Piezoelectric thin film and piezoelectric thin film element
A piezoelectric thin film with controlled surface roughness and tilted crystal grain orientations addresses the peeling issue in AlN-based films, enhancing adhesion and piezoelectric properties.
Patent Information
- Application Number
- JP2024033910
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-12-18
- Filing Date
- 2024-03-06
- Publication Date
- 2024-10-03
AI Technical Summary
The electrode layer in conventional piezoelectric thin films made of aluminum nitride (AlN) easily peels off from the surface, compromising the integrity and performance of the piezoelectric element.
A piezoelectric thin film with a specific crystal structure and surface roughness is developed, featuring a combination of first and second crystal grains with tilted (0001) planes and controlled developed area ratio, enhancing the adhesion of the electrode layers.
The solution effectively suppresses electrode peeling and improves piezoelectric properties by ensuring strong adhesion between the electrode layers and the thin film surface, maintaining the film's structural integrity and performance.
Smart Images

Figure 2024134527000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a piezoelectric thin film and a piezoelectric thin film element. [Background technology]
[0002] Aluminum nitride (AlN) is a piezoelectric material having a wurtzite structure. The piezoelectric strain constant d of AlN is smaller than that of conventional piezoelectric materials having a perovskite structure (e.g., lead zirconate titanate), but the piezoelectric output coefficient g of AlN is larger than that of conventional piezoelectric materials. Furthermore, AlN is a relatively inexpensive material. For these reasons, AlN has been attracting attention in recent years. For example, Patent Document 1 below discloses AlN in which part of Al is replaced with additive elements such as divalent elements and tetravalent elements in order to improve the piezoelectric properties. For example, Patent Document 2 below discloses AlN in which part of Al is replaced with Group 3 elements or Group 13 elements. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2013-219743 A [Patent Document 2] JP 2020-77788 A Summary of the Invention [Problem to be solved by the invention]
[0004] In general, a piezoelectric element (piezoelectric thin film element) using a thin film (piezoelectric thin film) having piezoelectricity has an electrode layer formed directly on the surface of the piezoelectric thin film. However, the electrode layer is easily peeled off from the surface of a conventional piezoelectric thin film made of AlN.
[0005] An object of one aspect of the present invention is to provide a piezoelectric thin film that suppresses peeling of an electrode layer from the surface of the piezoelectric thin film, and a piezoelectric thin film element including the piezoelectric thin film. [Means for solving the problem]
[0006] For example, one aspect of the present invention relates to a piezoelectric thin film according to any one of the following items [1] to [6], and a piezoelectric thin film element according to the following item [7].
[0007] [1] A piezoelectric thin film having a first main surface and a second main surface located on a back side of the first main surface, It comprises crystalline aluminum nitride having a wurtzite structure, The aluminum nitride contains a divalent element and a tetravalent element, or the aluminum nitride contains a trivalent element; The development area ratio of the second main surface is 0.001 or more and 0.100 or less. Piezoelectric thin film.
[0008] [2] A method for manufacturing a crystal grain having a crystal structure comprising: both the first grains and the second grains comprise aluminum nitride; the (0001) plane of the aluminum nitride in the first crystal grain is parallel to the first main surface; the (0001) plane of the aluminum nitride in the second crystal grains is inclined with respect to the (0001) plane of the aluminum nitride in the first crystal grains; A plurality of second crystal grains are exposed at the second main surface. [1] The piezoelectric thin film according to claim 1.
[0009] [3] A piezoelectric thin film having a first main surface and a second main surface located on a back side of the first main surface, A plurality of first crystal grains and a plurality of second crystal grains, both the first grains and the second grains comprise crystalline aluminum nitride having a wurtzite structure; the (0001) plane of the aluminum nitride in the first crystal grain is parallel to the first main surface; the (0001) plane of the aluminum nitride in the second crystal grains is inclined with respect to the (0001) plane of the aluminum nitride in the first crystal grains; a plurality of second crystal grains are exposed at the second main surface; The development area ratio of the second main surface is 0.001 or more and 0.100 or less. Piezoelectric thin film.
[0010] [4] The angle between the (0001) plane of the aluminum nitride in the first crystal grains and the (0001) plane of the aluminum nitride in the second crystal grains is 0.1° or more and 30° or less; The piezoelectric thin film according to [2] or [3].
[0011] [5] A secondary electron image of the second major surface is taken with a scanning electron microscope; The secondary electron image is parallel to the first principal surface; the ratio of the total area of the plurality of second crystal grains in the secondary electron image is 0.01% or more and 20% or less; The piezoelectric thin film according to any one of [2] to [4].
[0012] [6] A secondary electron image of the second major surface is taken with a scanning electron microscope; The secondary electron image is parallel to the first principal surface; The Heywood diameter of the secondary crystal grains measured in a secondary electron image is 5 nm or more and 2000 nm or less. The piezoelectric thin film according to any one of [2] to [5].
[0013] [7] A piezoelectric thin film according to any one of [1] to [6], A first electrode layer; A second electrode layer; and Including, the first major surface directly overlies the first electrode layer; a second electrode layer directly overlying the second major surface; Piezoelectric thin film element. Effect of the Invention
[0014] According to one aspect of the present invention, there is provided a piezoelectric thin film that suppresses peeling of an electrode layer from a surface of the piezoelectric thin film, and a piezoelectric thin film element including the piezoelectric thin film. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a schematic exploded perspective view of a piezoelectric thin film element according to one embodiment of the present invention. [Diagram 2] FIG. 2 shows a schematic cross section of the piezoelectric thin film element shown in FIG. 1, and the cross section shown in FIG. 2 is perpendicular to the first main surface of the piezoelectric thin film. [Diagram 3] FIG. 3 is a schematic diagram showing the orientation of the (0001) plane of aluminum nitride in the first crystal grain included in the cross section shown in FIG. 2, the orientation of the (0001) plane of aluminum nitride in the second crystal grain included in the cross section shown in FIG. 2, and the orientation of the first main surface of the piezoelectric thin film shown in FIG. 2. [Figure 4] FIG. 4 is a schematic diagram of an electron beam diffraction pattern including diffraction spots originating from lattice planes of aluminum nitride in a first crystal grain included in the cross section shown in FIG. 2 and diffraction spots originating from lattice planes of aluminum nitride in a second crystal grain included in the cross section shown in FIG. 2. [Diagram 5] FIG. 5 is a perspective view of a unit cell constituting the crystal structure (wurtzite structure) of aluminum nitride contained in a piezoelectric thin film according to one embodiment of the present invention. [Figure 6] (a) in Figure 6 is a perspective view of a unit cell showing the (0001) plane of aluminum nitride, (b) in Figure 6 is a perspective view of a unit cell showing the (0002) plane of aluminum nitride, and (c) in Figure 6 is a perspective view of a unit cell showing the (10-10) plane of aluminum nitride. [Figure 7] (a) in Figure 7 is a secondary electron image of a portion of the second principal surface of the piezoelectric thin film of Example 7, where the secondary electron image shown in (a) in Figure 7 is parallel to the first principal surface, and (b) in Figure 7 is a monochrome image obtained by image processing (binarization processing) of the secondary electron image shown in (a) in Figure 7. [Figure 8] FIG. 8 is an image of a cross section of the piezoelectric thin film of Example 7, where the cross section shown in FIG. 8 is perpendicular to the first major surface of the piezoelectric thin film. [Figure 9] (a) in Figure 9 is an electron beam diffraction pattern measured by irradiating an electron beam at measurement point 1 in the cross section shown in Figure 8, and (b) in Figure 9 is an electron beam diffraction pattern measured by irradiating an electron beam at measurement point 2 in the cross section shown in Figure 8. [Figure 10](a) in Figure 10 is an electron beam diffraction pattern measured by irradiating an electron beam at measurement point 3 in the cross section shown in Figure 8, and (b) in Figure 10 is an electron beam diffraction pattern measured by irradiating an electron beam at measurement point 4 in the cross section shown in Figure 8. [Figure 11] (a) in Figure 11 is an electron beam diffraction pattern measured by irradiating an electron beam at measurement point 5 in the cross section shown in Figure 8, and (b) in Figure 11 is an electron beam diffraction pattern measured by irradiating an electron beam at measurement point 6 in the cross section shown in Figure 8. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, preferred embodiments of the present invention will be described with reference to the drawings. In the drawings, equivalent components are given the same reference numerals. The present invention is not limited to the following embodiments. X, Y, and Z shown in Figs. 1 to 3 and 7 represent three coordinate axes that are perpendicular to each other. The directions of the X-axis, Y-axis, and Z-axis are common to Figs. 1 to 3 and 7.
[0017] As shown in FIG. 1, the piezoelectric thin film element 10 according to this embodiment includes a first electrode layer 1 (lower electrode layer), a piezoelectric thin film 3, and a second electrode layer 2 (upper electrode layer). The piezoelectric thin film 3 according to this embodiment includes crystalline aluminum nitride having a wurtzite structure. The piezoelectric thin film 3 has a first main surface s31 and a second main surface s32 located on the back side of the first main surface s31. The "main surface" is the surface with the largest area among multiple surfaces of a polyhedron (for example, the piezoelectric thin film 3 which is a thin rectangular parallelepiped). The first main surface s31 of the piezoelectric thin film 3 directly overlaps the surface s1 of the first electrode layer 1. The surface s2 of the second electrode layer 2 directly overlaps the second main surface s32 of the piezoelectric thin film 3. The thickness of the first electrode layer 1 (the width of the first electrode layer 1 in the Z-axis direction) may be approximately or completely uniform. The first main surface s31 of the piezoelectric thin film 3 is a flat plane. The surface s1 of the first electrode layer 1 is also a flat plane. 1 are parallel to the first principal surface s31 of the piezoelectric thin film 3 and the surface s1 of the first electrode layer 1. The Z axis shown in FIG. 1 is perpendicular to the first principal surface s31 of the piezoelectric thin film 3 and the surface s1 of the first electrode layer 1.
[0018] The developed interfacial area ratio Sdr of the second main surface s32 of the piezoelectric thin film 3 is 0.001 or more and 0.100 or less (0.1% or more and 10% or less). The developed interfacial area ratio may be rephrased as the developed surface area ratio. The developed area ratio Sdr is defined as follows.
[0019] The position of any point P included in any plane XY parallel to the first main surface s31 of the piezoelectric thin film 3 (i.e., the plane XY including the X-axis and the Y-axis) is expressed as (x, y, 0). x is the coordinate of the point P in the X-axis direction, and y is the coordinate of the point P in the Y-axis direction. 0 (zero) is the coordinate of the point P in the Z-axis direction. The position of any point Q included in the second main surface s32 of the piezoelectric thin film 3 is expressed as (x, y, z). (x, y) of the point Q coincides with (x, y) of the point P. The z of the point Q is the coordinate of the point Q in the Z-axis direction, and the absolute value of z corresponds to the distance between the points P and Q. Since the second main surface s32 of the piezoelectric thin film 3 is a surface extending along the plane XY in a three-dimensional coordinate system composed of the X-axis, the Y-axis, and the Z-axis, the z of the point Q is determined to a single value by specifying (x, y) of the point Q included in the second main surface s32. Therefore, the second principal surface s32 of the piezoelectric thin film 3 is expressed by a function z=f(x, y). A defined region (plane) in a plane XY parallel to the first principal surface s31 of the piezoelectric thin film 3 is expressed as A. An area B of the second principal surface s32 in the defined region A (integral region) is expressed by the following formula 1. The area B can be said to be an area of a portion of the second principal surface s32 that overlaps with the defined region A (integral region) in a direction (Z-axis direction) perpendicular to the first principal surface s31. A developed area ratio Sdr of the second principal surface s32 is defined by the following formula 2. The following formula 2 is simplified as the following formula 3. For convenience of notation, the area of the defined region A is also expressed as A in the following formulas 2 and 3. The developed area ratio Sdr of the second principal surface s32 of the piezoelectric thin film 3 may be measured by an atomic force microscope (AFM).
number
number
number
[0020] The developed area ratio Sdr is one of the indexes indicating the surface roughness of the second principal surface s32 of the piezoelectric thin film 3. The developed area ratio Sdr of 0.001 or more and 0.100 or less means that the area of the second principal surface s32 of the piezoelectric thin film 3 is larger than the area of a perfect plane. In other words, the developed area ratio Sdr of 0.001 or more and 0.100 or less means that the area (adhesion area) of the interface between the second principal surface s32 and the surface s2 of the second electrode layer 2 is larger than the area of the interface between a perfect plane and the surface s2 of the second electrode layer 2. By the developed area ratio Sdr being 0.001 or more and 0.100 or less, the adhesion of the second electrode layer 2 to the second principal surface s32 of the piezoelectric thin film 3 is improved, and peeling of the second electrode layer 2 from the second principal surface s32 of the piezoelectric thin film 3 is suppressed. When the developed area ratio Sdr is less than 0.001, the second electrode layer 2 is easily peeled off from the second principal surface s32 of the piezoelectric thin film 3. When the development area ratio Sdr is larger than 0.100, the second electrode layer 2 is easily peeled off from the second main surface s32 of the piezoelectric thin film 3, and the piezoelectric characteristics of the piezoelectric thin film 3 (for example, d 33 ) is prone to deterioration.
[0021] The developed area ratio Sdr of the second main surface s32 of the piezoelectric thin film 3 may be 0.002 or more and 0.055 or less (0.2% or more and 5.5% or less), or 0.004 or more and 0.043 or less (0.4% or more and 4.3% or less), because peeling of the second electrode layer 2 from the second main surface s32 of the piezoelectric thin film 3 is easily suppressed and the piezoelectric characteristics of the piezoelectric thin film 3 are easily improved. For similar reasons, the developed area ratio Sdr of the second main surface s32 of the piezoelectric thin film 3 may be greater than 0.015 and less than 0.100 (greater than 1.5% and less than 10%), greater than 0.015 and less than 0.055 (greater than 1.5% and less than 5.5%), greater than 0.015 and less than 0.043 (greater than 1.5% and less than 4.3%), 0.020 or more and less than 0.100 (2.0% or more and less than 10%), 0.020 or more and less than 0.055 (2.0% or more and less than 5.5%), or 0.020 or more and less than 0.043 (2.0% or more and less than 4.3%).
[0022] The crystalline aluminum nitride contained in the piezoelectric thin film 3 has a hexagonal wurtzite structure. That is, as shown in Fig. 5, a unit cell uc of aluminum nitride (wurtzite structure) is a hexagonal prism. For example, when the unit cell uc is made of only Al and N, the unit cell uc may be a regular hexagonal prism. Aluminum nitride may contain a divalent element Ed and a tetravalent element Et. A part of Al in the unit cell uc of the wurtzite structure may be substituted with a divalent element Ed or a tetravalent element Et. The piezoelectric thin film 3 may be composed only of AlN containing a divalent element Ed and a tetravalent element Et. In other words, the piezoelectric thin film 3 may be composed only of Al, N, a divalent element Ed, and a tetravalent element Et. The aluminum nitride may contain the trivalent element Etr. A part of Al in the unit cell uc of the wurtzite structure may be substituted with the trivalent element Etr. The piezoelectric thin film 3 may be made of only AlN containing the trivalent element Etr. In other words, the piezoelectric thin film 3 may be made of only Al, N, and the trivalent element Etr. Aluminum nitride may contain all of the divalent element Ed, the trivalent element Etr, and the tetravalent element Et. The piezoelectric thin film 3 may be made of only AlN containing the divalent element Ed, the trivalent element Etr, and the tetravalent element Et. In other words, the piezoelectric thin film 3 may be made of only Al, N, the divalent element Ed, the trivalent element Etr, and the tetravalent element Et. The piezoelectric thin film 3 may be made of pure AlN. In other words, the piezoelectric thin film 3 may be made of only Al and N. As described later, the piezoelectric thin film 3 may further contain other elements in addition to Al, N, the divalent element Ed, the trivalent element Etr, and the tetravalent element Et.
[0023] The unit cell uc shown in each of (a) in FIG. 6, (b) in FIG. 6, and (c) in FIG. 6 is the same as the unit cell uc shown in FIG. 5. At each of the 12 vertices of the unit cell uc (hexagonal prism) shown in each of (a) in FIG. 6, (b) in FIG. 6, and (c) in FIG. 6, one element from among aluminum, a divalent element Ed, a trivalent element Etr, and a tetravalent element Et may be arranged. However, in order to show each fundamental vector and each lattice plane of the unit cell uc, Al, N, a divalent element Ed, a trivalent element Etr, and a tetravalent element Et are omitted in (a) in FIG. 6, (b) in FIG. 6, and (c) in FIG. 6. In the unit cell uc, a1, a2, a3, and c are fundamental vectors (crystal axes) constituting the unit cell uc. The orientation of a1 is [2-1-10]. The orientation of a2 is [-12-10]. The orientation of a3 is [-1-120]. The orientation of c is
[0001] . The lengths of a1, a2, and a3 may be approximately equal to each other. The lengths of a1, a2, and a3 may be completely equal to each other. All of a1, a2, and a3 may be approximately perpendicular to c. All of a1, a2, and a3 may be completely perpendicular to c. The angle between a1, a2, and a3 may be approximately 120°. The angle between a1, a2, and a3 may be completely 120°. (a) of FIG. 6 shows the (0001) plane of aluminum nitride. (b) of FIG. 6 shows the (0002) plane of aluminum nitride. (c) of FIG. 6 shows the (10-10) plane of aluminum nitride. The (0001) plane is approximately or completely parallel to the (0002) plane. The (10-10) plane is nearly or completely perpendicular to the (0002) plane.
[0024] For example, the crystal structure of aluminum nitride may be identified by X-ray diffraction and electron beam diffraction. For example, diffracted X-rays from a lattice plane (e.g., (0002) plane) that is approximately or completely parallel to the first main surface s31 of the piezoelectric thin film 3 among the multiple lattice planes of aluminum nitride may be detected by out-of-plane diffraction method at the second main surface s32 of the piezoelectric thin film 3. For example, diffracted X-rays from a lattice plane (e.g., (10-10) plane) that is approximately or completely perpendicular to the first main surface s31 of the piezoelectric thin film 3 among the multiple lattice planes of aluminum nitride may be detected by in-plane diffraction method at the second main surface s32 of the piezoelectric thin film 3.
[0025] FIG. 2 shows a schematic cross section of the piezoelectric thin film element 10 shown in FIG. 1. The cross section shown in FIG. 2 is perpendicular to the first main surface s31 of the piezoelectric thin film 3. As shown in FIG. 2, the piezoelectric thin film 3 may include a plurality of first crystal grains c1 and a plurality of second crystal grains c2. The piezoelectric thin film 3 may be composed of only a plurality of first crystal grains c1 and a plurality of second crystal grains c2. Both the first crystal grains c1 and the second crystal grains c2 include crystalline aluminum nitride having a wurtzite structure. Each of the plurality of first crystal grains c1 may be a columnar crystal. Each of the plurality of second crystal grains c2 may also be a columnar crystal. Each of the plurality of first crystal grains c1 may be a single crystal or a polycrystal. Each of the plurality of second crystal grains c2 may also be a single crystal or a polycrystal. A plurality of first crystal grains c1 are exposed to the second main surface s32 of the piezoelectric thin film 3. Some of the first crystal grains c1 among all the first crystal grains c1 included in the piezoelectric thin film 3 may be exposed to the second main surface s32 of the piezoelectric thin film 3. All the first crystal grains c1 included in the piezoelectric thin film 3 may be exposed to the second main surface s32 of the piezoelectric thin film 3. Instead of the entirety of each first crystal grain c1, only an end of each first crystal grain c1 may be exposed to the second main surface s32 of the piezoelectric thin film 3. A plurality of second crystal grains c2 are exposed to the second main surface s32 of the piezoelectric thin film 3. A portion of the second crystal grains c2 among all the second crystal grains c2 included in the piezoelectric thin film 3 may be exposed to the second main surface s32 of the piezoelectric thin film 3. All the second crystal grains c2 included in the piezoelectric thin film 3 may be exposed to the second main surface s32 of the piezoelectric thin film 3. Instead of the entirety of each second crystal grain c2, an end portion of each second crystal grain c2 may be exposed to the second main surface s32 of the piezoelectric thin film 3.
[0026] FIG. 3 shows the orientation of the (0001) plane of aluminum nitride in the first crystal grains c1 included in the cross section shown in FIG. 2, the orientation of the (0001) plane of aluminum nitride in the second crystal grains c2 included in the cross section shown in FIG. 2, and the orientation of the first main surface s31 of the piezoelectric thin film 3 shown in FIG. 2. The first reference plane c1(0001) shown in FIG. 3 is a plane including the (0001) plane of aluminum nitride in the first crystal grains c1. The second reference plane c2(0001) shown in FIG. 3 is a plane including the (0001) plane of aluminum nitride in the second crystal grains c2. In the cross section shown in FIG. 3, the first reference plane c1(0001), the second reference plane c2(0001), and the first main surface s31 of the piezoelectric thin film 3 are all represented by straight lines. 3, the (0001) plane of aluminum nitride in each of the first crystal grains c1 (i.e., the first reference plane c1(0001)) is approximately or completely parallel to the first main surface s31 of the piezoelectric thin film 3. In other words, the (0001) plane of aluminum nitride in each of the first crystal grains c1 is approximately or completely parallel to the surface s1 of the first electrode layer 1. The above-mentioned defined region A (integral region) may be a plane parallel to the (0001) plane of each of the first crystal grains c1. On the other hand, the (0001) plane of aluminum nitride in each of the second crystal grains c2 (i.e., the second reference plane c2(0001)) is inclined with respect to the (0001) plane of aluminum nitride in each of the first crystal grains c1 (i.e., the first reference plane c1(0001)). In other words, the (0001) plane of aluminum nitride in each of the second crystal grains c2 is inclined with respect to the first main surface s31 of the piezoelectric thin film 3 and the surface s1 of the first electrode layer 1.
[0027] Since the (0001) plane of aluminum nitride in each first crystal grain c1 is substantially or completely parallel to the first main surface s31 (flat plane) of the piezoelectric thin film 3, only at least one lattice plane of the (0001) plane and the (0002) plane of aluminum nitride in each first crystal grain c1 is likely to be exposed on the back surface (second main surface s32) of the first main surface s31. Therefore, a portion of the second main surface s32 of the piezoelectric thin film 3 where only one or more first crystal grains c1 are exposed is substantially or completely parallel to the first main surface s31 of the piezoelectric thin film 3. In other words, a portion of the second main surface s32 of the piezoelectric thin film 3 consisting of only one or more first crystal grains c1 is unlikely to include surface defects such as kinks and steps and is likely to be flat. On the other hand, the (0001) plane of aluminum nitride in each second crystal grain c2 is inclined with respect to the (0001) plane of aluminum nitride in the first crystal grain c1. Therefore, not only the (0001) plane and the (0002) plane of aluminum nitride in each second crystal grain c2, but also other lattice planes (e.g., (10-10) plane) in each second crystal grain c2 are likely to be exposed to the second main surface s32. Therefore, the portion of the second main surface s32 of the piezoelectric thin film 3 where one or more second crystal grains c2 are exposed is likely to include surface defects such as kinks and steps. In other words, the portion of the second main surface s32 of the piezoelectric thin film 3 where one or more second crystal grains c2 are exposed is likely to be an inclined convex portion, and the portion of the second main surface s32 of the piezoelectric thin film 3 where one or more first crystal grains c1 are exposed is likely to be a flat surface or a concave portion. For the above reasons, since the piezoelectric thin film 3 includes a plurality of second crystal grains c2 in addition to a plurality of first crystal grains c1, a plurality of convex portions and concave portions are easily formed on the second main surface s32 of the piezoelectric thin film 3. As a result, the second main surface s32 is easily roughened, and the developed area ratio Sdr of the second main surface s32 is easily set to a value of 0.001 to 0.100. The convex portions and concave portions formed on the second main surface s32 of the piezoelectric thin film 3 and the surface s2 of the second electrode layer 2 are engaged with each other, so that the adhesion of the second electrode layer 2 to the second main surface s32 of the piezoelectric thin film 3 is easily improved. In other words, the anchor effect due to the convex portions and concave portions formed on the second main surface s32 of the piezoelectric thin film 3 easily suppresses peeling of the second electrode layer 2 from the second main surface s32 of the piezoelectric thin film 3.
[0028] Aluminum nitride is polarized in a crystal orientation perpendicular to the (0001) plane (i.e.,
[0001] ). Therefore, the (0001) plane of aluminum nitride in the multiple first crystal grains c1 is oriented approximately or completely parallel to the first main surface s31 (surface s1 of the first electrode layer 1) of the piezoelectric thin film 3, which tends to improve the piezoelectric characteristics of the piezoelectric thin film 3. Furthermore, in the process of forming the piezoelectric thin film 3, the second crystal grains c2 inclined relative to the first crystal grains c1 grow, so that a stress that stretches the first crystal grains c1 in the c-axis direction tends to act from the second crystal grains c2 to the growing first crystal grains c1. As a result, the crystallinity of the first crystal grains c1 is improved, the orientation of the (0001) plane of aluminum nitride in the first crystal grains c1 is improved, and the piezoelectric characteristics of the piezoelectric thin film 3 tend to be improved.
[0029] Diffracted X-rays originating from the (0002) plane of aluminum nitride in the first crystal grains c1 are detected by out-of-plane diffraction at the second main surface s32 of the piezoelectric thin film 3. The (0001) plane is substantially or completely parallel to the (0002) plane. Therefore, by detecting diffracted X-rays originating from the (0002) plane of aluminum nitride in the first crystal grains c1 by out-of-plane diffraction, it can be confirmed that the (0001) plane of aluminum nitride in the first crystal grains c1 is substantially or completely parallel to the first main surface s31 of the piezoelectric thin film 3. Diffracted X-rays originating from the (10-10) plane of aluminum nitride in the first crystal grains c1 are detected by in-plane diffraction at the second main surface s32 of the piezoelectric thin film 3. As described later, the inclination of the (0001) plane of aluminum nitride in the second crystal grains c2 can be confirmed by electron beam diffraction.
[0030] As shown in FIG. 3, the angle θ between the first reference plane c1 (0001) and the second reference plane c2 (0001) can be expressed as the angle θ between the (0001) plane of aluminum nitride in the first crystal grains c1 and the (0001) plane of aluminum nitride in the second crystal grains c2. For example, the angle θ between the (0001) plane of aluminum nitride in the first crystal grains c1 and the (0001) plane of aluminum nitride in the second crystal grains may be 0.1° or more and 30° or less. With an increase in the angle θ, multiple convex portions and concave portions are likely to be formed on the second main surface s32 of the piezoelectric thin film 3. In other words, with an increase in the angle θ, the development area ratio Sdr is likely to increase. When the angle θ is 0.1° or more and 30° or less, peeling of the second electrode layer 2 from the second main surface s32 of the piezoelectric thin film 3 is likely to be suppressed, and the piezoelectric characteristics of the piezoelectric thin film 3 are likely to be improved. For the same reason, the angle θ may be 0.4° or more and 17° or less.
[0031] The electron beam diffraction pattern dp shown in FIG. 4 is measured by irradiating an electron beam onto any one of the second crystal grains c2 exposed on the cross section of the piezoelectric thin film 3 (a cross section perpendicular to the first main surface s31 of the piezoelectric thin film 3). The central spot d(0000) in the electron beam diffraction pattern dp is a spot of the electron beam that is not diffracted by the piezoelectric thin film 3. The diffraction spot d1(0002) in the electron beam diffraction pattern dp is a spot of the electron beam diffracted by the (0002) plane of the aluminum nitride in the first crystal grain c1. The diffraction spot d1(000-2) in the electron beam diffraction pattern dp is a spot of the electron beam diffracted by the (000-2) plane of the aluminum nitride in the first crystal grain c1. The diffraction spot d2(0002) in the electron beam diffraction pattern dp is a spot of the electron beam diffracted by the (0002) plane of the aluminum nitride in the second crystal grain c2. The diffraction spot d2(000-2) in the electron beam diffraction pattern dp is a spot of the electron beam diffracted by the (000-2) plane of the aluminum nitride in the second crystal grain c2. For convenience of explanation, the spots of the electron beam diffracted by lattice planes other than the (0002) plane and the (000-2) plane are omitted in FIG. The ratio of the total volume of the second crystal grains c2 in the piezoelectric thin film 3 is smaller than the ratio of the total volume of the first crystal grains c1 in the piezoelectric thin film 3. For example, the ratio of the total volume of the second crystal grains c2 in the piezoelectric thin film 3 may be 0.005 volume % or more and 25.0 volume % or less, and the ratio of the total volume of the first crystal grains c1 in the piezoelectric thin film 3 may be 75.0 volume % or more and 99.995 volume % or less. Due to the magnitude relationship of the above volume ratios, the electron beam diffraction pattern dp measured by irradiating an electron beam on one second crystal grain c2 includes not only diffraction spots originating from the second crystal grains c2 but also diffraction spots originating from the first crystal grains c1 present in the vicinity of the second crystal grains c2. Furthermore, due to the magnitude relationship of the above volume ratios, the intensity (brightness) of each diffraction spot originating from the second crystal grains c2 is lower than the intensity of each diffraction spot originating from the first crystal grains c1, and the diameter of each diffraction spot originating from the second crystal grains c2 is smaller than the diameter of each diffraction spot originating from the first crystal grains c1. On the other hand, when an electron beam diffraction pattern is measured by irradiating an electron beam on any one of the first crystal grains c1 exposed on the cross section of the piezoelectric thin film 3 (a cross section perpendicular to the first main surface s31 of the piezoelectric thin film 3), the electron beam diffraction pattern is likely to include only the diffraction spots originating from the first crystal grain c1 and is unlikely to include the diffraction spots originating from the second crystal grains c2. Therefore, by comparing the electron beam diffraction pattern measured by irradiating the electron beam on the first crystal grain c1 with the electron beam diffraction pattern dp measured by irradiating the electron beam on the second crystal grain c2, the diffraction spots originating from the first crystal grain c1 and the diffraction spots originating from the second crystal grains c2 can be distinguished. The reference line L1 in the electron beam diffraction pattern dp is a straight line passing through the center of the central spot d(0000) and the center of the diffraction spot d1(0002) derived from the (0002) plane of the aluminum nitride in the first crystal grain c1. The reference line L2 in the electron beam diffraction pattern dp is a straight line passing through the center of the central spot d(0000) and the center of the diffraction spot d2(0002) derived from the (0002) plane of the aluminum nitride in the second crystal grain c2. Since the (0002) plane is parallel to the (0001) plane, the angle θ between the (0001) plane of the aluminum nitride in the first crystal grain c1 and the (0001) plane of the aluminum nitride in the second crystal grain c2 can be determined from the angle α between the reference line L1 and the reference line L2. In other words, the angle α between the reference line L1 and the reference line L2 is equal to the angle θ between the (0001) plane of the aluminum nitride in the first crystal grain c1 and the (0001) plane of the aluminum nitride in the second crystal grain.
[0032] 7(a) is a secondary electron image aa of a part of the second principal surface s32 of the piezoelectric thin film 3. The secondary electron image aa of the second principal surface s32 is captured by a scanning electron microscope (SEM). The secondary electron image aa of the second principal surface s32 is approximately or completely parallel to the first principal surface s31 of the piezoelectric thin film 3. In other words, the secondary electron image aa of the second principal surface s32 may be approximately or completely parallel to the (0001) plane of aluminum nitride in the multiple first crystal grains c1. As described above, when the second crystal grains c2 are exposed on the second main surface s32 of the piezoelectric thin film 3, the secondary electron image ia includes the first crystal grains c1 exposed on the second main surface s32 and the second crystal grains c2 exposed on the second main surface s32. As described above, the ends of the second crystal grains c2 exposed on the second main surface s32 are inclined on the second main surface s32, so the brightness of each second crystal grain c2 in the secondary electron image ia is different from the brightness of each first crystal grain c1 in the secondary electron image ia. That is, the first crystal grains c1 and the second crystal grains c2 in the secondary electron image ia are distinguished from each other by contrast (difference in brightness). The bright parts in the secondary electron image ia are the second crystal grains c2, and the dark parts in the secondary electron image ia are the first crystal grains c1. The secondary electron image ia shown in (a) of FIG. 7 shows that the second crystal grains c2 (multiple convex parts) are distributed in a plane consisting of the first crystal grains c1. The monochrome image ib shown in Fig. 7(b) is a secondary electron image ia binarized based on the difference in brightness between the first crystal grains c1 and the second crystal grains c2 in the secondary electron image ia. By using the monochrome image ib, the outline, size, and area of each of the multiple second crystal grains c2 exposed on the second main surface s32 can be measured more accurately.
[0033] The ratio (area fraction RA) of the total area of the plurality of second crystal grains c2 in the secondary electron image ia (monochrome image ib) may be 0.01% or more and 20% or less. The total area of all the second crystal grains c2 exposed in the secondary electron image ia is A TOTAL The area of the entire secondary electron image ia may be expressed as Ai, and the area fraction RA may be expressed as (A TOTAL / Ai) × 100. That is, A TOTAL / Ai may be 0.01% or more and 20% or less (0.0001 or more and 0.2 or less). Secondary electron images ia may be captured at 10 different parts included in the second main surface s32 of the piezoelectric thin film 3, and the average value of the ratio of the total area of the plurality of second crystal grains c2 in the secondary electron images ia (monochrome images ib) of the 10 different parts (area fraction RA) may be 0.01% or more and 20% or less. When the area fraction RA is 0.01% or more and 20% or less, peeling of the second electrode layer 2 from the second main surface s32 of the piezoelectric thin film 3 is easily suppressed. Furthermore, when the area fraction RA is 0.01% or more and 20% or less, the crystallinity of the first crystal grains c1 is easily improved, the orientation of the (0001) plane of aluminum nitride in the first crystal grains c1 is easily improved, and the piezoelectric characteristics of the piezoelectric thin film 3 are easily improved.
[0034] The Heywood diameter d of the second crystal grain c2 measured in the secondary electron image ia (monochrome image ib) may be 5 nm or more and 2000 nm or less. The area of any one of the second crystal grains c2 measured in the secondary electron image ia (monochrome image ib) is A C2 The Heywood diameter d of any one of the second crystal grains c2 can be expressed as (4A C2 / π) 1 / 2 (4A C2 / π) 1 / 2 is an area of A C2 In other words, the Heywood diameter d can be rephrased as a circle-equivalent diameter. When the Heywood diameter d is 5 nm or more and 2000 nm or less, the developed area ratio Sdr of the second main surface s32 tends to be 0.001 or more and 0.100 or less, and peeling of the second electrode layer 2 from the second main surface s32 of the piezoelectric thin film 3 is easily suppressed.
[0035] Any image analysis software may be used to binarize the secondary electron image ia, and to measure the area fraction RA and the Heywood diameter of the secondary crystal grains. The image analysis software may be a commercially available product or a non-commercial product. For example, Mac-View manufactured by Mountech Co., Ltd. may be used as the image analysis software.
[0036] As described above, the aluminum nitride contained in the piezoelectric thin film 3 may contain a divalent element Ed and a tetravalent element Et. Alternatively, the aluminum nitride contained in the piezoelectric thin film 3 may contain a trivalent element Etr. The aluminum nitride contained in the piezoelectric thin film 3 may contain all of the divalent element Ed, the trivalent element Etr, and the tetravalent element Et. Doping of the aluminum nitride with the divalent element Ed and the tetravalent element Et, or doping of the aluminum nitride with the trivalent element Etr distorts the wurtzite structure of the aluminum nitride, or changes the strength of the chemical bonds between atoms in the wurtzite structure. As a result, the piezoelectric thin film 3 is likely to contain both the first crystal grains c1 and the second crystal grains c2, the development area ratio Sdr is likely to be controlled to be 0.001 or more and 0.100 or less, and the piezoelectric characteristics of the piezoelectric thin film 3 are likely to be improved. The divalent element Ed may be at least one element selected from the group consisting of magnesium (Mg), calcium (Ca), strontium (Sr) and barium (Ba). The trivalent element Etr may be at least one element selected from the group consisting of scandium (Sc), yttrium (Y), lanthanoids and indium (In). The tetravalent element Et may be at least one element selected from the group consisting of zirconium (Zr), germanium (Ge), titanium (Ti) and hafnium (Hf).
[0037] The content of aluminum in aluminum nitride may be expressed as [Al] atomic % ([Al] mol %). The total content of divalent element Ed in aluminum nitride may be expressed as [Ed] atomic % ([Ed] mol %). For example, the content of magnesium in aluminum nitride may be expressed as [Mg] atomic % ([Mg] mol %). The total content of trivalent element Etr in aluminum nitride may be expressed as [Etr] atomic % ([Etr] mol %). For example, the content of scandium in aluminum nitride may be expressed as [Sc] atomic % ([Sc] mol %). The total content of tetravalent element Et in aluminum nitride may be expressed as [Et] atomic % ([Et] mol %). For example, the content of zirconium in aluminum nitride may be expressed as [Zr] atomic % ([Zr] mol %). For example, the content of hafnium in aluminum nitride may be expressed as [Hf] atomic % ([Hf] mol %). ([Ed]+[Et]) / ([Al]+[Ed]+[Et]) may be 0.03 to 0.60 (3% to 60%), or 0.40 to 0.44 (40% to 44%). For example, ([Mg]+[Zr]) / ([Al]+[Mg]+[Zr]) may be 0.03 to 0.60 (3% to 60%), or 0.40 to 0.44 (40% to 44%). For example, ([Mg]+[Hf]) / ([Al]+[Mg]+[Hf]) may be 0.03 to 0.60 (3% to 60%), or 0.03 to 0.59 (3% to 59%). When ([Ed]+[Et]) / ([Al]+[Ed]+[Et]) is 0.03 to 0.60, 0.03 to 0.59, or 0.40 to 0.44, the development area ratio Sdr is easily controlled to 0.001 to 0.100. Furthermore, when ([Ed]+[Et]) / ([Al]+[Ed]+[Et]) is 0.03 to 0.60, 0.03 to 0.59, or 0.40 to 0.44, the piezoelectric characteristics of the piezoelectric thin film 3 are easily improved. [Ed] / ([Ed]+[Et]) may be 0.25 or more and 0.60 or less, or 0.40 or more and 0.56 or less. For example, [Mg] / ([Mg]+[Zr]) may be 0.25 or more and 0.60 or less, or 0.40 or more and 0.56 or less. For example, [Hf] / ([Mg]+[Hf]) may be 0.25 or more and 0.60 or less, or 0.26 or more and 0.58 or less. When [Ed] / ([Ed]+[Et]) is 0.25 or more and 0.60 or less, 0.26 or more and 0.58 or less, or 0.40 or more and 0.56 or less, the development area ratio Sdr is easily controlled to 0.001 or more and 0.100 or less. Furthermore, when [Ed] / ([Ed]+[Et]) is 0.40 or more and 0.56 or less, the piezoelectric characteristics of the piezoelectric thin film 3 are likely to be improved. [Etr] / ([Al]+[Etr]) may be 0.10 or more and 0.40 or less (10% or more and 40% or less). For example, [Sc] / ([Al]+[Sc]) may be 0.10 or more and 0.40 or less (10% or more and 40% or less). When [Etr] / ([Al]+[Etr]) is 0.10 or more and 0.40 or less, the development area ratio Sdr is easily controlled to 0.001 or more and 0.100 or less. Furthermore, when [[Etr] / ([Al]+[Etr]) is 0.10 or more and 0.40 or less, the piezoelectric characteristics of the piezoelectric thin film 3 are easily improved.
[0038] The aluminum nitride contained in the piezoelectric thin film 3 may further contain at least one additive element selected from the group consisting of monovalent elements and pentavalent elements. The monovalent element may be at least one element selected from the group consisting of lithium (Li), sodium (Na), potassium (K), rubidium (Rb), and cesium (Cs). The pentavalent element may be at least one element selected from the group consisting of chromium (Cr), vanadium (V), niobium (Nb), and tantalum (Ta). The aluminum nitride contained in the piezoelectric thin film 3 may further contain other elements such as oxygen (O) and argon (Ar).
[0039] The first electrode layer 1 may contain at least one element selected from the group consisting of platinum (Pt), iridium (Ir), gold (Au), rhodium (Rh), palladium (Pd), silver (Ag), nickel (Ni), copper (Cu), aluminum (Al), molybdenum (Mo), tungsten (W), vanadium (V), chromium (Cr), niobium (Nb), tantalum (Ta), ruthenium (Ru), zirconium (Zr), hafnium (Hf), titanium (Ti), yttrium (Y), scandium (Sc), and magnesium (Mg). The first electrode layer 1 may be a metal element or an alloy.
[0040] The second electrode layer 2 may contain at least one element selected from the group consisting of Pt, Ir, Au, Rh, Pd, Ag, Ni, Cu, Al, Mo, W, V, Cr, Nb, Ta, Ru, Zr, Hf, Ti, Y, Sc, and Mg. The second electrode layer 2 may be a metal element or an alloy.
[0041] The piezoelectric thin film element 10 may further include a substrate. The first electrode layer 1 may directly or indirectly overlap the substrate. The piezoelectric thin film element 10 may further include an adhesion layer. The adhesion layer may be interposed between the substrate and the first electrode layer 1. In other words, the first electrode layer 1 may indirectly overlap the substrate via the adhesion layer.
[0042] For example, the substrate may be a semiconductor substrate (such as a silicon substrate or a gallium arsenide substrate), an optical crystal substrate (such as a sapphire substrate), an insulator substrate (such as a glass substrate or a ceramic substrate), a metal substrate (such as a stainless steel plate), or a silicon-on-insulator (SOI) substrate. The substrate may be crystalline. For example, the substrate may be single crystal or polycrystalline.
[0043] For example, the adhesion layer may contain at least one element selected from the group consisting of aluminum (Al), silicon (Si), titanium (Ti), zinc (Zn), yttrium (Y), zirconium (Zr), chromium (Cr), molybdenum (Mo), hafnium (Hf), tantalum (Ta), tungsten (W), platinum (Pt), and ruthenium (Ru). The adhesion layer may be a metal element, an alloy, or a compound (such as an oxide). The adhesion layer may be another piezoelectric thin film (e.g., aluminum nitride), a polymer, or a ceramic. The adhesion layer has a function of suppressing peeling of the first electrode layer due to mechanical impact or the like. The adhesion layer may be referred to as an interface layer, a support layer, a buffer layer, or an intermediate layer.
[0044] For example, the thickness of the substrate may be 50 μm or more and 10,000 μm or less. For example, the thickness of the adhesion layer may be 0.003 μm or more and 2 μm or less. For example, the thickness of the first electrode layer 1 may be 0.01 μm or more and 1 μm or less. For example, the thickness of the piezoelectric thin film 3 may be 100 nm or more and 30,000 nm or less. For example, the thickness of the second electrode layer 2 may be 0.01 μm or more and 1 μm or less. The thicknesses of the substrate, adhesion layer, first electrode layer 1, piezoelectric thin film 3, and second electrode layer 2 may each be approximately or completely uniform.
[0045] The crystal structures of the substrate, adhesion layer, first electrode layer, piezoelectric thin film, and second electrode layer may be identified by X-ray diffraction and electron diffraction. The compositions of the substrate, adhesion layer, first electrode layer, piezoelectric thin film, and second electrode layer may be identified by at least one of X-ray fluorescence analysis (XRF), X-ray photoelectron spectroscopy (XPS), energy dispersive X-ray analysis (EDX), inductively coupled plasma mass spectrometry (ICP-MS), laser ablation inductively coupled plasma mass spectrometry (LA-ICP-MS), and electron probe microanalyzer (EPMA). The thicknesses of the substrate, adhesion layer, first electrode layer, piezoelectric thin film, and second electrode layer may be measured by a scanning electron microscope in a cross section of the piezoelectric thin film element parallel to the stacking direction.
[0046] The adhesion layer, the first electrode layer, the piezoelectric thin film, and the second electrode layer may be sequentially laminated on the surface of the substrate by a vapor phase growth method such as sputtering. In particular, the piezoelectric thin film is formed by RF (Radio Frequency) magnetron sputtering. The adhesion layer, the first electrode layer, the piezoelectric thin film, and the second electrode layer may be formed by sputtering using at least one type of target. The adhesion layer, the first electrode layer, the piezoelectric thin film, and the second electrode layer may be formed by sputtering using multiple targets. The target may contain at least one element among the elements constituting each layer or the piezoelectric thin film. By selecting and combining targets having a predetermined composition, the composition of each of the adhesion layer, the first electrode layer, the piezoelectric thin film, and the second electrode layer can be controlled to a desired composition. For example, the target may be a metal element, an alloy, or an oxide. For example, when the piezoelectric thin film is aluminum nitride containing a divalent element and a tetravalent element, a target made of aluminum, a target made of a divalent element, and a target made of a tetravalent element may be used. One or more alloys made of two or more elements selected from the group consisting of aluminum, divalent elements, and tetravalent elements may be used as the target. For example, when the piezoelectric thin film is aluminum nitride containing a trivalent element, a target made of aluminum and a target made of a trivalent element may be used. For example, when the piezoelectric thin film is aluminum nitride containing a divalent element, a trivalent element, and a tetravalent element, a target made of aluminum, a target made of a divalent element, a target made of a trivalent element, and a target made of a tetravalent element may be used. One or more alloys made of two or more elements selected from the group consisting of aluminum, divalent elements, trivalent elements, and tetravalent elements may be used as the target. The composition of the sputtering atmosphere may be a control factor for the composition of each of the adhesion layer, the first electrode layer, the piezoelectric thin film, and the second electrode layer. For example, nitrogen gas is a raw material for the piezoelectric thin film (aluminum nitride). The input power (power density) applied to the cathode on which each target is placed may be a control factor for the composition and thickness of each of the adhesion layer, the first electrode layer, the piezoelectric thin film, and the second electrode layer.The total pressure of the sputtering atmosphere, the partial pressure or concentration of the source gas in the atmosphere, the duration of sputtering of each target, the temperature of the substrate surface, and the substrate bias may also be factors controlling the composition and thickness of each of the adhesion layer, the first electrode layer, the piezoelectric thin film, and the second electrode layer. A piezoelectric thin film having a desired shape or pattern may be formed by etching (e.g., plasma etching).
[0047] In conventional RF magnetron sputtering, the supply of cathode power (electrical power) to the cathode on which the target is placed and the supply of substrate bias (electrical power) to the substrate electrode (substrate including the first electrode layer) are performed in parallel, and then the supply of the cathode power and the substrate bias are stopped at the same time. On the other hand, in the process of forming the piezoelectric thin film according to the present embodiment, the supply of the cathode power and the substrate bias are performed in parallel, and then the supply of the cathode power is stopped first, and the supply of the substrate bias is continued for a further predetermined time. Furthermore, in the process of forming the piezoelectric thin film according to the present embodiment, the substrate bias is 20 W. In the process of the supply of the cathode power and the supply of the substrate bias being performed in parallel, partial epitaxial growth of a plurality of first crystal grains made of aluminum nitride with the (0001) plane oriented tends to proceed on the surface of the first electrode layer. However, by continuing the supply of the substrate bias of 20 W even after the supply of the cathode power is stopped, the atoms (Al, the divalent element Ed, the trivalent element Etr, the tetravalent element Et, etc.) that reach the surface of the aluminum nitride during the growth process from the target are likely to move near the surface of the aluminum nitride. As a result, multiple lattice defects are likely to be formed on the surface of the aluminum nitride. Multiple abnormal grains (second crystal grains) grow from the multiple lattice defects, forming a second main surface with an expanded area ratio of 0.001 or more and 0.100 or less. When the supply of the cathode power and the supply of the substrate bias are stopped at the same time, the growth of the multiple second crystal grains is suppressed, and the expanded area ratio is likely to become less than 0.001.
[0048] The piezoelectric thin film element according to the present embodiment has a wide variety of applications. For example, the piezoelectric thin film element may be a piezoelectric microphone, a harvester, an oscillator, a resonator, an acoustic multilayer film, or a filter. For example, the piezoelectric thin film element may be a piezoelectric actuator. The piezoelectric actuator may be used for haptics. That is, the piezoelectric actuator may be used in various devices that require feedback by skin sensation (tactile sensation). For example, the device that requires feedback by skin sensation may be a wearable device, a touch pad, a display, or a game controller. For example, the piezoelectric actuator may be used in a head assembly, a head stack assembly, or a hard disk drive. For example, the piezoelectric actuator may be used in a printer head or an inkjet printer device. The piezoelectric actuator may be used in a piezoelectric switch. For example, the piezoelectric thin film element may be a piezoelectric sensor or a piezoelectric transducer. For example, the piezoelectric sensor or the piezoelectric transducer may be used in a gyro sensor, a pressure sensor, a pulse wave sensor, an ultrasonic sensor, an ultrasonic transducer, or a shock sensor. The ultrasonic transducer may be a Piezoelectric Micromachined Ultrasonic Transducer (PMUT). Products using the piezoelectric micromachined ultrasonic transducer may be biometric sensors such as fingerprint sensors and ultrasonic blood vessel authentication sensors, sensors for medical or health care, or Time of Flight (ToF) sensors. For example, the filter may be a BAW (Bulk Acoustic Wave) filter or a SAW (Surface Acoustic Wave) filter. Each of the piezoelectric thin film elements described above may be a part or the whole of a Micro Electro Mechanical System (MEMS).
[0049] The present invention is not necessarily limited to the above-described embodiment. Various modifications of the present invention are possible without departing from the spirit of the present invention, and these modifications are also included in the present invention. EXAMPLES
[0050] The present invention will be described in detail with reference to the following examples and comparative examples, but the present invention is not limited to the following examples.
[0051] Example 1 A wafer made of single crystal silicon (Si) was used as the substrate. The diameter of the substrate was 8 inches, and the thickness of the substrate was 725 μm. The thickness of the substrate was uniform. The main surface of the substrate was parallel to the (100) plane of Si.
[0052] An adhesion layer was formed directly on the entire main surface of the substrate by RF magnetron sputtering in a vacuum chamber. The adhesion layer was made of aluminum nitride without any additive elements. A single element of Al was used as the sputtering target. The atmosphere in the vacuum chamber was a mixed gas of Ar and N2. The input power per unit area of the sputtering target was 3.72 W / cm2. 2 The temperature of the substrate during the formation of the adhesion layer was maintained at 300° C. The substrate bias was 30 W. The thickness of the adhesion layer was uniform. The thickness of the adhesion layer was adjusted to 30 nm.
[0053] A first electrode layer made of Mo was formed on the entire surface of the adhesive layer by RF magnetron sputtering in a vacuum chamber. Mo alone was used as the sputtering target. The atmosphere in the vacuum chamber was Ar gas. The input power per unit area of the sputtering target was 0.93 W / cm. 2 The temperatures of the substrate and the adhesive layer during the formation of the first electrode layer were maintained at 600° C. The thickness of the first electrode layer was uniform. The thickness of the first electrode layer was adjusted to 0.2 μm.
[0054] A piezoelectric thin film was formed directly on the entire surface of the first electrode layer by RF magnetron sputtering in a vacuum chamber. The sputtering targets were each made of a single metal, Al, Mg, or Zr. In other words, three types of metal targets were used. The atmosphere in the vacuum chamber was a mixed gas of Ar and N2. The input power per unit area (cathode power) of each sputtering target was 3.72 W / cm2. 2 The deposition pressure (air pressure inside the vacuum chamber) was 0.2 Pa. The substrate bias was 20 W. The supply of the substrate bias was stopped 10 seconds after the supply of the cathode power was stopped. The thickness of the piezoelectric thin film was adjusted to about 1000 nm.
[0055] The laminate produced by the above procedure consisted of a substrate, an adhesion layer laminated directly on the substrate, a first electrode layer laminated directly on the adhesion layer, and a piezoelectric thin film laminated directly on the first electrode layer.
[0056] <Composition of piezoelectric thin film> The composition of the piezoelectric thin film was analyzed by X-ray fluorescence analysis (XRF method). A wavelength dispersive X-ray fluorescence spectrometer (RIGAKU AZX-400) manufactured by Rigaku Corporation was used for the XRF method. The analysis results showed that the piezoelectric thin film was made of aluminum nitride containing magnesium and zirconium. ([Mg]+[Zr]) / ([Al]+[Mg]+[Zr]) in the piezoelectric thin film is shown in Table 1 below. The definition of ([Mg]+[Zr]) / ([Al]+[Mg]+[Zr]) is as described above. In Table 1 below, ([Mg]+[Zr]) / ([Al]+[Mg]+[Zr]) is expressed as "(Mg+Zr) ratio". [Mg] / ([Mg]+[Zr]) in the piezoelectric thin film is shown in Table 1 below. The definition of [Mg] / ([Mg]+[Zr]) is as described above. In Tables 1 to 3 below, [Mg] / ([Mg]+[Zr]) is expressed as "Mg ratio."
[0057] <Crystal structure of piezoelectric thin film> The crystal structure of the piezoelectric thin film was analyzed by X-ray diffraction (XRD). For the XRD, a multipurpose X-ray diffractometer (SmartLab) manufactured by Rigaku Corporation was used. 2θ-θ scan, ω scan, and 2θχ-φ scan were performed on the surface of the piezoelectric thin film using the above-mentioned X-ray diffractometer. The results of the analysis by XRD method are as follows. The piezoelectric thin film was made of crystalline aluminum nitride having a wurtzite structure. The aluminum nitride included a (0001) plane oriented parallel to the first major surface of the piezoelectric thin film (the surface of the first electrode layer). The first electrode layer had a body-centered cubic structure. The (110) plane of the body-centered cubic structure was parallel to the first major surface of the piezoelectric thin film (the surface of the first electrode layer).
[0058] <Developed area ratio Sdr> The developed area ratio Sdr of the second principal surface (exposed principal surface) of the piezoelectric thin film was measured by an atomic force microscope (AFM). The developed area ratio Sdr was measured in three measurement areas randomly selected from the second principal surface. In the direction parallel to the first principal surface of the piezoelectric thin film, each measurement area was a square with a side length of 5 μm. The average value of the developed area ratio Sdr of the three measurement areas was calculated. The measurement of the developed area ratio Sdr was performed based on the international standard (ISO25178). The atomic force microscope used was a Park XE-HDD manufactured by Park Systems Corporation. The average value of the developed area ratio Sdr is shown in Table 1 below.
[0059] <Cross section of piezoelectric thin film> The cross section of the piezoelectric thin film was observed by a transmission electron microscope (TEM). A Titan G2 manufactured by Thermo Fisher Scientific Inc. (formerly FEI company) was used as the TEM. The cross section observed by the TEM was perpendicular to the first main surface (surface of the first electrode layer) of the piezoelectric thin film. The results of the observation of the cross section of the piezoelectric thin film were as follows. A plurality of first crystal grains (columnar crystals) grew substantially or completely perpendicular to the first main surface (surface of the first electrode layer) of the piezoelectric thin film. A plurality of second crystal grains grew obliquely to the plurality of first crystal grains. Ends of the plurality of second crystal grains were exposed on the second main surface of the piezoelectric thin film. In other words, each of the plurality of convex portions formed on the second main surface of the piezoelectric thin film was composed of an end of one or more second crystal grains.
[0060] An electron diffraction pattern was measured at each of a plurality of measurement points in the cross section observed by the TEM. The electron diffraction pattern was also measured by the above-mentioned TEM. The electron diffraction pattern measured at any one of the first crystal grains exposed in the cross section included a diffraction spot originating from the (0002) plane of aluminum nitride in the first crystal grain. The electron diffraction pattern measured at any one of the second crystal grains exposed in the cross section included not only a diffraction spot originating from the (0002) plane of aluminum nitride in the first crystal grain, but also a diffraction spot originating from the (0002) plane of aluminum nitride in the second crystal grain. In other words, the (0002) plane (and the (0001) plane) of aluminum nitride in the second crystal grain was inclined with respect to the (0002) plane (and the (0001) plane) of aluminum nitride in the first crystal grain. In the electron diffraction pattern measured at the second crystal grain, the angle α between the reference line L1 and the reference line L2 was measured. The definitions of the reference line L1 and the reference line L2 are as described above. The angle θ between the (0001) plane of aluminum nitride in the first crystal grains and the (0001) plane of aluminum nitride in the second crystal grains was determined based on the angle α. The average value of the angle θ determined at a total of three measurement points is shown in Table 1 below.
[0061] <Area fraction and Heywood diameter> Secondary electron images of each of the ten measurement regions in the second principal surface of the piezoelectric thin film were taken by a scanning electron microscope (SEM). The ten measurement regions were randomly selected from the second principal surface. An SEM S-4700 manufactured by Hitachi High-Tech Corporation was used. Each secondary electron image was parallel to the first principal surface of the piezoelectric thin film. Each secondary electron image was rectangular, and the dimensions of each secondary electron image were 12.8 μm in length and 9.01 μm in width. A monochrome image of each secondary electron image was obtained by image processing (binarization processing) of each secondary electron image. The area fraction RA of multiple second crystal grains in each monochrome image was measured. The definition of the area fraction RA is as described above. The average value of the area fraction RA measured in the ten measurement regions is shown in Table 1 below. The Heywood diameter of each second crystal grain in each monochrome image was measured. The definition of the Heywood diameter is as described above. The maximum and minimum values of the Heywood diameter measured in the 10 measurement regions (secondary electron images) are shown in Table 1 below. Image processing of each secondary electron image and measurement of the area fraction RA and the Heywood diameter were performed using image analysis software. As the image analysis software, image analysis software (not for sale) manufactured by TDK Corporation was used.
[0062] <Piezoelectric constant d 33 > Piezoelectric constant d of the piezoelectric thin film 33 (Unit: pC / N) was measured. 33 The details of the measurement are as follows: The piezoelectric constant d 33 The average values are shown in Table 1 below. Measurement equipment: Piezotest 33 Meter (PM200) Frequency: 110Hz Clamping pressure: 0.25N
[0063] <Peeling rate of second electrode layer> The peeling rate of the second electrode layer was measured by the following crosshatch test, which was a method conforming to Japanese Industrial Standard K 5600-5-6:1999 (ISO 2409:1992). A second electrode layer made of silver was formed on the entire second principal surface of the piezoelectric thin film by sputtering. The thickness of the second electrode layer was approximately uniform. The thickness of the second electrode layer was adjusted to 60 μm. In the crosshatch test, the second electrode layer was divided into 1000 grids (squares) by forming multiple cross hatch cuts on the surface of the second electrode layer that were perpendicular to each other. The interval between the cuts was 1 mm. After the grids were formed, adhesive tape was attached to the entire surface of the second electrode layer. As the adhesive tape was peeled off from the surface of the second electrode layer, the number n of grids from which at least a part of the second electrode layer had peeled off from the second principal surface of the piezoelectric thin film was counted. The total number of grids formed on the surface of the second electrode layer is represented as N, and the peeling rate of the second electrode layer is defined as (n / N)×100. The peeling rate is shown in Table 1 below.
[0064] (Examples 2 to 18, Comparative Examples 1 and 2) In the process of forming the piezoelectric thin film in each of Examples 2 to 18 and Comparative Examples 1 and 2, the input power (cathode power) per unit area of each sputtering target was changed. In the process of forming the piezoelectric thin film in Comparative Example 1, no substrate bias (electric power) was supplied. That is, the substrate bias in the process of forming the piezoelectric thin film in Comparative Example 1 was 0 W. The substrate bias in the process of forming the piezoelectric thin film in Comparative Example 2 was 20 W. The supply of the substrate bias in Comparative Example 2 was stopped 60 seconds after the supply of the cathode power was stopped. In the process of forming the piezoelectric thin film in each of Examples 12 to 16, a target made of simple metal Hf was used instead of a target made of simple metal Zr. In the process of forming the piezoelectric thin film in each of Examples 17 and 18, a target made of an elemental metal Sc was used instead of a target made of an elemental metal Zr. In the process of forming the piezoelectric thin film in each of Examples 17 and 18, a target made of an elemental metal Mg was not used.
[0065] Except for the above points, the piezoelectric thin films of Examples 2 to 18 and Comparative Examples 1 and 2 were prepared in the same manner as in Example 1. The piezoelectric thin films of Examples 2 to 18 and Comparative Examples 1 and 2 were analyzed and measured in the same manner as in Example 1. The results of the analyses and measurements of the piezoelectric thin films of Examples 2 to 18 and Comparative Examples 1 and 2 are shown in Tables 1 to 3 below. In Table 2 below, ([Mg]+[Et]) / ([Al]+[Mg]+[Et]) is expressed as the "(Mg+Et) ratio." In Table 3 below, [Sc] / ([Al]+[Sc]) is represented as "Sc ratio."
[0066] The piezoelectric thin films of Examples 2 to 11 and Comparative Examples 1 and 2 were made of aluminum nitride containing magnesium and zirconium. The piezoelectric thin film in each of Examples 12 to 16 was made of aluminum nitride containing magnesium and hafnium. The piezoelectric thin film in each of Examples 17 and 18 was made of aluminum nitride containing scandium. The piezoelectric thin films of each of Examples 2 to 18 and Comparative Examples 1 and 2 were made of crystalline aluminum nitride having a wurtzite structure. The aluminum nitride in each of Examples 2 to 18 and Comparative Examples 1 and 2 included a (0001) plane oriented parallel to the first main surface (surface of the first electrode layer) of the piezoelectric thin film.
[0067] In all of Examples 2 to 18 and Comparative Examples 1 and 2, a plurality of first crystal grains (columnar crystals) grew substantially or completely perpendicular to the first main surface (surface of the first electrode layer) of the piezoelectric thin film. In all of Examples 2 to 18 and Comparative Example 2, a plurality of second crystal grains grew obliquely relative to a plurality of first crystal grains, whereas in Comparative Example 1, a plurality of second crystal grains was not detected. In all of Examples 2 to 18 and Comparative Example 2, the ends of the second crystal grains were exposed on the second main surface of the piezoelectric thin film. That is, in all of Examples 2 to 18 and Comparative Example 2, the multiple convex portions formed on the second main surface of the piezoelectric thin film were each composed of an end of one or more second crystal grains.
[0068] [Table 1]
[0069] [Table 2]
[0070] [Table 3]
[0071] Fig. 7(a) is a secondary electron image of a part of the second principal surface of the piezoelectric thin film of Example 7, measured by the SEM described above. The secondary electron image shown in Fig. 7(a) is parallel to the first principal surface. Fig. 7(b) is a monochrome image obtained by image processing (binarization processing) of the secondary electron image shown in Fig. 7(a).
[0072] Fig. 8 is an image of a cross section of the piezoelectric thin film of Example 7, which was measured by the TEM described above. The cross section shown in Fig. 8 is perpendicular to the first main surface of the piezoelectric thin film. The six asterisks (*) in Fig. 8 represent measurement points 1 to 6. Fig. 8 shows that the ends of the second crystal grains c2 are exposed on the second main surface s32 as convex portions. FIG. 9(a) is an electron beam diffraction pattern measured by irradiating an electron beam on measurement point 1 (first crystal grain) in the cross section shown in FIG. FIG. 9(b) is an electron beam diffraction pattern measured by irradiating an electron beam on measurement point 2 in the cross section shown in FIG. Figure 10(a) is an electron beam diffraction pattern measured by irradiating an electron beam on measurement point 3 (second crystal grain) in the cross section shown in Figure 8. The angle between the reference line L1 and the reference line L2 in Figure 10(a) was 11°. Figure 10(b) is an electron beam diffraction pattern measured by irradiating an electron beam on measurement point 4 (second crystal grain) in the cross section shown in Figure 8. The angle between the reference line L1 and the reference line L2 in Figure 10(b) was 12°. FIG. 11(a) is an electron beam diffraction pattern measured by irradiating an electron beam on measurement point 5 (first crystal grain) in the cross section shown in FIG. FIG. 11(b) is an electron beam diffraction pattern measured by irradiating an electron beam on measurement point 6 (first crystal grain) in the cross section shown in FIG. In each of the electron beam diffraction patterns of Example 7 described above, the four numerical values assigned to each diffraction spot are indices indicating the orientation of the lattice plane from which each diffraction spot originates. [Industrial Applicability]
[0073] For example, a piezoelectric thin film according to one aspect of the present invention may be used in a microphone, a sensor, a transducer, a filter, a harvester, or an actuator. [Explanation of symbols]
[0074] 1...first electrode layer, 2...second electrode layer, 3...piezoelectric thin film, 10...piezoelectric thin film element, s1...surface of the first electrode layer, s2...surface of the second electrode layer, s31...first main surface of the piezoelectric thin film, s32...second main surface of the piezoelectric thin film, c1...first crystal grain, c2...second crystal grain, uc...unit cell of aluminum nitride (wurtzite structure), θ...angle between the (0001) plane of aluminum nitride in the first crystal grain and the (0001) plane of aluminum nitride in the second crystal grain, Ed...divalent element, Etr...trivalent element, Et...tetravalent element.
Claims
1. A piezoelectric thin film having a first main surface and a second main surface located on a rear side of the first main surface, It comprises crystalline aluminum nitride having a wurtzite structure, The aluminum nitride contains a divalent element and a tetravalent element, or the aluminum nitride contains a trivalent element, The developed area ratio of the second main surface is 0.001 or more and 0.100 or less. Piezoelectric thin film.
2. A plurality of first crystal grains and a plurality of second crystal grains, both the first crystal grains and the second crystal grains comprise the aluminum nitride; a (0001) plane of the aluminum nitride in the first crystal grain is parallel to the first main surface, a (0001) plane of the aluminum nitride in the second crystal grains is inclined with respect to a (0001) plane of the aluminum nitride in the first crystal grains, A plurality of the second crystal grains are exposed on the second main surface. The piezoelectric thin film according to claim 1 .
3. A piezoelectric thin film having a first main surface and a second main surface located on a rear side of the first main surface, A plurality of first crystal grains and a plurality of second crystal grains, both the first grains and the second grains comprise crystalline aluminum nitride having a wurtzite structure; a (0001) plane of the aluminum nitride in the first crystal grain is parallel to the first main surface, a (0001) plane of the aluminum nitride in the second crystal grains is inclined with respect to a (0001) plane of the aluminum nitride in the first crystal grains, A plurality of the second crystal grains are exposed at the second main surface, The developed area ratio of the second main surface is 0.001 or more and 0.100 or less. Piezoelectric thin film.
4. an angle between a (0001) plane of the aluminum nitride in the first crystal grains and a (0001) plane of the aluminum nitride in the second crystal grains is 0.1° or more and 30° or less; The piezoelectric thin film according to claim 2 or 3.
5. a secondary electron image of the second main surface is taken by a scanning electron microscope; the secondary electron image is parallel to the first principal surface, a ratio of a total area of the plurality of second crystal grains in the secondary electron image is 0.01% or more and 20% or less; The piezoelectric thin film according to claim 2 or 3.
6. a secondary electron image of the second main surface is taken by a scanning electron microscope; the secondary electron image is parallel to the first principal surface, the Heywood diameter of the second crystal grains measured in the secondary electron image is 5 nm or more and 2000 nm or less; The piezoelectric thin film according to claim 2 or 3.
7. A piezoelectric thin film according to any one of claims 1 to 3, A first electrode layer; A second electrode layer; Equipped with the first major surface directly overlies the first electrode layer; the second electrode layer directly overlies the second major surface; Piezoelectric thin film element.
Citation Information
Patent Citations
Acoustic wave device
JP2013219743A
Piezoelectric thin film, manufacturing method thereof, and use thereof
JP2020077788A