Polishing composition

A polishing composition with surface-modified abrasive grains enhances the polishing rate of silicon nitride by modifying the abrasive grains with specific compounds, addressing the inefficiencies of conventional compositions and improving the polishing rate ratio with silicon oxide.

JP2024134682AActive Publication Date: 2024-10-04FUJIMI INCORPORATED
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023045005
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04
Estimated Expiration
2043-03-22

AI Technical Summary

Technical Problem

Conventional polishing compositions for silicon nitride do not adequately increase the polishing rate, particularly when compared to silicon oxide, as they do not effectively leverage the nitrogen-silicon bond in silicon nitride.

Method used

A polishing composition comprising surface-modified abrasive grains, modified with a first compound having a silicon atom and a second compound with a carbon and hydrogen atom, is used to enhance the polishing rate of silicon nitride relative to silicon oxide.

Benefits of technology

The composition significantly increases the polishing rate of silicon nitride compared to silicon oxide, achieving a polishing rate ratio of up to 1150 Å/min to 70 Å/min, thereby improving the efficiency of semiconductor manufacturing processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134682000001
    Figure 2024134682000001
  • Figure 2024134682000002
    Figure 2024134682000002
Patent Text Reader

Abstract

To provide a polishing composition capable of enhancing a polishing speed of an object to be polished having a nitrogen atom-silicon atom bond such as silicon nitride etc., relative to the polishing speed of an object to be polished having a silicon atom-oxygen atom bond such as silicon oxide etc.SOLUTION: A polishing composition is for polishing an object to be polished, and comprises: a surface-modified abrasive whose surface is modified with a first compound having a silicon atom and a second compound having a silicon atom different from the first compound; and an aqueous carrier, wherein the first compound has a sulfur atom, and the second compound has carbon and hydrogen atoms, but does not have a nitrogen atom.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polishing composition for polishing an object to be polished. [Background technology]

[0002] In the semiconductor device manufacturing process, there is a demand for polishing silicon nitride, which has poor chemical reactivity, at a high speed. Many of the polishing compositions conventionally used for polishing silicon nitride contain abrasive grains and an acid. For example, Patent Document 1 discloses a polishing composition containing phosphoric acid or a phosphoric acid derivative. Patent Document 2 discloses a polishing composition containing colloidal silica and an organic acid having a sulfonic acid group or a phosphonic acid group, and having a pH of 2.5 to 5. However, these conventional polishing compositions do not fully satisfy the user's demands regarding the polishing speed of silicon nitride.

[0003] In order to solve such problems, Patent Document 3 provides a polishing composition capable of polishing silicon nitride at a higher speed and a polishing method using the same. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 06-124932 [Patent Document 2] JP 2010-41037 A [Patent Document 3] JP 2012-040671 A Summary of the Invention [Problem to be solved by the invention]

[0005] In the process of developing a new polishing composition, the present inventors found that there exists a problem of increasing the polishing rate of an object to be polished having a nitrogen atom-silicon atom bond, such as silicon nitride, relative to the polishing rate of an object to be polished having a silicon atom-oxygen atom bond, such as silicon oxide.

[0006] However, it has also been found that the polishing composition disclosed in Patent Document 3 cannot solve such problems.

[0007] Therefore, an object of the present invention is to provide a polishing composition that can increase the polishing rate of an object to be polished having a nitrogen atom-silicon atom bond, such as silicon nitride, relative to the polishing rate of an object to be polished having a silicon atom-oxygen atom bond, such as silicon oxide. [Means for solving the problem]

[0008] One aspect of the present invention is a polishing composition for polishing an object to be polished, comprising: a surface-modified abrasive whose surface is modified with a first compound having a silicon atom and a second compound having a silicon atom different from the first compound; and an aqueous carrier, wherein the first compound has a sulfur atom, and the second compound has carbon and hydrogen atoms, but no nitrogen atoms. Effect of the Invention

[0009] It is possible to provide a polishing composition that can increase the polishing rate of an object to be polished that has a nitrogen atom-silicon atom bond, such as silicon nitride, relative to the polishing rate of an object to be polished that has a silicon atom-oxygen atom bond, such as silicon oxide. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will be described in detail below. In this specification, "X to Y" means "X or more and Y or less", with the numerical values ​​(X and Y) described before and after it being included as the lower and upper limits. When "X to Y" are described multiple times, for example, when "X1 to Y1 or X2 to Y2" is described, the disclosure with each numerical value as the upper limit, the disclosure with each numerical value as the lower limit, and the combination of the upper and lower limits are all disclosed (that is, they are a legitimate basis for amendment). Specifically, amendments with X1 or more, amendments with Y2 or less, amendments with X1 or less, amendments with Y2 or more, amendments with X1 to X2, amendments with X1 to Y2, etc. must all be deemed legitimate. In addition, when features or aspects of the present disclosure are described in terms of a Markush group, a person skilled in the art will recognize that the present disclosure is thereby described in terms of any individual component or subgroup of components of the Markush group. Unless otherwise specified, the components constituting the polishing composition may be contained in a combination of two or more types, and descriptions of the amounts used, added, etc. may mean the total amount when two or more types are combined.

[0011] <Polishing composition> One aspect of the present invention is a polishing composition for polishing an object to be polished, comprising a surface-modified abrasive whose surface is modified with a first compound having a silicon atom and a second compound having a silicon atom different from the first compound, and an aqueous carrier, wherein the first compound has a sulfur atom, and the second compound has a carbon atom and a hydrogen atom, but does not have a nitrogen atom. This aspect makes it possible to increase the polishing speed of an object to be polished having a nitrogen atom-silicon atom bond, such as silicon nitride, relative to the polishing speed of an object to be polished having a silicon atom-oxygen atom bond, such as silicon oxide.

[0012] [Surface-modified abrasives] The polishing composition of one embodiment of the present invention contains surface-modified abrasive grains, the surface of which is modified with a first compound having a silicon atom (also referred to simply as the "first compound" in this specification) and a second compound having a silicon atom different from the first compound (also referred to simply as the "second compound" in this specification).

[0013] In one embodiment of the present invention, the surface-modified abrasive is obtained by modifying the surface of an abrasive (e.g., silica particles) with a first compound and a second compound. The surface-modified abrasive of this embodiment can be prepared by a step of preparing a dispersion of an abrasive (e.g., silica particles) and a step of modifying the surface of the abrasive (e.g., silica particles) with the first compound and the second compound. Hereinafter, several embodiments of the preparation of the surface-modified abrasive will be described, taking as an example a silica particle as the object to be surface-modified.

[0014] In one embodiment of the present invention, the dispersion of silica particles is, for example, colloidal silica produced by a sol-gel method. In one embodiment of the present invention, the dispersion of silica particles can be obtained, for example, by carrying out a hydrolysis-condensation reaction using a hydrolyzable silicon compound (for example, an alkoxysilane or a derivative thereof) as a raw material. In one embodiment of the present invention, the dispersion is an aqueous dispersion.

[0015] In one embodiment of the present invention, the lower limit of the average primary particle size of the silica particles is 5 nm or more, 7 nm or more, 9 nm or more, or 11 nm or more. In one embodiment of the present invention, the upper limit of the average primary particle size of the silica particles is less than 35 nm, 30 nm or less, 28 nm or less, 26 nm or less, 24 nm or less, 22 nm or less, 20 nm or less, 18 nm or less, 16 nm or less, or 14 nm or less. The average primary particle size of the silica particles can be measured by the method described in the Examples.

[0016] In one embodiment of the present invention, the lower limit of the average secondary particle size of the silica particles is 15 nm or more, 18 nm or more, 21 nm or more, 24 nm or more, 27 nm or more, 30 nm or more, or 32 nm or more. In one embodiment of the present invention, the upper limit of the average secondary particle size of the silica particles is less than 70 nm, 60 nm or less, 55 nm or less, 50 nm or less, 45 nm or less, or 40 nm or less. The average secondary particle size of the silica particles can be measured by the method described in the Examples.

[0017] In one embodiment of the present invention, the average degree of association of the silica particles (average secondary particle size / average primary particle size) is not particularly limited, and is 1.2 or more, 1.4 or more, 1.6 or more, 1.8 or more, 2.0 or more, 2.2 or more, 2.4 or more, or 2.6 or more. The average degree of association of the silica particles (average secondary particle size / average primary particle size) is not particularly limited, and is 4.6 or less, 4.4 or less, 4.2 or less, 4.0 or less, 3.8 or less, 3.6 or less, 3.4 or less, 3.2 or less, or 3.0 or less.

[0018] In one embodiment of the present invention, the concentration of the silica particles in the dispersion is 5% by mass or more, 7% by mass or more, 9% by mass or more, 11% by mass or more, 13% by mass or more, 15% by mass or more, 17% by mass or more, or 19% by mass or more. In one embodiment of the present invention, the concentration of the silica particles in the dispersion is 40% by mass or less, 38% by mass or less, 36% by mass or less, 34% by mass or less, 32% by mass or less, 30% by mass or less, 29% by mass or less, 28% by mass or less, 27% by mass or less, 26% by mass or less, 24% by mass or less, or 22% by mass or less.

[0019] In one embodiment of the present invention, the modification of the surface of the silica particles with a first compound is carried out by adding the first compound and / or its precursor (also referred to herein simply as "silane compound 1") to a dispersion of the silica particles.

[0020] In one embodiment of the present invention, the first compound has an oxygen atom. In one embodiment of the present invention, the first compound has an oxo acid group. By the first compound having an oxygen atom or a sulfonic acid group, the polishing rate of an object to be polished having a silicon atom-oxygen atom bond, such as silicon oxide, is suppressed, and the polishing rate of an object to be polished having a nitrogen atom-silicon atom bond, such as silicon nitride, is maintained high.

[0021] In one embodiment of the present invention, the silane compound 1 is not particularly limited as long as it is converted into the first compound through some treatment. In one embodiment of the present invention, the silane compound 1 is a silane compound having a functional group that can be chemically converted into a sulfonic acid group, and the first compound is obtained by converting the functional group into a sulfonic acid group.

[0022] In one embodiment of the present invention, the silane compound 1 may be 1) a compound having a sulfonate group that can be converted to a sulfonic acid group by hydrolysis, or 2) a compound having a mercapto group and / or a sulfide group that can be converted to a sulfonic acid group by oxidation. In one embodiment of the present invention, examples of the compound having a mercapto group and / or a sulfide group include 3-mercaptopropyltrimethoxysilane, 2-mercaptopropyltriethoxysilane, 2-mercaptoethyltrimethoxysilane, 2-mercaptoethyltriethoxysilane, and bis(3-triethoxysilylpropyl)disulfide.

[0023] In one embodiment of the present invention, the first compound is at least one of 3-mercaptopropyltrimethoxysilane, 2-mercaptopropyltriethoxysilane, 2-mercaptoethyltrimethoxysilane, 2-mercaptoethyltriethoxysilane, and bis(3-triethoxysilylpropyl)disulfide in which the mercapto group and / or sulfide group is converted to a sulfonic acid group.

[0024] In one embodiment of the present invention, the silane compound 1 may be in the form of a solution. A solvent may be used to make it into a solution, and an example of the solvent is an organic solvent (hydrophilic solvent). An example of the organic solvent (hydrophilic solvent) is at least one organic solvent selected from the group consisting of methanol, ethanol, and isopropanol. As the organic solvent, methanol or ethanol is preferred from the viewpoint of low vapor pressure, and ethanol is more preferred from the viewpoint of easy handling.

[0025] In one embodiment of the present invention, when the silane compound 1 is in the form of a solution, the concentration of the silane compound 1 is, for example, 0.01 to 100 mass %. Note that 100 mass % means that the silane compound 1 may be in the form of a stock solution as it is, rather than being dissolved in an organic solvent (hydrophilic solvent).

[0026] In one embodiment of the present invention, the amount of the first compound or the silane compound 1 used in modifying the surface of the silica particles is independently 0.5 parts by mass or more, 0.7 parts by mass or more, 0.9 parts by mass or more, 1.1 parts by mass or more, 1.3 parts by mass or more, 1.5 parts by mass or more, 1.7 parts by mass or more, 1.9 parts by mass or more, 2.1 parts by mass or more, or 2.3 parts by mass or more, relative to 100 parts by mass of the silica particles. In one embodiment of the present invention, the amount of the first compound or the silane compound 1 used in modifying the surface of the silica particles is independently 10.0 parts by mass or less, 8.0 parts by mass or less, 6.0 parts by mass or less, 4.0 parts by mass or less, 3.0 parts by mass or less, 2.8 parts by mass or less, or 2.6 parts by mass or less.

[0027] In one embodiment of the present invention, the temperature when the silica particles are reacted with the first compound and / or the silane compound 1 is 20 to 100°C, 30 to 95°C, 40 to 90°C, 50 to 85°C, 60 to 80°C, or 65 to 75°C. In one embodiment of the present invention, the temperature when the silica particles are reacted with the first compound and / or the silane compound 1 is in the range from room temperature (about 20°C) to the boiling point of the above-mentioned solvent. In one embodiment of the present invention, the time when the silica particles are reacted with the first compound and / or the silane compound 1 is 10 minutes or more, 30 minutes or more, 1 hour or more, 4 hours or more, 8 hours or more, 12 hours or more, or 15 hours or more. In one embodiment of the present invention, the time when the silica particles are reacted with the first compound and / or the silane compound 1 is 25 hours or less, or 20 hours or less. In one embodiment of the present invention, from the viewpoint of completing the hydrolysis, the temperature is preferably 50° C. or more and the time is preferably 15 hours or more.

[0028] In one embodiment of the present invention, the silica particles and the first compound and / or the silane compound 1 may be reacted with each other under stirring.

[0029] In one embodiment of the present invention, when a compound having a functional group that is a mercapto group and / or a sulfide group is used as the silane compound 1, the functional group can be oxidized by subjecting it to an oxidation treatment, whereby the functional group is converted into a sulfonic acid group.

[0030] Examples of the oxidizing agent include at least one of nitric acid, hydrogen peroxide, oxygen, ozone, organic peracid (percarboxylic acid), bromine, hypochlorite, potassium permanganate, and chromic acid. Among these oxidizing agents, hydrogen peroxide and organic peracid (peracetic acid, perbenzoic acid) are preferred because they are relatively easy to handle and have a good oxidation yield.

[0031] In one embodiment of the present invention, the amount of the oxidizing agent used (in terms of effective concentration) is 5 parts by mass or more, 7 parts by mass or more, 9 parts by mass or more, or 11 parts by mass or more, relative to 100 parts by mass of the silica particles. In one embodiment of the present invention, the amount of the oxidizing agent used (in terms of effective concentration) is 20 parts by mass or less, 18 parts by mass or less, 16 parts by mass or less, or 14 parts by mass or less, relative to 100 parts by mass of the silica particles.

[0032] In one embodiment of the present invention, the temperature of the oxidation treatment is 50 to 85° C., 60 to 80° C., or 62 to 70° C. In one embodiment of the present invention, the time of the oxidation treatment is 8 hours or more, 12 hours or more, or 15 hours or more. In one embodiment of the present invention, the time of the oxidation treatment is 25 hours or less, or 20 hours or less.

[0033] In one embodiment of the present invention, the modification of the surface of the silica particles with the second compound is carried out by adding the second compound and / or its precursor (also referred to as "silane compound 2" in this specification) to a dispersion liquid of the silica particles. There is no particular limitation on the silane compound 2 as long as it can be converted into the second compound through some treatment.

[0034] In one embodiment of the invention, the second compound is (Si)R 1 R 2 R 3 R 4 where R 1 , R 2 , R 3 and R 4 are each independently a hydrogen atom, an alkoxy group, an alkyl group, or an alkenyl group; R 1 , R 2 , R 3 and R 4 At least one of R is an alkoxy group. 1 , R 2 , R 3 and R 4 At least one of R is an alkyl group or an alkenyl group. 1 , R2 , R 3 and R 4 Two or three of the groups are alkoxy groups.

[0035] In one embodiment of the present invention, the alkoxy group has 1 to 6, 1 to 5, 1 to 4, 1 to 3, or 1 or 2. In one embodiment of the present invention, the alkyl group has 1 to 6, 1 to 5, 1 to 4, 1 to 3, or 1 or 2. In one embodiment of the present invention, the alkenyl group has 2 to 6, 2 to 5, 2 to 4, or 2 or 3.

[0036] In one embodiment of the invention, the second compound is (Si)R 1 R 2 R 3 R 4 where R 1 , R 2 , R 3 and R 4 are each independently a hydrogen atom, an alkoxy group having 1 to 6 carbon atoms, an alkyl group having 1 to 6 carbon atoms, or an alkenyl group having 2 to 6 carbon atoms; R 1 , R 2 , R 3 and R 4 At least one of R is an alkoxy group having 1 to 6 carbon atoms; 1 , R 2 , R 3 and R 4 At least one of them is an alkyl group having 1 to 6 carbon atoms or an alkenyl group having 2 to 6 carbon atoms.

[0037] In one embodiment of the present invention, the above R 1 , R 2 , R 3 and R 4 The total number of carbon atoms in R is 10 or less, 9 or less, 8 or less, 7 or less, or 6 or less. In such an embodiment, the molecular size of the surface-modified abrasive grains can be reduced, thereby suppressing aggregation of the surface-modified abrasive grains and improving the polishing rate of an object to be polished having a nitrogen atom-silicon atom bond.1 , R 2 , R 3 and R 4 The total number of carbon atoms in is 4 or more.

[0038] In one embodiment of the present invention, the second compound is selected from the group consisting of methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, vinyltrimethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, isopropyltrimethoxysilane, isopropyltriethoxysilane, n-butyltrimethoxysilane, n-butyltriethoxysilane, n-pentyltrimethoxysilane, n-hexyltrimethoxysilane, n-heptyltrimethoxysilane, n-octyltrimethoxysilane, and 2-ethylhexyltrimethoxysilane. , n-decyltrimethoxysilane, n-dodecyltrimethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, isopropyltrimethoxysilane, isopropyltriethoxysilane, n-butyltrimethoxysilane, n-butyltriethoxysilane, n-pentyltrimethoxysilane, n-hexyltrimethoxysilane, n-heptyltrimethoxysilane, n-octyltrimethoxysilane, 2-ethylhexyltrimethoxysilane, n-decyltrimethoxysilane, and n-dodecyltrimethoxysilane.

[0039] In one embodiment of the present invention, the amount of the second compound or the silane compound 2 used to modify the surface of the silica particles is, independently, 0.1 parts by mass or more, 0.2 parts by mass or more, more than 0.25 parts by mass, 0.3 parts by mass or more, 0.35 parts by mass or more, 0.4 parts by mass or more, 0.5 parts by mass or more, 0.8 parts by mass or more, 1.0 parts by mass or more, 3.0 parts by mass or more, 5.0 parts by mass or more, 7.0 parts by mass or more, or 9.0 parts by mass or more, per 100 parts by mass of the silica particles. In one embodiment of the present invention, the amount of the second compound or the silane compound 2 used is, independently, 30 parts by mass or less, 20 parts by mass or less, 15 parts by mass or less, 12 parts by mass or less, 10 parts by mass or less, less than 10 parts by mass, 9.0 parts by mass or less, 7.0 parts by mass or less, 6.0 parts by mass or less, 5.0 parts by mass or less, 4.0 parts by mass or less, 3.0 parts by mass or less, 2.0 parts by mass or less, 1.5 parts by mass or less, 1.2 parts by mass or less, less than 1.0 parts by mass, 0.9 parts by mass or less, 0.8 parts by mass or less, 0.7 parts by mass or less, 0.6 parts by mass or less, 0.4 parts by mass or less, or 0.3 parts by mass or less, per 100 parts by mass of the silica particles.

[0040] In one embodiment of the present invention, the temperature at which the silica particles are reacted with the second compound and / or the silane compound 2 is 20 to 100° C., 30 to 95° C., 40 to 90° C., 50 to 85° C., 55 to 80° C., or 58 to 70° C. In one embodiment of the present invention, the temperature at which the silica particles are reacted with the second compound and / or the silane compound 2 is in the range from room temperature (about 20° C.) to the boiling point of the solvent.

[0041] In one embodiment of the present invention, the time for reacting the silica particles with the second compound and / or the silane compound 2 is 1 minute or more, 3 minutes or more, 5 minutes or more, 10 minutes or more, 20 minutes or more, 30 minutes or more, 40 minutes or more, or 50 minutes or more. In one embodiment of the present invention, the time for reacting the silica particles with the second compound and / or the silane compound 2 is 10 hours or less, 8 hours or less, 6 hours or less, 4 hours or less, or 2 hours or less. In one embodiment of the present invention, from the viewpoint of completing the hydrolysis, the temperature is preferably 50° C. or more and the time is preferably 30 minutes or more.

[0042] In one embodiment of the present invention, the silica particles and the second compound and / or the silane compound 2 may be reacted with each other under stirring.

[0043] In one embodiment of the present invention, in preparing the surface-modified abrasive grains, the order of mixing the first compound and / or silane compound 1, the second compound and / or silane compound 2, and any oxidizing agent is not particularly limited. For example, silica particles are treated with silane compound 1, and then with an oxidizing agent, and then with the second compound and / or silane compound 2. Alternatively, silane compound 1, the oxidizing agent, and the second compound may be mixed at the same time.

[0044] In one embodiment of the present invention, the ratio (parts by mass) of the second compound or silane compound 2 to the first compound or silane compound 1 is 0.01 or more, 0.03 or more, 0.08 or more, 0.1 or more, 0.15 or more, 0.18 or more, 0.20 or more, 0.22 or more, 0.24 or more, 0.26 or more, 0.28 or more, 0.30 or more, 0.32 or more, 0.34 or more, 0.36 or more, 0.38 or more, 0.40 or more, 0.50 or more, 1.0 or more, 2.0 or more, 3.0 or more, or 3.5 or more. Increasing the amount (parts by mass) of the second compound or silane compound 2 increases the effect of suppressing the polishing rate of the polishing object having a silicon atom-oxygen atom bond. In one embodiment of the present invention, the ratio (parts by mass) of the second compound or silane compound 2 to the amount (parts by mass) of the first compound or silane compound 1 is 10 or less, 8.0 or less, 6.0 or less, 5.0 or less, 4.0 or less, less than 4.0, 3.0 or less, 2.0 or less, 1.0 or less, 0.80 or less, 0.60 or less, 0.50 or less, 0.40 or less, 0.30 or less, 0.28 or less, 0.20 or less, 0.18 or less, or 0.15 or less. If the amount (parts by mass) of the second compound or silane compound 2 is reduced, the effect of suppressing the polishing rate of the polishing object having a silicon atom-oxygen atom bond is reduced.

[0045] In one embodiment of the present invention, when the dispersion liquid of the surface-modified abrasive contains a solvent other than water, a solvent removal step for removing the solvent may be included as necessary. For example, the dispersion medium mainly composed of the reaction solvent may be replaced with water, or the solvent may be removed using an evaporator.

[0046] In this manner, the surface-modified abrasive grains can be prepared.

[0047] In one embodiment of the present invention, the concentration of the surface-modified abrasive grains in the polishing composition is 0.1 mass% or more, 0.5 mass% or more, 1.0 mass% or more, 1.5 mass% or more, 2.0 mass% or more, 2.5 mass% or more, 3.0 mass% or more, 3.5 mass% or more, 4.0 mass% or more, or 4.5 mass% or more. In one embodiment of the present invention, the concentration of the surface-modified abrasive grains in the polishing composition is 20 mass% or less, 15 mass% or less, 10 mass% or less, 9 mass% or less, 8 mass% or less, 7 mass% or less, 6 mass% or less, or 5.5 mass% or less. Within such a range, the polishing rate can be improved while suppressing costs. In addition, when the polishing composition contains two or more types of abrasive grains, the content of the abrasive grains means the total amount of these.

[0048] In one embodiment of the present invention, the lower limit of the average primary particle size of the surface-modified abrasive grains is 5 nm or more, 7 nm or more, 9 nm or more, or 11 nm or more. In one embodiment of the present invention, the upper limit of the average primary particle size of the surface-modified abrasive grains is less than 35 nm, 30 nm or less, 28 nm or less, 26 nm or less, 24 nm or less, 22 nm or less, 20 nm or less, 18 nm or less, 16 nm or less, or 14 nm or less. If it is 35 nm or more, the expected effect of the present invention may not be achieved. The average primary particle size of the surface-modified abrasive grains can be measured by the method described in the Examples.

[0049] In one embodiment of the present invention, the lower limit of the average secondary particle size of the surface-modified abrasive grains is 15 nm or more, 18 nm or more, 21 nm or more, 24 nm or more, 27 nm or more, 30 nm or more, or 32 nm or more. In one embodiment of the present invention, the upper limit of the average secondary particle size of the surface-modified abrasive grains is less than 70 nm, 60 nm or less, 55 nm or less, 50 nm or less, 45 nm or less, or 40 nm or less. If the average secondary particle size of the surface-modified abrasive grains exceeds 40 nm, the polishing rate of the first object to be polished having a silicon atom-oxygen atom bond increases, and there is a risk that the ratio of the polishing rate (Å / min) of the second object to the polishing rate (Å / min) of the first object to be polished becomes significantly low. The average secondary particle size of the surface-modified abrasive grains can be measured by the method described in the Examples.

[0050] In one embodiment of the present invention, the average degree of association (average secondary particle size / average primary particle size) of the surface-modified abrasive grains is not particularly limited, and is 1.2 or more, 1.4 or more, 1.6 or more, 1.8 or more, 2.0 or more, 2.2 or more, 2.4 or more, or 2.6 or more. As the average degree of association of the abrasive grains increases, there is an advantageous effect that the polishing rate of the object to be polished by the polishing composition is improved. The average degree of association (average secondary particle size / average primary particle size) of the surface-modified abrasive grains is not particularly limited, and is 4.6 or less, 4.4 or less, 4.2 or less, 4.0 or less, 3.8 or less, 3.6 or less, 3.4 or less, 3.2 or less, or 3.0 or less. As the average degree of association of the abrasive grains decreases, defects can be reduced more.

[0051] In one embodiment of the present invention, the polishing composition may contain abrasive grains other than the surface-modified abrasive grains. The abrasive grains other than the surface-modified abrasive grains may be at least one of inorganic particles and organic particles. In one embodiment of the present invention, the inorganic particles are at least one of silica particles, zirconia particles, alumina particles, ceria particles, titania particles, and silicon carbide particles whose surfaces are unmodified or whose surfaces are modified with a compound other than the first compound and the second compound. In one embodiment of the present invention, the organic particles may be polymethylmethacrylate (PMMA) particles. In one embodiment of the present invention, the proportion of the surface-modified abrasive grains according to one aspect of the present invention among the abrasive grains contained in the polishing composition is 80% by mass or more, 85% by mass or more, 90% by mass or more, 95% by mass or more, 98% by mass or more, 99% by mass or more, 99.5% by mass or more, 99.8% by mass or more, or 100% by mass.

[0052] [Aqueous carrier] The polishing composition according to one embodiment of the present invention includes an aqueous carrier. Examples of the aqueous carrier include water; alcohols such as methanol, ethanol, and ethylene glycol; ketones such as acetone, and mixtures thereof. Of these, water is preferred as the aqueous carrier. That is, according to one embodiment of the present invention, the aqueous carrier includes water. According to a more preferred embodiment of the present invention, the aqueous carrier is substantially composed of water. The above-mentioned "substantially" means that an aqueous carrier other than water may be included as long as the objective effect of the present invention can be achieved, and more specifically, the aqueous carrier is preferably composed of 90% by mass or more and 100% by mass or less of water and 0% by mass or more and 10% by mass or less of an aqueous carrier other than water, and more preferably composed of 99% by mass or more and 100% by mass or less of water and 0% by mass or more and 1% by mass or less of an aqueous carrier other than water. Most preferably, the aqueous carrier is water. The aqueous carrier may unavoidably include a first compound having a silicon atom and a second compound having a silicon atom different from the first compound.

[0053] From the viewpoint of not inhibiting the action of the components contained in the polishing composition, the aqueous carrier is preferably water that contains as few impurities as possible, for example, water with a total transition metal ion content of 100 ppb or less. Specifically, deionized water (ion-exchanged water) that has been removed from impurity ions by ion exchange resin and then removed from foreign matter by passing through a filter, pure water, ultrapure water, or distilled water is preferably used.

[0054] [pH and pH adjusters] In one embodiment of the present invention, the pH of the polishing composition is less than 7.0, 6.5 or less, 6.0 or less, 5.5 or less, 5.0 or less, 4.5 or less, 4.0 or less, less than 4.0, 3.8 or less, 3.5 or less, 3.2 or less, 3.0 or less, 2.8 or less, 2.6 or less, 2.4 or less, or 2.2 or less. In one embodiment of the present invention, the pH of the polishing composition is 1.0 or more, 1.2 or more, 1.4 or more, 1.6 or more, 1.8 or more, 1.9 or more, 2.0 or more, 2.2 or more, 2.4 or more, 2.6 or more, 2.8 or more, 3.0 or more, or 3.5 or more. The pH of the polishing composition can be measured by the method described in the examples. If the pH of the polishing composition is 7.0 or higher, the polishing rate of a first object to be polished having a silicon atom-oxygen atom bond will increase and the polishing rate of a second object to be polished having a nitrogen atom-silicon atom bond will decrease, which may result in a significantly lower ratio of the polishing rate (Å / min) of the second object to be polished to the polishing rate (Å / min) of the first object to be polished.

[0055] In one embodiment of the present invention, the polishing composition includes a pH adjuster. The pH adjuster can be at least one of an acid and a base. In one embodiment of the present invention, the acid can be at least one of an inorganic acid and an organic acid. In one embodiment of the present invention, the inorganic acid can include hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid, boric acid, carbonic acid, hypophosphorous acid, phosphorous acid, and phosphoric acid. In one embodiment of the invention, organic acids include formic acid, acetic acid, propionic acid, butyric acid, valeric acid, 2-methylbutyric acid, n-hexanoic acid, 3,3-dimethylbutyric acid, 2-ethylbutyric acid, 4-methylpentanoic acid, n-heptanoic acid, 2-methylhexanoic acid, n-octanoic acid, 2-ethylhexanoic acid, benzoic acid, glycolic acid, salicylic acid, glyceric acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, maleic acid, phthalic acid, malic acid, tartaric acid, citric acid, lactic acid, diglycolic acid, 2-furancarboxylic acid, 2,5-furandicarboxylic acid, 3-furancarboxylic acid, 2-tetrahydrofurancarboxylic acid, methoxyacetic acid, methoxyphenylacetic acid, and phenoxyacetic acid.

[0056] The type and amount of the pH adjuster used are not particularly limited, and may be appropriately adjusted so that the polishing composition has a desired pH.

[0057] [Zeta potential] In one embodiment of the present invention, the surface-modified abrasive grains contained in the polishing composition may have a negative zeta potential. Here, the "zeta (ζ) potential" refers to the potential difference that occurs at the interface between a solid and a liquid in contact with each other when they undergo relative motion. The zeta potential of the surface-modified abrasive grains is -10 mV or less, -15 mV or less, -20 mV or less, -25 mV or less, -30 mV or less, -35 mV or less, or -39 mV or less. The zeta potential of the silica particles is -80 mV or more, -70 mV or more, -60 mV or more, -50 mV or more, -40 mV or more, -39 mV or more, -34 mV or more, or -30 mV or more. When the abrasive grains have a zeta potential in such a range, the polishing speed of the object to be polished can be further improved. The zeta (ζ) potential can be measured by the method described in the Examples.

[0058] [Electrical conductivity] In one embodiment of the present invention, the electrical conductivity of the polishing composition is 0.5 mS / cm or more, 1.0 mS / cm or more, 1.0 mS / cm or more, 2.0 mS / cm or more, 3.0 mS / cm or more, 4.0 mS / cm or more, 5.0 mS / cm or more, 6.0 mS / cm or more, or 7.0 mS / cm or more. In one embodiment of the present invention, the electrical conductivity of the polishing composition is 11.0 mS / cm or less, 10.5 mS / cm or less, 10.0 mS / cm or less, 9.5 mS / cm or less, 9.0 mS / cm or less, 8.0 mS / cm or less, 7.0 mS / cm or less, 6.0 mS / cm or less, 5.0 mS / cm or less, or 4.0 mS / cm or less. If the electrical conductivity (EC) of the polishing composition is within this range, the polishing rate of the object to be polished can be maintained high, and the repulsion between the abrasive grains can be appropriately adjusted to ensure stability. The electrical conductivity can be measured by the method described in the Examples.

[0059] [Other ingredients] In one embodiment of the present invention, the polishing composition may further contain, as necessary, known additives that can be used in polishing compositions, such as a complexing agent, a preservative, and an antifungal agent.

[0060] In one embodiment of the present invention, the object to be polished is substantially composed of a surface-modified abrasive grain having a surface modified with a first compound and a second compound, an aqueous carrier, a pH adjuster, and at least one selected from the group consisting of a complexing agent, a preservative, and an antifungal agent. 1 , Z 2 , Z 3 , … Z p "Consisting essentially of (p is an integer of 2 or more)" means "Z 1 , Z 2 , Z 3 , ...Zp is intended to have a total content of more than 99 mass % (upper limit: 100 mass %) based on the composition.

[0061] In one embodiment of the present invention, the polishing composition may be a one-liquid type or a multi-liquid type such as a two-liquid type. The polishing composition of one aspect of the present invention may be prepared by diluting, for example, 10 to 20 times with a diluent such as water.

[0062] [Polished object] The polishing composition of one embodiment of the present invention is used for polishing an object to be polished.

[0063] In one embodiment of the present invention, the object to be polished includes at least one of an object to be polished having a silicon atom-oxygen atom bond (conveniently, a first object to be polished) and an object to be polished having a nitrogen atom-silicon atom bond (conveniently, a second object to be polished).

[0064] In one embodiment of the present invention, examples of the polishing object having silicon atom-oxygen atom bonds include TEOS type silicon oxide (hereinafter also simply referred to as "TEOS") produced using tetraethyl orthosilicate as a precursor, HDP (High Density Plasma), USG (Undoped Silicate Glass) film, PSG (Phosphorus Silicate Glass), BPSG (Boron-Phospho Silicate Glass), RTO (Rapid Thermal Oxidation), etc. In one embodiment of the present invention, examples of the polishing object having nitrogen atom-silicon atom bonds include silicon nitride film, SiCN (silicon carbonitride), etc.

[0065] In one embodiment of the present invention, the first object to be polished is silicon oxide derived from tetraethyl orthosilicate.In one embodiment of the present invention, the second object to be polished is silicon nitride.

[0066] In one embodiment of the present invention, the polishing object may include objects other than those having silicon-oxygen bonds and those having nitrogen-silicon bonds. In one embodiment of the present invention, such objects may be polycrystalline silicon (polysilicon), metals, SiGe, etc. Examples of such metals include tungsten, copper, aluminum, cobalt, hafnium, nickel, gold, silver, platinum, palladium, rhodium, ruthenium, iridium, osmium, etc.

[0067] [Polishing rate ratio of polishing composition] In one embodiment of the present invention, the object to be polished is designed so that the ratio of the polishing rate (Å / min) of the second object to be polished to the polishing rate (Å / min) of the first object to be polished is 10 or more, 13 or more, 16 or more, 20 or more, 22 or more, 28 or more, 30 or more, 35 or more, or 40 or more. In one embodiment of the present invention, the object to be polished is designed so that the ratio of the polishing rate (Å / min) of the second object to the polishing rate (Å / min) of the first object to be polished is 100 or less, 90 or less, 80 or less, 70 or less, 60 or less, 50 or less, 40 or less, 30 or less, 20 or less, or 18 or less.

[0068] <Method of manufacturing the polishing composition> In one embodiment of the present invention, the method for producing a polishing composition comprises mixing the surface-modified abrasive grains, an aqueous carrier, optionally a pH adjuster, and optionally other components. In one embodiment of the present invention, when the surface-modified abrasive grains are prepared in the form of a dispersion liquid and contain an aqueous carrier, a separate aqueous carrier may not be contained. In one embodiment of the present invention, when the surface-modified abrasive grains are prepared in the form of a dispersion liquid and contain an aqueous carrier, a separate aqueous carrier may be contained. The concentration and pH of each component may be adjusted by adjusting the amount of the aqueous carrier.

[0069] The temperature at which the components constituting the polishing composition are mixed is not particularly limited, but is preferably 10° C. or higher and 40° C. or lower, and may be heated to increase the dissolution rate. The mixing time is also not particularly limited as long as the components can be mixed uniformly.

[0070] [Polishing method and semiconductor substrate manufacturing method] The polishing composition of one aspect of the present invention is suitable for use in polishing an object having a first object to be polished having a silicon atom-oxygen atom bond and a second object to be polished having a nitrogen atom-silicon atom bond. Thus, one aspect of the present invention provides a polishing method for polishing an object to be polished having a first object to be polished having a silicon atom-oxygen atom bond and a second object to be polished having a nitrogen atom-silicon atom bond with the polishing composition of one aspect of the present invention. One aspect of the present invention provides a method for producing a semiconductor substrate, comprising a step of polishing a semiconductor substrate including a first object to be polished having a silicon atom-oxygen atom bond and a second object to be polished having a nitrogen atom-silicon atom bond by the polishing method.

[0071] In one embodiment of the present invention, the polishing apparatus used may be a general polishing apparatus equipped with a holder for holding a substrate or the like having an object to be polished, a motor capable of changing the rotation speed, and the like, and having a polishing platen onto which a polishing pad (polishing cloth) can be attached.

[0072] In one embodiment of the present invention, the polishing pad may be made of any material, including general nonwoven fabric, polyurethane, and porous fluororesin, without any particular limitations. The polishing pad is preferably provided with grooves for storing the polishing liquid.

[0073] In one embodiment of the present invention, the polishing conditions are, for example, preferably 10 to 500 rpm rotation speed of the polishing platen or less. The pressure (polishing pressure) applied to the substrate having the object to be polished is preferably 0.5 to 10 psi. There is no particular limitation on the method of supplying the polishing composition to the polishing pad, and for example, a method of continuously supplying the composition using a pump or the like is adopted. There is no limitation on the amount of supply, but it is preferable that the surface of the polishing pad is always covered with the polishing composition of the present invention.

[0074] [Polishing speed, selectivity] In one embodiment of the present invention, the polishing speed of an object having a silicon atom-oxygen atom bond is 120 Å / min or less, 110 Å / min or less, 100 Å / min or less, 90 Å / min or less, 80 Å / min or less, 70 Å / min or less, 60 Å / min or less, 50 Å / min or less, 40 Å / min or less, or 30 Å / min or less. In one embodiment of the present invention, the polishing speed of an object having a silicon atom-oxygen atom bond is 10 Å / min or more, 20 Å / min or more, 30 Å / min or more, 40 Å / min or more, 50 Å / min or more, 60 Å / min or more, 70 Å / min or more, 80 Å / min or more, or 90 Å / min or more.

[0075] In one embodiment of the present invention, the polishing speed of an object having a nitrogen atom-silicon atom bond is 700 Å / min or more, 800 Å / min or more, 900 Å / min or more, 1000 Å / min or more, 1050 Å / min or more, 1100 Å / min or more, 1130 Å / min or more, or 1150 Å / min or more. In one embodiment of the present invention, the polishing speed of an object having a nitrogen atom-silicon atom bond is 1500 Å / min or less, 1400 Å / min or less, 1300 Å / min or less, 1200 Å / min or less, 1100 Å / min or less, 1000 Å / min or less, or 900 Å / min or less.

[0076] In one embodiment of the present invention, the ratio of the polishing rate (Å / min) of the second object to be polished to the polishing rate (Å / min) of the first object to be polished is 10 or more, 13 or more, 16 or more, 20 or more, 22 or more, 28 or more, 30 or more, 35 or more, or 40 or more. In one embodiment of the present invention, the ratio of the polishing rate (Å / min) of the second object to be polished to the polishing rate (Å / min) of the first object to be polished is 100 or less, 90 or less, 80 or less, 70 or less, 60 or less, 50 or less, 40 or less, 30 or less, 20 or less, or 18 or less. If the selectivity is outside the above range, the surface condition of the finally obtained polished object may be inferior.

[0077] [Polishing speed suppressor] The second compound has an effect of suppressing the polishing rate of an object to be polished having a silicon atom-oxygen atom bond. 1 R 2 R 3 R 4 where R 1 , R 2 , R 3 and R 4 are each independently a hydrogen atom, an alkoxy group having 1 to 6 carbon atoms, an alkyl group having 1 to 6 carbon atoms, or an alkenyl group having 2 to 6 carbon atoms; R 1 , R 2 , R 3 and R 4 At least one of R is an alkoxy group having 1 to 6 carbon atoms; 1 , R 2 , R 3 and R 4 At least one of the above is an agent for suppressing the polishing rate of an object to be polished having a silicon atom-oxygen atom bond, which contains a compound which is an alkyl group having 1 to 6 carbon atoms or an alkenyl group having 2 to 6 carbon atoms.

[0078] R 1 , R 2 , R 3 and R 4 The above description can be applied to the description of EXAMPLES

[0079] The present invention will be described in more detail with reference to the following examples and comparative examples. However, the technical scope of the present invention is not limited to the following examples. In the following, unless otherwise specified, the operations were performed under the conditions of room temperature (25°C) and relative humidity of 40 to 50% RH.

[0080] <Production of Polishing Composition> [Example 1] (Preparation of surface-modified abrasives) First step: 1 kg of an aqueous dispersion of colloidal silica produced by a sol-gel method (colloidal silica concentration: 20 mass %, average primary particle diameter: 12 nm, average secondary particle diameter: 34 nm) was prepared.

[0081] Second step: 5.0 g of 3-mercaptopropyltrimethoxysilane as silane compound 1 was added thereto in a mixed form with 20 g of ethanol, and the mixture was heated and stirred at 70° C. for 18 hours.

[0082] Third step: 80 g of 31% by mass hydrogen peroxide solution was added thereto, and the mixture was heated and stirred at 70° C. for 18 hours. This converted the mercapto groups in 3-mercaptopropyltrimethoxysilane into sulfonic acid groups.

[0083] Fourth step: 0.5 g of ethyltrimethoxysilane was added thereto as the second compound, and the mixture was heated and stirred at 70° C. for 1 hour.

[0084] Fifth step: Then, the ethanol was removed using an evaporator to produce an aqueous dispersion of the surface-modified abrasive grains.

[0085] The particle size (average primary particle size, average secondary particle size) of the surface-modified abrasive grains is not particularly different from the particle size (average primary particle size, average secondary particle size) of the raw material colloidal silica.

[0086] (Production of polishing composition) A polishing composition was produced by adding maleic acid as a pH adjuster to an aqueous dispersion of surface-modified abrasive (anion-modified colloidal silica) to adjust the pH to 2, and then adding water to adjust the concentration of the surface-modified abrasive to 5 mass%.

[0087] [Examples 2 to 6, Comparative Example 5] Each polishing composition was produced in the same manner as in Example 1, except that the colloidal silica, the silane compound 1, the second compound, and the pH were changed as shown in Table 1.

[0088] [Comparative Example 1] A polishing composition was produced in the same manner as in Example 1, except that the fourth step was not performed.

[0089] [Comparative Example 2] A polishing composition was produced in the same manner as in Example 1, except that the second, third and fourth steps were not performed.

[0090] [Comparative Example 3] A polishing composition was produced in the same manner as in Example 2, except that the second and third steps were not performed.

[0091] [Comparative Example 4] A polishing composition was produced in the same manner as in Example 2, except that the silane compound 1 was changed as shown in Table 1 and the third step was not carried out.

[0092] <Measurement method> [Average primary particle size] The average primary particle size was measured using Micromeritics' Flow Sorb II From the specific surface area (BET value) of the silica particles measured by the BET method using a 2300" and the true density of the silica particles, 6000 / [true density (g / cm 3 ) × BET value (m 2 The calculation was made using the formula:

[0093] [Average secondary particle diameter] The average secondary particle diameter was measured as the volume average particle diameter (arithmetic mean diameter based on volume; Mv) using a dynamic light scattering particle size / particle size distribution analyzer UPA-UTI151 (manufactured by Nikkiso Co., Ltd.).

[0094] [Zeta potential of surface-modified abrasives] The zeta potential of the surface-modified abrasive grains in the polishing composition was calculated by subjecting the polishing composition to an ELS-Z2 manufactured by Otsuka Electronics Co., Ltd., measuring the composition at a measurement temperature of 25°C using a flow cell by the laser Doppler method (electrophoretic light scattering measurement method), and analyzing the obtained data using the Smoluchowski formula.

[0095] [pH of polishing composition] The pH of the polishing composition was measured using a glass electrode type hydrogen ion concentration indicator (Model: F-23, manufactured by Horiba, Ltd.). Specifically, after three-point calibration using standard buffer solutions (phthalate pH buffer solution pH: 4.01 (25°C), neutral phosphate pH buffer solution pH: 6.86 (25°C), and carbonate pH buffer solution pH: 10.01 (25°C)), the glass electrode was placed in the polishing composition, and the pH was measured after 2 minutes or more had passed and the pH stabilized.

[0096] [Electrical Conductivity of Polishing Composition] The electrical conductivity (EC) of the polishing composition was measured with a tabletop electrical conductivity meter (manufactured by Horiba, Ltd., model number: DS-71 LAQUA (registered trademark)).

[0097] [Polishing speed] The object to be polished is 200mm wafer (SiO 2 (Silicon oxide film), a film produced using tetraethyl orthosilicate as a precursor, manufactured by Advanced Materials Technology Co., Ltd., product name: P-TEOS 10KA Blanket), 200mm wafer (Si 3 N 4 (Silicon nitride film), manufactured by Advanced Materials Technology Co., Ltd., product name: LP-SiN 3.5KA Blanket), Each wafer was polished under the following polishing conditions using the polishing composition obtained above, and the polishing rate was measured. In addition, the ratio of the polishing rate of silicon oxide to the polishing rate of silicon nitride (selectivity, Si 3 N 4 / SiO 2 ) was calculated.

[0098] (polishing conditions) Polishing machine: CMP single-sided polishing machine for 200mm wafers Polishing pad: Polyurethane pad (IC1010, manufactured by Nitta DuPont Co., Ltd.) Pressure: 4.0psi Platen rotation speed: 123 rpm Head (carrier) rotation speed: 117 rpm Flow rate of polishing composition: 200ml / min Polishing time: 1 minute.

[0099] The polishing speed (polishing rate) of the object to be polished was calculated by the following formula.

[0100]

number

[0101] The film thickness of the polished object before and after polishing was measured using an optical interference type film thickness measuring device (KLA-Tencor Corporation, model number: A-SET) and evaluated by dividing the difference by the polishing time.

[0102] [Table 1]

[0103] As shown in the above table, the polishing compositions of the Examples can increase the polishing rate of an object having a nitrogen atom-silicon atom bond, such as silicon nitride, relative to the polishing rate of an object having a silicon atom-oxygen atom bond, such as silicon oxide. In particular, the composition of Example 2 is particularly effective in suppressing the polishing rate of silicon oxide and maintaining a high polishing rate of silicon nitride, etc.

[0104] On the other hand, Comparative Examples 1 to 3 do not contain at least one of the first compound and the second compound, and do not achieve the expected effect. Also, Comparative Examples 4 and 5 contain two compounds, but Comparative Example 4 does not contain the second compound, and Comparative Example 5 does not contain the first compound, and therefore do not achieve the expected effect.

Claims

1. a surface-modified abrasive having a surface modified with a first compound having a silicon atom and a second compound having a silicon atom different from the first compound; An aqueous carrier; Including, the first compound has a sulfur atom, A polishing composition for polishing an object to be polished, wherein the second compound has carbon and hydrogen atoms and does not have nitrogen atoms.

2. 2. The polishing composition according to claim 1, wherein the average secondary particle size of the surface-modified abrasive is 40 nm or less.

3. The polishing composition according to claim 1 , wherein the first compound has an oxygen atom.

4. The polishing composition according to claim 1 , wherein the first compound has an oxoacid group.

5. The polishing composition according to claim 1 , wherein the first compound has a sulfonic acid group.

6. The second compound is (Si)R 1 R 2 R 3 R 4 where R 1 , R 2 , R 3 and R 4 are each independently a hydrogen atom, an alkoxy group having 1 to 6 carbon atoms, an alkyl group having 1 to 6 carbon atoms, or an alkenyl group having 2 to 6 carbon atoms; R 1 , R 2 , R 3 and R 4 At least one of R is an alkoxy group having 1 to 6 carbon atoms; 1 , R 2 , R 3 and R 4 2. The polishing composition according to claim 1, wherein at least one of the groups is an alkyl group having 1 to 6 carbon atoms or an alkenyl group having 2 to 6 carbon atoms.

7. R 1 , R 2 , R 3 and R 4 The polishing composition according to claim 6 , wherein the total number of carbon atoms in is 10 or less.

8. 2. The polishing composition according to claim 1, wherein the amount of the second compound is less than 10 parts by mass per 100 parts by mass of the abrasive grains to be surface-modified.

9. 2. The polishing composition according to claim 1, wherein the object to be polished comprises a first object to be polished having a silicon atom-oxygen atom bond and a second object to be polished having a nitrogen atom-silicon atom bond.

10. The polishing composition according to claim 9 , wherein the first object to be polished is silicon oxide derived from tetraethyl orthosilicate.

11. The polishing composition according to claim 9, wherein the second object to be polished is silicon nitride.

12. 10. The polishing composition according to claim 9, which is designed so that the ratio of the polishing rate (Å / min) of the second object to the polishing rate (Å / min) of the first object to be polished is 10 or more.

13. The polishing composition according to claim 1 , having a pH of less than 7.

0.

14. (Si)R 1 R 2 R 3 R 4 where R 1 , R 2 , R 3 and R 4 are each independently a hydrogen atom, an alkoxy group having 1 to 6 carbon atoms, an alkyl group having 1 to 6 carbon atoms, or an alkenyl group having 2 to 6 carbon atoms; R 1 , R 2 , R 3 and R 4 At least one of R is an alkoxy group having 1 to 6 carbon atoms; 1 , R 2 , R 3 and R 4 2. An agent for suppressing the polishing rate of an object to be polished having a silicon atom-oxygen atom bond, comprising a compound in which at least one of the above is an alkyl group having 1 to 6 carbon atoms or an alkenyl group having 2 to 6 carbon atoms.

Citation Information

Patent Citations

  • Silica-based slurry

    JP2008141214A

  • Polishing composition and polishing method

    JP2017092373A

  • Polishing composition and manufacturing method thereof, polishing method, and substrate manufacturing method

    JP2022056348A

  • Reward system

    KR1020230029306A

  • Polishing

    JP1994124932A