Activated carbon and its manufacturing method, and device

By employing powdered activated carbon, polysaccharide thickener, and water-soluble polymer, followed by acid and heat treatment, the method addresses the limitations of binder-containing activated carbon, resulting in a product with enhanced crushing strength, heat resistance, and chemical resistance for diverse industrial uses.

JP2024134537APending Publication Date: 2024-10-03OSAKA GAS CHEM KK

Patent Information

Application Number
JP2024041006
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-20
Filing Date
2024-03-15
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing activated carbon molded products face issues with heat resistance, chemical resistance, and crushing strength due to the presence of binders, which degrade under high temperatures and solvents, leading to swelling, dissolution, and powder scattering.

Method used

The production method involves using powdered activated carbon, polysaccharide thickener, and water-soluble polymer, followed by acid treatment and heat treatment to create activated carbon with improved crushing strength, heat resistance, and chemical resistance.

Benefits of technology

The resulting activated carbon maintains its structural integrity and adsorption capacity under harsh conditions, including high temperatures and exposure to acids, alkalis, and organic solvents, making it suitable for various applications such as water purifiers and gas removal systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134537000001
    Figure 2024134537000001
Patent Text Reader

Abstract

To provide activated carbon having excellent crushing strength, heat resistance, and chemical resistance, its manufacturing method, and a device.SOLUTION: The activated carbon of the present invention satisfies the following requirements (1) to (3). (1) The crushing strength is 5.0 N or more. (2) The total pore volume having a diameter of 30 nm or less is 0.3 mL / g or more and 1.2 mL / g or less. (3) The mass loss rate up to 500°C and the mass loss rate from 500°C or more to 800°C or less in an inert gas atmosphere, as measured using a thermal mass-differential thermal analyzer, are 5.0 mass% or less, and 1.0 mass% or more and 25 mass% or less, respectively based on the dry mass of the activated carbon when the activated carbon is maintained at 115°C for 3 hours in an inert gas atmosphere.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to activated carbon and a method and apparatus for producing the same. [Background technology]

[0002] Activated carbon is an adsorbent with a high adsorption capacity due to its specific surface area. Since pores of various diameters can be given depending on the raw materials and the manufacturing conditions of carbonization and activation, the substances that can be adsorbed are also diverse. For this reason, activated carbon has traditionally been used in a wide range of applications in the industrial and consumer fields, such as purification and decolorization by adsorbing impurities, and deodorization by adsorbing odorous components. In recent years, with the development of technology in various fields, the performance requirements for activated carbon have become more sophisticated. Furthermore, with the recent trend toward low environmental impact, more highly functional activated carbon is required from the perspective of suppressing the release of harmful substances into the environment. For this reason, many studies have been conducted on highly functional activated carbon using various raw materials and carbonization and activation conditions.

[0003] In addition, many studies are being conducted on granular activated carbon and activated carbon molded products that are made from existing powdered activated carbon, molded and solidified with a binder to give them the desired functions.

[0004] For example, Patent Document 1 proposes a technique in which a thermoplastic resin is mixed with an adsorbent such as activated carbon, and the mixture is injection molded to obtain a molded product.

[0005] Patent Document 2 proposes a technique for obtaining an adsorbent molded product by bonding and / or adhering a thermoplastic resin to particles of an adsorbent such as activated carbon.

[0006] Patent Document 3 proposes a technique for obtaining activated carbon molded products by mixing fibrous activated carbon particles with polysaccharide, molding the mixture into a desired shape, and then heating the mixture to form a thermo-irreversible gel of the polysaccharide.

[0007] Patent Document 4 proposes a water purifier equipped with a cartridge in which a housing is filled with a specific activated carbon molded product obtained by mixing powdered activated carbon with a fibrous binder and molding the mixture. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2013-237854 A [Patent Document 2] Special Publication No. 2012-508645 [Patent Document 3] JP 2007-269555 A [Patent Document 4] JP 2017-136589 A Summary of the Invention [Problem to be solved by the invention]

[0009] However, in each of Patent Documents 1 to 4, the molded products contain a binder component in addition to carbon, so that it is difficult to use them under conditions where the heat resistance or chemical resistance of the binder component is problematic. For example, the binders described in Patent Documents 1 and 2 deteriorate in organic solvents. In addition, all of the binders described in Patent Documents 1 to 4 decompose when used constantly under high-temperature conditions, for example, at 200°C or higher. For this reason, it is difficult to use the molded products described in Patent Documents 1 to 4.

[0010] Furthermore, in all of Patent Documents 1 to 4, depending on the conditions, there is a concern that the molded product may swell or dissolve over time, resulting in a decrease in strength. Therefore, for example, when the molded product is used in a water purifier, there is a problem that the particles may be crushed during element molding and use. Also, when the molded product is used in gas removal or as a catalyst carrier, there is a problem that the powder may scatter during use.

[0011] The present invention has been made in view of the above problems, and an object of the present invention is to provide activated carbon having excellent crushing strength, heat resistance, and chemical resistance, and a method and apparatus for producing the same. [Means for solving the problem]

[0012] Means for Solving the Problems The present inventors have conducted intensive research to solve the above problems, and as a result have discovered that an activated carbon excellent in crushing strength, heat resistance, and chemical resistance can be obtained by kneading and molding powdered activated carbon, a thickening polysaccharide, a water-soluble polymer, and water as raw materials, and then subjecting the resulting molded product to an acid treatment and a heat treatment, thereby completing the present invention.

[0013] Furthermore, as a result of intensive research conducted by the present inventors to solve the above problems, it was discovered that an activated carbon obtained by kneading and molding powdered activated carbon or powdered carbon, a water-soluble polymer, and water as raw materials and then performing an activation treatment on the resulting molded product has excellent crushing strength, heat resistance, and chemical resistance, and thus the present invention was completed.

[0014] The present invention includes the following embodiments.

[0015] [1] Activated carbon satisfying the following requirements (1) to (3): (1) Crushing strength is 5.0 N or more; (2) Total pore volume having a diameter of 30 nm or less is 0.3 mL / g or more and 1.2 mL / g or less; (3) Mass loss rate up to 500°C in an inert gas atmosphere and mass loss rate at 500°C or more and 800°C or less, measured using a thermal gravimetric differential thermal analyzer, are 5.0 mass% or less and 1.0 mass% or more and 25 mass% or less, respectively, based on the dry mass of the activated carbon when the activated carbon is maintained at 115°C in an inert gas atmosphere for 3 hours.

[0016] [2] The activated carbon according to [1], further satisfying at least one requirement selected from the group consisting of the following (4) to (6): (4) The content of sulfur atoms is 0.01% by mass or more and 5.0% by mass or less. (5) The specific surface area, determined by the BET method from the N2 adsorption isotherm at -196°C, is 500 m 2 / g or more 1300m 2 (6) The ignition residue when incinerated in air at 850°C is 5.0 mass% or less.

[0017] [3] The activated carbon according to [2], which satisfies all of the requirements (4) to (6).

[0018] [4] An apparatus comprising the activated carbon according to any one of [1] to [3].

[0019] [5] A method for removing at least one substance selected from the group consisting of impurities, pollutants, residual chlorine, volatile organic compounds (VOCs), and coloring components, using the apparatus described in [4].

[0020] [6] A method for producing activated carbon, comprising a step of obtaining activated carbon that satisfies the following requirements (1) to (3): (1) the crushing strength is 5.0 N or more; (2) the total volume of pores having a diameter of 30 nm or less is 0.3 mL / g or more and 1.2 mL / g or less; and (3) the mass loss rate up to 500°C in an inert gas atmosphere and the mass loss rate from 500°C to 800°C, measured using a thermogravimetric differential thermal analyzer, are 5.0 mass% or less and 1.0 mass% to 25 mass%, respectively, based on the dry mass of the activated carbon when it is held at 115°C in an inert gas atmosphere for 3 hours.

[0021] [7] A method for producing activated carbon according to [6], comprising: a kneading step of kneading powdered activated carbon, a thickening polysaccharide, a water-soluble polymer, and water; a molding step of molding the kneaded mixture obtained in the kneading step; an acid treatment step of treating the molded product obtained in the molding step with an acid; and a heat treatment step of the acid-treated molded product obtained in the acid treatment step.

[0022] [8] A method for producing activated carbon according to [6], comprising: a kneading step of kneading powdered activated carbon, a thickening polysaccharide, a water-soluble polymer, and water; a molding step of molding the kneaded mixture obtained in the kneading step; an acid treatment step of acid-treating the molded product obtained in the molding step; a drying step of drying the acid-treated molded product obtained in the acid treatment step; and a heat treatment step of the dried product obtained in the drying step.

[0023] [9] A method for producing activated carbon according to any one of [6], comprising: a kneading step of kneading powdered activated carbon or powdered carbon with a water-soluble polymer and water; a molding step of molding the mixture obtained in the kneading step; and a step of activating the molded product obtained in the molding step.

[0024]

[10] A method for producing activated carbon according to [6], comprising: a kneading step of kneading powdered activated carbon or powdered carbon with a water-soluble polymer and water; a molding step of molding the mixture obtained in the kneading step; a drying step of drying the molded product obtained in the molding step; and a step of activating the dried product obtained in the drying step.

[0025]

[11] The method for producing activated carbon according to any one of [6] to

[10] , wherein the activated carbon further satisfies at least one requirement selected from the group consisting of the following (4) to (6): (4) The content of sulfur atoms is 0.01% by mass or more and 5.0% by mass or less. (5) The specific surface area, determined by the BET method from the N2 adsorption isotherm at -196°C, is 500 m 2 / g or more 1300m 2 (6) The ignition residue when incinerated in air at 850°C is 5.0 mass% or less.

[0026]

[12] The method for producing activated carbon according to

[11] , wherein the activated carbon satisfies all of the requirements (1) to (6).

[0027]

[13] The method for producing activated carbon described in [7] or [8], wherein the thickening polysaccharide comprises at least one selected from the group consisting of alginic acid and its salts, and carboxymethylcellulose and its salts.

[0028]

[14] The method for producing activated carbon described in [7], [8], or

[13] , wherein the amount of the thickening polysaccharide is 5 parts by mass or more and 30 parts by mass or less per 100 parts by mass of the water.

[0029]

[15] The method for producing activated carbon described in [7], [8],

[13] , or

[14] , wherein the thickening polysaccharide contains sodium alginate.

[0030]

[16] The method for producing activated carbon according to any one of [7] to

[15] , wherein the water-soluble polymer comprises at least one selected from the group consisting of lignosulfonic acid and salts thereof.

[0031]

[17] The method for producing activated carbon according to any one of [7] to

[16] , wherein the amount of the water-soluble polymer is 10 parts by mass or more and 100 parts by mass or less per 100 parts by mass of the powdered activated carbon or the powdered carbon.

[0032]

[18] The method for producing activated carbon according to any one of [7] to

[17] , wherein the water-soluble polymer contains sodium lignosulfonate. Effect of the Invention

[0033] According to the present invention, it is possible to provide activated carbon having excellent crushing strength, heat resistance, and chemical resistance, and a method and apparatus for producing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0034] Hereinafter, an embodiment for carrying out the present invention (hereinafter, simply referred to as "the present embodiment") will be described in detail. Note that the following present embodiment is an example for explaining the present invention, and the present invention is not limited to only this embodiment.

[0035] [Activated carbon] The activated carbon of this embodiment satisfies the following requirements (1) to (3). (1) The crushing strength is 5N or more. (2) The total volume of pores having a diameter of 30 nm or less is 0.3 mL / g or more and 1.2 mL / g or less. (3) The mass loss rate up to 500°C under an inert gas atmosphere measured using a thermogravimetric differential thermal analyzer (hereinafter also simply referred to as "mass loss rate up to 500°C"), and the mass loss rate at 500°C or more and 800°C or less under an inert gas atmosphere measured using a thermogravimetric differential thermal analyzer (hereinafter also simply referred to as "mass loss rate at 500°C or more and 800°C or less") are 5.0% by mass or less and 1.0% by mass or more and 25% by mass or less, respectively, based on the dry mass of the activated carbon when maintained at 115°C under an inert gas atmosphere for 3 hours.

[0036] By satisfying these specific requirements, the activated carbon has excellent crushing strength, heat resistance, and chemical resistance. Such activated carbon tends to maintain its crushing strength even when exposed to any of acids, alkalis, and organic solvents. Therefore, when the activated carbon is used by filling it into a column, cartridge, adsorption tower, filter, or sheet (hereinafter also simply referred to as "column, etc."), it tends to maintain its function as an adsorbent even under harsh conditions such as high temperature and low pH.

[0037] Activated carbon can be obtained by using powdered activated carbon, thickening polysaccharides, water-soluble polymers, and water as raw materials, kneading and molding the raw materials, and subjecting the resulting molded product to an acid treatment and a heat treatment. Activated carbon can also be obtained by using powdered activated carbon or powdered carbon, water-soluble polymers, and water as raw materials, kneading and molding the raw materials, and subjecting the resulting molded product to an activation treatment. For example, any powdered activated carbon or powdered carbon can be used as a raw material for such activated carbon, including wood-based activated carbon powders that have traditionally only been available in powder form, and the thermal or chemical stability of carbon allows it to be used stably for various purposes.

[0038] The activated carbon has a crushing strength of 5N or more. Therefore, even if the activated carbon is permeated with, for example, gas, water, oil, and organic solvents, it tends not to collapse. For example, activated carbon in a powder form or with poor strength and durability tends to have a crushing strength of less than 5N, and when such activated carbon is packed into a column or the like, the resistance to air or liquid passage increases as it collapses. Therefore, the amount of activated carbon packed may be limited. On the other hand, the activated carbon of this embodiment has a crushing strength of 5N or more, so that it can be packed into a column or the like with a high amount. Therefore, by using the activated carbon of this embodiment, a column or the like having high adsorption performance can be obtained, and for example, removal and treatment of pollutants contained in exhaust gas, waste liquid, and wastewater can be easily performed. The upper limit of the crushing strength is not particularly limited, but is, for example, 100N or less. In this embodiment, the crushing strength is measured using a known hardness tester such as a Kiya hardness tester. For a specific measurement method, refer to the Examples.

[0039] From the viewpoint of more effectively and reliably achieving the object of the present invention, the crushing strength of the activated carbon is preferably 10N or more and 50N or less, more preferably 15N or more and 48N or less, and even more preferably 20N or more and 47N or less.

[0040] The activated carbon has a total pore volume having a diameter of 30 nm or less of 0.3 mL / g or more and 1.2 mL / g or less. When the total pore volume is 0.3 mL / g or more, the gasification of the water-soluble polymer and thickening polysaccharide of the raw material can be more suitably suppressed in the production process of the activated carbon, and the gas adsorption into the pores tends to be more suitably controlled. When the total pore volume is 1.2 mL / g or less, the carbonization of the water-soluble polymer and thickening polysaccharide of the raw material can be more sufficiently performed in the production process of the activated carbon, and the powdered activated carbon particles contained in the activated carbon also tend to maintain a sufficient strength. Therefore, when the total pore volume is in the above range, activated carbon having better crushing strength, heat resistance, and chemical resistance can be obtained. In this embodiment, the total pore volume is measured using a nitrogen adsorption method. For a specific measurement method, refer to the Examples.

[0041] Since there is a tendency to obtain activated carbon having even better crushing strength, heat resistance, and chemical resistance, the total pore volume is preferably 0.4 mL / g or more and 1.1 mL / g or less, and more preferably 0.5 mL / g or more and 0.9 mL / g or less.

[0042] The activated carbon has a mass loss rate of 5.0% or less by mass up to 500°C and a mass loss rate of 1.0% or more by mass to 25% or less by mass, based on the dry mass of the activated carbon when kept at 115°C for 3 hours in an inert gas atmosphere. Therefore, the activated carbon tends to be able to withstand use conditions up to 500°C. For example, the mass loss rate of a conventional activated carbon molded product containing an organic binder tends to exceed 5.0% by mass up to 500°C, and the mass loss rate of 1.0% or more by mass to 25% or less by mass at 500°C to 800°C is not in the range. If such activated carbon is packed in a column or the like, the activated carbon may collapse when the use temperature reaches, for example, 200°C. On the other hand, the activated carbon of the present embodiment has a mass loss rate up to 500° C. and a mass loss rate from 500° C. to 800° C. both within a specific range, and therefore, even when packed in a column or the like, the activated carbon tends to be stable and durable up to an operating temperature of, for example, about 500° C. Therefore, the activated carbon of the present embodiment can be used, for example, for waste oil treatment at high temperatures or for catalytic applications.

[0043] The lower limit of the mass loss rate up to 500°C is not particularly limited, but is, for example, 0.01% by mass or more. In this embodiment, the mass loss rate up to 500°C and the mass loss rate from 500°C to 800°C are measured and calculated using a thermogravimetric differential thermal analyzer. For specific measurement and calculation methods, see the Examples. It is preferable to use nitrogen as the inert gas.

[0044] Since activated carbon having superior crushing strength, heat resistance, and chemical resistance tends to be obtained, the mass loss rate up to 500°C is preferably 0.1% by mass or more and 4.5% by mass or less, and more preferably 1.0% by mass or more and 4.3% by mass or less.

[0045] Since activated carbon having superior crushing strength, heat resistance, and chemical resistance tends to be obtained, the mass loss rate at 500° C. to 800° C. is preferably 3.0% by mass to 24% by mass, and more preferably 3.5% by mass to 20% by mass. The lower limit of the mass loss rate at 500° C. to 800° C. is more preferably 5.0% by mass or more.

[0046] It is preferable that the activated carbon further satisfies at least one requirement selected from the group consisting of the following (4) to (6). (4) The content of sulfur atoms is 0.01% by mass or more and 5.0% by mass or less. (5) The specific surface area calculated by the BET method from the N2 adsorption isotherm at -196°C is 500 m 2 / g or more 1300m 2 / g or less. (6) The ignition residue when incinerated in air at 850°C is 5.0 mass% or less.

[0047] Such activated carbon tends to be more excellent in crushing strength, heat resistance, and chemical resistance. Since activated carbon having even more excellent crushing strength, heat resistance, and chemical resistance tends to be obtained, the activated carbon preferably satisfies the above requirements (1) to (3) and at least one requirement selected from the group consisting of (4) to (6), more preferably satisfies the above requirements (1) to (3) and at least two requirements selected from the group consisting of (4) to (6), and more preferably satisfies all of the above requirements (1) to (6).

[0048] In the activated carbon, the content of sulfur atoms is preferably 0.01% by mass or more and 5.0% by mass or less. When the content of sulfur atoms is within the above range, the carbonization of the water-soluble polymer and thickening polysaccharide as raw materials can be performed more sufficiently in the production process of the activated carbon, and the gasification of the water-soluble polymer and thickening polysaccharide tends to be more suitably suppressed. Therefore, the carbonization reaction of the water-soluble polymer and thickening polysaccharide proceeds more appropriately, and activated carbon with better crushing strength, heat resistance, and chemical resistance tends to be obtained. In this embodiment, the content of sulfur atoms is measured and calculated using known analytical devices such as an atomic absorption spectrometer, an inductively coupled plasma mass spectrometer (ICP-MS), an ion chromatograph (IC), and an energy dispersive X-ray analyzer (EDX). For specific measurement and calculation methods, refer to the Examples.

[0049] Since activated carbon having even better crushing strength, heat resistance, and chemical resistance tends to be obtained, the content of sulfur atoms is preferably 0.05% by mass or more and 4.0% by mass or less, and more preferably 0.1% by mass or more and 3.0% by mass or less.

[0050] The specific surface area of ​​activated carbon calculated by the BET method from the N2 adsorption isotherm at -196°C is 500 m 2 / g or more 1300m 2 / g or less is preferable. When the specific surface area is within the above range, the carbonization of the water-soluble polymer and thickening polysaccharide of the raw material can be performed more sufficiently in the production process of the activated carbon, and the gasification of the water-soluble polymer and thickening polysaccharide tends to be more suitably suppressed. Therefore, the carbonization reaction of the water-soluble polymer and thickening polysaccharide proceeds more appropriately, and activated carbon with better crushing strength, heat resistance, and chemical resistance tends to be obtained. In this embodiment, the specific surface area is determined by the BET method from the adsorption isotherm of N2 at -196 ° C. For a specific measurement method, refer to the Examples.

[0051] Since there is a tendency to obtain activated carbon with even better crushing strength, heat resistance, and chemical resistance, the specific surface area of ​​the activated carbon is set to 550 m 2 / g or more 1250m2 / g or less, and 2 / g or more 1200m 2 / g or less. The specific surface area of ​​the activated carbon is preferably 550 m 2 / g or more 1000m 2 / g or less, and 2 / g or more 800m 2 / g or less.

[0052] The activated carbon preferably has an ignition residue of 5.0% by mass or less when incinerated at 850° C. in air. When the ignition residue is within the above range, the activated carbon tends to generate very little elution even when it is permeated with, for example, gas, water, oil, and organic solvent. For example, conventional coal activated carbon tends to have an ignition residue of more than 5.0% by mass when incinerated at 850° C. in air, and when such coal activated carbon is packed into a column or the like, it tends to generate elution depending on the type of gas or solvent, and to cause problems such as product contamination. On the other hand, the activated carbon of the present embodiment has an ignition residue of 5.0% by mass or less when incinerated at 850° C. in air, and therefore tends to be able to obtain a column or the like that is unlikely to generate elution even when packed into a column or the like and is unlikely to cause product contamination. Therefore, by using the activated carbon of the present embodiment, for example, water purifiers and edible oil refining tend to be able to be performed safely. The lower limit of the ignition residue is not particularly limited, but is, for example, 0.001% by mass or more. In this embodiment, the ignition residue is measured by incinerating activated carbon by a known method in air at 850° C. For specific measurement methods, see the Examples.

[0053] Since activated carbon having superior crushing strength, heat resistance, and chemical resistance tends to be obtained, the ignition residue is preferably 0.01% by mass or more and 4.5% by mass or less, and more preferably 0.1% by mass or more and 4.0% by mass or less.

[0054] The shape of the activated carbon varies depending on the application, and is not particularly limited. Examples of such shapes include rods such as cylinders, elliptical cylinders, elliptical truncated cones, and polygonal prisms such as triangular prisms, quadrangular prisms, pentagonal prisms, and hexagonal prisms, pellets, substrates (sheets), and blocks. For example, when used in a column or the like, the shape is preferably cylindrical. In this specification, the term "cylindrical shape" does not necessarily mean a strict cylinder in terms of geometry, and includes cylindrical shapes in which the cross-sectional shape (hereinafter simply referred to as "cross-sectional shape") in a plane perpendicular to the central axis of the cylinder is oval, right circular, and elliptical, and also includes cylinders that are somewhat curved or have a somewhat uneven surface. In this specification, a right circular or elliptical shape means, for example, a shape with a ratio of the major axis to the minor axis (major axis / minor axis) of 3 or less. As the cross-sectional shape, a circle and an ellipse are preferable because they enable the activated carbon to be packed more densely in a column or the like.

[0055] When activated carbon has a cylindrical shape, the diameter of the cross-sectional shape varies depending on the application, but for example, when used in a column, it is usually about 1.0 mm to 10.0 mm. In this specification, the "diameter" means the diameter of the circle when the cross-sectional shape is circular. On the other hand, when the cross-sectional shape is egg-shaped, oval, or elliptical, the "diameter" means the longest direction (i.e., the long axis direction) in these shapes. In this specification, the "circular" includes not only a perfect circle, but also an egg shape, a right circle, and an ellipse.

[0056] When the activated carbon has a cylindrical shape, the longitudinal length of the cylinder varies depending on the application, but for example, when used in a column or the like, it is usually about 1.0 mm or more and 20.0 mm or less.

[0057] When the activated carbon is in the form of pellets, the planar shape can be, for example, a shape applicable to columns and the like. Examples of such shapes include, for example, circular, elliptical, rectangular, rod-like, and distorted shapes in plan view. When the activated carbon is in the form of pellets, the thickness is not particularly limited, and known adsorbents that are applied to columns and the like can be used as a reference. The thickness is preferably a thickness that can be applied to columns and the like, and is usually 100 μm or more and 10,000 μm or less.

[0058] When the activated carbon is in the form of a cylindrical pellet, the diameter of the pellet is preferably 2.0 mm or more and 10 mm or less, and the aspect ratio is preferably 1:1 to 1:10. Such pellets are suitable as an adsorbent in a column or the like. In this specification, the aspect ratio means the ratio of the diameter to the height of one piece of activated carbon, that is, the diameter of the activated carbon: the height of the activated carbon. The aspect ratio means the average aspect ratio of 30 pieces of activated carbon randomly taken.

[0059] The activated carbon is preferably obtained through a kneading process of kneading powdered activated carbon, a thickening polysaccharide, a water-soluble polymer, and water, a molding process of molding the kneaded product obtained in the kneading process, an acid treatment process of acid-treating the molded product obtained in the molding process, and a heat treatment process of the acid-treated molded product obtained in the acid treatment process. It is also preferable that the activated carbon is obtained through a kneading process of kneading powdered activated carbon, a thickening polysaccharide, a water-soluble polymer, and water, a molding process of molding the kneaded product obtained in the kneading process, an acid treatment process of acid-treating the molded product obtained in the molding process, a drying process of drying the acid-treated molded product obtained in the acid treatment process, and a heat treatment process of the dried product obtained in the drying process. Furthermore, it is also preferable that the activated carbon is obtained through a kneading step of kneading powdered activated carbon or powdered carbon with a water-soluble polymer and water, a molding step of molding the kneaded product obtained in the kneading step, and a step of activating the molded product obtained in the molding step. According to such a specific step, activated carbon satisfying the above requirements (1) to (3) can be more preferably obtained. According to such a specific step, activated carbon satisfying the above requirements (1) to (3) and at least one requirement selected from the group consisting of the above requirements (4) to (6) can be more preferably obtained, activated carbon satisfying the above requirements (1) to (3) and at least two requirements selected from the group consisting of the above requirements (4) to (6) can be more preferably obtained, and activated carbon satisfying all of the above requirements (1) to (6) can be particularly preferably obtained. Therefore, activated carbon having excellent crushing strength, heat resistance, and chemical resistance can be more preferably obtained.

[0060] [Kneading process] The activated carbon is preferably obtained through a kneading process in which powdered activated carbon, a thickening polysaccharide, a water-soluble polymer, and water are kneaded. It is also preferable that the activated carbon is obtained through a kneading process in which powdered activated carbon or powdered carbon, a water-soluble polymer, and water are kneaded.

[0061] The kneading step can be carried out by a known method. Examples of such a method include a method of kneading each component using a blender, a paddle mixer, a kneader mixer, a screw mixer, a Henschel mixer, and a conical mixer. The temperature in the kneading step is usually room temperature, and the components are kneaded until they can be held by hand.

[0062] The kneading temperature can be, for example, from 5° C. to 50° C. The kneading time can be, for example, from 5 minutes to 60 minutes.

[0063] (powder activated carbon) The powdered activated carbon used as the raw material of the activated carbon is not particularly limited, and various types can be used. Examples of the powdered activated carbon include wood, wood flour, fruit shells such as coconut shells, seeds such as palm kernels, plums, and peaches, by-products during pulp production, bagasse, blackstrap molasses, coal (peat, lignite, brown coal, bituminous coal, etc.), anthracite, petroleum distillation residue components, petroleum pitch, coke, and coal tar, and other plant-based or fossil-based raw materials; various synthetic resins such as phenol resins, vinyl chloride resins, vinyl acetate resins, melamine resins, urea resins, resorcinol resins, celluloid, epoxy resins, polyurethane resins, polyester resins, acrylic resins, and polyamide resins; synthetic rubbers such as polybutylene, polybutadiene, and polychloroprene; other synthetic wood; and powdered activated carbon made from synthetic pulp, etc. These raw materials for the powdered activated carbon can be used alone, or two or more types can be mixed in any ratio depending on the required specifications. Of these, powdered activated carbon made from wood flour and coconut shells is preferred because it tends to give activated carbon with superior crushing strength, heat resistance, and chemical resistance.

[0064] The powdered activated carbon may contain additives, etc., if necessary. The additives, etc. may be added to the activated carbon, if necessary. Examples of such additives include water, coal tar, anhydrous tar, hard pitch, coal tar pitch, and petroleum pitch. The additives, etc. may be used alone, or two or more types may be mixed in any ratio according to the required specifications. The additives, etc. are usually mixed in an amount of 1 part by mass to 50 parts by mass per 100 parts by mass of the raw material or activated carbon. When mixing the raw material or activated carbon with the additive, the oxygen content of the raw material or activated carbon may be adjusted in advance to a range of 1% by mass to 20% by mass per 100% by mass of the raw material or activated carbon, if necessary. The oxygen content can be adjusted, for example, by mixing the raw material or activated carbon with oxygen under heating at 150°C to 300°C.

[0065] The powdered activated carbon may be activated carbon that has been carbonized or infusible as necessary and then activated. The carbonization method, infusibility method, and activation method are not particularly limited, and conventional methods can be used. Examples of the activation method include a gas activation method in which a carbon raw material, its carbonized product, or its infusible product is heat-treated in an activation gas at about 500°C to 1000°C, and a chemical activation method in which a carbon raw material, its carbonized product, or its infusible product is mixed with an activator and heat-treated at about 300°C to 800°C. Examples of the activation gas include water vapor and carbon dioxide. Examples of the activator include phosphorus or sulfur acid, zinc chloride, potassium hydroxide, and sodium hydroxide. The activated carbon obtained by the activation treatment may be used as it is. The activated carbon obtained by the activation treatment may be used after being washed with acid or water, heat-treated, and dried to remove attached components and surface functional groups of the activated carbon.

[0066] The average particle size (D50) of the powdered activated carbon is usually about 0.1 μm or more and 1000 μm or less. Since activated carbon having better crushing strength, heat resistance, and chemical resistance tends to be obtained, the average particle size (D50) of the powdered activated carbon is preferably 0.1 μm or more and 100 μm or less. When the average particle size (D50) of the powdered activated carbon is in the above range, the particle surface area becomes suitable, and the amount of the water-soluble polymer tends to be suitably adjusted. Therefore, activated carbon having better crushing strength, heat resistance, and chemical resistance tends to be obtained. In this specification, the average particle size (D50) is measured as a volume-based median size using a laser diffraction light scattering particle size distribution measuring device. In addition, powdered activated carbon or powdered carbon having a desired average particle size (D50) can be obtained, for example, by sieving or classification.

[0067] These powdered activated carbons can be used alone or in a mixture of two or more in any ratio according to the required specifications. In addition, components other than the powdered activated carbon may be appropriately mixed according to the required specifications of the activated carbon, as long as the carbon content after the heat treatment is not less than 80 mass %.

[0068] The powdered activated carbon may be used in the form of a slurry dispersed in a solvent such as water. For example, when water is used as a solvent, the content of the powdered activated carbon in the slurry is preferably 5% by mass or more and 50% by mass or less, more preferably 20% by mass or more and 40% by mass or less, relative to 100% by mass of water. When the slurry is used as a raw material for activated carbon, activated carbon having superior crush strength, heat resistance, and chemical resistance tends to be obtained.

[0069] The blending ratio of powdered activated carbon to thickening polysaccharide is preferably 30:70 to 97:3, more preferably 50:50 to 95:5, by mass. When the blending amount of powdered activated carbon is 30 parts by mass or more, the activated carbon tends to be more hardened and less likely to become embrittled. When the blending amount of powdered activated carbon is 97 parts by mass or less, the adsorption capacity of the activated carbon tends to be large. When the blending ratio is within the above range, the activated carbon tends to be more excellent in crushing strength, heat resistance, and chemical resistance.

[0070] (Powdered Carbon) The powdered carbon used as the raw material for activated carbon is not particularly limited, and various types can be used. Examples of powdered carbon include wood, wood flour, fruit shells such as coconut shells, seeds such as palm kernels, plums, and peaches, by-products during pulp production, bagasse, blackstrap molasses, coal (peat, lignite, brown coal, bituminous coal, etc.), anthracite, petroleum distillation residue components, petroleum pitch, coke, and coal tar, and other plant-based or fossil-based raw materials; various synthetic resins such as phenolic resins, vinyl chloride resins, vinyl acetate resins, melamine resins, urea resins, resorcinol resins, celluloid, epoxy resins, polyurethane resins, polyester resins, acrylic resins, and polyamide resins; synthetic rubbers such as polybutylene, polybutadiene, and polychloroprene; other synthetic wood; and pulp made from crushed carbon. These raw materials for powdered carbon can be used alone, or two or more types can be mixed in any ratio depending on the required specifications. Of these, powdered carbon made from wood flour, coal, and coconut shells is preferred because it tends to give activated carbon with superior crushing strength, heat resistance, and chemical resistance.

[0071] The powdered carbon may contain additives, etc., as necessary. The additives, etc. may also be added to the activated carbon, as necessary. For such additives, etc., and their blending amounts, as well as for adjusting the amount of oxygen when mixing the additives with the raw material or the activated carbon, refer to the additives, etc., and blending amounts exemplified above for the powdered activated carbon.

[0072] The powdered carbon may be carbonized or infusible carbon as required. The carbonization method and the infusibility method are not particularly limited, and conventional methods can be used.

[0073] The average particle size (D50) of the powdered carbon is usually about 0.1 μm or more and 1000 μm or less. Since activated carbon having better crushing strength, heat resistance, and chemical resistance tends to be obtained, the average particle size (D50) of the powdered carbon is preferably 0.1 μm or more and 100 μm or less. When the average particle size (D50) of the powdered carbon is in the above range, the particle surface area becomes suitable, and the amount of the water-soluble polymer tends to be suitably adjusted. Therefore, activated carbon having even better crushing strength, heat resistance, and chemical resistance tends to be obtained.

[0074] These powdered carbons can be used alone or in combination of two or more in any ratio according to the required specifications. In addition, components other than the powdered carbon can be appropriately mixed according to the required specifications as the activated carbon, as long as the carbon content after activation treatment is not less than 80 mass %.

[0075] (Thickening polysaccharides) The thickening polysaccharides used as the raw material of activated carbon are not particularly limited, and both natural and synthetic products can be used. Examples of such thickening polysaccharides include alginic acid, carboxymethylcellulose, xanthan gum, gellan gum, pectin, carrageenan, gum arabic, succinoglycan, guardran, locust bean gum, guar gum, tara gum, tamarin or sulfur seed gum, pullulan, soybean polysaccharides, gelatin, agar, and propylene glycol. These thickening polysaccharides may be salts such as sodium salts, potassium salts, magnesium salts, and calcium salts. As the salts, sodium salts and potassium salts are preferred.

[0076] These thickening polysaccharides can be used alone or in combination of two or more in any ratio according to the required specifications. In the present embodiment, components other than the thickening polysaccharides may be appropriately mixed according to the required specifications as activated carbon.

[0077] Among these, the thickening polysaccharide is preferably a thickening polysaccharide having at least one substituent selected from the group consisting of a carboxy group and a sulfonic acid group, since it is easily compatible with the surface of the powdered activated carbon. Examples of such thickening polysaccharides include alginic acid and its salts, carboxymethylcellulose and its salts, xanthan gum, gellan gum, pectin, carrageenan, gum arabic, and succinoglycan. Among these, the thickening polysaccharide more preferably contains at least one selected from the group consisting of alginic acid and its salts, and carboxymethylcellulose and its salts, more preferably contains at least one selected from the group consisting of alginates and carboxymethylcellulose salts, and even more preferably contains sodium alginate. As the salt, the above salts may be referred to. As the salt, sodium salts and potassium salts are preferred. These thickening polysaccharides tend to be more compatible with the surface of the powdered activated carbon, and to obtain activated carbon having excellent crush strength, heat resistance, and chemical resistance, as well as excellent durability.

[0078] The amount of thickening polysaccharide blended is preferably 5.0 parts by mass to 30 parts by mass, more preferably 7.0 parts by mass to 27 parts by mass, and even more preferably 10 parts by mass to 25 parts by mass, relative to 100 parts by mass of water. When the amount of thickening polysaccharide blended is within the above range, activated carbon having superior crushing strength, heat resistance, and chemical resistance tends to be obtained.

[0079] (Water-soluble polymer) The water-soluble polymer used as the raw material of activated carbon can be either naturally derived or synthetic. Naturally derived products include, for example, plant-derived products such as starch, methylcellulose, lignin sulfonic acid and its salts, and animal-derived products such as protein, collagen, phosphorus or sulfur lipids. Synthetic products include, for example, resins such as phenolic resins and acrylic resins. Salts include sodium salts, potassium salts, magnesium salts, calcium salts, and ammonium salts. As salts, sodium salts and potassium salts are preferred.

[0080] These water-soluble polymers can be used alone or in combination of two or more at any ratio depending on the required specifications. In this embodiment, components other than the water-soluble polymer may be appropriately mixed depending on the required specifications of the activated carbon.

[0081] Among these, the water-soluble polymer preferably contains at least one selected from the group consisting of lignin sulfonic acid and its salts, and phenolic resins, since the more carbon remaining after heat treatment, the more excellent the crushing strength, heat resistance, and chemical resistance, as well as the more excellent the durability of the activated carbon obtained. Among these, the water-soluble polymer more preferably contains at least one selected from the group consisting of lignin sulfonic acid and its salts, more preferably contains lignin sulfonate, and even more preferably contains sodium lignin sulfonate. Since lignin sulfonic acid and its salts have a larger amount of carbon remaining after heat treatment, activated carbon tends to have more excellent crushing strength, heat resistance, and chemical resistance, as well as excellent durability. In addition, lignin sulfonic acid and its salts are less likely to block all the pores of the activated carbon, and since they are naturally derived products, they tend to reduce the burden on the environment.

[0082] The amount of the water-soluble polymer is preferably 10 parts by mass or more and 150 parts by mass or less, more preferably 20 parts by mass or more and 130 parts by mass or less, even more preferably 25 parts by mass or more and 100 parts by mass or less, and even more preferably 30 parts by mass or more and 80 parts by mass or less, relative to 100 parts by mass of the powdered activated carbon or powdered carbon. When the amount of the water-soluble polymer is within the above range, the powdered activated carbon or powdered carbon can be more sufficiently solidified, so that activated carbon with better crushing strength, heat resistance, and chemical resistance tends to be obtained. In addition, the carbon derived from the water-soluble polymer remaining after the heat treatment or activation treatment can be suitably controlled, so that activated carbon with excellent adsorption performance tends to be obtained.

[0083] (water) Examples of water include pure water such as ion-exchanged water, ultrafiltered water, reverse osmosis water, and distilled water, as well as ultrapure water from which ionic impurities have been removed as much as possible.

[0084] (Additives) In the kneading step, an additive may be further added. For example, sodium carbonate may be used as such an additive. By adding sodium carbonate in the kneading step, the viscosity reduction caused by the protonation of the water-soluble polymer or the thickening polysaccharide during kneading is less likely to occur, and a kneaded product having a more suitable viscosity tends to be obtained.

[0085] [Molding process] The activated carbon is preferably obtained through a molding step in which the kneaded product obtained in the kneading step is molded.

[0086] The molding method is not particularly limited, and known conditions can be adopted depending on the quality required for the activated carbon. For example, when obtaining activated carbon having a cylindrical shape or a pellet shape, the shape and size can be appropriately set and extrusion molding can be performed.

[0087] The extrusion molding machine is not particularly limited, and a known extrusion molding machine can be used. For example, a multi-screw extrusion molding machine equipped with kneading blades and screws inside can be used as such a molding machine. In addition, when obtaining pelletized activated carbon, for example, an extrusion granulator such as a disk pelletizer can be used.

[0088] After the molding step, the molded product may be washed and / or dried. The conditions for washing and / or drying are not particularly limited, and known conditions may be used. For the drying treatment, the drying step described below may be referred to. In this embodiment, the molded product may be directly subjected to the next acid treatment step without washing and drying. If such a molded product is used, hydrogen ions are more likely to penetrate into the molded product more efficiently in the acid treatment step described below, and the starting thickening polysaccharide is more likely to harden, so that a denser activated carbon tends to be obtained. As a result, an activated carbon with better crushing strength, heat resistance, and chemical resistance tends to be obtained.

[0089] [Acid treatment process] The activated carbon is preferably obtained through an acid treatment step in which the molded product obtained in the molding step is treated with an acid. The acid treatment method is not particularly limited, and known conditions can be adopted depending on the quality required for the activated carbon. By passing through the acid treatment step, the thickening polysaccharide in the molded product is hardened by hydrogen ions, so that the carbonization reaction of the thickening polysaccharide proceeds more appropriately in the heat treatment step described below, and a denser activated carbon tends to be obtained. As a result, an activated carbon having superior crush strength, heat resistance, and chemical resistance can be obtained.

[0090] The acid is not particularly limited, and any acid such as a mineral acid or an organic acid may be used. Examples of mineral acids include hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, and carbonic acid. Examples of organic acids include monobasic acids (e.g., acetic acid, lactic acid, and gluconic acid), dibasic acids (e.g., maleic acid, and fumaric acid), and polybasic acids (e.g., tartaric acid). These acids may be used alone or in combination of two or more in any ratio depending on the required specifications.

[0091] The acid is preferably a mineral acid, more preferably hydrochloric acid, which tends to give an activated carbon having superior crushing strength, heat resistance, and chemical resistance because it is easily permeated into the molded product and can more rapidly induce hardening of the thickening polysaccharide.

[0092] The amount of the acid used is preferably 1 to 20 times by mass relative to the amount of the molded product, and more preferably 5 to 15 times by mass. When the amount of the acid used is within the above range, the acid is more likely to penetrate into the molded product and the thickening polysaccharide can be hardened more quickly, which tends to result in activated carbon having superior crushing strength, heat resistance, and chemical resistance.

[0093] The acid treatment method is not particularly limited, and known conditions can be adopted depending on the quality required for the activated carbon. Examples of such methods include a method of immersing the molded product in acid and a method of spraying acid on the molded product.

[0094] The acid treatment temperature is usually about 20° C. or more and 70° C. or less. The acid treatment time depends on the acid treatment temperature, but in consideration of sufficient acid treatment and productivity, it is preferably about 1 minute or more and 20 hours or less, and more preferably about 5 minutes or more and 18 hours or less.

[0095] [Drying process] The activated carbon is preferably obtained through a drying step in which the acid-treated molded product obtained in the acid treatment step is dried.

[0096] The drying method is not particularly limited, and known drying methods such as natural drying, heat drying, and hot air drying can be used. As the drying method, a method of heating and / or reducing pressure is preferable. As the method of drying by heating, a method of drying by hot air is preferable because it is possible to dry stably without unevenness in drying. As for the drying conditions, it is preferable to dry the molded product until the moisture content is 20% by mass or less, and more preferably until the moisture content is 10% by mass or less.

[0097] Examples of the heating method include a heating method using a stationary constant temperature dryer, a stationary hot air dryer, a vacuum dryer, a rotary evaporator, a mixed dryer such as a conical dryer or a Nauter dryer, etc. The heating temperature may be any temperature at which the molded product hardens but does not melt, and is preferably, for example, 40°C or higher and 900°C or lower. The heating temperature may be 300°C or lower. The heating method may also be a method in which the heating temperature is increased stepwise from room temperature (25°C) to the above heating temperature.

[0098] The pressure reducing method may be, for example, a pressure reducing method using an oil pump, an oilless pump, an aspirator, etc. The pressure in the pressure reducing method is usually 0.00001 MPa or more and 0.05 MPa or less.

[0099] The drying time depends on the drying temperature, but is usually about 1 minute to 20 hours.

[0100] [Heat treatment process] The activated carbon is preferably obtained through a step of heat-treating the acid-treated molded product obtained in the acid treatment step. In addition, when a drying step is performed, the activated carbon is preferably obtained through a step of heat-treating the dried product obtained in the drying step.

[0101] By passing through the heat treatment step, the carbonization reaction of the water-soluble polymer and the thickening polysaccharide proceeds sufficiently, the raw powdered activated carbon particles can be more firmly bound, and the gasification of the water-soluble polymer and the thickening polysaccharide proceeds less easily, so that activated carbon having superior crushing strength, heat resistance, and chemical resistance can be obtained.

[0102] The heat treatment step is a step for carbonizing the thickening polysaccharide and the water-soluble polymer, and a known heat treatment method can be used depending on the quality required for the activated carbon. For example, an electric furnace such as a box-type heat treatment furnace can be used as the heat treatment method.

[0103] The heat treatment temperature is preferably such that the thickening polysaccharide and the water-soluble polymer are carbonized and the ratio of carbon in the entire activated carbon exceeds 90% by mass relative to 100% by mass of the activated carbon. The heat treatment temperature is more preferably 400°C or higher and 1000°C or lower, and even more preferably 450°C or higher and 950°C or lower. When the heat treatment temperature is within the above range, the carbonization reaction of the water-soluble polymer and the thickening polysaccharide proceeds more sufficiently, the raw powdered activated carbon particles can be more firmly bound, and the gasification of the water-soluble polymer and the thickening polysaccharide tends to proceed less easily. As a result, activated carbon with better crushing strength, heat resistance, and chemical resistance tends to be obtained.

[0104] The heat treatment time is preferably 10 minutes or more and 4 hours or less, more preferably 30 minutes or more and 2 hours or less. When the heat treatment temperature is within the above range, the carbonization reaction of the water-soluble polymer and the thickening polysaccharide proceeds more sufficiently, the raw powdered activated carbon particles can be further firmly bonded, and excessive gasification of the water-soluble polymer and the thickening polysaccharide tends to be less likely to proceed. As a result, activated carbon with even better crushing strength, heat resistance, and chemical resistance tends to be obtained.

[0105] The heat treatment atmosphere may be air or nitrogen, but is preferably performed under a nitrogen stream, since this tends to result in activated carbon having superior crushing strength, heat resistance, and chemical resistance.

[0106] [Activation Treatment Step] The activated carbon is preferably obtained by subjecting the molded product obtained in the molding process to an activation treatment. When the activation treatment is performed through a drying process, the activated carbon is preferably obtained by subjecting the dried product obtained in the drying process to an activation treatment. For the drying process, the above-mentioned drying process may be referred to.

[0107] The activation treatment improves the performance of the activated carbon and allows the carbonization reaction of the water-soluble polymer to proceed sufficiently, so that the powdered carbon particles of the raw material can be more firmly bound together, resulting in activated carbon with superior crushing strength, heat resistance, and chemical resistance.

[0108] The activation process is a process for forming pores in the powdered activated carbon or powdered carbon and carbonizing the water-soluble polymer, and a known activation process can be used depending on the quality required for the activated carbon. Examples of such activation processes include a method using a rotary kiln or a fluidized furnace.

[0109] The activation temperature is preferably such that pores are provided in the powdered activated carbon or powdered carbon and the water-soluble polymer is carbonized. The activation temperature is more preferably 500°C or more and 1000°C or less, and even more preferably 770°C or more and 970°C or less. When the activation temperature is within the above range, pores are formed in the powdered activated carbon or powdered carbon, the carbonization reaction of the water-soluble polymer proceeds more sufficiently, and the raw powdered activated carbon or powdered carbon particles tend to be more firmly bound. As a result, activated carbon with better crushing strength, heat resistance, and chemical resistance tends to be obtained. The activation treatment may be performed while gradually increasing the activation temperature from room temperature (25°C) to the above activation temperature.

[0110] The activation treatment time is preferably 10 minutes to 24 hours, more preferably 30 minutes to 12 hours. When the activation treatment time is within the above range, pores are formed in the powdered activated carbon or powdered carbon, and the carbonization reaction of the water-soluble polymer proceeds more sufficiently, tending to more firmly bind the raw powdered activated carbon or powdered carbon particles. As a result, activated carbon with even better crushing strength, heat resistance, and chemical resistance tends to be obtained.

[0111] The atmosphere for the activation treatment is preferably an atmosphere containing water vapor or carbon dioxide. For example, a water vapor stream is preferred because this tends to result in activated carbon having superior crushing strength, heat resistance, and chemical resistance.

[0112] The activated carbon thus obtained may be used as it is, or may be subjected to the following steps according to the quality required as an adsorbent in a column or the like: adjusting the particle size by crushing, grinding, and classification; increasing the purity by additional washing, for example, with water, an organic solvent, an aqueous acid solution, or an aqueous alkali solution; and imparting durability and adjusting the structure by additional heat treatment, to obtain activated carbon.

[0113] [Activated carbon manufacturing method] Examples of the method for producing activated carbon in this embodiment include a method in which powdered activated carbon, thickening polysaccharide, and water-soluble polymer are first blended and mixed in predetermined amounts in solid form such as powder, and water is added to the mixture, stirred, molded, and treated with acid without drying; and a method in which powdered activated carbon, thickening polysaccharide, water-soluble polymer, and water are each added in predetermined amounts, mixed and stirred, molded, and treated with acid without drying. When molding, an acid for acid treatment may be added, or the molded product may be contacted with acid without drying after it is obtained. The thickening polysaccharide and the water-soluble polymer are then carbonized by a high-temperature heat treatment to obtain activated carbon. The acid-treated molded product may be dried before the heat treatment, or may be directly heat-treated without drying.

[0114] Another method for producing the activated carbon of this embodiment is, for example, to first mix and mix a predetermined amount of the powdered activated material or powdered carbon and the water-soluble polymer in a solid form such as powder, add water to the mixture, stir, and mold it. Then, to form pores in the powdered activated carbon or powdered carbon, the water-soluble polymer is carbonized by performing an activation treatment at a high temperature, thereby obtaining activated carbon. During the activation treatment, a molded product may be obtained, and then the molded product may be dried to perform the activation treatment.

[0115] The method for producing activated carbon preferably includes a step of obtaining activated carbon that satisfies the above requirements (1) to (3), more preferably includes a step of obtaining activated carbon that satisfies the above requirements (1) to (3) and at least one of the above requirements selected from the group consisting of (4) to (6), more preferably includes a step of obtaining activated carbon that satisfies the above requirements (1) to (3) and at least two of the above requirements selected from the group consisting of (4) to (6), and even more preferably includes a step of obtaining activated carbon that satisfies all of the above requirements (1) to (6).The method for producing activated carbon more preferably includes a kneading step of kneading powdered activated carbon, a thickening polysaccharide, a water-soluble polymer, and water, a molding step of molding the kneaded mixture obtained in the kneading step, an acid treatment step of acid-treating the molded product obtained in the molding step, and a step of heat-treating the acid-treated molded product obtained in the acid treatment step. The method for producing activated carbon more preferably includes a kneading step of kneading powdered activated carbon, a thickening polysaccharide, a water-soluble polymer, and water, a molding step of molding the mixture obtained in the kneading step, an acid treatment step of acid-treating the molded product obtained in the molding step, a drying step of drying the acid-treated molded product obtained in the acid treatment step, and a heat treatment step of the dried product obtained in the drying step.The method for producing activated carbon more preferably includes a kneading step of kneading powdered activated carbon or powdered carbon, a water-soluble polymer, and water, a molding step of molding the mixture obtained in the kneading step, and an activation treatment step of activating the molded product obtained in the molding step. The method for producing activated carbon preferably includes a kneading step of kneading powdered activated carbon or powdered carbon with a water-soluble polymer and water, a molding step of molding the mixture obtained in the kneading step, a drying step of drying the molded product obtained in the molding step, and an activation treatment step of activating the dried product obtained in the drying step. According to such specific steps, it is possible to more preferably obtain activated carbon that satisfies the above requirements (1) to (3), preferably satisfies the above requirements (1) to (3) and at least one requirement selected from the group consisting of (4) to (6), more preferably satisfies the above requirements (1) to (3) and at least two requirements selected from the group consisting of (4) to (6), and even more preferably satisfies all of the above requirements (1) to (6).Therefore, activated carbon having superior crushing strength, heat resistance, and chemical resistance can be more preferably obtained.

[0116] The above requirements (1) to (6) for the activated carbon and the details of each step in the method for producing the activated carbon, including the drying step, are as described above.

[0117] The production method of this embodiment may include, after the acid treatment step, a step of adjusting the particle size by crushing, grinding, and classification by a known method, a step of increasing the purification level by additional washing using, for example, water, an organic solvent, an aqueous acid solution, and an aqueous alkali solution, a step of imparting durability by additional heat treatment, and a step of adjusting the structure by additional heat treatment. By including these steps, the production method of this embodiment can more preferably obtain activated carbon having superior crushing strength, heat resistance, and chemical resistance.

[0118] [Application] The activated carbon of the present embodiment can be suitably used in various applications requiring crushing strength, heat resistance, and chemical resistance. Examples of such applications include water purifiers, wastewater treatment, waste oil treatment, oil and fat refining, air purifiers, gas removal, and catalysts and their carriers. Activated carbon can be used stably for a long period of time and is very unlikely to disintegrate. Therefore, activated carbon can be used stably for a long period of time even when exposed to, for example, acids, alkalis, and organic solvents, and even under high temperature conditions.

[0119] More specifically, activated carbon is suitable for the following applications: (1) Water purifier: household water purifier elements; industrial water purifier elements. (2) Wastewater treatment: wastewater and effluent containing organic chlorines such as trichloroethane; circulating water treatment from aquariums and land-based aquaculture farms; pig wastewater with a high organic nitrogen content; wastewater containing heavy metals such as lead, hexavalent chromium, nickel, mercury, zinc, cadmium, and selenium; wastewater and effluent from dairy manufacturing plants, fishery processing plants, and slaughterhouses with a high water-soluble protein content; for example, wastewater from rivers, lakes, and factories containing P (phosphorus), S (sulfur), and N (nitrogen), wastewater from pulp factories and effluent, wastewater discharged from photographic development, wastewater from car washes containing a mixture of wax and detergent, industrial wastewater and agricultural wastewater discharged from factories and businesses containing various nitrogen compounds including organic alkalis such as tetramethylammonium hydroxide, and various difficult-to-decompose substances; contaminated groundwater, leachate from waste disposal sites, industrial wastewater containing chlorinated organic solvents, and wastewater containing chlorinated volatile organic compound (VOC) solvents, etc. (3) Waste oil treatment: Wastewater, waste liquid, and waste food containing vegetable oils (e.g., rapeseed oil, sesame oil, soybean oil, corn oil, palm oil, almond oil, and peanut oil), animal oils (e.g., butter and lard), and processed oils (e.g., margarine and sulfur), such as oils and lard, discharged from ordinary households, commercial kitchens, and buildings, and from sewage and wastewater treatment facilities of public utilities. (4) Fat and oil refining: vegetable oils, animal oils, processed oils, and lards. (5) Air purifiers: household air filters and industrial air filters. (6) Gas adsorption: pollutants such as dioxins, various organic solvents, halogen-containing organic solvents, sulfur-containing organic solvents, sulfur-containing compounds, and nitrogen-containing compounds. (7) Catalysts and their supports: oxidation catalysts using activated carbon, catalysts supporting fine metal particles such as nickel or palladium, catalysts supporting metal oxides such as copper oxide or zinc oxide, and catalysts supporting metal salts such as copper chloride or zinc acetate.

[0120] [Apparatus and removal method] The device of the present embodiment includes activated carbon, and the removal method of the present embodiment includes a step of removing the substance to be removed from a composition containing the substance, using the device of the present embodiment.

[0121] The function of activated carbon is utilized by an apparatus containing it. The apparatus is preferably a treatment apparatus. In this specification, the term "treatment apparatus" is not particularly limited as long as it is an apparatus that can remove or treat substances to be removed contained in a composition that is a treatment target such as wastewater, waste liquid, and oil, using the activated carbon of this embodiment. Examples of such treatment apparatus include apparatuses that contain filters, columns, tanks or baths, tubes, cartridges, cylinders, and sheets containing activated carbon (hereinafter also simply referred to as "filters, etc. containing activated carbon"), and filtration apparatuses.

[0122] The substance to be removed is not particularly limited, but may be, for example, at least one selected from the group consisting of impurities, pollutants, residual chlorine, volatile organic compounds (VOCs), and colored components.

[0123] Filtration devices include, for example, cartridge-type filters containing activated carbon, membrane treatment devices, and ultrafiltration membrane devices.

[0124] The treatment device may be equipped with other adsorption filters in addition to the activated carbon-containing filter, etc. Examples of such other adsorption filters include metal filters made of stainless steel, aluminum, bronze, copper, titanium, nickel, etc.; and resin filters made of polypropylene, polyvinyl chloride, polyvinylidene chloride, polyethylene, polyamide, fluorine-based resin, etc.

[0125] Additionally, the treatment equipment may be of the batch or continuous type, and activated carbon may be used in either mode. EXAMPLES

[0126] EXAMPLES The present invention will be explained in more detail below by showing examples and comparative examples, but the present invention is not limited to these examples in any way.

[0127] Example 1 The raw material wood flour was activated with zinc chloride, washed and dried. Then, the powder was sieved to obtain a powder with an average particle size (D50) of 30 μm, and the powder remaining under the sieve was collected. The collected powder was dispersed in distilled water and filtered to obtain an aqueous solution of a slurry containing 25% by mass of powdered activated carbon with an average particle size (D50) of 30 μm. 800 g of the aqueous solution of this slurry, 60 g of sodium alginate (manufactured by Wako Pure Chemical Industries) as a thickening polysaccharide, and 140 g of sodium lignin sulfonate (Borresperse NA (trade name) manufactured by Borreguard) as a water-soluble polymer were put into a mixer (Henschel mixer manufactured by Universe Co., Ltd.) and kneaded at room temperature for 10 minutes to obtain a kneaded product. The kneaded product was put into an extrusion granulator (Universe Co., Ltd., V-20 model (trade name)) and molded into pellets with a diameter of about 5 mm and a longitudinal length of about 3 mm to 5 mm, thereby obtaining pellets as molded products. The obtained pellets were not dried, but were immersed in 10 times the mass of 5% hydrochloric acid at room temperature (25°C) for 12 hours for acid treatment. The obtained acid-treated pellets were then heated at 140°C for 3 hours in a constant temperature dryer (Yamato Scientific Co., Ltd., DVS402 (trade name)) and dried. The obtained dried pellets were placed in a box-type heat treatment furnace (electric furnace, JTEKT Thermosystems Co., Ltd., KBF848N2 (trade name)) and heated from room temperature to 500°C over 1 hour under a nitrogen stream, and then heat-treated at 500°C for 1 hour to obtain activated carbon 1.

[0128] Example 2 Activated carbon 2 was obtained in the same manner as in Example 1, except that the material was molded into pellets using a disc pelletizer (F-5 model (product name) manufactured by Dalton Co., Ltd.) instead of an extrusion granulator (V-20 model (product name) manufactured by Universe Co., Ltd.).

[0129] Example 3 The raw material wood flour was activated with zinc chloride, washed and dried. Then, it was classified so that the average particle diameter (D50) was 40 μm, and powdered activated carbon was obtained. 500 g of this powdered activated carbon, 60 g of sodium alginate (manufactured by Wako Pure Chemical Industries) as a thickening polysaccharide, 150 g of sodium lignin sulfonate (Borresperse NA (trade name) manufactured by Borreguard) as a water-soluble polymer, and 600 g of water were put into a mixer (Henschel mixer manufactured by Universe Co., Ltd.) and kneaded at room temperature for 10 minutes to obtain a kneaded product. This kneaded product was put into a disk pelletizer (F-5 type (trade name) manufactured by Dalton Co., Ltd.) and molded into a pellet shape with a diameter length of about 5 mm and a longitudinal length of about 3 mm to 5 mm, to obtain a pellet as a molded body. The obtained pellets were not dried, but were immersed in 10 times the amount of 5% by mass hydrochloric acid for 12 hours at room temperature (25°C) for acid treatment. The acid-treated pellets were then heated at 140°C for 3 hours in a constant temperature dryer (DVS402 (trade name) manufactured by Yamato Scientific Co., Ltd.) and dried. The dried pellets were placed in a box-type heat treatment furnace (electric furnace, KBF848N2 (trade name) manufactured by JTEKT Thermo Systems Co., Ltd.) and heated from room temperature to 900°C over 1 hour under a nitrogen stream, and then heat-treated at 900°C for 1 hour to obtain activated carbon 3.

[0130] Example 4 Coconut shells from the Philippines were carbonized at a temperature of 600°C for about 2 hours, and pulverized to an average particle size of 20 μm to 80 μm to obtain powdered carbon. Then, 1000 g of the obtained powder, 260 g of sodium lignin sulfonate (Borresperse NA (trade name) manufactured by Borreguard) as a water-soluble polymer, and 150 g of water were put into a mixer (High-speed mixer DH-5 (trade name) manufactured by Universe Co., Ltd.) and kneaded at room temperature for 10 minutes to obtain a kneaded product. Then, the kneaded product was put into an extrusion molding machine (Disc Pelleter (trade name) manufactured by Fuji Paudal Co., Ltd.) with a hole diameter of 3.0 mm and extrusion molding was performed to obtain a pellet-shaped molded product with a diameter length of 2.0 mm to 3.0 mm and a longitudinal length of about 5.0 mm to 10.0 mm. The obtained molded product was placed in a rotary kiln. Thereafter, while excluding air from the rotary kiln, the temperature was raised from room temperature to 800°C at a rate of 5°C / min until it reached 800°C, after which it was dried for 5 minutes. Subsequently, in the rotary kiln, the dried product was brought into contact with water vapor under a water vapor stream and subjected to activation treatment at 900°C for 80 minutes to obtain activated carbon 4.

[0131] Example 5 Activated carbon 5 was obtained in the same manner as in Example 4, except that the drying treatment was performed while increasing the temperature from room temperature to 800°C at a rate of 10°C / min instead of from room temperature to 800°C at a rate of 5°C / min.

[0132] Example 6 Activated carbon 6 was obtained in the same manner as in Example 5, except that 23 g of sodium carbonate (manufactured by Wako Pure Chemical Industries, Ltd.) was further added in the kneading step.

[0133] Comparative Example 1 Activated carbon 7 was obtained in the same manner as in Example 2, except that the molded pellets were dried without being immersed in 5% by mass hydrochloric acid for 12 hours.

[0134] Comparative Example 2 The dried pellets obtained in the same manner as in Example 2 were obtained as activated carbon 8. That is, activated carbon 8 was activated carbon obtained without being heat-treated in a box-type heat treatment furnace.

[0135] Comparative Example 3 The dried pellets obtained in the same manner as in Example 2 were placed in a box-type heat treatment furnace (electric furnace, KBF848N2 (product name) manufactured by JTEKT Thermo Systems Corp.) and heated from room temperature to 200°C over 1 hour under a nitrogen stream, and then heat-treated at 200°C for 1 hour to obtain activated carbon 9. That is, activated carbon 9 was obtained in the same manner as in Example 2, except that the heat treatment conditions in the box-type heat treatment furnace were changed from 500°C to 200°C.

[0136] Comparative Example 4 Activated carbon 10 was obtained in the same manner as in Example 2, except that 60 g of methylcellulose (manufactured by Wako Pure Chemical Industries, Ltd.) was used instead of 60 g of sodium alginate (manufactured by Wako Pure Chemical Industries, Ltd.).

[0137] Comparative Example 5 The dried pellets obtained in the same manner as in Comparative Example 4 were obtained as activated carbon 11. That is, activated carbon 11 was activated carbon obtained without being heat-treated in a box-type heat treatment furnace.

[0138] Comparative Example 6 Activated carbon 12 was obtained in the same manner as in Example 2, except that 140 g of cellulose powder (manufactured by Wako Pure Chemical Industries, Ltd.) was used instead of 140 g of sodium lignin sulfonate (Borresperse NA (trade name) manufactured by Borreguard).

[0139] Comparative Example 7 Activated carbon 13 was obtained in the same manner as in Example 2, except that 20 g of Kibushi clay (manufactured by Kyoritsu Material Co., Ltd.) was used instead of 140 g of sodium lignin sulfonate (Borresperse NA (trade name) manufactured by Borreguard).

[0140] Comparative Example 8 The dried pellets obtained in the same manner as in Comparative Example 7 were placed in a box-type heat treatment furnace (electric furnace, KBF848N2 (product name) manufactured by JTEKT Thermo Systems Corp.) and heated from room temperature to 200°C over one hour under a nitrogen stream, and then heat-treated at 200°C for one hour to obtain activated carbon 14. That is, activated carbon 14 was obtained in the same manner as in Comparative Example 7, except that the heat treatment conditions in the box-type heat treatment furnace were changed from 500°C to 200°C.

[0141] [Evaluation method] (1) Crushing strength The crushing strength (N) of the activated carbon obtained in the examples and comparative examples was measured. Specifically, a Kiya hardness tester (Kiya hardness tester 043019-A (product number) manufactured by Fujiwara Seisakusho Co., Ltd.) was used to gradually apply force perpendicular to the axial direction of the cylindrical activated carbon, and the force applied when the activated carbon collapsed was taken as the crushing strength (N). This crushing strength measurement was performed on 32 separate pieces of activated carbon, and the average value was calculated from the crushing strength values, and this value was taken as the crushing strength (N) of the activated carbon.

[0142] (2) Total pore volume The total pore volume (mL / g) having a diameter of 30 nm or less of the activated carbon obtained in the examples and comparative examples was measured using a specific surface area / pore distribution measuring device (BELSORP (registered trademark)-miniII (product name) manufactured by Microtrack-Bell). Specifically, using nitrogen as the adsorption gas, the equilibrium adsorption pressure and the gas adsorption amount were measured at each measurement point at -196°C to obtain an adsorption isotherm. Analysis software (BELMaster (trademark) manufactured by Microtrack-Bell) was used for the analysis.

[0143] (3) Mass loss rate up to 500°C, and mass loss rate from 500°C to 800°C Using the activated carbon obtained in the examples and comparative examples, the mass reduction rate (mass%) up to 500°C and the mass reduction rate (mass%) at 500°C or more and 800°C or less were measured. Specifically, first, using a constant temperature dryer (DVS402 (trade name) manufactured by Yamato Scientific Co., Ltd.), the activated carbon obtained in the examples and comparative examples was kept at 115°C for 3 hours under a nitrogen atmosphere as an inert gas, and dried to obtain dried activated carbon, and its mass was measured. Then, using a thermogravimetric differential thermal analyzer (sample observation differential scanning calorimeter, Thermo Plus EVO2 (trade name) manufactured by Rigaku Corporation), the dried activated carbon was heated from room temperature to 800°C at 10 (°C / min) under a nitrogen atmosphere as an inert gas, to measure the mass at 500°C and the mass at 800°C. The mass reduction rate up to 500°C was calculated as the reduction ratio relative to the dry mass of the dried activated carbon, that is, using the following calculation formula (1). The mass reduction rate at 500° C. or higher and 800° C. or lower was calculated as the reduction rate relative to the dry mass of the dried activated carbon, that is, using the following calculation formula (2). Mass reduction rate up to 500°C (mass%) = 100 × {(mass of dry activated carbon) - (mass at 500°C)} / (mass of dry activated carbon) ... (1) Mass reduction rate (mass%) from 500°C to 800°C = 100 × {(mass at 500°C) - (mass at 800°C)} / (mass of dried activated carbon) ... (2)

[0144] (4) Sulfur atom content The content (mass%) of sulfur atoms was measured using the activated carbon obtained in the examples and comparative examples. Specifically, first, the activated carbon obtained in the examples and comparative examples was dried by holding it at 115°C for 3 hours under a nitrogen atmosphere as an inert gas using a constant temperature dryer (DVS402 (trade name) manufactured by Yamato Scientific Co., Ltd.) to obtain dried activated carbon, and its mass was measured. Then, the dried activated carbon was burned at 950°C in a quartz tube under air, and the generated gas was absorbed in 5.0% by mass hydrogen peroxide solution, and the mass of the hydrogen peroxide solution after absorption was measured. Then, the sulfate ion concentration in the hydrogen peroxide solution after absorption was measured using an ion chromatograph (ICS-2100 / AS-AP / CMS7.2 (trade name) manufactured by Thermo Fisher Scientific Co., Ltd.). The content (mass%) of sulfur atoms in the activated carbon was calculated as a ratio to the dry mass of the dried activated carbon, that is, using the following calculation formula (3). Sulfur atom content (mass%) = 100 × {(sulfate ion concentration) × (mass of hydrogen peroxide solution after absorption) × 32.0 / 98.1} / (mass of dry activated carbon) ... (3)

[0145] (5) Specific surface area The specific surface area (m 2 Specifically, the specific surface area (m2) was determined by the BET method from the N2 adsorption isotherm at -196°C. 2 The specific surface area (P / g) was determined as follows. That is, first, the activated carbon obtained in the examples and comparative examples was heated at 250°C for 3 hours under reduced pressure (vacuum degree: 0.1 kPa or less) using a specific surface area / pore distribution measuring device (BELSORP (registered trademark)-mini (product name) manufactured by Microtrack-Bel Co., Ltd.), and then the nitrogen adsorption isotherm of the activated carbon at -196°C was measured. Using the obtained nitrogen adsorption isotherm, a straight line was calculated from the obtained curve by BET analysis in the region of relative pressure P / P0 = 0.05 or more and 0.20 or less by the multipoint method, and the specific surface area was calculated from this straight line.

[0146] (6) Ignition residue The activated carbon obtained in the Examples and Comparative Examples was used to measure the ignition residue (mass%) when incinerated in air at 850° C. Specifically, a pre-weighed amount of activated carbon was placed in a crucible and incinerated in air at 850° C. The ignition residue was calculated as the ratio of the mass of the residue after incineration to the mass of the activated carbon.

[0147] (7) Chemical resistance Chemical resistance was evaluated using the activated carbon obtained in the examples and comparative examples. Specifically, the activated carbon was immersed in each of the chemicals of 1 mol / L hydrochloric acid, 1 mol / L aqueous sodium hydroxide solution, and ethanol for 24 hours. After that, using a constant temperature dryer (DVS402 (trade name) manufactured by Yamato Scientific Co., Ltd.), each of the immersed activated carbons was kept at 115°C for 3 hours and dried. The dried activated carbons were used to measure the respective crushing strengths (N) in the same manner as in the above (1) Crushing Strength Measurement Method.

[0148] The results are shown in Table 1.

[0149] [Table 1]

Claims

1. Activated carbon that satisfies the following requirements (1) to (3). (1) The crushing strength is 5.0 N or more. (2) The total volume of pores having a diameter of 30 nm or less is 0.3 mL / g or more and 1.2 mL / g or less. (3) The mass loss rate up to 500° C. and the mass loss rate at 500° C. or higher and 800° C. or lower, as measured using a thermogravimetric differential thermal analyzer, are 5.0% by mass or less and 1.0% by mass or more and 25% by mass or less, respectively, based on the dry mass of the activated carbon when the activated carbon is maintained at 115° C. for 3 hours in an inert gas atmosphere.

2. The activated carbon according to claim 1, further satisfying at least one requirement selected from the group consisting of the following (4) to (6): (4) The content of sulfur atoms is 0.01% by mass or more and 5.0% by mass or less. (5) N at -196°C 2 The specific surface area calculated by the BET method from the adsorption isotherm is 500 m 2 / g or more 1300m 2 / g or less. (6) The ignition residue when incinerated in air at 850° C. is 5.0 mass % or less.

3. The activated carbon according to claim 2, which satisfies all of the requirements (4) to (6).

4. An apparatus comprising the activated carbon according to any one of claims 1 to 3.

5. A method for removing at least one substance selected from the group consisting of impurities, pollutants, residual chlorine, volatile organic compounds (VOCs), and coloring components from a composition containing the substance using the device described in claim 4.

6. A method for producing activated carbon, comprising the steps of obtaining activated carbon that satisfies the following requirements (1) to (3): (1) The crushing strength is 5.0 N or more. (2) The total volume of pores having a diameter of 30 nm or less is 0.3 mL / g or more and 1.2 mL / g or less. (3) The mass loss rate up to 500° C. and the mass loss rate at 500° C. or higher and 800° C. or lower, as measured using a thermogravimetric differential thermal analyzer, are 5.0% by mass or less and 1.0% by mass or more and 25% by mass or less, respectively, based on the dry mass of the activated carbon when the activated carbon is maintained at 115° C. for 3 hours in an inert gas atmosphere.

7. A kneading step of kneading powdered activated carbon, a thickening polysaccharide, a water-soluble polymer, and water; A molding step of molding the kneaded product obtained in the kneading step; an acid treatment step of treating the molded product obtained in the molding step with acid; and a step of heat-treating the acid-treated molded product obtained in the acid treatment step.

8. A kneading step of kneading powdered activated carbon, a thickening polysaccharide, a water-soluble polymer, and water; A molding step of molding the kneaded product obtained in the kneading step; an acid treatment step of treating the molded product obtained in the molding step with acid; a drying step for drying the acid-treated molded product obtained in the acid treatment step; The method for producing activated carbon according to claim 6, further comprising a step of heat-treating the dried product obtained in the drying step.

9. A kneading step of kneading powdered activated carbon or powdered carbon, a water-soluble polymer, and water; A molding step of molding the kneaded product obtained in the kneading step; The method for producing activated carbon according to claim 6, further comprising a step of subjecting the molded product obtained in the molding step to an activation treatment.

10. A kneading step of kneading powdered activated carbon or powdered carbon, a water-soluble polymer, and water; A molding step of molding the kneaded product obtained in the kneading step; A drying step of drying the molded product obtained in the molding step; The method for producing activated carbon according to claim 6, further comprising a step of subjecting the dried product obtained in the drying step to an activation treatment.

11. The method for producing activated carbon according to any one of claims 6 to 10, wherein the activated carbon further satisfies at least one requirement selected from the group consisting of the following (4) to (6): (4) The content of sulfur atoms is 0.01% by mass or more and 5.0% by mass or less. (5) N at -196°C 2 The specific surface area calculated by the BET method from the adsorption isotherm is 500 m 2 / g or more 1300m 2 / g or less. (6) The ignition residue when incinerated in air at 850° C. is 5.0 mass % or less.

12. The method for producing activated carbon according to claim 11, wherein the activated carbon satisfies all of the requirements (1) to (6).

13. The method for producing activated carbon according to claim 7 or 8, wherein the thickening polysaccharide comprises at least one selected from the group consisting of alginic acid and its salts, and carboxymethylcellulose and its salts.

14. The method for producing activated carbon according to claim 7 or 8, wherein the thickening polysaccharide is mixed in an amount of 5 parts by mass or more and 30 parts by mass or less with respect to 100 parts by mass of the water.

15. The method for producing activated carbon according to claim 7 or 8, wherein the thickening polysaccharide comprises sodium alginate.

16. The method for producing activated carbon according to any one of claims 7 to 10, wherein the water-soluble polymer comprises at least one selected from the group consisting of lignin sulfonic acid and salts thereof.

17. The method for producing activated carbon according to any one of claims 7 to 10, wherein the amount of the water-soluble polymer is 10 parts by mass or more and 100 parts by mass or less with respect to 100 parts by mass of the powdered activated carbon or the powdered carbon.

18. The method for producing activated carbon according to any one of claims 7 to 10, wherein the water-soluble polymer comprises sodium lignin sulfonate.

Citation Information

Patent Citations

  • Activated carbon molded product and method for manufacturing the same

    JP2007269555A

  • Adsorbent molded articles and their use

    JP2012508645A

  • Resin bonded sorbent

    JP2013237854A

  • Active carbon and water purifier using the same

    JP2017136589A

Cited By

  • Carbon molecular sieve and method for manufacturing same, and gas separation device

    WO2026205198A1