Recovery method of ferroalloy powder

The method of slurry formation, emulsification, magnetic separation, and solvent volatilization effectively addresses the inefficiencies of existing oil removal processes, achieving reduced energy use, enhanced separation, and high-purity iron alloy recovery.

JP2024135288APending Publication Date: 2024-10-04NIPPON STEEL CORPORATION
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023045906
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing methods for removing oil from oil-containing iron alloy powder are energy-intensive, require high equipment costs, emit significant carbon dioxide, and fail to effectively separate magnetic and non-magnetic substances, leading to reduced metal value and increased slag usage.

Method used

A method involving slurry formation, emulsification with a volatile hydrophobic solvent, magnetic separation, and solvent removal through volatilization, followed by classification to separate and recover high-purity iron alloy powder.

Benefits of technology

Reduces energy consumption, increases oil removal and recovery rates, and effectively separates magnetic and non-magnetic substances, resulting in high-purity iron alloy powder with minimal residual solvent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135288000001_ABST
    Figure 2024135288000001_ABST
Patent Text Reader

Abstract

To provide a recovery method of ferroalloy powder, enabling reduction of energy for removal of oil content from the ferroalloy powder and enabling increase of an oil content removal rate and a solid-liquid separation speed.SOLUTION: A method for recovering ferroalloy powder by separating oil from a mixture including oil attached thereto and including ferroalloy powder and non-magnetic matter is provided, including the following steps: a slurrying step of forming slurry by mixing the mixture with water in such a manner that the mixed matter has a viscosity in the range of 0.003 to 1.00 Pa S, thereby producing slurry; a first emulsifying step of adding a first volatile hydrophobic solvent to the slurry, and then mixing the mixture to form a first emulsion; a first magnetic separation step of separating and recovering a powder phase from the first emulsion by magnetic separation; a residual solvent removal step of volatilizing and removing the first volatile hydrophobic solvent remaining in the powder phase obtained in the first magnetic separation step; and a ferroalloy powder recovery step of separating and recovering the ferroalloy powder by wet classification from the slurry including the powder phase obtained in the residual solvent removal step.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for recovering ferroalloy powder. [Background technology]

[0002] In various manufacturing industries, including the steel manufacturing industry, large amounts of mixtures in which powders containing hydrophilic particles are dispersed in water or aqueous solutions are discharged. The mixtures are often discharged in the form of aqueous slurries. The powders contained in the mixtures are diverse, and in the steel manufacturing industry, for example, they include scale, roll grinding dust, etc.

[0003] For example, scale and roll grinding dust are contaminated with oil and moisture (e.g., rolling oil, lubricating oil, and cooling water used in rolling) that are inevitably generated during industrial production. Such scale and roll grinding dust that contain oil and moisture contain 5 to 50% moisture and a few percent oil. Therefore, for the purpose of recycling or efficient use, it is necessary to remove the oil and moisture from the ferroalloy powder such as scale and roll grinding dust.

[0004] Conventionally, a method of removing oil from an alloy ferro-powder containing oil (hereinafter also referred to as oil-containing powder) has been known to involve combustion treatment using a rotary kiln or the like. However, since the oil concentration of the oil-containing powder is low, a fuel supporting the combustion is required for the combustion treatment, which poses a problem of requiring a large amount of energy. In particular, when the oil concentration of the oil-containing powder is lower, high-grade (expensive) energy such as COG (coke oven gas) or heavy oil may be used as the fuel supporting the combustion, and in such cases, the above problem becomes more serious. Furthermore, when the powder is combusted, CO2 emissions also increase, which goes against the CO2 reduction that has become a particular issue in recent years.

[0005] Furthermore, in the case of scale with oil attached (hereinafter also referred to as oil-containing scale), the scale after combustion treatment to remove the oil is often used as an iron source in the sintering process, etc. However, during the combustion treatment, FeO (wustite) and Fe3O4 (magnetite), which are the main components in the scale, are oxidized to Fe2O3 (hematite), which causes a problem of increasing the amount of coke used in the sintering process.

[0006] In addition, the combustion process requires the use of fuel oil, which increases the running costs, and the combustion process is carried out in a furnace, which must be resistant to high temperatures, which increases the equipment costs. To separate oil from ferroalloy powder containing oil, it is necessary to remove it from the surface of the alloy powder, but the combustion process in a kiln, etc., has the problem of high running costs and equipment costs as mentioned above. Furthermore, the combustion process uses auxiliary fuel and oxidizes the components of the ferroalloy powder, which may result in a large amount of CO2 emissions, making it unsuitable for the carbon neutral era.

[0007] In addition, roll grinding dust, which contains alloy iron powder containing rare metals (Cr, Ni, Mo, V, Nb), grinding wheel powder, oil, and water, is often burned together with oil-containing scale in the rotary kiln described above to remove the oil and recover the powder, which is then recycled as an iron source. If the powder recovered from roll grinding dust is recycled as an iron source, it becomes the raw material for low-tramp element steel materials such as ordinary steel, and the rare metal components contained in the roll grinding dust become almost impossible to separate, resulting in the problem that the metallic value inherent to the rare metals cannot be utilized.

[0008] In response to such problems, various methods for separating oil from oil-containing powder without carrying out combustion treatment have been investigated.

[0009] For example, Patent Document 1 discloses a method in which an organic solvent is mixed as an extractant with oil-containing scale and stirred to extract the oil from the scale into the organic solvent, and centrifugal force is applied by utilizing the difference in specific gravity to separate the scale into a solvent phase, a water phase, and a scale phase.

[0010] Patent Document 2 discloses a method in which centrifugal force is applied to an emulsion containing scale in a liquid cyclone to separate the oil from a mixture containing oil-containing powder, and the powder is recovered.

[0011] Patent Document 3 discloses a method for filtering a grinding oil mixture containing sludge generated in a metal strip grinding line to obtain a sludge mixture containing a small amount of grinding oil.

[0012] Patent Document 4 discloses a method in which a coagulant and magnetic particles are added to an oil emulsion obtained by stirring a mixture of oil and water, the mixture is further stirred to form magnetic flocs, and then the oil and water are separated by magnetic separation.

[0013] Patent Document 5 discloses a method for recycling roll scraps, which includes a grinding scrap sorting and management step of sorting and managing the grinding scraps, which are generated when grinding a metalworking roll and contain oil and moisture, into a first grinding scrap containing Fe, Cr, Ni, and Mo but not containing W or V, and a second grinding scrap containing Fe, Cr, Ni, and Mo and also containing W or V; a grinding scrap moisture removal step of drying the first and second grinding scraps to remove moisture; a grinding scrap oil removal step of washing the first and second grinding scraps with a solvent to remove oil; and a grinding scrap metal component recovery step of putting the first and second grinding scraps into a melting furnace to recover metal components. [Prior art documents] [Patent documents]

[0014] [Patent Document 1] JP 2015-132011 A [Patent Document 2] JP 2017-177018 A [Patent Document 3] Japanese Patent Application Publication No. 7-116960 [Patent Document 4] JP 2003-277771 A [Patent Document 5] JP 2016-196671 A Summary of the Invention [Problem to be solved by the invention]

[0015] However, the method described in Patent Document 1 has a problem that it requires an expensive centrifuge. Furthermore, when performing a countercurrent continuous process described later to improve the oil removal rate, it is necessary to connect multiple extractions and phase separations with pumps and piping, and to have a control system for controlling them. This requires multiple expensive centrifuges, which is complicated and prone to operational problems.

[0016] The method described in Patent Document 2 had a problem in that, when the powder has a high content of fine particles, the recovery rate of the particles in the liquid cyclone decreases.

[0017] In addition, when filtering a slurry containing water, oil, and hydrophilic particles, the method described in Patent Document 3 frequently causes clogging of the filtering surface. Furthermore, the filtering speed is low, so the filtering device becomes very large, making stable operation difficult.

[0018] The method described in Patent Document 4 has a problem in that the oil adhering to the magnetic particles cannot be separated and the oil content cannot be reduced to a low level.

[0019] In the method described in Patent Document 5, a moisture removal step by drying is carried out before an oil removal step in which oil is removed by a solvent. In the gaps between particles constituting the roll grinding waste, water (boiling point 100°C) and oil (boiling point over 200°C) are mixed and exist. Therefore, there is a problem that the oil acts as an obstacle to evaporating the moisture, and the temperature must be several tens of degrees higher than the boiling point of water and it takes a long time. In addition, when a moisture removal step is carried out before an oil removal step as in the method described in Patent Document 5, a part of the oil often vaporizes, causing a significantly worse odor, and therefore there is a problem that an exhaust gas treatment facility is usually required.

[0020] As described above, none of the techniques disclosed in Patent Documents 1 to 5, which involve treatment without combustion treatment, can fully solve the problem of oil separation from oil-containing powder.

[0021] In light of the above, in a method for removing oil from oil-containing powder to recover high-purity powder, there is a strong demand for a method that consumes less energy when removing the oil (oil removal energy) and can recover powder with a high recovery rate.

[0022] Furthermore, when attempting to separate oil from roll grinding waste (a mixture of rare metals, grinding wheel powder, oil, and water) using a conventional process that does not involve combustion treatment, the oil can be separated, but there are cases where the alloy ferroelectric powder containing rare metals (Cr, Ni, Mo, V, Nb, etc.) and the grinding wheel components cannot be sufficiently separated. In other words, the powder phase after separation of the oil recovered using the conventional method may be a mixture of alloy ferroelectric powder containing rare metal components (magnetic material) and grinding wheel components (non-magnetic material).

[0023] Grindstone components include non-magnetic materials such as silica (SiO2) and alumina (Al2O3). Therefore, when recycling a powder phase containing a mixture of alloy iron powder and grindstone components as a roll material or stainless steel material, it is necessary to add a large amount of calcium source (lime, etc.) to adjust the composition of the slag before melting it, and therefore it is necessary to discharge a large amount of slag.

[0024] The present invention has been made in view of the above problems, and an object of the present invention is to provide a method for recovering ferroalloy powder which, unlike conventional oil separation by combustion treatment, reduces the energy required for removing oil from ferroalloy powder containing oil, increases the oil removal rate and powder recovery rate, and is capable of separating magnetized and non-magnetized materials. [Means for solving the problem]

[0025] The gist of the present invention is as follows.

[0026] [1] A method for recovering ferroalloy powder, comprising the steps of: separating oil from a mixture having oil attached thereto and containing ferroalloy powder and non-magnetic matter; and recovering the ferroalloy powder, a slurrying step of mixing the mixture with water to produce a slurry having a viscosity in the range of 0.003 to 1.00 Pa·S; a first emulsification step of adding a first volatile hydrophobic solvent to the slurry and then mixing to form a first emulsion; a first magnetic separation step of separating and recovering a powder phase from the first emulsion by magnetic separation; a residual solvent removal step of introducing the powder phase obtained in the first magnetic separation step into a hot water bath having a water temperature higher than the boiling point of the first volatile hydrophobic solvent, and volatilizing and removing the first volatile hydrophobic solvent remaining in the powder phase; an alloy iron powder recovery step of separating and recovering an alloy iron powder from the slurry containing the powder phase obtained in the residual solvent removal step by wet classification; A method for recovering ferroalloy powder, comprising: [2] A method for recovering ferroalloy powder, comprising the steps of: separating oil from a mixture having oil attached thereto and containing ferroalloy powder and non-magnetic matter; and recovering the ferroalloy powder, a slurrying step of mixing the mixture with water to produce a slurry having a viscosity in the range of 0.003 to 1.00 Pa·S; a first emulsification step of adding a first volatile hydrophobic solvent to the slurry and then mixing to form a first emulsion; a first magnetic separation step of separating and recovering a powder phase from the first emulsion by magnetic separation; a residual solvent removal step of introducing the powder phase obtained in the first magnetic separation step into a hot water bath having a water temperature higher than the boiling point of the first volatile hydrophobic solvent, and volatilizing and removing the first volatile hydrophobic solvent remaining in the powder phase; an alloy iron powder recovery step of separating and recovering an alloy iron powder from the slurry containing the powder phase obtained in the residual solvent removal step by dry classification; Equipped with The alloy iron powder recovery step includes: a dehydration step of dehydrating the slurry containing the powder phase obtained in the residual solvent removal step using a dehydrator; a drying step of drying the powder phase obtained in the dehydration step; a classification step of separating and recovering an alloy iron powder from the powder phase obtained in the drying step by dry classification; A method for recovering ferroalloy powder, comprising: [3] The method for recovering alloy iron powder according to the above [1] or [2], characterized in that the oil concentration in the solid matter in the slurry containing the powder phase obtained in the residual solvent removal step is 1.5 mass% or less. [4] The method for recovering ferroalloy powder according to the above [1], characterized in that the wet classification is either a liquid cyclone or magnetic separation. [5] The method for recovering ferroalloy powder according to the above [2], characterized in that the dry classification is performed using a centrifugal air current classifier, magnetic separation, or gravity separation using a heavy liquid. [6] A method for recovering ferroalloy powder according to the above [1] or [2], characterized in that the washing step consisting of the first emulsification step and the first magnetic separation step is repeated one or more times. [7] The method for recovering ferroalloy powder described in [6] above, further comprising, between the first magnetic separation step and the residual solvent removal step, a second emulsification step of adding a second volatile hydrophobic solvent to the powder phase obtained in the first magnetic separation step, followed by mixing to form a second emulsion, and a second magnetic separation step of separating and recovering the second powder phase from the second emulsion by magnetic separation, characterized in that the washing step and the rinsing step consisting of the second emulsification step and the second magnetic separation step are performed in a single counterflow tank as a counterflow type continuous process. [8] The method for recovering ferroalloy powder according to the above [1] or [2], characterized in that the specific gravity of the first volatile hydrophobic solvent is greater than 1.05 and less than 2.0. [9] The method for recovering ferroalloy powder according to the above [1] or [2], characterized in that the boiling point of the first volatile hydrophobic solvent at normal pressure is less than 95°C. Effect of the Invention

[0027] According to the above-described aspects of the present invention, it is possible to provide a method for recovering ferroalloy powder, which can reduce the energy required for removing oil from oil-containing powder, increase the oil removal rate and powder recovery rate, and separate magnetized and non-magnetized materials. [Brief description of the drawings]

[0028] [Figure 1] FIG. 2 is a schematic diagram showing the state of oil and moisture in oil-containing scale. [Diagram 2] 4 is a flowchart illustrating a powder recovery method according to the present embodiment. [Diagram 3] FIG. 2 is a schematic diagram for explaining an overview of the powder recovery method according to the present embodiment. [Figure 4] FIG. 1 is a schematic diagram showing a powder recovery facility according to the present embodiment and a continuous treatment (continuous process) using the same. [Diagram 5] FIG. 2 is a schematic diagram showing a modified example of the powder recovery equipment according to the present embodiment and a continuous treatment (continuous process) using the same. [Figure 6]1 is a graph showing the relationship between the blending ratio of water and powder (water / powder (g / g)) and the viscosity (Pa·s) of the slurry in Example 1. [Figure 7] 1 is a graph showing the relationship between the viscosity (Pa·s) of a slurry and the oil removal rate (%) in Example 1. [Figure 8] 2 is a graph showing the relationship between the oil content (%) and the alloy content (%) in Example 1. [Figure 9] This is a schematic diagram of the emulsion state during oil extraction when the processing object is roll grinding chips. [Figure 10] FIG. 10 is a schematic diagram showing the emulsion shown in FIG. 9 broken by using a magnet. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0029] The method for recovering ferroalloy powder according to the present embodiment will be described with reference to the drawings. In this specification and the drawings, components having substantially the same functional configurations are denoted by the same reference numerals to avoid repetitive explanation. A numerical range expressed using "~" means a range including the numerical values ​​before and after "~" as the lower and upper limits.

[0030] First, the subject to be treated, the solution, etc. in the method for recovering ferroalloy powder will be described together with new findings obtained by the present inventors.

[0031] The method for recovering ferroalloy powder of this embodiment is a method for recovering ferroalloy powder from which oil has been removed using magnetic force and from which non-magnetic substances (e.g., grinding stone components) have been separated. Therefore, the object to be treated in the method for recovering ferroalloy powder of this embodiment is a powder having oil attached thereto and containing magnetic substances (oil-containing powder), such as scales generated in the rolling process and roll grinding dust. The scale referred to here is scale that contains oil and moisture, and is sometimes called oil-containing scale or oil-containing sludge. Roll grinding dust is grinding dust generated when grinding various metal processing rolls used in the steelmaking process, and is sometimes called roll dust. Oil-containing powders such as scale and roll grinding dust may contain non-magnetic materials, and roll grinding dust in particular often contains grinding stone components (silica, alumina, etc.) used in grinding.

[0032] The particle size of the oil-containing powder to be treated is not particularly limited, but for example, the oil-containing powder may be one having an average particle size of 5 μm to 200 μm. In the case of roll grinding dust, it contains grindstone components, and these grindstone components also have an average particle size of about 5 μm to 200 μm. The particle size of the powder can be measured by a laser diffraction / scattering method, and the average particle size is based on volume.

[0033] Next, the form of oil and water in oil-containing scale will be described using the case where the oil-containing powder is oil-containing scale as an example. Note that even if the powder is roll grinding dust, the form will be the same as that shown in Figure 1.

[0034] Fig. 1 is a schematic diagram showing the form in which oil and water exist in oil-impregnated scale. For the sake of convenience, the shapes and dimensional ratios of the components shown in Fig. 1 are illustrated to be different from the actual shapes and dimensional ratios, but the oil-impregnated powder in this embodiment is not limited to that shown in Fig. 1. As shown in Fig. 1, water and oil in oil-impregnated scale exist as oil and water in the bulk, oil and water in gaps, oil and water in capillaries, and oil and water adsorbed to the scale. Oil and water refers to a state in which oil and water are mixed. Moreover, the bulk here refers to the outer region of the scale particle that does not touch the interface of the scale particle.

[0035] Oil and moisture in the bulk refers to the moisture and oil present around scale particles. Oil and moisture in pores refers to the moisture and oil surrounded by gaps formed by aggregations of large and small solid particles such as scale. Oil and moisture in capillaries refers to the moisture and oil bound together by capillary pressure within the capillaries on the surface of the scale. Oil and moisture adsorbed to particles such as scale refers to the moisture and oil chemically adsorbed to the scale.

[0036] The oil and moisture in the bulk have almost no binding strength with particle groups such as scale, and are easily separated by applying external pressure. They can be separated by mechanical force, for example, dehydration and deoiling using a pressurized dehydrator or centrifugal dehydrator, or by natural dehydration and deoiling by leaving to stand.

[0037] On the other hand, because the oil and water in the gaps are surrounded by solid particles such as scale, it is very difficult to separate them by dehydration / de-oiling using mechanical force or by leaving them to stand.

[0038] Furthermore, the oil and moisture in the capillaries is moisture and oil that is held inside the capillaries on the surface of particles such as scale by capillary force, and like the oil and moisture in the voids, it is difficult to separate it by dehydration / deoiling using mechanical force or by leaving it to stand.

[0039] Furthermore, the oil and moisture adsorbed to particles such as scale is water and oil that is chemically bound to the surface or inside of the particles, and can only be separated by evaporation due to an increase in temperature or by chemical reaction.In other words, the oil and moisture in the gaps, in the capillaries, and adsorbed to the particles cannot be easily separated by normal dehydration and deoiling operations (mechanical dehydration and deoiling operations using a centrifugal dehydrator or filter press, or natural dehydration and deoiling by leaving to stand, etc.).

[0040] Regarding these problems, the present inventors have investigated a method of using a solvent as a means of separating and removing oil and moisture, particularly oil. From the results of the investigation, it was thought that the oil in the bulk, gaps and capillaries, as well as the oil adhering to powders such as alloy iron powder and non-magnetic matter that make up scale and roll grinding dust, could be separated from the powder by adsorbing it with a solvent, and further investigations were carried out.

[0041] For example, when an organic solvent is added to oil-containing scale as shown in Figure 1 and then stirred to extract the oil from the scale, the oil in the bulk is easily extracted because it comes into contact with the organic solvent. On the other hand, the oil in the gaps and capillaries is surrounded by scale, and water is also present in the gaps and capillaries at the same time as the oil. Therefore, the oil in the gaps and capillaries and the organic solvent are blocked by the water and scale, and the organic solvent cannot easily come into contact with the oil in the gaps and capillaries. In other words, the oil in the gaps and capillaries is difficult to extract and the oil content is difficult to reduce by simply adding an organic solvent and stirring.

[0042] The inventors have discovered that the oil content in oil-containing scale can be reduced by extracting the oil in the gaps and capillaries, which cannot be easily separated by ordinary dehydration and deoiling operations, with an easily volatile hydrophobic organic solvent (hereinafter also referred to as a volatile hydrophobic solvent), and then volatilizing the volatile hydrophobic solvent in the gaps and capillaries.

[0043] In addition, when a hydrophobic organic solvent is used as a means for separating oil from oil-containing powder, when a mixture of the organic solvent, oil-containing powder, and water is strongly stirred, an emulsion (emulsion) is formed in which many powder particles are dispersed in the aqueous phase between the solvent droplets, and the oil can be extracted by the solvent. However, it has been found that if emulsification is insufficient, the extraction of oil by the solvent does not proceed sufficiently. In areas where emulsification is insufficient, the powder does not have sufficient fluidity in the slurry consisting of water and oil-containing powder, so the solvent is not mixed uniformly and the probability of contact between the solvent and powder is significantly reduced, which is thought to make it difficult to extract the oil. Therefore, when making an emulsion from a mixture of a hydrophobic organic solvent and oil-containing powder, it is important to determine the mixing ratio after fully understanding the area in which the emulsion will be made.

[0044] In addition, generally, when a mixture of a hydrophobic organic solvent and water is strongly stirred and left to stand, an emulsion is temporarily formed, but the emulsion state is often dissolved in a short time. However, when a mixture containing a fine powder with high hydrophilicity (wettability), such as the above-mentioned mixture of fine oil-containing powder, organic solvent, and water, is strongly stirred and left to stand, the oil extraction can be promoted, but the emulsion may be stabilized without being easily broken. This is because the fine powder, which is a solid content, functions as an emulsifier, and the fine powder is present at the interface between the fine water droplets and the organic solvent phase, or the interface between the fine organic solvent droplets and the water phase, thereby stabilizing the emulsion. When the emulsion is stabilized, it becomes difficult to separate the hydrophobic organic solvent, water, and fine powder. Therefore, in order to recover powder such as alloy iron powder, it is necessary to break the emulsion.

[0045] Therefore, the present inventors have investigated a method of applying a magnetic force to an emulsion using a magnetic separator capable of magnetic sorting (hereinafter simply referred to as magnetic separation) as a method of breaking down an emulsion and recovering powder containing magnetic substances from which oil and water have been removed. As a result, they have found that it is possible to break down an emulsion and separate the powder phase by magnetic force, and to recover only the powder phase from which the oil has been removed. In this way, by applying a magnetic force to an emulsion, the powder containing magnetic substances in the emulsion is moved in the direction in which the magnetic force acts, and the emulsion is dissolved (demulsified), i.e., broken, in a short time.

[0046] However, when magnetized materials such as alloy iron powder and non-magnetized materials such as grinding stone components are mixed in the oil-containing powder, it is difficult to quickly replace (separate) the magnetized materials and non-magnetized materials in the emulsion-state slurry, and it has been found that there are cases where the magnetized materials and non-magnetized materials cannot be separated in the powder phase from which the oil has been removed. The reason for this is explained below.

[0047] Fig. 9 is a schematic diagram of the emulsion state during oil extraction when the treatment object is roll grinding chips. Fig. 10 is a schematic diagram of the emulsion shown in Fig. 10 broken by using a magnet (i.e., by magnetic attraction).

[0048] As shown in Figure 9, the solvent droplets spread evenly in the aqueous phase, and the ferroalloy powder (magnetic material) and grinding wheel powder (non-magnetic material) with oil attached are dispersed in the aqueous phase around the solvent droplets. When the ferroalloy powder and grinding wheel powder come into contact with the solvent droplets, the oil attached to the surfaces of the ferroalloy powder and grinding wheel powder are extracted into the solvent phase.

[0049] Next, when a magnet is brought close to this emulsion, as shown in Figure 10, the magnetic ferroalloy powder is attracted to the magnet and the powder in the aqueous phase between the solvent droplets disappears, and the solvent droplets coalesce and are separated into a powder phase (cake phase), a solvent phase containing oil, and an aqueous phase. At this time, the grinding wheel components are non-magnetic, but since they exist in the narrow area between the solvent droplets (dotted line area in Figure 9) in the emulsion state, it is physically difficult for them to exchange places with the ferroalloy powder (i.e., separate) even if a magnet is brought close as shown in Figure 10. Therefore, when a magnet is brought close, many of the non-magnetic grinding wheel components are attracted to the magnet so that they are caught up in the magnetic ferroalloy powder, and it is not possible to completely separate the ferroalloy powder and grinding wheel powder components in the emulsion.

[0050] Even when an emulsion containing alloy ferroelectric powder and grinding wheel components is centrifuged, the alloy ferroelectric powder and the grinding wheel components are unlikely to be interchanged in the narrow aqueous phase between the solvent droplets, and the alloy ferroelectric powder and the grinding wheel components cannot be completely separated from each other.

[0051] Therefore, the present inventors have studied a method for separating the ferroalloy powder and the grinding wheel component in the powder phase from which the oil has been removed, and have found that only the ferroalloy powder can be efficiently recovered by classifying the powder phase consisting of the ferroalloy powder and the grinding wheel component by wet classification or dry classification. However, it is important that the majority of the fluid part when classifying the ferroalloy powder and the grinding wheel component is a single phase, and the single phase may be a liquid phase or a gas phase. When the fluid part is an aqueous phase, it becomes a water slurry, and the ferroalloy powder and the grinding wheel powder can move freely, and the ferroalloy powder and the grinding wheel powder can be separated from each other by magnetic separation or centrifugation (wet classification). Similarly, when the fluid part is a gas phase, the ferroalloy powder and the grinding wheel powder can move freely, and the ferroalloy powder and the grinding wheel powder can be separated from each other by magnetic separation or centrifugation (dry classification).

[0052] The present invention has been made based on the new findings described above. Next, a method for recovering ferroalloy powder according to one embodiment of the present invention will be described with reference to the drawings.

[0053] <1. Powder recovery method> Fig. 2 is a flow chart showing the method for recovering ferroalloy powder according to this embodiment, and Fig. 3 is a schematic diagram for explaining the outline of the method for recovering ferroalloy powder according to this embodiment.

[0054] As shown in FIG. 2, the method for recovering ferroalloy powder according to this embodiment includes a slurrying step S1, a first emulsifying step S2-1, a first magnetic separation step S2-2, a residual solvent removing step S4, and a ferroalloy powder recovering step S5. Each step will be described below with reference to Fig. 3. For convenience of explanation, Fig. 3 shows a case where a magnetic separator is provided in each step, but the method for recovering ferroalloy powder according to this embodiment is not limited by the devices and facilities used.

[0055] (Slurrying step S1) The slurrying step S1 is a step in which a mixture (powder) 10 having oil attached thereto and containing ferroalloy powder and non-magnetic matter is mixed with water 20 in a container to produce a slurry 30 (FIG. 3(a)). In the slurrying step S1, first, powder 10 and water 20 are put into a container and stirred (mixed) to disperse powder 10 in water 20, thereby generating slurry 30.

[0056] The powder 10 is a mixture containing an alloy ferromagnetic powder, which is a magnetic material, and a non-magnetic material, such as scale and roll grinding dust. In the case of roll grinding dust, the non-magnetic material is a grinding wheel component. The powder 10 may be a mixture of scale and roll grinding dust. The scale is a magnetic material whose main components are FeO and Fe3O4, but may contain components with low magnetic properties.

[0057] From the viewpoint of improving the recovery efficiency of the ferroalloy powder by magnetic force, it is preferable that the content of the magnetic material in the powder 10 is high, and specifically, the content of the magnetic material is preferably 20 mass% or more. Furthermore, when the content of the magnetic material in the powder 10 is low, for example, less than 20 mass%, the total content of the magnetic material in the entire powder 10 may be increased to 20 mass% or more by newly adding magnetic material such as iron powder to the powder 10. By doing so, both the magnetic material in the original powder and the newly added magnetic material can be recovered by magnetic force. However, it is preferable from the viewpoint of energy that the proportion of the magnetic material newly added is less than the proportion of the magnetic material originally present in the powder, in consideration of the reuse of the recovered material.

[0058] Here, scale refers to iron oxide, mainly composed of FeO and Fe3O4, which is generated on the surface of a slab during hot rolling. Such scale is finely crushed during hot rolling and discharged together with the coolant water. In other words, a water-containing slurry (water-containing scale) in which fine scale is dispersed in the coolant water is discharged. In such a case, when using the water-containing slurry, the slurrying step S1 may be omitted and the water-containing slurry may be directly used in the first emulsion step described later. In addition, the water-containing slurry generated during hot rolling generally contains 3 to 8 mass % of oil (mass % relative to the total mass of the powder).

[0059] The specific gravity of the powder 10 used in this embodiment is not particularly limited, but may be more than 1.05. The powder 10 is preferably hydrophilic particles such as scales and roll grinding dust. Hydrophilic particles are particles that have an affinity for water and have the property of being easily mixed with water. It is more preferable that the oil-containing powder 10 is composed only of hydrophilic particles, but may contain other types of particles, such as hydrophobic particles, as long as the effects of the present invention are not impaired. The hydrophobic particles are particles that are hydrophobic to water, and examples of such particles include coke powder and plastic powder.

[0060] The specific gravity of the powder 10 is preferably greater than the specific gravity of the first volatile hydrophobic solvent (hereinafter also referred to as the cleaning solvent) 50 used in the subsequent first emulsification step S2-1. This allows the water 20 present between the particles of the powder 10 to be replaced with the first volatile hydrophobic solvent 50 when the emulsion is subsequently broken down to effect phase separation, and as a result, the energy required to dry the powder 10 can be reduced.

[0061] The particle size of the powder 10 is not particularly limited, but the volume-based 50% particle size (d 50 ) is preferably 200 μm or less. In this embodiment, the water 20 present between the particles of the powder 10 is replaced with the first volatile hydrophobic solvent 50, thereby reducing the energy required for drying the powder 10 and efficiently recovering the powder. The first volatile hydrophobic solvent 50 evaporates with lower energy than the water 20. Therefore, by replacing the water 20 present between the particles of the powder 10 with the first volatile hydrophobic solvent 50, the energy required for drying the powder 10 can be reduced. And, the smaller the particle diameter of the powder 10, the larger the gaps present between the particles of the powder 10, so that more water 20 can be replaced with the first volatile hydrophobic solvent 50, and as a result, the above-mentioned effect is enhanced. From this viewpoint, it is preferable that the particle diameter of the powder 10 is small, and the volume-based 50% particle diameter (d 50 ) is preferably 100 μm or less, more preferably 80 μm or less, and even more preferably 50 μm or less. On the other hand, if the volumetric 50% particle size of the powder 10 is less than 1 μm, the amount of capillary water and adsorbed water will be greater than the interstitial water. As a result, the hydrophilicity of the powder 10 will be very high, and even if the treatment of this embodiment is performed, it may be difficult to remove the water 20 present between the particles of the powder 10. Therefore, the lower limit of the volumetric 50% particle size of the powder 10 is preferably 1 μm or more.

[0062] The volumetric 50% particle size of powder 10 (d 50) can be measured, for example, by the following measurement method using a laser diffraction particle size distribution analyzer. Specifically, first, the oily powder to be measured is slurried with water, and a small amount of sodium hexametaphosphate solution is added as a dispersant to prepare a mixed liquid. The mixed liquid is then stirred and irradiated with ultrasonic waves to disperse the oily powder in the mixed liquid. Next, the mixed liquid is placed in the laser diffraction particle size distribution analyzer, and the particle size distribution is measured.

[0063] The amount of water 20 added in the slurrying step S1 is equal to or more than the amount that makes the powder 10 slurried in the water 20. In the subsequent first emulsification step, the first volatile hydrophobic solvent 50 is added to the slurry 30, and the viscosity of the slurry 30 increases. Therefore, it is better to set the viscosity in the slurrying step S1 lower than the target viscosity. Specifically, water 20 is added to the powder 10 so that the viscosity of the slurry in the slurrying step S1 is 1.00 Pa·S or less. The viscosity of the slurry is preferably 0.65 Pa·S or less, more preferably 0.50 Pa·S or less, and even more preferably 0.35 Pa·S or less. On the other hand, if the amount of water added in the slurrying step S1 is too large, the contact probability between the powder 10 and the first volatile hydrophobic solvent 50 decreases after the first emulsification step. In such a case, it is necessary to extend the extraction time of the oil from the powder 10 or increase the stirring strength, which is not preferable from the viewpoint of work efficiency. Therefore, the amount of water 20 added to the powder 10 is adjusted so that the viscosity of the slurry becomes 0.003 Pa·S or more, and more preferably, 0.10 Pa·S or more.

[0064] The viscosity of the slurry can be determined by first measuring the viscous resistance torque with a rotational viscometer and converting the obtained viscous resistance torque into viscosity. Specifically, 300 ml of the prepared slurry is placed in a tall beaker, and the rotor part of the rotational viscometer is immersed in the slurry and rotated to measure the viscous resistance torque of the slurry acting on the rotor part. The obtained viscous resistance torque is then converted into viscosity.

[0065] Here, the reason for limiting the viscosity in the slurrying step S1 will be explained below together with the results of the inventor's investigation. The present inventors have studied the correlation between the degree of emulsification in the first emulsification step S2-1 and the progress of oil extraction, and have found that when emulsification is insufficient, the extraction of oil by the cleaning solvent is also insufficient. This is thought to be because, when emulsification is insufficient, the powder does not have sufficient fluidity in the slurry, so that even if the cleaning solvent is added, the solvent is not mixed uniformly and the extraction of oil is not promoted. That is, in order to extract oil from the powder in the emulsion, each particle of the powder needs to come into contact with a droplet of the cleaning solvent. To do this, it is necessary for the powder to be able to move freely in the aqueous phase. As a result of studying an index to evaluate this "ability to move freely in the aqueous phase," the present inventors have found that it can be evaluated by the viscosity of the slurry. When the ratio of oil-containing powder in the slurry increases, the viscosity of the slurry increases rapidly and the fluidity of the slurry decreases significantly, so that even if emulsification is attempted thereafter, the opportunity for the powder to come into contact with the droplets of the cleaning solvent decreases rapidly. For this reason, in this embodiment, as described above, it is important to set the viscosity of the slurry in the slurrying step S1 to 1.00 Pa·S or less.

[0066] In addition, in this embodiment, from the viewpoint of stable emulsification, the powder 10 and water 20 are mixed in advance to prepare the slurry 30, and in the next step, the first volatile hydrophobic solvent 50 is added to the slurry 30. When the powder 10, the water 20, and the first volatile hydrophobic solvent 50 are mixed at the same time, the mixing of the water 20 and the powder 10 may not proceed smoothly, and emulsification may be difficult. In particular, when the mixing ratio (g / g) of the water / powder is small, emulsification becomes difficult and the oil removal performance decreases. Therefore, in the slurrying step S1, it is preferable to mix the water 20 and the powder 10 in advance, form a slurry, and then add and mix the first volatile hydrophobic solvent 50 to the obtained slurry to emulsify it.

[0067] The mixing device used in the slurrying step S1 is not particularly limited, but for example, a vessel equipped with stirring blades for stirring the mixture of the powder 10 and water 20, a line mixer, or the like can be used.

[0068] (Washing step S2) (First emulsification step S2-1) The first emulsification step S2-1 is a step of adding a first volatile hydrophobic solvent 50 to the slurry 30 produced in the slurrying step S1 and stirring the mixture to form an emulsion 40 (FIG. 3(b)). In the first emulsification step S2-1, first, a first volatile hydrophobic solvent 50 having a specific gravity of more than 1.05 and less than 2.0 is added to a container containing a slurry 30 consisting of powder 10 and water 20, and the mixture is further stirred to form an emulsion 40. Note that in the first emulsification step S2-1, the slurry 30 may be transferred from the container used in the slurrying step S1 to another container to form the emulsion 40.

[0069] In general, an emulsion means a dispersion solution of two immiscible liquids, one of which is dispersed as fine droplets in the other liquid, and is also called an emulsion. The emulsion 40 according to this embodiment means a dispersion solution in which two liquids (water 20 and a first volatile hydrophobic solvent 50) with different specific gravities and solid powder 10 are suspended.

[0070] The first volatile hydrophobic solvent 50 is a liquid having volatility and hydrophobicity, that is, a liquid having a property of low affinity for water (difficult to dissolve in water or difficult to mix with water). The first volatile hydrophobic solvent 50 is, for example, a liquid having a solubility in water of 0 g / L or more and 10.0 g / L or less at room temperature (25° C.). If the solubility of the first volatile hydrophobic solvent 50 in water is high, a large amount of water 20 remains in the first volatile hydrophobic solvent 50 when the water 20 present between the particles of the powder 10 is replaced with the first volatile hydrophobic solvent 50. In this case, there is a possibility that the energy required for drying the powder phase after the residual solvent removal step S4 cannot be sufficiently reduced. From this viewpoint, the solubility of the first volatile hydrophobic solvent 50 in water is preferably 10.0 g / L or less at room temperature, more preferably 5.0 g / L or less. In this case, the water 20 remaining in the first volatile hydrophobic solvent 50 can be further reduced.

[0071] In this embodiment, "hydrophobic" may also mean a property including lipophilicity, and the first volatile hydrophobic solvent 50 may be, for example, an organic solvent or various oils having hydrophobicity.

[0072] The specific gravity of the first volatile hydrophobic solvent 50 is not particularly limited because it does not have a significant effect on the magnetic separation for separating oil from the powder. In addition, considering the specific gravity difference of each element after the emulsion is broken, it is preferable that the specific gravity of the first volatile hydrophobic solvent 50 is larger than that of water and smaller than that of the powder 10 to be recovered. Specifically, it is preferable that the specific gravity of the first volatile hydrophobic solvent 50 is greater than 1.05 and less than 2.0. This makes it possible to separate the water and the first volatile hydrophobic solvent 50 generated after breaking the emulsion by the specific gravity difference. However, as described above, the specific gravity of the first volatile hydrophobic solvent 50 is not limited to the above range and may be 1.05 or less, as long as the water and the first volatile hydrophobic solvent 50 generated after breaking the emulsion can be separated by the specific gravity difference.

[0073] The boiling point of the first volatile hydrophobic solvent 50 is preferably less than 95°C at normal pressure. If the upper limit of the boiling point is less than 95°C, the first volatile hydrophobic solvent 50 remaining in the powder phase can be easily removed (for example, with water vapor, which is an inexpensive energy source) after the powder phase is recovered in a subsequent process. The lower limit of the boiling point of the first volatile hydrophobic solvent 50 is not particularly limited, but since the oil extraction operation is easily performed at room temperature, it is preferable to set it to 50°C or higher.

[0074] In addition, the volatile heat value of the first volatile hydrophobic solvent 50 is preferably smaller than that of water. In this case, the first volatile hydrophobic solvent 50 can be easily removed by volatilization, and can be easily separated from the powder 10.

[0075] In addition, as the solvent used as the first volatile hydrophobic solvent 50, it is preferable to select a solvent with a large KB value (kauri-butanol value) in order to remove oil from the powder 10 more efficiently. By using a solvent with a large KB value as the first volatile hydrophobic solvent 50, the oil can be more easily absorbed. From the viewpoint of the KB value, it is preferable to use, for example, trichloroethylene, 1-bromopropane, n-hexane, etc. as the first volatile hydrophobic solvent 50. In addition, hydrofluoroether may be used as the first volatile hydrophobic solvent 50.

[0076] The amount of the first volatile hydrophobic solvent 50 added to the oil-adhered powder 10 (the rate of addition of cleaning solvent) is not particularly limited, but may be appropriately determined depending on the type of solvent used, the equipment used, etc. From the viewpoint of the rate of removal of oil, a larger amount is preferable.

[0077] As described above, in this embodiment, by adding magnetic material such as iron powder to the powder 10 to increase the ratio of magnetic material in the powder 10, the recovery ratio can be improved.

[0078] (1st magnetic separation process S2-2) The first magnetic separation step S2-2 is a step of separating and recovering the first powder phase 10a from the first emulsion 40 formed in the first emulsification step S2-2 by magnetic separation (FIG. 3(c)).

[0079] The first magnetic separation step S2-2 is performed using a first magnetic separator 80. From the viewpoint of magnetic separation efficiency, it is preferable to use a drum-type separator as the first magnetic separator 80. Hereinafter, a case where a drum-type separator is used as the first magnetic separator 80 will be described.

[0080] First, as shown in Fig. 3(c), the emulsion 40 and the drum 81 of the first magnetic separator 80 are brought into contact with each other, and a magnetic force is applied to the emulsion 40 by a magnet 82 fixed inside the drum 81. When the magnetic force is applied to the emulsion 40, only the powder 10 in the emulsion 40 is magnetically attracted to the surface of the drum 81, and as the drum 81 rotates, the powder phase (first powder phase) 10a is collected.

[0081] When the powder 10 of the emulsion 40 is magnetically attracted to the surface of the drum 81 , the solvent droplets in the emulsion coalesce into a solvent phase, resulting in the emulsion 40 breaking down and separating into water 20 and the first volatile hydrophobic solvent 50 .

[0082] By the above steps, the powder phase 10a made up of magnetized and non-magnetized materials from which the oil has been removed can be collected. In addition, residual water and solvent may be present in the powder phase 10a magnetically attached to the surface of the drum 81. In such a case, it is preferable to apply pressure to the powder phase 10a magnetically attached to the surface of the drum 81 using a squeeze roll 83 as shown in Fig. 3(c) to remove the liquid. The liquid removing means is not limited to the squeeze roll 83, and a squeeze guide 84 (see Fig. 4) as described later may also be used.

[0083] The washing step S2, which is composed of the first emulsification step S2-1 and the first magnetic separation step S2-2, may be repeated two or more times, thereby further increasing the oil removal rate.

[0084] Furthermore, in order to further increase the efficiency of removing the residual solvent, a residual solvent removing step is further performed. However, before performing the residual solvent removing step, the following rinsing step S3 may be performed.

[0085] (Rinsing step S3) (Second emulsification step S3-1) (Second magnetic separation process S3-2) In this embodiment, a second emulsification step S3-1 (Figure 3(d)) may be performed in which a second volatile hydrophobic solvent 51 is added to the powder phase 10a obtained in the washing step S2 and then mixed to form a second emulsion 41, and a second magnetic separation step (Figure 3(e)) may be performed in which the second powder phase 10aa is separated and recovered from the second emulsion by magnetic separation.

[0086] As described above, residual water and solvent may be present in the powder phase 10a magnetically attached to the surface of the drum 81. Therefore, by performing emulsification and magnetic separation again using the powder phase 10a obtained in the washing step S2, it is possible to recover a powder (second powder phase 10aa) from which oil has been further removed.

[0087] The specific implementation methods and conditions of the second emulsification step S3-1 and the second magnetic separation step S3-2 may be similar to those of the first emulsification step S2-1 and the first magnetic separation step S2-2, respectively.

[0088] For example, the first volatile hydrophobic solvent 50 and the second volatile hydrophobic solvent 51 may be the same solvent or different solvents. However, from the viewpoint of efficiency in carrying out the residual solvent removal step and the drying step described below, it is preferable that the first volatile hydrophobic solvent 50 and the second volatile hydrophobic solvent 51 are the same solvent.

[0089] In addition, the specific gravity of the second volatile hydrophobic solvent 51 is not particularly limited because it does not have a significant effect on the magnetic separation for separating oil from the oil-containing powder, similar to the first volatile hydrophobic solvent 50. In addition, considering the specific gravity difference of each element after the emulsion is broken, it is preferable that the specific gravity is larger than water and smaller than the specific gravity of the powder 10 to be recovered. Specifically, it is preferable that the specific gravity of the second volatile hydrophobic solvent 51 is greater than 1.05 and less than 2.0. This makes it possible to separate the water generated after the emulsion is broken from the second volatile hydrophobic solvent 51 by the specific gravity difference. However, as described above, the specific gravity of the second volatile hydrophobic solvent 51 is not limited to the above range and may be 1.05 or less, as long as the water generated after the emulsion is broken from the first volatile hydrophobic solvent 50 can be separated by the specific gravity difference.

[0090] In addition, the rinsing step S3 consisting of the second emulsification step S3-1 and the second magnetic separation step S3-2 may be repeated two or more times, thereby further increasing the oil removal rate.

[0091] In this embodiment, from the viewpoint of improving the efficiency of the recovery operation and the recovery speed, it is preferable to carry out the cleaning step S2 and the rinsing step S3 in a countercurrent continuous process in one counterflow tank. Details of the recovery equipment using the countercurrent continuous process will be described later.

[0092] The amount of the second volatile hydrophobic solvent 51 to be added is preferably calculated as follows. First, the residual solvent phase removed in the rinsing step S3 is separated by gravity separation into an aqueous phase containing almost no oil and a solvent phase containing oil, and the absorbance of the solvent phase containing oil is measured. From the measured absorbance value obtained, the amount of residual oil in the powder phase after the rinsing step S3 is estimated, and the amount of the second volatile hydrophobic solvent 51 added is adjusted so that the estimated value of the residual oil amount is equal to or less than a target value.

[0093] That is, when the residual solvent phase removed by the rinsing step S3 contains a large amount of oil (when the absorbance is high), it can be determined that a large amount of oil that was not completely removed from the powder phase 10a remains, and in that case, the amount of the second volatile hydrophobic solvent 51 added is increased. On the other hand, when there is almost no oil remaining in the residual solvent phase removed by the rinsing step S3 (when the absorbance is low), it can be said that the oil has been sufficiently removed from the powder phase 10a, so it is sufficient to reduce the amount of the second volatile hydrophobic solvent 51 added. This allows the residual solvent phase to be efficiently removed from the powder phase 10a, and also allows the amount of residual oil in the powder phase after recovery to be controlled by the absorbance of the residual solvent phase containing the oil removed by the rinsing step S3.

[0094] The absorbance of the residual solvent phase containing the oil removed in the rinsing step S3 is measured, for example, by placing the residual solvent phase to be measured in a sealed cell and measuring the absorbance with an absorbance meter. Since oil is generally yellowish, an absorption wavelength of about 350 to 500 nm may be used when measuring the absorbance of the residual solvent phase containing oil.

[0095] The oil-containing solvent phase recovered from the waste liquid (washing waste liquid) discharged in the washing step S2 may be distilled and then regenerated as an oil-free volatile hydrophobic solvent. This regenerated volatile hydrophobic solvent can be used as the first volatile hydrophobic solvent or the second volatile hydrophobic solvent. In addition, the solvent phase recovered from the waste liquid (rinsing waste liquid) discharged in the rinsing step S3 has a low oil content and can therefore be used as the first volatile hydrophobic solvent (cleaning solvent). From the viewpoint of such reuse, it is preferable to use the same solvent as the first volatile hydrophobic solvent 50 and the second volatile hydrophobic solvent 51.

[0096] (Residual solvent removal step S4) After the cleaning step S2 (or the rinsing step S3), a residual solvent removal step S4 is performed to remove the first volatile hydrophobic solvent 50 remaining in the recovered powder phase 10a (or the powder phase 10aa) (FIG. 3(f)). If the rinsing step S3 is performed, the second volatile hydrophobic solvent 51 is also removed in this step. The first volatile hydrophobic solvent 50 that has not been completely discharged may remain in the collected powder phase 10a. In addition, when the rinsing step S3 is performed, the second volatile hydrophobic solvent 51 that has not been completely discharged may remain in the collected powder phase 10aa. In such a case, it is preferable to remove these remaining solvents. Specifically, these solvents may be removed by, for example, drying or volatilization. Note that FIG. 3(f) shows a method of removing the remaining solvent by volatilization.

[0097] When the first volatile hydrophobic solvent 50 and the second volatile hydrophobic solvent 51 are removed by drying, the drying temperature is preferably a temperature higher than the boiling point of the first volatile hydrophobic solvent 50. This allows each solvent to be dried and removed efficiently from the powder phase 10a (or the powder phase 10aa). When a hydrophobic solvent different from the first volatile hydrophobic solvent 50 is used as the second volatile hydrophobic solvent 51 in the rinsing step, the solvent may be dried and removed at a temperature higher than the boiling points of the first volatile hydrophobic solvent 50 and the second volatile hydrophobic solvent 51. When the first volatile hydrophobic solvent 50 and the second volatile hydrophobic solvent 51 are removed by drying, the non-magnetic substances can be separated by classifying the obtained powder phase 10a as it is by magnetic separation or the like. In other words, when the residual solvent is removed by drying, the powder phase 10a can be classified into magnetic substances and non-magnetic substances by magnetic separation or the like without forming a slurry.

[0098] The drying means is not particularly limited, but for example, an indirect heating type dryer, a vacuum indirect heating type dryer, or the like may be used for drying.

[0099] When the first volatile hydrophobic solvent 50 and the second volatile hydrophobic solvent 51 are removed by volatilization, the first volatile hydrophobic solvent 50 is first volatilized and removed by being put into a hot water bath with a water temperature higher than the boiling point of the first volatile hydrophobic solvent 50, as shown in FIG. 3(f). The powder phase 10a (or the powder phase 10aa) put into the hot water bath is slurried to become the slurry 42, and after the solvent is volatilized and removed, the alloy iron powder recovery step S5 is carried out to classify the slurry 42. Details will be described later. In addition, when a hydrophobic solvent different from the first volatile hydrophobic solvent 50 is used as the second volatile hydrophobic solvent 51 in the rinsing step S3, the water temperature of the hot water bath may be set to the higher of the boiling points of the first volatile hydrophobic solvent 50 and the second volatile hydrophobic solvent 51.

[0100] As described above, a part of the liquid contained in the powder phase (powder cake) 10a after the washing step S2 or the powder phase (powder cake) 10aa after the rinsing step S3 is the first volatile hydrophobic solvent 50 or the second volatile hydrophobic solvent 51. Therefore, the powder phase 10a or the powder phase 10aa can be dried with less energy (amount of heat of vaporization). As shown in the examples described later, the energy required to dry the powder phase can be measured by differential scanning calorimetry (DSC), but it can also be measured by other methods, such as the Karl Fischer method.

[0101] (Ferrous alloy powder recovery process S5) The powder phase 10a (or powder phase 10aa) after the residual solvent removal step S4 contains a mixture of magnetized and non-magnetized matter. Therefore, in this embodiment, a step is carried out to recover the ferroalloy powder 10b from the slurry 42 containing the powder phase 10a (or powder phase 10aa) obtained by the residual solvent removal step S4, that is, to separate the non-magnetized matter from the slurry (FIG. 3(g)).

[0102] When the residual solvent removal step S4 is performed by volatilization, the powder phase 10a (or powder phase 10aa) introduced into the hot water tank is in the form of a slurry, and therefore, in the ferroalloy powder recovery step S5, the slurry 42 is subjected to wet classification to separate and recover the ferroalloy powder 10b. The specific means for wet classification is not particularly limited, but a liquid cyclone or magnetic separation is preferable.

[0103] The slurry 42 obtained in the residual solvent removal step S4 may be dehydrated by a dehydrator or the like to form a powder phase (dehydration step), and then the powder phase may be dried (drying step), and the ferroalloy powder 10b may be separated and collected by dry classification (classification step). The specific means of dry classification is not particularly limited, but a centrifugal air current classifier, magnetic separation, or specific gravity separation using a heavy liquid is preferable. As a dehydrator used in the dehydration step, a magnetic separator similar to the first magnetic separator 80 may be used, or a centrifuge, a screw press, a filter type dehydrator, or the like may be used.

[0104] In order to efficiently separate the ferroalloy powder from the non-magnetic materials in the ferroalloy powder recovery step S5, it is preferable that the oil concentration in the solid matter in the slurry 42 obtained in the residual solvent removal step S4 is low. That is, the efficiency of separation of the ferroalloy powder from the non-magnetic materials is affected by the oil removal rate in the washing step (or rinsing step), and the more the oil is removed from the powder, that is, the lower the oil concentration in the solid matter in the slurry 42, the higher the recovery efficiency of the ferroalloy powder can be. Preferably, the oil concentration in the solid matter in the slurry 42 is 1.5 mass% or less.

[0105] Through the above steps, the ferroalloy powder 10b from which the oil and the solvents have been removed can be collected.

[0106] The method for recovering ferroalloy powder according to the present embodiment has been described above, but the temperature and pressure at which each step is carried out are not particularly limited, and the steps may be carried out, for example, at room temperature and pressure. In the above, the residual solvent removing step S4 is performed after the rinsing step S3, but the rinsing step S3 may be omitted and the residual solvent removing step S4 may be performed after the cleaning step S2.

[0107] In addition, in the method for recovering ferroalloy powder according to this embodiment, each of the steps from the slurrying step S1 to the ferroalloy powder recovery step S5 can be performed as a batch process. However, from the viewpoints of solid-liquid separation speed, powder recovery speed, and productivity, it is preferable to perform these steps simultaneously in a continuous process.

[0108] According to the method for recovering ferroalloy powder of this embodiment, a magnetic separator is used to extract and remove oil using a volatile hydrophobic solvent, so that the energy required for removing oil from oil-containing powder can be significantly reduced compared to conventional combustion treatment methods. In addition, since the voids in the recovered powder phase contain a large amount of volatile hydrophobic solvent, the solvent can be easily removed, and low-moisture, high-purity ferroalloy powder containing almost no oil can be efficiently recovered. In other words, according to the method for recovering ferroalloy powder of this embodiment, a new and improved method for recovering ferroalloy powder can be provided that can increase the oil removal rate and solid-liquid separation speed. Furthermore, in the method for recovering ferroalloy powder according to this embodiment, after the solvent is removed by volatilization, the ferroalloy powder and non-magnetic matter (e.g., grinding wheel components) are separated. As described above, a powder phase from which oil and solvent have been efficiently and sufficiently removed can be obtained, and therefore the ferroalloy powder can be recovered from the powder phase with high efficiency.

[0109] <2. Ferroalloy powder recovery equipment> Next, an embodiment of an ferroalloy powder recovery facility for carrying out the ferroalloy powder recovery method of the present embodiment described above will be described.

[0110] The ferroalloy powder recovery equipment according to this embodiment is an equipment for recovering ferroalloy powder by separating oil from a mixture having oil attached thereto and containing ferroalloy powder and non-magnetic matter. Each device in the ferroalloy powder recovery equipment of this embodiment may be provided as a batch type (see FIG. 3), but from the viewpoint of improving the efficiency of the recovery work and the recovery speed, the emulsification device and the magnetic separator may be disposed in one counterflow tank, and each step may be carried out simultaneously while the treatment is continued, so-called a counterflow type continuous process. In the following description, a countercurrent continuous process will be taken as an example of the recovery equipment of this embodiment.

[0111] FIG. 4 is a schematic diagram showing a ferroalloy powder recovery facility 1 according to this embodiment and a continuous treatment (continuous process) using the same. The powder recovery equipment 1 of this embodiment includes a slurrying device 60, a first emulsifying device 70, a first magnetic separator 80 that separates and recovers the first powder phase by magnetic force, and a residual solvent removing device 73. The first emulsifying device 70 and the first magnetic separator 80 are arranged in a vertical line from upstream to downstream in a counterflow tank 100 filled with the slurry and each volatile hydrophobic solvent. In this embodiment, the "upstream" refers to the first emulsifying device 70 side, and the "downstream" refers to the second magnetic separator 90 side. In other words, the flow from upstream to downstream means the transport direction of the powder phase. On the other hand, the flow of the aqueous phase and the solvent phase is from downstream to upstream, and is a countercurrent to the flow of the powder phase.

[0112] The slurrying device 60 is a device that performs the slurrying step S1, and stirs and mixes the mixture (powder) 10 containing the ferroalloy powder having oil attached thereto and the non-magnetic material with water 20 to generate the slurry 30. As the slurrying device 60, a known device can be used, and for example, a vessel equipped with an agitating blade and a motor for stirring the mixture of the powder 10 and the water 20, a line mixer, or the like can be used.

[0113] The slurrying device 60 can be connected to a downstream first emulsifying device 70, for example, via piping. A pump P is connected to the piping, and the slurry 30 is sent to the emulsifying device 70 by the pump P. Note that, although the slurry 30 is introduced from above the equipment in Fig. 4, it may be introduced from the side of the equipment.

[0114] The first emulsification device 70 is a device that performs the first emulsification step S2-1, and stirs and mixes the slurry 30 and the first volatile hydrophobic solvent 50 to form the emulsion 40. Since this embodiment is a countercurrent type, the solvent phase flows from downstream to upstream. In other words, the first volatile hydrophobic solvent 50 used in the first emulsification device 70 flows in from the downstream side, so the introduction position of the first volatile hydrophobic solvent 50 is downstream of the first emulsification device 70. Specifically, it is preferable that the first volatile hydrophobic solvent 50 is introduced from above the second emulsification device 71. However, the introduction position of the first volatile hydrophobic solvent 50 is not limited to one place, and it may be introduced from above the first emulsification device 70. A known device can be used for the first emulsification device 70, and for example, a vessel equipped with an agitator blade and a motor for agitating the mixture of the slurry 30 and the first volatile hydrophobic solvent 50, a line mixer, or the like can be used.

[0115] The recovery equipment 1 of this embodiment is a countercurrent type continuous recovery equipment in which the flow of the powder phase and the flow of the aqueous phase and the solvent phase are countercurrent, so the second volatile hydrophobic solvent 51 used in the subsequent rinsing step S3 flows into the cleaning step S1. In other words, since the first emulsification device 70 uses two solvents, the first volatile hydrophobic solvent 50 and the second volatile hydrophobic solvent 51, it is preferable that the first volatile hydrophobic solvent 50 and the second volatile hydrophobic solvent 51 are the same type of solvent.

[0116] The first emulsification device 70 stirs and mixes the slurry 30 and the first volatile hydrophobic solvent 50 by rotating the stirring blades with the motor M. As a result, the powder 10, the water 20, and the first volatile hydrophobic solvent 50 are strongly stirred, so that the above-mentioned emulsion 40 can be produced. Furthermore, the first volatile hydrophobic solvent 50 acts as an extractant for the oil, and the oil is extracted from the powder 10.

[0117] The first magnetic separator 80 is a device that performs the first magnetic separation step S2-2, and separates and recovers the first powder phase by magnetic force. The first magnetic separator 80 is disposed downstream of the first emulsifier 70. From the viewpoint of magnetic separation efficiency, it is preferable to use a drum-type separator. Hereinafter, a case where a drum-type separator is used as the first magnetic separator 80 will be described.

[0118] The first magnetic separator 80 includes a drum 81, a magnet 82 provided in the drum 81, and a squeeze guide 84 provided on the upper part of the drum 81. The first magnetic separator 80 is provided such that at least a part of the drum 81 and the magnet 82 are immersed in the emulsion 40, and a magnetic force acts on the emulsion 40 by the magnet 82 fixed in the drum 81. When the magnetic force acts on the emulsion 40, only the powder 10 in the emulsion 40 is magnetically attracted to the surface of the drum 81, and as the drum 81 rotates, a powder phase (first powder phase) 10a is collected.

[0119] When the powder 10 of the emulsion 40 is magnetically attracted to the surface of the drum 81 , the solvent droplets in the emulsion coalesce into a solvent phase, resulting in the emulsion 40 breaking down and separating into water 20 and the first volatile hydrophobic solvent 50 .

[0120] The squeeze guide 84 is a deliquification means provided above the drum 81. The squeeze guide 84 applies pressure to the residual water and the residual solvent adhering to the recovered powder phase 10a, thereby making it possible to deliquify the first powder phase 10a.

[0121] The recovery equipment 1 of this embodiment may further include a second emulsifier 71 and a second magnetic separator 90 for carrying out the rinsing step S3 in order to further increase the efficiency of removing the residual solvent in the powder phase 10a.

[0122] The second emulsification apparatus 71 is an apparatus for carrying out the second emulsification step S3-1, in which a second volatile hydrophobic solvent 51 is further added to the first powder phase 10a recovered by the first magnetic separator 80, and then the mixture is stirred and mixed to form an emulsion 40. The second volatile hydrophobic solvent 51 used here is the same type of solvent as the first volatile hydrophobic solvent 50. Furthermore, as the second emulsification apparatus 71, an apparatus having the same configuration as the first emulsification apparatus 70 may be adopted.

[0123] The second magnetic separator 90 is a device that executes the second magnetic separation step S3-2. The first powder phase 10a collected by the first magnetic separator 80 may contain residual solvent containing oil, or oil may remain on the powder surface. Therefore, by performing magnetic separation again by the second magnetic separator, it is possible to separate and collect powder from which more oil has been removed (second powder phase 10aa). The second magnetic separator 90 may be a device having the same configuration as the first magnetic separator.

[0124] In addition, in the powder recovery equipment 1 of this embodiment, a residual solvent removal device 73 and a dehydrator 91 may be further provided to remove the solvent remaining in the first powder phase 10a recovered by the first magnetic separator 80, or, if the rinsing step S3 is performed, to remove the solvent remaining in the second powder phase 10aa recovered by the second magnetic separator 90 (residual solvent removal step S4).

[0125] The residual solvent removal device 73 is a device that removes the first volatile hydrophobic solvent 50 and the second volatile hydrophobic solvent 51 remaining in the first powder phase 10a or the second powder phase 10aa by volatilization. A known configuration can be adopted as a specific configuration of the residual solvent removal device 73, and an example of the configuration includes a hot water tank filled with hot water and a motor M for stirring. First, the first powder phase 10a or the second powder phase 10aa is put into a hot water tank filled with hot water, and the stirring blade is rotated by a motor M, thereby removing the solvent remaining in the first powder phase 10a or the second powder phase 10aa. The hot water used for the volatilization removal is recovered at the most downstream of the recovery equipment 1, and can be reused by being put into the residual solvent removal device 73 again. The solvent removed by the volatilization removal is recovered in a distillation device (not shown) and rectified, so that it can be reused again as the first volatile hydrophobic solvent 50 or the second volatile hydrophobic solvent 51.

[0126] In the volatilization removal using the residual solvent removal device 73, hot water is used. Therefore, it is desirable to provide a heat insulating wall W between the second magnetic separator 90 and the residual solvent removal device 73 to prevent thermal energy from being transferred downstream. The heat insulating wall W is desirably provided at a boundary other than the inlet for conveying and feeding the powder phase 10aa among the cross section (boundary) of the counterflow tank 100 between the second magnetic separator 90 and the residual solvent removal device 73, but it is sufficient that the height of the heat insulating wall W is at a position higher than the water surface of the hot water. In addition, it is desirable to provide a rotary valve with high sealing properties at the inlet for conveying and feeding the first powder phase 10a or the second powder phase 10aa, and to convey and feed the first powder phase 10a or the second powder phase 10aa.

[0127] The dehydrator 91 is a device for recovering the ferroalloy powder 10b by dehydrating the slurry containing the first powder phase 10a or the second powder phase 10aa from which the solvent has been removed by volatilization in a hot water tank. The specific configuration of the dehydrator 91 may be the same as that of the first magnetic separator 80 or the second magnetic separator 90. Alternatively, a liquid cyclone may be used as the dehydrator 91.

[0128] After the residual solvent is removed from the powder phase by the residual solvent remover 73 in this manner, the slurry containing the powder phase is dehydrated by the dehydrator 91 and wet classified, so that the ferroalloy powder 10b can be separated and recovered from the powder phase. The non-magnetic matter (e.g., grinding stone components) separated from the powder phase is separated into water and the non-magnetic matter by filtration or the like.

[0129] 5 shows a modified example of the ferroalloy powder recovery equipment 1 according to this embodiment. The configuration of the recovery equipment 1 of this modified example up to the residual solvent removal device 73 is the same as that of FIG. 5, in the recovery equipment of this modification, the slurry from which the solvent has been removed in the residual solvent removal equipment 73 is subjected to wet classification by the dehydrator 91, but this slurry is recovered from downstream and is again fed into the residual solvent removal equipment 73. Therefore, the slurry is continuously circulated between the residual solvent removal equipment 73 and the dehydrator 91, and the non-magnetic materials contained in the powder phase are not sufficiently classified by the dehydrator 91 and are discharged as the powder phase 10aa while remaining in the ferroalloy powder.

[0130] Therefore, in this modification, the powder phase 10aa containing the non-magnetic substances remaining in the ferroalloy powder is dried in a drying device to remove moisture, and the dried powder phase aa is then classified by a dry classifier. The specific means of the dry classification is not particularly limited, but a centrifugal air classifier, magnetic separation, or gravity separation using a heavy liquid is preferable. This allows only the ferroalloy powder 10b to be separated and recovered from the powder phase containing the ferroalloy powder and the non-magnetic substances.

[0131] 4 and 5, the magnetic separators 80 and 90 and the dehydrator 91 rotate in a direction parallel to the liquid flow (clockwise), but may rotate in a direction opposite to the liquid flow (counterclockwise). When the powder contains many particles with weak magnetic properties, it is preferable to rotate them in the opposite direction. 4 or 5, one or more magnetic drums for preventing outflow may be installed between the washing step S2 and the phase separation step. The powder that has flowed out by the washing step S2, i.e., the powder that could not be magnetically attracted, can be magnetically attracted by the magnetic drum for preventing outflow and returned to the first emulsification device 70. Note that since the powder that could not be magnetically attracted by the washing step S2 contains many particles with weak magnetic attraction, it is preferable that the rotation direction of the magnetic drum for preventing outflow is the opposite direction (counterclockwise).

[0132] A preferred embodiment of the recovery equipment 1 of this embodiment has been described above. However, as described above, the recovery equipment 1 can also be a batch type equipment, and in that case, the same technical concept as that of the countercurrent type can be applied.

[0133] In addition, the recovery equipment 1 of this embodiment is a countercurrent type continuous recovery equipment, and the flow of the aqueous phase and the solvent phase is from downstream to upstream. Therefore, in order to allow the volatile hydrophobic solvent introduced from above the second emulsification device to contribute sufficiently to the emulsification, it is preferable to provide an overflow weir between the first magnetic separator and the second emulsification device. This allows the introduced solvent to remain around the second emulsification device, resulting in sufficient emulsification. In addition, when the powder 10 can be easily slurried, the powder 10 may be directly charged into the first emulsification device 70 . Moreover, the rinsing step S3 may be further added and performed multiple times, thereby further increasing the oil removal rate. A second volatile hydrophobic solvent may also be added to the first emulsification step S2-1. EXAMPLES

[0134] Next, examples (experimental examples) of this embodiment will be described. In each of the examples described below, various tests were performed to confirm the effects of this embodiment. Note that each of the following examples was performed at room temperature and normal pressure.

[0135] <Example 1> Oil-laden roll grinding dust (oil content: 7.5 mass%, alloy content: 76.0 mass%) and water were mixed under the conditions shown in Table 1 to prepare a slurry. Then, a volatile hydrophobic solvent (cleaning solvent) with a specific gravity of 0.65 to 1.43 was added and mixed to prepare an emulsion.

[0136] Next, a neodymium magnet (surface area: 14.5 cm) was placed in the resulting emulsion. 2After immersing the neodymium magnet in a magnetic flux density at the surface: approximately 5,000 gauss for five seconds, the magnet was pulled up and the powder phase (cake before deliquor removal), mainly consisting of magnetic materials that had been magnetically attached to the magnet surface, was collected.

[0137] Next, a rubber plate was pressed against the powder phase magnetically attached to the magnet surface and squeezed to remove the liquid from the magnet surface.

[0138] After dehydration, the powder phase was scraped off the magnet surface, the oil content in the powder phase was measured, and the oil removal rate was calculated from the oil content in the powder before and after treatment.

[0139] After removing the powder phase adhering to the magnet surface, the magnet was immersed in the emulsion again to recover the magnetic material remaining in the emulsion. This operation was repeated until the magnetic material was no longer magnetically attached to the magnet surface.

[0140] The recovered magnetic material was put into hot water adjusted to 98° C. (a temperature higher than the boiling point of the hydrophobic solvent) and mixed for 10 minutes, and the hydrophobic solvent was removed by volatilization to recover a slurry.

[0141] In Comparative Examples 1-1 to 1-3, Invention Examples 1-4 to 1-10, and Invention Examples 1-15 and 1-16, the temperature of the slurry after removing the hydrophobic solvent was lowered to room temperature, and then a neodymium magnet (surface area: 14.5 cm 2 After immersing the neodymium magnet in a magnetic flux density of approximately 5,000 gauss (magnetic flux density at the surface: approximately 5,000 gauss) for five seconds, the neodymium magnet was pulled up and the powder phase (ferroalloy powder) consisting mainly of the magnetic material magnetized to the magnet surface was collected. Next, a rubber sheet was pressed against the powder phase consisting mainly of the magnetic material magnetized to the magnet surface and squeezed to remove the liquid from the magnet surface. Next, after removing the powder phase adhering to the magnet surface, the magnet was immersed in the slurry again and the magnetized material remaining in the slurry was collected. This operation was repeated until the magnetized material was no longer magnetically attached to the magnet surface. After drying all of the collected magnetized material, the constituent metal elements of the roll (Fe, Ni, V, Cr, Mo, Mn, Nb, W) were treated as alloying elements, and the rest were treated as grinding wheel components to calculate the alloying element content (alloy content) of the entire collected magnetized material by fluorescent X-ray analysis.

[0142] In Examples 1-11, the temperature of the slurry after removing the hydrophobic solvent was lowered to room temperature, the slurry concentration was adjusted to 10% by mass, the adjusted slurry was put into a liquid cyclone, and a slurry containing a large amount of powder phase mainly composed of magnetized matter was collected from the bottom of the liquid cyclone. The collected slurry was then dried to collect the powder phase mainly composed of magnetized matter, and the alloy element content of the roll constituent metal elements (Fe, Ni, V, Cr, Mo, Mn, Nb, W) was calculated as alloy elements and the rest as grinding wheel components relative to the entire powder phase mainly composed of magnetized matter by fluorescent X-ray analysis.

[0143] In Examples 1-12 to 1-14, the temperature of the slurry after removing the hydrophobic solvent was lowered to room temperature, and then the slurry was filtered to obtain a powder phase mainly composed of magnetized materials, which was then dried. Then, in Example 1-12, a neodymium magnet (surface area: 14.5 cm 2 The roll was subjected to magnetic separation using a magnetic flux density of approximately 5,000 gauss (magnetic flux density at the surface: approximately 5,000 gauss) and the magnetized material (alloy components) was recovered. After that, fluorescent X-ray analysis was used to calculate the alloy element content of the constituent metal elements of the roll (Fe, Ni, V, Cr, Mo, Mn, Nb, W) as alloy elements and the rest as grinding wheel components in the total magnetized material recovered. In invention examples 1-13, the powder phase mainly composed of magnetized material was introduced into a heavy liquid (aqueous solution of sodium polytungstate) whose specific gravity was adjusted to 3, mixed, and then left to stand, and the precipitate that settled out was collected. The collected precipitate was thoroughly washed with water on filter paper, and the solid matter on the filter paper was dried, and then the constituent metal elements of the roll (Fe, Ni, V, Cr, Mo, Mn, Nb, W) were treated as alloy elements, and the rest were treated as grinding wheel components, and the alloy element content relative to the entire collected magnetized material was calculated by fluorescent X-ray analysis. In Example 1-14, the dried powder mainly composed of the magnetic material obtained by drying was classified by a centrifugal air classifier into particles with a high specific gravity and particles with a low specific gravity. For the particles with a high specific gravity, the constituent metal elements of the roll (Fe, Ni, V, Cr, Mo, Mn, Nb, W) were regarded as alloy elements, and the rest were regarded as grinding wheel components, and the alloy element content relative to the entire magnetic material was calculated by fluorescent X-ray analysis.

[0144] In this example, the alloy recovery rate was evaluated as excellent (passed) when the alloy content was 85.0% by mass or more. The reason for setting the evaluation standard value at "85.0% by mass" is as follows. For example, when the metal components are melted and reduced using a material with an alloy content of 85% (15% grindstone content), the specific gravity of the metal is 7, the specific gravity of the slag is 2.5 (specific gravity near the melting point), and the basicity of the slag is 1.5. The ratio of molten metal to molten slag is 70:30 (weight ratio), and the volume ratio is 45:55. In other words, when the metal components are melted and reduced using a material with an alloy content of 85%, about half of the melting reduction furnace is occupied by molten slag, and a lot of energy is consumed to remove the slag. Therefore, if a material with an alloy content lower than 85% by mass is used, the amount of metal produced per unit volume of the melting reduction furnace will be further reduced, so the invention was evaluated as having an excellent alloy recovery rate when the alloy content of the alloy ferroalloy powder after recovery processing is 85.0% by mass or more.

[0145] [Table 1]

[0146] Comparative Examples 1-1 to 1-3 and Invention Examples 1-4 to 1-7 are examples in which the mixing ratio of the cleaning solvent to the powder (cleaning solvent / powder (g / g)) was kept constant (2.00 (g / g)), and only the mixing ratio of water to powder (water / powder (g / g)) was changed from 0.18 to 1.06 (g / g). When the water / powder ratio was 0.33 (g / g) or less (Comparative Example 1-1 and Comparative Example 1-2), a slurry could not be formed, and when the viscosity of the slurry was measured, the measurement range was exceeded (exceeding 100 Pa·S), and the measurement itself could not be performed. In Comparative Example 1-3, where the water / powder ratio was 0.47 (g / g), the oil content was reduced, but the alloy content of the final recovered product was 80.1%, which was not much better than the alloy content of the original sample of 76.0%. In Examples 1-4 to 1-7, where the water / powder ratio was 0.62 (g / g) to 1.06 (g / g), the oil content in the powder phase after the solvent was removed by evaporation was 1.4% or less, and in Examples 1-6 to 1-7, this was improved to 0.3%. As the oil content decreased, the alloy content in the final recovered material increased, reaching 85.2% or more, and in Example 1-7, it improved to 98.1%.

[0147] 6 and 7 are graphs showing the relationship between the blending ratio of water and powder (water / powder (g / g)) and the viscosity (Pa s) of the slurry, and the relationship between the viscosity (Pa s) of the slurry and the oil removal rate (mass%) in Comparative Example 1-3 and Invention Examples 1-4 to 1-7. Also, Fig. 8 is a graph showing the relationship between the oil content and the alloy content in Comparative Example 1-0 to Comparative Example 1-3 and Invention Examples 1-4 to 1-7. As shown in the graphs of Figures 6 and 7, when the water / powder ratio becomes smaller, the viscosity of the slurry increases, and mixing with the cleaning solvent becomes insufficient, resulting in a tendency for the oil removal rate to decrease. Also, as shown in the graph of Figure 8, as the oil content decreases, the alloy content of the final recovered material tends to increase. In particular, when the oil content was 1.4% (Invention Example 1-4), the alloy content was 85.2%, and as the oil content decreased further, the alloy content in the final recovered material increased further. From this, it can be said that an oil content of 1.4% or less is preferable.

[0148] Since the true specific gravity of the grindstone component and the alloy component in the grinding waste is different, and the ferroalloy component is magnetic, by reducing the oil content to 1.4% or less, a final recovered product with an alloy content of 85% or more can be obtained by wet classification using magnetic separation (Invention Example 1-4 to Invention Example 1-10) or liquid cyclone (Invention Example 1-11), or by dry classification using magnetic separation (Invention Example 1-12), heavy liquid separation (Invention Example 1-13), or centrifugal air classifier (Invention Example 1-14). In particular, when the oil content was less than 0.5 mass%, the alloy content exceeded 95% (Invention Examples 1-5 to 1-14).

[0149] Inventive Examples 1-9 and 1-10, hydrofluoroether and n-hexane were used as the hydrophobic solvent (cleaning solvent), and it was confirmed that oil could be removed.

[0150] <Example 2> Using the counterflow continuous recovery equipment shown in Figure 5, oil was extracted from the roll grinding dust with oil attached by the counterflow method, the hydrophobic solvent was removed by volatilization, and the grinding dust was dehydrated (magnetically attracted) to recover the grinding dust cake. After the recovered grinding dust cake was dried, the alloy components were separated and recovered using a centrifugal air classifier. The details of the second embodiment will be described below.

[0151] First, the oil-laden grinding waste (oil content: 7.5%, moisture: 20%, alloy content: 76% by mass) was fed into a slurrying device at 3.8 kg / min and mixed with water to produce a slurry with a slurry concentration of 40% by mass. The viscosity of the slurry was 0.12 Pa·S. The slurry was then fed into the first emulsifying device and further subjected to magnetic separation using the first magnetic separator (washing step). Furthermore, an oil-free volatile hydrophobic solvent (1-bromopropane) was fed into the second emulsification device at a rate of 2.0 kg / min, and water was fed into the second emulsification device at a rate of 2.7 L / min. The powder phase (powder cake) after magnetic separation by the first magnetic separator was mixed with the water and the volatile hydrophobic solvent to form an emulsion, which was then subjected to magnetic separation by the second magnetic separator (rinsing step).

[0152] In this way, the oil adhering to the roll grinding waste in the washing and rinsing steps was extracted with a volatile hydrophobic solvent, and after deliquescence, the powder phase mainly consisting of the magnetic material after deliquescence was placed in a residual solvent removal device containing warm water adjusted to 90°C, where the solvent remaining in the powder phase was volatilized and the powder phase was made into a slurry with water.

[0153] After that, the powder phase was recovered by magnetic dehydration using a dehydrator (a third magnetic separator was used as the dehydrator). The non-magnetic grindstone components, together with the excess water, were re-introduced into the residual solvent removal process by the pump after the third magnetic separation process, and were taken into the powder phase generated during magnetic separation, and were discharged as roll grinding chips after deoiling. The water and oil-containing solvent introduced in the washing step and rinsing step moved in the opposite direction to the flow of the grinding chips (to the left side of the paper in the case of Figure 5). In the phase separation tank, the phase was separated into water and oil-containing solvent, and the separated water was again introduced into the slurrying process or the second emulsification process and used again. In addition, the oil-containing solvent was distilled in a distillation device not shown, separated into oil and solvent, and the regenerated solvent was introduced into the second emulsification process. The oil content in the recovered powder phase was 0.3 mass%, and the oil removal rate was 96%. The moisture content was 25 mass % and the alloy content was 76.7%.

[0154] The collected powder phase was dried in a drying oven at 120° C. to obtain 50 kg of dried powder, which was then classified using a centrifugal air classifier to obtain 35.7 kg of alloy powder with an alloy content of 94.7%.

[0155] <Example 3> Using the counterflow continuous recovery equipment shown in Figure 4, oil was extracted from the roll grinding waste with oil attached by the counterflow method, and the hydrophobic solvent was removed by volatilization, after which the alloy components were magnetically attracted from the slurry to separate and recover the alloy components. The grindstone components that were not magnetically attracted during the magnetic attraction were separated from the water by filtration. The details of the third embodiment will be described below.

[0156] First, the oil-laden grinding waste (oil content: 7.5%, moisture: 20%, alloy content: 76% by mass) was fed into a slurrying device at 3.8 kg / min and mixed with water to produce a slurry with a slurry concentration of 40% by mass. The viscosity of the slurry was 0.12 Pa·S. The slurry was then fed into the first emulsifying device and further subjected to magnetic separation using the first magnetic separator (washing step).

[0157] Furthermore, an oil-free volatile hydrophobic solvent (1-bromopropane) was fed into the second emulsification device at a rate of 2.0 kg / min, and water was fed into the second emulsification device at a rate of 2.7 L / min. The powder phase (powder cake) after magnetic separation by the first magnetic separator was mixed with the water and the volatile hydrophobic solvent to form an emulsion, which was then subjected to magnetic separation by the second magnetic separator (rinsing step).

[0158] In this way, the oil adhering to the roll grinding waste in the washing and rinsing steps was extracted with a volatile hydrophobic solvent, and after deliquescence, the powder phase mainly consisting of the magnetic material after deliquescence was placed in a residual solvent removal device containing warm water adjusted to 90°C, where the solvent remaining in the powder phase was volatilized and the powder phase was made into a slurry with water.

[0159] After that, magnetic materials (ferroalloy powder) consisting of alloy components were collected from the slurry by magnetic separation. The non-magnetic grindstone components were put into a filter together with excess water, filtered, and the grindstone components were separated and collected. The filtered excess water was again put into the residual solvent removal process. The water and oil-containing solvent put in the cleaning step and rinsing step move in the opposite direction to the flow of the grinding debris (to the left side of the paper in the case of Figure 4). Phase separation into water and oil-containing solvent was performed in the phase separation tank, and the separated water was put into the slurrying step or the second emulsification step again and used again. In addition, the oil-containing solvent was distilled in a distillation device not shown in the figure, separated into oil and solvent, and the recycled solvent was put into the second emulsification step. The oil content in the collected magnetized material was 0.3 mass%, and the oil removal rate was 96%. The moisture content was 25 mass%, and the alloy content was 95.2%.

[0160] In Examples 1 to 3, the oil content of the powder before oil removal and the recovered powder phase (cake) was measured as follows. First, the powder before oil removal and the collected cake were each dried in a dryer at 105°C for 2 hours, and then the oil was extracted with n-hexane using a Soxhlet extractor. Subsequently, the mixture containing the extracted n-hexane and oil was heated to volatilize the n-hexane, and the weight of the residue (oil) was measured, and the oil content in the powder before oil removal and the cake before oil removal were calculated. The oil removal rate is a value obtained by subtracting the oil content of the cake (powder phase) after oil removal from the oil content of the powder before oil removal as the numerator and the oil content of the powder before oil removal as the denominator.

[0161] In Examples 1 to 3, the viscosity of the slurry was determined by first measuring the viscous resistance torque using a rotational viscometer and converting the obtained viscous resistance torque into a viscosity. Specifically, 300 ml of the prepared slurry was placed in a tall beaker, and the rotor of the rotational viscometer was rotated while immersed in the slurry, thereby measuring the viscous resistance torque of the slurry acting on the rotor. The obtained viscous resistance torque was then converted into a viscosity. The rotational viscometer used was a "VISCOMETER DVL-8 type (manufactured by Toki Sangyo Co., Ltd.)." [Explanation of symbols]

[0162] 1. Ferroalloy powder recovery equipment 10 Powder (oil-containing powder) 10a 1st powder phase (powder phase) 10aa 2nd powder phase (powder phase) 20 water 30 Slurry 40 Emulsion 50 First volatile hydrophobic solvent (cleaning solvent) 51 Second volatile hydrophobic solvent (rinsing solvent) 60 Slurrying Equipment 70 First emulsifier 71 Second Emulsifier 73 Residual Solvent Removal Equipment 80 First magnetic separator 81 Drums 82 Magnet 90 Second magnetic separator 91 Dehydrator 100 Counterflow tank W Insulated wall

Claims

1. 1. A method for recovering ferroalloy powder, comprising the steps of: separating oil from a mixture having oil attached thereto and containing ferroalloy powder and non-magnetic matter; and recovering the ferroalloy powder, the method comprising the steps of: a slurrying step of mixing the mixture with water to have a viscosity in the range of 0.003 to 1.00 Pa·S to generate a slurry; a first emulsification step of adding a first volatile hydrophobic solvent to the slurry and then mixing to form a first emulsion; a first magnetic separation step of separating and recovering a powder phase from the first emulsion by magnetic separation; a residual solvent removal step of introducing the powder phase obtained in the first magnetic separation step into a hot water bath having a water temperature higher than the boiling point of the first volatile hydrophobic solvent, and volatilizing and removing the first volatile hydrophobic solvent remaining in the powder phase; an alloy iron powder recovery step of separating and recovering an alloy iron powder from the slurry containing the powder phase obtained in the residual solvent removal step by wet classification; A method for recovering ferroalloy powder, comprising:

2. 1. A method for recovering ferroalloy powder, comprising the steps of: separating oil from a mixture having oil attached thereto and containing ferroalloy powder and non-magnetic matter; and recovering the ferroalloy powder, the method comprising the steps of: a slurrying step of mixing the mixture with water to have a viscosity in the range of 0.003 to 1.00 Pa·S to generate a slurry; a first emulsification step of adding a first volatile hydrophobic solvent to the slurry and then mixing to form a first emulsion; a first magnetic separation step of separating and recovering a powder phase from the first emulsion by magnetic separation; a residual solvent removal step of introducing the powder phase obtained in the first magnetic separation step into a hot water bath having a water temperature higher than the boiling point of the first volatile hydrophobic solvent, and volatilizing and removing the first volatile hydrophobic solvent remaining in the powder phase; an alloy iron powder recovery step of separating and recovering an alloy iron powder from the slurry containing the powder phase obtained in the residual solvent removal step by dry classification; Equipped with The alloy iron powder recovery step includes: a dehydration step of dehydrating the slurry containing the powder phase obtained in the residual solvent removal step using a dehydrator; a drying step of drying the powder phase obtained in the dehydration step; a classification step of separating and recovering an alloy iron powder from the powder phase obtained in the drying step by dry classification; A method for recovering ferroalloy powder, comprising:

3. 3. The method for recovering alloy iron powder according to claim 1, wherein the oil concentration in the solid matter in the slurry containing the powder phase obtained in the residual solvent removal step is 1.5 mass % or less.

4. 2. The method for recovering ferroalloy powder according to claim 1, wherein the wet classification is performed by either a liquid cyclone or magnetic separation.

5. 3. The method for recovering ferroalloy powder according to claim 2, wherein the dry classification is any one of a centrifugal air current classifier, magnetic separation, and gravity separation using a heavy liquid.

6. 3. The method for recovering ferroalloy powder according to claim 1, wherein the washing step consisting of the first emulsification step and the first magnetic separation step is repeated one or more times.

7. Between the first magnetic separation step and the residual solvent removal step, a second emulsification step of adding a second volatile hydrophobic solvent to the powder phase obtained in the first magnetic separation step, and then mixing to form a second emulsion; a second magnetic separation step of separating and recovering a second powder phase from the second emulsion by magnetic separation; Equipped with 7. The method for recovering ferroalloy powder according to claim 6, characterized in that the washing step and the rinsing step consisting of the second emulsification step and the second magnetic separation step are carried out in one counterflow tank as a counterflow type continuous process.

8. 3. The method for recovering ferroalloy powder according to claim 1 or 2, characterized in that the specific gravity of the first volatile hydrophobic solvent is greater than 1.05 and less than 2.

0.

9. 3. The method for recovering ferroalloy powder according to claim 1 or 2, characterized in that the boiling point of the first volatile hydrophobic solvent at normal pressure is less than 95°C.

Citation Information

Patent Citations

  • Method for treating oil-containing iron powder

    JP2002146442A

  • Oil content separating method, and oil content separating device

    JP2015132011A

  • Roll chip recycling method

    JP2016196671A

  • Processing method for grinding oil mixture containing sludge, its processing facility and sludge briquette

    JP1995116960A

  • Oil reforming equipment having water-oil separation mean

    JP2003277771A