Ethylene-based copolymer, composition comprising copolymer and use thereof

The ethylene copolymer composition, using ethylene, 1-butene, and non-conjugated polyene with specific ratios and metallocene catalysts, addresses adhesion and moldability issues in conventional copolymers, enhancing adhesive strength and suitability for industrial belts.

JP2024134866APending Publication Date: 2024-10-04MITSUI CHEMICALS INC
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2023045290
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Conventional ethylene/α-olefin/nonconjugated polyene copolymers face issues with poor adhesion to synthetic fibers and inadequate moldability, particularly in applications requiring high adhesive strength and industrial belts.

Method used

An ethylene copolymer composition comprising ethylene, 1-butene, an aromatic vinyl compound, and a non-conjugated polyene, with specific molecular content ratios and intrinsic viscosity, enhanced by a metallocene catalyst and crosslinking agents, to improve adhesion and moldability.

Benefits of technology

The ethylene copolymer composition exhibits high adhesive strength, excellent moldability, and suitable for industrial belts, with improved adhesion to fiber materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134866000001
    Figure 2024134866000001
  • Figure 2024134866000002
    Figure 2024134866000002
  • Figure 2024134866000003
    Figure 2024134866000003
Patent Text Reader

Abstract

To provide an ethylene-based copolymer composition suitable for an industrial belt or the like by developing an ethylene-based copolymer having high adhesive force and excellent molding processability.SOLUTION: There is provided an ethylene-based copolymer (L) composed of ethylene [A], 1-butene [B], an aromatic vinyl compound [C] and a non-conjugated polyene [D] which satisfies the following requirements (1) to (4). (1) The content of a structural unit derived from ethylene [A] is 50 to 80 mol% when the total of the structural units of [A], [B], [C] and [D] is defined as 100 mol%. (2) The content of a structural unit derived from the aromatic vinyl compound [C] is 0.1 to 5.0 mol% when the total of the structural units of [A], [B], [C] and [D] is defined as 100 mol%. (3) The content of a structural unit derived from the non-conjugated polyene [D] is 0.5 to 4.0 mol% when the total of the structural units of [A], [B], [C] and [D] is defined as 100 mol. (4) The intrinsic viscosity [η] is in the range of 0.5 to 2.5 dl / g.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a crosslinkable ethylene-based copolymer, a composition containing the copolymer, a laminate using the composition and a layer containing a fiber material, and uses thereof. [Background technology]

[0002] Ethylene-α-olefin-non-conjugated polyene copolymers such as EPDM generally have excellent weather resistance, heat resistance, and ozone resistance, and are used in industrial automotive parts, industrial rubber products, electrical insulation materials, civil engineering and construction materials, rubberized fabrics, and more.

[0003] Conventional ethylene-α-olefin-non-conjugated polyene copolymers have the disadvantage of inferior adhesion to synthetic fibers compared to polar rubbers such as nitrile rubber, chloroprene rubber, and chlorosulfonated polyethylene. As a method to solve this drawback, it has been disclosed that an adhesive solution of a chlorosulfonated copolymer is used to improve the adhesion between ethylene-α-olefin-non-conjugated polyene copolymer and synthetic fibers (Patent Document 1).

[0004] On the other hand, as an ethylene-based copolymer that can be applied to cross-linked rubber and the like having excellent mechanical properties by improving the roll processability and low-temperature setting properties, which are problems of ethylene-α-olefin-non-conjugated polyene copolymers, an ethylene-based copolymer has been proposed which is a random copolymer consisting of ethylene, α-olefin, aromatic vinyl compound and non-conjugated diene, in which the molar ratio of ethylene to α-olefin is in the range of 30 / 70 to 90 / 10, the aromatic vinyl compound content is in the range of 0.01 to 30 mol %, the non-conjugated diene content is in the range of 0.1 to 30 mol %, and the Mooney viscosity at 100°C is 15 to 150 (Patent Document 2).

[0005] However, in today's world where environmental issues such as non-halogenation are a concern, it is difficult to say that such adhesive technology that utilizes the polarity of halogenation is optimal. Also, a conventional adhesive method is known in which synthetic fibers are treated with resorcinol-formaldehyde latex (RFL) and then embedded in rubber to crosslink and adhere. More specifically, a method is known in which isocyanates or isocyanuric acid derivatives are used in the RFL treatment. However, even if these methods are applied to rubbers that use ethylene-α-olefin-non-conjugated polyene copolymers, it is difficult to obtain sufficient adhesion. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Special Publication No. 42-23632 [Patent Document 2] Japanese Patent Application Publication No. 8-134140 Summary of the Invention [Problem to be solved by the invention]

[0007] According to the study by the present inventors, the ethylene-1-butene-non-conjugated polyene copolymer was used. In the case of the copolymer, the adhesive strength between sheets formed from a composition for a transmission belt containing the copolymer ( The object of the present invention is to improve the adhesiveness of the adhesive. The present invention aims to develop an ethylene copolymer having high strength and excellent moldability, and to obtain an ethylene copolymer composition suitable for industrial belts and the like. [Means for solving the problem]

[0008] The present invention relates to the following [1] to [7]. [1] An ethylene-based copolymer (L) consisting of ethylene [A], 1-butene [B], an aromatic vinyl compound [C], and a non-conjugated polyene [D], which satisfies the following requirements (1) to (4): (1) The content of structural units derived from ethylene [A] is 50 to 80 mol % relative to 100 mol % of the total of the structural units [A], [B], [C] and [D]. (2) The content of the structural unit derived from the aromatic vinyl compound [C] is 0.1 to 5.0 mol % relative to 100 mol % of the total of the structural units [A], [B], [C] and [D]. (3) The content of the structural unit derived from the non-conjugated polyene [D] is 0.5 to 4.0 mol % relative to 100 mol % of the total of the structural units [A], [B], [C] and [D]. (4) The intrinsic viscosity [η] is in the range of 0.5 to 2.5 dl / g. [2] The ethylene copolymer (L) according to item [1], wherein the aromatic vinyl compound [C] is styrene. [3] An ethylene-based copolymer composition comprising the ethylene-based copolymer (L) according to item [1] or [2] and a crosslinking agent (M). [4] A laminate in which a layer [I] made of the ethylene copolymer composition according to item [3] is in contact with a layer [II] containing a fiber material. [5] Item [4] The laminate according to item [4], wherein the fiber material of the layer [II] is canvas. [6] The laminate according to item [4], wherein the fiber material of the layer [II] contains RFL-treated fiber. [7] An industrial belt comprising the laminate according to item [4]. Effect of the Invention

[0009] The ethylene copolymer (L) of the present invention and compositions thereof have high adhesive strength and are therefore excellent in moldability when producing laminates, and are therefore suitable for producing industrial belts and the like. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] <Ethylene-based copolymer (L)> The ethylene-based copolymer (L) of the present invention is an ethylene-based copolymer (L) consisting of ethylene [A], 1-butene [B], an aromatic vinyl compound [C], and a non-conjugated polyene [D], which satisfies the following requirements (1) to (4):

[0011] The ethylene-based copolymer (L) of the present invention is also called an ethylene-1-butene-aromatic vinyl compound-non-conjugated polyene copolymer, and contains structural units derived from 1-butene [B] in addition to structural units derived from ethylene [A], aromatic vinyl compound [C], and non-conjugated polyene [D], and therefore has good low-temperature flexibility and cold resistance.

[0012] <Requirement (1)> The content of the structural unit derived from ethylene [A] is in the range of 50 to 80 mol %, preferably 55 to 80 mol %, more preferably 60 to 80 mol %, and even more preferably 65 to 75 mol %, relative to 100 mol % of the total of the structural units [A], [B], [C] and [D].

[0013] <Requirement (2)> The content of the structural unit derived from the aromatic vinyl compound [C] is in the range of 0.1 to 5.0 mol %, preferably 0.5 to 5.0 mol %, and more preferably 1.0 to 5.0 mol %, relative to 100 mol % of the total of the structural units [A], [B], [C] and [D].

[0014] Since the ethylene-based copolymer (L) of the present invention contains structural units derived from the aromatic vinyl compound [C] in the above amount, it has good low-temperature flexibility and cold resistance and is more adhesive. Furthermore, a composition containing the ethylene-based copolymer (L) also has excellent adhesion to other materials.

[0015] <Aromatic vinyl compounds [C]> Specific examples of the aromatic vinyl compound [C] include styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, o,p-dimethylstyrene, o-ethylstyrene, m-ethylstyrene, p-ethylstyrene, o-chlorostyrene, p-chlorostyrene, and α-methylstyrene.

[0016] These aromatic vinyl compounds [C] can be used alone or in combination of two or more kinds. Of these, styrene is preferred.

[0017] <Requirement (3)> The content of the structural unit derived from the non-conjugated polyene [D] is in the range of 0.5 to 4.0 mol %, preferably 1.0 to 4.0 mol %, and more preferably 1.0 to 3.0 mol %, relative to 100 mol % of the total of the structural units [A], [B], [C] and [D]. Since the ethylene copolymer (L) of the present invention contains the structural units derived from the non-conjugated polyene [D] in the above amount, it has excellent crosslinkability, and the resulting copolymer has good mechanical properties.

[0018] <Non-conjugated polyene [D]> Specific examples of the non-conjugated polyene [D] include linear non-conjugated dienes such as 1,4-hexadiene, 1,6-octadiene, 2-methyl-1,5-hexadiene, 6-methyl-1,5-heptadiene, and 7-methyl-1,6-octadiene; cyclohexadiene, dicyclopentadiene, methyltetrahydroindene, 5-vinyl-2-norbornene, 5-ethylidene-2-norbornene, 5-methylene-2-norbornene, and 5-isopropylidene-2-norbornene. cyclic non-conjugated dienes such as norbornene and 6-chloromethyl-5-isopropenyl-2-norbornene; and trienes such as 2,3-diisopropylidene-5-norbornene, 2-ethylidene-3-isopropylidene-5-norbornene, 2-propenyl-2,5-norbornadiene, 1,3,7-octatriene, 1,4,9-decatriene, 4,8-dimethyl-1,4,8-decatriene, and 4-ethylidene-8-methyl-1,7-nonadiene.

[0019] These non-conjugated polyenes [D] can be used alone or in combination of two or more kinds. Among these, linear non-conjugated dienes such as 1,4-hexadiene, and cyclic non-conjugated dienes such as 5-ethylidene-2-norbornene, 5-ethylidene-2-norbornene, and 5-vinyl-2-norbornene are preferred, and among these, cyclic non-conjugated dienes are preferred, with 5-ethylidene-2-norbornene and 5-vinyl-2-norbornene being particularly preferred.

[0020] <Requirement (4)> The intrinsic viscosity [η] is in the range of 0.5 to 2.5 dl / g, preferably 1.0 to 2.5 dl / g, and more preferably 1.3 to 2.3 dl / g. The ethylene copolymer (L) of the present invention has an intrinsic viscosity [η] within the above range, and therefore has excellent moldability, and the resulting copolymer has good mechanical properties.

[0021] <Production method of ethylene copolymer (L)> The ethylene copolymer (L) of the present invention can be obtained by various known production methods, for example, a conventionally known production method using a metallocene catalyst.

[0022] When producing the ethylene copolymer (L) of the present invention, the ethylene [A], 1-butene [B], aromatic vinyl compound [C], and non-conjugated polyene [D] may each be derived from biomass.

[0023] Examples of metallocene catalysts that can be used in the production of the ethylene copolymer (L) of the present invention include compounds represented by the following general formula (X). [Main catalyst]

[0024] [ka]

[0025] [In formula (X), R′ and R″ each independently represent a hydrogen atom or a hydrocarbyl group having 1 to 20 carbon atoms, M represents titanium, and Y represents —NR * - and Z * Ha-SiR * 2 - and the two R * each independently represents a hydrogen atom or a hydrocarbyl group having 1 to 20 carbon atoms, one of p and q is 0 and the other is 1, When p is 0 and q is 1, M is in the +2 oxidation state and X' is 1,4-diphenyl-1,3-butadiene or 1,3-pentadiene; When p is 1 and q is 0, M is in the +3 oxidation state and X is 2-(N,N-dimethylamino)benzyl.

[0026] As the compound having a structure represented by the general formula (X), from the viewpoint of suppressing fogging and stickiness due to ultra-low molecular weight components of the obtained ethylene copolymer, (t-butylamido)dimethyl (η 5 -2-Methyl-s-indacen-1-yl)silanetitanium(II) 1,3-pentadiene (synonym: (t-butylamido)dimethyl(η 5 Particularly preferred is silanetitanium (II) 1,3-pentadiene (2-methyl-s-indacen-1-yl) (a compound having a structure represented by the following formula (XI)). The compound having a structure represented by the following formula (XI) can be obtained by the method described in JP-A-2001-522398, for example.

[0027] [ka]

[0028] The compound having the structure represented by the general formula (X) has excellent polymerizability of at least one type of polyene and / or cyclic olefin [C]. The ethylene copolymer (L) of the present invention synthesized using such a metallocene catalyst is a copolymer having a narrow molecular weight distribution and composition distribution and a uniform molecular structure. Therefore, the copolymer composition containing the ethylene copolymer (L) of the present invention and the molded article obtained from the composition tend to have excellent surface appearance.

[0029] [Co-catalyst] The ethylene copolymer (L) of the present invention can be synthesized, for example, by using the above metallocene catalyst as a main catalyst and a boron compound and / or an organoaluminum compound such as trialkylaluminum as a cocatalyst.

[0030] Examples of the boron-based compound include trityl tetrakis(pentafluorophenyl)borate, trimethylammonium tetrakis(pentafluorophenyl)borate, di(hydrogenated tallow alkyl)methylammonium tetrakis(pentafluorophenyl)borate, triethylammonium tetrakis(pentafluorophenyl)borate, tripropylammonium tetrakis(pentafluorophenyl)borate, tri(n-butyl)ammonium tetrakis(pentafluorophenyl)borate, tri(s-butyl)ammonium tetrakis(pentafluorophenyl)borate, N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate, N,N-dimethylanilinium n-butyl tris(pentafluorophenyl)borate, N,N-dimethylanilinium benzyl tris(pentafluorophenyl)borate, N,N-dimethylanilinium tetrakis(4-(t-butyldimethylsilyl)-2,3,5,6-tetra ... ammonium tetrakis(4-(triisopropylsilyl)-2,3,5,6-tetrafluorophenyl)borate, N,N-dimethylanilinium pentafluorophenoxytris(pentafluorophenyl)borate, N,N-diethylanilinium tetrakis(pentafluorophenyl)borate, N,N-dimethyl-2,4,6-trimethylanilinium tetrakis(pentafluorophenyl)borate, trimethylammonium tetrakis(2,3,4,6-tetrafluorophenyl)borate, triethyl tripropylammonium tetrakis(2,3,4,6-tetrafluorophenyl)borate, N,N-dimethylanilinium tetrakis(2,3,4,6-tetrafluorophenyl)borate, N,N-diethylanilinium tetrakis(2,3,4,6-tetrafluorophenyl)borate and N,N-dimethyl-2,4,6-trimethylanilinium tetrakis(2,3,4,6-tetrafluorophenyl)borate; dialkylammonium salts such as di(isopropyl)ammonium tetrakis(pentafluorophenyl)borate, tri(n-butyl)ammonium tetrakis(2,3,4,6-tetrafluorophenyl)borate, dimethyl(t-butyl)ammonium tetrakis(2,3,4,6-tetrafluorophenyl)borate, and dicyclohexylammonium tetrakis(pentafluorophenyl)borate; trisubstituted phosphonium salts such as triphenylphosphonium tetrakis(pentafluorophenyl)borate, tri(o-tolyl)phosphonium tetrakis(pentafluorophenyl)borate, and tri(2,6-dimethylphenyl)phosphonium tetrakis(pentafluorophenyl)borate; disubstituted oxonium salts such as diphenyloxonium tetrakis(pentafluorophenyl)borate, di(o-tolyl)oxonium tetrakis(pentafluorophenyl)borate, and di(2,6-dimethylphenyl)oxonium tetrakis(pentafluorophenyl)borate; Included are disubstituted sulfonium salts such as diphenylsulfonium tetrakis(pentafluorophenyl)borate, di(o-tolyl)sulfonium tetrakis(pentafluorophenyl)borate, and bis(2,6-dimethylphenyl)sulfonium tetrakis(pentafluorophenyl)borate.

[0031] Examples of the organoaluminum compound include trialkylaluminums such as trimethylaluminum, triethylaluminum, triisobutylaluminum, and tri-n-octylaluminum, tricycloalkylaluminums, isobutylaluminum dichloride, diethylaluminum chloride, ethylaluminum dichloride, ethylaluminum sesquichloride, methylaluminum dichloride, dimethylaluminum chloride, diisobutylaluminum hydride, LiAl(C 2 H 5 ) 4 , LiAl(C 7 H 15 ) 4Further examples include organoaluminum oxy compounds.

[0032] The organoaluminum oxy-compound may be a conventionally known aluminoxane, or may be a benzene-insoluble organoaluminum oxy-compound such as those exemplified in JP-A-2-78687.

[0033] <Crosslinking agent (M)> The crosslinking agent (M) (hereinafter also referred to as "vulcanizing agent"), which is one of the components contained in the ethylene copolymer composition of the present invention, includes crosslinking agents generally used in crosslinking rubber, such as organic peroxides, phenolic resins, sulfur-based compounds, hydrosilicone-based compounds, amino resins, quinones or their derivatives, amine-based compounds, azo-based compounds, epoxy-based compounds, isocyanate-based compounds, etc. Among these, organic peroxides and sulfur-based compounds are preferred.

[0034] <Organic peroxide> Examples of organic peroxides include dicumyl peroxide (DCP), di-tert-butyl peroxide, 2,5-di-(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexyne-3, 1,3-bis(tert-butylperoxyisopropyl)benzene, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, n-butyl-4,4-bis(tert-butylperoxy)valerate, benzoyl peroxide, p-chlorobenzoyl peroxide, 2,4-dichlorobenzoyl peroxide, tert-butyl peroxybenzoate, ert-butylperoxyisopropyl carbonate, diacetyl peroxide, lauroyl peroxide, and tert-butylcumyl peroxide.

[0035] When an organic peroxide is used as the crosslinking agent (M), the blending amount in the copolymer composition is generally 0.1 to 20 parts by mass, preferably 0.2 to 15 parts by mass, and more preferably 0.5 to 10 parts by mass, based on 100 parts by mass of the ethylene-based copolymer (L). When the blending amount of the organic peroxide is within the above range, there is no bloom on the surface of the obtained molded article, and the ethylene-based copolymer composition exhibits excellent crosslinking properties, which is preferable.

[0036] <Crosslinking aid> When an organic peroxide is used as a crosslinking agent, it is preferable to use a crosslinking assistant in combination. Examples of the crosslinking assistant include sulfur; quinone dioxime crosslinking assistant such as p-quinone dioxime; acrylic crosslinking assistant such as ethylene glycol dimethacrylate and trimethylolpropane trimethacrylate; allyl crosslinking assistant such as diallyl phthalate and triallyl isocyanurate; maleimide crosslinking assistant; divinylbenzene; and metal oxides such as zinc oxide (e.g., ZnO#1 / zinc oxide type 2 (JIS standard (K-1410)), manufactured by Hakusui Tech Co., Ltd.), magnesium oxide, and activated zinc oxide (e.g., zinc oxide such as "META-Z102" (trade name; manufactured by Inoue Seki Kogyo Co., Ltd.)).

[0037] When a crosslinking aid is used, the amount of the crosslinking aid in the ethylene copolymer composition is usually 0.5 to 10 mol, preferably 0.5 to 7 mol, more preferably 1 to 6 mol, per mol of the organic peroxide.

[0038] <Sulfur compounds> Examples of sulfur-based compounds include sulfur, sulfur chloride, sulfur dichloride, morpholine disulfide, alkylphenol disulfide, tetramethylthiuram disulfide, and selenium dithiocarbamate.

[0039] When a sulfur-based compound is used as a crosslinking agent, the blending amount in the copolymer composition is usually 0.1 to 10 parts by mass, preferably 0.2 to 7.0 parts by mass, and more preferably 0.3 to 5.0 parts by mass, based on 100 parts by mass of the ethylene-based copolymer (L). When the blending amount of the sulfur-based compound is within the above range, there is no bloom on the surface of the obtained molded article, and the ethylene-based copolymer composition shows excellent crosslinking properties.

[0040] <Vulcanization accelerator> When a sulfur-based compound is used as the crosslinking agent, it is preferable to use a vulcanization accelerator in combination. Examples of the vulcanization accelerator include N-cyclohexyl-2-benzothiazole sulfenamide, N-oxydiethylene-2-benzothiazole sulfenamide, N,N'-diisopropyl-2-benzothiazole sulfenamide, 2-mercaptobenzothiazole (e.g., Suncerer M (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)), 2-(4-morpholinodithio)benzothiazole (e.g., Noccelaer MDB-P (trade name; manufactured by Ouchi Shinko Chemical Industry Co., Ltd.)), 2-(2,4-dinitrophenyl)mercaptobenzothiazole, 2-(2,6-dinitrophenyl)mercaptobenzothiazole, Thiazole-based vulcanization accelerators such as ethyl-4-morpholinothio)benzothiazole and dibenzothiazyl disulfide (for example, Sancerer DM (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)); guanidine-based vulcanization accelerators such as diphenyl guanidine, triphenyl guanidine, and diorthotolyl guanidine; aldehyde amine-based vulcanization accelerators such as acetaldehyde-aniline condensation product and butyraldehyde-aniline condensation product; imidazoline-based vulcanization accelerators such as 2-mercaptoimidazoline; tetramethylthiuram monosulfide (for example, Sancerer DM (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)); thiuram-based vulcanization accelerators such as tetramethylthiuram disulfide (e.g., Sancerer TS (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)), tetramethylthiuram disulfide (e.g., Sancerer TT (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)), tetraethylthiuram disulfide (e.g., Sancerer TET (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)), tetrabutylthiuram disulfide (e.g., Sancerer TBT (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)), and dipentamethylenethiuram tetrasulfide (e.g., Sancerer TRA (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)); zinc dimethyldithiocarbamate, diethyldithio Examples of such vulcanization accelerators include dithioacid salt vulcanization accelerators such as zinc carbamate, zinc dibutyldithiocarbamate (e.g., Sancerar PZ, Sancerar BZ, and Sancerar EZ (trade names; manufactured by Sanshin Chemical Industry Co., Ltd.)) and tellurium diethyldithiocarbamate; thiourea vulcanization accelerators such as ethylenethiourea (e.g., Sancerar BUR (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.), Sancerar 22-C (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)), N,N'-diethylthiourea, and N,N'-dibutylthiourea; and xanthate vulcanization accelerators such as zinc dibutylxatogenate.

[0041] When a vulcanization accelerator is used, the blending amount of the vulcanization accelerator in the copolymer composition is generally 0.1 to 20 parts by mass, preferably 0.2 to 15 parts by mass, and more preferably 0.5 to 10 parts by mass, based on 100 parts by mass of the ethylene-based copolymer (L). When the blending amount of the vulcanization accelerator is within the above range, the copolymer composition exhibits excellent crosslinking properties without blooming on the surface of the obtained molded article. When a sulfur-based compound is used as a crosslinking agent, a vulcanization assistant can be used in combination.

[0042] Examples of the vulcanization aid include zinc oxide (e.g., ZnO#1 and zinc oxide type 2, manufactured by Hakusui Tech Co., Ltd.), magnesium oxide, and activated zinc oxide (e.g., zinc oxide such as "META-Z102" (trade name, manufactured by Inoue Seki Kogyo Co., Ltd.)). When a vulcanization aid is used, the blending amount of the vulcanization aid in the ethylene-based copolymer composition is usually 1 to 20 parts by mass based on 100 parts by mass of the ethylene-based copolymer (L).

[0043] <Ethylene-based copolymer composition> The ethylene-based copolymer composition of the present invention and the ethylene-based copolymer composition forming the layer [I] of the laminate of the present invention are compositions containing the above ethylene-based copolymer (L) and the above crosslinking agent (M), and preferably contain the above crosslinking agent (M) in an amount of 0.1 to 20 parts by mass, more preferably 0.2 to 15 parts by mass, and even more preferably 0.5 to 10 parts by mass, per 100 parts by mass of the above ethylene-based copolymer (L).

[0044] When the blending amount of the crosslinking agent (M) is within the above range, no bloom occurs on the surface of the obtained molded article, and the ethylene copolymer composition exhibits excellent crosslinking properties, which is suitable. The ethylene-based copolymer composition of the present invention contains a crosslinking agent (M) in addition to the ethylene-based copolymer (L), and therefore has good adhesion to other materials, for example layers containing fibrous materials such as industrial belts, and a crosslinked laminate has excellent adhesive strength with layers containing fibrous materials.

[0045] In addition to the ethylene copolymer (L) and the crosslinking agent (M), the ethylene copolymer composition of the present invention may contain other components according to the desired purpose within the range that does not impair the effects of the present invention. The other components may contain, for example, at least one selected from polymers other than the ethylene copolymer (L), specifically, elastomers such as EPDM, natural rubber, isoprene rubber, butadiene rubber, styrene-butadiene rubber, chloroprene rubber, nitrile rubber, butyl rubber, acrylic rubber, and silicone rubber, POM, fillers, softeners, antioxidants, processing aids, activators, heat stabilizers, weather stabilizers, antistatic agents, colorants, lubricants, and thickeners. Also. Each additive may be used alone or in combination of two or more.

[0046] Filler The filler constituting the ethylene copolymer composition of the present invention is a known rubber reinforcing agent blended into a rubber composition, and is usually an inorganic substance called carbon black or an inorganic reinforcing agent.

[0047] Specific examples of the filler used in the present invention include Asahi #55G and Asahi #60UG (both manufactured by Asahi Carbon Co., Ltd.), Seast (V, SO, 116, 3, 6, 9, SP, TA, etc.) carbon black (manufactured by Tokai Carbon Co., Ltd.), these carbon blacks which have been surface-treated with a silane coupling agent or the like, as well as silica, activated calcium carbonate, finely divided talc, finely divided silicic acid, light calcium carbonate, heavy calcium carbonate, talc, clay, and the like.

[0048] These fillers may be used alone or in combination of two or more. As the filler in the present invention, preferably used are carbon black, light calcium carbonate, heavy calcium carbonate, talc, clay, silica, etc.

[0049] When the copolymer composition of the present invention contains a filler, the filler may be blended in an amount of usually 0.5 to 300 parts by mass, preferably 0.5 to 250 parts by mass, per 100 parts by mass of the ethylene copolymer (L).

[0050] <Softener> Examples of the softener that may be contained in the copolymer composition for conveyor belts of the present invention include petroleum-based softeners such as process oil, lubricating oil, paraffin oil, liquid paraffin, petroleum asphalt, and Vaseline; coal tar-based softeners such as coal tar; fatty oil-based softeners such as castor oil, linseed oil, rapeseed oil, soybean oil, and coconut oil; waxes such as beeswax and carnauba wax; naphthenic acid, pine oil, rosin or derivatives thereof; synthetic polymer substances such as terpene resins, petroleum resins, and coumarone-indene resins; ester-based softeners such as dioctyl phthalate and dioctyl adipate; and other softeners such as microcrystalline wax, liquid polybutadiene, modified liquid polybutadiene, hydrocarbon-based synthetic lubricating oils, tall oil, and sub(factice). Of these, petroleum-based softeners and hydrocarbon-based synthetic lubricating oils are preferred, and process oil and liquid ethylene-propylene copolymer are particularly preferred.

[0051] Liquid ethylene-propylene copolymer The liquid ethylene-propylene copolymer particularly preferred as the softening agent in the present invention has a dynamic viscosity of 1 to 80,000 mm at 40°C. 2 / s is preferred.

[0052] Dynamic viscosity at 40℃ is 1mm 2 Ethylene-propylene copolymers with a viscosity of less than 80,000 mm / s contain a large amount of low molecular weight components that are easily volatile, which may result in a deterioration in the heat resistance of the resulting ethylene copolymer composition. 2 If the ratio exceeds 1 / s, the amount of high molecular weight components increases, which may result in insufficient viscosity, and the effect of improving the tackiness of the resulting copolymer composition for a conveyor belt may be reduced.

[0053] The liquid ethylene-propylene copolymer has excellent compatibility with the ethylene-based copolymer (L), and therefore the copolymer composition containing the liquid ethylene-propylene copolymer has good adhesion. When the ethylene copolymer composition contains a softener, the blending amount of the softener is generally 2 to 100 parts by mass, preferably 10 to 100 parts by mass, based on 100 parts by mass of the ethylene copolymer (L).

[0054] When the ethylene copolymer composition contains a softener, the blending amount of the softener is generally 2 to 100 parts by mass, preferably 10 to 100 parts by mass, based on 100 parts by mass of the ethylene copolymer (L).

[0055] <Anti-aging agent (stabilizer)> By blending an antioxidant (stabilizer) with the ethylene copolymer composition of the present invention, the life of the seal packing formed therefrom can be extended. Examples of such antioxidants include conventionally known antioxidants, such as amine-based antioxidants, phenol-based antioxidants, and sulfur-based antioxidants.

[0056] Examples of the anti-aging agents include aromatic secondary amine-based anti-aging agents such as phenylbutylamine and N,N-di-2-naphthyl-p-phenylenediamine; phenol-based anti-aging agents such as dibutylhydroxytoluene and tetrakis[methylene(3,5-di-t-butyl-4-hydroxy)hydrocinnamate]methane; thioether-based anti-aging agents such as bis[2-methyl-4-(3-n-alkylthiopropionyloxy)-5-t-butylphenyl]sulfide; dithiocarbamate-based anti-aging agents such as nickel dibutyldithiocarbamate; and sulfur-based anti-aging agents such as 2-mercaptobenzoylimidazole, 2-mercaptobenzimidazole, zinc salt of 2-mercaptobenzimidazole, dilaurylthiodipropionate, and distearylthiodipropionate.

[0057] When the ethylene copolymer composition contains an antioxidant, the amount of the antioxidant is usually 0.3 to 10 parts by mass, preferably 0.5 to 7.0 parts by mass, based on 100 parts by mass of the ethylene copolymer (L). When the amount of the antioxidant is within the above range, there is no bloom on the surface of the obtained molded article, and furthermore, the occurrence of vulcanization inhibition can be suppressed.

[0058] <Processing aids> As the processing aid, a wide variety of processing aids that are generally compounded with rubber can be used.Specific examples include ricinoleic acid, stearic acid, palmitic acid, lauric acid, barium stearate, zinc stearate, calcium stearate, zinc laurate, and esters.Of these, stearic acid is preferred.

[0059] When the copolymer composition contains a processing aid, it can be appropriately blended in an amount of usually 1 to 3 parts by mass per 100 parts by mass of the ethylene copolymer (L). When the blending amount of the processing aid is within the above range, it is preferable because the processability such as kneading processability, extrusion processability, and injection moldability is excellent. The processing aid may be used alone or in combination with two or more kinds.

[0060] <Activator> Examples of the activator include amines such as di-n-butylamine, dicyclohexylamine, and monoethanolamine; activators such as diethylene glycol, polyethylene glycol, lecithin, triaryl methylate, and zinc compounds of aliphatic or aromatic carboxylic acids; zinc peroxide preparations; octadecyltrimethylammonium bromide, synthetic hydrotalcite, and special quaternary ammonium compounds.

[0061] When the copolymer composition contains an activator, the amount of the activator is usually 0.2 to 10 parts by mass, preferably 0.3 to 5 parts by mass, based on 100 parts by mass of the ethylene copolymer (L).

[0062] <Laminate> The laminate of the present invention is a laminate in which a layer [I] made of the ethylene copolymer composition of the present invention is in contact with a layer [II] containing a fibrous material.

[0063] <<Layer [I] made of ethylene-based copolymer composition>> The layer [I] made of an ethylene-based copolymer composition constituting the laminate of the present invention is preferably a layer obtained by crosslinking the above-mentioned ethylene-based copolymer composition.

[0064] <Layer containing fibrous material [II]> The layer [II] containing a fiber material that constitutes the laminate of the present invention contains a fiber material in at least a part of the layer.

[0065] <Textile materials> Examples of fiber materials forming the layer [II] of the present invention include various known fiber materials, for example, natural fibers such as cotton and wood cellulose fibers; organic fiber materials such as fibers made of synthetic resins such as polyamide, polyester, polyvinyl alcohol, rayon, polyparaphenylene benzobisoxazole, polyethylene, polypropylene, polyarylate, polyimide, polyphenylene sulfide, polyether ether ketone, polylactic acid, polycaprolactone, polybutylene succinate, and fluorine-based polymers; and inorganic fiber materials such as glass fibers, PAN-based carbon fibers, pitch-based carbon fibers, alumina fibers, silicon carbide fibers, aluminum borate fibers, and potassium titanate whiskers.

[0066] These fiber materials may be long fibers (filaments) or short fibers (staples), and may be cord yarns, spun yarns, woven fabrics, knitted fabrics, canvas, nonwoven fabrics, and the like.

[0067] Examples of the polyamide include aliphatic polyamides such as nylon 6, nylon 6,6, and nylon 6,10; semi-aromatic polyamides such as polymetaxylylene adipamide (MXD6), polyhexamethylene terephthalamide (6T), and copolymer polyamides containing these units; and fully aromatic polyamides such as polybenzamide, poly-p-phenylene terephthalamide, and poly-m-phenylene isophthalamide.

[0068] Furthermore, these fiber materials may be surface-treated by a known method such as RFL treatment in order to improve adhesion between the fiber materials themselves or between the fiber materials and the layer [I] made of the ethylene-based copolymer composition.

[0069] <RFL Processing> RFL treatment is a process in which textile materials are treated with a treatment liquid (RFL liquid) containing resorcinol, formalin, and latex, and this RFL liquid is a mixture of the initial condensation product of resorcinol and formalin and rubber latex. Examples of rubber latex that can be used include styrene-butadiene-vinylpyridine terpolymer (VP), styrene-butadiene copolymer (SBR), chloroprene (CR), acrylonitrile-butadiene copolymer (NBR), hydrogenated NBR (H-NBR), chlorosulfonated ethylene (CSM), and natural rubber. These can be used alone or in a blend of two or more types.

[0070] <Method of manufacturing laminate> To manufacture the laminate of the present invention, various known methods for manufacturing laminates can be adopted. For example, a method of laminating a layer [I] of an uncrosslinked ethylene copolymer composition previously manufactured (molded) by a known method with a layer [II] containing a fiber material, a method of crosslinking the layer [I] of an ethylene copolymer composition after laminating, a method of laminating a layer [I] of a crosslinked ethylene copolymer composition with a layer [II] containing a fiber material, a method of extrusion coating the layer [I] of an ethylene copolymer composition on the layer [II] containing a fiber material, a method of extrusion coating the layer [I] of an ethylene copolymer composition, and a method of crosslinking the layer [I] of an ethylene copolymer composition after extrusion coating can be adopted.

[0071] The layer [I] made of the ethylene copolymer composition can be produced by various known methods. The ethylene copolymer composition can be obtained by kneading the ethylene-α-olefin-non-conjugated polyene copolymer (L), the crosslinking agent (M), and, if necessary, additives such as a filler, a softener, an antioxidant, and a processing aid, using various known kneading and mixing devices, for example, a Banbury mixer, a kneader, an internal mixer (internal mixer) such as an Intermix, a roll, and the like.

[0072] The uncrosslinked ethylene-based copolymer composition obtained by kneading may be molded into an intended shape by various molding methods such as an extrusion molding machine, a calendar roll, a press, an injection molding machine, or a transfer molding machine, and then crosslinked to form a layer [I] consisting of the ethylene-based copolymer composition, which may then be laminated (bonded) with a layer [II] containing a fiber material; alternatively, the uncrosslinked ethylene-based copolymer composition may be molded into an intended shape by the above-mentioned method, and then laminated (bonded) with a layer [II] containing a fiber material, thereby crosslinking the composition.

[0073] The layer [I] made of the ethylene copolymer composition may be crosslinked by heating using a crosslinking agent or by irradiating with light, gamma rays or electron beams. In addition, when crosslinking, a mold may be used, or crosslinking may be performed without using a mold. When a mold is not used, the molding and crosslinking steps are usually performed continuously. As a heating method in the crosslinking tank, a heating tank using hot air, a glass bead fluidized bed, UHF (ultra-high frequency electromagnetic waves), steam, etc. may be used.

[0074] <<Applications of the laminate>> A laminate in which a layer [I] made of the ethylene-based copolymer composition of the present invention is in contact with a layer [II] containing a fiber material is suitably used for automobile hoses, water hoses, and gas hoses; industrial belts such as transmission belts and conveyor belts; and escalator handrails.

[0075] Examples of the automobile hose include brake hoses, radiator hoses, heater hoses, and air cleaner hoses. Examples of the transmission belt include a V-belt, a flat belt, a toothed belt, etc. Examples of the conveyor belt include a light conveyor belt, a cylindrical belt, a rough top belt, a conveyor belt with flanges, a conveyor belt with a U-shaped guide, a conveyor belt with a V-guide, etc. EXAMPLES

[0076] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these.

[0077] Example 1 [Production of ethylene-1-butene-styrene-ENB copolymer (L-1)] Dehydrated and purified n-hexane (C6) was fed at a rate of 1880 mL / h to one of the feed ports of a 0.95 L continuous polymerization reactor, and [N-(1,1-dimethylethyl)-1,1-dimethyl-1-[(1,2,3,3A,8A-η)-1,5,6,7-tetrahydro-2-methyl-S-indacene-1-yl]silane aminate (2-)-κN][(1,2,3,4-η)-1,3-pentadiene]-titanium (catalyst A) and triphenylcarbenium were fed from the other feed port. Tetrakis(pentafluorophenyl)borate catalyst B) and a hexane solution of triisobutylaluminum (TiBA) (zirconium concentration of catalyst A: 0.250 mmol / L, catalyst B: 1.200 mmol / L, aluminum concentration of TiBA: 10.0 mmol / L) were continuously fed at rates of 155 mL / h, 160 mL / h, and 100 mL / h, respectively, 1-butene at 183 g / h, styrene at 199 g / h, and 5-ethylidene-2-norbornene (ENB) at 55 g / h.

[0078] At the same time, continuous solution polymerization was carried out under conditions of 82.6 g / h of ethylene (C2") through another supply inlet of the polymerization vessel, a polymerization temperature of 87.3°C, a total pressure of 3.6 MPaG, and a residence time of 18.3 minutes. When the copolymerization reaction was carried out under the above conditions, ethylene-1-butene-styrene-ENB copolymer was obtained in a homogeneous solution state.

[0079] After that, a small amount of methanol was added to the copolymer solution continuously withdrawn from the top of the polymerization vessel to terminate the polymerization reaction, and the mixture was vacuum dried at 150-180°C for 0.5 hours. The structural units derived from ethylene (ethylene content) of the obtained ethylene-1-butene-styrene-ENB copolymer (L-1) were measured by the measurement method described below. The results are shown in Table 1.

[0080] [Measurement method] The molar amount is 1 The intensity was measured using a H-NMR spectrometer. Solvent: deuterated 1,1,2,2-tetrachloroethane (TCE)-d2, measurement temperature: 120°C, observation range: 20 ppm, repetition time: 7 seconds, pulse width: 45° (6.15 μsec), using a measurement device (500.16 MHz, JEOL ECA-500 type). 1 The H-NMR spectrum was measured and calculated. The calculated content (mol %) was rounded off to one decimal place.

[0081] [Reference example 1] Reference Example 1 shows the copolymer (E-1) obtained in Production Example 1 below.

[0082] <Production Example 1> According to the description of [Synthesis Example C1] of WO 2015 / 122415, ethylene-1-butene-5-ethylidene-2-norbornene (ENB) copolymer (E-1) was obtained. The physical properties of the obtained copolymer (E-1) were measured by the method described above. The results are shown in Table 1.

[0083] [Table 1]

[0084] The physical properties of the ethylene copolymer composition were measured by the following methods. [Physical properties of ethylene copolymer composition (uncrosslinked) [Physical property test 1: Mooney viscosity] The Mooney viscosity ML(1+4)100°C of Blend 2 (compound) was measured using a Mooney viscometer (SMV-301 model, manufactured by Shimadzu Corporation) in accordance with JIS K 6300 (1994).

[0085] [Physical property test 2: Evaluation of crosslinking (vulcanization) characteristics] The vulcanization rate (tC90) of Compound 2 at 180° C. was measured using a vulcanization measuring device: MDR2000 (manufactured by ALPHA TECHNOLOGIES) as follows.

[0086] The torque change obtained under conditions of constant temperature and constant shear rate was measured. The time required to reach 90% of the difference between the maximum torque (S'Max) and the minimum torque (S'Min) was defined as tc90 (min). The measurement conditions were a temperature of 180°C and a time of 15 minutes. The smaller this tc90, the faster the vulcanization speed (crosslinking speed).

[0087] <Measurement of Adhesion> The tackiness of the uncrosslinked ethylene copolymer composition was measured by a probe tack test. The test was carried out using a tack tester (TAC-II) manufactured by Rhesca. A stainless steel cylindrical probe with a diameter of 5 mm was brought into contact with the test specimen, and the adhesive force (tack) (gf) generated when peeling was measured. The contact speed of the probe to the test specimen was 120 mm / min, the applied pressure was 50 gf, the applied pressure time was 20 seconds, the peel speed was 120 mm / min, and the temperature was 50°C.

[0088] [Example 2] [Production of ethylene copolymer composition] The copolymer (L-1) obtained in Example 1 was used, and a 6-inch roll was used to mix 100 parts by mass of the copolymer (L-1) with zinc oxide "Zinc Oxide Type 2" (trade name; manufactured by Hakusui Tech Co., Ltd.) as a vulcanization aid, stearic acid as a processing aid, carbon black "Asahi #70" (trade name; manufactured by Asahi Carbon Co., Ltd.) as a reinforcing agent, and paraffin-based process oil "Diana Process Oil PW-380" (trade name; manufactured by Idemitsu Kosan Co., Ltd.) as a softener in the amounts shown in Table 2, and then kneaded. The kneading conditions were a front roll / rear roll temperature of 50°C / 50°C, and a front roll / rear roll peripheral speed of 18 rpm / 15 rpm (kneading A).

[0089] Next, after confirming that the temperature of the above blend had reached 40°C, a peroxide "Percumyl D-40" (product name; manufactured by NOF Corporation) was added as a crosslinking agent in the blend amount shown in Table 2 and kneaded into the above blend using a 6-inch roll (kneading B).

[0090] The adhesive strength (gf) of the obtained uncrosslinked sheet having a thickness of 2 mm was measured by the method described above. The results are shown in Table 2. Next, the obtained uncrosslinked sheet having a thickness of 2 mm was pressed at 170° C. for 30 minutes using a 100-ton press molding machine to produce a crosslinked sheet. The physical properties of the obtained crosslinked sheet were measured by the methods described above. The results are shown in Table 2.

[0091] [Comparative Example 1] The same procedure as in Example 2 was repeated, except that the copolymer (F-1) obtained in Reference Example 1 was used instead of the copolymer (L-1) used in Example 2. The results are shown in Table 2.

[0092] [Table 2]

Claims

1. The ethylene-based copolymer (L) is composed of ethylene [A], 1-butene [B], an aromatic vinyl compound [C], and a non-conjugated polyene [D], and satisfies the following requirements (1) to (4): (1) The content of the structural unit derived from ethylene [A] is 50 to 80 mol %, relative to 100 mol % of the total of the structural units [A], [B], [C] and [D]. (2) The content of the structural unit derived from the aromatic vinyl compound [C] is 0.1 to 5.0 mol %, relative to 100 mol % of the total of the structural units [A], [B], [C] and [D]. (3) The content of the structural unit derived from the non-conjugated polyene [D] is 0.5 to 4.0 mol %, relative to 100 mol % of the total of the structural units [A], [B], [C] and [D]. (4) The intrinsic viscosity [η] is in the range of 0.5 to 2.5 dl / g.

2. The ethylene copolymer (L) according to claim 1, wherein the aromatic vinyl compound [C] is styrene.

3. An ethylene-based copolymer composition comprising the ethylene-based copolymer (L) according to claim 1 or 2 and a crosslinking agent (M).

4. A laminate comprising a layer [I] made of the ethylene copolymer composition according to claim 3 and a layer [II] containing a fiber material in contact with each other.

5. 5. The laminate according to claim 4, wherein the textile material of the layer [II] is canvas.

6. The laminate according to claim 4, wherein the fibrous material of the layer [II] comprises RFL-treated fibers.

7. An industrial belt comprising the laminate according to claim 4.

Citation Information

Patent Citations

  • Ethylenic quaternary copolymer rubber

    JP1996225615A

  • Polyene elastomer composition

    JP1998265625A

  • Polyene elastomer composition

    JP1998273558A

  • Olefinic elastomer composition

    JP1998273567A

  • Rubber-modified styrene resin composition and preparation thereof

    JP1998306182A