Epitaxial wafer, SOI wafer, and their manufacturing method
Epitaxial wafers and SOI wafers with carbon-defect-rich silicon layers address the challenge of high-frequency characteristics and harmonic reduction, offering simpler processing and cost-effective manufacturing for high-frequency devices.
Patent Information
- Application Number
- JP2023045162
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2043-03-22
AI Technical Summary
Existing semiconductor wafers face challenges in achieving high-frequency characteristics and reducing harmonics without using high-resistivity substrates, leading to complex manufacturing processes and low productivity.
Development of epitaxial wafers with a silicon epitaxial film containing a high concentration of carbon defects formed on a normal resistivity substrate, and SOI wafers with a similar structure, which act as trap-rich layers to inhibit inversion layer formation, allowing for simpler processing and enhanced harmonic reduction.
The proposed wafers exhibit excellent harmonic reduction abilities, enabling easier manufacturing and suitability for high-frequency devices without the need for high-resistivity substrates, thus improving productivity and reducing costs.
Smart Images

Figure 2024134795000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an epitaxial wafer and an SOI wafer, and to a method for producing the same. [Background technology]
[0002] In recent years, the demand for large-capacity communications has been extremely high, and the development of devices applicable to the fifth and sixth generation mobile communications systems (commonly known as 5G and 6G) has accelerated. These communications devices incorporate integrated circuits, and the active elements (e.g., transistors) and passive elements (e.g., inductors) that make up the integrated circuits are required to have a high degree of operational stability in 5G and 6G environments. In particular, because these large-capacity communications systems are scheduled to use high frequency bands (millimeter waves to sub-terahertz bands), there is a social demand for device designs and material development that combine excellent high-frequency characteristics with power-saving performance.
[0003] Now, turning to materials necessary for semiconductor integrated circuits, silicon wafers manufactured by the Czochralski (CZ) method may be used as substrates for high-frequency integrated circuits. The silicon wafers used in this case need to have a high substrate resistivity in order to achieve small resistance loss and good high-frequency characteristics. Furthermore, for applications requiring better high-frequency characteristics, wafers with trap-rich layers formed thereon as described in Patent Document 1 and Patent Document 2 are often used. This is because, when a high-frequency signal is input to a device formed on a high-resistivity substrate, a phenomenon is known in which the resistivity changes due to the formation of an inversion layer in the substrate, and a high substrate resistivity can be maintained by capturing carriers generated in the inversion layer at a deep level in the trap-rich layer.
[0004] In particular, for passive elements, wafers with a polysilicon layer formed as a trap rich layer on a high resistivity substrate are used. On the other hand, SOI wafers with a trap rich layer are widely used for active elements. In the structure of such SOI wafers, a polysilicon layer as a trap rich layer, an oxide film as a dielectric layer, and a single crystal silicon layer are stacked in that order on a high resistivity substrate.
[0005] However, the manufacture of high resistivity substrates, such as 10,000 Ω·cm, which are widely used as substrates for high frequency integrated circuits, is technically difficult to control and results in low yields. In addition, the polysilicon used as the trap rich layer is difficult to process, which leads to poor productivity, and the SOI structure using polysilicon as the trap rich layer has a complex manufacturing process and significant cost issues. Therefore, there has been a demand for the development of technology that shows excellent high frequency characteristics, particularly the reduction of harmonics, in wafers in which a silicon epitaxial film is formed on a silicon single crystal substrate, without using a high resistivity substrate. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Special Publication No. 2015-503853 [Patent Document 2] JP 2019-129195 A [Patent Document 3] JP 2009-164590 A Summary of the Invention [Problem to be solved by the invention]
[0007] As described above, there has been a demand for epitaxial wafers and SOI wafers that can reduce harmonics without using a high resistivity substrate as a substrate for high frequency integrated circuits and can replace a polysilicon layer as a trap rich layer. Aiming to develop materials that meet such demands, the inventors have found that epitaxial wafers in which a silicon epitaxial film containing a high concentration of carbon is formed on a normal resistivity substrate, and SOI wafers using such epitaxial wafers, are promising. This makes it possible to provide substrates for high frequency integrated circuits that can be manufactured with fewer steps and with an easy processing process.
[0008] However, the ability to reduce these harmonics does not reach that of wafers that use conventional polysilicon layers as trap rich layers, and there is an urgent need to develop wafers that exhibit superior high frequency characteristics.
[0009] The present invention has been made in consideration of the above problems, and has an object to provide an epitaxial wafer and an SOI wafer that can be manufactured in a small number of steps without using a high resistivity substrate, have an easy processing process, and more reliably reduce harmonics, as well as a manufacturing method thereof. [Means for solving the problem]
[0010] In order to solve the above problems, the epitaxial wafer of the present invention is an epitaxial wafer having a silicon epitaxial film on a silicon single crystal substrate having a resistivity of 10 Ω cm or more and 5000 Ω cm or less, wherein the carbon atom concentration in the silicon epitaxial film is 5×10 17 atoms / cm 3 More than 2×10 19 atoms / cm 3 and carbon defects are formed in the silicon epitaxial film.
[0011] In such an epitaxial wafer, the silicon epitaxial film in which carbon defects are formed acts as a trap rich layer and inhibits the formation of an inversion layer, so that it is possible to exhibit excellent harmonic reduction capability using a silicon single crystal substrate. Therefore, it is not necessary to use a high resistivity substrate, so that it can be manufactured with a small number of steps and the processing process can be simplified.
[0012] Moreover, such epitaxial wafers exhibit excellent harmonic reduction capability and are therefore preferably used as wafers for high frequency devices.
[0013] The SOI wafer of the present invention preferably has a structure in which a dielectric layer and a silicon single crystal film are formed in this order on the silicon epitaxial film of the epitaxial wafer.
[0014] With such SOI wafers, the silicon epitaxial film with carbon defects acts as a trap rich layer and inhibits the formation of an inversion layer, so that a silicon single crystal substrate can be used to demonstrate excellent harmonic reduction capabilities. Therefore, it is not necessary to use a high resistivity substrate, so the wafer can be manufactured with fewer steps and the processing process can be simplified.
[0015] Moreover, such SOI wafers exhibit excellent harmonic reduction capability and are therefore preferably used as wafers for high frequency devices.
[0016] The epitaxial wafer manufacturing method of the present invention further comprises forming a layer having a carbon atom concentration of 5×10 17 atoms / cm 3 More than 2×10 19 atoms / cm 3 It is preferable to vapor-grow a silicon epitaxial film having a thickness of less than 100 nm, and then heat-treat the film at a temperature of 900° C. to 1100° C. for a time period of 1 hour to 36 hours to form carbon defects in the silicon epitaxial film.
[0017] This method for producing an epitaxial wafer can easily produce an epitaxial wafer that exhibits excellent harmonic reduction capability. In addition, since there is no need to use a high resistivity substrate, the production can be performed with a small number of steps, and the processing process can be simplified.
[0018] Furthermore, since the epitaxial wafer produced by such a method exhibits excellent harmonic reduction capability, it is preferable to produce it as a wafer for high frequency devices.
[0019] Here, by subjecting the epitaxial wafer having the above carbon atom concentration to a heat treatment, excellent harmonic characteristics can be achieved due to the action of the silicon epitaxial film in which carbon defects are formed. The reason for this is believed to be that the carbon defects formed in the silicon epitaxial film by the heat treatment form deep levels, which enhance the function as a trap rich layer and inhibit the formation of an inversion layer. Therefore, the epitaxial wafer of the present invention is suitable for use as a wafer for high frequency devices.
[0020] In addition, the method for producing an SOI wafer preferably includes producing an epitaxial wafer by the above-mentioned method, and bonding a silicon epitaxial film of the epitaxial wafer to a silicon single crystal substrate having a dielectric layer formed on its surface via the dielectric layer.
[0021] This method of manufacturing an SOI wafer can easily produce an SOI wafer that exhibits excellent harmonic reduction capability. In addition, since there is no need to use a high resistivity substrate, the number of manufacturing steps can be reduced and the processing process can be simplified.
[0022] Moreover, since the SOI wafer produced by this method exhibits excellent harmonic reduction capability, it is preferable to produce it as a wafer for high frequency devices. Effect of the Invention
[0023] The epitaxial wafer having the silicon epitaxial film in which carbon defects are formed according to the present invention can reduce harmonics more significantly due to the action of the silicon epitaxial film. This is believed to be because the silicon epitaxial film in which carbon defects are formed acts as a trap rich layer and inhibits the formation of an inversion layer. In addition, the SOI wafer having the silicon epitaxial film in which carbon defects are formed according to the present invention also exhibits excellent harmonic reduction capability due to the action of the silicon epitaxial film. The epitaxial wafer manufacturing method and SOI wafer manufacturing method according to the present invention can easily manufacture epitaxial wafers and SOI wafers that exhibit the above-mentioned excellent harmonic reduction capability. In particular, since excellent harmonic reduction capability can be exhibited even when a silicon single crystal substrate of normal resistivity is used, there is no need to use a high resistivity substrate, and the device can be manufactured with a reduced number of steps, making the processing process easier. [Brief description of the drawings]
[0024] [Figure 1] FIG. 2 is a flow diagram showing an example of a method for producing an epitaxial wafer according to the present invention. [Diagram 2] FIG. 1 is a flow diagram showing an example of a method for producing an SOI wafer according to the present invention. [Diagram 3] 1 is a planar TEM image including the interface between the silicon epitaxial film and the substrate in Experimental Example 1, where the carbon atom concentration is 7.0×1018 atoms / cm3. [Figure 4] 1 is a cross-sectional TEM image including the interface between the silicon epitaxial film and the substrate in Experimental Example 1, where the carbon atom concentration is 7.0×1018 atoms / cm3. [Diagram 5] 1 is a planar TEM image including the interface between the silicon epitaxial film and the substrate in Experimental Example 1, where the carbon atom concentration is 2.0 × 1019 atoms / cm3. [Figure 6] 1 shows the results of measuring the lifetime of epitaxial wafers of Experimental Example 1 and Experimental Example 2. [Figure 7] 1 is a graph showing the relationship between second harmonic characteristics and carbon atom concentration of epitaxial wafers of Experimental Examples 1 and 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] The present invention will be described in detail below, but the present invention is not limited thereto.
[0026] As described above, the demand for smaller, more energy-efficient, and less costly communications equipment has created a demand for epitaxial wafers that can further improve high-frequency characteristics, in particular reducing harmonics.
[0027] The present inventors have conducted extensive research into this problem. First, a silicon single crystal substrate having a resistivity of 10 Ω·cm or more and 5000 Ω·cm or less is subjected to a deposition process in a gas atmosphere containing silicon and carbon (e.g., monomethylsilane gas or trimethylsilane gas) under reduced pressure to a thickness of 0.5 to 5.5 μm and a carbon atom concentration of 5×10 17 atoms / cm 3 More than 2×10 19 atoms / cm 3 A carbon-doped silicon epitaxial film of less than 1000 nm was then formed on the epitaxial wafers. Then, to achieve a higher degree of harmonic reduction, the epitaxial wafers with the carbon-doped silicon epitaxial film were heat-treated in an atmosphere of 900°C to 1100°C. Electrodes with a line length of 2200 μm were formed on these wafers, and the second harmonics were measured. As a result, it was found that the heat-treated wafers showed a superior effect of reducing second harmonics compared to samples that were not heat-treated.
[0028] Of these, the carbon atom concentration is 2×10 19 atoms / cm 3 It was found that if the silicon epitaxial film has a carbon concentration of less than 2 × 10, no defects other than carbon defects are formed, and there is no need to worry about other types of defects in the wafer deteriorating the device characteristics. 19 atoms / cm 3 In the above cases, it was confirmed that white defects, which are not carbon defects, were formed by heat treatment. As a result, the carbon atom concentration was 2×10 19 atoms / cm 3It is preferable that the amount of the ion exchange is less than 1000 nm.
[0029] The reason why the heat-treated sample was able to reduce the second harmonic more than the epitaxial wafer that was not heat-treated is that the carbon atom concentration in the silicon epitaxial film was 5×10 17 atoms / cm 3 More than 2×10 19 atoms / cm 3 This is less than the typical carbon solid solubility in silicon of 3 × 10 17 atoms / cm 3 This is because the concentration of carbon atoms in the silicon epitaxial film is much higher than that in the silicon epitaxial film, and the formation of carbon defects due to the heat treatment is expected. Carbon atoms aggregate to form carbon defects, which in turn form new deep levels in the silicon epitaxial film, resulting in a higher trap density than before the heat treatment.
[0030] This indicates that a silicon epitaxial film in which carbon defects are formed by heat treatment is effective as a trap-rich layer, and that it can also be applied to trap-rich SOI wafers used as substrates for active elements.
[0031] Based on the above findings, the inventors have come up with the present invention. That is, one aspect of the present invention is an epitaxial wafer having a silicon epitaxial film on a silicon single crystal substrate having a resistivity of 10 Ω·cm or more and 5000 Ω·cm or less, wherein the carbon atom concentration in the silicon epitaxial film is 5×10 17 atoms / cm 3 More than 2×10 19 atoms / cm 3 and carbon defects are formed in the silicon epitaxial film.
[0032] In another embodiment of the present invention, a silicon single crystal substrate having a resistivity of 10 Ω cm or more and 5000 Ω cm or less is formed under reduced pressure with a carbon atom concentration of 5×10 17 atoms / cm 3 More than 2×10 19atoms / cm 3 and then subjecting the resulting silicon epitaxial film to a heat treatment at a temperature of 900° C. or higher and 1100° C. or lower for a time period of 1 hour or higher and 36 hours or shorter, thereby forming carbon defects in the silicon epitaxial film.
[0033] The present invention will be described in detail below with reference to the drawings, but the present invention is not limited thereto.
[0034] [Epitaxial wafer and its manufacturing method] An example of the method for producing an epitaxial wafer of the present invention is shown in Figure 1. This method is a method for producing an epitaxial wafer using a silicon epitaxial film in which carbon defects are formed as the trap rich layer as described above.
[0035] First, a silicon single crystal substrate 1 having a resistivity of 10 Ω·cm or more and 5000 Ω·cm or less is prepared. Next, a gas containing silicon atoms and carbon atoms is supplied onto the silicon single crystal substrate under reduced pressure to form a 5×10 17 atoms / cm 3 More than 2×10 19 atoms / cm 3 A silicon epitaxial film 2 having a carbon atom concentration of less than 1000 nm (hereinafter, referred to as a carbon-doped silicon epitaxial film) is vapor-grown. Then, the epitaxial wafer having the carbon-doped silicon epitaxial film 2 is heat-treated, whereby carbon defects can be formed in the silicon epitaxial film.
[0036] The vapor phase growth of the carbon-doped silicon epitaxial film 2 can be performed under reduced pressure to reduce the concentration of impurities other than carbon doped into the silicon epitaxial film. The pressure for forming the carbon-doped silicon epitaxial film 2 need not be particularly limited as long as it is reduced pressure, but it is preferably performed at about 10 Torr, for example, 5 Torr to 20 Torr (10 Torr is about 1.3 kPa, 5 Torr to 20 Torr is about 0.67 kPa to 2.7 kPa).
[0037] Carbon doping in the vapor phase growth of the carbon-doped silicon epitaxial film 2 uses a gas (source gas) containing silicon atoms and carbon atoms, as described above. The source gas preferably contains at least one of monomethylsilane gas and trimethylsilane gas. By using these gases, the silicon epitaxial film can be easily and satisfactorily doped with carbon. In addition, the vapor phase growth atmosphere may contain hydrogen, argon, or the like as a carrier gas when the source gas is supplied.
[0038] The carbon-doped silicon epitaxial film 2 can be formed satisfactorily by vapor-phase growth at 600 to 1000° C. under reduced pressure.
[0039] In addition, it is preferable to appropriately set the pressure, temperature, time, and raw material gas concentration of the vapor phase growth so that the carbon-doped silicon epitaxial film 2 to be formed has a desired thickness. The upper and lower limits of the thickness of the carbon-doped silicon epitaxial film are not particularly limited, but may be, for example, 0.1 μm to 10 μm in consideration of productivity and cost. In this way, the film has sufficient high-frequency characteristics at a lower cost. More preferably, the thickness may be 0.5 μm to 5.5 μm inclusive, but is not limited thereto.
[0040] The method of heat treatment after the deposition of the carbon-doped silicon epitaxial film 2 is not particularly limited, and for example, a heat treatment furnace for a general silicon wafer or a chamber used for vapor phase growth of the carbon-doped silicon epitaxial film can be used.
[0041] The lower limit of the heat treatment temperature in the heat treatment can be set to 900°C or more. This promotes the formation of carbon defects, improving manufacturing efficiency. The heat treatment time can be set to 1 hour or more. This allows sufficient carbon defects to be formed, improving quality. The upper limit of the heat treatment temperature can be set to 1100°C or less. This can suppress the effects of heavy metal diffusion. The upper limit of the heat treatment time can be set to 36 hours or less. This results in an epitaxial wafer that is excellent in terms of manufacturing efficiency.
[0042] In consideration of the above, carbon defects are formed in the silicon epitaxial film formed by vapor phase growth under reduced pressure by directly placing the epitaxial wafer in a heat treatment furnace whose heat treatment temperature is raised to 900°C or higher and 1100°C or lower, and performing heat treatment under conditions of 1 hour or higher and 36 hours or lower. In this case, the type of gas used during the heat treatment can be selected according to the application, and can be, for example, oxygen gas or an inert gas such as argon or nitrogen.
[0043] In this manner, the epitaxial wafer of the present invention can be manufactured. The silicon epitaxial film 3 in which carbon defects are formed by the heat treatment functions as a trap rich layer.
[0044] Of these, 5 x 10 17 atoms / cm 3 More than 2×10 19 atoms / cm 3 If the carbon atom concentration is less than 2 × 10, a sufficient amount of carbon defects are formed by the heat treatment, and the second harmonic can be reduced more than before the heat treatment. 19 atoms / cm 3 In the above cases, many defects other than carbon defects are formed after heat treatment, resulting in deterioration of quality.
[0045] The silicon single crystal substrate 1 on which the carbon-doped silicon epitaxial film 2 is formed can be used for high frequency devices by setting the resistivity to 10 Ω·cm or more and 5000 Ω·cm or less as described above. It is more preferable that the resistivity is 1000 Ω·cm or more and 5000 Ω·cm or less, which has particularly good high frequency characteristics and allows resistivity control in crystal manufacturing.
[0046] Thus, the epitaxial wafer of the present invention is suitable as a wafer for high frequency devices.
[0047] Incidentally, a wafer in which a carbon-doped epitaxial film is formed on a silicon single crystal substrate is described in Patent Document 3.
[0048] In Patent Document 3, an epitaxial film containing a high concentration of carbon is mentioned, but the intended uses are different, and the structure, manufacturing process, and resistivity are different. The present invention is intended to be used in wafers for high-frequency devices, and Patent Document 3 is intended mainly for image pickup devices. Therefore, the wafer of the present invention has a two-layer structure of a silicon single crystal substrate 1 and a silicon epitaxial film 3 in which carbon defects are formed, or a SOI structure described below. In contrast, the wafer of Patent Document 3 is manufactured with at least a three-layer structure of a silicon single crystal substrate, a carbon-doped epitaxial film, and a silicon epitaxial film. In addition, in terms of the heat treatment process, the present invention forms a carbon-doped silicon epitaxial film 2 by vapor phase growth under reduced pressure, and then performs heat treatment to form a silicon epitaxial film 3 in which carbon defects are formed. In addition, when manufacturing an SOI structure, it is manufactured by bonding two substrates manufactured by different processes. In contrast, the wafer of Patent Document 3 is characterized in that a film-forming process using a normal epitaxial growth furnace requires a temperature of 750° C. or higher, and does not include a heat treatment process after film formation. In addition, no bonding process is required when forming a multilayer structure.
[0049] Focusing on the required resistivity, the present invention is characterized in that the resistivity of the silicon single crystal substrate 1 can be widely used in the range of 10 Ω·cm to 5000 Ω·cm. In contrast, the wafer of Patent Document 3 is characterized in that at least one of the silicon epitaxial underlayer, carbon-doped epitaxial film, and silicon single crystal film is a low-resistance film with a resistivity of 1 Ω·cm or less in order to improve the performance of the imaging element, and is clearly different. Furthermore, the wafer of Patent Document 3 does not have the function of a trap rich layer in the epitaxial film, making it difficult to use it as a wafer for high-frequency devices.
[0050] As described above, according to the embodiment of the present invention, there is provided an epitaxial wafer having a silicon epitaxial film on a silicon single crystal substrate 1 having a resistivity of 10 Ω·cm or more and 5000 Ω·cm or less, and the carbon atom concentration in the silicon epitaxial film is 5×10 17 atoms / cm 3 More than 2×10 19 atoms / cm 3 In accordance with the present invention, there can be provided an epitaxial wafer characterized in that the thickness of the silicon epitaxial film is less than 100 nm and carbon defects are formed in the silicon epitaxial film.
[0051] Moreover, such an epitaxial wafer is suitable as a wafer for high frequency devices.
[0052] According to the embodiment of the present invention, a silicon single crystal substrate 1 having a resistivity of 10 Ω·cm or more and 5000 Ω·cm or less is formed with a carbon atom concentration of 5×10 17 atoms / cm 3 More than 2×10 19 atoms / cm 3 The present invention provides a method for producing an epitaxial wafer, characterized in that a silicon epitaxial film having a thickness of less than 100 nm is vapor-grown, and then the film is heat-treated at a heat treatment temperature of 900° C. or higher and 1100° C. or lower for a heat treatment time of 1 hour or higher and 36 hours or lower.
[0053] It is also possible to provide a method for producing an epitaxial wafer suitable as a wafer for high frequency devices.
[0054] [SOI wafers and their manufacturing methods] Next, a method for producing an SOI wafer will be described. An example of the method for producing an SOI wafer according to the present invention is shown in FIG. In particular, step S1 in FIG. 2 is a step for producing an epitaxial wafer (first substrate 4) having carbon defects formed therein, and is the same as the epitaxial wafer manufacturing method shown in FIG.
[0055] Here, the epitaxial wafer (first substrate 4) having the silicon epitaxial film 3 in which carbon defects are formed becomes the base wafer during bonding.
[0056] In addition, in step S2 of FIG. 2, a second substrate 5 is prepared separately from the epitaxial wafer. The second substrate 5 can be produced by first preparing a silicon single crystal substrate 6 and forming a dielectric layer 7 on the surface of the substrate. The silicon single crystal substrate 6 can be, for example, a silicon single crystal substrate 6 having a resistivity of about 10 Ω·cm, but is not limited to this. The dielectric layer 7 can be an oxide film or the like. When an oxide film is formed as the dielectric layer 7, the oxide film can be formed on the entire substrate surface by thermal oxidation. The second substrate 5 is a bond wafer.
[0057] The resistivity of the silicon single crystal substrate 6 on which the dielectric layer 7 is formed can be determined depending on the specifications of the device to be fabricated. On the other hand, the resistivity of the silicon single crystal substrate 1 on which the carbon-doped silicon epitaxial film 2 is formed is 10 Ω cm or more and 5000 Ω cm or less, as described above.
[0058] 2, the order of step S1 for producing the first substrate 4 and step S2 for producing the second substrate 5 does not matter. Either may be performed first, or they may be performed in parallel.
[0059] 2, after the first substrate 4 and the second substrate 5 are prepared as described above, the silicon epitaxial film 3 having carbon defects formed therein of the epitaxial wafer as the first substrate 4 is bonded (joined) to the silicon single crystal substrate 6 having a dielectric layer 7 formed on its surface as the second substrate 5 via the dielectric layer 7. In this manner, the SOI wafer 8 can be manufactured.
[0060] After bonding, the portion of the silicon single crystal substrate 6 on the dielectric layer 7 (e.g., oxide film) side can be thinned in step S4 of FIG. 2. This thinning can be performed to a desired thickness depending on the application by polishing or etching the silicon single crystal substrate 6 on the dielectric layer 7 (e.g., oxide film) side, or by ion implantation peeling. The ion implantation peeling can be performed, for example, by injecting hydrogen ions or the like from the dielectric layer 7 side of the silicon single crystal substrate 6 before bonding in FIG. 2 to form an ion implanted layer in the silicon single crystal substrate 6, and then peeling along the ion implanted layer by heat treatment or the like after bonding. As a result of the above, a thinned silicon single crystal film 9 (silicon single crystal film) is obtained.
[0061] In this manner, the SOI wafer 8 of the present invention can be manufactured. The SOI wafer 8 of the present invention is formed by forming a 5×10 17 atoms / cm 3 More than 2×10 19 atoms / cm 3 The SOI wafer 8 of the present invention has a structure in which a silicon epitaxial film 3 having carbon defects formed therein, which is obtained by heat-treating a carbon-doped silicon epitaxial film 2 containing carbon at a concentration of less than 1000 nm, a dielectric layer 7, and a silicon single crystal film 9 are arranged in this order. In this case, the silicon epitaxial film 3 having carbon defects formed therein functions as a trap rich layer. Therefore, the SOI wafer 8 of the present invention is suitable as a wafer for high frequency devices.
[0062] As described above, according to the embodiment of the present invention, there is provided an epitaxial wafer having a silicon epitaxial film on a silicon single crystal substrate 1 having a resistivity of 10 Ω·cm or more and 5000 Ω·cm or less, and the carbon atom concentration in the silicon epitaxial film is 5×10 17 atoms / cm 3 More than 2×10 19 atoms / cm 3 The present invention provides an SOI wafer (8) having a structure in which a dielectric layer (7) and a silicon single crystal film (9) are formed in this order on a silicon epitaxial film (3) having carbon defects formed therein, the epitaxial wafer being characterized in that the thickness of the epitaxial wafer is less than 100 nm and that carbon defects are formed in the silicon epitaxial film.
[0063] Moreover, such an SOI wafer 8 is suitable as a wafer for high frequency devices.
[0064] According to the embodiment of the present invention, a silicon single crystal substrate 1 having a resistivity of 10 Ω·cm or more and 5000 Ω·cm or less is formed with a carbon atom concentration of 5×10 17 atoms / cm 3 More than 2×10 19 atoms / cm 3 and then performing a heat treatment under conditions of a heat treatment temperature of 900° C. or more and 1100° C. or less and a heat treatment time of 1 hour or more and 36 hours or less to produce an epitaxial wafer by the epitaxial wafer manufacturing method for forming carbon defects in the silicon epitaxial film, and then providing a method for manufacturing an SOI wafer 8, characterized in that the silicon epitaxial film 3 of the epitaxial wafer in which carbon defects have been formed and a silicon single crystal substrate 6 having a dielectric layer 7 formed on its surface are bonded together with the dielectric layer 7 interposed therebetween.
[0065] Moreover, it is possible to provide a method for producing an SOI wafer 8 suitable as a wafer for a high frequency device.
[0066] [Harmonic characteristics] This paper explains the measurement of harmonic characteristics of epitaxial wafers and SOI wafers.
[0067] "In the case of SOI wafers" The harmonic characteristics of SOI wafers are measured as follows. To measure second harmonic characteristics (2HD characteristics), first remove the topmost silicon single crystal film, then form a co-planar waveguide (CPW) out of metal (e.g. aluminum) on the dielectric layer (e.g. oxide film), and ground probes to both ends of this metal electrode. After that, input a high-frequency signal into one of the electrodes, and measure the second harmonic output from the other side (e.g. input signal frequency: 1GHz, input power: 15dBm).
[0068] As a result, when carbon defects are formed by heat treatment in a carbon-doped silicon epitaxial film on a silicon single crystal substrate, the trap density of the trap rich layer is increased compared to before the heat treatment, and as a result, the carrier capture ability is improved, so that excellent second harmonic characteristics can be obtained even if the silicon single crystal substrate does not have a high resistivity.
[0069] The harmonic characteristics improve as the thickness of the silicon epitaxial film in which carbon defects are formed increases.
[0070] "In the case of epitaxial wafers" The harmonic characteristics of an epitaxial wafer are measured as follows. When measuring the second harmonic characteristics of an epitaxial wafer having a silicon epitaxial film in which carbon defects have been formed by heat treatment after forming a carbon-doped silicon epitaxial film on a silicon single crystal substrate, a co-planar waveguide (CPW) is formed of metal (e.g., aluminum) on the silicon epitaxial film in which carbon defects have been formed, using the same procedure as above, and probes are grounded to both ends of this metal electrode. After that, a high-frequency signal is input from one of the electrodes, and the second harmonic output from the other side is measured (e.g., input signal frequency: 1 GHz, input power: 15 dBm).
[0071] As a result, as in the case of SOI wafers, when carbon defects are formed by heat treatment in a carbon-doped silicon epitaxial film on a silicon single crystal substrate, the trap density of the trap rich layer is increased compared to that before the heat treatment, and as a result, the carrier capture ability is improved, so that excellent second harmonic characteristics can be obtained even if the silicon single crystal substrate does not have a high resistivity.
[0072] In this way, the epitaxial wafer and SOI wafer of the present invention can improve the second harmonic characteristics and are suitable as wafers for high frequency devices. EXAMPLES
[0073] The present invention will be described in more detail below with reference to Experimental Examples 1 to 4, but the present invention is not limited to these.
[0074] (Experimental Example 1) The epitaxial wafer of the present invention was manufactured according to FIG. 1. A carbon-doped silicon epitaxial film 2 (carbon atom concentration: 2.0×10) was formed on a silicon single crystal substrate 1 having a diameter of 300 mm, obtained by slicing an ingot manufactured by the Czochralski method using a low-pressure CVD apparatus, using monomethylsilane as a carbon source gas. 18 ~2.0×10 19 atoms / cm 3 After the deposition, the epitaxial wafer was subjected to a heat treatment at 1000°C for 12 hours in an oxygen atmosphere to form carbon defects in the silicon epitaxial film.
[0075] To investigate the structure of the epitaxial wafer, the carbon atom concentration during film formation was set to 7.0×10 18 atoms / cm 3 The epitaxial wafer with a carbon atom concentration of 2.0×10 19 atoms / cm 3TEM observation was performed after the heat treatment using the epitaxial wafer thus obtained. In the TEM observation, a planar TEM image (Fig. 3) including the interface between the silicon epitaxial film 3 in which carbon defects have been formed and the silicon single crystal substrate 1, and a cross-sectional TEM image (Fig. 4) including the surface of the silicon epitaxial film 3 in which carbon defects have been formed and the interface between the silicon epitaxial film 3 in which carbon defects have been formed and the silicon single crystal substrate 1 were obtained. Here, Fig. 3 is a planar TEM image of a thin specimen (approximately 500 nm thick) cut at a depth position including the interface between the silicon epitaxial film and the substrate, and Fig. 4 is a cross-sectional TEM image of a thin specimen (approximately 500 nm thick) cut to include the interface between the silicon epitaxial film and the substrate. As a result, the carbon atom concentration at the time of film formation was found to be 7.0 × 10 18 atoms / cm 3 It was found that in the epitaxial wafers described above, black carbon defects were formed throughout the entire silicon epitaxial film by applying heat treatment after film formation.
[0076] In contrast, the carbon atom concentration during film formation is 2.0 × 10 19 atoms / cm 3 It was found that in the epitaxial wafer, white defects that are not carbon defects are formed by heat treatment after film formation (appearance of silicon epitaxial film 10 with white defects) (see Fig. 5). Here, Fig. 5 is a planar TEM image of a thin specimen (approximately 500 nm thick) cut at a depth position that includes the interface between the silicon epitaxial film and the substrate.
[0077] The epitaxial wafer of Experimental Example 1 (carbon atom concentration: 2.0×10 18 ~2.0×10 19 atoms / cm 3 In order to investigate the trap density of the epitaxial wafer (film thickness: 5.5 μm), the carrier lifetime was measured by the μ-PCD method. As a result, the carrier lifetime of the epitaxial wafer of Experimental Example 1 was 1.0×10 18 atoms / cm 3 The wafer is about 384 μs and has a carbon atom concentration of 7.0 × 1018 atoms / cm 3 The wafer is about 145 μs long and has a carbon atom concentration of 2.0 × 10 19 atoms / cm 3 It was found that the lifetime of the epitaxial wafer was about 106 μs (see FIG. 6). Here, FIG. 6 shows the results of measuring the lifetime of an epitaxial wafer in which carbon defects were formed by the heat treatment in Experimental Example 1, and an epitaxial wafer in which no heat treatment was performed in Experimental Example 2 described below.
[0078] Next, the second harmonic characteristics were measured to investigate the harmonic characteristics of the epitaxial wafer of Experimental Example 1. An aluminum electrode with a line length of 2200 μm was formed on the silicon epitaxial film in which carbon defects were formed, and the second harmonic characteristics were measured. As a result, the second harmonic characteristics when the frequency of the input signal was set to 1 GHz were as follows: 18 atoms / cm 3 The wafer has a peak at about -19.6 dBm and a carbon atom concentration of 7.0 × 10 18 atoms / cm 3 The wafer is about -19.0 dBm and has a carbon atom concentration of 2.0 × 10 19 atoms / cm 3 The epitaxial wafer of Experimental Example 1 had a second harmonic characteristic of about -19.5 dBm. This result shows that the epitaxial wafer of Experimental Example 1 can reduce second harmonics (see FIG. 7). Here, FIG. 7 is a graph showing the relationship between the second harmonic characteristic and the carbon atom concentration of an epitaxial wafer in which carbon defects are formed by the heat treatment of Experimental Example 1 and an epitaxial wafer in which no heat treatment is performed of Experimental Example 2 described below.
[0079] (Experimental Example 2) An epitaxial wafer was manufactured in the same manner as the epitaxial wafer of Experimental Example 1, except that no heat treatment was performed after film formation. First, a carbon-doped silicon epitaxial film (carbon atom concentration: 2.0×10) was formed on a silicon single crystal substrate having a diameter of 300 mm obtained by slicing an ingot manufactured by the Czochralski method in a low-pressure CVD apparatus, using monomethylsilane as a carbon source gas.18 ~2.0×10 19 atoms / cm 3 , film thickness: 5.5 μm) was formed on the epitaxial wafer of Experimental Example 2.
[0080] To investigate the trap density of this epitaxial wafer, the carrier lifetime was measured by the μ-PCD method. As a result, the carrier lifetime of the epitaxial wafer of Experimental Example 2 was 1.0×10 18 atoms / cm 3 The wafer is about 953 μs and has a carbon atom concentration of 7.0 × 10 18 atoms / cm 3 The wafer is about 805 μs long and has a carbon atom concentration of 2.0 × 10 19 atoms / cm 3 It was found that the carrier lifetime for the epitaxial wafer in Experimental Example 1 was approximately 101 μs. Comparing Experimental Example 1 and Experimental Example 2 with reference to Figure 6, the carrier lifetime was reduced in Experimental Example 1, and this result indicates that the trap density of the epitaxial wafer in Experimental Example 1 was significantly increased by the heat treatment.
[0081] Next, to investigate the harmonic characteristics of this epitaxial wafer, the second harmonic characteristics were measured. An aluminum electrode with a line length of 2200 μm was formed on the silicon epitaxial film, and the second harmonic characteristics were measured. As a result, when the input signal frequency was set to 1 GHz, the second harmonic characteristics were 18 atoms / cm 3 The wafer is about -18.8 dBm and has a carbon atom concentration of 7.0 × 10 18 atoms / cm 3 The wafer has a peak at about -18.5 dBm and a carbon atom concentration of 2.0 × 10 19 atoms / cm 3 The wafer of Experimental Example 1 was approximately -19.3 dBm. Comparing Experimental Example 1 and Experimental Example 2 with reference to Fig. 7, the second harmonic characteristics were reduced in Experimental Example 1, and this result shows that the epitaxial wafer of Experimental Example 1 had an improved ability to reduce second harmonics due to the heat treatment.
[0082] From the above results, the carbon atom concentration of the carbon-doped silicon epitaxial film was set to 2 × 10 18 atoms / cm 3 More than 2×10 19 atoms / cm 3 It has been found that by setting the carbon defect density to less than 100 nm and fabricating an epitaxial wafer having a silicon epitaxial film in which carbon defects are formed by heat treatment, an epitaxial wafer with excellent high frequency characteristics can be obtained.
[0083] (Experimental Example 3) The SOI wafer of the present invention was manufactured according to FIG. 2. First, a silicon single crystal substrate 1 having a diameter of 300 mm was formed with a carbon atom concentration of 2×10 18 atoms / cm 3 More than 2×10 19 atoms / cm 3 An epitaxial wafer was prepared by forming a carbon-doped silicon epitaxial film 2 (film thickness: 5.5 μm) of less than 100 μm under the same conditions as in Experimental Example 1, and after the film formation, the obtained epitaxial wafer was subjected to a heat treatment at 1000° C. for 12 hours in an oxygen atmosphere to form carbon defects in the silicon epitaxial film. This was used as a base wafer (first substrate 4). Separately, a silicon wafer was prepared as a bond wafer (second substrate 5) by forming an oxide film of 400 nm thickness as a dielectric layer 7 on the surface of a silicon single crystal substrate 6 having a diameter of 300 mm. Next, the surface of the silicon epitaxial film 3 on which the carbon defects were formed of the base wafer was bonded to the oxide film surface (surface of the dielectric layer 7) of the bond wafer, and the silicon single crystal substrate 6 on the bond wafer side was polished to obtain an SOI wafer 8 with 1 μm of the silicon single crystal film remaining.
[0084] (Experimental Example 4) An epitaxial wafer was manufactured in the same manner as in the epitaxial wafer of Experimental Example 3, except that no heat treatment was performed after the deposition of the carbon-doped epitaxial film. 18 atoms / cm 3An epitaxial wafer was prepared by forming a carbon-doped silicon epitaxial film 2 (film thickness: 5.5 μm) under the same conditions as in Experimental Example 1, and this was used as a base wafer. Separately, a silicon wafer was prepared as a bond wafer, in which an oxide film with a thickness of 400 nm was formed as a dielectric layer 7 on the surface of a silicon single crystal substrate 6 with a diameter of 300 mm. Next, the surface of the carbon-doped silicon epitaxial film 2 of the base wafer was bonded to the oxide film surface (surface of the dielectric layer 7) of the bond wafer, and the silicon single crystal substrate 6 on the bond wafer side was polished to obtain an SOI wafer with 1 μm of the silicon single crystal film remaining.
[0085] The single crystal layer of these SOI wafers of (Experimental Example 3) and (Experimental Example 4) was polished and removed to expose the oxide film layer, after which an aluminum electrode with a line length of 2200 μm was formed on the oxide film, and the second harmonic characteristics were measured in the same manner as in Experimental Example 1. As a result, it was found that (Experimental Example 3) was about -1 dB better than (Experimental Example 4). From the above results, it was found that when the carbon atom concentration of the carbon-doped silicon epitaxial film was increased to 2×10 as shown in (Experimental Example 3), 18 atoms / cm 3 More than 2×10 19 atoms / cm 3 It has been found that by setting the thickness of the silicon epitaxial film 3 at less than 100 nm and fabricating an SOI wafer 8 having a silicon epitaxial film 3 in which carbon defects are formed by heat treatment, an SOI wafer 8 having excellent high frequency characteristics can be obtained.
[0086] The present invention is not limited to the above-mentioned embodiment. The above-mentioned embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention. [Explanation of symbols]
[0087] Reference Signs List 1, 6: silicon single crystal substrate, 2: carbon-doped silicon epitaxial film, 3: silicon epitaxial film having carbon defects formed therein, 4: first substrate, 5: second substrate, 7: dielectric layer, 8: SOI wafer, 9: thinned silicon single crystal film (silicon single crystal film), 10: silicon epitaxial film having white defects formed therein. S1, S2, S3, S4... steps.
Claims
1. An epitaxial wafer having a silicon epitaxial film on a silicon single crystal substrate having a resistivity of 10 Ω cm or more and 5000 Ω cm or less, wherein the carbon atom concentration in the silicon epitaxial film is 5×10 17 atoms / cm 3 Above 2 x 10 19 atoms / cm 3 and carbon defects are formed in the silicon epitaxial film.
2. 2. The epitaxial wafer according to claim 1, wherein the epitaxial wafer is a wafer for a high frequency device.
3. 2. An SOI wafer having a structure in which a dielectric layer and a silicon single crystal film are formed in this order on the silicon epitaxial film of the epitaxial wafer according to claim 1.
4. 4. The SOI wafer according to claim 3, which is a wafer for a high frequency device.
5. A silicon single crystal substrate having a resistivity of 10 Ω cm or more and 5000 Ω cm or less is formed under reduced pressure with a carbon atom concentration of 5×10 17 atoms / cm 3 Above 2 x 10 19 atoms / cm 3 and then subjecting the resulting silicon epitaxial film to a heat treatment at a temperature of 900° C. or higher and 1100° C. or lower for a time period of 1 hour or higher and 36 hours or shorter, thereby forming carbon defects in the silicon epitaxial film.
6. 6. The method for producing an epitaxial wafer according to claim 5, wherein the epitaxial wafer is a wafer for a high frequency device.
7. 6. A method for producing an SOI wafer, comprising: producing an epitaxial wafer by the method according to claim 5; and bonding a silicon epitaxial film of the epitaxial wafer to a silicon single crystal substrate having a dielectric layer formed on a surface thereof, via the dielectric layer.
8. 8. The method for producing an SOI wafer according to claim 7, wherein the SOI wafer is a wafer for a high frequency device.
Citation Information
Patent Citations
Manufacture of semiconductor device
JP1983103124A
Low defect epitaxial semiconductor substrate having gettering function, image sensor using the same, and fabrication method thereof
JP2007036250A
Epitaxial silicon wafer and method of manufacturing the same
JP2010199225A
Manufacturing method of epitaxial silicon wafer and epitaxial silicon wafer
JP2020155679A
Method for manufacturing epitaxial wafer
JP7416171B1
Cited By
SOI wafer and method for manufacturing same
WO2025041594A1