Molding adsorbent for canisters

A shaped adsorbent combining activated carbon fibers and granular activated carbon with a binder addresses the challenge of wide-concentration fuel gas adsorption and desorption in vehicle canisters, enhancing performance and reducing pressure loss.

JP2024135503APending Publication Date: 2024-10-04NIPPON PAPER IND CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023046221
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing adsorbents for vehicle fuel canisters face challenges in achieving high adsorption and desorption performance for evaporated fuel gases across a wide concentration range, particularly with activated carbon fibers, and there is a need for improved recovery performance and reduced pressure loss.

Method used

A shaped adsorbent is developed using a combination of activated carbon fibers and granular activated carbon, with specific weight ratios and pore volumes, along with a binder, to enhance adsorption and desorption efficiency.

Benefits of technology

The combined adsorbent achieves excellent adsorption and desorption performance for evaporated fuel gases from low to high concentrations, with high efficiency in purging and reduced pressure loss, suitable for use in vehicle canisters.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135503000001_ABST
    Figure 2024135503000001_ABST
Patent Text Reader

Abstract

To provide a molding adsorbent improved in an adsorption / desorption performance with respect to a transpiration fuel gas (n-butane, in particular) over a wide concentration range from low concentration to high concentration.SOLUTION: A compact containing active carbon fibers, granular active carbons and binders is prepared. In a total quantity of the active carbon fibers and the granular active carbons, regarding a weight ratio of the active carbon fibers and the granular active carbons, the active carbon fibers occupy 5 to 95 pts.wt. and the granular active carbons occupy 95 to 5 pts.wt. A ratio of the binders contained in a molding adsorbent is 0.3 to 20 pts.wt. of the binders with respect to 100 pts.wt. of the active carbon fibers and the granular active carbons. Further, a total pore volume of the granular active carbons is 0.90 to 2.50 cm3 / g, and a total pore volume of the active carbon fibers is 0.50 to 1.20 cm3 / g.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present disclosure relates to a molded adsorbent for a canister, and more particularly to a molded adsorbent for a canister that utilizes activated carbon. [Background technology]

[0002] In vehicles equipped with internal combustion engines that burn evaporated fuels such as gasoline, such as automobiles, motorcycles, and boats, the pressure inside the fuel tank fluctuates with changes in outside temperature, causing evaporated fuel gases that fill the fuel tank to be released from the fuel tank. The released evaporated fuel gases are believed to be one of the substances that cause PM2.5 and photochemical smog, so in order to prevent them from being released into the atmosphere, canisters (also known as evaporated fuel suppression devices) equipped with adsorbents such as activated carbon are installed.

[0003] With the growing awareness of environmental conservation in recent years, regulations on emissions of various gases have tended to become stricter every year, and therefore higher adsorption performance is also required for canisters. Furthermore, with the spread of idling stop systems and the like, the intake capacity of automobiles tends to be restricted, making it difficult to desorb gasoline adsorbed on the adsorbent in the canister. Therefore, there is a demand for even higher performance adsorbents used in canisters. Activated carbon is often used as the adsorbent for canisters, and proposals have been made for its shape, such as granular, pellet, or honeycomb shape (e.g., Patent Document 1).

[0004] Furthermore, in recent years, from the viewpoint of improving the performance of canisters, it has become common to store adsorbents in multiple chambers, such as by providing a main chamber and an auxiliary chamber (for example, Patent Document 2).

[0005] An activated carbon fiber sheet with specific properties has been proposed as one of the adsorbents suitable for canisters (for example, Patent Document 3). Patent Document 3 discloses an activated carbon fiber sheet with excellent adsorption and desorption performance for low-concentration evaporated fuel gas (mainly n-butane).

[0006] Furthermore, in order to improve the mechanical strength and packing density of molded adsorbents using activated carbon fibers, an activated carbon fiber molded adsorbent containing activated carbon fibers and alkali-resistant fibrillated cellulose fibers has been proposed (for example, Patent Document 4).

[0007] Also, an evaporative fuel emission control system has been proposed that can reduce DBL (daytime breathing loss) emissions to 20 mg or less using a relatively low purge volume as determined using the bleed emissions test method (BETP) (see, for example, Patent Document 5).

[0008] Compared to the traditional powdered and granular activated carbon, activated carbon fiber (or fibrous activated carbon) is sometimes called the third type of activated carbon. Among activated carbons in the broad sense, activated carbon fiber is said to have micropores directly open on the outer surface and tend to have a fast adsorption / desorption rate. However, when attempting to incorporate activated carbon fiber into a canister, research and development has not yet progressed sufficiently to determine what characteristics of activated carbon fiber are suitable for practical use in canisters. In particular, there is still significant room for development in improving the performance of adsorbents made from a mixture of granular activated carbon and activated carbon fiber. As mentioned above, Patent Document 3 and other documents have proposed activated carbon fiber sheets with excellent adsorption / desorption performance for low-concentration evaporated fuel gases. However, there has also been a demand for adsorbents with excellent adsorption / desorption performance for a wider range of evaporated fuel gases, from low to high concentrations. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Japanese Patent Application Laid-Open No. 2013-173137 [Patent Document 2] JP 2019-108880 A [Patent Document 3] Patent No. 6568328 [Patent Document 4] Japanese Patent Application Publication No. 10-5580 [Patent Document 5] Special Publication No. 2016-53354 Summary of the Invention [Problem to be solved by the invention]

[0010] In view of the above circumstances, one of the problems to be solved is to provide a molded adsorbent having excellent adsorption and desorption performance for evaporated fuel gases (e.g., n-butane) over a wide range of concentrations, from low to high. In another aspect, a further problem to be solved is to provide a molded adsorbent that has excellent adsorption properties for evaporated fuel gases (e.g., n-butane) over a wide range of concentrations from low to high, can be desorbed with high efficiency using canister purge air, and has excellent recovery performance. [Means for solving the problem]

[0011] As a result of extensive research, the present inventors have succeeded in producing an adsorbent with excellent performance by combining multiple types of specific activated carbon with different properties and forming a molded body containing a binder. The present disclosure provides a molded adsorbent containing at least two types of activated carbon, specifically, activated carbon fiber and granular activated carbon, with different characteristics.

[0012] The invention presented in this disclosure can be understood in multiple aspects and may include, for example, the following embodied aspects as means for solving problems. Note that in this disclosure, the invention presented in this disclosure is also simply referred to as "the present invention" either as a comprehensive concept or according to each individual aspect.

[0013] [1] A molded adsorbent for a canister, the molded adsorbent is a molded body containing activated carbon fiber, granular activated carbon, and a binder; the weight ratio of the activated carbon fiber to the granular activated carbon is 5 to 95 parts by weight and 95 to 5 parts by weight of the granular activated carbon in the total amount of the activated carbon fiber and the granular activated carbon; the content of the binder in the formed adsorbent is 0.3 to 20 parts by weight per 100 parts by weight of the activated carbon fiber and the granular activated carbon; The total pore volume of the granular activated carbon is 0.90 to 2.50 cm 3 / g, The total pore volume of the activated carbon fiber is 0.50 to 1.20 cm 3 / g, The molded adsorbent. [2] The formed adsorbent according to the above [1], wherein the average pore diameter of the granular activated carbon is 2.00 to 4.00 nm. [3] The specific surface area of ​​the granular activated carbon is 1400 to 2700 m 2 / g. [4] The average pore diameter of the granular activated carbon is 2.00 to 4.00 nm; The specific surface area of ​​the granular activated carbon is 1400 to 2700 m 2 / g, The molded adsorbent according to any one of the above [1] to [3]. [5] The total pore volume of the activated carbon fiber is smaller than the total pore volume of the granular activated carbon; The average pore diameter of the activated carbon fiber is smaller than the average pore diameter of the granular activated carbon. The molded adsorbent according to any one of the above [1] to [4]. [6] The average pore diameter of the granular activated carbon is 2.00 to 4.00 nm; The specific surface area of ​​the granular activated carbon is 1400 to 2700 m 2 / g, the total pore volume of the activated carbon fiber is smaller than the total pore volume of the granular activated carbon; The average pore diameter of the activated carbon fiber is smaller than the average pore diameter of the granular activated carbon. The molded adsorbent according to [1] above. [7] The total pore volume of the formed adsorbent is 0.90 to 2.00 cm 3 The formed adsorbent according to any one of the above [1] to [6], wherein the molecular weight is 1 / g. [8] The formed adsorbent according to any one of the above [1] to [7], wherein the formed adsorbent has an average pore diameter of 1.87 to 4.00 nm. [9] The molded adsorbent according to any one of [1] to [8] above, wherein the weight ratio of the activated carbon fiber to the granular activated carbon in the total amount of the activated carbon fiber and the granular activated carbon is 5 to 70 parts by weight of the activated carbon fiber and 95 to 30 parts by weight of the granular activated carbon.

[10] The effective adsorption / desorption rate of 100% n-butane is 75.0% or more; The effective adsorption / desorption rate of 0.2% n-butane is 60.0% or more. The molded adsorbent according to any one of the above [1] to [9].

[11] The formed adsorbent according to any one of the above [1] to

[10] , wherein the effective adsorption / desorption rate of 100% n-butane is 81.0% or more.

[12] The formed adsorbent according to any one of the above [1] to

[11] , which has an effective adsorption / desorption rate of 0.2% n-butane of 70.0% or more.

[13] The molded adsorbent according to any one of the above [1] to

[12] , wherein the binder is a fibrous binder. [Effects of the Invention]

[0014] According to one or more aspects of the invention presented in the present disclosure, it is possible to provide an adsorbent that has excellent adsorption and desorption performance for evaporated fuel gas (for example, n-butane) ranging from low concentration to high concentration. Furthermore, one or more aspects of the invention presented in the present disclosure provide an adsorbent that has excellent adsorption properties for evaporated fuel gases (e.g., n-butane) ranging from low to high concentrations, can be desorbed with high efficiency using purge air from the canister, and has excellent recovery performance. [Brief explanation of the drawings]

[0015] [Figure 1] FIG. 1 is a diagram schematically illustrating an example of a laminated adsorbent body formed by stacking a plurality of sheet-shaped adsorbent bodies, and an example of the flow direction of a fluid passing through the laminated adsorbent body. [Figure 2]FIG. 1 is a diagram showing an example of an adsorbent formed into a disk shape. [Figure 3] FIG. 1 is a diagram showing an example of an adsorbent formed into a cylindrical shape. DETAILED DESCRIPTION OF THE INVENTION

[0016] Hereinafter, an embodiment of the present invention will be described. In this disclosure, unless otherwise specified, the term "one embodiment" in relation to the present invention refers to any one embodiment in describing the present invention in detail, and does not deny or limit the existence of other or multiple embodiments. As described below, the present invention may include multiple embodiments within its scope. Furthermore, multiple embodiments may also be provided as modified forms, for example, by various combinations of the components (or technical features) described in this disclosure. Furthermore, in this disclosure, when the term "embodiment" is simply mentioned, it includes one or multiple embodiments unless otherwise specified.

[0017] In this disclosure, unless otherwise specified, the expression "AA to BB" in relation to a numerical range means "greater than or equal to AA and less than or equal to BB" (where "AA" and "BB" represent arbitrary numerical values). Furthermore, unless otherwise specified, the units of the lower and upper limits are the same as the units immediately following the latter (i.e., "BB" in this case). Furthermore, in this disclosure, the combination of the lower and upper limits of a numerical range can be arbitrarily selected from the group of lower or upper limit values ​​exemplified as preferred numerical values, etc. Furthermore, the expression "X and / or Y" means both X and Y, or either one of them.

[0018] In the present disclosure, the term "pore size" refers to the diameter or width of a pore, not the radius of the pore, unless otherwise specified. That is, in the present disclosure, the term "pore size" is synonymous with "pore diameter" unless otherwise specified.

[0019] 1. Molded adsorbent for canisters In one embodiment of the present invention, the molded adsorbent can be suitably used in a canister. A canister is a device equipped with an adsorbent, which adsorbs evaporated evaporated fuel onto the adsorbent to prevent it from being released into the atmosphere, and which desorbs the evaporated fuel adsorbed on the adsorbent and supplies it to the engine when the engine is running. Canisters are generally used in machines or devices equipped with internal combustion engines that use fuels containing highly volatile hydrocarbons, such as vehicles and ships equipped with internal combustion engines. Examples of vehicles include automobiles that use gasoline as fuel. Examples of ships include boats that use gasoline as fuel.

[0020] In one embodiment of the present invention, the molded adsorbent includes activated carbon fiber, granular activated carbon, and a binder. Here, the activated carbon fiber and granular activated carbon correspond to the adsorbent. In one preferred embodiment, the molded adsorbent may be a molded product of a mixture of activated carbon fiber, granular activated carbon, and a binder. In another preferred embodiment, the molded adsorbent may be a laminate structure in which a plurality of sheets, each having powdered activated carbon attached or supported on the surface of an activated carbon fiber sheet, are bound together using a binder.

[0021] In one embodiment of the present invention, the weight ratio of activated carbon fiber to granular activated carbon, based on the total amount of activated carbon fiber and granular activated carbon, can be 5 to 95 parts by weight of activated carbon fiber and 5 to 95 parts by weight of granular activated carbon. In other words, per 100 parts by weight of activated carbon fiber and granular activated carbon contained in the formed adsorbent, the amount of activated carbon fiber is preferably 5 to 95 parts by weight, and the amount of granular activated carbon is preferably 5 to 95 parts by weight. An example of specific numerical values ​​is shown below. Assuming a formed adsorbent containing 10 g of activated carbon fiber and granular activated carbon in total, for example, one example can include 5 g (50 parts by weight) of activated carbon fiber and 5 g (50 parts by weight) of granular activated carbon.

[0022] Although this varies depending on the desired performance of the formed adsorbent, for example, from the viewpoint of prioritizing adsorption / desorption performance for a wide range of concentrations of evaporated fuel gas (particularly n-butane) from low to high, the weight ratio of activated carbon fiber to granular activated carbon (activated carbon fiber:granular activated carbon) can be preferably 5-95 parts by weight:95-5 parts by weight, more preferably 5-70 parts by weight:95-30 parts by weight, and even more preferably 5-45 parts by weight:95-55 parts by weight, 5-40 parts by weight:95-60 parts by weight, or 5-35 parts by weight:95-65 parts by weight. An example of specific numerical values ​​is shown below. Assuming a formed adsorbent containing 10 g of activated carbon fiber and granular activated carbon in total, for example, an example may contain 2 g (20 parts by weight) of activated carbon fiber and 8 g (80 parts by weight) of granular activated carbon.

[0023] Regarding the content of activated carbon fiber and granular activated carbon, from the viewpoint of prioritizing the adsorption / desorption performance for evaporated fuel gas (especially n-butane) over a wide range of concentrations from low to high, the preferred contents are as follows.

[0024] The upper limit of the amount of activated carbon fiber in the molded adsorbent is preferably 95 parts by weight or less, more preferably 70 parts by weight or less, and even more preferably 45, 40, or 35 parts by weight or less per 100 parts by weight of the total weight of the activated carbon fiber and the granular activated carbon. The lower limit of the amount of activated carbon fiber in the molded adsorbent is preferably 5, 8, or 10 parts by weight or more per 100 parts by weight of the total weight of the activated carbon fiber and the granular activated carbon.

[0025] On the other hand, the upper limit of the amount of granular activated carbon in the molded adsorbent may be preferably 95, 92, or 90 parts by weight or less per 100 parts by weight of the total weight of the activated carbon fiber and the granular activated carbon. The lower limit of the amount of granular activated carbon in the molded adsorbent may be preferably 5 parts by weight or more, more preferably 30 parts by weight or more, and even more preferably 55, 60, or 65 parts by weight or more per 100 parts by weight of the total weight of the activated carbon fiber and the granular activated carbon.

[0026] As described above, in one embodiment of the present invention, activated carbon fiber and granular activated carbon are used as components constituting the formed adsorbent. Various embodiments of activated carbon fiber and granular activated carbon will be described in detail later.

[0027] In one embodiment of the present invention, a binder is used as one component constituting the molded adsorbent. The binder that can be used is preferably one that is unlikely to clog the pores of the activated carbon fiber and activated carbon, and examples of such materials include polyvinyl alcohol. Another preferred example of the binder is a fibrous binder. The fibrous binder is not particularly limited as long as it can be fibrillated to entangle the activated carbon fiber and granular activated carbon and shape them. A wide range of binders, both synthetic and natural, can be used. Examples of such fibrous binders include acrylic fiber, polyethylene fiber, polypropylene fiber, polyacrylonitrile fiber, cellulose fiber, nylon fiber, and aramid fiber.

[0028] In one embodiment of the present invention, the content of the binder in the molded adsorbent may be 0.3 to 20 parts by weight per 100 parts by weight of the activated carbon fiber and granular activated carbon. More specifically, the content is as follows. The lower limit of the binder content is preferably 0.3, 0.5, 0.8, 1.0, 2.0, or 3.0 parts by weight. The upper limit of the binder content is preferably 20, 18, 15, or 10 parts by weight. Here are some examples of specific numerical values. For example, assuming a molded adsorbent with a total content of activated carbon fiber and granular activated carbon of 10 g, 0.03 g to 2 g of binder can be added. Therefore, in this case, the total weight of activated carbon fiber, granular activated carbon, and binder in the molded adsorbent is 10.03 g to 12.0 g.

[0029] By blending the binder in the above-mentioned content ratio, the molded adsorbent can be prepared so as to achieve both mechanical strength and adsorption / desorption performance. If higher mechanical strength is desired, the amount of binder can be increased, and if adsorption / desorption performance is more important, the amount of binder can be set lower. Furthermore, such a content can be suitable for obtaining a molded adsorbent with low pressure loss.

[0030] The activated carbon fiber is preferably mixed in the form of defibrated fibers. By mixing the defibrated fibers with components such as granular activated carbon and a binder, the components are adequately entangled and bonded well, which improves the mechanical strength of the molded body and makes it more resistant to deformation.

[0031] In various further embodiments of the present invention, a more preferable molded adsorbent for a canister can be obtained by further satisfying one or any two or more of the following specified conditions. The preferable combination of the following specified conditions can be arbitrarily selected as desired depending on the required requirements, etc.

[0032] <Total pore volume of molded adsorbent> In one embodiment of the present invention, the total pore volume of the formed adsorbent is preferably 0.90 to 2.00 cm 3 / g or less. More specifically, it is as follows. In one embodiment of the present invention, the lower limit of the total pore volume of the formed adsorbent body is preferably 0.90 cm 3 / g or more, more preferably 0.98 or 1.00 cm 3 / g or more, more preferably 1.05 or 1.10 cm 3 / g or more. In one embodiment of the present invention, the upper limit of the total pore volume of the formed adsorbent body is preferably 2.00 cm 3 / g or less, more preferably 1.80 cm 3 / g or less, more preferably 1.50 cm 3 / g or less. Setting the total pore volume within the above range is suitable for obtaining a molded adsorbent that has excellent adsorption / desorption performance for evaporated fuel gases (especially n-butane) over a wide range of concentrations, from low to high, and is also suitable from the viewpoint of obtaining a molded adsorbent that can suppress pressure loss.

[0033] <Average pore size of molded adsorbent (average pore diameter)> In one embodiment of the present invention, the average pore size of the formed adsorbent may preferably be 1.87 to 4.00 nm. In one embodiment of the present invention, the lower limit of the average pore size of the formed adsorbent is preferably 1.87 nm or more, more preferably 1.90 nm or more, and even more preferably 2.00 nm or more. In one embodiment of the present invention, the upper limit of the average pore size of the formed adsorbent can be any value, but is preferably 4.00 nm or less, more preferably 3.00 nm or less, and even more preferably 2.50 nm or less. Setting the average pore size within the above range is suitable for obtaining a molded adsorbent that has excellent adsorption and desorption performance for evaporated fuel gases (particularly n-butane) over a wide range of concentrations from low to high.

[0034] <Specific surface area of ​​molded adsorbent> In one embodiment of the present invention, the specific surface area of ​​the formed adsorbent is preferably 1400 to 2500 m 2 / g or less. More specifically, it is as follows. In one embodiment of the present invention, the lower limit of the specific surface area of ​​the formed adsorbent body is preferably 1400 or 1410 m 2 / g or more, more preferably 1450, 1460, or 1480m 2 / g or more, more preferably 1490 or 1500m 2 / g or more. In one embodiment of the present invention, the upper limit of the specific surface area of ​​the molded adsorbent is generally 2500, 2400, or 2300 m, although a larger specific surface area is generally preferable from the viewpoint of adsorption and desorption performance. 2 / g or less. By setting the specific surface area within the above range, a molded adsorbent having better adsorption / desorption performance for evaporated fuel gas (particularly n-butane) can be obtained. Furthermore, in one embodiment of the present invention, a large specific surface area can be maintained for an adsorbent material used in a canister such as the above, while achieving a reduction in pressure loss in the canister.

[0035] <Ultramicropore volume of the formed adsorbent: V 0.7 > In this disclosure, the term "ultramicropores" refers to pores with a pore diameter of 0.7 nm or less. In one embodiment of the present invention, the ultramicropore volume of the formed adsorbent is preferably 0.05 to 0.30 cm 3 / g. More specifically, it is as follows. In one embodiment of the present invention, the lower limit of the ultramicropore volume of the formed adsorbent body is preferably 0.05 cm 3 / g or more, more preferably 0.08 cm 3 / g or more, more preferably 0.10 cm 3 / g or more. In one embodiment of the present invention, the upper limit of the ultramicropore volume of the formed adsorbent body is preferably 0.30 cm 3 / g or less, more preferably 0.29 cm 3 / g or less, more preferably 0.26, 0.24, 0.22, or 0.20 cm 3 / g or less. Setting the ultramicropore volume within the above range is suitable for producing a molded adsorbent that is excellent in terms of adsorption / desorption performance, pressure loss, and the like.

[0036] <Micropore volume of the formed adsorbent: V 2.0 > In this disclosure, the term "micropore" refers to a pore with a pore diameter of 2.0 nm or less. In one embodiment of the present invention, the micropore volume of the formed adsorbent is preferably 0.50 to 1.00 cm. 3 / g. More specifically, it is as follows. In one embodiment of the present invention, the lower limit of the micropore volume of the formed adsorbent body is preferably 0.50 cm 3 / g or more, more preferably 0.55 or 0.58 cm 3 / g or more, more preferably 0.59 or 0.60 cm 3 / g or more. In one embodiment of the present invention, the upper limit of the micropore volume of the formed adsorbent body is preferably 1.00 cm 3 / g or less, more preferably 0.90 cm 3 / g or less, more preferably 0.80 cm 3 / g or less. Setting the micropore volume within the above range is suitable for producing a molded adsorbent that is excellent in terms of adsorption / desorption performance, pressure loss, and the like.

[0037] <V: Pore volume of pores with diameters greater than 0.7 nm and less than 2.0 nm 0.7-2.0 > Pore ​​volume V of pores with a diameter of more than 0.7 nm and less than 2.0 nm 0.7-2.0 can be calculated by the following formula 1 using the value a of the ultramicropore volume and the value b of the micropore volume. V 0.7-2.0 =ba (Equation 1)

[0038] In one embodiment of the present invention, the pore volume V of the pores having a pore diameter of more than 0.7 nm and not more than 2.0 nm for the formed adsorbent is 0.7-2.0 is preferably 0.30 to 1.00 cm 3 / g. More specifically, it is as follows. In one embodiment of the present invention, the pore volume V of the pores having a pore diameter of more than 0.7 nm and not more than 2.0 nm for the formed adsorbent is 0.7-2.0 The lower limit is preferably 0.30 cm 3 / g or more, more preferably 0.36 cm 3 / g or more, more preferably 0.38, 0.40, or 0.43 cm 3 / g or more. In one embodiment of the present invention, the pore volume V of the pores having a pore diameter of more than 0.7 nm and not more than 2.0 nm for the formed adsorbent is 0.7-2.0 The upper limit is preferably 1.00 cm 3 / g or less, more preferably 0.90 cm 3 / g or less, more preferably 0.80, 0.75, 0.70, 0.65, or 0.60 cm 3 / g or less. The pore volume V 0.7-2.0 Setting the value of the adsorbent in the above range is suitable for obtaining a molded adsorbent excellent in adsorption / desorption performance and pressure loss.

[0039] <Ratio of the volume of ultramicropores to the volume of micropores: R 0.7 / 2.0 > The ratio R of the volume of ultramicropores with a pore diameter of 0.7 nm or less to the volume of micropores with a pore diameter of 2.0 nm or less 0.7 / 2.0 can be calculated by the following formula 2 using the value a of the ultramicropore volume and the value b of the micropore volume. R 0.7 / 2.0 =a / b×100(%) (Formula 2)

[0040] In one embodiment of the present invention, the abundance ratio R of the ultramicropore volume to the micropore volume of the formed adsorbent is 0.7 / 2.0 is preferably 10.0 to 60.0%. More specifically, it is as follows. In one embodiment of the present invention, the abundance ratio R of the ultramicropore volume to the micropore volume of the formed adsorbent is 0.7 / 2.0 The lower limit of the above range is preferably 10.0% or more, more preferably 13.0% or more, and even more preferably 15.0% or more. In one embodiment of the present invention, the abundance ratio R of the ultramicropore volume to the micropore volume of the formed adsorbent is 0.7 / 2.0 The upper limit of may be preferably 60.0% or less, more preferably 50% or less, and even more preferably 40, 30, or 25% or less. The abundance ratio R of the ultramicropore volume0.7 / 2.0 Setting the value of the adsorbent in the above range is suitable for obtaining a molded adsorbent excellent in adsorption / desorption performance and pressure loss.

[0041] <Dry density of molded adsorbent> In one embodiment of the present invention, the dry density of the molded adsorbent is preferably 0.010 to 0.400 g / cm 3 More specifically, it can be as follows. In the formed adsorbent body according to one embodiment of the present invention, the preferred lower and upper limits of the dry density of the formed adsorbent body may be as follows. The lower limit of the dry density of the molded adsorbent is preferably 0.010 g / cm 3 More preferably, 0.015 g / cm 3 More preferably, 0.020 g / cm 3 , 0.030, 0.040, 0.050, or 0.060 g / cm 3 It could be more than that. The upper limit of the dry density of the molded adsorbent body is preferably 0.400 g / cm 3 or less, more preferably 0.300 g / cm 3 More preferably, 0.250 g / cm or less 3 It can be the following:

[0042] By setting the dry density within the above range, it is possible to obtain a molded adsorbent having superior adsorption / desorption performance per volume required for canisters, within the range of the adsorbent capacity that can be stored in the canister. Furthermore, by setting the dry density at or above the above lower limit, it is possible to avoid a decrease in mechanical properties (e.g., strength) even when the molded adsorbent is formed into a sheet or disk shape. Furthermore, the dry density of the molded adsorbent can be adjusted by adjusting the fiber diameter of the carbon fiber, the fiber length by adjusting the stirring force during defibration of the carbon fiber, and the suction force when suction molding the mixed slurry with the binder. Adjusting the dry density can be one way to optimize the adsorption / desorption performance per volume and the pressure loss.

[0043] <n-Butane adsorption / desorption performance of molded adsorbent> In one embodiment of the present invention, the molded adsorbent preferably has a predetermined n-butane adsorption / desorption performance as an adsorbent. Since n-butane adsorption / desorption performance is an index of the adsorption / desorption performance of evaporated gases, those with excellent n-butane adsorption / desorption performance are suitable for use in automobile canisters. The n-butane adsorption / desorption performance can be expressed as the effective adsorption rate of n-butane per molded adsorbent, which is calculated by desorbing n-butane from the adsorbent under predetermined desorption conditions after sufficient absorption breakthrough, and then repeating the adsorption.

[0044] A preferred embodiment of the formed adsorbent of the present invention is a formed adsorbent having an effective adsorption / desorption rate (wt%) of n-butane within a predetermined range, where the effective adsorption / desorption rate (wt%) of n-butane is determined according to the measurement method shown in the Examples below (see Equation 8 below).

[0045] In a preferred embodiment of the formed adsorbent, the effective adsorption / desorption rate (wt%) of 100% n-butane is preferably 30.0 wt% or more, more preferably 35.0 wt% or more, and even more preferably 37.0, 39.0, or 40.0 wt% or more.

[0046] In one preferred embodiment of the formed adsorbent, the effective adsorption / desorption rate (wt%) of 0.2% n-butane is preferably 3.50 wt% or more, more preferably 3.80 wt% or more, and even more preferably 4.00 wt% or more.

[0047] A preferred embodiment of the formed adsorbent is one in which the effective adsorption / desorption rate (%) of n-butane is within a predetermined range, where the effective adsorption / desorption rate (%) of n-butane is determined according to the measurement method shown in the Examples below (see Equation 9 below).

[0048] In a preferred embodiment of the formed adsorbent, the effective adsorption / desorption rate (%) of 100% n-butane is preferably 75.0% or more, more preferably 79.0% or more, and even more preferably 80.0 or 81.0% or more.

[0049] In a preferred embodiment of the formed adsorbent, the effective adsorption / desorption rate (%) of 0.2% n-butane is preferably 50.0% or more, more preferably 55.0 or 56.0% or more, and even more preferably 60.0 or 70.0% or more.

[0050] <BWC of molded adsorbent> In a preferred embodiment of the formed adsorbent of the present invention, the BWC (Butane Working Capacity) is preferably within a predetermined range, as determined by the measurement method shown in the Examples below. In one preferred embodiment of the formed adsorbent, the BWC in the case of 100% n-butane can be preferably 0.4 to 10.0 g / dL.

[0051] <0 ppm maintenance time of molded adsorbent> The 0 ppm retention time (in the case of 0.2% n-butane) determined according to the measurement method shown in the Examples below is usually better the longer it is, but to give specific numerical values, in a preferred embodiment of the formed adsorbent of the present invention, it is preferably 15 minutes or 30 minutes or more, more preferably 40 minutes or more, and even more preferably 50 minutes, 55 minutes, 60 minutes, 65 minutes, 68 minutes, 69 minutes, or 70 minutes or more. The longer the 0 ppm maintenance time, the longer it takes for the adsorbent to begin releasing the adsorbed substance. Therefore, the 0 ppm maintenance time is an index of the strength of the adsorption force.

[0052] In another embodiment of the present invention, the molded adsorbent can have low pressure drop. Activated carbon fiber itself is a material with low pressure drop among several types of activated carbon. However, activated carbon fiber alone tends to easily lose its shape. Therefore, the inventors devised a method of molding activated carbon fiber with granular activated carbon and a binder to improve shape stability. Initially, it was anticipated that molding would improve shape stability, but that even in good cases, the average pressure drop between the molded body of activated carbon fiber and binder and the granular activated carbon and binder, or the pressure drop between the molded body of activated carbon fiber and a binder, would be large. However, unexpectedly, a molded adsorbent was obtained in which the pressure drop of the molded body of this three-component mixture was lower than that of a molded body of a two-component mixture of activated carbon fiber and a binder, or that of a molded body of a two-component mixture of granular activated carbon and a binder.

[0053] The mechanism of action is not entirely clear, but one hypothesis is that although activated carbon fiber and granular activated carbon are both activated carbons, they are different materials in terms of physical properties such as shape. Therefore, it is thought that the mixing of the different materials creates voids, which act to reduce pressure loss.

[0054] There may be various variations in the conditions for suppressing pressure loss using a three-component mixture, but one method is, for example, adjusting the balance of the amounts of activated carbon fiber and granular activated carbon mixed together or the state of their mixture.

[0055] In one embodiment of the present invention, the pressure loss may be preferably 0.05 to 0.52 kPa. More specifically, it is as follows. In one embodiment of the present invention, the upper limit of the pressure drop of the formed adsorbent may be preferably 0.52, 0.50, 0.45, or 0.43 kPa or less, more preferably 0.40, 0.38, 0.35, or 0.33 kPa or less, and even more preferably 0.30, 0.28, or 0.25 kPa or less. The lower the pressure loss, the more preferable it is, and from the viewpoint of the original purpose of adsorption, the lower limit of the pressure loss may preferably be 0.05 kPa, 0.08, or 0.10 kPa or more.

[0056] 2. Shape of the molded adsorbent In one embodiment of the present invention, the shape of the formed adsorbent is not particularly limited, and is preferably, for example, a shape that can be molded and allows gas to flow through. Specific shapes include, for example, columns with circular or polygonal end faces, truncated cones, truncated polygonal pyramids, and other truncated cones, as well as pellets and honeycombs, with preferred shapes being columns and rectangular parallelepipeds. Furthermore, a plurality of disk-, sheet-, or plate-shaped formed adsorbents may be stacked to form a laminate. Figures 1 to 3 show several embodiments. In the drawings, dimensions such as length and thickness are shown schematically to facilitate understanding of the invention, and are not limited thereto.

[0057] The laminated adsorbent 1 shown in FIG. 1 is a laminate formed by stacking four molded adsorbent sheets 10. The sheet-like molded adsorbent 10 is formed by stacking the main surfaces 10a of the sheets one on top of the other. In one embodiment, each sheet 10 can be formed by molding a mixture of activated carbon fiber, granular activated carbon, and a binder into a sheet. The binder can be preferably a fibrous binder.

[0058] The stacked adsorbent 1 may be housed in the canister in any manner. In a preferred embodiment, the sheet-shaped adsorbent is arranged so that the main surface 10a is not perpendicular to the flow direction of the fluid F, such as the evaporated gas. More preferably, as shown in FIG. 1, the main surface a may be arranged so that it is substantially parallel to the flow direction of the fluid F, such as the evaporated gas. By arranging the main surfaces a so that they are substantially parallel to the flow direction of the fluid F, such as the evaporated gas, the side end surfaces 10b of the multiple sheet-shaped adsorbents are arranged so that they face the flow direction of the fluid F. This arrangement can suppress pressure loss. In FIG. 1, the shorter side end surfaces 10b face the flow direction of the fluid F, but this is not a limitation; the longer side end surfaces 10c may also face the flow direction of the fluid F.

[0059] The stacked adsorbent may have a rectangular parallelepiped shape or a cubic shape as a whole.

[0060] Another embodiment of the present invention is shown in Figure 2. In the embodiment shown in Figure 2, the molded adsorbent body is molded into a disk shape. These disk-shaped molded adsorbents may be stacked to form a cylindrical shape.

[0061] Another embodiment of the present invention is shown in Figure 3. In the embodiment shown in Figure 3, the molded adsorbent body is integrally molded as a cylindrical molded body.

[0062] Another possible embodiment of the present invention is as follows. A laminated adsorbent may be formed by preparing activated carbon fiber sheets with granular activated carbon attached or supported on the surface thereof, and bonding the sheets together using a binder. The laminated adsorbent may have a structure in which granular activated carbon is sandwiched near the interface between the sheets, and the overall view of the laminated adsorbent may be substantially similar to the laminated adsorbent 1 shown in FIG. 1.

[0063] As described above, the adsorptive laminate according to one embodiment of the present invention can be easily processed or molded into various shapes, and is a material that is easy to handle.

[0064] 3. Granular activated carbon In the present disclosure, granular activated carbon refers to activated carbon with an average particle size of 100 to 3000 μm.

[0065] In one embodiment of the present invention, granular activated carbon is used as one type of activated carbon. Hereinafter, embodiments of granular activated carbon that can be used in the present invention will be described in more detail. In one embodiment of the present invention, the granular activated carbon that can be used in the molded adsorbent for canisters can be made into a more preferred embodiment by further satisfying at least one or any two or more of the following specified conditions. A preferred combination of the following specified conditions can be selected as desired depending on the required requirements, etc.

[0066] <Average particle size of granular activated carbon> In one embodiment of the present invention, the average particle size of the granular activated carbon used in the molded adsorbent may be preferably 100 to 3000 μm. More specifically, it is as follows. In one embodiment of the present invention, the lower limit of the average particle size of the granular activated carbon used in the formed adsorbent may be preferably 100 μm or more, more preferably 120, 140, or 160 μm or more, and even more preferably 180 μm or more. In one embodiment of the present invention, the upper limit of the average particle size of the granular activated carbon used in the formed adsorbent may be preferably 3000 μm or less, more preferably 2500, 2000, 1500, 1000, or 800 μm or less, and even more preferably 600 μm or less. The above-mentioned range of average particle size of the granular activated carbon used in the molded adsorbent is suitable for combining with activated carbon fibers to obtain a molded adsorbent with excellent adsorption / desorption performance for evaporated fuel gases (particularly n-butane) over a wide range of concentrations, from low to high. Furthermore, the above-mentioned range of average particle size of the granular activated carbon is also suitable from the viewpoint of obtaining a molded adsorbent that can suppress pressure loss.

[0067] <Total pore volume of granular activated carbon> In one embodiment of the present invention, the total pore volume of the granular activated carbon used in the formed adsorbent is preferably 0.90 to 2.50 cm 3 / g. More specifically, it is as follows. In one embodiment of the present invention, the lower limit of the total pore volume of the granular activated carbon used in the formed adsorbent is preferably 0.90 cm 3 / g or more, more preferably 1.00 cm 3 / g or more, more preferably 1.10, 1.20, or 1.30 cm 3 / g or more. In one embodiment of the present invention, the upper limit of the total pore volume of the granular activated carbon used in the formed adsorbent body is preferably 2.50 cm 3 / g or less, more preferably 2.20 or 2.00 cm 3 / g or less, more preferably 1.80, 1.70 or 1.60 cm 3 / g or less. Setting the total pore volume of the granular activated carbon within the above range is suitable for combining it with activated carbon fibers to obtain a molded adsorbent that has excellent adsorption / desorption performance for evaporated fuel gases (particularly n-butane) over a wide range of concentrations, from low to high. Setting the total pore volume of the granular activated carbon within the above range can be suitable for improving the adsorption / desorption performance for evaporated fuel gases (particularly n-butane) at relatively high concentrations, relative to activated carbon fibers. Furthermore, setting the total pore volume of the granular activated carbon within the above range is also suitable from the perspective of obtaining a molded adsorbent that can suppress pressure loss.

[0068] <Average pore size of granular activated carbon (average pore diameter)> In one embodiment of the present invention, the average pore size of the granular activated carbon contained in the molded adsorbent may be preferably 2.00 to 4.00 nm. More specifically, it is as follows. In one embodiment of the present invention, the lower limit of the average pore size of the granular activated carbon used in the formed adsorbent may be preferably 2.00 nm or more, more preferably 2.10 nm or more, and even more preferably 2.20 or 2.30 nm or more. In one embodiment of the present invention, the upper limit of the average pore size of the granular activated carbon used in the formed adsorbent can be any value, but is preferably 4.00 nm or less, more preferably 3.50 nm or less, and even more preferably 3.00 nm or less. Setting the average pore size of the granular activated carbon within the above range is suitable for combining with activated carbon fiber to obtain a molded adsorbent with excellent adsorption / desorption performance for evaporated fuel gases (particularly n-butane) over a wide range of concentrations, from low to high. Setting the average pore size of the granular activated carbon within the above range can be suitable for improving the adsorption / desorption performance for evaporated fuel gases (particularly n-butane) with relatively high concentrations, relative to activated carbon fiber. Furthermore, setting the average pore size of the granular activated carbon within the above range is also suitable from the viewpoint of obtaining a molded adsorbent that can suppress pressure loss.

[0069] <Specific surface area of ​​granular activated carbon> In one embodiment of the present invention, the specific surface area of ​​the granular activated carbon used in the molded adsorbent is preferably 1400 to 2700 m 2 / g. More specifically, it is as follows. In one embodiment of the present invention, the lower limit of the specific surface area of ​​the granular activated carbon used in the molded adsorbent is preferably 1400 m 2 / g or more, more preferably 1450 or 1500m 2 / g or more, more preferably 1550 or 1600m 2 / g or more. In one embodiment of the present invention, the specific surface area of ​​the granular activated carbon used in the molded adsorbent is generally preferably larger from the viewpoint of adsorption performance. In the case of an adsorbent for a canister, the upper limit of the specific surface area of ​​the granular activated carbon is generally 2700, 2600, or 2500 m. 2 / g or less. Setting the specific surface area of ​​the granular activated carbon within the above range is suitable for combining it with activated carbon fiber to obtain a molded adsorbent with excellent adsorption / desorption performance for evaporated fuel gases (particularly n-butane) over a wide range of concentrations, from low to high. Setting the specific surface area of ​​the granular activated carbon within the above range can be suitable for improving the adsorption / desorption performance for evaporated fuel gases (particularly n-butane) with relatively high concentrations, relative to activated carbon fiber. Furthermore, setting the average pore size of the granular activated carbon within the above range is also suitable from the viewpoint of obtaining a molded adsorbent that can suppress pressure loss.

[0070] Ultramicropore volume of granular activated carbon: V 0.7 > In one embodiment of the present invention, the ultramicropore volume of the granular activated carbon used in the formed adsorbent is preferably 0.05 to 0.30 cm. 3 / g. More specifically, it is as follows. In one embodiment of the present invention, the lower limit of the ultramicropore volume of the granular activated carbon used in the formed adsorbent is preferably 0.05 cm 3 / g or more, more preferably 0.08 cm 3 / g or more, more preferably 0.10 cm 3 / g or more. In one embodiment of the present invention, the upper limit of the ultramicropore volume of the granular activated carbon used in the formed adsorbent is preferably 0.30 cm 3 / g or less, more preferably 0.25 cm 3 / g or less, more preferably 0.23, 0.20, 0.18, or 0.15 cm 3 / g or less. Setting the ultramicropore volume of the granular activated carbon within the above range is suitable for producing a molded adsorbent that is excellent in terms of adsorption / desorption performance, pressure loss, and the like.

[0071] <Micropore volume of granular activated carbon: V 2.0 > In one embodiment of the present invention, the micropore volume of the granular activated carbon used in the formed adsorbent is preferably 0.40 to 1.00 cm.3 / g. More specifically, it is as follows. In one embodiment of the present invention, the lower limit of the micropore volume of the granular activated carbon used in the formed adsorbent is preferably 0.40 cm 3 / g or more, more preferably 0.45 or 0.50 cm 3 / g or more, more preferably 0.55 cm 3 / g or more. In one embodiment of the present invention, the upper limit of the micropore volume of the granular activated carbon used in the formed adsorbent is preferably 1.00 cm. 3 / g or less, more preferably 0.90 cm 3 / g or less, more preferably 0.80 cm 3 / g or less. Setting the micropore volume of the granular activated carbon within the above range is suitable for producing a molded adsorbent that is excellent in terms of adsorption / desorption performance, pressure loss, and the like.

[0072] <V: Pore volume of pores with diameters greater than 0.7 nm and less than 2.0 nm 0.7-2.0 (Granular activated carbon)> In one embodiment of the granular activated carbon used in the formed adsorbent, the pore volume V of pores having a pore diameter of more than 0.7 nm and not more than 2.0 nm is 0.7-2.0 is preferably 0.20 to 1.20 cm 3 / g. More specifically, it is as follows. In one embodiment of the granular activated carbon used in the formed adsorbent, the pore volume V of pores having a pore diameter of more than 0.7 nm and not more than 2.0 nm is 0.7-2.0 The lower limit is preferably 0.20 cm 3 / g or more, more preferably 0.30, 0.36, or 0.40 cm 3 / g or more, more preferably 0.43, 0.45, or 0.50 cm 3 / g or more. In one embodiment of the granular activated carbon used in the formed adsorbent, the pore volume V of pores having a pore diameter of more than 0.7 nm and not more than 2.0 nm is 0.7-2.0 The upper limit is preferably 1.20 cm 3 / g or less, more preferably 1.00 cm3 / g or less, more preferably 0.90, 0.80, 0.75, 0.70, 0.65, or 0.60 cm 3 / g or less. The pore volume V of the granular activated carbon 0.7-2.0 Setting the value of the adsorbent in the above range is suitable for obtaining a molded adsorbent excellent in adsorption / desorption performance and pressure loss.

[0073] <Ratio of the volume of ultramicropores to the volume of micropores: R 0.7 / 2.0 (About granular activated carbon) In one embodiment of the granular activated carbon used in the formed adsorbent, the abundance ratio R of the ultramicropore volume to the micropore volume is 0.7 / 2.0 is preferably 10.0 to 50.0%. More specifically, it is as follows. In one embodiment of the granular activated carbon used in the formed adsorbent, the abundance ratio R of the ultramicropore volume to the micropore volume is 0.7 / 2.0 The lower limit of the above range is preferably 10.0% or more, more preferably 12.0% or more, and even more preferably 14.0 or 15.0% or more. In one embodiment of the granular activated carbon used in the molded adsorbent, the abundance ratio R of the ultramicropore volume to the micropore volume is 0.7 / 2.0 The upper limit of the ratio may be preferably 50.0% or less, more preferably 40.0, 30.0, or 25% or less, and even more preferably 20.0% or less. The abundance ratio R of the relevant ultramicropore volume of granular activated carbon 0.7 / 2.0 Setting the value of the adsorbent in the above range is suitable for obtaining a molded adsorbent excellent in adsorption / desorption performance and pressure loss.

[0074] <Humidity-controlled density of granular activated carbon (at a temperature of 23°C and a relative humidity of 50%)> In one embodiment of the present invention, the granular activated carbon used in the formed adsorbent may preferably have a predetermined density. The density may be measured using the humidity-conditioned density. In this disclosure, the humidity-conditioned density is the density measured under conditions of 23°C and 50% relative humidity.

[0075] In one embodiment of the present invention, the humidity-controlled density (density under conditions of 23°C and 50% relative humidity) of the granular activated carbon used in the molded adsorbent is preferably 0.10 to 0.80 g / cm. 3 More specifically, it can be as follows. In one embodiment of the present invention, the lower limit of the humidity-controlled density (density under conditions of 23°C and 50% relative humidity) of the granular activated carbon used in the molded adsorbent is preferably 0.10 g / cm 3 or more, more preferably 0.15, 0.2, 0.25, or 0.30 g / cm 3 It could be more than that. In one embodiment of the present invention, the upper limit of the humidity-controlled density of the granular activated carbon used in the molded adsorbent is preferably 0.80 g / cm. 3 or less, more preferably 0.70, 0.60, 0.55, 0.50, or 0.45 g / cm 3 It can be the following: Setting the water content within the above range under the above conditions is suitable for producing a molded adsorbent that is excellent in terms of adsorption / desorption performance, pressure loss, and the like.

[0076] 4. Activated carbon fiber In one embodiment of the present invention, activated carbon fiber is used as one type of activated carbon. As a preferred embodiment of the present invention, for example, a formed adsorbent is provided in which the total pore volume of the activated carbon fiber is smaller than the total pore volume of the granular activated carbon, and the average pore diameter of the activated carbon fiber is smaller than the average pore diameter of the granular activated carbon.

[0077] Here, "the total pore volume of the activated carbon fiber is smaller than the total pore volume of the granular activated carbon" does not mean that it is smaller than the lower limit of the range of values ​​for the activated carbon fiber set forth in the present disclosure, but means that it is smaller than the total pore volume of the granular activated carbon employed in each individual molded adsorbent. For example, when the total pore volume of the activated carbon fiber contained in the molded adsorbent is 1.00 cm 3 / g, the total pore volume of the granular activated carbon is 1.00 cm 3 / g. In the present disclosure, unless otherwise specified, the same applies to other items such as the average pore diameter.

[0078] The above-mentioned granular activated carbon and activated carbon fiber are both types of activated carbon, but they can exhibit different performance characteristics in terms of various properties such as adsorption / desorption performance. Although the above-mentioned embodiment does not clearly distinguish between the roles of the two, it is possible to prepare the granular activated carbon to mainly play the role of adsorption / desorption for high-concentration evaporated fuel gas, and the activated carbon fiber to mainly play the role of adsorption / desorption for low-concentration evaporated fuel gas.

[0079] The following is a more detailed description of embodiments of activated carbon fibers that can be used in the present invention. Activated carbon fibers that can be used in the molded adsorbent for canisters can be made into more preferred embodiments by satisfying at least one or any two or more of the following specified conditions. Preferred combinations of the following specified conditions can be selected as desired depending on the required requirements.

[0080] <Fiber diameter of activated carbon fiber> In one embodiment of the present invention, the fiber diameter of the activated carbon fiber used in the molded adsorbent may be preferably 6.0 to 70.0 μm. More specifically, the diameter is as follows. In one embodiment of the present invention, the lower limit of the fiber diameter of the activated carbon fiber used in the molded adsorbent may be preferably 4.0 μm or more, more preferably 6.0 μm or more, and even more preferably 8.0, 10.0, 12.0, 14.0, 18.0, 19.0, or 20.0 μm or more. In one embodiment of the present invention, the upper limit of the fiber diameter of the activated carbon fiber used in the molded adsorbent can be any value from the viewpoint of suppressing pressure loss, but considering the balance with the adsorption / desorption performance, the upper limit can be, for example, 70.0 μm or less, preferably 65.0 or 60.0 μm or less, and more preferably 59.0, 58.0, 57.0, 56.0, or 55.0 μm or less. The fiber diameter of the activated carbon fiber that can be used in the molded adsorbent is within the above range, which is suitable for obtaining a molded adsorbent that is excellent in terms of adsorption / desorption performance and pressure loss.

[0081] <Average fiber length of activated carbon fibers (or average fiber length)> In one embodiment of the present invention, the average fiber length of the activated carbon fibers used in the molded adsorbent may preferably be 300 to 10,000 μm. In one embodiment of the present invention, the lower limit of the average fiber length of the activated carbon fibers used in the molded adsorbent may be preferably 300 μm or more, more preferably 500, 600, 700, 800, 850, or 900 μm or more, and even more preferably 950 μm or more. In one embodiment of the present invention, the upper limit of the average fiber length of the activated carbon fibers used in the molded adsorbent may be preferably 10,000, 7,500, or 5,000 μm, more preferably 4,000, 3,000, 2,500, 2,000, or 1,500 μm, and even more preferably 1,200 μm. When the average fiber length of the activated carbon fibers used in the molded adsorbent is within the above range, it is suitable for obtaining a molded adsorbent that is excellent in terms of adsorption / desorption performance and pressure loss.

[0082] <Fineness of activated carbon fiber precursor> In order to obtain activated carbon fibers having the above-described fiber diameters, the fiber diameter (as fineness) of the precursor fiber of the activated carbon fiber is preferably within the following ranges. That is, it can be said that using the following fibers as precursors is suitable for obtaining activated carbon fibers that are excellent in terms of adsorption / desorption performance and pressure loss. In one embodiment of the present invention, the fiber diameter (fineness) of the precursor fiber may preferably be 1.0 to 70.0 dtex. More specifically, it is as follows. The lower limit of the fiber diameter (fineness) of the precursor fiber is preferably 1.0 dtex or more, more preferably 4.0 or 7.0 dtex or more, and even more preferably 10.0 dtex or more. The upper limit of the fiber diameter (as fineness) of the precursor fiber can be, for example, 70.0 dtex or less, preferably 65.0 dtex or less, and more preferably 60.0 dtex.

[0083] <Total pore volume of activated carbon fiber> In one embodiment of the present invention, the total pore volume of the activated carbon fiber used in the formed adsorbent is preferably 0.50 to 1.20 cm. 3 / g. More specifically, it is as follows. In one embodiment of the present invention, the lower limit of the total pore volume of the activated carbon fiber used in the formed adsorbent is preferably 0.50 cm 3 / g or more, more preferably 0.60 or 0.70 cm 3 / g or more, more preferably 0.80 cm 3 / g or more. In one embodiment of the present invention, the upper limit of the total pore volume of the activated carbon fiber used in the formed adsorbent is preferably 1.20 cm 3 / g or less, more preferably 1.10 cm 3 / g or less, more preferably 1.00 cm 3 / g or less. Setting the total pore volume of the activated carbon fiber within the above range is suitable for combining it with granular activated carbon to obtain a molded adsorbent that has excellent adsorption / desorption performance for evaporated fuel gases (particularly n-butane) over a wide range of concentrations, from low to high. Setting the total pore volume of the activated carbon fiber within the above range can be suitable for improving the adsorption / desorption performance for evaporated fuel gases (particularly n-butane) with relatively low concentrations, relative to granular activated carbon. Furthermore, setting the average pore diameter of the activated carbon fiber within the above range is also suitable from the viewpoint of obtaining a molded adsorbent that can suppress pressure loss.

[0084] <Average pore size of activated carbon fiber> In one embodiment of the present invention, the average pore size of the activated carbon fiber used in the molded adsorbent may preferably be 1.60 to 4.00 nm. More specifically, this is as follows. In one embodiment of the present invention, the lower limit of the average pore size of the activated carbon fiber used in the formed adsorbent may be preferably 1.60 nm or more, more preferably 1.65 nm or more, and even more preferably 1.70 or 1.73 nm or more. In one embodiment of the present invention, the upper limit of the average pore size of the activated carbon fiber used in the formed adsorbent can be any value, but is preferably 4.00 or 3.50 nm or less, more preferably 3.00 or 2.50 nm or less, and even more preferably 2.30 or 2.10 nm or less. Setting the average pore size of the activated carbon fiber within the above range is suitable for combining with granular activated carbon to obtain a molded adsorbent with excellent adsorption / desorption performance for evaporated fuel gases (particularly n-butane) over a wide range of concentrations, from low to high. Setting the average pore size of the activated carbon fiber within the above range can be suitable for improving the adsorption / desorption performance for evaporated fuel gases (particularly n-butane) with relatively low concentrations, relative to granular activated carbon. Furthermore, setting the average pore size of the activated carbon fiber within the above range is also suitable from the viewpoint of obtaining a molded adsorbent that can suppress pressure loss.

[0085] <Specific surface area of ​​activated carbon fiber> In one embodiment of the present invention, the specific surface area of ​​the activated carbon fiber used in the molded adsorbent is preferably 1100 to 2400 m 2 / g. More specifically, it is as follows. In one embodiment of the present invention, the lower limit of the specific surface area of ​​the activated carbon fiber used in the molded adsorbent is preferably 1100 m 2 / g or more, more preferably 1200, 1300, 1400, 1500, or 1600 m 2 / g or more, more preferably 1700 or 1800m 2 / g or more. In one embodiment of the present invention, the specific surface area of ​​the activated carbon fiber used in the molded adsorbent is generally preferably larger from the viewpoint of adsorption performance. In the case of an adsorbent for a canister, the upper limit of the specific surface area is generally 2400, 2300, 2200, or 2100 m. 2 / g or less. Setting the specific surface area of ​​the activated carbon fiber within the above range is suitable for combining it with granular activated carbon to obtain a molded adsorbent with excellent adsorption / desorption performance for evaporated fuel gases (particularly n-butane) over a wide range of concentrations, from low to high. Setting the specific surface area of ​​the activated carbon fiber within the above range can be suitable for improving the adsorption / desorption performance for evaporated fuel gases (particularly n-butane) with relatively low concentrations, relative to granular activated carbon. Furthermore, setting the average pore diameter of the activated carbon fiber within the above range is suitable for suppressing pressure loss while maintaining a wide specific surface area.

[0086] <Ultramicropore volume of activated carbon fiber: V 0.7 > In one embodiment of the present invention, the ultramicropore volume of the activated carbon fiber used in the molded adsorbent is preferably 0.05 to 0.30 cm. 3 / g. More specifically, it is as follows. In one embodiment of the present invention, the lower limit of the ultramicropore volume of the activated carbon fiber used in the formed adsorbent is preferably 0.05 cm. 3 / g or more, more preferably 0.08 cm 3 / g or more, more preferably 0.10 cm 3 / g or more. In one embodiment of the present invention, the upper limit of the ultramicropore volume of the activated carbon fiber used in the formed adsorbent is preferably 0.30 cm. 3 / g or less, more preferably 0.25 cm 3 / g or less, more preferably 0.23, 0.20, 0.18, or 0.15 cm 3 / g or less. Setting the ultramicropore volume of the activated carbon fiber within the above range is suitable for forming a molded adsorbent that is excellent in terms of adsorption / desorption performance, pressure loss, and the like.

[0087] <Micropore volume of activated carbon fiber: V 2.0 > In one embodiment of the present invention, the micropore volume of the activated carbon fiber used in the molded adsorbent is preferably 0.40 to 1.00 cm. 3 / g. More specifically, it is as follows. In one embodiment of the present invention, the lower limit of the micropore volume of the activated carbon fiber used in the formed adsorbent is preferably 0.40 cm. 3 / g or more, more preferably 0.50 or 0.55 cm 3 / g or more, more preferably 0.60 or 0.62 cm 3 / g or more. In one embodiment of the present invention, the upper limit of the micropore volume of the activated carbon fiber used in the formed adsorbent is preferably 1.00 cm. 3 / g or less, more preferably 0.90 cm 3 / g or less, more preferably 0.80 cm 3 / g or less. Setting the micropore volume of the activated carbon fiber within the above range is suitable for producing a molded adsorbent that is excellent in terms of adsorption / desorption performance, pressure loss, and the like.

[0088] <V: Pore volume of pores with diameters greater than 0.7 nm and less than 2.0 nm 0.7-2.0 (About activated carbon fiber) In one embodiment of the activated carbon fiber used in the molded adsorbent, the pore volume V of pores having a pore diameter of more than 0.7 nm and not more than 2.0 nm is 0.7-2.0 is preferably 0.20 to 1.20 cm 3 / g. More specifically, it is as follows. In one embodiment of the activated carbon fiber used in the molded adsorbent, the pore volume V of pores having a pore diameter of more than 0.7 nm and not more than 2.0 nm is 0.7-2.0 The lower limit is preferably 0.20 cm 3 / g or more, more preferably 0.30, 0.36, or 0.40 cm 3 / g or more, more preferably 0.43, 0.45, 0.47 or 0.49 cm 3 / g or more. In one embodiment of the activated carbon fiber used in the molded adsorbent, the pore volume V of pores having a pore diameter of more than 0.7 nm and not more than 2.0 nm is 0.7-2.0 The upper limit is preferably 1.20 cm 3 / g or less, more preferably 1.00 cm 3 / g or less, more preferably 0.90, 0.80, 0.75, 0.70, 0.65, or 0.60 cm 3 / g or less. The pore volume V of the activated carbon fiber 0.7-2.0 Setting V in the above range is suitable for obtaining a molded adsorbent having excellent adsorption / desorption performance, particularly for low-concentration evaporated fuel gas (e.g., n-butane). 0.7-2.0 Setting the value of the particle diameter within the above range is also suitable for obtaining a molded adsorbent having excellent pressure loss.

[0089] <Ratio of the volume of ultramicropores to the volume of micropores: R 0.7 / 2.0 (About activated carbon fiber) In one embodiment of the activated carbon fiber used in the formed adsorbent, the abundance ratio R of the ultramicropore volume to the micropore volume 0.7 / 2.0 is preferably 15.0 to 60.0%. More specifically, it is as follows. In one embodiment of the activated carbon fiber used in the formed adsorbent, the abundance ratio R of the ultramicropore volume to the micropore volume 0.7 / 2.0 The lower limit of the above range is preferably 15.0% or more, more preferably 18.0% or more, and even more preferably 19.0% or more. In one embodiment of the activated carbon fiber used in the molded adsorbent, the abundance ratio R of the ultramicropore volume to the micropore volume is 0.7 / 2.0 The upper limit of the ratio may be preferably 60.0% or less, more preferably 50.0% or less, and even more preferably 40.0, 30.0, or 25.0% or less. The ratio R of the ultramicropore volume of the activated carbon fiber 0.7 / 2.0Setting V in the above range is suitable for obtaining a molded adsorbent having excellent adsorption / desorption performance, particularly for low-concentration evaporated fuel gas (e.g., n-butane). 0.7-2.0 Setting the value of the particle diameter within the above range is also suitable for obtaining a molded adsorbent having excellent pressure loss.

[0090] In one embodiment of the present invention, the molded adsorbent may contain other components in addition to the activated carbon fiber, granular activated carbon, and binder. However, it is preferable that the addition of other components be limited to an extent that does not impair the effect of suppressing pressure loss or does not substantially eliminate its significance.

[0091] 5. Canister The molded adsorbent body of the present invention is suitable as an adsorbent material to be housed in an automobile canister, that is, the present invention can also provide an automobile canister as another embodiment.

[0092] In one embodiment of the present invention, the automobile canister is equipped with the above-mentioned molded adsorbent as an adsorbent material. There are no particular restrictions on the structure of the automobile canister, and a general structure can be used. For example, an automobile canister having the following structure can be mentioned.

[0093] The housing and an adsorbent chamber that accommodates an adsorbent within the housing; a first opening for providing gas flow communication between the adsorbent chamber and the engine; a second opening for providing gas transfer communication between the adsorbent chamber and the fuel tank; a third opening that opens when a predetermined pressure is applied from the adsorbent chamber or from the outside air, and that allows gas to move between the adsorbent chamber and the outside air; A canister comprising:

[0094] In one embodiment of the present invention, the canister may contain the molded adsorbent of the present invention as the adsorbent material. As described above, the molded adsorbent of the present invention can reduce pressure loss, and therefore, even when packed tightly, the pressure loss can be reduced more than when a conventional activated carbon fiber sheet is packed.

[0095] The first, second, and third openings are gas inlets and outlets. The locations of the openings, which are gas inlets and outlets, are not particularly limited; however, the third opening, which is an outside air inlet and outlet, is preferably positioned so that the gas passes through the adsorbent sufficiently when moving between the first and / or second openings. For example, an embodiment may be employed in which the first and second openings are provided in a first side surface of the housing, and the third opening is provided in a second side surface opposite the first side surface.

[0096] The adsorbent chamber may be divided into multiple chambers. For example, the adsorbent chamber may be divided into two or more compartments by a partition wall. A perforated plate or the like may be used as the partition wall. Alternatively, an external second housing may be provided separately from the first housing, and the first and second housings may be connected via a gas passage to provide an additional adsorbent chamber. When multiple compartments or housings are provided in this manner, in a preferred embodiment, the adsorbents or adsorbent chambers may be arranged in each compartment or housing so that the adsorption capacity decreases from the first or second opening, through which gas flows in from the engine or fuel tank, toward the third opening.

[0097] A specific example is a composite canister comprising a main canister (first housing) and a second canister (second housing) attached to the outside air intake side. When a plurality of compartments or housings are provided in this way, the compartment or housing into which evaporated gas first flows from the engine or fuel tank is designated as the main body (first compartment or first housing) with the largest storage volume, and conventional inexpensive activated carbon is stored in this main body, while the second compartment or second housing, which has a relatively smaller storage volume, is stored therein with the molded adsorbent of the present invention, which has excellent low-concentration adsorption and desorption performance, thereby making it possible to produce a high-performance canister while keeping costs down.

[0098] When there are multiple adsorbent chambers, the concentration of evaporated fuel gas flowing in from the previous chamber becomes lower in the adsorbent chamber located further back from the engine or fuel tank (i.e., the adsorbent chamber located closer to the outside air inlet / outlet). Therefore, activated carbon with a high n-butane adsorption capacity at a low concentration of about 0.2% is suitable as an adsorbent to be stored in the second compartment or second housing located further back from the engine or fuel tank, or in an adsorbent chamber further back. Furthermore, when activated carbon is used in an adsorbent chamber closer to the outside air inlet, the formed adsorbent of the present invention has a high effective adsorption / desorption capacity by purging, making it suitable as an adsorbent for use in an automobile canister, as it can reduce the amount of evaporated fuel gas leaking when the automobile is parked for a long period of time.

[0099] Therefore, one preferred embodiment of the canister can be exemplified as follows. The canister is a canister for an automobile, and includes a main chamber and an auxiliary chamber for accommodating an adsorbent, the sub-chamber has a smaller capacity for accommodating the adsorbent than the main chamber, and is located closer to an opening communicating with outside air, The adsorbent of the present invention is housed in the auxiliary chamber. Canister.

[0100] In the above embodiment, there may be one main chamber and one sub-chamber, or two or more of each. When there are three or more adsorbent chambers, the formed adsorbent body of the present invention may be housed in at least one of the sub-chambers, preferably in the sub-chamber closest to the opening communicating with the outside air.

[0101] 6. Manufacturing method of molded adsorbent The molded adsorbent of the present invention can be obtained by molding an adsorbent material containing granular activated carbon and activated carbon fibers into a predetermined shape. The granular activated carbon and activated carbon fibers can be, for example, those that satisfy the conditions (total pore volume, average pore diameter, specific surface area, etc.) indicated as the preferred indices above.

[0102] In one embodiment of the present invention, the molded adsorbent can be obtained by mixing activated carbon fiber, granular activated carbon, and a binder and molding the mixture. In another embodiment of the present invention, a laminate can be formed by bonding activated carbon fiber sheets, on the surface of which granular activated carbon is attached, using a binder.

[0103] Activated carbon fibers can be produced, for example, by carbonizing and activating fibers having a predetermined fiber diameter. Common methods can be used for carbonization and activation. In the following, an embodiment in which an activated carbon fiber sheet is produced using a precursor sheet (raw material sheet) will be illustrated.

[0104] 6-1. Preparation of raw material sheet (precursor fiber sheet) <Type of fiber> Examples of fibers constituting the raw material sheet include cellulose-based fibers, pitch-based fibers, PAN-based fibers, and phenolic resin-based fibers, with cellulose-based fibers being preferred.

[0105] <Cellulosic fiber> Cellulose-based fibers are fibers primarily composed of cellulose and / or its derivatives. The cellulose and cellulose derivatives may be of any origin, such as chemically synthesized products, plant-derived, regenerated cellulose, or bacterially produced cellulose. Preferred examples of cellulose-based fibers include fibers made from plant cellulose materials obtained from trees, and fibers made from long fibrous regenerated cellulose materials obtained by chemically treating and dissolving plant cellulose materials (cotton, pulp, etc.). These fibers may also contain components such as lignin and hemicellulose.

[0106] Examples of raw materials for cellulosic fibers (plant cellulose materials, regenerated cellulose materials) include plant cellulose fibers such as cotton (short staple cotton, medium staple cotton, long staple cotton, extra-long staple cotton, etc.), hemp, bamboo, paper mulberry, mitsumata, banana, and tunicates; regenerated cellulose fibers such as cuprammonium rayon, viscose rayon, polynosic rayon, and bamboo-derived cellulose; purified cellulose fibers spun in organic solvents (N-methylmorpholine N-oxide); and acetate fibers such as diacetate and triacetate. Among these, at least one selected from cuprammonium rayon, viscose rayon, and purified cellulose fibers is preferred due to their availability.

[0107] The diameter of the single fiber constituting the cellulose-based fiber is preferably 5 to 75 μm and the density is preferably 1.4 to 1.9 μm. 3 / g.

[0108] The form of the cellulose-based fiber is not particularly limited, and can be prepared into raw yarn (unprocessed yarn), false twisted yarn, dyed yarn, single yarn, doubled-twisted yarn, covered yarn, etc. depending on the purpose. Furthermore, when the cellulose-based fiber contains two or more raw materials, it may be a blended yarn, a blended twisted yarn, etc. Furthermore, the above-mentioned various raw materials may be used alone or in combination of two or more. Among these, non-twisted yarn is preferred in order to achieve both moldability and mechanical strength of the composite material.

[0109] <Fiber sheet> A fiber sheet is a thin, wide sheet made of many fibers, and includes woven fabrics, knitted fabrics, nonwoven fabrics, and the like.

[0110] There is no particular limitation on the method for weaving cellulosic fibers, and any common method can be used. There is also no particular limitation on the weave of the fabric, and any of the three basic weaves, plain weave, twill weave, and satin weave, can be used.

[0111] In a woven fabric formed from cellulosic fibers, the gap between the warp and weft yarns of the cellulosic fibers is preferably 0.1 to 0.8 mm, more preferably 0.2 to 0.6 mm, and even more preferably 0.25 to 0.5 mm. Furthermore, the basis weight of the woven fabric made of cellulosic fibers is preferably 50 to 500 g / m 2 , more preferably 100 to 400 g / m 2 It is possible.

[0112] By setting the cellulosic fibers and the woven fabric made of cellulosic fibers within the above range, the carbon fiber fabric obtained by heat treating the woven fabric can have excellent strength.

[0113] The method for producing the nonwoven fabric is not particularly limited, and examples include a method in which a fiber sheet is obtained using the above-mentioned fibers cut to an appropriate length as a raw material by a dry method or a wet method, or a method in which a fiber sheet is obtained directly from a solution by an electrospinning method, etc. Furthermore, after the nonwoven fabric is obtained, treatment such as resin bonding, thermal bonding, spunlace, needle punching, etc. may be added in order to bond the fibers together.

[0114] 6-2. Catalyst In the first manufacturing method, a catalyst is supported on the raw material sheet prepared as described above. The catalyst is supported on the raw material sheet, and the sheet is subjected to a carbonization treatment. The sheet is then activated using water vapor, carbon dioxide, air, or the like, to obtain a porous activated carbon fiber sheet. Examples of the catalyst that can be used include phosphoric acid catalysts and organic sulfonic acid catalysts.

[0115] <Phosphoric acid catalyst> Examples of phosphoric acid catalysts include phosphorus oxyacids such as phosphoric acid, metaphosphoric acid, pyrophosphoric acid, phosphorous acid, phosphonic acid, phosphonous acid, and phosphinic acid; ammonium dihydrogen phosphate, diammonium hydrogen phosphate, triammonium phosphate; dimethylphosphonopropanamide; ammonium polyphosphate; polyphosphonitrile chloride; and condensates of phosphoric acid, tetrakis(hydroxymethyl)phosphonium salts, or tris(1-aziridinyl)phosphine oxide with urea, thiourea, melamine, guanine, cyanamide, hydrazine, dicyandiamide, or methylol derivatives thereof, with diammonium hydrogen phosphate being preferred. Phosphoric acid catalysts may be used alone or in combination. When the phosphoric acid catalyst is used as an aqueous solution, its concentration is preferably 0.05 to 2.0 mol / L, more preferably 0.1 to 1.0 mol / L.

[0116] <Organic sulfonic acid catalyst> As the organic sulfonic acid, an organic compound having one or more sulfo groups can be used, and for example, compounds having sulfo groups bonded to various carbon skeletons such as aliphatic and aromatic compounds can be used. From the viewpoint of handling, organic sulfonic acid catalysts with low molecular weights are preferred.

[0117] Examples of organic sulfonic acid catalysts include compounds represented by the formula R-SOH (wherein R represents a linear or branched alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 20 carbon atoms, or an aryl group having 6 to 20 carbon atoms, and the alkyl group, cycloalkyl group, and aryl group may each be substituted with an alkyl group, a hydroxyl group, or a halogen group). Examples of organic sulfonic acid catalysts include methanesulfonic acid, ethanesulfonic acid, propanesulfonic acid, 1-hexanesulfonic acid, vinylsulfonic acid, cyclohexanesulfonic acid, p-toluenesulfonic acid, p-phenolsulfonic acid, naphthalenesulfonic acid, benzenesulfonic acid, and camphorsulfonic acid. Of these, methanesulfonic acid is preferred. One type of organic sulfonic acid catalyst may be used alone, or two or more types may be used in combination.

[0118] When the organic sulfonic acid is used as an aqueous solution, the concentration thereof may be preferably 0.05 to 2.0 mol / L, more preferably 0.1 to 1.0 mol / L.

[0119] <Mixed catalyst> The phosphoric acid catalyst and the organic sulfonic acid catalyst may be mixed and used as a mixed catalyst. The mixing ratio may be adjusted appropriately.

[0120] <Catalyst retention> The catalyst is retained on the raw material sheet. Here, "retained" means that the catalyst is kept in contact with the raw material sheet, and can take various forms such as adhesion, adsorption, or impregnation. There are no particular limitations on the method for retaining the catalyst, but examples include a method of immersing the raw material sheet in an aqueous solution containing the catalyst, a method of sprinkling the aqueous solution containing the catalyst onto the raw material sheet, a method of contacting the raw material sheet with vaporized catalyst vapor, and a method of mixing the fibers of the raw material sheet with an aqueous solution containing the catalyst and then making paper.

[0121] From the viewpoint of sufficient carbonization, a preferred method is to immerse the raw material sheet in an aqueous solution containing the catalyst and impregnate the catalyst deep into the fibers. The temperature during immersion in the aqueous solution containing the catalyst is not particularly limited, but room temperature is preferred. The immersion time is preferably 10 seconds to 120 minutes, more preferably 20 seconds to 30 minutes. By immersion, the fibers constituting the raw material sheet are adsorbed with, for example, 1 to 150 mass %, preferably 5 to 60 mass % of the catalyst. After immersion, the raw material sheet is preferably removed and dried. The drying method may be, for example, leaving it at room temperature or introducing it into a dryer. Drying may be carried out after removal from the aqueous solution containing the catalyst until excess water evaporates and the sample weight remains constant. For example, in the case of room temperature drying, the drying time may be 0.5 days or more. After drying to almost completely eliminate the change in mass, the raw material sheet retaining the catalyst proceeds to the carbonization process.

[0122] 6-3. Carbonization After preparing the raw material sheet supporting the catalyst, the sheet is carbonized. The carbonization treatment to obtain the activated carbon fiber sheet can be carried out according to a general method for carbonizing activated carbon, but in a preferred embodiment, the treatment can be carried out as follows.

[0123] The carbonization treatment is usually carried out in an inert gas atmosphere. In the present invention, the inert gas atmosphere means an oxygen-free or low-oxygen atmosphere in which carbon is less likely to undergo a combustion reaction and is carbonized, and is preferably, for example, an argon, nitrogen, or other gas atmosphere.

[0124] The raw material sheet carrying the catalyst is subjected to a heat treatment in the above-mentioned predetermined gas atmosphere to be carbonized.

[0125] In one embodiment of the present invention, the heating temperature in the carbonization treatment may preferably be 300 to 1400° C. More specifically, it is as follows. The lower limit of the heating temperature is preferably 300°C or higher, more preferably 350°C or higher, and even more preferably 400°C or higher or 750°C or higher. The upper limit of the heating temperature is preferably 1400°C or lower, more preferably 1300°C or lower, and even more preferably 1200°C or lower or 1000°C or lower. By setting the heating temperature in this manner, a carbon fiber sheet in which the fiber morphology is maintained can be obtained. If the heating temperature is below the above lower limit, the carbon content of the carbon fiber will be 80% or less, and carbonization will likely be insufficient.

[0126] In one embodiment of the present invention, the heat treatment time in the carbonization treatment, including the time required for temperature rise, is preferably 10 to 180 minutes. More specifically, it is as follows. The lower limit of the heat treatment time, including the time required for temperature increase, is preferably 10 minutes or more, more preferably 11 minutes or more, even more preferably 12, 15, 20, or 25 minutes or more, and more preferably 30 minutes or more. The upper limit of the heat treatment time can be set arbitrarily, but is preferably 180 minutes or less, more preferably 160 minutes or less, and even more preferably 140 minutes or less. By thoroughly impregnating the raw material sheet with the catalyst, setting the heating temperature to the above-mentioned preferred temperature, and adjusting the heat treatment time, it is possible to adjust the degree of pore formation and to adjust the physical properties of the porous body, such as the specific surface area, the volume of various pores, and the average pore diameter. If the heat treatment time is shorter than the above lower limit, carbonization tends to be insufficient.

[0127] Furthermore, the heat treatment may be a reheat treatment in a predetermined gas atmosphere after the above-described heat treatment (sometimes referred to as a primary heat treatment). That is, the carbonization treatment may be carried out in multiple stages of heat treatments with different conditions, such as temperature. By carrying out the primary heat treatment and the reheat treatment under predetermined conditions, it may be possible to adjust the physical properties, promote carbonization and subsequent activation more smoothly, and obtain an activated carbon fiber sheet with excellent adsorption / desorption properties.

[0128] 6-4. Activation treatment In one embodiment of the present invention, the activation treatment can be carried out, for example, by supplying water vapor or carbon dioxide continuously after the heat treatment and maintaining the material at an appropriate activation temperature for a predetermined period of time, thereby obtaining an activated carbon fiber sheet.

[0129] In one embodiment of the present invention, the heating temperature in the activation treatment can be preferably 300 to 1400° C. More specifically, it is as follows. The lower limit of the activation temperature is preferably 300°C or higher, more preferably 350°C or higher, and even more preferably 400, 500, 600, 700, or 750°C or higher. On the other hand, the upper limit of the activation temperature can be preferably 1400°C or lower, more preferably 1300°C or lower, and even more preferably 1200 or 1000°C or lower. When the activation treatment is carried out immediately after the heat treatment, it is desirable to adjust the temperature to approximately the same as the heat treatment temperature.

[0130] The lower limit of the activation time is preferably 1 minute or more, more preferably 5 minutes or more. The upper limit of the activation time can be any value, but is preferably 180 minutes or less, more preferably 160 minutes or less, and even more preferably 140 minutes or less, 100 minutes or less, 50 minutes or less, or 30 minutes or less.

[0131] 6-5. Obtaining granular activated carbon A wide variety of granular activated carbons are commercially available, and the desired granular activated carbon can be obtained. Alternatively, granular activated carbon may be prepared by purchasing commercially available activated carbon and further subjecting it to processing such as pulverization or sieving. Alternatively, granular activated carbon may be prepared from plant-based raw materials using known methods.

[0132] 6-6. Preparation of compacts The method for processing a molded body containing activated carbon fiber, granular activated carbon, and a binder is not particularly limited, but for example, a mixture of the two can be prepared and molded. In one embodiment, the molded body can be produced, for example, as follows.

[0133] <Preparation of Slurry Containing Activated Carbon Fiber, Granular Activated Carbon, and Binder> The activated carbon fiber sheet and binder prepared in advance are mixed with water, and then defibrated and dispersed using a stirring means such as a mixer to mix the two, thereby obtaining a slurry containing both (first slurry). The activated carbon fiber sheet to be charged into the mixer may be cut into small pieces of an appropriate size depending on the scale of the mixer, etc.

[0134] Granular activated carbon is further added to the first slurry, and the granular activated carbon is mixed using a stirring means such as a spatula to obtain a slurry (second slurry) containing activated carbon fiber, granular activated carbon, and a binder. When dispersing the granular activated carbon, it is preferable to stir gently with a spatula or the like so as not to crush the granular activated carbon.

[0135] <Formation of molded body> The second slurry containing activated carbon fiber, granular activated carbon, and binder obtained as described above can be poured into a mold of a desired shape, pressed to remove water, and then dried to obtain a molded adsorbent.

[0136] <Preparation of laminated adsorbent> In yet another embodiment of the present invention, a molded adsorbent having granular activated carbon sandwiched between activated carbon fiber sheets can be produced, for example, as follows: First, an activated carbon fiber sheet is prepared. Granular activated carbon is attached to the main surface where the activated carbon fiber sheets are bonded together. For example, a mixed slurry containing granular activated carbon and a binder may be prepared, and the mixed slurry may be applied to the activated carbon fiber sheet. Alternatively, a simple slurry of granular activated carbon may be first applied to the activated carbon fiber sheet, and then a simple slurry of the binder may be applied. [Example]

[0137] The present invention will be explained in more detail below by way of examples, but the technical scope (or technical reach) of the invention presented in this disclosure is not limited to the following examples.

[0138] Various items relating to the physical properties and performance of activated carbon fiber, granular activated carbon, and molded adsorbent were measured and evaluated by the methods shown below. Note that various numerical values ​​defining the present invention can be determined by the following measurement and evaluation methods.

[0139] As a reference standard for the N2 adsorption BET analysis method for specific surface area, total pore volume, and average pore diameter, we referred to the basic physical properties related to adsorption performance in JIS K 1477. For the ultramicropore volume and micropore volume, we also referred to the simulation analysis method using N2 adsorption GCMC (GCMC: Grand Canonical Monte Carlo method) as a reference standard.

[0140] <Specific surface area> Approximately 30 mg of a measurement sample (activated carbon fiber sheet, granular activated carbon, or molded adsorbent, hereinafter the same) was collected, vacuum dried at 200°C for 20 hours, weighed, and measured using a high-precision gas / vapor adsorption measuring device, BELSORP-max II (Microtrac-Bell). The adsorption amount of nitrogen gas at the boiling point of liquid nitrogen (77 K) was measured at a relative pressure of 10 -8 Measurements were made in the range of order 0.990, and the adsorption isotherm of the sample was created. This adsorption isotherm was analyzed by the BET method, in which the analytical relative pressure range was automatically determined under the conditions of adsorption isotherm type I (ISO 9277), and the BET specific surface area per weight (unit: m 2 / g, and use this to calculate the specific surface area (unit: m 2 / g).

[0141] <Total pore volume> The total pore volume (unit: cm) obtained by the one-point method from the result of the isothermal adsorption curve obtained in the above specific surface area section at a relative pressure of 0.960 was calculated. 3 / g) was calculated.

[0142] <Average pore size (average pore diameter) unit: nm> It was calculated using the following formula 3. Average pore diameter = 4 × total pore volume × 103 ÷Specific surface area (Formula 3)

[0143] <Ultramicropore volume> The isothermal adsorption curve obtained in the above specific surface area section was analyzed by the GCMC method using the analysis software BELMaster attached to the high-precision gas / vapor adsorption analyzer BELSORP-max II (Microtrac BEL) with the following analysis settings: "Smoothing (moving average processing using one point before and after every point of the pore distribution analysis)", "Distribution function: No-assumption", "Pore size definition: Solid and Fluid Def. Pore Size", and "Kernel: Slit-C-Adsorption". From the pore distribution curve obtained during adsorption, the cumulative pore volume of 0.7 nm was read and used to calculate the ultramicropore volume (unit: cm). 3 / g).

[0144] <Micropore volume> The isothermal adsorption curve obtained in the above specific surface area section was analyzed by the GCMC method using the analysis software BELMaster attached to the high-precision gas / vapor adsorption analyzer BELSORP-max II (Microtrac BEL) with the following analysis settings: "Smoothing (moving average processing using one point before and after every point of the pore distribution analysis)", "Distribution function: No-assumption", "Pore size definition: Solid and Fluid Def. Pore Size", and "Kernel: Slit-C-Adsorption". From the pore distribution curve obtained during adsorption, the cumulative pore volume of 2.0 nm was read and used to calculate the micropore volume (unit: cm). 3 / g).

[0145] <Sheet basis weight> The measurement sample (activated carbon fiber sheet, etc.) is left to stand for 12 hours or more in an environment of 23±2°C temperature and 50±5% relative humidity, and the sheet basis weight (unit: g / m) is calculated from the weight and length and width dimensions. 2 ) was sought.

[0146] <Sheet thickness> The measurement sample (such as an activated carbon fiber sheet) was left standing for 12 hours or more in an environment with a temperature of 23 ± 2°C and a relative humidity of 50 ± 5%. Using a digital small thickness gauge FS-60DS (manufactured by Daiei Kagaku Seiki Co., Ltd.), the sheet thickness (unit: mm) when a load of 0.3 kPa was applied was measured.

[0147] <Sheet conditioned density: unit: g / cm 3 > It was calculated by the following formula (4). Sheet density = sheet basis weight ÷ sheet thickness ÷ 10 3 ···(Formula 4)

[0148] <Sheet moisture content> The measurement sample (such as an activated carbon fiber sheet) was left standing for 12 hours or more in an environment with a temperature of 23 ± 2°C and a relative humidity of 50 ± 5%. After that, 0.5 - 1.0 g of the sample was taken, and the moisture content (unit: %) was determined from the weight change when it was dried in a dryer at 115 ± 5°C for 3 hours or more.

[0149] <Dimensions of the formed adsorbent> The dimensions of the formed adsorbent were measured and obtained using a vernier caliper, a ruler, etc. The dry weight of the formed adsorbent was measured with an electronic balance.

[0150] <Dry density of the formed adsorbent: unit: g / cm 3 > It was calculated by the following formula (5). Density = dry weight of the formed adsorbent ÷ volume of the formed adsorbent ···(Formula 5) The volume of the formed adsorbent was calculated from the measurement results of the dimensions of the formed adsorbent.

[0151] <n - Butane adsorption and desorption performance> Tests were conducted with n-butane gas concentrations of 0.2% and 100%, with reference to the American Society for Testing and Materials Standard Test Method for Determination of Butane Working Capacity of Activated Carbon (ASTM D5228-16). The flow rates of n-butane gas and desorbing air were adjusted appropriately while referring to ASTM D5228-16, and the tests were conducted.

[0152] (1) Adsorption and desorption performance of 0.2% n-butane gas The molded adsorbent was dried in a dryer at 115±5°C for at least 3 hours, and then cooled and the dry weight was measured.The mass of an empty adsorption vessel (a stainless steel frame vessel with the same shape as the molded adsorbent, through which gas can flow, and equipped with an on-off valve at the inlet and outlet of the adsorption vessel) was measured, and the molded adsorbent was then filled into the adsorption vessel.

[0153] The adsorption vessel was then placed in a flow system, and n-butane gas diluted with air to a concentration of 0.2% was passed through the test tube at a test temperature of 25°C at a rate of 1.0 L / min to adsorb n-butane. The adsorption vessel's on-off valve was closed, the adsorption vessel was removed from the flow system, and its mass was measured. This flow of 0.2% n-butane gas was repeated until a constant mass was reached, i.e., until the adsorption amount was saturated. The adsorption vessel was reinstalled in the flow device, and n-butane was desorbed by flowing air through the test tube at 20.0 L / min for 12 minutes at a test temperature of 25°C. The on-off valve of the adsorption vessel was closed, the adsorption vessel was removed from the flow device, and its mass was measured.

[0154] This adsorption and desorption procedure was repeated twice, and the first adsorption amount, effective adsorption / desorption amount, effective adsorption / desorption amount rate, and effective adsorption / desorption rate were calculated using the following equations 6, 7, 8, and 9.

[0155] <Formula 6> 1st adsorption amount = 1st 0.2% n-butane adsorption amount The units of each value are as follows: First 0.2% n-butane adsorption amount (unit: g)

[0156] <Formula 7> Effective adsorption / desorption amount = (2nd 0.2% n-butane adsorption amount + 2nd 0.2% n-butane desorption amount) ÷ 2 The units of each value are as follows: Effective adsorption / desorption amount (unit: g) Second time 0.2% n-butane adsorption amount (unit: g) Second 0.2% n-butane desorption amount (unit: g)

[0157] <Formula 8> Effective adsorption / desorption rate = effective adsorption / desorption amount ÷ dry weight of molded adsorbent × 100 The units of each value are as follows: Effective adsorption / desorption rate (unit: wt%) Effective adsorption / desorption amount (unit: g) Dry weight of the formed adsorbent (unit: g)

[0158] <Formula 9> Effective adsorption / desorption rate = effective adsorption / desorption amount ÷ first adsorption amount × 100 The units of each value are as follows: Effective adsorption / desorption rate (unit: %) Effective adsorption / desorption amount (unit: g) First adsorption amount (unit: g)

[0159] <Measurement of 0 ppm maintenance time> The change in n-butane concentration at the outlet of the adsorption vessel when this 0.2% n-butane was passed through was measured every 6 seconds using a portable gas detector Cosmotector (model number: XP-3160, manufacturer: New Cosmos Electric Co., Ltd.). After repeating the first adsorption and desorption, the concentration change in the second adsorption was defined as 0 ppm if it was below the lower limit of quantification (25 ppm), and the time during which 0 ppm was maintained continuously from the beginning was defined as the 0 ppm maintenance time (minutes).

[0160] (2) Adsorption and desorption performance of 100% n-butane gas Instead of 0.2 n-butane gas, 100% n-butane gas was flowed at 0.5 L / min, and instead of 20.0 L / min of air for 12 min, 2.0 L / min of air was flowed at 719 × the volume of the formed adsorbent (unit: cm 3 The adsorption and desorption performance was measured in the same manner as in the above "(1) Adsorption and desorption performance of 0.2% n-butane gas" except that the gas was allowed to flow for 100 minutes.

[0161] This adsorption and desorption operation was carried out only once, and the adsorption amount, effective adsorption / desorption amount, effective adsorption / desorption amount rate, effective adsorption / desorption rate, and BWC were calculated using the following equations 10, 11, 12, 13, and 14.

[0162] <Formula 10> Adsorption amount = 100% n-butane adsorption amount The units of each value are as follows: 100% n-butane adsorption amount (unit: g)

[0163] <Formula 11> Effective adsorption / desorption amount = 100% n-butane desorption amount The units of each value are as follows: Effective adsorption / desorption amount (unit: g) 100% n-butane desorption amount (unit: g)

[0164] <Formula 12> Effective adsorption / desorption rate = effective adsorption / desorption amount ÷ dry weight of molded adsorbent × 100 The units of each value are as follows: Effective adsorption / desorption rate (unit: wt%) Effective adsorption / desorption amount (unit: g) Dry weight of the formed adsorbent (unit: g)

[0165] <Formula 13> Effective adsorption / desorption rate = effective adsorption / desorption amount ÷ adsorption amount × 100 The units of each value are as follows: Effective adsorption / desorption rate (unit: %) Effective adsorption / desorption amount (unit: g) Adsorption amount (unit: g)

[0166] <Formula 14> BWC (Butane Working Capacity) = Effective adsorption / desorption amount ÷ volume of formed adsorbent × 100 The units of each value are as follows: BWC (unit: g / dL) Effective adsorption / desorption amount (unit: g) Molded adsorbent volume (unit: cm 3 )

[0167] <Pressure loss measurement> Each molded adsorbent body of the Examples, Reference Examples, and Comparative Examples was prepared. As a container for housing the molded adsorbent body, a cylindrical container was prepared, with one end face and the other opposite end face each being open, and a frame (frame container) that allowed ventilation in the direction perpendicular to the end faces. The diameter (inner diameter) of each end face of the frame container was 7.7 cm (i.e., the area of ​​the open face: 46.56 cm). 2 The prepared molded adsorbent was packed inside a framed container so that no gaps were left, to prepare a test sample for measuring pressure loss.

[0168] The pressure loss was measured as follows: 60 L / min of air was passed through the test sample prepared as described above, and the differential pressure between the inlet and outlet of the test sample was measured using a testo 510 differential pressure meter (Testo Corporation), and the result was taken as the pressure loss (kPa).

[0169] <Measurement of the average particle size of granular activated carbon> The median diameter D50 of the particle size distribution measured using a laser diffraction particle size analyzer Mastersizer 3000 (Malvern) was taken as the average particle diameter.

[0170] <(ACF1) Preparation of activated carbon fiber> Carded with a basis weight of 400 g / m 2A web of rayon fiber (56 dtex, fiber length 102 mm) was impregnated with a 6-10% aqueous solution of diammonium hydrogen phosphate, squeezed, and then dried to give an 8-10% by weight coating. The resulting pretreated nonwoven fabric was heated to 900°C in a nitrogen atmosphere over 45 minutes and held at this temperature for 3 minutes. Subsequently, it was activated at that temperature for 19 minutes in a nitrogen stream containing water vapor with a dew point of 71°C, yielding activated carbon fiber.

[0171] <(ACF2) Preparation of activated carbon fiber sheet> Rayon fiber (17 dtex, fiber length 76 mm) basis weight 400 g / m 2 The needle-punched nonwoven fabric was impregnated with a 6-10% aqueous solution of diammonium hydrogen phosphate, squeezed, and then dried to deposit 8-10% by weight. The resulting pretreated nonwoven fabric was heated to 900°C in a nitrogen atmosphere over 40 minutes and held at this temperature for 3 minutes. Subsequently, activation treatment was carried out at that temperature for 17 minutes in a nitrogen stream containing water vapor with a dew point of 71°C, yielding an activated carbon fiber sheet.

[0172] <(ACF3) Preparation of activated carbon fiber sheet> Rayon fiber (1.7 dtex, fiber length 40 mm) basis weight 400 g / m 2 The needle-punched nonwoven fabric was impregnated with a 6-10% aqueous solution of diammonium hydrogen phosphate, squeezed, and then dried to deposit 8-10% by weight. The resulting pretreated nonwoven fabric was heated to 900°C in a nitrogen atmosphere over 40 minutes and held at this temperature for 3 minutes. Subsequently, activation treatment was carried out at that temperature for 19 minutes in a nitrogen stream containing water vapor with a dew point of 71°C, yielding an activated carbon fiber sheet.

[0173] <Granular activated carbon 1> Molded activated carbon KMAZ3 (manufactured by Shichisei Co., Ltd.) was pulverized, and the activated carbon of a size that could pass through a 500 μm mesh sieve conforming to ISO3301-1 / JIS Z-8801 standards but not through a 250 μm mesh sieve conforming to the same standards was designated as granular activated carbon 1. The average particle size was 381 μm.

[0174] <Granular activated carbon 2> Granular activated carbon CW480SZ (manufactured by Futamura Chemical Co., Ltd.) was used as granular activated carbon 2. The average particle size was 352 μm.

[0175] <Reference Example 1 (activated carbon fiber: granular activated carbon = 100:0)> Five parts by weight of acrylic fiber 50TWF (manufactured by Nippon Exlan Kogyo Co., Ltd.) was added to a mixer along with 0.5 L of water for 30 seconds to defibrate and disperse the fibrous binder. Next, 100 parts by weight of the activated carbon fiber sheet (ACF1) obtained above and 0.5 L of water were added, and the mixture was defibrated and dispersed for another 10 seconds to obtain a slurry (first slurry) containing dispersed defibrated activated carbon fiber. A metal cylinder with an inner diameter of 79 mm and a height of 400 mm, which could be divided at a position 24 mm from the bottom, was placed on a funnel equipped with a perforated plate for suction dehydration. The first slurry was poured into the metal cylinder and then suction dehydrated from the bottom to form a molded product. The bottom 24 mm section containing the wet compact was separated from the metal cylinder, and the top and bottom cross sections of the metal cylinder were sandwiched between punching plates, a 1 kg weight was placed on top, and the wet compact was crushed to a height of 24 mm if the height was greater than 24 mm. The cylinder was then dried at 120 °C for at least 4 hours. The metal cylinder was removed, and a disk-shaped adsorbent with an outer diameter of 77 mm and a height of 24 mm was obtained. The obtained molded adsorbent was more resistant to deformation than activated carbon fiber.

[0176] <Reference Example 2 (activated carbon fiber: granular activated carbon = 100:0)> A molded adsorbent having an outer diameter of 77 mm and a height of 24 mm was obtained in the same manner as in Reference Example 1, except that 100 parts by weight of an activated carbon fiber sheet (ACF2) was used instead of the activated carbon fiber (ACF1) used in Reference Example 1. The obtained molded adsorbent was less likely to lose its shape than the activated carbon fiber sheet.

[0177] <Reference Example 3 (activated carbon fiber: granular activated carbon = 100:0)> A molded adsorbent having an outer diameter of 77 mm and a height of 24 mm was obtained in the same manner as in Reference Example 1, except that 100 parts by weight of an activated carbon fiber sheet (ACF3) was used instead of the activated carbon fiber (ACF1) used in Reference Example 1. The obtained molded adsorbent was less likely to lose its shape than the activated carbon fiber sheet.

[0178] Example 1 (activated carbon fiber: granular activated carbon = 90:10) Five parts by weight of the fibrous binder used in Reference Example 1 was placed in a mixer together with 0.5 L of water and defibrated and dispersed for 30 seconds, and 90 parts by weight of the activated carbon fiber (ACF1) used in Reference Example 1 and 0.5 L of water were added, followed by further defibrating and dispersing for 10 seconds to obtain a first slurry.

[0179] Next, 10 parts by weight of granular activated carbon 1 was added to the first slurry and stirred with a spatula to obtain a second slurry in which activated carbon fiber and granular activated carbon were dispersed. The second slurry was suction dehydrated and dried in the same manner as in Reference Example 1 to obtain a disk-shaped molded adsorbent with an outer diameter of 77 mm and a height of 24 mm. The obtained molded adsorbent was less likely to lose its shape than activated carbon fiber.

[0180] Example 2 (activated carbon fiber: granular activated carbon = 60:40) A molded adsorbent having an outer diameter of 77 mm and a height of 24 mm was obtained in the same manner as in Example 1, except that the amount of the fibrous binder used in Example 1 was 5 parts by weight, the amount of the activated carbon fiber (ACF1) used in Example 1 was 60 parts by weight, and the amount of the granular activated carbon 1 used in Example 1 was 40 parts by weight. The obtained molded adsorbent was less likely to lose its shape than activated carbon fiber.

[0181] Example 3 (activated carbon fiber:granular activated carbon = 30:70) A molded adsorbent having an outer diameter of 77 mm and a height of 24 mm was obtained in the same manner as in Example 1, except that the amount of the fibrous binder used in Example 1 was 5 parts by weight, the amount of the activated carbon fiber sheet (ACF1) used in Example 1 was 30 parts by weight, and the amount of the granular activated carbon 1 used in Example 1 was 70 parts by weight. The obtained molded adsorbent was less likely to lose its shape than activated carbon fiber.

[0182] Example 4 (activated carbon fiber:granular activated carbon = 20:80) A molded adsorbent having an outer diameter of 77 mm and a height of 19 mm was obtained in the same manner as in Example 1, except that the amount of the fibrous binder used in Example 1 was 5 parts by weight, the amount of the activated carbon fiber sheet (ACF1) used in Example 1 was 20 parts by weight, and the amount of the granular activated carbon 1 used in Example 1 was 80 parts by weight. The obtained molded adsorbent was less likely to lose its shape than activated carbon fiber.

[0183] Example 5 (activated carbon fiber:granular activated carbon = 10:90) A molded adsorbent having an outer diameter of 77 mm and a height of 16 mm was obtained in the same manner as in Example 1, except that the amount of fibrous binder used in Example 1 was 5 parts by weight, the amount of activated carbon fiber sheet (ACF1) used in Example 1 was 10 parts by weight, and the amount of granular activated carbon 1 used in Example 1 was 90 parts by weight. The obtained molded adsorbent was less likely to lose its shape than activated carbon fiber.

[0184] Example 6 (activated carbon fiber:granular activated carbon = 60:40) A molded adsorbent having an outer diameter of 77 mm and a height of 24 mm was obtained in the same manner as in Example 1, except that the amount of the fibrous binder used in Example 1 was 5 parts by weight, the amount of the activated carbon fiber sheet (ACF2) used in Reference Example 2 was 60 parts by weight, and the amount of the granular activated carbon 1 used in Example 1 was 40 parts by weight. The obtained molded adsorbent was less likely to lose its shape than the activated carbon fiber sheet.

[0185] Example 7 (activated carbon fiber:granular activated carbon = 20:80) A molded adsorbent having an outer diameter of 77 mm and a height of 24 mm was obtained in the same manner as in Example 1, except that the amount of the fibrous binder used in Example 1 was 5 parts by weight, the amount of the activated carbon fiber sheet (ACF2) used in Example 6 was 20 parts by weight, and the amount of the granular activated carbon 1 used in Example 1 was 80 parts by weight. The obtained molded adsorbent was less likely to lose its shape than the activated carbon fiber sheet.

[0186] Example 8 (activated carbon fiber: granular activated carbon = 50:50) A molded adsorbent having an outer diameter of 77 mm and a height of 24 mm was obtained in the same manner as in Example 1, except that the amount of the fibrous binder used in Example 1 was 5 parts by weight, the amount of the activated carbon fiber sheet (ACF3) used in Reference Example 3 was 50 parts by weight, and the amount of the granular activated carbon 1 used in Example 1 was 50 parts by weight. The obtained molded adsorbent was less likely to lose its shape than the activated carbon fiber sheet.

[0187] Example 9 (activated carbon fiber:granular activated carbon = 20:80) A molded adsorbent having an outer diameter of 77 mm and a height of 24 mm was obtained in the same manner as in Example 8, except that the amount of the fibrous binder used in Example 1 was 5 parts by weight, the amount of the activated carbon fiber sheet (ACF3) used in Example 8 was 20 parts by weight, and the amount of the granular activated carbon 1 used in Example 1 was 80 parts by weight. The obtained molded adsorbent was less likely to lose its shape than the activated carbon fiber sheet.

[0188] Comparative Example 1 (activated carbon fiber: granular activated carbon = 90:10) A molded adsorbent having an outer diameter of 77 mm and a height of 24 mm was obtained in the same manner as in Example 1, except that the amount of fibrous binder used in Example 1 was 5 parts by weight, the amount of activated carbon fiber sheet (ACF3) used in Reference Example 3 was 90 parts by weight, and the amount of granular activated carbon 2 was 10 parts by weight. The obtained molded adsorbent was less likely to lose its shape than the activated carbon fiber sheet.

[0189] <Comparative Example 2 (activated carbon fiber: granular activated carbon = 50:50)> A molded adsorbent having an outer diameter of 77 mm and a height of 24 mm was obtained in the same manner as in Example 1, except that the amount of the fibrous binder used in Example 1 was 5 parts by weight, the amount of the activated carbon fiber sheet (ACF3) used in Comparative Example 1 was 50 parts by weight, and the amount of the granular activated carbon 2 used in Comparative Example 1 was 50 parts by weight. The obtained molded adsorbent was less likely to lose its shape than the activated carbon fiber sheet.

[0190] Comparative Example 3 (activated carbon fiber:granular activated carbon = 20:80) A molded adsorbent having an outer diameter of 77 mm and a height of 24 mm was obtained in the same manner as in Example 1, except that the amount of the fibrous binder used in Example 1 was 5 parts by weight, the amount of the activated carbon fiber sheet (ACF3) used in Comparative Example 1 was 20 parts by weight, and the amount of the granular activated carbon 2 used in Comparative Example 1 was 80 parts by weight. The obtained molded adsorbent was less likely to lose its shape than the activated carbon fiber sheet.

[0191] Comparative Example 4 (activated carbon fiber: granular activated carbon = 0:100) Five parts by weight of the fibrous binder used in Example 1 was placed in a mixer together with 0.5 L of water and defibrated and dispersed for 30 seconds, and then 100 parts by weight of the granular activated carbon 1 used in Example 1 and 0.5 L of water were added and stirred with a spatula to obtain a granular activated carbon adsorption slurry. This adsorption slurry was suction dehydrated and dried in the same manner as in Example 1 to obtain a disk-shaped molded adsorbent with an outer diameter of 77 mm and a height of 12 mm.

[0192] Comparative Example 5 (activated carbon fiber: granular activated carbon = 0:100) A disk-shaped molded adsorbent having an outer diameter of 77 mm and a height of 22 mm was obtained in the same manner as in Comparative Example 4, except that the granular activated carbon used in Comparative Example 4 was changed to 100 parts by weight of granular activated carbon 2.

[0193] The above physical properties were measured according to the above measurement methods for each of the adsorption materials used in Examples 1 to 9, Reference Examples 1 to 3, and Comparative Examples 1 to 3. The results are shown in Table 1. Tables 2-1, 2-2, 2-3, 2-4, 3-1, 3-2, 3-3, and 3-4 show the properties of the molded adsorbents of Examples 1 to 9, Reference Examples 1 to 3, and Comparative Examples 1 to 3, respectively. In the tables, the term "ACF" is an abbreviation for activated carbon fiber. In the tables, the term "AC" is an abbreviation for activated carbon.

[0194] [Table 1]

[0195] [Table 2-1]

[0196] [Table 2-2]

[0197] [Table 2-3]

[0198] [Table 2-4]

[0199] [Table 3-1]

[0200] [Table 3-2]

[0201] [Table 3-3]

[0202] [Table 3-4]

[0203] <Notes in Tables 3-1, 3-2, 3-3, and 3-4> 1) (100% effective n-butane adsorption / desorption amount / dry weight of molded adsorbent) x 100 (wt%) 2) (100% effective n-butane adsorption / desorption amount / 100% adsorption amount of n-butane) x 100 (%) 3) (100% effective n-butane adsorption / desorption amount / volume of formed adsorbent) x 100 (g / dL) 4) Average of the second adsorption amount of 0.2% n-butane and the second desorption amount of 0.2% n-butane 5) (0.2% n-butane effective adsorption / desorption amount / dry weight of molded adsorbent) x 100 (wt%) 6) (effective adsorption / desorption amount / 0.2% n-butane first adsorption amount) x 100 (%) 7) 0 ppm maintenance time after second adsorption of 0.2% n-butane

[0204] As shown in Tables 3-1, 3-2, 3-3, and 3-4, it was revealed that the molded adsorbents of Examples 1 to 9 were excellent in both 100% n-butane adsorption / desorption performance and 0.2% n-butane adsorption / desorption performance. [Explanation of symbols]

[0205] 1 laminated adsorbent, 10 sheet-shaped molded adsorbent, 10a main surface of sheet-shaped molded adsorbent, 10b side end surface of sheet-shaped molded adsorbent, 10c side end surface of sheet-shaped molded adsorbent, F gas flow direction, 2 disk-shaped molded adsorbent, 3 cylindrical molded adsorbent

Claims

1. A molded adsorbent for a canister, comprising: The molded adsorbent is a molded body including activated carbon fiber, granular activated carbon, and a binder, a weight ratio of the activated carbon fiber to the granular activated carbon in the total amount of the activated carbon fiber and the granular activated carbon is 5 to 95 parts by weight of the activated carbon fiber and 95 to 5 parts by weight of the granular activated carbon; a content ratio of the binder in the formed adsorbent is 0.3 to 20 parts by weight per 100 parts by weight of the activated carbon fiber and the granular activated carbon; The total pore volume of the granular activated carbon is 0.90 to 2.50 cm 3 / g, The total pore volume of the activated carbon fiber is 0.50 to 1.20 cm 3 / g, The shaped adsorbent.

2. 2. The formed adsorbent of claim 1, wherein the average pore diameter of the granular activated carbon is from 2.00 to 4.00 nm.

3. The specific surface area of ​​the granular activated carbon is 1400 to 2700 m 2 / g.

4. The average pore diameter of the granular activated carbon is 2.00 to 4.00 nm; The specific surface area of ​​the granular activated carbon is 1400 to 2700 m 2 / g, 2. The shaped adsorbent body of claim 1.

5. The total pore volume of the activated carbon fiber is smaller than the total pore volume of the granular activated carbon, The average pore diameter of the activated carbon fiber is smaller than the average pore diameter of the granular activated carbon.

2. The shaped adsorbent body of claim 1.

6. The average pore diameter of the granular activated carbon is 2.00 to 4.00 nm; The specific surface area of ​​the granular activated carbon is 1400 to 2700 m 2 / g, The total pore volume of the activated carbon fiber is smaller than the total pore volume of the granular activated carbon, The average pore diameter of the activated carbon fiber is smaller than the average pore diameter of the granular activated carbon.

2. The shaped adsorbent body of claim 1.

7. The total pore volume of the formed adsorbent is 0.90 to 2.00 cm 3 / g.

8. 2. The shaped adsorbent body of claim 1, wherein the average pore diameter of the shaped adsorbent body is from 1.87 to 4.00 nm.

9. 2. The formed adsorbent according to claim 1, wherein a weight ratio of the activated carbon fiber to the granular activated carbon in a total amount of the activated carbon fiber and the granular activated carbon is 5 to 70 parts by weight of the activated carbon fiber and 95 to 30 parts by weight of the granular activated carbon.

10. The effective adsorption / desorption rate of 100% n-butane is 75.0% or more, The effective adsorption / desorption rate of 0.2% n-butane is 60.0% or more.

10. The shaped adsorbent body of claim 9.

11. 11. The formed adsorbent according to claim 10, wherein the effective adsorption / desorption rate of 100% n-butane is 81.0% or more.

12. The formed adsorbent according to claim 11, wherein the effective adsorption / desorption rate of 0.2% n-butane is 70.0% or more.

13. The shaped adsorbent body of any one of claims 1 to 12, wherein the binder is a fibrous binder.

Citation Information

Patent Citations

  • Shaped adsorbent for canisters

    WO2022181616A1

  • Activated carbon fiber molded adsorbent

    JP1998005580A

  • Adsorbent, process for producing the same, canister and method for using the same