Optical fiber
The optical fiber design with a quartz-based core and varying germanium concentration addresses transmission loss and refraction profile challenges, enabling flexible optical control and reduced loss, meeting G.652 standards.
Patent Information
- Application Number
- JP2023044942
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-04
AI Technical Summary
Existing optical fibers face challenges in reducing transmission loss and controlling flexible refraction profiles, particularly those without alkali metal elements, and those with alkali metals, fluorine, and chlorine struggle with flexible optical property control.
An optical fiber design featuring a quartz-based core with varying germanium concentration along the radial position, combined with fluorine, alkali metals, and chlorine, to achieve a W-shaped refractive index profile, allowing for flexible optical characteristic design and reduced transmission loss.
The design enables flexible optical characteristic control while achieving transmission losses of 0.164 dB/km or less at 1550 nm, with a mode field diameter of 9.2 μm to 9.5 μm at 1310 nm, meeting G.652 standards.
Smart Images

Figure 2024134644000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to optical fibers. [Background technology]
[0002] Optical fibers for long-distance transmission are required to have various optical characteristics, such as chromatic dispersion characteristics, cutoff wavelength, mode field diameter, bending loss, etc. As such an optical fiber, for example, an optical fiber with germanium doped in the core portion is disclosed (Patent Document 1). In this optical fiber, the refraction profile is designed to satisfy the desired optical characteristics.
[0003] On the other hand, an optical fiber in which an alkali metal element such as potassium, fluorine, or chlorine is added to the core in order to reduce transmission loss has been disclosed (Patent Document 2). Such an optical fiber is very effective for long-distance transmission applications. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2014-142613 A [Patent Document 2] Special Publication No. 2007-504080 Summary of the Invention [Problem to be solved by the invention]
[0005] However, in the optical fiber of Patent Document 1, no alkali metal element is added to the core, and there is room for improvement in terms of reducing transmission loss. Also, in the optical fiber of Patent Document 2, it is difficult to control the refractive index profile flexibly and therefore the optical characteristics flexibly with only alkali metal elements, fluorine, and chlorine, and there is room for improvement in terms of designing the optical characteristics.
[0006] The present invention has been made in view of the above, and an object of the present invention is to provide an optical fiber that has reduced transmission loss and allows flexible design of optical characteristics. [Means for solving the problem]
[0007] In order to solve the above-mentioned problems and achieve the object, one aspect of the present invention is an optical fiber comprising: a core portion made of silica-based glass and having a center core; and a cladding portion made of silica-based glass having a refractive index lower than the maximum refractive index of the core portion and surrounding the outer periphery of the core portion, wherein the center core contains fluorine, an alkali metal element, chlorine, and germanium, and the germanium is distributed such that the germanium concentration varies depending on the radial position of the center core.
[0008] In the center core, the fluorine concentration may be 500 ppm or more and 10,000 ppm or less, the alkali metal concentration may be 10 ppm or more and 1,000 ppm or less, the chlorine concentration may be 15,000 ppm or less, and the germanium concentration may be 5,000 ppm or less.
[0009] In the center core, the germanium concentration may be higher in an outer periphery than in a radial center of the core.
[0010] In the center core, the radial distance from the center is r, the germanium concentration at the distance r is f(r), the minimum value of f(r) is minf(r), and the core radius of the center core is a, then the following equation (1) may be established.
number
[0011] The following formula (2) may hold:
number
[0012] The center core may contain germanium at a radial position where the relative refractive index difference Δ1 with respect to pure silica glass is a maximum value Δ1max.
[0013] The optical fiber may have a transmission loss of 0.164 dB / km or less at a wavelength of 1550 nm.
[0014] The optical fiber may have a transmission loss of 0.160 dB / km or less at a wavelength of 1550 nm.
[0015] The optical fiber may have a germanium concentration of 2500 ppm or less in the center core, and a transmission loss at a wavelength of 1550 nm of 0.154 dB / km or less.
[0016] The optical fiber may have a mode field diameter of 9.2 μm or more and 9.5 μm or less at a wavelength of 1310 nm.
[0017] The optical fiber may have a step or W-shaped refractive index profile.
[0018] The germanium may be distributed to form the refractive index profile according to a refractive index profile determined by the fluorine, the alkali metal element, and the chlorine.
[0019] The core portion is the center core, and the relative refractive index difference Δ1 of the center core with respect to pure silica glass is 0% or more and 0.15% or less, and the relative refractive index difference Δclad of the cladding portion with respect to pure silica glass is -0.3% or more and -0.15% or less, and if the core diameter of the center core is 2a, 2a may be 8.0 μm or more and 13.0 μm or less.
[0020] The core portion is composed of the center core and a depressed layer formed to surround the outer periphery of the center core and having a refractive index smaller than that of the cladding portion, wherein the relative refractive index difference Δ1 with respect to pure silica glass in the center core is 0% or more and 0.20% or less, and the relative refractive index difference Δclad with respect to pure silica glass in the cladding portion is -0.2% or less, and when the core diameter of the center core is 2a, 2a is 9.0 μm or more and 14.0 μm or less, and when the outer diameter of the depressed layer is 2b, b / a is 1.2 or more and 4.0 or less. Effect of the Invention
[0021] According to the present invention, it is possible to realize an optical fiber that has reduced transmission loss and allows flexible design of optical characteristics. [Brief description of the drawings]
[0022] [Figure 1] FIG. 1 is a schematic cross-sectional view of an optical fiber according to an embodiment, taken along a plane perpendicular to the longitudinal direction thereof. [Diagram 2] FIG. 2 is a schematic diagram of a refractive index profile of the optical fiber according to the embodiment. [Diagram 3] FIG. 3 is a schematic diagram showing an example of the relationship between the refractive index profile and the distribution of the dopant concentration of the optical fiber according to the embodiment. [Figure 4] FIG. 4 is a schematic diagram of another example of the refractive index profile of the center core. [Diagram 5] FIG. 5 is a schematic diagram of yet another example of the refractive index profile. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. Note that the present invention is not limited to the embodiment described below. In addition, in each drawing, the same or corresponding components are appropriately assigned the same reference numerals. In addition, in this specification, the cutoff wavelength or effective cutoff wavelength refers to the cable cutoff wavelength (λcc) defined in ITU-T G.650.1 of the International Telecommunications Union (ITU). In addition, other terms not specifically defined in this specification shall follow the definitions and measurement methods in G.650.1 and G.650.2.
[0024] (Embodiment) FIG. 1 is a schematic cross-sectional view of an optical fiber according to an embodiment taken along a plane perpendicular to the longitudinal direction. The optical fiber 1 is made of silica glass and includes a core 1a and a cladding 1b having a refractive index lower than the maximum refractive index of the core 1a and surrounding the outer periphery of the core 1a. The portion of the optical fiber 1 including the core 1a and the cladding 1b is a portion of the optical fiber made of glass, and may be referred to as a glass optical fiber. The optical fiber 1 also includes a coating layer 1c that surrounds the outer periphery of the cladding 1b. The coating layer 1c includes a primary layer 1ca that surrounds the outer periphery of the cladding 1b, and a secondary layer 1cb that surrounds the outer periphery of the primary layer 1ca. The optical fiber including the coating layer 1c may be referred to as an optical fiber core.
[0025] The core portion 1a is composed of a center core 1aa and a depressed layer 1ab that is formed so as to surround the outer periphery of the center core 1aa and has a refractive index smaller than that of the cladding portion 1b.
[0026] The optical fiber 1 has a refractive index profile as shown in Fig. 2, for example. Fig. 2 shows the refractive index profile in the radial direction from the center (core center) of the core portion 1a of the optical fiber 1. The refractive index profile is shown in terms of the relative refractive index difference with respect to pure silica glass. Here, pure silica glass refers to extremely high-purity silica glass that does not substantially contain dopants that change the refractive index and has a refractive index of approximately 1.444 at a wavelength of 1550 nm.
[0027] The refractive index profile of the optical fiber 1 is a so-called W-shaped refractive index profile. In FIG. 2, profile P11 shows the refractive index profile of the core 1a, and profile P12 shows the refractive index profile of the cladding 1b. In the core 1a, the center core 1aa has a core radius of a and a diameter (core diameter) of 2a. The depressed layer 1ab has an inner diameter of 2a and an outer diameter of 2b. The center core 1aa is the part of the core 1a that has the maximum average refractive index. The maximum relative refractive index difference of the center core 1aa with respect to the refractive index of pure silica glass is Δ1. The relative refractive index difference of the average refractive index of the depressed layer 1ab with respect to the refractive index of pure silica glass is Δ2. The relative refractive index difference of the average refractive index of the cladding 1b with respect to the refractive index of pure silica glass is Δclad.
[0028] Here, the refractive index profile of the center core 1aa of the core portion 1a may not only be a step type with a geometrically ideal shape, but may also have a shape with unevenness formed due to manufacturing characteristics at the top, or may have a shape with a skirt from the top. In this case, the refractive index of the region that is approximately flat at the top of the refractive index profile within the range of the core diameter 2a of the core portion 1a in the manufacturing design is an index for determining Δ1. Even if the approximately flat region is thought to be divided into multiple places, or if a continuous change occurs and it is difficult to define the approximately flat region, it has been confirmed that it is possible to obtain characteristics close to the desired if at least any part of the core portion 1a other than the part where the refractive index changes suddenly toward the adjacent layer is within the range of a predetermined Δ1, and the difference between the maximum value and the minimum value Δ is within a certain value ±30%, and there is no particular problem.
[0029] The average refractive index of the depressed layer 1ab and the cladding portion 1b is the average value of the refractive index in the radial direction of the refractive index profile.
[0030] The constituent materials of the optical fiber 1 will be described. The center core 1aa of the core portion 1a is made of silica glass containing fluorine (F), an alkali metal element, chlorine (Cl), and germanium (Ge). The alkali metal element is, for example, potassium (K) or sodium (Na). Germanium is a dopant that increases the refractive index of the silica glass. Chlorine and alkali metal elements are dopants that increase the refractive index of the silica glass and decrease its viscosity. Fluorine is a dopant that decreases the refractive index of the silica glass. These dopants may be doped as compounds.
[0031] The depressed layer 1ab is made of silica glass containing at least fluorine, and the cladding portion 1b is made of silica glass containing at least fluorine.
[0032] In the refractive index profile shown in Figure 2, the refractive index level of the pure silica glass exists between the maximum and minimum values of the refractive index of the center core. To realize such a refractive index profile, the distribution of each dopant is adjusted so that a refractive index profile can be formed by doping with germanium when the refractive index of the silica glass is to be increased above that of pure silica glass, and by doping with fluorine when the refractive index of the silica glass is to be decreased below that of pure silica glass.
[0033] The primary layer 1ca and the secondary layer 1cb are made of resin. This resin is, for example, an ultraviolet curing resin. The ultraviolet curing resin is, for example, a mixture of various resin materials and additives, such as oligomers, diluting monomers, photopolymerization initiators, silane coupling agents, sensitizers, and lubricants. As the oligomer, conventionally known materials such as polyether urethane acrylate, epoxy acrylate, polyester acrylate, and silicone acrylate can be used. As the diluting monomer, conventionally known materials such as monofunctional monomers and polyfunctional monomers can be used. In addition, the additives are not limited to those described above, and conventionally known additives used for ultraviolet curing resins and the like can be widely used.
[0034] The dopants contained in the center core 1aa will be described in more detail. Fig. 3 is a schematic diagram showing an example of the relationship between the refractive index profile and the distribution of the dopant concentration of the optical fiber according to the embodiment. In Fig. 3, line L11 shows the refractive index profile of the center core 1aa, line L12 shows the refractive index profile of the depressed layer 1ab, and line L13 shows the refractive index profile of the cladding portion 1b. Line L2 shows the germanium concentration, line L3 shows the fluorine concentration, line L4 shows the alkali metal concentration, and line L5 shows the chlorine concentration. However, in Fig. 3, the refractive index profile is shown based on the average refractive index of the cladding portion 1b.
[0035] As shown in Fig. 3, germanium is distributed such that the germanium concentration varies depending on the radial position of the center core 1aa. In the center core 1aa, the germanium concentration is higher in the outer periphery than in the radial center of the core. In addition, germanium is contained in the center core 1aa at the radial position (position indicated by arrow A) where the relative refractive index difference Δ1 is the maximum value Δ1max.
[0036] Germanium has a larger change in refractive index relative to the doping concentration than chlorine or alkali metal elements. Therefore, by distributing germanium so that the germanium concentration varies depending on the radial position of the center core 1aa, it is easy to control the refractive index profile of the center core 1aa. As a result, the optical characteristics of the optical fiber 1 can be easily designed. For example, germanium may be distributed to form a desired refractive index profile according to the refractive index profile determined by fluorine, alkali metal elements, and chlorine.
[0037] In addition, by making the germanium concentration in the outer periphery of the center core 1aa higher than that in the radial core center, Rayleigh scattering in the core center can be further reduced, and the zero dispersion wavelength can be easily controlled to within the range of 1302 nm to 1312 nm, which is the short wavelength side of the G.652 standard, while keeping the cable cutoff wavelength below 1260 nm as specified in the ITU-T G.652 standard. Since the intensity of light propagating in the fundamental mode of the propagation modes of the optical fiber 1 is high at the core center, reducing Rayleigh scattering at the core center is effective for reducing transmission loss. In this way, the optical fiber 1 achieves reduced transmission loss and flexible design of optical characteristics.
[0038] In this case, it is preferable that the following formula (1) is satisfied, where r is the radial distance from the center of center core 1aa, f(r) is the germanium concentration at distance r, minf(r) is the minimum value of f(r), and a is the core radius of center core 1aa. When formula (1) is satisfied, it is preferable to make the germanium concentration higher in the outer periphery than the germanium concentration at the radial core center.
number
[0039] Furthermore, if formula (2) holds, it is more preferable to make the germanium concentration higher in the outer periphery than the germanium concentration in the center of the core in the radial direction.
number
[0040] In addition, since germanium is contained in the center core 1aa at the radial position (position indicated by arrow A in FIG. 3) where the relative refractive index difference Δ1 is the maximum value Δ1max, the value of Δ1max can be adjusted by the germanium concentration. As described above, germanium has a large change in refractive index with respect to its concentration, so a desired Δ1max can be achieved with a smaller concentration.
[0041] In the center core 1aa, for example, the fluorine concentration is 500 ppm or more and 10000 ppm or less, the alkali metal concentration is 10 ppm or more and 1000 ppm or less, the chlorine concentration is 500 ppm or more and 15000 ppm or less, and the germanium concentration is 500 ppm or more and 5000 ppm or less. Such concentrations are preferable in terms of low loss of the optical fiber 1 because they can obtain both effects of low transmission loss due to the decrease in viscosity of the center core 1aa caused by the alkali metal and chlorine, and low transmission loss due to the relatively low germanium concentration. Due to these effects, for example, the optical fiber 1 has a transmission loss of 0.164 dB / km or less at a wavelength of 1550 nm, and preferably 0.160 dB / km or less. In particular, in order to make the transmission loss at a wavelength of 1550 nm 0.164 dB / km or less, it is preferable that formula (1) or formula (2) is established. Furthermore, if the germanium concentration in the center core 1aa is 2500 ppm or less, the optical fiber 1 is likely to have a transmission loss of 0.154 dB / km or less at a wavelength of 1550 nm.
[0042] Also, the optical fiber 1 preferably has a mode field diameter of 9.2 μm or more and 9.5 μm or less at a wavelength of 1310 nm, for example, which allows the optical fiber 1 to achieve a relatively large mode field diameter range within the G.652B standard.
[0043] The preferred structural parameters of the optical fiber 1 are, for example, Δ1 is 0% or more and 0.20% or less, Δclad is -0.2% or less, 2a is 9.0 μm or more and 14.0 μm or less, and b / a is 1.2 or more and 4.0 or less. With these structural parameter values, an optical fiber equivalent to the ITU-T G.652.D standard or the ITU-T G.654.E standard can be realized with good manufacturability. In particular, in order to set the cable cutoff wavelength to 1260 nm or less as specified by the ITU-T G.652 standard, to set the mode field diameter to a relatively large value of 9.2 μm or more and 9.5 μm or less, and to set the transmission loss to 0.164 dB / km or less, it is preferable to set 0.25%≦|Δ1-Δclad|≦0.28% and 10 μm≦2a≦12 μm.
[0044] In the optical fiber 1 configured as above, the transmission loss is reduced and the optical characteristics can be flexibly designed.
[0045] (Another example of the refractive index profile of the center core) In the optical fiber according to the embodiment, the refractive index profile of the center core is not limited to that shown in Fig. 2. Fig. 4 is a schematic diagram of another example of the refractive index profile of the center core. In Fig. 4, the dashed line indicates the level of the refractive index of pure silica glass.
[0046] Fig. 4(a) is a refractive index profile in which the germanium concentration in the outer periphery is higher than the germanium concentration in the center of the core in the radial direction, similar to Figs. 2 and 3. Hereinafter, the refractive index profiles in Figs. 2 and 3 may be referred to as the refractive index profile of pattern A, and the refractive index profile in Fig. 4(a) may be referred to as the refractive index profile of pattern B. According to pattern B, similar to pattern A, it is possible to further reduce the Rayleigh scattering in the center of the core and further reduce the transmission loss, and it is easy to control the zero dispersion wavelength to the range of 1302 nm to 1312 nm, which is the short wavelength side of the G.652 standard, while keeping the cable cutoff wavelength below 1260 nm as specified in the ITU-T G.652 standard.
[0047] Figure 4(b) shows a refractive index profile (sometimes referred to as pattern C) in which the germanium concentration in the outer periphery is lower than the germanium concentration in the center of the core in the radial direction, unlike patterns A and B. With pattern C, for example, it is easy to control the zero dispersion wavelength to within the range of 1312 nm to 1322 nm, which is on the longer wavelength side of the G.652 standard, while keeping the cable cutoff wavelength below 1260 nm as specified in the ITU-T G.652 standard.
[0048] Figure 4(c) shows a refractive index profile (sometimes referred to as pattern D) in which the germanium concentration in the outer periphery is higher than the germanium concentration in the center of the core in the radial direction, similar to patterns A and B. According to pattern D, similar to patterns A and B, it is possible to further reduce Rayleigh scattering in the center of the core and thereby further reduce transmission loss, and it is easy to control the zero dispersion wavelength to within the range of 1302 nm to 1312 nm, which is on the short wavelength side of the G.652 standard, while keeping the cable cutoff wavelength below 1260 nm as specified in the ITU-T G.652 standard.
[0049] 4(d) shows a refractive index profile (sometimes referred to as pattern E) in which the germanium concentration in the outer periphery is lower than the germanium concentration in the center of the core in the radial direction, similar to pattern C. According to pattern D, for example, it is easy to control the zero dispersion wavelength to the range of 1312 nm to 1322 nm, which is on the longer wavelength side of the G.652 standard, while keeping the cable cutoff wavelength below 1260 nm as specified by the ITU-T G.652 standard.
[0050] Figure 4(e) shows a refractive index profile (sometimes referred to as pattern F) in which the germanium concentration in the outer periphery is higher than the germanium concentration in the center of the core in the radial direction, similar to patterns A, B, and D. Pattern F, like patterns A, B, and D, can further reduce Rayleigh scattering in the center of the core and further reduce transmission loss, and also makes it easy to control the zero dispersion wavelength to within the range of 1302 nm to 1312 nm, which is on the short wavelength side of the G.652 standard, while keeping the cable cutoff wavelength below 1260 nm as specified in the ITU-T G.652 standard.
[0051] In the optical fiber according to the embodiment, the center core contains fluorine, an alkali metal element, chlorine, and germanium, and the germanium is distributed such that the germanium concentration varies depending on the radial position of the center core, so that it is possible to realize various refractive index profiles such as patterns A to F. Therefore, in the optical fiber according to the embodiment, the transmission loss is reduced, and the optical characteristics can be flexibly designed.
[0052] The optical fiber according to the embodiment can be manufactured, for example, by the following steps. First, silica soot is produced in a known VAD (Vapor Axial Deposition) apparatus using silicon tetrachloride (SiCl4) gas, germanium tetrachloride (GeCl4) gas, silicon fluoride (SiF4) gas, hydrogen gas, oxygen gas, and an inert gas.
[0053] At this time, the distribution of germanium concentration in the radial direction can be adjusted by adjusting the position and angle of the burner that supplies germanium tetrachloride (SiCl4) and the flow rate of germanium tetrachloride.
[0054] For example, when realizing the refractive index profile of pattern A, germanium tetrachloride is not flowed when producing the silica soot near the central axis, but instead germanium tetrachloride is started to flow from a point where the diameter is larger than the diameter of the hole to be drilled later, and then the flow rate of germanium tetrachloride is gradually increased, and then germanium tetrachloride is flowed at a certain flow rate value for a certain period of time, and then the supply of germanium tetrachloride is stopped.
[0055] For example, when realizing the refractive index profile of pattern B, germanium tetrachloride is not flowed when producing the silica soot near the central axis, but instead germanium tetrachloride is started to flow from a point where the diameter is larger than the diameter of the hole to be drilled later, and then the flow rate is gradually increased until a certain flow rate value is reached and the supply of germanium tetrachloride is stopped.
[0056] For example, when realizing the refractive index profile of pattern C, germanium tetrachloride is not flowed when producing the silica soot near the central axis, but germanium tetrachloride is started to flow from a point where the diameter is larger than the diameter to be drilled later, and then the flow rate of germanium tetrachloride is gradually reduced, and then the supply of germanium tetrachloride is stopped.
[0057] For example, when realizing the refractive index profile of pattern D, germanium tetrachloride is not flowed when producing the silica soot near the central axis, but instead, germanium tetrachloride is flowed at a gradually increasing flow rate from a point where the diameter is larger than the diameter of the hole to be drilled later, and then the flow rate is maximized at a position corresponding to the outer periphery of the core portion, and then the supply of germanium tetrachloride is stopped.
[0058] For example, when realizing the refractive index profile of pattern E, germanium tetrachloride is not flowed when producing the silica soot near the central axis, but instead a predetermined amount of germanium tetrachloride is flowed starting from a point where the diameter is larger than the diameter of the hole to be drilled later, and then the flow rate is reduced so that the flow rate is minimized at a position corresponding to the outer periphery of the core portion, and then the supply of germanium tetrachloride is stopped.
[0059] For example, when realizing the refractive index profile of pattern F, germanium tetrachloride is not flowed when producing the silica soot near the central axis, but instead a predetermined amount of germanium tetrachloride is flowed from a point where the diameter is larger than the diameter of the hole to be drilled later, and then the flow rate is increased in steps so that the flow rate is maximized at a position corresponding to the outer periphery of the core portion, and then the supply of germanium tetrachloride is stopped.
[0060] The silica soot is then sintered and vitrified to produce a silica glass base material. During the sintering and vitrification, helium gas and chlorine gas are flowed to dope the silica glass with chlorine. The chlorine-based gas flowed during the sintering and vitrification is not limited to chlorine gas, and may be, for example, silicon tetrachloride gas.
[0061] After that, a hole is formed in the center of the produced silica glass base material by a drilling method to make a tube. Next, K is deposited on the inner surface of the tube. The deposition of K can be performed by the aerosol method described below. First, potassium chloride (KCl) raw material is heated above its melting point in an electric furnace to melt and evaporate, and then aerosol particles are generated by a cooling gas and transported into the hole of the chlorine-doped tube by an argon carrier gas, whereby K is deposited.
[0062] Then, an oxyhydrogen flame is applied to the surface of the tube under vacuum to perform a collapsing process, thereby obtaining a silica glass base material with K doped in the center.
[0063] In the above method, K is doped in the gas phase, but the doping method is not limited to this. For example, after forming silica soot, it may be pre-sintered in a temperature range where densification does not occur, and then K may be doped by a liquid immersion method or the like. In the above method, K chloride is used as the material containing K, but this is not the only option, and other compounds such as nitrates, iodides, bromides, etc. may also be used.
[0064] The OVD (Outside Vapor Deposition) method is used to form fluorine-doped silica soot on the base material obtained as described above. This silica soot is the silica soot that will become the depressed layer. In the OVD method, for example, silicon tetrachloride (SiCl4) gas, fluorine tetrachloride (SiF4) gas, hydrogen gas, oxygen gas, and inert gas are used. Note that germanium tetrachloride (GeCl4) gas may also be used at the initial stage of forming this silica soot to form and adjust a germanium-doped region on the outer periphery of the silica glass base material. The silica soot thus formed is vitrified to form a depressed layer, thereby obtaining an optical fiber base material. In the above process, the flow rate of each gas is adjusted so that the concentrations of various dopants contained in the center core are fluorine concentration of 500 ppm to 10,000 ppm, alkali metal concentration of 10 ppm to 1,000 ppm, chlorine concentration of 15,000 ppm, and germanium concentration of 5,000 ppm or less.
[0065] Instead of the above-mentioned OVD method, the optical fiber preform may be obtained by performing a jacketing process multiple times in which an F-doped jacket tube is attached and integrated with an oxyhydrogen flame. In addition, between the jacketing processes, the preform may be appropriately stretched with an oxyhydrogen flame.
[0066] The completed optical fiber preform is then drawn into an optical fiber.
[0067] Although the refractive index profile of the optical fiber 1 according to the above embodiment is a W-type, the refractive index profile is not limited to this and may be, for example, a step type.
[0068] Fig. 5 shows a step-type refractive index profile. In Fig. 5, profile P21 shows the refractive index profile of the core portion 1a, and profile P22 shows the refractive index profile of the cladding portion 1b. In the case of Fig. 5, the center core corresponds to the entire core portion 1a.
[0069] The present invention is not limited to the above-mentioned embodiment. The present invention also includes a configuration in which the above-mentioned components are appropriately combined. Further effects and modifications can be easily derived by those skilled in the art. Therefore, the broader aspects of the present invention are not limited to the above-mentioned embodiment, and various modifications are possible. [Explanation of symbols]
[0070] 1: Optical fiber 1a: Core part 1aa: Center core 1ab Depressed layer 1b: Clad section 1c: Covering layer 1ca: Primary layer 1cb: Secondary layer A: Arrow
Claims
1. a core portion made of silica glass and having a center core; a cladding portion made of silica glass having a refractive index lower than the maximum refractive index of the core portion and surrounding an outer periphery of the core portion; Equipped with the center core includes fluorine, an alkali metal element, chlorine, and germanium; The germanium is distributed such that the germanium concentration varies depending on the radial position of the center core. Optical fiber.
2. In the center core, the fluorine concentration is 500 ppm or more and 10,000 ppm or less, the alkali metal concentration is 10 ppm or more and 1,000 ppm or less, the chlorine concentration is 15,000 ppm or less, and the germanium concentration is 5,000 ppm or less.
2. The optical fiber of claim 1.
3. In the center core, the germanium concentration is higher in an outer periphery than in a center of the core in a radial direction.
2. The optical fiber of claim 1.
4. In the center core, the distance from the center in the radial direction is r, the germanium concentration at the distance r is f(r), the minimum value of f(r) is minf(r), and the core radius of the center core is a, then the following formula (1) is established.
2. The optical fiber of claim 1. [0010]
5. The following formula (2) holds true:
5. The optical fiber of claim 4. [0025]
6. The center core contains germanium at a radial position where the relative refractive index difference Δ1 with respect to pure silica glass is a maximum value Δ1max.
2. The optical fiber of claim 1.
7. The transmission loss at a wavelength of 1550 nm is 0.164 dB / km or less.
2. The optical fiber of claim 1.
8. The transmission loss at a wavelength of 1550 nm is 0.160 dB / km or less.
2. The optical fiber of claim 1.
9. The germanium concentration in the center core is 2500 ppm or less, The transmission loss at a wavelength of 1550 nm is 0.154 dB / km or less.
2. The optical fiber of claim 1.
10. The mode field diameter at a wavelength of 1310 nm is 9.2 μm or more and 9.5 μm or less.
2. The optical fiber of claim 1.
11. Has a step or W-shaped refractive index profile 2. The optical fiber of claim 1.
12. The germanium is distributed to form the refractive index profile according to a refractive index profile determined by the fluorine, the alkali metal element, and the chlorine. The optical fiber of claim 11.
13. The core portion is the center core, and the relative refractive index difference Δ1 of the center core with respect to pure silica glass is 0% or more and 0.15% or less, and the relative refractive index difference Δclad of the cladding portion with respect to pure silica glass is -0.3% or more and -0.15% or less, and the core diameter of the center core is 2a, 2a is 8.0 μm or more and 13.0 μm or less.
2. The optical fiber of claim 1.
14. the core portion is composed of the center core and a depressed layer that is formed so as to surround an outer periphery of the center core and has a refractive index smaller than that of a cladding portion, The relative refractive index difference Δ1 of the center core with respect to pure silica glass is 0% or more and 0.20% or less, the relative refractive index difference Δclad of the cladding portion with respect to pure silica glass is -0.2% or less, the core diameter of the center core is 2a, 2a is 9.0 μm or more and 14.0 μm or less, and the outer diameter of the depressed layer is 2b, b / a is 1.2 or more and 4.0 or less.
2. The optical fiber of claim 1.
Citation Information
Patent Citations
OPTICAL FIBER CONTAINING ALKALI METAL OXIDE AND METHOD AND APPARATUS FOR MANUFACTURING THE SAME
JP2007504080A
Optical fiber and silica glass preform for optical fiber
JP2014142613A