Composite particles and use thereof

Composite particles with a fluorine-containing compound on the surface and a (meth)acrylic resin shell address shell pinholes and mechanical weakness, enhancing their use in various applications including dispersions and films.

JP2024135524APending Publication Date: 2024-10-04SEKISUI PLASTICS CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023046249
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing hollow particles face issues such as pinholes in the shell and mechanical weakness, leading to potential collapse of the hollow part, especially when enlarged.

Method used

Development of composite particles comprising hollow particles with a fluorine-containing compound attached to the surface, utilizing a shell made of (meth)acrylic resin, which enhances mechanical strength and prevents pinhole formation.

Benefits of technology

The composite particles effectively prevent shell pinholes and hollow portion collapse, enabling applications in dispersions, coating agents, heat insulating films, antireflection films, low dielectric constant films, and photosensitive resin compositions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135524000001
    Figure 2024135524000001
  • Figure 2024135524000002
    Figure 2024135524000002
  • Figure 2024135524000003
    Figure 2024135524000003
Patent Text Reader

Abstract

To provide composite particles that can suppress the occurrence of pinholes in the shell and that can prevent crushing of a hollow portion due to deformation.SOLUTION: Composite particles contain hollow particles and a fluorine-containing compound. The hollow particles have a shell and a hollow portion surrounded by the shell. The fluorine-containing compound adheres to the surface of the hollow particles.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composite particle and its use. [Background technology]

[0002] Particles having voids inside are used as microcapsule particles by incorporating various substances into the voids. Particles having voids inside are also called hollow particles, and are used as light scattering materials, low reflection materials, heat insulating materials, low dielectric constant materials, etc.

[0003] For example, Patent Documents 1 and 2 describe hollow particles obtained by preparing oil droplets containing a radical reactive monomer and a hydrophobic organic solvent that has low compatibility with a polymer of the monomer in an aqueous solvent, and then polymerizing the oil droplets.

[0004] Furthermore, Patent Documents 3, 4 and 5 describe hollow particles whose shells are formed from monomers having fluorine atoms. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Publication No. 2002-80503 [Patent Document 2] Japanese Patent Publication No. 2005-215315 [Patent Document 3] Japanese Patent Application Publication No. 2005-213366 [Patent Document 4] Japanese Patent Publication No. 2020-183500 [Patent Document 5] International Publication No. 2005 / 097870 Summary of the Invention [Problem to be solved by the invention]

[0006] In the hollow particles described in Patent Documents 1 and 2, the shell is formed by laminating polymers precipitated in a hydrophobic organic solvent, and therefore pores (pinholes) penetrating from the shell surface to the hollow part are likely to occur.

[0007] The hollow particles described in Patent Documents 3, 4, and 5 have a shell formed from a monomer having a fluorine atom, and therefore the mechanical strength of the shell is easily reduced, and when the hollow portion is enlarged, particles with a crushed shape may be generated.

[0008] The present invention has been made in view of the above, and has an object to provide composite particles that can suppress the occurrence of pinholes in the shell and prevent the hollow portion from collapsing due to deformation, and uses thereof. [Means for solving the problem]

[0009] As a result of intensive research into achieving the above object, the present inventors have succeeded in developing desired particles containing hollow particles and a fluorine-containing compound, and have found that the above object can be achieved by using said particles. The present invention was completed as a result of further research.

[0010] The present invention provides the following aspects. Item 1. A method for producing a porous material comprising hollow particles and a fluorine-containing compound, The hollow particle has a shell and a hollow portion surrounded by the shell, The fluorine-containing compound is attached to the surface of the hollow particles. composite particles. Section 2. Item 2. The composite particle according to item 1, wherein the fluorine-containing compound is at least one selected from the group consisting of (per)fluoroalkyl compounds, polyvinylidene fluoride, polytetrafluoroethylene, and ethylene-tetrafluoroethylene copolymers. Item 3. The composite particle according to item 1 or 2, wherein the shell contains a (meth)acrylic resin. Item 4. The (meth)acrylic resin comprises a polymer derived from a (meth)acrylic reactive monomer having an epoxy group and / or a polymer derived from a (meth)acrylic reactive monomer having an oxetane group. Composite particles according to item 3. Item 5. The composite particle according to any one of Items 1 to 4, wherein the shell has a density of 1.31 to 1.45. Item 6. A dispersion comprising the composite particle according to any one of items 1 to 5. Item 7. A coating agent comprising the composite particle according to any one of items 1 to 5. Item 8. A heat insulating film comprising the composite particle according to any one of items 1 to 5. Item 9. An antireflection film comprising the composite particle according to any one of items 1 to 5. Item 10. A light extraction film comprising the composite particle according to any one of items 1 to 5. Item 11. A low dielectric constant film comprising the composite particle according to any one of items 1 to 5. Item 12. A photosensitive resin composition comprising the composite particle according to any one of items 1 to 5. Effect of the Invention

[0011] The composite particles of the present invention can suppress the occurrence of pinholes in the shell and can prevent the hollow portion from collapsing due to deformation. Because the composite particles of the present invention have such excellent properties, they can be suitably used in a wide range of applications, such as dispersions, coating agents, heat insulating films, anti-reflective films, light extraction films, low dielectric constant films, and photosensitive resin compositions. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, preferred embodiments of the present invention will be described in detail. The following description of the components may be based on representative embodiments and specific examples, but the present invention is not limited to such embodiments.

[0013] In this specification, the expressions "contain" and "include" include the concepts of "contain", "include", "consist essentially of" and "consist only of".

[0014] In the numerical ranges described in stages in this specification, the upper or lower limit of a certain numerical range can be arbitrarily combined with the upper or lower limit of another numerical range. In addition, in the numerical ranges described in this specification, the upper or lower limit of the numerical range may be replaced with a value shown in an example or a value that can be unambiguously derived from an example. Furthermore, in this specification, a numerical value connected with "~" means a numerical range that includes the numerical values ​​before and after "~" as the lower and upper limits.

[0015] In this specification, "A and / or B" means "one of A and B" or "both A and B", and specifically means "A", "B", or "A and B".

[0016] In this specification, room temperature means a temperature within the range of 20°C to 25°C.

[0017] In this specification, the term "(per)fluoroalkyl compound" means a "(per)fluoroalkyl group-containing compound."

[0018] In this specification, the term "(per)fluoroalkyl group" means a "perfluoroalkyl group" or a "fluoroalkyl group".

[0019] In this specification, the term "perfluoroalkyl group" refers to an alkyl group in which all hydrogen atoms have been substituted with fluorine atoms.

[0020] In this specification, the term "fluoroalkyl group" refers to a group in which some of the hydrogen atoms in an alkyl group have been substituted with fluorine atoms, and does not include the above-mentioned perfluoroalkyl groups.

[0021] As used herein, "(meth)acrylic" means acrylic or methacrylic, and "(meth)acrylate" means acrylate or methacrylate.

[0022] <Composite particles> The composite particles of the present invention have the following configurations (1) to (3): (1) Contains hollow particles and a fluorine-containing compound. (2) The hollow particles have a shell and a hollow portion surrounded by the shell. (3) The fluorine-containing compound is attached to the surface of the hollow particles.

[0023] The composite particles of the present invention have the above-mentioned configurations (1) to (3), and therefore, The occurrence of pinholes in the shell can be suppressed, and the collapse of the hollow portion due to deformation can be prevented. Here, "preventing the collapse of the hollow portion due to deformation" means that the composite particle maintains its spherical shape.

[0024] The composite particles of the present invention are preferably substantially composed of hollow particles and a fluorine-containing compound. Here, "substantially composed of hollow particles and a fluorine-containing compound" means that, in addition to the hollow particles and the fluorine-containing compound, other compounds are contained in small amounts within a range that does not impair the effects of the present invention. For example, when inevitable impurities are mixed in addition to the hollow particles and the fluorine-containing compound, it means that "substantially composed of hollow particles and a fluorine-containing compound".

[0025] It is particularly preferable that the composite particles of the present invention consist only of hollow particles and a fluorine-containing compound.

[0026] The composite particles of the present invention have a fluorine-containing compound attached to the surface of the hollow particles. It is preferable that at least a part of the surface of the hollow particles of the present invention is coated with a fluorine-containing compound. In other words, it is preferable that at least a part of the surface of the hollow particles of the present invention is coated with a fluorine-containing compound.

[0027] In the present invention, it is more preferable that at least a portion of the surface of the hollow particles is covered with a layer made of a fluorine-containing compound.

[0028] In the present invention, the phrase "the entire surface of the hollow particle is coated with a fluorine-containing compound" means that 100% of the surface of the hollow particle is coated with the fluorine-containing compound.

[0029] In the present invention, a portion of the surface of the hollow particle is coated with a fluorine-containing compound means that typically 1% or more and less than 100% of the surface of the hollow particle is coated with the fluorine-containing compound.

[0030] The lower limit of the above "part of the surface of the hollow particle" is usually 1% or more, preferably 30% or more, more preferably 50% or more, even more preferably 60% or more, still more preferably 70% or more, particularly preferably 80% or more, and most preferably 90% or more.

[0031] The upper limit of the above "part of the surface of the hollow particle" is not particularly limited, but is usually less than 100%, and may be 99.9% or less, 99.5% or less, 99% or less, or 95% or less.

[0032] As one embodiment of the present invention, it is preferable that the fluorine-containing compound is attached to the surface of the hollow particle via electrostatic interaction, van der Waals force, chemical bond, etc. The chemical bond is not particularly limited, and examples thereof include a covalent bond, an ionic bond, a coordinate bond, a chelate bond, and a hydrogen bond.

[0033] As one embodiment of the present invention, it is more preferable that the fluorine-containing compound is attached to the surface of the hollow particles via electrostatic interaction.

[0034] As one embodiment of the present invention, at least a part of the surface of the hollow particle is preferably covered with a fluorine-containing compound via electrostatic interaction, van der Waals forces, chemical bonds, etc. Here, the chemical bonds are not particularly limited, and examples thereof include covalent bonds, ionic bonds, coordinate bonds, chelate bonds, hydrogen bonds, etc.

[0035] As one embodiment of the present invention, it is more preferable that at least a part of the surface of the hollow particle is coated with a fluorine-containing compound via electrostatic interaction.

[0036] In the present invention, the mass ratio of the hollow particles to the fluorine-containing compound (mass of hollow particles:mass of fluorine-containing compound) is preferably 100:4 to 100:58, more preferably 100:6 to 100:56, even more preferably 100:8 to 100:54, still more preferably 100:10 to 100:52, and particularly preferably 100:12 to 100:50.

[0037] In the present invention, the content of the fluorine-containing compound in 100% by mass of the composite particles is preferably from 2% by mass to 36% by mass, more preferably from 4% by mass to 34% by mass, even more preferably from 6% by mass to 32% by mass, and still more preferably from 8% by mass to 30% by mass.

[0038] <Hollow particles> The composite particles of the present invention contain hollow particles. The hollow particles have a shell and a hollow portion surrounded by the shell. The composite particles of the present invention contain hollow particles having a structure in which the hollow portion is surrounded by a shell. The composite particles of the present invention are characterized in that the interior of the hollow particles has a hollow structure.

[0039] In the present invention, the average particle size of the hollow particles is preferably 10 nm to 150 nm, more preferably 30 nm to 120 nm. If the average particle size of the hollow particles is 10 nm or more, the aggregation of composite particles containing hollow particles can be further suppressed, and the handling property can be further improved. If the average particle size of the hollow particles is 150 nm or less, the scattering at the surface unevenness or particle interface can be further suppressed when the composite particles containing hollow particles are kneaded with a coating agent, resin, etc.

[0040] In the present invention, the lower limit of the average particle diameter of the hollow particles can be 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, and 70 nm. In the present invention, the upper limit of the average particle diameter of the hollow particles can be 150 nm, 140 nm, 130 nm, 120 nm, 110 nm, 100 nm, and 90 nm. These upper and lower limits can be combined in any combination.

[0041] In the present invention, the hollow particles preferably have a void ratio of 10 to 90% by volume, more preferably 15 to 80% by volume, and even more preferably 20 to 70% by volume.

[0042] In the present invention, the lower limit of the hollow ratio of the hollow particles can be 10 volume%, 15 volume%, 20 volume%, 25 volume%, 30 volume%, 32 volume%, 34 volume%, 36 volume%, 38 volume%, and 40 volume%. In the present invention, the upper limit of the hollow ratio of the hollow particles can be 90 volume%, 80 volume%, 70 volume%, 60 volume%, 55 volume%, and 50 volume%. These upper and lower limits can be combined in any combination.

[0043] In the present invention, the shell preferably comprises at least one or more layers. In the present invention, when the shell comprises at least one or more layers, the layer constituting the shell may comprise one layer, or may comprise two or more layers (e.g., two layers, three layers, four layers, etc.).

[0044] In the present invention, the shell preferably contains a (meth)acrylic resin. In the present invention, the shell more preferably contains a (meth)acrylic resin that does not contain a fluorine atom.

[0045] In the present invention, the hollow particles have a shell consisting of at least one layer, and the at least one layer preferably contains a (meth)acrylic resin. In the present invention, the hollow particles have a shell consisting of at least one layer, and the at least one layer more preferably contains a (meth)acrylic resin that does not contain a fluorine atom.

[0046] In the present invention, the hollow particles have a shell consisting of at least one or more layers, and the at least one or more layers are preferably made of a (meth)acrylic resin. In the present invention, the hollow particles have a shell consisting of at least one or more layers, and the at least one or more layers are preferably made of a (meth)acrylic resin that does not contain fluorine atoms.

[0047] As one embodiment of the present invention, the entire shell is preferably composed of a (meth)acrylic resin that does not contain fluorine atoms.

[0048] In another embodiment of the present invention, the content of the (meth)acrylic resin not containing fluorine atoms in 100 mass% of the shell is preferably 60 mass% or more, more preferably 70 mass% or more, even more preferably 80 mass% or more, still more preferably 90 mass% or more, and particularly preferably 95 mass% or more.

[0049] <(Meth)acrylic resin> The (meth)acrylic resin is a polymer obtained by reacting a (meth)acrylic reactive monomer. The (meth)acrylic resin is preferably a polymer having a crosslinked structure (also referred to as a "crosslinked polymer") obtained by further adding a crosslinkable monomer to a polymer obtained by reacting a (meth)acrylic reactive monomer and reacting the polymer.

[0050] The (meth)acrylic resin preferably contains a polymer derived from a (meth)acrylic reactive monomer having an epoxy group and / or a polymer derived from a (meth)acrylic reactive monomer having an oxetane group. In other words, the (meth)acrylic resin preferably contains a polymer containing a structural unit derived from a (meth)acrylic reactive monomer having an epoxy group and / or a polymer containing a structural unit derived from a (meth)acrylic reactive monomer having an oxetane group.

[0051] The (meth)acrylic resin more preferably contains a polymer derived from a (meth)acrylic reactive monomer having an epoxy group. In other words, the (meth)acrylic resin more preferably contains a polymer containing a structural unit derived from a (meth)acrylic reactive monomer having an epoxy group.

[0052] The epoxy group or oxetane group is a functional group that reacts with a compound having an amino group, a carboxy group, a chlorosulfone group, a mercapto group, a hydroxyl group, an isocyanate group, or the like to produce a polymer.

[0053] When the (meth)acrylic reactive monomer has an epoxy group or an oxetane group, a polymer having a crosslinked structure (crosslinked polymer) can be produced by radically polymerizing the (meth)acrylic reactive monomer having an epoxy group or an oxetane group and then reacting the epoxy group or the oxetane group with a crosslinkable monomer.

[0054] In the present invention, the shell preferably contains a (meth)acrylic resin, and the (meth)acrylic resin preferably contains a polymer derived from a (meth)acrylic reactive monomer having a silyl group. In other words, in the present invention, the shell preferably contains a (meth)acrylic resin, and the (meth)acrylic resin preferably contains a polymer containing a structural unit derived from a (meth)acrylic reactive monomer having a silyl group.

[0055] In the case where the (meth)acrylic reactive monomer has a silyl group, a polymer having a crosslinked structure (crosslinked polymer) can be produced by radically polymerizing the (meth)acrylic reactive monomer having a silyl group and then reacting the silyl group with a crosslinkable monomer.

[0056] The (meth)acrylic resin preferably contains a polymer having as its constituent a copolymer consisting of a (meth)acrylic reactive monomer having an epoxy group or an oxetane group and a (meth)acrylic reactive monomer having a silyl group. In the copolymer, the ratio (mass ratio) of the (meth)acrylic reactive monomer unit having an epoxy group or an oxetane group to the (meth)acrylic reactive monomer unit having a silyl group is preferably in the range of 1:100 to 1:0.001. Within such a ratio range, composite particles containing hollow particles with a higher shell strength can be obtained, so that when used in optical scattering materials, low reflection materials, etc., desired properties (light scattering properties, low refractive index, etc.) can be obtained.

[0057] In the above copolymer, a more preferred ratio (mass ratio) of the (meth)acrylic reactive monomer unit having an epoxy group or an oxetane group to the (meth)acrylic reactive monomer unit having a silyl group is in the range of 1:10 to 1:0.001 (the former:the latter), and an even more preferred ratio (mass ratio) of the former:the latter is in the range of 1:1 to 1:0.01 (the former:the latter).

[0058] In the (meth)acrylic resin, the total content of the (meth)acrylic reactive monomer having an epoxy group or an oxetane group and the (meth)acrylic reactive monomer having a silyl group is preferably 10 mass % or more, more preferably 30 mass % or more, even more preferably 50 mass % or more, and still more preferably 70 mass % or more of the total components derived from the (meth)acrylic reactive monomers.

[0059] The content of the (meth)acrylic reactive monomer having an epoxy group or an oxetane group is preferably 50 parts by mass to 90 parts by mass, more preferably 55 to 88 parts by mass, and still more preferably 60 to 85 parts by mass, relative to 100 parts by mass in total of the (meth)acrylic reactive monomer having an epoxy group or an oxetane group and the (meth)acrylic reactive monomer having a silyl group.

[0060] The content of the (meth)acrylic reactive monomer having an epoxy group is preferably 50 parts by mass to 90 parts by mass, more preferably 55 to 88 parts by mass, and still more preferably 60 to 85 parts by mass, relative to 100 parts by mass in total of the (meth)acrylic reactive monomer having an epoxy group and the (meth)acrylic reactive monomer having a silyl group.

[0061] In the present invention, when the shell of the hollow particle contains a (meth)acrylic resin, the content of the (meth)acrylic resin is preferably 5 to 100 parts by mass, more preferably 10 to 100 parts by mass, even more preferably 50 to 100 parts by mass, even more preferably 75 to 100 parts by mass, particularly preferably 90 to 100 parts by mass, and most preferably 99 to 100 parts by mass, relative to 100 parts by mass of the shell of the hollow particle. When the content of the (meth)acrylic resin is 5 parts by mass or more relative to 100 parts by mass of the shell of the hollow particle, the dispersibility in the organic binder used for preparing the heat insulating coating material is further improved, and whitening of the coating film can be further prevented.

[0062] The (meth)acrylic resin preferably contains a polymer derived from a crosslinkable monomer containing a nitrogen atom (a polymer containing a structural unit derived from a crosslinkable monomer containing a nitrogen atom). The (meth)acrylic resin is a crosslinked polymer having nitrogen atoms, which is obtained by polymerizing the (meth)acrylic reactive monomer and then crosslinking the polymer with a crosslinkable monomer containing a nitrogen atom.

[0063] The (meth)acrylic resin more preferably contains a polymer derived from an amine compound (a polymer containing a structural unit derived from an amine compound).

[0064] The (meth)acrylic resin more preferably contains a polymer derived from an aliphatic amine compound or a heterocyclic amine compound (a polymer containing a structural unit derived from an aliphatic amine compound or a heterocyclic amine compound).

[0065] The (meth)acrylic resin more preferably contains a polymer derived from an aliphatic amine compound (a polymer containing a structural unit derived from an aliphatic amine compound).

[0066] When the (meth)acrylic resin contains a polymer derived from an amine compound, the content of the amine compound is usually 1 to 75 parts by mass, preferably 5 to 70 parts by mass, more preferably 10 to 65 parts by mass, even more preferably 15 to 60 parts by mass, still more preferably 20 to 55 parts by mass, and particularly preferably 22 to 50 parts by mass, relative to 100 parts by mass of the total of the (meth)acrylic reactive monomers, from the viewpoint of improving the heat resistance and mechanical strength of the hollow particles. The amine compound is preferably an aliphatic amine compound or a heterocyclic amine compound, and more preferably an aliphatic amine compound.

[0067] <(Meth)acrylic reactive monomer> The (meth)acrylic reactive monomer has a (meth)acrylic reactive functional group. Examples of the (meth)acrylic reactive monomer include esters of (meth)acrylic acid and alcohols having 1 to 25 carbon atoms.

[0068] Examples of esters of (meth)acrylic acid and alcohols having 1 to 25 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tertiary butyl (meth)acrylate, n-pentyl (meth)acrylate, cyclohexyl (meth)acrylate, n-heptyl (meth)acrylate, iso-octyl (meth)acrylate, n-nonyl (meth)acrylate, i Examples of such esters include so-decyl (meth)acrylate, norbornyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, lauryl (meth)acrylate, tetradecyl acrylate, tetradecyl methacrylate, iso-stearyl (meth)acrylate, isobornyl (meth)acrylate, phenoxyethylene glycol mono(meth)acrylate, phenoxydiethylene glycol (meth)acrylate, 2-ethylhexyl (meth)acrylate, etc. These esters can be used alone or in combination of two or more.

[0069] The (meth)acrylic reactive monomer is preferably a reactive monomer having a (meth)acrylic reactive functional group and a non-(meth)acrylic reactive functional group. A reactive monomer having a (meth)acrylic reactive functional group and a non-(meth)acrylic reactive functional group can be polymerized based on either one of the two functional groups to produce polymer particles. The other functional group remaining in the polymer particles is reacted with a crosslinkable monomer to make the polymer particles into a polymer having a crosslinked structure (crosslinked polymer).

[0070] Before crosslinking as described above, the non-reactive solvent is mixed with the reactive monomer in advance or absorbed into the polymer particles after the polymer particles are produced, and then the crosslinking reaction is carried out, whereby the polymer and the non-reactive solvent are phase-separated to obtain microcapsule particles containing the non-reactive solvent. The non-reactive solvent is then removed to obtain hollow particles.

[0071] The (meth)acrylic reactive monomer is preferably a (meth)acrylic reactive monomer having an epoxy group or an oxetane group. Examples of the (meth)acrylic reactive monomer having an epoxy group or an oxetane group include glycidyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate glycidyl ether, (3-ethyloxetan-3-yl)methyl (meth)acrylate, and 3,4-epoxycyclohexylmethyl (meth)acrylate. These monomers can be used alone or in combination of two or more. Glycidyl (meth)acrylate means glycidyl methacrylate (glycidyl methacrylate) and glycidyl acrylate (glycidyl acrylate).

[0072] The (meth)acrylic reactive monomer is preferably a (meth)acrylic reactive monomer having a silyl group. Examples of the (meth)acrylic reactive monomer having a silyl group include 3-methacryloxypropyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, and 3-acryloxypropyltrimethoxysilane. These monomers can be used alone or in combination of two or more.

[0073] <Cross-linking monomer> The crosslinkable monomer is preferably a nitrogen atom-containing crosslinkable monomer, and the nitrogen atom-containing crosslinkable monomer is preferably an amine compound.

[0074] The amine compound is preferably an aliphatic amine compound and / or a heterocyclic amine compound, and more preferably an aliphatic amine compound.

[0075] <Aliphatic amine compounds> Examples of the aliphatic amine compound include ethylenediamine, N,N,N',N'-tetramethylethylenediamine, propylenediamine, N,N,N',N'-tetramethylpropylenediamine, dimethylaminopropylamine, diethylaminopropylamine, dibutylaminopropylamine, diethylenetriamine, N,N,N',N'',N''-pentamethyldiethylenetriamine, triethylenetetramine, tetraethylenepentamine, 3,3'-diaminodipropylamine, butanediamine, pentanediamine, hexanediamine, trimethylhexanediamine, N,N,N',N'-tetramethylhexanediamine, bis(2-dimethylaminoethyl)ether, 2-[2-(dimethylamino)ethoxy]ethanol, triethanolamine, dimethylaminohexanol, and 3,9-bis(3-aminopropyl)-2,4,8,10-tetraoxyspiro(5,5)undecane adduct. These aliphatic amine compounds can be used alone or in combination of two or more.

[0076] In the present invention, the aliphatic amine compound is preferably ethylenediamine.

[0077] <Heterocyclic amine compounds> Examples of the heterocyclic amine compound include pyrrolidine, piperidine, piperazine, N-methylpiperazine, N,N'-dimethylpiperazine, N-aminoethylpiperazine, N,N',N'-trimethylaminoethylpiperazine, morpholine, methylmorpholine, ethylmorpholine, quinuclidine (1-azabicyclo[2.2.2]octane), triethylenediamine (1,4-diazabicyclo[2.2.2]octane), pyrrole, pyrazole, pyridine, hexahydro-1,3,5-tris(3-dimethylaminopropyl)-1,3,5-triazine, 1,8-diazabicyclo-[5.4.0]-7-Undecene, Imidazole, 1-Methylimidazole, 2-Methylimidazole, 3-Methylimidazole, 4-Methylimidazole, 5-Methylimidazole, 1-Ethylimidazole, 2-Ethylimidazole, 3-Ethylimidazole, 4-Ethylimidazole, 5-Ethylimidazole, 1-n-Propylimidazole, 2-n-Propylimidazole, 1-Isopropylimidazole, 2-Isopropylimidazole Imidazole, 1-n-butylimidazole, 2-n-butylimidazole, 1-isobutylimidazole, 2-isobutylimidazole, 2-undecyl-1H-imidazole, 2-heptadecyl-1H-imidazole, 1,2-dimethylimidazole, 1,3-dimethylimidazole, 2,4-dimethylimidazole, 2-ethyl-4-methylimidazole, 1-phenylimidazole, 2-phenyl-1H-imidazole 4-Methyl-2-phenyl-1H-imidazole, 2-Phenyl-4-methylimidazole, 1-Benzyl-2-methylimidazole, 1-Benzyl-2-phenylimidazole, 1-Cyanoethyl-2-methylimidazole, 1-Cyanoethyl-2-ethyl-4-methylimidazole, 1-Cyanoethyl-2-undecylimidazole, 1-Cyanoethyl-2-phenylimidazole, 2-Phenylimidazole isothiocyanate Examples of the heterocyclic amine compounds include anuric acid adduct, 2-methylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 1-cyanoethyl-2-phenyl-4,5-di(2-cyanoethoxy)methylimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, and 1-benzyl-2-phenylimidazole hydrochloride. These heterocyclic amine compounds can be used alone or in combination of two or more.

[0078] In the present invention, the heterocyclic amine compound is preferably N-aminoethylpiperazine.

[0079] <Fluorine-containing compounds> In the composite particles of the present invention, a fluorine-containing compound is attached to the surface of the hollow particles. It is preferable that the composite particles of the present invention have a surface treated with a fluorine-containing compound. In other words, it is preferable that the surface of the hollow particles of the present invention is treated with a fluorine-containing compound. By treating the surface of the hollow particles with a fluorine-containing compound, the dispersibility in an organic solvent is further improved, and the composite particles can be given the property that the binder is more difficult to penetrate into the hollow parts of the hollow particles.

[0080] In the present invention, the fluorine-containing compound is preferably at least one selected from the group consisting of (per)fluoroalkyl compounds, polyvinylidene fluoride, polytetrafluoroethylene, and ethylene-tetrafluoroethylene copolymers.

[0081] In the present invention, the fluorine-containing compound is more preferably a (per)fluoroalkyl compound.

[0082] <(Per)fluoroalkyl compounds> In the present invention, the (per)fluoroalkyl compound is preferably at least one compound selected from the group consisting of (per)fluoroalkyl group-containing phosphate esters and salts thereof, (per)fluoroalkyl group-containing sulfonic acids and salts thereof, (per)fluoroalkyl group-containing carboxylic acids and salts thereof, (per)fluoroalkyl alcohols, (per)fluoroalkyl alkylene oxide adducts, fluoroalkyl esters of (meth)acrylic acid, and fluoroalkyl group-containing silane compounds.

[0083] In the present invention, the (per)fluoroalkyl compound is more preferably at least one compound selected from the group consisting of (per)fluoroalkyl group-containing phosphate esters and salts thereof, fluoroalkyl esters of (meth)acrylic acid, and fluoroalkyl group-containing silane compounds.

[0084] In the present invention, the (per)fluoroalkyl compound is more preferably at least one compound selected from the group consisting of (per)fluoroalkyl group-containing phosphate esters, fluoroalkyl esters of (meth)acrylic acid, and fluoroalkyl group-containing silane compounds.

[0085] <(Per)fluoroalkyl group-containing phosphate esters and their salts> In the present invention, examples of the salt of a (per)fluoroalkyl group-containing phosphate ester include metal salts of a (per)fluoroalkyl group-containing phosphate ester and ammonium salts of a (per)fluoroalkyl group-containing phosphate ester.

[0086] In the present invention, the (per)fluoroalkyl group-containing phosphate ester and the salt thereof can be used either alone or in combination of two or more kinds.

[0087] Examples of the metal salt include sodium salt, potassium salt, magnesium salt, calcium salt, and the like.

[0088] The (per)fluoroalkyl group-containing phosphate ester and salt thereof preferably have a straight-chain or branched-chain (per)fluoroalkyl group having 1 to 20 carbon atoms (1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20).

[0089] The above (per)fluoroalkyl group-containing phosphate ester and salt thereof more preferably have a straight-chain or branched-chain (per)fluoroalkyl group having 1 to 15 carbon atoms (1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14 or 15).

[0090] The above (per)fluoroalkyl group-containing phosphate ester and salts thereof more preferably have a straight-chain or branched-chain (per)fluoroalkyl group having 1 to 12 carbon atoms (1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11 or 12).

[0091] The above-mentioned (per)fluoroalkyl group-containing phosphate ester and salts thereof are more preferably R 1 has a linear or branched (per)fluoroalkyl group having 1 to 10 carbon atoms (1, 2, 3, 4, 5, 6, 7, 8, 9 or 10).

[0092] <Fluoroalkyl ester of (meth)acrylic acid> The fluoroalkyl ester of (meth)acrylic acid is, for example, trifluoromethyl (meth)acrylate, 2,2,2-trifluoroethyl (meth)acrylate (2,2,2-trifluoroethyl acrylate or 2,2,2-trifluoroethyl methacrylate), Perfluoroethyl (meth)acrylate, 3,3,3-trifluoropropyl (meth)acrylate, perfluoro-n-propyl (meth)acrylate, 4,4,4-trifluorobutyl (meth)acrylate, perfluoro-n-butyl (meth)acrylate, perfluoro-n-pentyl (meth)acrylate, Perfluoro-n-hexyl (meth)acrylate, perfluoro-n-heptyl (meth)acrylate, Perfluoro-n-octyl (meth)acrylate, Perfluoro-n-nonyl (meth)acrylate, perfluoro-n-decyl (meth)acrylate, 2,2,3,3-tetrafluoropropyl (meth)acrylate, 1H,1H,5H-octafluoropentyl (meth)acrylate, 2,2,3,3,4,4,5,5,6,6,7,7-dodecafluoroheptyl (meth)acrylate, 1,1,1,3,3,3-Hexafluoroisopropyl (meth)acrylate 2,2,3,4,4,4-Hexafluorobutyl (meth)acrylate 3-perfluorohexyl-2-hydroxypropyl (meth)acrylate, pentafluorophenyl (meth)acrylate. These fluoroalkyl esters of (meth)acrylic acid can be used alone or in combination of two or more kinds.

[0093] The fluoroalkyl ester of (meth)acrylic acid is preferably at least one compound selected from the group consisting of trifluoromethyl (meth)acrylate, 2,2,2-trifluoroethyl (meth)acrylate, and perfluoroethyl (meth)acrylate.

[0094] <Fluoroalkyl group-containing silane compound> The fluoroalkyl group-containing silane compound is preferably a compound represented by the following formula (1): R 1 -(CH2)n-Si-(OR 2 )3 formula (1) [In the formula, R 1 represents a linear or branched (per)fluoroalkyl group having 1 to 6 carbon atoms (1, 2, 3, 4, 5 or 6). R 2 represents a linear or branched alkyl group having 1 to 4 carbon atoms (1, 2, 3 or 4). n represents an integer of 0 to 4 (0, 1, 2, 3, or 4).

[0095] In the above formula (1), R 1Examples of the linear or branched (per)fluoroalkyl group having 1 to 6 carbon atoms (1, 2, 3, 4, 5 or 6) and represented by the formula (I) include a trifluoromethyl group, a (per)fluoroethyl group, a (per)fluoro-n-propyl group, a (per)fluoroisopropyl group, a (per)fluoro-n-butyl group, a (per)fluoroisobutyl group, a (per)fluoro-sec-butyl group, a (per)fluoro-tert-butyl group, a (per)fluoro-n-pentyl group, a (per)fluoro-1,1-dimethylpropyl group, a (per)fluoro-1,2-dimethylpropyl group, a (per)fluoro-1-methylbutyl group, a (per)fluoro-2-methylbutyl group, a (per)fluoro-3-methylbutyl group, a (per)fluoro-n-hexyl group, a (per)fluoro-1-methylpentyl group, Examples of the perfluoro group include (per)fluoro-2-methylpentyl group, (per)fluoro-3-methylpentyl group, (per)fluoroisohexyl group, (per)fluoro-1,1-dimethylbutyl group, (per)fluoro-1,2-dimethylbutyl group, (per)fluoro-2,2-dimethylbutyl group, (per)fluoro-1,3-dimethylbutyl group, (per)fluoro-2,3-dimethylbutyl group, (per)fluoro-3,3-dimethylbutyl group, (per)fluoro-1-ethylbutyl group, (per)fluoro-2-ethylbutyl group, (per)fluoro-1,1,2-trimethylpropyl group, (per)fluoro-1,2,2-trimethylpropyl group, (per)fluoro-1-ethyl-1-methylpropyl group, (per)fluoro-1-ethyl-2-methylpropyl group, etc. Here, "perfluoro" means perfluoro or fluoro.

[0096] In the above formula (1), R 1 is preferably a linear (per)fluoroalkyl group having 1 to 6 carbon atoms (1, 2, 3, 4, 5 or 6).

[0097] The linear (per)fluoroalkyl group having 1 to 6 carbon atoms (1, 2, 3, 4, 5, or 6) is a trifluoromethyl group, a (per)fluoroethyl group, a (per)fluoro-n-propyl group, a (per)fluoro-n-butyl group, a (per)fluoro-n-pentyl group, or a (per)fluoro-n-hexyl group. Here, "(per)fluoro" means perfluoro or fluoro.

[0098] In the above formula (1), R 2 The linear or branched alkyl group having 1 to 4 carbon atoms (1, 2, 3 or 4) represented by the formula (I) is a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group or a tert-butyl group.

[0099] In the above formula (1), R 2 is preferably a methyl group, an ethyl group, an n-propyl group or an isopropyl group, more preferably a methyl group or an ethyl group, and even more preferably a methyl group.

[0100] In the above formula (1), n ​​is preferably 0, 1, 2 or 3, more preferably 0, 1 or 2, and even more preferably 1 or 2.

[0101] In the present invention, it is a preferred embodiment that the fluoroalkyl group-containing silane compound does not include trimethoxy(3,3,3-trifluoropropyl)silane and a silane coupling agent represented by the following formula (2). [ka] (In the formula, R 1 each independently represents an alkyl group having 1 to 6 carbon atoms, an alkoxyalkyl group having 2 to 4 carbon atoms, or a phenyl group which may have a substituent. R 2 each independently represents an alkyl group having 1 to 6 carbon atoms, an alkoxyalkyl group having 2 to 4 carbon atoms, or a phenyl group which may have a substituent. R 3 represents a divalent organic group having 1 to 30 carbon atoms. R4 represents a hydrogen atom or a methyl group. m represents an integer of 0 to 2. R 1 and R 2 R is a substituent of an alkyl group having 1 to 6 carbon atoms represented by the following formula: 1 and R 2 and R 1 and R 2 Each of the substituents of the phenyl group represented by the following formula (I) represents a fluorine atom.

[0102] In the above formula (2), R 1 and R 2 Examples of the alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, an isobutyl group, and an n-hexyl group.

[0103] In the above formula (2), R 1 and R 2 Examples of the alkoxyalkyl group having 2 to 4 carbon atoms include a methoxymethyl group, a methoxyethyl group, an ethoxymethyl group, a methoxybutyl group, an ethoxyethyl group, a butoxymethyl group, and structural isomers thereof.

[0104] In the above formula (2), R 3 Examples of the divalent organic group having 1 to 30 carbon atoms include alkanediyl groups such as methylene, ethylene, trimethylene, tetramethylene, pentamethylene, hexamethylene, heptamethylene, octamethylene, nonamethylene, decamethylene, undecamethylene, dodecamethylene, tridecamethylene, and tetradecamethylene. The alkanediyl group may have a branched structure substituted with an alkyl group.

[0105] <(Per)fluoroalkyl group-containing sulfonic acids and their salts> Examples of the (per)fluoroalkyl group-containing sulfonic acid and its salt include (Per)fluoromethanesulfonic acid and its metal or ammonium salts, (Per)fluoroethanesulfonic acid and its metal or ammonium salts, (Per)fluoro-n-propanesulfonic acid and its metal or ammonium salts, (Per)fluoro-n-butanesulfonic acid and its metal or ammonium salts, (Per)fluoro-n-pentanesulfonic acid and its metal or ammonium salts, (Per)fluoro-n-hexanesulfonic acid and its metal or ammonium salts, (Per)fluoro-n-heptanesulfonic acid and its metal or ammonium salts, Examples include (per)fluoro-n-octanesulfonic acid and its metal salts or ammonium salts, etc. Here, "(per)fluoro" means perfluoro or fluoro. These (per)fluoroalkyl group-containing sulfonic acids and salts thereof can be used alone or in combination of two or more.

[0106] Examples of the metal salt include sodium salt, potassium salt, magnesium salt, calcium salt, and the like.

[0107] <(Per)fluoroalkyl group-containing carboxylic acid and its salt> The (per)fluoroalkyl group-containing carboxylic acid and its salt include (Per)fluoromethanecarboxylic acids and their metal or ammonium salts, (Per)fluoroethanecarboxylic acid and its metal or ammonium salts, (Per)fluoro-n-propanecarboxylic acid and its metal or ammonium salts, (Per)fluoro-n-butanecarboxylic acid and its metal or ammonium salts, (Per)fluoro-n-pentanecarboxylic acid and its metal or ammonium salts, (Per)fluoro-n-hexanecarboxylic acid and its metal or ammonium salts, (Per)fluoro-n-heptanecarboxylic acid and its metal or ammonium salts, Examples of the carboxylic acid having a (per)fluoroalkyl group and its salts include (per)fluoro-n-octanesulfonic acid and its metal salts or ammonium salts. Here, "(per)fluoro" means perfluoro or fluoro. These (per)fluoroalkyl group-containing carboxylic acids and their salts can be used alone or in combination of two or more.

[0108] Examples of the metal salt include sodium salt, potassium salt, magnesium salt, calcium salt, and the like.

[0109] <(Per)fluoroalkyl alcohol> The (per)fluoroalkyl alcohol is preferably an alcohol having a linear or branched (per)fluoroalkyl group having 1 to 14 carbon atoms.

[0110] Examples of the (per)fluoroalkyl alcohol include 2,2,2-Trifluoroethanol, 2,2,3,3,3-Pentafluoropropanol, 1H,1H-Heptafluorobutanol, 2-((per)fluorobutyl)ethanol, 2-((per)fluorohexyl)ethanol, 2-((per)fluorooctyl)ethanol, 2-((per)fluorodecyl)ethanol, 2-((per)fluoro-3-methylbutyl)ethanol, 2-((per)fluoro-5-methylhexyl)ethanol, 2-((per)fluoro-7-methyloctyl)ethanol, 2-((per)fluoro-9-methyldecyl)ethanol, 1H,1H,3H-Tetrafluoropropanol, 1H,1H,5H-Octafluoropentanol, 1H,1H,7H-Dodecafluoroheptanol, 1H,1H,9H-Hexadecafluorononanol, 2H-Hexafluoropropanol, 1H,1H,7H-Dodecafluoroheptanol, 1H,1H,9H-Hexadecafluorononanol, 1H-Hexafluoropropanol, 1H,1H,9H-Hexadecafluoroprop ... Examples of the fluoro-2-propanol include fluoro-2-propanol, 1H,1H,3H-hexafluorobutanol, 2,2-bis(trifluoromethyl)propanol, 2,2-bis(trifluoromethyl)-2-heptafluoropropylethanol, 6-((per)fluoroethyl)hexanol, 6-((per)fluorobutyl)hexanol, 3-((per)fluorohexyl)propanol, 6-((per)fluorohexyl)hexanol, 3-((per)fluorooctyl)-1-propanol, 6-((per)fluorooctyl)hexanol, 6-((per)fluoro-1-methylethyl)hexanol, 6-((per)fluoro-3-methylbutyl)hexanol, 6-((per)fluoro-5-methylhexyl)hexanol, and 6-((per)fluoro-7-methyloctyl)hexanol. Here, "(per)fluoro" means perfluoro or fluoro. These (per)fluoroalkyl alcohols can be used alone or in combination of two or more kinds.

[0111] <(Per)fluoroalkyl alkylene oxide adduct> The (per)fluoroalkyl alkylene oxide adduct is preferably a (per)fluoroalkyl ethylene oxide adduct.

[0112] <Commercially available (per)fluoroalkyl compounds> As the (per)fluoroalkyl compound, known commercially available products can be widely used. Commercially available products include, for example, Megafac F-114, Megafac F-251, Megafac F-253, Megafac F-281, Megafac F-410, Megafac F-430, Megafac F-444, Megafac F-477, Megafac F-510, Megafac F-551, Megafac F-552, Megafac F-553, Megafac F-554, Megafac F-555, Megafac F-556, and Megafac F-557. , Megafack F-558, Megafack F-559, Megafack F-560, Megafack F-561, Megafack F-562, Megafack F-563, Megafack F-565, Megafack F-568, Megafack F-569, Megafack F-570, Megafack F-572, Megafack F-574, Megafack F-575, Megafack F-576, Megafack R-40, Megafack R-40-LM, Megafack R-41 , Megafac R-94, Megafac RS-56, Megafac RS-72-K, Megafac RS-75, Megafac RS-76-E, Megafac RS-76-NS, Megafac RS-78, Megafac RS-90, Megafac DS-21 (all manufactured by DIC Corporation), FC-4430, FC-4432 (all manufactured by 3M Japan Ltd.), Surflon S-211, Surflon S-221, Surflon S-231, Surflon S-2 32, Surflon S-233, Surflon S-241, Surflon S-242, Surflon S-243, Surflon S-420, Surflon S-431, Surflon S-386, Surflon S-611, Surflon S-647, Surflon S-651, Surflon S-653, Surflon S-656, Surflon S-658, Surflon S-693, Surflon S-CFJ, Surflon FPE-50 (all manufactured by AGC Seimi Chemical Co., Ltd.). These commercially available products may be used alone or in combination of two or more.

[0113] <Polyvinylidene fluoride> Examples of the polyvinylidene fluoride include vinylidene fluoride homopolymers, vinylidene fluoride copolymers having a vinylidene fluoride ratio of 50 mol % or more, etc. Examples of the vinylidene fluoride copolymers include copolymers of vinylidene fluoride with at least one selected from the group consisting of tetrafluoroethylene, hexafluoropropylene, trifluoroethylene, trichloroethylene, and vinyl fluoride, etc.

[0114] The polyvinylidene fluoride is preferably a vinylidene fluoride homopolymer.

[0115] As the polyvinylidene fluoride, a wide variety of known commercially available products can be used. Examples of commercially available products include "Kynar 720 (vinylidene fluoride content: 100 mass%)" manufactured by Arkema, "Kynar 710 (vinylidene fluoride content: 100 mass%)" manufactured by Kureha Corporation, "KFT#850 (vinylidene fluoride content: 100 mass%)" manufactured by Solvay Specialty Polymers, "Solef 1006 (vinylidene fluoride content: 100 mass%)" and "Solef 1008 (vinylidene fluoride content: 100 mass%)" manufactured by Solvay Specialty Polymers. These can be used alone or in combination of two or more types.

[0116] <Polytetrafluoroethylene> Examples of the polytetrafluoroethylene include polytetrafluoroethylene (PTFE), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroethylene-perfluoroalkoxy group copolymer (PFA), tetrafluoroethylene-olefin copolymer (ETFE), etc. These polytetrafluoroethylenes can be used alone or in combination of two or more kinds.

[0117] As the polytetrafluoroethylene, a wide variety of known commercially available products can be used. Examples of commercially available products include "Polyflon PTFE" manufactured by Daikin Industries, Ltd., "Teflon (registered trademark) PTFE" manufactured by Mitsui-Chemours Fluoroproducts, Inc., and "Fluon (registered trademark) PTFE" manufactured by AGC Inc. These commercially available products can be used alone or in combination of two or more kinds.

[0118] <Ethylene-tetrafluoroethylene copolymer> The ethylene-tetrafluoroethylene copolymer preferably has a molar ratio of ethylene units to tetrafluoroethylene units in the range of 5:95 to 80:20.

[0119] As the ethylene-tetrafluoroethylene copolymer, a wide variety of known commercially available products can be used. Examples of commercially available products include "NEOFLON (registered trademark) ETFE EP-610" and "NEOFLON (registered trademark) ETFE EP-546" manufactured by Daikin Industries, Ltd., and "Fluon LM-ETFE (registered trademark) LM-720AP", "Fluon LM-ETFE (registered trademark) LM-730AP", and "Fluon LM-ETFE (registered trademark) LM-740AP" manufactured by AGC Inc. These commercially available products can be used alone or in combination of two or more kinds.

[0120] In the present invention, polyvinylidene fluoride, polytetrafluoroethylene and ethylene-tetrafluoroethylene copolymers are not included in the above-mentioned (per)fluoroalkyl compounds.

[0121] <Other additives> As long as the effects of the present invention are not impaired, the composite particles of the present invention may contain additives such as pigment particles (pigments), dyes, stabilizers, UV absorbers, defoamers, thickeners, heat stabilizers, leveling agents, lubricants, and antistatic agents.

[0122] The pigment particles are not particularly limited as long as they are pigment particles used in the technical field. For example, there are iron oxide pigments such as micaceous iron oxide and iron black; lead oxide pigments such as red lead and yellow lead; titanium oxide pigments such as titanium white (rutile titanium oxide), titanium yellow and titanium black; cobalt oxide; zinc oxide pigments such as zinc yellow; molybdenum oxide pigments such as molybdenum red and molybdenum white. The pigment particles can be used alone or in combination of two or more kinds.

[0123] <Dispersion containing composite particles> The embodiments of the dispersion containing the composite particles of the present invention will be exemplified below.

[0124] In this embodiment, the dispersion liquid contains a dispersion medium and the composite particles of the present invention. The dispersion medium is not particularly limited as long as it is a liquid that does not completely dissolve the composite particles of the present invention.

[0125] Examples of the dispersion medium include water such as natural water, purified water, distilled water, ion-exchanged water, and pure water; alcohol-based solvents such as methanol, ethanol, butanol, isobutanol, and n-propyl alcohol; ketone-based solvents such as acetone, methyl ethyl ketone, methyl propyl ketone, methyl isobutyl ketone, diisobutyl ketone, and cyclohexanone diacetone alcohol; ether-based solvents such as ethylene glycol mono-n-propyl ether, diethylene glycol mono-n-propyl ether, and propylene glycol monomethyl ether; ester-based solvents such as methyl acetate, ethyl acetate, butyl acetate, methoxybutyl acetate, amyl acetate, propyl acetate, ethyl lactate, methyl lactate, and butyl lactate; hydrocarbon-based solvents such as toluene, xylene, solvent naphtha, hexane, cyclohexane, ethylcyclohexane, methylcyclohexane, heptane, octane, and decane; and halogen-based solvents such as methyl chloride, methylene chloride, chloroform, and carbon tetrachloride. These dispersion media can be used alone or in combination of two or more.

[0126] <Applications of composite particles> The composite particle of the present invention is useful as an additive for master pellets for forming molded articles such as coating agents, paints, paper, information recording paper, light diffusion films (optical sheets), heat insulating films, thermoelectric conversion materials, light guide plate inks, anti-reflection films, light extraction films, photosensitive resin films, light diffusion plates, and light guide plates; or as an additive for cosmetics.

[0127] <Coating agent> The embodiments of the coating agent containing the composite particles of the present invention will be exemplified below.

[0128] In this embodiment, the coating agent contains the composite particles of the present invention. The coating agent may further contain a binder in addition to the composite particles of the present invention.

[0129] The binder may be any known binder commonly used in this field, such as a thermosetting resin or a thermoplastic resin.

[0130] More specifically, examples of the binder include fluorine-based resins, polyamide resins, acrylic resins, polyurethane resins, acrylic urethane resins, butyral resins, etc. These binders can be used alone or in combination of two or more kinds.

[0131] The binder may be a homopolymer of one reactive monomer or a copolymer of multiple monomers.

[0132] The reactive monomer used in the binder is Methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, (cyclo)hexyl (meth)acrylate, heptyl (meth)acrylate, iso-octyl (meth)acrylate, nonyl (meth)acrylate, iso-decyl (meth)acrylate, norbornyl (meth)acrylate, iso Monofunctional reactive monomers such as esters of (meth)acrylic acid with alcohols having 1 to 25 carbon atoms, such as bornyl (meth)acrylate, adamantyl (meth)acrylate, lauryl (meth)acrylate, tetradecyl (meth)acrylate, iso-stearyl (meth)acrylate, isobornyl (meth)acrylate, phenoxyethylene glycol (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, and 2-ethylhexyl (meth)acrylate; Trimethylolpropane tri(meth)acrylate, tripropylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, pentaerythritol tri(meth)acrylate (pentaerythritol triacrylate or pentaerythritol trimethacrylate), pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, di polyfunctional reactive monomers such as pentaerythritol penta(meth)acrylate, tripentaerythritol octa(meth)acrylate, tetrapentaerythritol deca(meth)acrylate, isocyanuric acid tri(meth)acrylate, isocyanuric acid di(meth)acrylate, polyester tri(meth)acrylate, polyester di(meth)acrylate, bisphenol di(meth)acrylate, diglycerin tetra(meth)acrylate, adamantyl di(meth)acrylate, isobornyl di(meth)acrylate, dicyclopentane di(meth)acrylate, tricyclodecane di(meth)acrylate, and ditrimethylolpropane tetra(meth)acrylate; Examples include:

[0133] In addition, when using these reactive monomers, a polymerization initiator that initiates a curing reaction by ionizing radiation may be used. Examples of the polymerization initiator include imidazole derivatives, bisimidazole derivatives, N-arylglycine derivatives, organic azide compounds, titanocenes, aluminate complexes, organic peroxides, N-alkoxypyridinium salts, and thioxanthone derivatives.

[0134] In addition, as the binder, for example, an inorganic binder such as a hydrolyzate of silicon alkoxide can be used. Examples of silicon alkoxide include tetramethoxysilane, tetraethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 2-hydroxyethyltrimethoxysilane, 2-hydroxyethyltriethoxysilane, 2-hydroxypropyltrimethoxysilane, 2-hydroxypropyltriethoxysilane, 3-hydroxypropyltrimethoxysilane, 3-hydroxypropyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltriacetoxysilane, allyltrimethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxytrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyl Pyrtriethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-isocyanatopropyltrimethoxysilane, 3-isocyanatopropyltriethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane, 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-ureidopropyltrimethoxysilane, 3-ureidopropyltriethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, diethyldimethoxysilane, and diethyldiethoxysilane.

[0135] As the binder, a wide variety of known commercially available products can be used, such as "DIANAL LR-102" and "DIANAL BR-106" manufactured by Mitsubishi Rayon Co., Ltd.

[0136] In this embodiment, when the coating agent contains a binder and the composite particles of the present invention, the content of the composite particles in the coating agent is appropriately adjusted depending on the application, but is usually 0.1 to 1000 parts by mass per 100 parts by mass of the binder.

[0137] The coating agent usually contains a dispersion medium, which may be either an aqueous or oil-based medium.

[0138] Examples of the oily medium include hydrocarbon solvents such as toluene and xylene, ketone solvents such as methyl ethyl ketone and methyl isobutyl ketone, ester solvents such as ethyl acetate and butyl acetate, and ether solvents such as dioxane and ethylene glycol diethyl ether.

[0139] The aqueous medium includes water and alcohol-based solvents.

[0140] The coating agent may contain, in addition to the composite particles of the present invention, additives such as a hardener, a colorant, an antistatic agent, and a leveling agent.

[0141] The substrate to which the coating agent is applied is not particularly limited, and a substrate depending on the application can be used. For example, for optical applications, transparent substrates such as glass substrates and transparent resin substrates are used.

[0142] <Master Pellet> The following are examples of the master pellets containing the composite particles of the present invention.

[0143] In this embodiment, the master pellet contains the composite particle of the present invention. The master pellet may further contain a base resin in addition to the composite particle of the present invention.

[0144] The base resin may be a known thermoplastic resin commonly used in this field. Examples of the thermoplastic resin include (meth)acrylic resin, (meth)acrylic acid alkyl-styrene copolymer resin, polycarbonate resin, polyester resin, polyethylene resin, polypropylene resin, polystyrene resin, etc. These thermoplastic resins may be used alone or in combination of two or more.

[0145] The base resin is preferably at least one selected from the group consisting of (meth)acrylic resins, alkyl (meth)acrylate-styrene copolymer resins, polycarbonate resins and polyester resins, in order to further improve transparency.

[0146] The above-mentioned base resin may contain small amounts of additives such as ultraviolet absorbers, heat stabilizers, colorants, and fillers.

[0147] In this embodiment, the master pellets can be produced by melt-kneading the base resin and the composite particles of the present invention, followed by a molding method such as extrusion molding or injection molding.

[0148] In this embodiment, the content of the composite particles in the master pellet is preferably 0.1 to 60% by mass, more preferably 0.3 to 30% by mass, and even more preferably 0.4 to 10% by mass.

[0149] In this embodiment, the master pellets are molded into a molded article by, for example, extrusion molding, injection molding, or press molding. A base resin may be added during molding.

[0150] The base resin is preferably added in such an amount that the content of the composite particles in the final molded product is 0.1 to 60% by mass.

[0151] During molding, small amounts of additives such as ultraviolet absorbers, heat stabilizers, colorants, and fillers may be added.

[0152] <Cosmetics> The embodiments of the cosmetic preparation containing the composite particles of the present invention will be exemplified below.

[0153] In this embodiment, the cosmetic contains the composite particle of the present invention. In this embodiment, examples of the cosmetic include solid cosmetic such as face powder and foundation, powder cosmetic such as baby powder and body powder, and liquid cosmetic such as lotion, milky lotion, cream, liquid foundation, body lotion, and pre-shave lotion.

[0154] The content of the composite particles in the cosmetic varies depending on the type of the cosmetic.

[0155] In the case of solid cosmetic preparations such as face powder and foundation, the content of the composite particles in the cosmetic preparation is preferably 1 to 20% by mass, and more preferably 3 to 15% by mass.

[0156] In the case of powdery cosmetics such as baby powder and body powder, the content of the composite particles in the cosmetics is preferably 1 to 20 mass %, more preferably 3 to 15 mass %.

[0157] In the case of liquid cosmetics such as lotion, milky lotion, cream, liquid foundation, body lotion, and pre-shave lotion, the content of the composite particles in the cosmetics is preferably 1 to 15 mass %, more preferably 3 to 10 mass %.

[0158] In this embodiment, the cosmetic composition may contain other ingredients, for example, inorganic compounds such as mica and talc, coloring pigments such as iron oxide, titanium oxide, ultramarine, Prussian blue, and carbon black, or synthetic dyes such as azo dyes, in order to improve optical functions or tactile feel.

[0159] When the cosmetic is a liquid cosmetic, the liquid medium is not particularly limited, but water, alcohol, hydrocarbons, silicone oil, vegetable or animal fats and oils, etc. may be used.

[0160] In this embodiment, in addition to the other ingredients described above, various functions can be added to the cosmetic by adding moisturizing agents, anti-inflammatory agents, whitening agents, UV care agents, germicides, antiperspirants, cooling agents, fragrances, and the like that are commonly used in cosmetics.

[0161] <Anti-reflective film> The embodiments of the anti-reflection film containing the composite particles of the present invention will be exemplified below.

[0162] In this embodiment, the anti-reflective film contains the composite particles of the present invention. In this embodiment, examples of the anti-reflective film include a film and a sheet-like shape.

[0163] In this embodiment, a film containing the composite particles or a sheet-shaped object containing the composite particles can be used as an anti-reflection film because the refractive index is reduced by the air layer in the hollow portion of the composite particles.

[0164] In this embodiment, the antireflection film can be obtained by applying the coating agent to a substrate by a well-known method such as a dipping method, a spraying method, a spin coating method, a spinner method, or a roll coating method, drying the coating, and, if necessary, heating, irradiating with ultraviolet light, baking, or the like.

[0165] <Light extraction film> The embodiments of the light extraction film containing the composite particles of the present invention will be exemplified below.

[0166] In this embodiment, the light extraction film contains the composite particles of the present invention. In LEDs, organic EL lighting, etc., the difference in refractive index between the air layer and the light-emitting layer is large, so the emitted light is easily trapped inside the element. Therefore, a light extraction film is used for the purpose of improving the light emission efficiency.

[0167] In this embodiment, the light extraction film may be, for example, a film, a sheet-like object, etc. A film containing composite particles or a sheet-like object containing composite particles can be used as a light extraction film because the refractive index is reduced by the air layer in the hollow portion of the composite particles.

[0168] In this embodiment, the light extraction film can be obtained by applying the coating agent to a substrate by a well-known method such as a dipping method, a spraying method, a spin coating method, a spinner method, or a roll coating method, drying the coating, and further, if necessary, heating, irradiating with ultraviolet light, baking, or the like.

[0169] <Thermal insulation film> The embodiment of the heat insulating film containing the composite particles of the present invention will be exemplified below.

[0170] In this embodiment, the heat insulating film contains the composite particles of the present invention. Examples of the heat insulating film include a film and a sheet-like shape.

[0171] In this embodiment, the film containing the composite particles or the sheet-shaped product containing the composite particles can be used as a heat insulating film because it has an air layer in the hollow space of the composite particles. In addition, because the particle diameter of the composite particles is small, the heat insulating film has high transparency. Furthermore, because the binder does not easily penetrate into the hollow space of the composite particles, the heat insulating film has high heat insulating properties.

[0172] In this embodiment, the heat insulating film can be obtained by applying the above-mentioned coating agent to a substrate by a well-known method such as a dipping method, a spraying method, a spin coating method, a spinner method, or a roll coating method, drying the coating, and further, if necessary, heating, irradiating with ultraviolet rays, baking, or the like.

[0173] <Low dielectric constant film> The embodiments of the low dielectric constant film containing the composite particles of the present invention will be exemplified below.

[0174] In this embodiment, the low dielectric constant film contains the composite particles of the present invention. Examples of the low dielectric constant film include a film and a sheet-like shape.

[0175] In this embodiment, a film containing the composite particles or a sheet-shaped object containing the composite particles can be used as a low dielectric constant film because the composite particles have an air layer in the hollow portion thereof. In addition, because the particle diameter of the composite particles is small, the low dielectric constant film has high transparency.

[0176] In this embodiment, the low dielectric constant film can be obtained by applying the coating agent to a substrate by a well-known method such as a dipping method, a spraying method, a spin coating method, a spinner method, or a roll coating method, drying the coating, and further, if necessary, heating, irradiating with ultraviolet rays, baking, or the like.

[0177] <Photosensitive resin composition> The embodiments of the photosensitive resin composition containing the composite particles of the present invention will be exemplified below.

[0178] In this embodiment, the photosensitive resin composition contains the composite particles of the present invention. The photosensitive resin composition containing the composite particles has a low refractive index because the composite particles have an air layer in the hollow portion thereof. In addition, the photosensitive resin composition has high transparency because the composite particles have a small particle diameter.

[0179] In this embodiment, the photosensitive resin composition can be obtained by applying the coating agent to a substrate by a well-known method such as a dipping method, a spraying method, a spin coating method, a spinner method, or a roll coating method, drying the coating, and further, if necessary, heating, irradiating with ultraviolet light, baking, or the like.

[0180] <Method of manufacturing composite particles> The composite particles of the present invention can be produced by surface-treating hollow particles with a fluorine-containing compound. Specifically, the composite particles of the present invention can be produced by surface-treating hollow particles in an aqueous dispersion of hollow particles with a fluorine-containing compound.

[0181] The method for producing the composite particles of the present invention will be described in detail below. Hereinafter, the step of surface-treating the hollow particles with a fluorine-containing compound may be simply referred to as the "surface treatment step."

[0182] In the surface treatment step, details of the fluorine-containing compound are as described above in <Composite particles> unless otherwise specified.

[0183] In the surface treatment step, the amount of the fluorine-containing compound used is preferably 4 parts by mass or more and 58 parts by mass or less, more preferably 6 parts by mass or more and 56 parts by mass or less, even more preferably 8 parts by mass or more and 54 parts by mass or less, still more preferably 10 parts by mass or more and 52 parts by mass or less, and particularly preferably 12 parts by mass or more and 50 parts by mass or less, relative to 100 parts by mass of the hollow particles.

[0184] In the surface treatment step, the amount of the fluorine-containing compound used is preferably from 4 to 58 parts by mass, more preferably from 6 to 56 parts by mass, even more preferably from 8 to 54 parts by mass, still more preferably from 10 to 52 parts by mass, and particularly preferably from 12 to 50 parts by mass, relative to 1,000 parts by mass of the hollow particle aqueous dispersion.

[0185] The surface treatment step is preferably carried out in the following order: step (1), step (2) and step (3). Step (1): In a vessel, a fluorine-containing compound and a surfactant are dissolved in an organic solvent. Step (2): A hollow particle dispersion liquid is added and stirred at room temperature to prepare a slurry. Step (3): The prepared slurry is cross-flow washed with an organic solvent using a filter.

[0186] In the above step (1), examples of the organic solvent include lower alcohols such as methanol, ethanol, 1-propanol, 2-propanol (isopropyl alcohol), 1-butanol, 2-butanol, 2-methyl-1-propanol, and 2-methyl-2-propanol.

[0187] In the above step (1), as the surfactant, a wide variety of known surfactants commonly used in this field can be used. Examples of the surfactant include anionic surfactants, cationic surfactants, amphoteric surfactants, nonionic surfactants, etc. These surfactants can be used alone or in combination of two or more.

[0188] In the above step (1), the surfactant is preferably an anionic surfactant.

[0189] Examples of the anionic surfactant include carboxylic acids, sulfonic acids, sulfates, and phosphates. The anionic surfactant is preferably a phosphate. The phosphate is preferably a polyoxyethylene alkyl ether phosphate.

[0190] Examples of polyoxyethylene alkyl ether phosphates include polyoxyethylene tridecyl ether phosphate, polyoxyethylene tridecyl ether phosphate, polyoxyethylene alkyl (C8) ether phosphate, polyoxyethylene alkyl (C8) ether phosphate monoethanolamine salt, polyoxyethylene alkyl (C12,13) ​​ether phosphate, polyoxyethylene lauryl ether phosphate, polyoxyethylene tridecyl ether phosphate, polyoxyethylene alkyl (C12-15) ether phosphate, etc. These polyoxyethylene alkyl ether phosphates can be used alone or in combination of two or more.

[0191] In the above step (1), the amount of the fluorine-containing compound used is preferably 15 parts by mass or more and 400 parts by mass or less, more preferably 20 parts by mass or more and 350 parts by mass or less, and even more preferably 25 parts by mass or more and 325 parts by mass or less, relative to 100 parts by mass of the surfactant.

[0192] In the above step (1), the amount of the organic solvent used is preferably 500 parts by mass or more and 4000 parts by mass or less, more preferably 1000 parts by mass or more and 3500 parts by mass or less, relative to 100 parts by mass of the total amount of the fluorine-containing compound and the surfactant used.

[0193] The method for producing the hollow particle dispersion used in the above step (2) will be described later in <Method for producing hollow particles>.

[0194] In the above step (3), any filter that is commonly used in this field and is known in the art can be widely used as the filter, so long as it allows the composite particles in the slurry to pass through.

[0195] Since the diameter of the hollow particles in the slurry is usually 1 nm or more and 200 nm or less, the pore size of the filter is preferably 1 nm or more and 200 nm or less. As a filter with such a pore size, for example, a ceramic filter or the like can be used.

[0196] In the above step (3), the organic solvent is Hydrocarbon solvents such as toluene, xylene, hexane, and cyclohexane; Ketone solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; Ester solvents such as ethyl acetate, methyl acetate, n-butyl acetate, isobutyl acetate, sec-butyl acetate, and tert-butyl acetate; Ether solvents such as isopropyl ether and tetrahydrofuran; Glycol solvents such as ethylene glycol, diethylene glycol, triethylene glycol, and propylene glycol; Glycol ether solvents such as diethylene glycol monomethyl ether and propylene glycol monomethyl ether; Amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone These organic solvents can be used alone or in combination of two or more kinds.

[0197] After the cross-flow washing in the above step (3), it is preferable to adjust the solid content concentration in the composite particle dispersion using the organic solvent used in step (3). The solid content concentration in the composite particle dispersion is preferably 4 to 50 mass%, more preferably 6 to 40 mass%, 8 to 30 mass%, and even more preferably 10 to 20 mass%.

[0198] In the present invention, the composite particles may be used as a dry powder by removing the solvent from the dispersion liquid of the composite particles and drying the same, if necessary. The method for drying the composite particles is not particularly limited, but examples thereof include reduced pressure drying.

[0199] <Method of manufacturing hollow particles> The hollow particles can be produced, for example, through a process including a step of preparing polymer particles containing a non-reactive solvent (polymerization process), a step of phase-separating the non-reactive solvent from the polymer particles (phase separation process), and a step of removing the non-reactive solvent (solvent removal process).

[0200] The method for producing hollow particles may be a method in which a polymerization step and a phase separation step are carried out simultaneously by reacting reactive monomers, or a method in which polymer particles are first formed before phase separation of a non-reactive solvent, and then phase separation is caused. The method in which polymer particles are first formed and then phase separation is caused is preferred because it can suppress the generation of pinholes and improve monodispersity.

[0201] In the method in which polymer particles are first formed before phase separation of the non-reactive solvent and then phase separation occurs, specifically, a reactive monomer having a (meth)acrylic reactive functional group and a non-(meth)acrylic reactive functional group is polymerized based on either one of the two functional groups to produce polymer particles.

[0202] The non-reactive solvent is contained in the polymer particles by mixing it with the reactive monomer in advance or by allowing it to be absorbed into the polymer particles after the production of the polymer particles.

[0203] Next, the remaining functional group of the two functional groups is polymerized to separate the polymer from the non-reactive solvent, thereby obtaining microcapsule particles containing the non-reactive solvent. The non-reactive solvent is then removed to obtain hollow particles.

[0204] As described above, by separating the polymerization process from the phase separation process, The gaps between the polymer shells that existed in conventional manufacturing methods no longer exist, suppressing the occurrence of pinholes in the shells of the resulting hollow particles. The shape of microcapsule particles and hollow particles does not depend on oil droplets, but on the shape and particle size distribution of polymer particles before phase separation, making it easy to obtain microcapsule particles and hollow particles with high monodispersity. This manufacturing method will now be described.

[0205] (A) Polymerization process In the polymerization step, a reactive monomer having a (meth)acrylic reactive functional group and a non-(meth)acrylic reactive functional group is polymerized based on either one of the functional groups to produce polymer particles. The non-reactive solvent is contained in the polymer particles by mixing it with the reactive monomer in advance or by absorbing it after the polymer particles are produced.

[0206] (a) Method for Producing Polymer Particles As a method for producing the polymer particles, any method can be adopted from among known methods such as bulk polymerization, solution polymerization, dispersion polymerization, suspension polymerization, and emulsion polymerization. Among them, the suspension polymerization and emulsion polymerization methods, which can relatively easily produce polymer particles, are preferred. Furthermore, the emulsion polymerization method, which can easily produce polymer particles with high monodispersity, is more preferred.

[0207] <Polymerization initiator> In carrying out the polymerization, it is preferable to add a compound for reacting the functional group to be the subject of the polymerization reaction. When polymerizing a (meth)acrylic reactive functional group, a polymerization initiator can be used as the compound.

[0208] Examples of the polymerization initiator include persulfates such as ammonium persulfate (ammonium peroxodisulfate), potassium persulfate, and sodium persulfate; organic peroxides such as cumene hydroperoxide, di-tert-butyl peroxide, dicumyl peroxide, benzoyl peroxide, lauroyl peroxide, dimethylbis(tert-butylperoxy)hexane, dimethylbis(tert-butylperoxy)hexyne-3, bis(tert-butylperoxyisopropyl)benzene, bis(tert-butylperoxy)trimethylcyclohexane, butyl-bis(tert-butylperoxy)valerate, tert-butyl 2-ethylhexaneperoxy acid, dibenzoyl peroxide, paramenthane hydroperoxide, and tert-butyl peroxybenzoate; 2,2-Azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, 2,2-Azobis[2-(2-imidazolin-2-yl)propane]disulfate dihydrate, 2,2-Azobis(2-amidinopropane)dihydrochloride, 2,2-Azobis[N-(2-carboxyethyl)-2-methylpropionamidine]hydrate, 2,2-Azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane}dihydrochloride, 2,2-Azobis[2-(2-imidazolin-2-yl)propane], 2,2-Azobis(1-imino-1-pyrrolidino -2-Ethylpropane) dihydrochloride, 2,2-azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propionamide}, 2,2-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], 4,4-azobis(4-cyanopentanoic acid), 2,2-azobisisobutyronitrile (2,2-azobis(2-methyl-butyronitrile), 2,2-azobis(2-isopropylbutyronitrile), 2,2-azobis(2,3-dimethylbutyronitrile), 2,2-azobis(2,4-dimethylbutyronitrile), ), 2,2-azobis(2-methylcapronitrile), 2,2-azobis(2,3,3-trimethylbutyronitrile), 2,2-azobis(2,4,4-trimethylvaleronitrile), 2,2-azobis(2,4-dimethylvaleronitrile), 2,2-azobis(2,4-dimethyl-4-ethoxyvaleronitrile), 2,2-azobis(2,4-dimethyl-4-n-butoxyvaleronitrile), 2,2-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2-azobis[N-(2-propenyl)-2-methylpropionamide], 2,2 azo compounds such as azobis(N-butyl-2-methylpropionamide), 2,2-azobis(N-cyclohexyl-2-methylpropionamide), 1,1-azobis(1-acetoxy-1-phenylethane), 1,1-azobis(cyclohexane-1-carbonitrile), dimethyl-2,2-azobis(2-methylpropionate), dimethyl-2,2-azobisisobutyrate, dimethyl-2,2'-azobis(2-methylpropionate), 2-(carbamoylazo)isobutyronitrile, and 4,4-azobis(4-cyanovaleric acid).These polymerization initiators can be used alone or in combination of two or more kinds.

[0209] In addition, a redox initiator obtained by combining the above-mentioned persulfate and organic peroxide polymerization initiator with a reducing agent such as sodium sulfoxylate formaldehyde, sodium hydrogen sulfite, ammonium hydrogen sulfite, sodium thiosulfate, ammonium thiosulfate, hydrogen peroxide, sodium hydroxymethanesulfinate, L-ascorbic acid and its salts, cuprous salts, and ferrous salts may be used as the polymerization initiator.

[0210] In the case of emulsion polymerization, the polymerization initiator is preferably a water-soluble polymerization initiator capable of emulsion polymerization in an aqueous solvent.

[0211] Examples of the water-soluble polymerization initiator include persulfates such as ammonium persulfate (ammonium peroxodisulfate), potassium persulfate, and sodium persulfate; 2,2-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, 2,2-azobis[2-(2-imidazolin-2-yl)propane]disulfate dihydrate, 2,2-azobis(2-amidinopropane)dihydrochloride, 2,2-azobis[N-(2-carboxyethyl)-2-methylpropionamidine]hydrate, 2,2-azobis{2-[1-(2-hydro Examples of the azotized compounds include 2,2-azobis[2-(2-imidazolin-2-yl)propane], 2,2-azobis(1-imino-1-pyrrolidino-2-ethylpropane) dihydrochloride, 2,2-azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propionamide}, 2,2-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], and 4,4-azobis(4-cyanopentanoic acid). These water-soluble polymerization initiators can be used alone or in combination of two or more.

[0212] The polymer particles are preferably polymerized first based on the (meth)acrylic reactive functional group, so that the polymer particles have unreacted non-(meth)acrylic reactive functional groups. If the polymer is polymerized first based on the non-(meth)acrylic reactive functional group, the non-reactive solvent may be difficult to absorb.

[0213] <Chain transfer agent> A chain transfer agent may be used during polymerization of the reactive monomer. Examples of the chain transfer agent include alkyl mercaptans such as n-hexyl mercaptan, n-octyl mercaptan, tert-octyl mercaptan, n-dodecyl mercaptan, and tert-dodecyl mercaptan; phenolic compounds such as α-methylstyrene dimer, 2,6-di-tert-butyl-4-methylphenol, and styrenated phenol; allyl compounds such as allyl alcohol; and halogenated hydrocarbon compounds such as dichloromethane, dibromomethane, and carbon tetrachloride. These chain transfer agents can be used alone or in combination of two or more. The upper limit of the amount of the chain transfer agent used is 10 parts by mass relative to 100 parts by mass of the reactive monomer.

[0214] <Surfactant> A surfactant may be used during polymerization of the reactive monomer. The type of surfactant is not particularly limited, and for example, a wide variety of known surfactants can be used.

[0215] Examples of the surfactant include anionic surfactants, cationic surfactants, amphoteric surfactants, and nonionic surfactants. These surfactants can be used alone or in combination of two or more. Among these surfactants, anionic surfactants are preferred.

[0216] The upper limit of the amount of the surfactant used is usually 5 parts by mass based on 100 parts by mass of the reactive monomer.

[0217] As the anionic surfactant, a wide variety of known commercially available products can be used, such as "Aqualon AR-1025" manufactured by Daiichi Kogyo Seiyaku Co., Ltd.

[0218] <Dispersion aid> When preparing the polymer particles, a hydrophilic monomer may be used as a reactive monomer other than the (meth)acrylic reactive monomer. The hydrophilic monomer plays a role as a dispersion assistant, so that the use of the hydrophilic monomer can improve the dispersion stability during polymerization.

[0219] The type of the hydrophilic monomer is not particularly limited, and for example, known hydrophilic monomers can be widely adopted. Examples of the hydrophilic monomer include carboxyl group-containing vinyl monomers and their salts; sulfone group-containing vinyl monomers and vinyl sulfate monoesters and their salts; phosphoric acid group-containing vinyl monomers and their salts; hydroxyl group-containing vinyl monomers; nitrogen-containing vinyl monomers, etc. These hydrophilic monomers can be used alone or in combination of two or more.

[0220] Examples of the carboxyl group-containing vinyl monomer include (anhydride) maleic acid, maleic acid monoalkyl ester, fumaric acid, fumaric acid monoalkyl ester, crotonic acid, itaconic acid, itaconic acid monoalkyl ester, itaconic acid glycol monoether, citraconic acid, citraconic acid monoalkyl ester, cinnamic acid, and salts thereof. Examples of these salts include alkali metal salts (sodium salt, potassium salt, etc.), ammonium salts, amine salts, and quaternary ammonium salts of the carboxyl group-containing vinyl monomers. The carboxyl group-containing vinyl monomers and their salts can be used alone or in combination of two or more.

[0221] Examples of sulfone group-containing vinyl monomers and vinyl sulfate monoesters include vinyl sulfonic acid, (meth)allyl sulfonic acid, p-styrene sulfonic acid, sulfopropyl (meth)acrylate, 2-hydroxy-3-(meth)acryloxypropyl sulfonic acid, 2-(meth)acryloylamino-2,2-dimethylethanesulfonic acid, 2-(meth)acryloyloxyethanesulfonic acid, 3-(meth)acryloyloxy-2-hydroxypropanesulfonic acid, and the like. Acid, 2-(meth)acrylamido-2-methylpropanesulfonic acid, 3-(meth)acrylamido-2-hydroxypropanesulfonic acid, alkyl (carbon number 3-18)allylsulfosuccinic acid, sulfate ester of poly(n=2-30)oxyalkylene (ethylene, propylene, butylene, etc., which may be single, random, or block) mono(meth)acrylate [poly(n=5-15)oxypropylene monomethacrylate sulfate ester, etc.], and salts thereof. Examples of these salts include alkali metal salts (sodium salt, potassium salt, etc.), ammonium salts, amine salts, and quaternary ammonium salts of the above-mentioned sulfonic acid-containing vinyl monomers and vinyl sulfate monoesters. The above-mentioned sulfonic acid-containing vinyl monomers and vinyl sulfate monoesters, and salts thereof can be used alone or in combination of two or more.

[0222] Among the above-mentioned sulfone group-containing vinyl monomers and vinyl sulfate monoesters, and salts thereof, sodium p-styrenesulfonate is preferred from the viewpoint of further enhancing the dispersion stability during polymerization.

[0223] Examples of the phosphoric acid group-containing vinyl monomer include 2-hydroxyethyl (meth)acryloyl phosphate, phenyl-2-acryloyloxyethyl phosphate, and salts thereof. Examples of the salts include alkali metal salts (sodium salt, potassium salt, etc.), ammonium salts, amine salts, and quaternary ammonium salts of the phosphoric acid group-containing vinyl monomer. The phosphoric acid group-containing vinyl monomer and the salts thereof can be used alone or in combination of two or more.

[0224] Examples of hydroxyl group-containing vinyl monomers include hydroxystyrene, N-methylol (meth)acrylamide, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, polyethylene glycol mono(meth)acrylate, and (meth)allyl alcohol. The above hydroxyl group-containing vinyl monomers can be used alone or in combination of two or more.

[0225] Examples of nitrogen-containing vinyl monomers include quaternized products of tertiary amine group-containing vinyl monomers such as aminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, (meth)acrylamide, N-methyl(meth)acrylamide, N-butylacrylamide, diacetone acrylamide, (meth)acrylonitrile, dimethylaminoethyl (meth)acrylate, and diethylaminoethyl (meth)acrylamide (which have been quaternized using a quaternizing agent such as methyl chloride, dimethyl sulfate, benzyl chloride, or dimethyl carbonate).

[0226] (b) Absorption of non-reactive solvents The absorption of the non-reactive solvent into the polymer particles can be carried out during or after the production of the polymer particles. The absorption of the non-reactive solvent can be carried out in the presence or absence of a dispersion medium that is not compatible with the non-reactive solvent. It is preferable to carry out the absorption in the presence of a dispersion medium, since the absorption of the non-reactive solvent can be carried out efficiently. When the method for producing polymer particles uses a medium, the medium may be used as a dispersion medium as it is, or the polymer particles may be once isolated from the medium and then dispersed in another dispersion medium.

[0227] A non-reactive solvent that is incompatible with the dispersion medium is added to the dispersion medium containing the polymer particles, and the non-reactive solvent can be absorbed into the polymer particles by stirring or the like for a certain period of time.

[0228] The absorption of the non-reactive solvent during the production of the polymer particles can be achieved by selecting a suitable dispersion medium and non-reactive solvent for the production of the polymer particles. For example, when the polymer particles are produced by emulsion polymerization in a water solvent, the production of the polymer particles and the absorption of the polymer particles can be performed simultaneously by adding a non-reactive solvent that is not compatible with water to the water solvent in advance and polymerizing a reactive monomer. The production of the polymer particles and the absorption of the polymer particles can be performed simultaneously to reduce the time required for the absorption of the non-reactive solvent.

[0229] <Dispersion medium> The dispersion medium is not particularly limited as long as it is a liquid that does not completely dissolve the polymer particles. For example, ion-exchanged water; alcohols such as ethyl alcohol, methyl alcohol, and isopropyl alcohol; alkanes such as butane, pentane, hexane, cyclohexane, heptane, decane, and hexadecane; aromatic hydrocarbons such as toluene and xylene; ester solvents such as ethyl acetate and butyl acetate; ketone solvents such as methyl ethyl ketone and methyl isobutyl ketone; halogen-based solvents such as methyl chloride, methylene chloride, chloroform, and carbon tetrachloride. These dispersion media can be used alone or in combination of two or more.

[0230] <Non-reactive solvent> The non-reactive solvent is not particularly limited as long as it is a liquid that is incompatible with the dispersion medium. In this case, incompatible with the dispersion medium means that the solubility of the non-reactive solvent in the dispersion medium (at 25° C.) is 10% by weight or less.

[0231] For example, when ion-exchanged water is used as the dispersion medium, examples of non-reactive solvents that can be used include butane, pentane, hexane, cyclohexane, heptane, decane, hexadecane, toluene, xylene, ethyl acetate, butyl acetate, methyl ethyl ketone, methyl isobutyl ketone, 1,4-dioxane, methyl chloride, methylene chloride, chloroform, carbon tetrachloride, etc. These non-reactive solvents can be used alone or in combination of two or more.

[0232] The amount of the non-reactive solvent to be added is not particularly limited, but is 20 to 5000 parts by mass relative to 100 parts by mass of the polymer particles. If it is less than 20 parts by mass, the hollow part of the obtained macrocapsule particles or hollow particles may become small, and the desired characteristics may not be obtained. If it exceeds 5000 parts by mass, the hollow part may become too large, and the strength of the obtained microcapsule particles or hollow particles may decrease.

[0233] (B) Phase separation process Following the polymerization step, the remaining reactive functional groups are polymerized to cause phase separation between the polymer and the non-reactive solvent, resulting in microcapsule particles encapsulating the non-reactive solvent.

[0234] In this specification, the term "hollow" in hollow particles is not limited to the case where air is present in the hollow portion, but also includes the case where a gas other than air is present in the hollow portion.

[0235] In addition, in this specification, hollow particles are not limited to hollow particles in which a gas exists in the hollow portion, but also include microcapsule particles in which a non-reactive solvent or other dispersion medium exists in the hollow portion.

[0236] The compound added to polymerize the remaining reactive functional groups can be the same as the polymerization initiator for polymerizing the (meth)acrylic reactive functional groups and the crosslinking agent (crosslinkable monomer) for polymerizing the non-(meth)acrylic reactive functional groups described in the above polymerization step.

[0237] (C) Solvent removal (substitution) process In the present invention, the hollow particles can be converted into hollow particles having a gas such as air or another solvent present in the hollow portion by removing or replacing the non-reactive solvent encapsulated in the microcapsule particles as necessary.

[0238] The method for removing the non-reactive solvent is not particularly limited, but may be reduced pressure drying, etc. Conditions for the reduced pressure drying include a pressure of 500 Pa or less, 30 to 200° C., and 30 minutes to 50 hours.

[0239] The non-reactive solvent can also be replaced by a solvent replacement operation. For example, this operation includes adding a suitable dispersion medium to microcapsule particles containing a non-reactive solvent or a dispersion liquid thereof, and replacing the non-reactive solvent inside the particles with the dispersion medium by stirring or the like, and then removing the excess non-reactive solvent and dispersion medium by a vacuum drying method, a centrifugation method, an ultrafiltration method, or the like. The solvent replacement operation may be performed only once or multiple times.

[0240] In the present invention, the hollow particles may be used as a dry powder by removing the solvent from a dispersion liquid of the hollow particles and drying the particles, if necessary. The method for drying the hollow particles is not particularly limited, but examples thereof include reduced pressure drying. EXAMPLES

[0241] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the following examples and comparative examples, "room temperature" means a temperature within the range of 20°C to 25°C.

[0242] (Average particle size and hollowness) The average particle size and hollow ratio of the hollow particles contained in the hollow particle aqueous dispersion were measured by the following method.

[0243] Specifically, the hollow particle aqueous dispersion obtained in the manufacturing example was dried for 3 hours in a vacuum dryer at 90°C (pressure 100 kPa or less) and then crushed with a spatula to obtain a dry powder. The obtained dry powder was sprinkled on a collodion film-attached mesh (manufactured by Nissin EM Co., Ltd.) and then stained with ruthenium tetroxide. Then, using a transmission electron microscope (TEM) (Hitachi High-Tech Corporation's "HT7800"), an accelerating voltage of 100 kV was used to select a portion where the hollow particles were uniformly dispersed at a magnification of 70,000 times, and a TEM photograph of the hollow particles was taken.

[0244] From the TEM photograph, 100 hollow particles that did not overlap were randomly selected. For each of the 100 selected hollow particles, the longest diameter and the shortest diameter were measured using the analysis software EMIP-EX, and the average value [(longest diameter + shortest diameter) / 2] was taken as the particle diameter of each hollow particle. The average value of the particle diameters of the 100 hollow particles was taken as the average particle diameter of the hollow particles contained in the hollow particle aqueous dispersion obtained in the production example.

[0245] In addition, for each of the 100 selected hollow particles, the inner diameter (the diameter of the hollow part of the hollow particle) was measured at five or more points passing through the center of the hollow particle, and the average inner diameter of the 100 hollow particles was taken as the average inner diameter of the hollow particles.

[0246] Furthermore, [(average inner diameter of hollow particles) 3 / (average particle size of hollow particles) 3 The hollow ratio (volume %) of the hollow particles contained in the aqueous dispersion of hollow particles obtained in the Production Examples was calculated from the formula: [% by volume]×100.

[0247] (Dispersed particle size) The dispersed particle diameter of the composite particles in the composite particle propylene glycol monomethyl ether dispersion was measured by the following method.

[0248] Specifically, the composite particle propylene glycol monomethyl ether dispersion obtained in the example was further diluted with propylene glycol monomethyl ether to prepare a composite particle propylene glycol monomethyl ether dispersion having a solid content of 0.1% by mass.

[0249] The Z-average particle size of the prepared composite particle propylene glycol monomethyl ether dispersion was measured under the following conditions using a particle size measuring device ("VASCO γ" manufactured by Cordouan Technologies). In the following examples and comparative examples, the Z-average particle size was taken as the dispersed particle size of the composite particles in the composite particle propylene glycol monomethyl ether dispersion. <Conditions for particle size measurement device> ·Measurement temperature: 25℃ ·Optical path length: 100μm Measurement time: 60 seconds Number of times: 3 Analysis method: Cumulant

[0250] (Shell Density) The shell density of the composite particles in the composite particle propylene glycol monomethyl ether dispersion was measured by the following method.

[0251] Specifically, 0.5 g of the composite particle propylene glycol monomethyl ether dispersion obtained in the example was precisely weighed and dried for 3 hours in a vacuum dryer at 90°C (pressure 100 kPa or less) to obtain a powder. The weight of the obtained powder was measured to obtain the solid content ratio x in the dispersion. p was calculated.

[0252] Next, the liquid density ρ of the composite particle propylene glycol monomethyl ether dispersion was measured at a measurement temperature of 23°C using a vibration type liquid density meter (DMA1001 manufactured by Anton Paar Japan Co., Ltd.). d and the liquid density ρ of propylene glycol monomethyl ether alone without composite particles s and were measured.

[0253] The shell density ρ of the composite particles in the composite particle propylene glycol monomethyl ether dispersion is calculated from the following formula: p was measured. ρ p =x p / {(1 / ρ d )-(1-x p ) / ρ s}

[0254] (Binder Hollow Ratio) The volume fraction of air in the composite particles contained in the binder (binder hollow fraction) was measured as follows.

[0255] Specifically, 0.2 g of the composite particle propylene glycol monomethyl ether dispersion obtained in the example, 0.98 g of pentaerythritol triacrylate ("NK Ester A-TMM-3LM-N" manufactured by Shin-Nakamura Chemical Co., Ltd., functional group number 3) as a binder, and 0.5 g of methanol as an organic solvent were accurately weighed into a glass bottle, and mixed uniformly using an ultrasonic cleaner to obtain a composite particle dispersion.

[0256] Next, the obtained composite particle dispersion liquid was dried in a vacuum dryer at 90° C. for 16 hours to completely remove the propylene glycol monomethyl ether and methanol contained in the system by volatilization, thereby obtaining a binder containing composite particles.

[0257] The obtained binder containing the composite particles was stored for 30 minutes in a constant temperature and humidity environment set at a room temperature of 23°C and a humidity of 55%, and then the refractive index of the binder and the refractive index of the shell of the composite particle contained in the binder (hereinafter referred to as the "refractive index of the shell of the composite particle") were measured using an Abbe refractometer (Atago's "NAR-1T SOLID"), and the refractive index of the binder was 1.485, and the refractive index of the shell of the composite particle was 1.537.

[0258] The refractive index of air is 1.00 and the density of air is 0 (g / cm 3 ), the refractive index of the shell of the composite particle is 1.537, and the density of the shell of the composite particle (g / cm 3 ), the refractive index of the binder is 1.485 and the density of the binder is 1.18 (g / cm 3 ), the volume fraction q of air in the composite particles contained in the binder (=binder hollowness) (volume %) was calculated by solving the following [Maxwell-Garnett equation]. Note that the above "shell density of composite particles" refers to the "shell density" of each example shown in Table 2 described later. [Maxwell-Garnett equation] (Na 2 -Nm 2 ) / (Na 2 +2Nm 2 )=q(Np 2 -Nm 2 ) / (Np2 +2Nm 2 )

[0259] (Production Example 1) Production of Hollow Particle Water Dispersion A In a 5 L stainless steel beaker, 3,600 parts by mass of ion-exchanged water, 1.6 parts by mass of an anionic surfactant (product name "Aqualon AR-1025" manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), 6.0 parts by mass of sodium p-styrenesulfonate, and 4.0 parts by mass of ammonium peroxodisulfate were added and dissolved.

[0260] A mixed solution of 168 parts by mass of glycidyl methacrylate, 32 parts by mass of 3-methacryloxypropyltriethoxysilane, 4.0 parts by mass of n-octyl mercaptan, and 200 parts by mass of toluene was further added to the stainless steel beaker, and the mixture was stirred at room temperature for 10 minutes using an ultrasonic homogenizer (manufactured by Branson, model SONIFIER 450) to prepare an emulsion.

[0261] The prepared emulsion was placed in a 5 L reactor equipped with a stirrer and a thermometer, and the inside was replaced with nitrogen to create a nitrogen atmosphere, after which the temperature was raised to 70° C. and polymerization reaction was carried out for 2 hours at 70° C. with stirring. Next, 100 parts by mass of ethylenediamine was added, the temperature was raised to 80° C. under a nitrogen atmosphere, and then the reaction was carried out for 16 hours at 80° C. with stirring to obtain a hollow particle dispersion.

[0262] 4,000 parts by mass of the obtained hollow particle dispersion was cross-flow washed with 20,000 parts by mass of ion-exchanged water using a ceramic filter having a pore size of 50 nm, and then appropriately concentrated and ion-exchanged water was added so that the solid content became 10% by mass, thereby obtaining a 10% by mass aqueous hollow particle dispersion A.

[0263] The average particle size of the hollow particles contained in the resulting 10% by mass aqueous dispersion A of hollow particles was 82 nm, and the hollowness was 45% by volume.

[0264] The blend compositions and physical properties of the production examples are shown in Table 1. [Table 1]

[0265] Example 1 To a 7-L stainless steel beaker, 15 parts by mass of a (per)fluoroalkyl group-containing phosphate ester ("Surflon FPE-50" manufactured by AGC Seimi Chemical Co., Ltd.) as a fluorine-containing compound and 45 parts by mass of a polyoxyethylene alkyl ether phosphate ("Phosphanol RS-710" manufactured by Toho Chemical Industry Co., Ltd.) as an anionic surfactant were added, and the mixture was dissolved with 2,000 parts by mass of isopropyl alcohol.

[0266] Further, 1000 parts by mass of the 10% by mass hollow particle aqueous dispersion A obtained in Production Example 1 was added, and the mixture was stirred at room temperature for 30 minutes using an ultrasonic homogenizer. Next, the mixture was cross-flow washed with 20,000 parts by mass of propylene glycol monomethyl ether using a ceramic filter having a pore size of 50 nm, and then appropriately concentrated and propylene glycol monomethyl ether was added so that the solid content became 10% by mass, thereby obtaining a 10% by mass composite particle propylene glycol monomethyl ether dispersion.

[0267] The obtained dispersion was dried and observed with a transmission electron microscope (TEM), revealing that spherical composite particles with intact hollows were obtained. The dispersed particle diameter of the composite particles in the obtained dispersion was 92 nm, and the shell density was 1.31 g / cm. 3 In addition, when a binder containing composite particles was produced using the obtained dispersion, the binder had a hollow ratio of 42 volume %.

[0268] Example 2 A 10% by mass dispersion of composite particles in propylene glycol monomethyl ether was obtained in the same manner as in Example 1, except that 30 parts by mass of Surflon FPE-50 and 30 parts by mass of Phosphanol RS-710 were used.

[0269] The obtained dispersion was dried and observed by TEM. It was found that the composite particles had a spherical shape with no collapsed hollows. The dispersed particle diameter of the composite particles in the obtained dispersion was 98 nm, and the shell density was 1.35 g / cm. 3 In addition, when a binder containing composite particles was produced using the obtained dispersion, the binder had a hollow ratio of 42 volume %.

[0270] Example 3 A 10% by mass dispersion of composite particles in propylene glycol monomethyl ether was obtained in the same manner as in Example 1, except that 45 parts by mass of Surflon FPE-50 and 15 parts by mass of Phosphanol RS-710 were used.

[0271] The obtained dispersion was dried and observed by TEM. It was found that the composite particles had a spherical shape with no collapsed hollows. The dispersed particle diameter of the composite particles in the obtained dispersion was 102 nm, and the shell density was 1.41 g / cm. 3 In addition, when a binder containing composite particles was produced using the obtained dispersion, the binder had a hollow ratio of 43 volume %.

[0272] The blend compositions and physical properties in the examples are shown in Table 2.

[0273] In Table 2, the average particle size means the average particle size of the hollow particles contained in the hollow particle aqueous dispersion obtained in the Production Example, and the hollow ratio means the hollow ratio of the hollow particles contained in the hollow particle aqueous dispersion obtained in the Production Example.

[0274] [Table 2]

[0275] As shown in Table 2, it was confirmed that the hollow ratio of the hollow particles measured by TEM and the hollow ratio of the binder were very close in numerical value in Examples 1 to 3. From this result, it is considered that there are almost no pinholes in the shells of the composite particles obtained in Examples 1 to 3, and the binder does not penetrate into the hollow parts.

Claims

1. The present invention relates to a method for producing a porous porous material comprising the steps of: The hollow particle has a shell and a hollow portion surrounded by the shell, The fluorine-containing compound is attached to the surface of the hollow particles. composite particles.

2. 2. The composite particle according to claim 1, wherein the fluorine-containing compound is at least one selected from the group consisting of (per)fluoroalkyl compounds, polyvinylidene fluoride, polytetrafluoroethylene, and ethylene-tetrafluoroethylene copolymers.

3. The composite particle according to claim 1 , wherein the shell contains a (meth)acrylic resin.

4. The composite particle according to claim 3 , wherein the (meth)acrylic resin comprises a polymer derived from a (meth)acrylic reactive monomer having an epoxy group and / or a polymer derived from a (meth)acrylic reactive monomer having an oxetane group.

5. 2. The composite particle according to claim 1, wherein the density of the shell is from 1.31 to 1.

45.

6. A dispersion comprising the composite particles according to any one of claims 1 to 5.

7. A coating agent comprising the composite particles according to any one of claims 1 to 5.

8. A heat insulating film comprising the composite particles according to any one of claims 1 to 5.

9. An anti-reflective coating comprising the composite particles according to any one of claims 1 to 5.

10. A light extraction film comprising the composite particles according to any one of claims 1 to 5.

11. A low dielectric constant film comprising the composite particle according to any one of claims 1 to 5.

12. A photosensitive resin composition comprising the composite particle according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Pressure-sensitive adhesive tape or sheet

    JP1995003222A

  • Composition for forming low refractive index membrane and substrate having cured membrane of the same

    JP2006291077A

  • Cosmetic

    JP2015124220A

  • Hollow particle and use therefor

    JP2021054941A

  • Hollow polymer fine particle and method for producing the same

    JP2002080503A