Electrolytic electrode, and method of producing electrolytic electrode
The electrolytic electrode with a ruthenium and metal element coating optimizes crystal plane spacing for reduced overvoltage, addressing high voltage issues in electrolysis and achieving efficient, low-power electrolysis for saline water and chlorine gas production.
Patent Information
- Application Number
- JP2023045039
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2043-03-22
AI Technical Summary
Existing electrolysis processes face high voltage requirements due to resistance and overvoltage issues, leading to increased power consumption and potential voltage increases over time, particularly in ion-exchange membrane salt electrolysis.
An electrolytic electrode comprising a conductive base material with a first coating layer containing a first catalyst and a second coating layer containing a ruthenium element and a metal element that forms a rutile structure, with a specific molar ratio to optimize crystal plane spacing for reduced overvoltage, as determined by X-ray diffraction.
The electrode enables electrolysis at lower voltages, reducing power consumption and minimizing by-product production, particularly suitable for saline water electrolysis and chlorine gas generation.
Smart Images

Figure 2024134704000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrode for electrolysis and a method for producing an electrode for electrolysis. [Background technology]
[0002] In the ion exchange membrane method salt electrolysis process, a technology that can maintain a low electrolysis voltage for a long period of time is required to reduce power consumption. A detailed analysis of the breakdown of electrolysis voltage includes, in addition to the theoretically required voltage, voltages caused by the resistance of the ion exchange membrane and the structural resistance of the electrolytic cell, overvoltages of the anode and cathode, and voltages caused by the distance between the anode and cathode. In addition, when electrolysis is continued for a long period of time, voltage increases due to impurities in the salt water and various other causes may occur. Among the above-mentioned electrolysis voltages, various studies have been conducted to reduce the overvoltage of the anode. For example, Patent Document 1 discloses an invention of an insoluble anode in which a coating of platinum group oxide such as ruthenium is provided on a titanium substrate. This anode is called a DSA (Dimension Stable Anode). Patent Documents 2 to 6 also disclose electrodes for electrolysis. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Special Publication No. 46-021884 [Patent Document 2] International Publication No. 2012 / 081635 [Patent Document 3] International Publication No. 2011 / 078353 [Patent Document 4] JP 2012-112033 A [Patent Document 5] JP 2012-172199 A [Patent Document 6] JP 2009-142733 A Summary of the Invention [Problem to be solved by the invention]
[0004] Therefore, an object of the present invention is to provide an electrode for electrolysis which has a low voltage during electrolysis. Another object of the present invention is to provide a method for producing an electrode for electrolysis which has a low voltage during electrolysis. [Means for solving the problem]
[0005] The present invention provides an electrode for electrolysis comprising a conductive substrate, a first coating layer coating the conductive substrate, and a second coating layer coating the first coating layer, the first coating layer comprises a first catalyst; The second coating layer includes a second catalyst containing ruthenium element and a metal element (A) capable of forming a rutile structure when an oxide is formed, and a molar ratio of the ruthenium element to the metal element (A) in the second catalyst is such that a crystal plane spacing calculated by the Braggs equation of a Miller index (101) plane in a spectrum obtained by X-ray diffraction of the second catalyst is 99.6 to 100% of a peak value.
[0006] The metal element (A) is preferably titanium element and / or tin element.
[0007] The molar ratio [ruthenium element / metal element (A)] is preferably more than 50 / 50 and not more than 90 / 10.
[0008] The above-mentioned electrodes for electrolysis are preferably for electrolysis of saline solution.
[0009] The electrode for electrolysis is preferably an anode.
[0010] The present invention also provides a method for producing an electrode for electrolysis comprising a conductive base material, a first coating layer coating the conductive base material, and a second coating layer coating the first coating layer, the first coating layer comprises a first catalyst; A step of mixing ruthenium element with a metal element (A) capable of forming a rutile structure when an oxide is formed, and performing X-ray diffraction; A step of plotting the crystal plane spacing calculated by the Braggs equation of the Miller index (101) plane in the spectrum obtained by X-ray diffraction for each mixed molar ratio; selecting a molar ratio that is 99.6 to 100% of the peak value of the crystal plane spacing; mixing the ruthenium element and the metal element (A) in the selected molar ratio to prepare a catalyst for the second coating layer; and The present invention provides a method for producing an electrode for electrolysis, comprising a step of coating a surface of the first coating layer with the catalyst for a second coating layer to form a second coating layer.
[0011] The metal element (A) is preferably titanium element and / or tin element.
[0012] The above-mentioned electrodes for electrolysis are preferably for electrolysis of saline solution.
[0013] The electrode for electrolysis is preferably an anode.
[0014] The present invention also provides a method for producing chlorine gas, which comprises electrolyzing saline solution using the above-mentioned electrode for electrolysis to produce chlorine gas. Effect of the Invention
[0015] By using the electrode for electrolysis of the present invention, electrolysis can be performed at a low voltage. Moreover, according to the method for producing an electrode for electrolysis of the present invention, an electrode for electrolysis capable of performing electrolysis at a low voltage can be easily produced. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a cross-sectional view showing one embodiment of an electrode for electrolysis of the present invention. [Diagram 2] 1 is a graph showing the relationship between the molar ratio of ruthenium and titanium in Example 1 and the crystal plane spacing calculated by the Braggs equation of the Miller index (101) plane. [Diagram 3]1 is a graph showing the relationship between the molar ratio of ruthenium and tin in Example 2 and the crystal plane spacing calculated by the Braggs equation of the Miller index (101) plane. [Figure 4] 1 shows a linear sweep voltammogram in an example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] [Electrode for electrolysis] The electrode for electrolysis of the present invention comprises a conductive base material, a first coating layer that coats the conductive base material, and a second coating layer that coats the first coating layer. Fig. 1 is a cross-sectional view showing one embodiment of the electrode for electrolysis of the present invention. The electrode for electrolysis 1 shown in Fig. 1 comprises a conductive base material 2, a layer (first coating layer) 3 that coats the conductive base material 2, and a layer (second coating layer) 4 that coats the first coating layer 3.
[0018] The first coating layer 3 covers the entire outer periphery of the cylindrical conductive substrate 2 and is in contact with the conductive substrate 2. The second coating layer 4 covers the entire outer periphery of the first coating layer 3 and is in contact with the first coating layer 3. The electrode 1 for electrolysis is composed of the conductive substrate 2, the first coating layer 3, and the second coating layer 4, but may also include layers other than these.
[0019] (Conductive base material) The conductive substrate is not particularly limited as long as it is made of a material having conductivity.When the electrode for electrolysis of the present invention is used for electrolysis of salt water, the electrode for electrolysis of the present invention is used in a high concentration salt water close to saturation, and in an atmosphere where chlorine gas is generated, so the material of the conductive substrate is preferably a valve metal having corrosion resistance.Examples of the valve metal include titanium, tantalum, niobium, zirconium, etc., and titanium is preferable from the viewpoint of economic efficiency and excellent affinity with the first coating layer.
[0020] The shape of the conductive substrate is not particularly limited and may be selected appropriately depending on the purpose, and is preferably, for example, an expanded shape, a porous plate, a wire mesh, etc. The conductive substrate preferably has a thickness of 0.1 to 2 mm.
[0021] It is preferable that the conductive substrate and the first coating layer are in contact with each other. It is preferable that the conductive metal surface (particularly the surface in contact with the first coating layer) is subjected to a surface area increasing treatment from the viewpoint of excellent adhesion with the first coating layer. Examples of the surface area increasing treatment include blasting treatment using cut wire, steel grid, alumina grid, etc., and acid treatment using sulfuric acid or hydrochloric acid. The increasing treatment may be performed by combining a plurality of treatments. Among them, it is preferable to perform a combination of blasting treatment and acid treatment. It is preferable to form irregularities on the surface of the conductive substrate by blasting treatment, and then perform acid treatment.
[0022] (first coating layer) The first coating layer contains a catalyst (first catalyst) for promoting at least one of the electrolytic reactions. Examples of metal elements that the first catalyst may contain include ruthenium, titanium, iridium, tantalum, niobium, tin, cobalt, manganese, molybdenum, lanthanum, zirconium, platinum, and the like. The first catalyst may contain the above metal elements as simple metals or as metal compounds such as metal oxides. The first catalyst may contain only one of the above metal elements, or may contain two or more of them. The above metal elements preferably contain ruthenium, and more preferably further contain one or more selected from the group consisting of titanium, iridium, and platinum.
[0023] The thickness of the first coating layer is preferably 0.1 to 7 μm, and more preferably 0.5 to 3 μm. When the thickness of the first coating layer is 0.1 μm or more, it is easy to maintain high initial electrolysis performance. When the thickness is 5 μm or less, it is economically excellent.
[0024] (Second coating layer) The second coating layer includes a catalyst (second catalyst) for promoting at least one of the electrolytic reactions. The first catalyst and the second catalyst have different compositions. It is preferable that the first coating layer and the second coating layer are in contact with each other. The second catalyst includes at least a ruthenium element and a metal element that can have a rutile structure when an oxide is formed. In this specification, the metal element that can have a rutile structure when an oxide is formed may be referred to as "metal element (A)". Examples of the metal element (A) include titanium element, tin element, vanadium element, manganese element, cesium element, germanium element, silver element, copper element, lead element, and iridium element. Among them, the metal element (A) is preferably titanium element and / or tin element. Only one type of metal element (A) may be used, or two or more types of metal elements (A) may be used.
[0025] Examples of oxides having a rutile structure that the metal element (A) can have include vanadium oxides such as VO2, manganese oxides such as β-MnO2, cesium oxides such as CsO2, germanium oxides such as GeO2, silver oxides such as AgO2, copper oxides such as CuO2, lead oxides such as PbO2, and iridium oxides such as IrO2.
[0026] The second catalyst may contain other metal elements other than the ruthenium element and the metal element (A). Examples of the other metal elements include platinum. The other metal elements may be used alone or in combination of two or more.
[0027] The second catalyst may contain the ruthenium element, the metal element (A), and the other metal elements as simple metals or as metal compounds such as metal oxides. Among these, it is preferable to contain them as metal oxides.
[0028] The molar ratio of the ruthenium element and the metal element (A) in the second catalyst is such that the crystal plane spacing calculated by the Braggs equation of the Miller index (101) plane in the spectrum obtained by X-ray diffraction of the second catalyst is 99.6 to 100% of the peak value. As a result, no correlation was found between the crystallite size calculated by the Sherrer equation and the Halder-Wagner method and the cell voltage, whereas a correlation was found between the crystal plane spacing calculated by the Braggs equation of the Miller index (101) plane and the cell voltage. When the crystal plane spacing is 99.6% or more of the peak value, the cell voltage is significantly reduced and the amount of by-products such as oxygen is small.
[0029] The crystal plane spacing is 99.6% or more of the peak value, preferably 99.7% or more, more preferably 99.8% or more, and even more preferably 99.9% or more. In particular, when the metal element (A) is titanium element, it is preferably 99.7% or more, more preferably 99.8% or more, and even more preferably 99.9% or more. When the metal element (A) is tin element, it is preferably 99.9% or more.
[0030] The molar ratio of the ruthenium element to the metal element (A) in the second catalyst [ruthenium element / metal element (A)] is, for example, 20 / 80 to 90 / 10. In one embodiment, the molar ratio is preferably more than 50 / 50 (for example, more than 50 / 50 to 90 / 10 or less), more preferably 55 / 45 to 80 / 20, and particularly preferred when the metal element (A) is titanium element. In another embodiment, the molar ratio is preferably 35 / 65 or more (for example, 35 / 65 to 90 / 10), more preferably 35 / 65 to 80 / 10, and even more preferably 36 / 64 to 65 / 35, and particularly preferred when the metal element (A) is tin element.
[0031] The total proportion of ruthenium element and metal element (A) (particularly titanium element and / or tin element) in the second catalyst is preferably 80 mol% or more, more preferably 90 mol% or more, even more preferably 95 mol% or more, particularly preferably 97 mol% or more, and may be 98 mol% or more, 99 mol% or more, or 99.5 mol% or more, relative to the total amount (100 mol%) of all metal elements in the second catalyst.
[0032] The proportion of iridium element in the second catalyst is preferably 5 mol % or less, more preferably 1 mol % or less, further preferably 0.1 mol % or less, and particularly preferably 0.01 mol % or less, based on the total amount (100 mol %) of all metal elements in the second catalyst. When the proportion is low, the amount of by-products such as oxygen produced is smaller.
[0033] The thickness of the second coating layer is preferably 0.1 to 1.0 μm, and more preferably 0.3 to 0.5 μm. When the thickness of the second coating layer is 0.1 μm or more, it is easy to maintain high initial electrolysis performance. When the thickness is 0.5 μm or less, it is economically excellent.
[0034] The total amount of metal elements of the second catalyst in the second coating layer is preferably 5 to 100 parts by mol, more preferably 10 to 65 parts by mol, relative to 100 parts by mol of the total amount of metal elements of the first catalyst in the first coating layer.
[0035] The electrolysis electrode of the present invention has a current density value of 0.80 mA / cm at 1.0 V vs. Ag / AgCl as measured by linear sweep voltammetry (LSV). 2 It is preferable that the concentration is equal to or higher than 0.90 mA / cm. 2 More preferably, 0.95 mA / cm 2 The current density is 0.80 mA / cm or more. 2If the voltage during electrolysis is more than this, the voltage during electrolysis can be further reduced. The LSV is measured using a three-electrode cell, a platinum mesh as a control electrode, Ag / AgCl as a reference electrode, and 200 g / L NaCl as an electrolyte, at a sweep rate of 10 mV / s, specifically by the method described in the Examples.
[0036] The electrode for electrolysis of the present invention is preferably an anode. The electrode for electrolysis is preferably for electrolysis of an aqueous alkali chloride solution, and more preferably for electrolysis of saline solution. When the electrode for electrolysis of the present invention is used as such an electrode, the voltage during electrolysis is particularly low.
[0037] The electrode for electrolysis of the present invention can be produced by the method for producing an electrode for electrolysis of the present invention described below, but is not limited to such a method and can also be produced by any known or commonly used method.
[0038] [Method of manufacturing electrodes for electrolysis] The electrode for electrolysis of the present invention can be manufactured by the method for manufacturing an electrode for electrolysis of the present invention. The method for manufacturing an electrode for electrolysis of the present invention is a method for manufacturing an electrode for electrolysis comprising the conductive base material, the first coating layer that coats the conductive base material, and the second coating layer that coats the first coating layer. The manufacturing method includes at least a step of mixing ruthenium element and a metal element (metal element (A)) that can have a rutile structure when an oxide is formed, and performing X-ray diffraction (X-ray diffraction step), a step of plotting the crystal plane spacing calculated by the Braggs equation of the Miller index (101) plane in the spectrum obtained by X-ray diffraction for each mixed molar ratio (crystal plane spacing plot step), a step of selecting a molar ratio that is 99.6 to 100% of the peak value of the crystal plane spacing (molar ratio selection step), a step of mixing ruthenium element and metal element (A) at the selected molar ratio to prepare a catalyst for a second coating layer (catalyst preparation step), and a step of coating the surface of the first coating layer with the catalyst for a second coating layer to form a second coating layer (second coating layer formation step).
[0039] (First coating layer formation step) The manufacturing method may include a step of forming the first coating layer on the surface of the conductive substrate (first coating layer forming step). The method of forming the first coating layer may employ a known or conventional method, for example, a coating film formed by applying a coating liquid of a metal simple substance or a metal compound that forms the first catalyst on the surface of the conductive substrate is baked in an oxygen-containing atmosphere to form the first coating layer. By baking the coating liquid in an oxygen-containing atmosphere, the components in the coating liquid are pyrolyzed to form the first coating layer, which is a catalyst layer. By the pyrolysis, the metal compound or the like that serves as a precursor is baked in an oxygen-containing atmosphere and decomposed into a metal oxide or a metal simple substance and a gaseous substance. By baking in an oxidizing atmosphere, a metal oxide is easily formed.
[0040] The metal compound is not particularly limited, but may be metal salts such as chlorides, nitrates, sulfates, and metal alkoxides. The solvent used in the coating liquid may be selected depending on the type of the metal or metal compound, and may be water, alcohols such as butanol, or the like. The metal concentration in the coating liquid is not particularly limited, but is preferably 10 to 150 g / L from the viewpoint of appropriately controlling the thickness of the first coating layer.
[0041] Examples of the method for applying the coating liquid to the surface of the conductive substrate include a dip method in which the conductive substrate is immersed in the coating liquid, a method in which the coating liquid is applied to the surface of the conductive substrate with a brush, a roll method in which the conductive substrate is passed through a sponge-like roll impregnated with the coating liquid, and an electrostatic coating method in which the conductive substrate and the coating liquid are oppositely charged and sprayed. Among these, the roll method and the electrostatic coating method are preferred from the viewpoint of superior industrial productivity.
[0042] It is preferable to dry the coating film. This allows the coating film to be formed more firmly on the surface of the conductive substrate. The drying conditions can be appropriately selected depending on the composition of the coating liquid and the type of solvent, and it is preferable to dry the coating film at a temperature of 10 to 90° C. for 1 to 20 minutes.
[0043] The baking temperature when baking the coating film in an oxygen-containing atmosphere can be appropriately selected depending on the composition of the coating liquid and the type of solvent, but is preferably 300 to 650°C. The longer the baking time, the more preferable it is, but from the viewpoint of electrode productivity, the thermal decomposition time per time is preferably 5 to 60 minutes. If necessary, the cycle of coating, drying, and baking of the coating liquid can be repeated to make the thickness of the first coating layer thicker. Furthermore, after the first coating layer is formed, baking can be performed for a long period of time if necessary to improve the stability of the first coating layer.
[0044] (X-ray diffraction process) In the X-ray diffraction step, ruthenium element and metal element (A) are mixed and X-ray diffraction is performed. In the X-ray diffraction step, X-ray diffraction analysis is performed on a plurality of mixtures having different mixing ratios of ruthenium element and metal element (A). The types of mixtures to be subjected to X-ray diffraction are three or more, preferably four or more, in order to obtain a peak of the crystal plane spacing, and if a peak value is not obtained, the analysis is performed until the peak value is obtained. The mixing ratio (molar ratio) of ruthenium element and metal element (A) in the mixture [ruthenium element:metal element (A)] is preferably selected from the range of 1:9 to 9:1 such that the total is an integer ratio of 10, and more preferably includes 3:7, 4:6, and 6:4. The mixture may be calcined before X-ray diffraction. The calcination temperature is, for example, 300 to 600°C.
[0045] The ruthenium element and the metal element (A) to be mixed may be these metal elements or metal compounds such as oxides, etc. The metal elements and metal compounds are preferably mixed in the form of powder.
[0046] (Crystal plane spacing plot process) In the above-mentioned crystal plane spacing plotting step, the crystal plane spacing calculated by the Braggs equation of the Miller index (101) plane in the spectrum obtained by X-ray diffraction is plotted for each mixed molar ratio. That is, first, a graph is created by X-ray analysis, with the x-axis representing the ratio (mol %) of ruthenium element or metal element (A) and the y-axis representing the crystal plane spacing calculated by the Braggs equation of the Miller index (101) plane.
[0047] (Mole ratio selection step) In the molar ratio selection step, the peak value of the crystal plane spacing is identified from the graph created in the crystal plane spacing plotting step, and a molar ratio of ruthenium element and metal element (A) that is 99.6 to 100% of the peak value of the crystal plane spacing is selected. When the mixing ratio is selected from the range of 1:9 to 9:1 such that the total of the mixing ratio is an integer ratio of 10, the peak value may be selected from these mixing ratios. The ratio to the peak value is preferably as described above.
[0048] (Catalyst production process) In the catalyst preparation step, the ruthenium element and the metal element (A) are mixed in the molar ratio selected in the molar ratio selection step to prepare a catalyst for the second coating layer. The ruthenium element and the metal element (A) may each be a simple metal or a metal compound. Examples of the ruthenium compound and the compound of the metal element (A) include those exemplified and explained as the metal compound that can be contained in the second coating layer. After mixing, a treatment such as calcination may be performed.
[0049] (Second coating layer formation step) In the second coating layer forming step, the surface of the first coating layer is coated with the catalyst for the second coating layer to form the second coating layer. The method for forming the second coating layer can be a known or conventional method, for example, a coating film formed by applying a coating liquid containing a catalyst for the second coating layer on the surface of the first coating layer is baked in an oxygen-containing atmosphere to prepare the second catalyst and form the second coating layer. By baking the coating liquid in an oxygen-containing atmosphere, the components in the coating liquid are pyrolyzed to form the second coating layer, which is a catalyst layer. By the pyrolysis, a metal compound or the like serving as a precursor is baked in an oxygen-containing atmosphere and decomposed into a metal oxide or a metal element and a gaseous substance. By baking in an oxidizing atmosphere, it is easy to form a metal oxide.
[0050] The solvent used in the coating solution can be selected depending on the type of the metal or metal compound, and can be water, alcohols such as butanol, etc. The metal concentration in the coating solution is not particularly limited, but is preferably 10 to 150 g / L from the viewpoint of appropriately controlling the thickness of the second coating layer.
[0051] Examples of the method for applying the coating liquid to the surface of the first coating layer include a dip method in which the conductive substrate on which the first coating layer is formed is immersed in the coating liquid, a method in which the coating liquid is applied to the surface of the first coating layer with a brush, a roll method in which the conductive substrate on which the first coating layer is formed is passed through a sponge-like roll impregnated with the coating liquid, and an electrostatic coating method in which the first coating layer surface of the conductive substrate and the coating liquid are charged with opposite charges and sprayed. Among these, the roll method and the electrostatic coating method are preferred from the viewpoint of superior industrial productivity.
[0052] It is preferable to dry the coating film. This allows the coating film to be formed more firmly on the surface of the first coating layer. The drying conditions can be appropriately selected depending on the composition of the coating liquid and the type of solvent, and it is preferable to dry the coating film at a temperature of 10 to 200° C. for 1 to 20 minutes.
[0053] The baking temperature when the coating film is baked in an oxygen-containing atmosphere can be appropriately selected depending on the composition of the coating liquid and the type of solvent, but is preferably 300 to 650°C, and more preferably 350 to 500°C. A longer baking time is preferable, but from the viewpoint of electrode productivity, the thermal decomposition time per cycle is preferably 5 to 60 minutes. The baking temperature of the second coating layer is preferably lower than the baking temperature of the first coating layer. By lowering the baking temperature of the second coating layer, a lower overvoltage can be achieved from the beginning of electrolysis.
[0054] If necessary, the cycle of coating, drying and baking of the coating solution can be repeated to make the second coating layer thicker. Furthermore, after the second coating layer is formed, baking can be performed for a long period of time as necessary to improve the stability of the second coating layer.
[0055] When electrolysis is performed using the electrode for electrolysis of the present invention, electrolysis can be performed at a low voltage. Furthermore, according to the method for producing an electrode for electrolysis of the present invention, an electrode for electrolysis that can perform electrolysis at a low voltage can be easily produced. Therefore, the electrode for electrolysis of the present invention can be used for various electrolysis. In particular, it is preferably used as an anode for generating chlorine gas, and more preferably used as an anode for salt electrolysis (specifically, an anode for salt electrolysis in an ion exchange membrane method). By using the electrode for electrolysis of the present invention as an anode for salt electrolysis, sodium hydroxide and chlorine gas can be produced by electrolyzing salt water.
[0056] [Electrolytic cell] An electrolytic cell can be provided using the electrode for electrolysis of the present invention. The electrolytic cell includes at least an anode, a cathode, and a cation exchange membrane disposed between the anode and the cathode. It is preferable to use the electrode for electrolysis of the present invention as the anode. The electrolytic cell can be used for various electrolysis, and the following describes its use in electrolysis of an aqueous alkali chloride solution as a representative example.
[0057] The electrolysis can be carried out under known or conventional conditions without any particular limitations. For example, an aqueous alkali chloride solution of 2.5 to 5.5 normality (N) is supplied to the anode chamber, and water or a diluted aqueous alkali hydroxide solution is supplied to the cathode chamber. The electrolysis temperature is 50 to 120° C., the current density is 5 to 100 A / dm 2 The electrolysis can be carried out under the following conditions.
[0058] The configuration of the electrolytic cell is not particularly limited, and may be, for example, a monopolar or bipolar type. The material constituting the electrolytic cell is not particularly limited, and for example, titanium, which is resistant to alkali chlorides and chlorine, is preferable as the material of the anode chamber. Nickel, which is resistant to alkali hydroxides and hydrogen, is preferable as the material of the cathode chamber. The electrodes may be arranged with an appropriate gap between the cation exchange membrane and the anode, but the anode and the cation exchange membrane may be arranged in contact with each other without any problems. In addition, the cathode is generally arranged with an appropriate gap from the cation exchange membrane, but a contact type electrolytic cell (zero gap type electrolytic cell) without this gap can also be used without any problems.
[0059] As the cathode, a known one can be used, and examples thereof include a cathode in which nickel, nickel oxide, an alloy of nickel and tin, activated carbon and an oxide, ruthenium oxide, platinum, or the like is coated on a nickel base material. EXAMPLES
[0060] Hereinafter, one embodiment of the present disclosure will be described in more detail based on examples.
[0061] Example 1 (X-ray diffraction measurement) Ruthenium oxide and titanium oxide powders were mixed in molar ratios [ruthenium element:titanium element] of 30:70, 40:60, 60:40, and 70:30, respectively, and baked at 450°C for 20 minutes to prepare four types of catalyst mixtures. Then, X-ray diffraction measurements were performed on each catalyst mixture to obtain XRD spectra, and the crystal plane spacing of the Miller index (101) plane was calculated using the Braggs formula with analysis software. Then, a graph was plotted with the x-axis representing the proportion (mol%) of ruthenium element and the y-axis representing the crystal plane spacing (Å). The graph obtained is shown in Figure 2. The conditions of the X-ray diffraction measurements and the analysis software are as follows. As shown in Figure 2, the catalyst mixture with the molar ratio of 60:40 showed a peak in the crystal plane spacing. Table 1 also shows the crystal plane spacing of each catalyst mixture and its ratio to the peak value. [X-ray diffraction] Equipment: Rigaku Corporation, sample horizontal type multipurpose X-ray diffraction equipment "UltimaIV" Measurement conditions X-ray source: CuKα ray Tube current: 40KV Tube voltage: 40mA Scan speed: 3° / min. [Analysis software] Qualitative analysis: PDXL Database:ICDD
[0062] [Table 1]
[0063] Example 2 (X-ray diffraction measurement) Ruthenium oxide and tin oxide powders were mixed in molar ratios [ruthenium element:tin element] of 30:70, 40:60, and 60:40, respectively, and baked at 450°C for 10 minutes to prepare three types of catalyst mixtures. Then, X-ray diffraction measurements were performed on each catalyst mixture to obtain XRD spectra, and the crystal plane spacing of the Miller index (101) plane was calculated using the Braggs formula with analysis software. Then, a graph was plotted with the x-axis representing the proportion (mol%) of ruthenium element and the y-axis representing the crystal plane spacing (Å). The obtained graph is shown in FIG. 3. The conditions of the X-ray diffraction measurements and the analysis software were the same as those in Example 1. As shown in FIG. 3, the catalyst mixture with the molar ratio of 40:60 showed a peak in the crystal plane spacing. Table 2 also shows the crystal plane spacing of each catalyst mixture and its ratio to the peak value.
[0064] [Table 2]
[0065] Example 3 (Preparation of electrodes for electrolysis) The catalyst mixtures prepared in Examples 1 and 2 were dissolved in butanol to a concentration of 7.0 mass % to prepare a catalyst solution. The above catalyst solution was applied to the surface of a first coating layer (material: Pt-IrO2-RuO2-TiO2, thickness: 5-10 μm) formed on the surface of a valve metal (titanium) (thickness: 1-3 mm) that is a conductive substrate, dried at 120°C to form a coating film, and fired at 400°C or 450°C to form a second coating layer (thickness: 0.5 μm), to prepare an electrode for electrolysis.
[0066] <Evaluation> The electrode for electrolysis obtained in Example 3 was evaluated as follows.
[0067] (1) Cell voltage measurement A two-chamber saline electrolysis cell incorporating an ion exchanger was used, the electrolysis electrode prepared in Example 3 was used as the anode, a Ni mesh coated with a precious metal catalyst was used as the cathode, the ion exchange membrane was "N2030WX" (manufactured by Chemours) and 200 g / L NaCl was used as the electrolyte. The temperature was 80°C and the current density was 4 kA / m. 2 Electrolysis was performed under the above conditions, and the cell voltage was measured. The results are shown in Table 3. The cell voltage was measured by measuring the lead wires welded to the anode and cathode with a tester.
[0068] [Table 3]
[0069] As shown in Tables 1 to 3, the electrode using the mixed catalyst with a mixture ratio that gave a high peak in the crystal plane spacing had a low cell voltage.
[0070] (2) LSV (Linear Sweep Voltammetry) A three-electrode cell was used, with a platinum mesh as the control electrode and Ag / AgCl as the reference electrode. The electrolysis electrode obtained in Example 3 was used as the working electrode. 200 g / L NaCl was used as the electrolyte. The sweep rate was 10 mV / s. Figure 4 shows the linear sweep voltammogram, and Table 4 shows the current density value at 1.0 V vs. Ag / AgCl.
[0071] [Table 4]
[0072] As shown in Table 4 and Figure 4, the electrode using the mixed catalyst with a mixture ratio that gave a high peak in the crystal plane spacing had a high current value, suggesting that electrolysis was possible at a low voltage.
[0073] Variations of the invention according to the present disclosure are described below. [Appendix 1] An electrode for electrolysis comprising a conductive base material, a first coating layer coating the conductive base material, and a second coating layer coating the first coating layer, the first coating layer comprises a first catalyst; an electrode for electrolysis, wherein the second coating layer includes a second catalyst containing ruthenium element and a metal element (A) capable of forming a rutile structure when an oxide is formed, and a molar ratio of the ruthenium element to the metal element (A) in the second catalyst is such that a crystal plane spacing calculated by the Braggs equation of a Miller index (101) plane in a spectrum obtained by X-ray diffraction of the second catalyst is 99.6 to 100% of a peak value. [Appendix 2] The electrode for electrolysis according to Appendix 1, wherein the metal element (A) is titanium element and / or tin element. [Appendix 3] The electrode for electrolysis according to appendix 1 or 2, wherein the molar ratio [ruthenium element / metal element (A)] is greater than 50 / 50 and is 90 / 10 or less. [Appendix 4] The electrode for electrolysis according to any one of Appendices 1 to 3, which is for electrolyzing saline solution. [Appendix 5] The electrode for electrolysis according to any one of Appendices 1 to 4, which is an anode. [Appendix 6] A method for producing an electrode for electrolysis comprising a conductive base material, a first coating layer coating the conductive base material, and a second coating layer coating the first coating layer, the first coating layer comprises a first catalyst; A step of mixing ruthenium element with a metal element (A) capable of forming a rutile structure when an oxide is formed, and performing X-ray diffraction; A step of plotting the crystal plane spacing calculated by the Braggs equation of the Miller index (101) plane in the spectrum obtained by X-ray diffraction for each mixed molar ratio; selecting a molar ratio that is 99.6 to 100% of the peak value of the crystal plane spacing; mixing the ruthenium element and the metal element (A) in the selected molar ratio to prepare a catalyst for a second coating layer; and A method for producing an electrode for electrolysis, comprising: a step of coating a surface of the first coating layer with the catalyst for the second coating layer to form a second coating layer. [Appendix 7] The method for producing an electrode for electrolysis according to Appendices 6, wherein the metal element (A) is titanium element and / or tin element. [Appendix 8] The method for producing an electrode for electrolysis according to appendix 6 or 7, wherein the electrode for electrolysis is for electrolysis of saline solution. [Appendix 9] The method for producing an electrode for electrolysis according to any one of Appendices 6 to 8, wherein the electrode for electrolysis is an anode. [Appendix 10] A method for producing chlorine gas, comprising electrolyzing saline solution using the electrode for electrolysis according to any one of Appendices 1 to 5 to produce chlorine gas. [Explanation of symbols]
[0074] 1 Electrode for electrolysis 2 Conductive base material 3 First coating layer 4 Second coating layer
Claims
1. An electrode for electrolysis comprising a conductive substrate, a first coating layer coating the conductive substrate, and a second coating layer coating the first coating layer, the first coating layer comprises a first catalyst; an electrode for electrolysis, wherein the second coating layer includes a second catalyst containing ruthenium element and a metal element (A) capable of forming a rutile structure when an oxide is formed, and a molar ratio of the ruthenium element to the metal element (A) in the second catalyst is such that a crystal plane spacing calculated by the Braggs equation of a Miller index (101) plane in a spectrum obtained by X-ray diffraction of the second catalyst is 99.6 to 100% of a peak value.
2. 2. The electrode for electrolysis according to claim 1, wherein the metal element (A) is titanium element and / or tin element.
3. 2. The electrode for electrolysis according to claim 1, wherein the molar ratio [ruthenium element / metal element (A)] is greater than 50 / 50 and is not greater than 90 / 10.
4. The electrode for electrolysis according to any one of claims 1 to 3, which is used for electrolysis of saline solution.
5. The electrode for electrolysis according to claim 4, which is an anode.
6. A method for producing an electrode for electrolysis comprising: a conductive base material; a first coating layer coating the conductive base material; and a second coating layer coating the first coating layer, the first coating layer comprises a first catalyst; A step of mixing ruthenium element with a metal element (A) capable of forming a rutile structure when an oxide is formed, and performing X-ray diffraction; A step of plotting the crystal plane spacing calculated by the Braggs equation of the Miller index (101) plane in a spectrum obtained by X-ray diffraction for each mixed molar ratio; selecting a molar ratio that is 99.6 to 100% of the peak value of the crystal plane spacing; mixing the ruthenium element and the metal element (A) in the selected molar ratio to prepare a catalyst for a second coating layer; and A method for producing an electrode for electrolysis, comprising: a step of coating a surface of the first coating layer with the catalyst for the second coating layer to form a second coating layer.
7. The method for producing an electrode for electrolysis according to claim 6, wherein the metal element (A) is titanium element and / or tin element.
8. 8. The method for producing an electrode for electrolysis according to claim 6 or 7, wherein the electrode for electrolysis is for electrolysis of saline solution.
9. The method for producing an electrode for electrolysis according to claim 8, wherein the electrode for electrolysis is an anode.
10. A method for producing chlorine gas, comprising electrolyzing saline solution using the electrode for electrolysis according to claim 4 to produce chlorine gas.
Citation Information
Patent Citations
Nanocrystal metal oxide composite electrode and method for preparing same
CN101532147A
Electrolysis electrodes, their preparation methods, and electrolytic cells
CN104562078B
Anode for electrolysis
JP1987243790A
Electrolysis electrode, electrolysis tank, and method for manufacturing electrolysis electrode
JP2013166994A
Anode for electrolytic generation of chlorine
JP2021529251A