (for example, Sancerer DM (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)); thiuram-based vulcanization accelerators such as tetramethylthiuram disulfide (e.g., Sancerer TS (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)), tetramethylthiuram disulfide (e.g., Sancerer TT (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)), tetraethylthiuram disulfide (e.g., Sancerer TET (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)), tetrabutylthiuram disulfide (e.g., Sancerer TBT (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)), and dipentamethylenethiuram tetrasulfide (e.g., Sancerer TRA (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)); zinc dimethyldithiocarbamate, diethyldithio Examples of such vulcanization accelerators include dithioacid salt vulcanization accelerators such as zinc carbamate, zinc dibutyldithiocarbamate (e.g., Sancerar PZ, Sancerar BZ, and Sancerar EZ (trade names; manufactured by Sanshin Chemical Industry Co., Ltd.)) and tellurium diethyldithiocarbamate; thiourea vulcanization accelerators such as ethylenethiourea (e.g., Sancerar BUR (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.), Sancerar 22-C (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)), N,N'-diethylthiourea, and N,N'-dibutylthiourea; and xanthate vulcanization accelerators such as zinc dibutylxatogenate.
[0050] When a vulcanization accelerator is used, the blending amount of the vulcanization accelerator in the copolymer composition is generally 0.1 to 20 parts by mass, preferably 0.2 to 15 parts by mass, and more preferably 0.5 to 10 parts by mass, based on 100 parts by mass of the ethylene copolymer (A). When the blending amount of the vulcanization accelerator is within the above range, the ethylene copolymer composition exhibits excellent crosslinking properties without blooming on the surface of the obtained molded article. When a sulfur-based compound is used as a crosslinking agent, a vulcanization assistant can be used in combination.
[0051] Examples of the vulcanization aid include zinc oxide (e.g., ZnO#1 and zinc oxide type 2, manufactured by Hakusui Tech Co., Ltd.), magnesium oxide, and activated zinc oxide (e.g., zinc oxide such as "META-Z102" (trade name, manufactured by Inoue Seki Kogyo Co., Ltd.)). When a vulcanization aid is used, the amount of the vulcanization aid blended in the ethylene-based copolymer composition is usually 1 to 20 parts by mass based on 100 parts by mass of the ethylene-based copolymer (A).
[0052] Filler The filler constituting the ethylene copolymer composition of the present invention is a known rubber reinforcing agent blended into a rubber composition, and is usually an inorganic substance called carbon black or an inorganic reinforcing agent.
[0053] Specific examples of the filler used in the present invention include Asahi #55G and Asahi #60UG (both manufactured by Asahi Carbon Co., Ltd.), Seast (V, SO, 116, 3, 6, 9, SP, TA, etc.) carbon black (manufactured by Tokai Carbon Co., Ltd.), these carbon blacks which have been surface-treated with a silane coupling agent or the like, as well as silica, activated calcium carbonate, finely divided talc, finely divided silicic acid, light calcium carbonate, heavy calcium carbonate, talc, clay, and the like.
[0054] These fillers may be used alone or in combination of two or more. As the filler in the present invention, preferably used are carbon black, silica, light calcium carbonate, heavy calcium carbonate, talc, clay, and the like.
[0055] When the copolymer composition of the present invention contains a filler, the filler may be blended in an amount of usually 50 to 300 parts by mass, preferably 80 to 250 parts by mass, per 100 parts by mass of the ethylene copolymer (A).
[0056] Since the ethylene copolymer composition of the present invention contains the above-mentioned modified copolymer (B), it does not require a softener, but the following softener may be used in combination. <Softener> Examples of softeners include petroleum-based softeners such as process oil, lubricating oil, paraffin oil, liquid paraffin, petroleum asphalt, and Vaseline; coal tar-based softeners such as coal tar; fatty oil-based softeners such as castor oil, linseed oil, rapeseed oil, soybean oil, and coconut oil; waxes such as beeswax and carnauba wax; naphthenic acid, pine oil, rosin or derivatives thereof; synthetic polymeric substances such as terpene resins, petroleum resins, and coumarone-indene resins; ester-based softeners such as dioctyl phthalate and dioctyl adipate; and others, such as microcrystalline wax, liquid polybutadiene, modified liquid polybutadiene, hydrocarbon-based synthetic lubricating oils, tall oil, and sub(factice). Of these, petroleum-based softeners are preferred, and process oil is particularly preferred.
[0057] When the ethylene copolymer composition contains a softener, the blending amount of the softener is generally 2 to 100 parts by mass, preferably 10 to 100 parts by mass, based on 100 parts by mass of the ethylene copolymer (A).
[0058] <Anti-aging agent (stabilizer)> By blending an antioxidant (stabilizer) with the ethylene copolymer composition of the present invention, the life of the seal packing formed therefrom can be extended. Examples of such antioxidants include conventionally known antioxidants, such as amine-based antioxidants, phenol-based antioxidants, and sulfur-based antioxidants.
[0059] Examples of the anti-aging agents include aromatic secondary amine-based anti-aging agents such as phenylbutylamine and N,N-di-2-naphthyl-p-phenylenediamine; phenol-based anti-aging agents such as dibutylhydroxytoluene and tetrakis[methylene(3,5-di-t-butyl-4-hydroxy)hydrocinnamate]methane; thioether-based anti-aging agents such as bis[2-methyl-4-(3-n-alkylthiopropionyloxy)-5-t-butylphenyl]sulfide; dithiocarbamate-based anti-aging agents such as nickel dibutyldithiocarbamate; and sulfur-based anti-aging agents such as 2-mercaptobenzoylimidazole, 2-mercaptobenzimidazole, zinc salt of 2-mercaptobenzimidazole, dilaurylthiodipropionate, and distearylthiodipropionate.
[0060] When the ethylene copolymer composition contains an antioxidant, the amount of the antioxidant is usually 0.3 to 10 parts by mass, preferably 0.5 to 7.0 parts by mass, based on 100 parts by mass of the ethylene copolymer (A). When the amount of the antioxidant is within the above range, there is no bloom on the surface of the obtained molded article, and further, the occurrence of vulcanization inhibition can be suppressed.
[0061] <Processing aids> As the processing aid, a wide variety of processing aids that are generally compounded with rubber can be used.Specific examples include ricinoleic acid, stearic acid, palmitic acid, lauric acid, barium stearate, zinc stearate, calcium stearate, zinc laurate, and esters.Of these, stearic acid is preferred.
[0062] When the copolymer composition contains a processing aid, it can be appropriately blended in an amount of usually 1 to 3 parts by mass per 100 parts by mass of the ethylene copolymer (A). When the blending amount of the processing aid is within the above range, it is preferable because the processability such as kneading processability, extrusion processability, and injection moldability is excellent. The processing aid may be used alone or in combination with two or more kinds.
[0063] <Activator> Examples of the activator include amines such as di-n-butylamine, dicyclohexylamine, and monoethanolamine; activators such as diethylene glycol, polyethylene glycol, lecithin, triaryl methylate, and zinc compounds of aliphatic or aromatic carboxylic acids; zinc peroxide preparations; octadecyltrimethylammonium bromide, synthetic hydrotalcite, and special quaternary ammonium compounds.
[0064] When the copolymer composition contains an activator, the amount of the activator is usually 0.2 to 10 parts by mass, preferably 0.3 to 5 parts by mass, based on 100 parts by mass of the ethylene copolymer (A).
[0065] <Laminate> The laminate of the present invention is a laminate in which a layer [I] made of the ethylene copolymer composition of the present invention is in contact with a layer [II] containing a fibrous material.
[0066] <<Layer [I] made of ethylene-based copolymer composition>> The layer [I] made of an ethylene-based copolymer composition constituting the laminate of the present invention is preferably a layer obtained by crosslinking the above-mentioned ethylene-based copolymer composition.
[0067] <Layer containing fibrous material [II]> The layer [II] containing a fiber material that constitutes the laminate of the present invention contains a fiber material in at least a part of the layer.
[0068] <Textile materials> Examples of fiber materials forming the layer [II] of the present invention include various known fiber materials, for example, natural fibers such as cotton and wood cellulose fibers; organic fiber materials such as fibers made of synthetic resins such as polyamide, polyester, polyvinyl alcohol, rayon, polyparaphenylene benzobisoxazole, polyethylene, polypropylene, polyarylate, polyimide, polyphenylene sulfide, polyether ether ketone, polylactic acid, polycaprolactone, polybutylene succinate, and fluorine-based polymers; and inorganic fiber materials such as glass fibers, PAN-based carbon fibers, pitch-based carbon fibers, alumina fibers, silicon carbide fibers, aluminum borate fibers, and potassium titanate whiskers.
[0069] These fiber materials may be long fibers (filaments) or short fibers (staples), and may be cord yarns, spun yarns, woven fabrics, knitted fabrics, canvas, nonwoven fabrics, and the like.
[0070] Examples of the polyamide include aliphatic polyamides such as nylon 6, nylon 6,6, and nylon 6,10; semi-aromatic polyamides such as polymetaxylylene adipamide (MXD6), polyhexamethylene terephthalamide (6T), and copolymer polyamides containing these units; and fully aromatic polyamides such as polybenzamide, poly-p-phenylene terephthalamide, and poly-m-phenylene isophthalamide.
[0071] Furthermore, these fiber materials may be surface-treated by a known method such as RFL treatment in order to improve adhesion between the fiber materials themselves or between the fiber materials and the layer [I] made of the ethylene-based copolymer composition.
[0072] <RFL Processing> RFL treatment is a process in which textile materials are treated with a treatment liquid (RFL liquid) containing resorcinol, formalin, and latex, and this RFL liquid is a mixture of the initial condensation product of resorcinol and formalin and rubber latex. Examples of rubber latex that can be used include styrene-butadiene-vinylpyridine terpolymer (VP), styrene-butadiene copolymer (SBR), chloroprene (CR), acrylonitrile-butadiene copolymer (NBR), hydrogenated NBR (H-NBR), chlorosulfonated ethylene (CSM), and natural rubber. These can be used alone or in a blend of two or more types.
[0073] <Method of manufacturing laminate> In order to manufacture the laminate of the present invention, various known methods for manufacturing laminates can be adopted. For example, a method of laminating a layer [I] made of an uncrosslinked ethylene-based copolymer composition previously manufactured (molded) by a known method with a layer [II] containing a fiber material, and then crosslinking the layer [I] made of the ethylene-based copolymer composition, a method of laminating a layer [I] made of a crosslinked ethylene-based copolymer composition with a layer [II] containing a fiber material, or a method of extrusion coating a layer [I] made of an ethylene-based copolymer composition on a layer [II] containing a fiber material, and then crosslinking the layer [I] made of the ethylene-based copolymer composition, The layer [I] made of the ethylene copolymer composition can be produced by various known methods.
[0074] The ethylene-based copolymer composition can be obtained by kneading the ethylene-based copolymer (A) and the modified copolymer (B), if necessary, the trans-polyoctenylene (C), and further additives such as a filler, an antioxidant, and a processing aid, using various known kneading and mixing devices, for example, a Banbury mixer, a kneader, an internal mixer (internal mixer) such as an Intermix, and a roll.
[0075] The uncrosslinked ethylene-based copolymer composition obtained by kneading may be molded into an intended shape by various molding methods such as an extrusion molding machine, a calendar roll, a press, an injection molding machine, or a transfer molding machine, and then crosslinked to form a layer [I] consisting of the ethylene-based copolymer composition, which may then be laminated (bonded) with a layer [II] containing a fiber material; alternatively, the uncrosslinked ethylene-based copolymer composition may be molded into an intended shape by the above-mentioned method, and then laminated (bonded) with a layer [II] containing a fiber material, thereby crosslinking the composition.
[0076] The layer [I] made of the ethylene copolymer composition may be crosslinked by heating using a crosslinking agent or by irradiating with light, gamma rays or electron beams.
[0077] In addition, when crosslinking, a mold may be used, or crosslinking may be performed without using a mold. When a mold is not used, the molding and crosslinking steps are usually performed continuously. As a heating method in the crosslinking tank, a heating tank using hot air, a glass bead fluidized bed, UHF (ultra-high frequency electromagnetic waves), steam, etc. may be used.
[0078] <<Applications of the laminate>> A laminate in which a layer [I] made of the ethylene-based copolymer composition of the present invention is in contact with a layer [II] containing a fiber material is suitably used for automobile hoses, water hoses, and gas hoses; industrial belts such as transmission belts and conveyor belts; and escalator handrails.
[0079] Examples of the automobile hose include brake hoses, radiator hoses, heater hoses, and air cleaner hoses. Examples of the transmission belt include a V-belt, a flat belt, a toothed belt, etc. Examples of the conveyor belt include a light conveyor belt, a cylindrical belt, a rough top belt, a flanged conveyor belt, a U-shaped guide conveyor belt, a V-guide conveyor belt, etc. EXAMPLES
[0080] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these. The ethylene / α-olefin / non-conjugated polyene copolymer (A) used in the examples of the present invention is shown below.
[0081] [Ethylene-α-olefin-non-conjugated polyene copolymer] According to the description of [Synthesis Example C1] of WO 2015 / 122415, an ethylene-1-butene-5-ethylidene-2-norbornene (ENB) copolymer having the following physical properties was obtained. Hereinafter, this is referred to as "ethylene copolymer (A-1)". The constitution and physical properties of the ethylene copolymer (A-1) are as follows: Structural units derived from ethylene: 67.7 mol% Structural units derived from 1-butene: 30.0 mol% Structural units derived from ENB: 2.3 mol% Mooney Viscosity ML(1+4)100℃:30 Mooney Viscosity ML(1+4)125℃:22 B value: 1.3
[0082] [Physical properties of ethylene copolymer (A-1)] <Molar amounts of structural units derived from ethylene, structural units derived from α-olefins, and structural units derived from non-conjugated polyenes> The molar amount is 1 The intensity was measured using a H-NMR spectrometer. Details of the measurement conditions are described in WO 2015 / 122415.
[0083] <Mooney Viscosity> The Mooney viscosity (ML(1+4) 100° C., 125° C.) was measured using a Mooney viscometer (Shimadzu Corporation, SMV202 type) in accordance with JIS K6300 (1994).
[0084] The measurement solvent was o-dichlorobenzene-d4 / benzene-d6 (4 / 1 [v / v]) at a measurement temperature of 120°C.13 A C-NMR spectrum (100 MHz, JEOL ECX400P) was measured, and calculation was performed based on the following formula (i). B value=([EX]+2[Y]) / [2×[E]×([X]+[Y])]···(i) [Here, [E], [X] and [Y] represent the mole fractions of structural units derived from ethylene [L], 1-butene [M] and ENB [C], respectively, and [EX] represents the ethylene [L]-1-butene [M] dyad sequence fraction.]
[0085] The ethylene-α-olefin-non-conjugated polyene copolymers used in the comparative examples of the present invention are shown below.
[0086] [Ethylene-α-olefin-non-conjugated polyene copolymer] The following ethylene-propylene-ENB copolymer (copolymer-2) was used as the ethylene-α-olefin-non-conjugated polyene copolymer. Product name: Mitsui EPT 4045M: Mooney viscosity ML (1+4) 100℃ = 45, ethylene content = 45 wt%, diene (ENB) content = 7.6 wt%.
[0087] [Modified ethylene-α-olefin copolymer (B)] As the modified ethylene-α-olefin copolymer (B), the styrene-modified ethylene-propylene copolymer (B-1) produced in the following Production Example 1 was used. The physical properties of the obtained styrene-modified ethylene-propylene copolymer (B-1) were measured by the following methods.
[0088] <Weight average molecular weight (Mw), Mw / Mn> The molecular weights (Mw) and Mw / Mn of the modified ethylene-α-olefin copolymer (B) and unmodified ethylene-α-olefin copolymer (B′) were determined by the following high-speed GPC measurement apparatus. High-speed GPC measurement device: Tosoh HLC8320GPC Mobile phase: THF (Wako Pure Chemical Industries, Ltd., stabilizer-free, liquid chromatography grade) Column: Two Tosoh TSKgel Super MultiporeHZ-M columns connected in series Sample concentration: 5mg / mL Mobile phase flow rate: 0.35mL / min Measurement temperature: 40℃ Standard sample for calibration curve: Tosoh PStQuick MP-M
[0089] <Ethylene content (mol%)> The ethylene content of the styrene-modified ethylene-propylene copolymer (B-1) and the unmodified ethylene-propylene copolymer (b) was measured using a JEOL ECP500 nuclear magnetic resonance spectrometer under the following conditions: solvent: ortho-dichlorobenzene / heavy benzene (80 / 20 vol%) mixed solvent; sample concentration: 55 mg / 0.6 mL; measurement temperature: 120°C; observation nucleus: 13C (125 MHz); sequence: single pulse proton decoupling; pulse width: 4.7 μ / s (45° pulse); repetition time: 5.5 s; accumulation count: 10,000 or more; and chemical shift reference value: 27.50 ppm.
[0090] The ethylene contents of the styrene-modified ethylene-propylene copolymer (B-1) and the unmodified ethylene-propylene copolymer (b) were determined from the 13C-NMR spectra measured as described above, based on the reports of GJ Ray (Macromolecules, 10, 773 (1977)), JC Sandall (Macromolecules, 15, 353 (1982)), K. Kimura (Polymer, 25, 4418 (1984)), and others in "Polymer Analysis Handbook" (published by Asakura Publishing, pp. 163-170).
[0091] [Production Example 1] In a 2-liter continuous polymerization reactor equipped with an agitator and thoroughly purifying the atmosphere with nitrogen, 1 liter of dehydrated and purified hexane was placed, and ethylaluminum sesquichloride (Al(C2H5) 1.5 ·Cl 1.5After continuously feeding a hexane solution of VO(OC2H5)Cl2 adjusted to 16 mmol / L as a catalyst at a rate of 500 mL / h, hexane was continuously fed at a rate of 500 mL / h. Meanwhile, the polymerization liquid was continuously withdrawn from the top of the reactor so that the polymerization liquid in the reactor was always 1 L.
[0092] Next, ethylene gas was supplied at a rate of 47 L / h, propylene gas at a rate of 47 L / h, and hydrogen gas at a rate of 20 L / h using a bubbling tube. The copolymerization reaction was carried out at 35°C by circulating a coolant through a jacket attached to the outside of the reactor. This resulted in a polymerization solution containing an ethylene-propylene copolymer. The obtained polymerization solution was washed three times with 500 mL of 0.2 mol / L hydrochloric acid per 1 L of the polymerization solution, then three times with 500 mL of distilled water per 1 L of the polymerization solution, dried over magnesium sulfate, and the solvent was distilled off under reduced pressure. The obtained viscous liquid was dried under reduced pressure at 130°C for 24 hours to obtain an ethylene-propylene copolymer (b). The ethylene content of this ethylene-propylene copolymer (b) was 54.9 mol%, Mw was 14,000, Mw / Mn was 2.0, and the 100°C kinetic viscosity was 2,100 mm 2 / s. Next, 327 g of unmodified copolymer (b) was placed in a 1 L glass autoclave, and the inside of the autoclave was replaced with nitrogen. Then, the temperature was raised to 160°C while stirring, and 87 g of styrene and 7.3 g of di-tert-butyl peroxide were fed over 8 hours, and the reaction was allowed to continue for 1 hour after the completion of the feeding. Next, the pressure was reduced for 1 hour while gradually passing nitrogen through the vacuum pump to remove impurities (unreacted styrene and decomposition products of di-tert-butyl peroxide). The above operations yielded a styrene-modified ethylene-propylene copolymer (B-1). The styrene content (modification amount) of this styrene-modified ethylene-propylene copolymer (B-1) was 21 mass%, Mw was 61,000, and Mw / Mn was 7.8.
[0093] [Trans-polyoctenylene (C)] As the trans-polyoctenylene (C), VESTENAMER 8012 (C-1), a trade name of Evonik Industries, was used.
[0094] <Physical Properties of Ethylene-Based Copolymer Composition (Non-Crosslinked Product)> <Mooney Viscosity> Mooney Viscosity ML(1+4)100℃ <Measurement of Adhesion> The adhesion between the layer [I] made of the uncrosslinked ethylene copolymer composition and the layer [II] containing a fiber material was measured by a probe tack test. The test was carried out using a Rhesca tacking tester (TAC-II). A stainless steel cylindrical probe with a diameter of 5 mm was brought into contact with the test specimen, and the adhesive strength (gf) generated when peeling was measured. The contact speed of the probe to the test specimen was 120 mm / min, the applied pressure was 50 gf, the applied pressure time was 20 seconds, the peel speed was 120 mm / min, and the temperature was 50°C.
[0095] <<Physical Properties of Crosslinked Ethylene-Based Copolymer Composition>> <Tear strength> In accordance with JIS K6252, a 2 mm thick sheet after crosslinking was used, and measurements were performed on uncut angle dumbbell test pieces at a measurement environment temperature of 23°C and a tensile speed of 500 mm / min.
[0096] <Durometer A hardness> According to JIS K 6253, the sheet hardness (type A durometer, HA) was measured using six 2 mm crosslinked sheets with smooth surfaces, stacking the flat parts to a thickness of approximately 12 mm. However, specimens with foreign matter, air bubbles, or scratches were not used. The dimensions of the measurement surface of the specimen were set so that measurements could be made with the tip of the indenter at a position 12 mm or more away from the end of the specimen.
[0097] <Tensile stress at break, tensile elongation at break> The tensile stress at break and the tensile elongation at break of the sheet were measured by the following method. The sheet was punched out to prepare No. 3 dumbbell test pieces as described in JIS K 6251 (1993). Using these test pieces, tensile tests were carried out according to the method specified in JIS K6251, section 3, at a measurement temperature of 25°C and a tensile speed of 500 mm / min, and the tensile stress at break (TB) and tensile elongation at break (EB) were measured.
[0098] Example 1 The ethylene copolymer (A-1) was masticated for 30 seconds, and 100 parts by weight of the masticated ethylene copolymer (A-1) was mixed with 5 parts by weight of zinc oxide (ZnO#1) as a crosslinking aid, 1 part by weight of stearic acid as a lubricant, 2 parts by weight of tetrakis[methylene(3,5-di-t-butyl-4-hydroxy)hydrocinnamate]methane (trade name Irganox 1010, manufactured by BASFF Japan Co., Ltd.) as an antiaging agent, 4 parts by weight of 2-mercaptobenzimidazole (trade name Sandant MB, manufactured by Sanshin Chemical Industry Co., Ltd.), 50 parts by weight of carbon black (manufactured by Asahi Carbon Co., Ltd., trade name Asahi#70), 10 parts by weight of the modified copolymer (B-1), and trans-polyoctenylene (C) (trade name: VESTENAMER, manufactured by Evonik Industries) (trade name: Evonik Industries). 5 parts by mass of 8012 were mixed for 2 minutes in a 1.7-liter Banbury mixer [manufactured by Kobe Steel, Ltd.]. After that, the ram was raised and cleaned, and the mixture was mixed for another minute and discharged at about 150°C to obtain a compound (mixture A). This mixing was performed at a filling rate of 70%.
[0099] Next, 177 parts by weight of this compound (kneaded dough A) was wound around a 6-inch roll (surface temperature of front roll 50°C, surface temperature of rear roll 50°C, rotation speed of front roll 16 rpm, rotation speed of rear roll 18 rpm), and 6.8 parts by weight of dicumyl peroxide (manufactured by NOF Corp., trade name Parkmil D40) was added as a crosslinking agent. The mixture was kneaded for 10 minutes, and then cut into a sheet to prepare an uncrosslinked sheet (kneaded dough B) with a thickness of 2 mm.
[0100] The adhesive strength (gf) of the resulting uncrosslinked sheet having a thickness of 2 mm was measured by the method described above. The results are shown in Table 1. Next, the obtained uncrosslinked sheet having a thickness of 2 mm was pressed at 170° C. for 15 minutes using a 100-ton press molding machine to produce a crosslinked sheet. The physical properties of the obtained crosslinked sheet were measured by the methods described above. The results are shown in Table 1.
[0101] Comparative Example 1 Instead of the copolymer (L-1) used in Example 1, the copolymer-2 was used, and the trans-polyoctenylene (C) and modified copolymer (B-1) were not used, and a softener (trade name: Diana Process Oil, manufactured by Idemitsu Kosan Co., Ltd.) was used to obtain an uncrosslinked copolymer composition by the method described in Example 1. Then, sulfur was added as a crosslinking agent, and tetramethylthiuram disulfide (trade name: Suncerer TT, manufactured by Sanshin Chemical Industry Co., Ltd.), dipentamethylenethiuram tetrasulfide (trade name: Suncerer TRA, manufactured by Sanshin Chemical Industry Co., Ltd.), zinc dibutyldithiocarbamate (trade name: Suncerer BZ, manufactured by Sanshin Chemical Industry Co., Ltd.) and ethylenethiourea (trade name: Suncerer 22-C, manufactured by Sanshin Chemical Industry Co., Ltd.) were added as vulcanization accelerators, and a crosslinked sheet was produced by the method described in Example 1, and the physical properties were evaluated. The results are shown in Table 1.
[0102] Comparative Example 2 Dicumyl peroxide was added to the A kneaded dough prepared in Comparative Example 1, and an uncrosslinked copolymer composition and a crosslinked copolymer composition were obtained by the method described in Example 1, and the physical properties were evaluated by the methods described above. The results are shown in Table 1.
[0103] Comparative Example 3 Instead of the modified copolymer (B-1) used in Example 1, a softener (product name: Diana Process Oil, manufactured by Idemitsu Kosan Co., Ltd.) was used, and an uncrosslinked copolymer composition and a crosslinked copolymer composition were obtained by the method described in Example 1, and the physical properties were evaluated by the method described above. The results are shown in Table 1. [Table 1]
Claims
1. An ethylene-based copolymer composition comprising the following components (A) and (B): (A): An ethylene-α-olefin-non-conjugated polyene copolymer containing ethylene [L], an α-olefin [M] having 4 to 20 carbon atoms, and a non-conjugated polyene [N], which satisfies the following requirements (a-1) to (a-4). <Requirement (a-1)> The molar ratio [[L] / [M]] of the structural unit derived from ethylene [L] to the structural unit derived from an α-olefin [M] having 4 to 20 carbon atoms is 40 / 60 to 90 / 10. <Requirement (a-2)>: The content of the structural unit derived from the non-conjugated polyene [N] is 0.1 to 6.0 mol % relative to 100 mol % of the total of the structural units [L], [M] and [N]. <Requirement (a-3)> The Mooney viscosity ML(1+4)125°C at 125°C is 5 to 100. <Requirement (a-4)>: The B value represented by the following formula (i) is 1.20 or more. B value = ([EX]+2[Y]) / [2×[E]×([X]+[Y])]...(i) [Here, [E], [X] and [Y] respectively represent the molar fractions of ethylene [L], α-olefin [M] having 4 to 20 carbon atoms, and non-conjugated polyene [N], and [EX] represents the dyad chain fraction of ethylene [L]-α-olefin [M] having 4 to 20 carbon atoms.] (B): A modified ethylene / α-olefin copolymer satisfying the following requirements (b-1) to (b-3). <Requirement (b-1)>: The content of structural units derived from ethylene is in the range of 15 to 85 mol % (wherein the total content of structural units derived from ethylene and the content of structural units derived from an α-olefin is 100 mol %). <Requirement (b-2)>: The weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) is in the range of 1,000 to 100,000. <Requirement (b-3)>: A modified ethylene / α-olefin copolymer having a substituent derived from a compound having a carbon-carbon unsaturated bond, wherein the content of the moiety derived from the compound having a carbon-carbon unsaturated bond in the modified ethylene / α-olefin copolymer is in the range of 1 to 70 mass %.
2. The ethylene-based copolymer composition according to claim 1, wherein the α-olefin [M] having 4 to 20 carbon atoms constituting the ethylene / α-olefin / non-conjugated polyene copolymer (A) is 1-butene.
3. The modified ethylene / α-olefin copolymer (B) satisfies the requirement (b-1) above, that the ethylene structural unit content is in the range of 40 to 60 mol %, and the requirement (b-2) above, that the weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) is in the range of 2,000 to 80,000; The ethylene-based copolymer composition according to claim 1, further comprising, in the requirement (b-3), the compound having a carbon-carbon unsaturated bond is one or more compounds selected from a vinyl aromatic compound, an unsaturated carboxylic acid, and an unsaturated carboxylic acid derivative, and the content of the site derived from the compound having a carbon-carbon unsaturated bond in the modified ethylene-α-olefin copolymer is in the range of 1 to 40 mass%.
4. The ethylene-based copolymer composition according to claim 3, characterized in that in the modified ethylene-α-olefin copolymer (B), in the requirement (b-3), the compound having a carbon-carbon unsaturated bond is a vinyl aromatic compound, and the content of the portion derived from the vinyl aromatic compound is in the range of 3 to 40 mass%.
5. 2. The ethylene-based copolymer composition according to claim 1, comprising 0.5 to 100 parts by mass of the modified ethylene / α-olefin copolymer (B) per 100 parts by mass of the ethylene / α-olefin / non-conjugated polyene copolymer (A).
6. The ethylene copolymer composition according to claim 1, comprising a trans-polyoctenylene (C).
7. The ethylene-based copolymer composition according to claim 6, which contains 0.5 to 50 parts by mass of trans-polyoctenylene (C) per 100 parts by mass of the ethylene / α-olefin / non-conjugated polyene copolymer (A).
8. A layer [I] comprising the ethylene copolymer composition according to any one of claims 1 to 7, and a fiber and a layer [II] containing a fiber material.
9. The laminate according to claim 8 , wherein the ethylene-based copolymer composition is crosslinked.
10. The laminate according to claim 8, wherein the textile material of the layer [II] is canvas.
11. An industrial belt comprising the laminate of claim 8.
Citation Information
Patent Citations
JP1967-023632B
Ethylene propylene rubber compound
JP2528033B2
Cited By
Crosslinked body
WO2026089013A1