Two-pack type epoxy resin adhesive, and resin cured product

By using silica particles with epoxy groups in the curing agent, the adhesive addresses thixotropy and viscosity issues, providing a two-component epoxy resin with improved application characteristics and mechanical strength.

JP2024135943AInactive Publication Date: 2024-10-04KK TOSHIBA +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023046863
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing two-component epoxy resin adhesives face challenges in maintaining high thixotropy and initial viscosity after mixing, leading to potential dripping when applied on walls or ceilings due to gravity, necessitating improved properties for easier application and prevention of dripping.

Method used

Incorporation of silica particles with an average size of 1 μm to 10 μm, bonded with epoxy groups, into the curing agent to enhance thixotropy and initial viscosity, while minimizing aggregation, along with controlled ratios and dispersibility to maintain uniformity and mechanical strength.

Benefits of technology

The adhesive achieves high thixotropy and initial viscosity, preventing dripping and ensuring uniform distribution of silica particles in the cured resin, enhancing mechanical properties and application ease.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135943000001_ABST
    Figure 2024135943000001_ABST
Patent Text Reader

Abstract

To provide a two-pack type epoxy resin adhesive having high thixotropy.SOLUTION: A two-pack type epoxy resin adhesive includes: a first liquid containing an epoxy resin; and a second liquid containing an amine compound, and first silica particles which have an epoxy group coupled thereto and have average particle diameter of 1 μm or more and 10 μm or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] An embodiment of the present invention relates to a two-component epoxy resin adhesive and a cured resin. [Background technology]

[0002] Two-part epoxy resin adhesives, which consist of a liquid base agent containing epoxy resin and a liquid hardener containing an amine compound and are mixed with the base agent and hardener just before use, are widely used to bond components.

[0003] For example, when a two-part epoxy resin adhesive is used on the walls or ceilings of a structure, it is required that the adhesive be easy to apply after mixing the two parts and that it be prevented from dripping due to gravity after application. In order to make it easy to apply the adhesive after mixing the two parts and to prevent it from dripping due to gravity after application, it is desirable to increase the thixotropy of the adhesive after mixing the two parts and to increase the initial viscosity immediately after mixing. Thixotropy refers to the property of reversibly decreasing the viscosity of a high-viscosity fluid when force is applied to it. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 11-20063 Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a two-component epoxy resin adhesive having high thixotropy. [Means for solving the problem]

[0006] The two-component epoxy resin adhesive of the embodiment comprises a first liquid containing an epoxy resin, and a second liquid containing an amine compound and first silica particles having epoxy groups bonded thereto and an average particle size of 1 μm or more and 10 μm or less. [Brief description of the drawings]

[0007] [Figure 1] 1 is a schematic diagram of a two-component epoxy resin adhesive according to an embodiment. [Diagram 2] FIG. 2 is an explanatory diagram of a first silica particle according to the embodiment. [Diagram 3] FIG. 2 is a schematic cross-sectional view of a cured resin product according to an embodiment. [Figure 4] FIG. 2 is an explanatory diagram of the action and effect of the two-component epoxy resin adhesive of the embodiment. [Diagram 5] FIG. [Figure 6] FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The two-component epoxy resin adhesive of the embodiment comprises a first liquid containing an epoxy resin, and a second liquid containing an amine compound and silica particles having epoxy groups bonded thereto and an average particle size of 1 μm or more and 10 μm or less.

[0009] The cured resin product of the embodiment includes a resin and silica particles having an average particle size of 1 μm or more and 10 μm or less, and has a decomposition peak temperature of 402° C. or less in a thermogram obtained by thermal evolved gas mass spectrometry.

[0010] FIG. 1 is a schematic diagram of a two-component epoxy resin adhesive according to an embodiment.

[0011] The two-component epoxy resin adhesive 100 of the embodiment is composed of a base agent 10 and a curing agent 20. The base agent 10 is an example of a first liquid. The curing agent 20 is an example of a second liquid. The two-component epoxy resin adhesive 100 is a two-component adhesive that cures by mixing the base agent 10 and the curing agent 20.

[0012] The base agent 10 includes, for example, an epoxy resin 11 and second silica particles 12. The base agent 10 is liquid at 25°C.

[0013] The epoxy resin 11 is, for example, a bisphenol A type epoxy resin, a bisphenol F type epoxy resin, a bisphenol S type epoxy resin, a biphenyl type epoxy resin, a naphthalene type epoxy resin, or a novolac type epoxy resin.

[0014] The second silica particles 12 may be, for example, spherical, spheroidal, cylindrical, or irregular in shape, but are not particularly limited thereto. Fig. 1 illustrates the case where the shape of the second silica particles 12 is spherical.

[0015] The second silica particles 12 have an average particle size of, for example, 1 μm or more and 10 μm or less. The second silica particles 12 are contained in the base material 10 in an amount of, for example, 39% by weight or more and 79% by weight or less.

[0016] The material of the second silica grains 12 is, for example, fused silica or crystalline silica.

[0017] The base material 10 does not necessarily have to contain the second silica particles 12 .

[0018] The curing agent 20 includes an amine compound 21 and a first silica particle 22. The curing agent 20 is liquid at 25°C. The curing agent 20 includes, for example, a silane coupling agent. Since the amine compound 21 has a low viscosity at 25°C, an anti-settling agent for silica may be added. The curing agent 20 may be stirred immediately before mixing with the base agent 10.

[0019] The amine compound 21 is, for example, an aliphatic amine, an aromatic amine, or an imine. The amine compound 21 is, for example, poly(propylene glycol) diamine.

[0020] The first silica particles 22 may be, for example, spherical, spheroidal, cylindrical, or irregular in shape, but are not particularly limited thereto. Fig. 1 illustrates an example in which the shape of the first silica particles 22 is spherical.

[0021] The average particle size of the first silica particles 22 is, for example, 1 μm or more and 10 μm or less. The first silica particles 22 are contained in the hardener 20 in an amount of, for example, 14% by weight or more and 83% by weight or less.

[0022] The material of the first silica grains 22 is, for example, fused silica or crystalline silica.

[0023] When mixing the base agent 10 and the curing agent 20, for example, they are mixed in a ratio such that the epoxy equivalent of the base agent 10 is equal to the active hydrogen equivalent of the amine compound of the curing agent 20. The active hydrogen equivalent of the amine compound can be considered as the effective amine equivalent. By mixing them in the above ratio, the number of functional groups of the base agent 10 and the number of functional groups of the curing agent 20 become equal, improving the curing characteristics of the resin.

[0024] When considering a state in which the epoxy equivalent of the base agent 10 and the active hydrogen equivalent of the amine compound of the curing agent 20 are equal, the ratio of the first silica particles 22 contained in the curing agent 20 to the sum of the first silica particles 22 contained in the curing agent 20 and the second silica particles 12 contained in the base agent 10 is, for example, 5% by weight or more and 50% by weight or less. This range is preferable because it can provide sufficient thixotropy and an appropriately high viscosity of the curing agent.

[0025] In addition, when considering a state in which the epoxy equivalent of the base agent 10 and the active hydrogen equivalent of the amine compound in the liquid of the curing agent 20 are equal, the sum of the first silica particles 22 contained in the curing agent 20 and the second silica particles 12 contained in the base agent 10 is, for example, 130 parts by weight or more and 390 parts by weight or less, when the epoxy resin contained in the base agent 10 is 100 parts by weight. This range is preferable because it can provide sufficient thixotropy and appropriately increase the viscosity of the base agent and the curing agent.

[0026] FIG. 2 is an explanatory diagram of the first silica particle of the embodiment.

[0027] 2, an epoxy group is bonded to the first silica particle 22. The epoxy group is bonded to the first silica particle 22 by a silane coupling agent contained in the curing agent 20.

[0028] As a bonding method, silica particles and a silane coupling agent may be placed in a curing agent and allowed to react for, for example, half a day. This is a method called the integral method. Alternatively, silica particles whose surfaces have been previously coated with a silane coupling agent containing an epoxy group may be used. This is a method called the surface treatment method.

[0029] In addition, the second silica particles 12 contained in the base material 10 may also be bonded with epoxy groups as shown in Fig. 2. In this case, the epoxy groups are bonded to the second silica particles 12 by, for example, a silane coupling agent contained in the base material 10.

[0030] The average particle size of the second silica particles 12 and the first silica particles 22 can be determined, for example, from the measured long diameter of a plurality of silica particles in an image (SEM image) obtained by a scanning electron microscope (SEM).

[0031] Whether or not the base material 10 contains an epoxy resin can be determined by, for example, pyrolysis-gas chromatography / mass spectrometry.

[0032] Whether the curing agent 20 contains an amine compound can be determined by, for example, ion chromatography.

[0033] Moreover, whether or not an epoxy group is bonded to the second silica particles 12 or the first silica particles 22 by a silane coupling agent can be determined by, for example, pyrolysis gas chromatography mass spectrometry.

[0034] 3 is a schematic cross-sectional view of a cured resin material according to an embodiment. The cured resin material according to an embodiment is an epoxy resin cured material 200. The epoxy resin cured material 200 is a cured product of the two-component epoxy resin adhesive 100 according to an embodiment.

[0035] The cured epoxy resin material 200 contains an epoxy resin 31 and silica particles 32 .

[0036] The epoxy resin 31 is, for example, a bisphenol A type epoxy resin, a bisphenol F type epoxy resin, a bisphenol S type epoxy resin, a biphenyl type epoxy resin, a naphthalene type epoxy resin, or a novolac type epoxy resin.

[0037] The silica particles 32 are so-called fillers. The silica particles 32 are, for example, spherical, spheroidal, cylindrical, or irregular in shape, and are not particularly limited. Fig. 3 illustrates an example in which the silica particles 32 have a spherical shape.

[0038] The material of the silica grains 32 is, for example, fused silica or crystalline silica.

[0039] The silica particles 32 have an average particle size of 1 μm or more and 10 μm or less. The silica particles 32 are contained in the epoxy resin cured material 200 in an amount of, for example, 32 vol % or more and 60 vol % or less.

[0040] The volume ratio of the silica particles 32 in the epoxy resin cured material 200 is represented by the occupancy rate of the silica particles 32 in the cross section obtained by obtaining an SEM image of the cross section of the epoxy resin cured material 200. The occupancy rate of the silica particles 32 can be obtained by, for example, image analysis of the SEM image.

[0041] For example, the occupancy rate of the silica particles 32 is measured for seven regions, and the average value of the occupancy rates of five regions excluding the regions with the maximum and minimum occupancy rates is calculated. The calculated average value is regarded as the volume fraction of the silica particles 32 in the cured epoxy resin material 200.

[0042] The decomposition peak temperature of the thermogram obtained by analyzing the epoxy resin cured material 200 using evolved gas analysis mass spectrometry (EGA-MS) is 402° C. or lower. The EGA-MS method is a method in which a sample is heated and the gas generated is directly introduced into a mass spectrometer and measured.

[0043] For example, when a two-component epoxy resin adhesive is used on the wall or ceiling of a structure, it is required that the adhesive be easily applied after mixing the two components and that it is prevented from dripping due to gravity after application. In order to facilitate application of the adhesive after mixing the two components and to prevent dripping due to gravity after application, it is desirable to increase the thixotropy of the adhesive after mixing the two components and to increase the initial viscosity immediately after mixing.

[0044] For example, by including silica particles in the curing agent, it is possible to increase the thixotropy of the adhesive after mixing the two liquids. In particular, by reducing the particle size of the silica particles included, it is possible to increase the thixotropy of the adhesive after mixing the two liquids. For example, by including silica particles with an average particle size of less than 1 μm, it is possible to achieve high thixotropy.

[0045] However, if the average particle size of the silica particles contained in the curing agent is less than 1 μm, the curing agent before mixing tends to aggregate. Therefore, the curing agent before mixing becomes difficult to handle. In addition, if the curing agent before mixing aggregates, for example, the properties of the adhesive after curing become non-uniform.

[0046] In the curing agent 20 of the two-component epoxy resin adhesive 100 of the embodiment, epoxy groups are bonded to the first silica particles 22. By bonding the epoxy groups, even if the average particle size of the first silica particles 22 is as large as 1 μm or more, the adhesive after mixing of the two components can exhibit high thixotropy. In addition, since the average particle size of the first silica particles 22 is as large as 1 μm or more, aggregation of the curing agent 20 before mixing is less likely to occur.

[0047] Furthermore, the initial viscosity immediately after mixing can be increased by bonding epoxy groups to the first silica particles 22. It is more preferable that both the second silica particles 12 and the first silica particles 22 have epoxy groups, since this can increase the mechanical strength.

[0048] FIG. 4 is a diagram showing an example of a reaction that occurs in the second liquid contained in the two-liquid epoxy resin adhesive of the embodiment.

[0049] As shown in the upper diagram of Fig. 4, the first silica particles 22 contained in the curing agent 20 are bonded to epoxy groups by a silane coupling agent. Furthermore, it is considered that the epoxy groups of the first silica particles 22 contained in the curing agent 20 react with an amine compound, and the amine compound bonds to the epoxy groups, as shown in the lower diagram of Fig. 4. In other words, it is considered that the first silica particles 22 are bonded to the side chains of the amine compound.

[0050] In the curing agent 20 of the embodiment, the first silica particles 22 are bonded to the side chains of the amine compound, so that the apparent molecular weight of the amine compound is increased. Therefore, even if the first silica particles having an average particle size of 1 μm or more and 10 μm or less are used, the initial viscosity of the adhesive after mixing the base agent 10 and the curing agent 20 is high, and it is considered that high thixotropy is exhibited.

[0051] When the base agent 10 and the curing agent 20 are mixed, the epoxy resin of the base agent 10 and the amine compound 21 of the curing agent 20 bond to each other to form a crosslinked structure skeleton, and the adhesive is cured. In the two-component epoxy resin adhesive 100 of the embodiment, the first silica particles 22 are bonded to the side chains of the amine compound that forms the crosslinked structure skeleton. Therefore, the first silica particles 22 can be incorporated into the crosslinked structure skeleton.

[0052] By incorporating the first silica particles 22 into the crosslinked structure skeleton, for example, the dispersibility of the silica particles 32 contained in the epoxy resin cured material 200 formed by mixing the main agent 10 and the curing agent 20 can be improved. The silica particles contained as a filler are aggregated to some extent in a powder state before mixing to form secondary particles. When mixing this with the main epoxy resin, the secondary particles are crushed using a mixer or the like, but it is difficult to completely crush all the particles to primary particles. On the other hand, since the viscosity of the curing agent is lower than that of the main epoxy resin, it is easy to disperse the curing agent to primary particles even with a mixer. In the embodiment, the silica particles incorporated into the crosslinked structure increase, and the silica outside the crosslinked structure decreases, and the silica particles that have not been crushed to primary particles from secondary particles can be reduced. In other words, the silica not incorporated into the crosslinked structure skeleton decreases, and the silica particles 32 are distributed in a well-dispersed state in the epoxy resin cured material 200. Therefore, the properties of the epoxy resin cured material 200 are homogenized.

[0053] The average particle size of the first silica particles 22 contained in the curing agent 20 is preferably 1 μm or more and 10 μm or less, and more preferably 2 μm or more and 5 μm or less. When the average particle size of the first silica particles 22 is larger than the above lower limit, aggregation of the curing agent 20 is suppressed. When the average particle size of the first silica particles 22 is smaller than the above upper limit, the thixotropy of the adhesive after mixing the base agent 10 and the curing agent 20 is increased.

[0054] The first silica particles 22 are preferably contained in the hardener 20 at 14% by weight or more and 83% by weight or less. When the content is 14% by weight or more, the thixotropy of the adhesive after mixing the base agent 10 and the hardener 20 is further increased. When the content is 83% by weight or less, the viscosity of the hardener 20 does not become too high, and aggregation is suppressed.

[0055] The average particle size of the second silica particles 12 contained in the base agent 10 is preferably 1 μm or more and 10 μm or less, and more preferably 2 μm or more and 5 μm or less. When the average particle size of the second silica particles 12 is larger than the above lower limit, aggregation of the base agent 10 is suppressed. When the average particle size of the second silica particles 12 is smaller than the above upper limit, the thixotropy of the adhesive after mixing the base agent 10 and the curing agent 20 is increased.

[0056] The second silica particles 12 are preferably contained in the base agent 10 at 39% by weight or more and 79% by weight or less. By containing the second silica particles 12 at 39% by weight or more, the thixotropy of the adhesive after mixing the base agent 10 and the curing agent 20 is further increased. Furthermore, by containing the second silica particles 12 at 79% by weight or less, the viscosity of the base agent 10 does not become too high, and aggregation is suppressed.

[0057] Considering a state in which the epoxy equivalent of the base agent 10 and the active hydrogen equivalent of the amine compound of the curing agent 20 are equal, the ratio of the first silica particles 22 contained in the curing agent 20 to the sum of the first silica particles 22 contained in the curing agent 20 and the second silica particles 12 contained in the base agent 10 is preferably 5% by weight or more and 50% by weight or less. By being 5% by weight or more, the thixotropy of the adhesive after mixing the base agent 10 and the curing agent 20 is increased. Also, by being 50% by weight or less, the viscosity of the curing agent 20 does not become too high, and aggregation is suppressed.

[0058] When considering a state in which the epoxy equivalent of the base agent 10 and the active hydrogen equivalent of the amine compound of the curing agent 20 are equal, the sum of the first silica particles 22 contained in the curing agent 20 and the second silica particles 12 contained in the base agent 10 is preferably 130 parts by weight or more and 390 parts by weight or less, when the epoxy resin contained in the base agent 10 is 100 parts by weight. By being 130 parts by weight or more, the ratio of the filler in the formed epoxy resin cured product is increased, and the properties of the epoxy resin cured product are improved. By being 390 parts by weight or less, the viscosity of the adhesive after mixing the base agent 10 and the curing agent 20 is prevented from becoming too high.

[0059] The epoxy resin contained in the base agent 10 preferably has a relatively high viscosity in order to increase the viscosity after mixing the base agent 10 with the curing agent 20. For example, the epoxy resin contained in the base agent 10 is preferably a bisphenol A type epoxy resin.

[0060] The epoxy resin cured material 200 of the embodiment contains silica particles 32 having an average particle size of 1 μm or more and 10 μm or less. By containing the silica particles 32 as a filler, the epoxy resin cured material 200 is improved in, for example, mechanical strength and insulating properties.

[0061] The epoxy resin cured material 200 has a decomposition peak temperature of 402° C. or lower in a thermogram obtained by analysis using thermal evolved gas mass spectrometry.

[0062] It is believed that the density of the crosslinking points of the crosslinking structure skeleton is reduced by the incorporation of silica particles, which have a larger particle size than one molecule of the main epoxy resin 11 or the curing agent amine compound 21 in the epoxy resin cured material 200, into the crosslinking structure skeleton. The reason why the decomposition peak temperature of the thermogram becomes low at 402°C or less is believed to be due to the reduced density of the crosslinking points of the crosslinking structure skeleton.

[0063] In other words, since the epoxy resin cured material 200 has a decomposition peak temperature of 402°C or less in the thermogram, the number of silica particles outside the crosslinked structure skeleton in the epoxy resin cured material 200 is reduced, the risk of silica particles agglomerating is reduced, and dispersibility is improved.

[0064] From the viewpoint of further improving the dispersibility of the silica particles in the cured epoxy resin material 200, the decomposition peak temperature of the thermogram obtained by analysis using thermal evolved gas mass spectrometry is preferably 401°C or lower, and more preferably 400°C or lower.

[0065] The average particle size of the silica particles 32 contained in the epoxy resin cured material 200 is preferably 1 μm or more and 10 μm or less, and more preferably 2 μm or more and 5 μm or less. When the average particle size of the silica particles 32 is within the above range, the properties of the epoxy resin cured material 200 are improved.

[0066] As described above, according to the embodiment, it is possible to provide a two-component epoxy resin adhesive having high thixotropy and high initial viscosity. It is also possible to provide a two-component epoxy resin adhesive in which aggregation of the curing agent is suppressed. It is also possible to provide a resin cured product having excellent mechanical properties in which silica particles are well dispersed.

[0067] Examples will now be described. EXAMPLES

[0068] Example 1 The base material was prepared by mixing 286 parts by weight of epoxy-treated silica particles with an average particle size of 2 μm with 100 parts by weight of bisphenol A type epoxy resin. The epoxy-treated silica particles are silica particles to which epoxy groups are bonded by a silane coupling agent. The hardener was prepared by mixing 52 parts by weight of epoxy-treated silica particles with an average particle size of 2 μm with 40 parts by weight of poly(propylene glycol) diamine.

[0069] The base agent and hardener were mixed in a ratio where the epoxy equivalent of the bisphenol A epoxy resin was equal to the active hydrogen equivalent of the poly(propylene glycol) diamine. The hardener was stirred in a planetary centrifugal mixer just before weighing to prevent the silica particles from settling, and then the base agent and hardener were mixed and stirred in a planetary centrifugal mixer to produce an adhesive. The adhesive was then cured. The object was created.

[0070] Example 2 The base material was prepared by mixing 286 parts by weight of silica particles with an average particle size of 2 μm with 100 parts by weight of bisphenol A type epoxy resin. The hardener was prepared by mixing 52 parts by weight of epoxy-treated silica particles with an average particle size of 2 μm with 40 parts by weight of poly(propylene glycol) diamine. The silica particles in the base material are silica particles to which no epoxy groups are bonded.

[0071] The base agent and curing agent were mixed in a ratio where the epoxy equivalent of the bisphenol A epoxy resin was equal to the active hydrogen equivalent of the poly(propylene glycol) diamine. The curing agent was stirred with a planetary centrifugal mixer just before weighing to prevent the silica particles from settling, and then the base agent and curing agent were mixed and stirred with a planetary centrifugal mixer to create the adhesive.

[0072] Comparative Example 1 A base resin was prepared by mixing 100 parts by weight of bisphenol A type epoxy resin with 338 parts by weight of epoxy-treated silica having an average particle size of 2 μm. 40 parts by weight of poly(propylene glycol)diamine was prepared as a curing agent.

[0073] The base agent and hardener were mixed in a ratio where the epoxy equivalent of the bisphenol A epoxy resin and the active hydrogen equivalent of the poly(propylene glycol) diamine were equal. The base agent and hardener were mixed and stirred using a planetary centrifugal mixer to create an adhesive. The adhesive was then cured to create a cured product.

[0074] Comparative Example 2 100 parts by weight of bisphenol A type epoxy resin was prepared as the base material, and 40 parts by weight of poly(propylene glycol)diamine was prepared as the hardener. The base material and hardener were mixed to produce a hardened material.

[0075] Comparative Example 3 The base resin was prepared by mixing 286 parts by weight of silica particles with an average particle size of 2 μm and 1 part by weight of a silane coupling agent containing an epoxy group with 100 parts by weight of bisphenol A type epoxy resin. The hardener was prepared by mixing 52 parts by weight of silica particles with an average particle size of 2 μm with 40 parts by weight of poly(propylene glycol) diamine. The silica particles in the hardener are silica particles to which no epoxy groups are bonded.

[0076] The base agent and curing agent were mixed in a ratio where the epoxy equivalent of the bisphenol A epoxy resin was equal to the active hydrogen equivalent of the poly(propylene glycol) diamine. The curing agent was stirred with a planetary centrifugal mixer just before weighing to prevent the silica particles from settling, and then the base agent and curing agent were mixed and stirred with a planetary centrifugal mixer to create the adhesive.

[0077] Comparative Example 4 The base resin was prepared by mixing 100 parts by weight of bisphenol A type epoxy resin with 338 parts by weight of silica particles having an average particle size of 2 μm and 1 part by weight of a silane coupling agent containing an epoxy group. 40 parts by weight of poly(propylene glycol)diamine was prepared as a curing agent.

[0078] Comparative Example 5 The base resin was prepared by mixing 286 parts by weight of epoxy-treated silica particles with an average particle size of 2 μm with 100 parts by weight of bisphenol A type epoxy resin. The hardener was prepared by mixing 52 parts by weight of silica particles with an average particle size of 2 μm with 40 parts by weight of poly(propylene glycol) diamine. The silica particles in the hardener are silica particles to which no epoxy groups are bonded.

[0079] The base agent and curing agent were mixed in a ratio where the epoxy equivalent of the bisphenol A epoxy resin was equal to the active hydrogen equivalent of the poly(propylene glycol) diamine. The curing agent was stirred with a planetary centrifugal mixer just before weighing to prevent the silica particles from settling, and then the base agent and curing agent were mixed and stirred with a planetary centrifugal mixer to create the adhesive.

[0080] The base agent and hardener were mixed in a ratio where the epoxy equivalent of the bisphenol A epoxy resin and the active hydrogen equivalent of the poly(propylene glycol) diamine were equal. The base agent and hardener were mixed and stirred using a planetary centrifugal mixer to create an adhesive.

[0081] The initial viscosity immediately after mixing the two liquids was 48.0 (Pa s) for Example 1, 48.5 (Pa s) for Example 2, and 4.7 (Pa s) for Comparative Example 1. The reason that the inclusion of epoxy-treated silica in the curing agent increases the initial viscosity is thought to be that in the case of Comparative Example 1, where epoxy-treated silica was only in the base agent, the amine compound does not bond to the silica particles immediately after mixing the two liquids and exists as a single molecule, so that it has higher fluidity and does not increase in viscosity compared to when it is bonded to silica particles.

[0082] When epoxy-treated silica is included in the hardener, the amine compound and epoxy-treated silica bond in the hardener before the two liquids are mixed, increasing the apparent molecular weight. This causes the fluidity of the hardener to decrease immediately after the two liquids are mixed, which increases the initial viscosity.

[0083] The initial viscosity immediately after mixing the two liquids was 9.4 (Pa·s) for Comparative Example 3 and 5.3 (Pa·s) for Comparative Example 4.

[0084] In Comparative Example 3, although the curing agent contains silica particles, the epoxy group is not bonded to the amine compound, so there is no significant increase in initial viscosity as in the Examples, and the initial viscosity is low. Adhesives with low initial viscosity tend to drip.

[0085] The initial viscosity immediately after mixing the two components was 8.9 (Pa s) in Comparative Example 5. In Comparative Example 5, although the base resin contains epoxy-treated silica, the hardener does not contain epoxy-group-treated silica, so there was no increase in initial viscosity like in the Examples. Adhesives with low initial viscosity tend to drip.

[0086] 5 is a diagram showing the measurement results of the examples. The shear rate dependency of the viscosity of the adhesive of Example 1 and the adhesive of Comparative Example 1 was measured by a rheometer. The measurement results are shown in FIG.

[0087] As shown in Figure 5, the viscosity of the adhesive of Example 1 decreases with increasing shear rate. The adhesive of Example 1 exhibited a tendency to shear thinning. In other words, the adhesive of the example had high thixotropy. Materials that have a tendency to shear thinning tend not to drip and are easy to apply, especially when applied to walls and ceilings.

[0088] The adhesive of Example 1 had a viscosity of 2444 (Pa s) at a shear rate of 0.01 (1 / s), and a viscosity of 392 (Pa s) at a shear rate of 0.1 (1 / s). The thixotropic index, which can be calculated by dividing the viscosity at a shear rate of 0.01 (1 / s) by the viscosity at a shear rate of 0.1 (1 / s), was 6.2.

[0089] On the other hand, as shown in Figure 5, the viscosity of the adhesive of Comparative Example 1 increases with increasing shear rate. The adhesive of Comparative Example 1 exhibited a tendency to shear thickening. In other words, the adhesive of Comparative Example 1 had low thixotropy. Materials that have a tendency to shear thickening and low viscosity at low shear rates tend to drip and are not suitable for application to walls and ceilings in particular.

[0090] The adhesive of Comparative Example 1 had a viscosity of 12 (Pa s) at a shear rate of 0.01 (1 / s), and a viscosity of 11 (Pa s) at a shear rate of 0.1 (1 / s).The thixotropic index, which can be calculated by dividing the viscosity at a shear rate of 0.01 (1 / s) by the viscosity at a shear rate of 0.1 (1 / s), was 1.2.

[0091] In addition, in the adhesive of Example 2, similar to the adhesive of Example 1, high thixotropy was obtained.

[0092] Fig. 6 is a diagram showing the measurement results of the examples. Measurement was carried out by thermal evolved gas mass spectrometry for the cured products of Example 1, Comparative Example 1, and Comparative Example 2. Fig. 6 shows the thermograms obtained by the measurements.

[0093] As shown in Fig. 6, the peak decomposition temperature of the cured product of Example 1 was 400°C. The peak decomposition temperature of the cured product of Comparative Example 1 was 402°C. The peak decomposition temperature of the cured product of Comparative Example 2 was 406°C.

[0094] The reason why the decomposition peak temperatures of the cured products of Example 1 and Comparative Example 1 were lower than those of the cured product of Comparative Example 2 which did not contain silica particles is believed to be that the epoxy-treated silica particles with large particle size entered the crosslinked structure skeleton consisting of the bisphenol A type epoxy resin and the amine compound, decreasing the crosslinking point density and decreasing the decomposition peak temperature.

[0095] In the sample of Example 1, the decomposition peak temperature is further decreased compared to Comparative Example 1, which suggests that the amount of silica incorporated in the crosslinked structure skeleton is increased.

[0096] Although some embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. For example, components of one embodiment may be replaced or changed with components of another embodiment. These embodiments and their modifications are included in the scope and spirit of the invention, and are included in the scope of the invention and its equivalents described in the claims.

[0097] The technical solution of the present invention is described below.

[0098] (Technical proposal 1) a first liquid containing an epoxy resin; a second liquid containing an amine compound and first silica particles having an epoxy group bonded thereto and an average particle size of 1 μm or more and 10 μm or less; A two-component epoxy resin adhesive comprising:

[0099] (Technical proposal 2) A two-component epoxy resin adhesive as described in Technical Proposal 1, wherein the second liquid further contains a silane coupling agent, and the epoxy groups are bonded to the first silica particles by the silane coupling agent.

[0100] (Technical proposal 3) A two-component epoxy resin adhesive according to Technical Scheme 1 or 2, wherein the first liquid further contains second silica particles having an average particle size of 1 μm or more and 10 μm or less.

[0101] (Technical proposal 4) A two-component epoxy resin adhesive according to Technical Proposal 3, wherein epoxy groups are bonded to the second silica particles by a silane coupling agent.

[0102] (Technical proposal 5) A two-component epoxy resin adhesive described in any one of Technical Schemes 1 to 3, wherein the first silica particles are contained in the second liquid at a concentration of 14% by weight or more and 83% by weight or less.

[0103] (Technical proposal 6) A two-component epoxy resin adhesive according to Technical Proposal 3, wherein the second silica particles are contained in the first liquid at a concentration of 39% by weight or more and 79% by weight or less.

[0104] (Technical proposal 7) When considering a state in which the epoxy resin equivalent of the first liquid is equal to the active hydrogen equivalent of the amine compound of the second liquid, A two-component epoxy resin adhesive according to Technical Proposal 3, wherein the ratio of the first silica particles contained in the second liquid to the sum of the first silica particles contained in the second liquid and the second silica particles contained in the first liquid is 5% by weight or more and 50% by weight or less.

[0105] (Technical proposal 8) When considering a state in which the epoxy resin equivalent of the first liquid is equal to the active hydrogen equivalent of the amine compound of the second liquid, A two-component epoxy resin adhesive according to Technical Proposal 3, wherein the sum of the first silica particles contained in the second liquid and the second silica particles contained in the first liquid is 130 parts by weight or more and 390 parts by weight or less, when the epoxy resin contained in the first liquid is 100 parts by weight.

[0106] (Technical proposal 9) Resin and Silica particles having an average particle size of 1 μm or more and 10 μm or less; Equipped with A cured resin, the decomposition peak temperature of which in a thermogram obtained by thermal evolved gas mass spectrometry is 402°C or lower.

[0107] (Technical proposal 10) The resin cured product according to Technical Proposal 9, wherein the resin comprises an epoxy resin.

[0108] (Technical proposal 11) The cured resin material according to Technical Scheme 9 or 10, comprising 32 volume % or more and 60 volume % or less of the silica particles. [Explanation of symbols]

[0109] 10 Base agent (first liquid) 11 Epoxy Resin 12 Secondary silica particles 20 Hardener (second liquid) 21 Amine compounds 22 First Silica Particles 100 Two-component epoxy resin adhesive 200 Epoxy resin hardened material (hardened resin material)

Claims

1. a first liquid containing an epoxy resin; a second liquid containing an amine compound and first silica particles having an epoxy group bonded thereto and an average particle size of 1 μm or more and 10 μm or less; A two-component epoxy resin adhesive comprising:

2. The two-part epoxy resin adhesive according to claim 1 , wherein the second liquid further contains a silane coupling agent, and the epoxy groups are bonded to the first silica particles by the silane coupling agent.

3. The two-component epoxy resin adhesive according to claim 1 , wherein the first liquid further contains second silica particles having an average particle size of 1 μm or more and 10 μm or less.

4. The two-component epoxy resin adhesive according to claim 3 , wherein epoxy groups are bonded to the second silica particles by a silane coupling agent.

5. 2. The two-component epoxy resin adhesive according to claim 1, wherein the first silica particles are contained in the second liquid in an amount of 14% by weight or more and 83% by weight or less.

6. 4. The two-component epoxy resin adhesive according to claim 3, wherein the second silica particles are contained in the first liquid in an amount of 39% by weight or more and 79% by weight or less.

7. When considering a state in which the epoxy resin equivalent of the first liquid is equal to the active hydrogen equivalent of the amine compound of the second liquid, 4. The two-component epoxy resin adhesive according to claim 3, wherein a ratio of the first silica particles contained in the second liquid to a sum of the first silica particles contained in the second liquid and the second silica particles contained in the first liquid is 5% by weight or more and 50% by weight or less.

8. When considering a state in which the epoxy resin equivalent of the first liquid is equal to the active hydrogen equivalent of the amine compound of the second liquid, 4. The two-component epoxy resin adhesive according to claim 3, wherein a sum of the first silica particles contained in the second liquid and the second silica particles contained in the first liquid is 130 parts by weight or more and 390 parts by weight or less, when the epoxy resin contained in the first liquid is 100 parts by weight.

9. Resin and Silica particles having an average particle size of 1 μm or more and 10 μm or less; Equipped with A cured resin, having a decomposition peak temperature of 402°C or lower in a thermogram obtained by thermal evolved gas mass spectrometry.

10. The cured resin product according to claim 9 , wherein the resin comprises an epoxy resin.

11. The cured resin according to claim 9 , comprising 32 volume % or more and 60 volume % or less of the silica particles.

Citation Information

Patent Citations

  • Double fluid type epoxy resin adhesive, and repairing and reinforcing method of concrete construction employing the same

    JP1999020063A