Resin composition, wafer protective film, wafer protective member and method for removing wafer protective film
A resin composition with shellac and alcohol-soluble resins forms a water-resistant and easily removable wafer protective film, addressing foreign matter adhesion and water ingress issues in semiconductor manufacturing, ensuring reliable bonding and efficient processing.
Patent Information
- Application Number
- JP2023046935
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
AI Technical Summary
In semiconductor manufacturing processes, the presence of minute foreign matter on bonding surfaces can cause poor bonding, and existing protective materials fail to provide adequate water resistance and ease of removal, leading to issues during cooling and cleaning steps.
A resin composition comprising shellac resin and an alcohol-soluble resin, such as polyoxazoline or polyvinyl butyral, is used to form a wafer protective film that is water-resistant and soluble in cleaning liquids, allowing easy removal with organic solvents.
The film effectively prevents water ingress and foreign matter adhesion, ensuring reliable bonding by maintaining integrity during processing and facilitating easy post-processing removal, enhancing manufacturing efficiency.
Smart Images

Figure 2024135994000001 
Figure 2024135994000002 
Figure 2024135994000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a resin composition, a wafer protective film, a wafer protective member, and a method for removing the wafer protective film. [Background technology]
[0002] In the semiconductor manufacturing process, methods for electrically bonding a semiconductor chip and a semiconductor wafer include wire bonding and bump bonding. In recent years, direct electrical bonding (hybrid bonding) between a semiconductor chip and a semiconductor wafer without using bumps or the like has been considered for the purposes of high integration of chips, three-dimensional mounting, improving transmission speed, and improving transmission capacity.
[0003] When a semiconductor chip and a semiconductor wafer are electrically and directly bonded to each other, there is a problem that the presence of minute foreign matter (e.g., foreign matter on the submicron order) on the bonding surface is likely to cause bonding defects. Therefore, from the viewpoint of suppressing adhesion of foreign matter to the bonding surface during manufacturing processes for manufacturing semiconductor chips from a semiconductor wafer, such as a back-grinding process and a dicing process of the semiconductor wafer, it is desirable to protect the wiring surface of the semiconductor wafer to be diced with a protective material.
[0004] For example, a method for manufacturing semiconductor chips has been proposed, which includes a step of laminating a surface protection tape with a mask integrated therewith, the surface protection tape having a mask material layer provided on the surface protection tape, to a pattern surface of a semiconductor wafer, grinding the back surface of the semiconductor wafer, peeling off the surface protection tape and then dicing the semiconductor chips into individual pieces by plasma dicing, and removing the mask material layer with a remover (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2019-087682 A Summary of the Invention [Problem to be solved by the invention]
[0006] In semiconductor manufacturing processes such as the backgrinding process of semiconductor wafers, water is used for cooling, cleaning, etc., but it is necessary to prevent water from entering the wiring surface. Therefore, protective materials for semiconductor wafers are required to be water-resistant (water-resistant).
[0007] Furthermore, in order to prevent foreign matter from adhering, protective materials for semiconductor wafers are required to protect the bonding surfaces of the semiconductor chips obtained by dicing the semiconductor wafer into individual chips until immediately before bonding, and to be easily removed with a cleaning liquid such as an organic solvent immediately before bonding.
[0008] The present disclosure has been made in consideration of the above, and aims to provide a resin composition capable of forming a wafer protective film that has excellent water resistance and solubility in cleaning fluids, a wafer protective film that has excellent water resistance and solubility in cleaning fluids, and a wafer protective member and a method for removing the wafer protective film using this film. [Means for solving the problem]
[0009] Means for solving the above problems include the following aspects. <1> Shellac resin, An organic solvent; A resin composition for protecting a wafer comprising the above compound. <2> Further includes an alcohol-soluble resin <1> The resin composition according to claim 1. <3> The content of the alcohol-soluble resin is 5% by mass to 40% by mass based on the total amount of the shellac resin. <2> The resin composition according to claim 1. <4> The alcohol-soluble resin contains at least one of polyoxazoline and polyvinyl butyral. <3> The resin composition according to claim 1. <5> <1> ~ <4> 2. A wafer protective film formed from the resin composition according to claim 1. <6> A substrate; The substrate is formed <5> The wafer protective film according to claim 1, A wafer protection member comprising: <7> <5> Protecting a wafer using the wafer protective film according to claim 1; removing the wafer protective film from the wafer or from chips obtained by dicing the wafer; A method for removing a wafer protective film comprising the steps of: Effect of the Invention
[0010] According to the present disclosure, it is possible to provide a resin composition capable of forming a wafer protective film having excellent water resistance and solubility in cleaning fluids, a wafer protective film having excellent water resistance and solubility in cleaning fluids, and a wafer protective member and a method for removing the wafer protective film using this film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] In the present disclosure, a numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the lower and upper limits. In this disclosure, the term "step" refers not only to an independent step, but also to a step that is clearly connected to other steps. Even if they are indistinguishable, they are included in this term as long as the intended purpose of the process is achieved. In the present disclosure, when a plurality of substances corresponding to each component are present in the composition, the amount of each component contained in the composition means the total amount of the plurality of substances present in the composition, unless otherwise specified. In the numerical ranges described in the present disclosure in stages, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit value of the numerical range may be replaced with a value shown in the examples.
[0012] [Resin composition for wafer protection] The resin composition for protecting a wafer according to the present disclosure contains a shellac resin and an organic solvent. The wafer protective film formed using the resin composition of the present disclosure has excellent water resistance and excellent solubility in a cleaning solution. The excellent water resistance prevents the wafer protective film from dissolving in water, and the excellent solubility in a cleaning solution prevents the wafer protective film from leaving residue on the wafer after cleaning.
[0013] The excellent water resistance of the wafer protective film prevents the wafer protective film from dissolving in water (e.g., cooling water) during back grinding of the semiconductor wafer. Furthermore, the film is prevented from peeling off, preventing foreign matter in the cleaning water from adhering to the wiring surface of the wafer.
[0014] Because the wafer protective film has excellent solubility in cleaning liquid, for example, the bonding surface of the semiconductor chip obtained by dicing the semiconductor wafer can be protected by the wafer protective film until just before bonding of the semiconductor chips, and the film can be easily removed with a cleaning liquid such as an organic solvent just before bonding.
[0015] In the present disclosure, the cleaning liquid for the wafer protective film is not particularly limited as long as it is a liquid capable of dissolving the wafer protective film, and examples thereof include organic solvents such as alcohols and ketones; and basic aqueous solutions containing amines, ammonium salts, alkali metal hydroxides, etc. Examples of alcohols include ethanol, propanol, butanol, etc. The cleaning liquid may contain one kind of organic solvent, or may contain two or more kinds of organic solvents. The cleaning liquid may contain components other than the organic solvent.
[0016] The resin composition of the present disclosure is preferably used for forming a wafer protective film in a semiconductor manufacturing process. It may also be used for purposes other than forming a wafer protective film, such as purposes requiring water resistance and solubility in organic solvents.
[0017] (Shellac resin) The resin composition of the present disclosure includes a shellac resin.
[0018] Shellac resin is a resinous substance secreted by lac scale insects, which is purified by known methods such as solution extraction, soda method, and thermal fusion method, and the resin content includes natural shellac resins mainly composed of ester compounds with resin acids such as aleuritic acid, jaralic acid, and lacxijaralic acid, and synthetic shellac resins. The shellac resin may be purified shellac resin, bleached shellac resin, decolorized shellac resin, or modified shellac resin such as styrenated shellac and acrylated shellac.
[0019] The shellac resin may contain a structure formed by the reaction of the following structural unit (1), or may be a polymer formed by the reaction of a carboxy group and a hydroxy group in a plurality of structural units (1). R in the structural unit (1) represents a substituent.
[0020] [ka]
[0021] An example of the shellac resin is a polymer represented by the following general formula (2) (n is an integer of 0 or more): In the shellac resin, the reaction position between the carboxy group and the hydroxy group in the structural unit (1) is not limited to the position represented by general formula (2).
[0022] [ka]
[0023] The content of the shellac resin may be 60% by mass to 100% by mass, or 70% by mass to 100% by mass, based on the total amount of the resin components (excluding the organic solvent). When the resin composition contains a resin component other than the shellac resin, the content of the shellac resin may be 60% by mass to 90% by mass, or 70% by mass to 90% by mass, based on the total amount of the resin components (excluding the organic solvent).
[0024] (Organic solvent) The resin composition of the present disclosure contains an organic solvent. The organic solvent is preferably a solvent capable of dissolving the shellac resin, or a solvent capable of dissolving the shellac resin and an alcohol-soluble resin used as needed.
[0025] Examples of the organic solvent contained in the resin composition include organic solvents such as alcohols and ketones. Examples of the alcohols include ethanol, propanol, butanol, etc. Examples of the ketones include acetone, methyl ethyl ketone, methyl isobutyl ketone, etc. The organic solvent may be used alone or in combination of two or more kinds.
[0026] When the resin composition contains an alcohol-soluble resin described below, the resin composition preferably contains an alcohol as the organic solvent.
[0027] The content of the organic solvent is not particularly limited as long as the resin composition can be applied to a substrate or the like to form a film. For example, the concentration of the total resin components in the resin composition may be 10% by mass to 50% by mass, or 20% by mass to 40% by mass.
[0028] (Alcohol-soluble resin) The resin composition of the present disclosure preferably further contains an alcohol-soluble resin. By using shellac resin in combination with an alcohol-soluble resin, the solubility in a cleaning solution (particularly alcohol) is improved, and the cleaning time tends to be shortened.
[0029] The alcohol-soluble resin is not particularly limited as long as it is a resin soluble in alcohol, and examples thereof include polyamide, polyvinyl acetal, polyurethane, polyvinyl alcohol, polyvinylpyrrolidone, polyacrylic acid, polyethyleneimine, rosin, polyoxazoline, polyvinyl butyral, etc. Among them, polyoxazoline and polyvinyl butyral are preferred from the viewpoint of the balance of film-forming property, water resistance, and washability of the resin composition. The alcohol-soluble resin may be used alone or in combination of two or more kinds.
[0030] The content of the alcohol-soluble resin may be 5% by mass to 40% by mass, 10% by mass to 35% by mass, or 15% by mass to 30% by mass, based on the total amount of the shellac resin. When the content of the alcohol-soluble resin is 5% by mass or more, the solubility in a cleaning liquid tends to be improved, and when the content of the alcohol-soluble resin is 40% by mass or less, the water resistance tends to be excellent.
[0031] When the alcohol-soluble resin is polyoxazoline, the content of polyoxazoline may be 10% by mass to 40% by mass, 15% by mass to 35% by mass, or 20% by mass to 30% by mass, based on the total amount of the shellac resin.
[0032] When the alcohol-soluble resin is polyvinyl butyral, the content of polyvinyl butyral may be 5% by mass to 20% by mass, 10% by mass to 20% by mass, or 12% by mass to 18% by mass, based on the total amount of the shellac resin. When the polyvinyl butyral content is 20 mass % or less, the water resistance tends to be superior.
[0033] The content of resin components other than polyoxazoline and polyvinyl butyral may be 20% by mass or less, 10% by mass or less, or 0% by mass, based on the total amount of the shellac resin.
[0034] [Wafer protection film] The wafer protective film of the present disclosure is formed from the resin composition of the present disclosure. For example, the wafer protective film can be produced by applying the resin composition of the present disclosure to a substrate such as a separator to form a coating film, and drying the coating film as necessary to volatilize the organic solvent.
[0035] The thickness of the wafer protective film of the present disclosure may be appropriately changed depending on the application, and may be, for example, 1 μm to 50 μm, or 3 μm to 30 μm.
[0036] [Wafer protection materials] The wafer protection member of the present disclosure includes a substrate and the wafer protection film of the present disclosure formed on the substrate. The substrate may be a separator such as a polyethylene terephthalate substrate (PET substrate) that is peeled off when the wafer protection film is used, or may be a backgrind tape used when backgrinding a silicon wafer. The wafer protection member of the present disclosure may be, for example, a BGT integrated wafer protection member in which the backgrind tape (BGT) and the wafer protection film are integrated.
[0037] A BGT-integrated wafer protection member can be produced, for example, by laminating a wafer protection film formed on a separator and a backgrind tape (BGT), which is a base material having an adhesive layer.
[0038] [How to remove the protective film on the wafer] The method for removing a wafer protective film disclosed herein includes protecting a wafer (semiconductor wafer) using a wafer protective film, and removing the wafer protective film from the wafer or chips obtained by dicing the wafer.
[0039] In the removal method of the present disclosure, the wafer protective film that protects the semiconductor wafer has excellent water resistance, which prevents the wafer protective film from dissolving in water or peeling off from the semiconductor wafer during a semiconductor wafer processing step, such as a back-grinding step that uses cooling water.
[0040] Furthermore, the wafer protective film that protects the semiconductor wafer has excellent solubility in cleaning solutions such as organic solvents, etc. Therefore, after the semiconductor wafer processing step is completed, for example, immediately before bonding of the semiconductor chip after the dicing step is completed, the wafer protective film on the semiconductor chip can be easily removed, and the manufacturing efficiency of the semiconductor manufacturing device, etc. is excellent.
[0041] For example, when using a BGT-integrated wafer protection member equipped with a wafer protection film, the separator of the BGT-integrated wafer protection member is peeled off, and the exposed wafer protection film is attached to the wiring surface of the semiconductor wafer. Then, a backgrinding process and a dicing process (e.g., a dicing process such as plasma dicing, blade dicing, or laser dicing) are performed. After the backgrinding process and before the dicing process, the BGT is peeled off, and after the dicing process, the wafer protection film is removed with a cleaning solution such as an organic solvent just before bonding the semiconductor chips obtained by dividing the semiconductor wafer.
[0042] The method of removing the wafer protective film with a cleaning liquid such as an organic solvent is not particularly limited, and the wafer protective film may be removed by contacting the wafer protective film with the cleaning liquid using a cleaning method such as immersion, spin cleaning, spray (shower) cleaning, ultrasonic cleaning, etc. When the wafer protective film is removed by immersion, the immersion time may be adjusted taking into consideration the type of cleaning liquid, the thickness and material of the wafer protective film, etc. When the wafer protective film contains an alcohol-soluble resin, particularly when it contains at least one of polyoxazoline and polyvinyl butyral, the film is more efficiently removed and the immersion time tends to be shorter. EXAMPLES
[0043] Examples of the present disclosure will be described below, but the present disclosure is not limited to the following examples.
[0044] [Example 1] (Preparation of Resin Composition) A base resin, shellac resin (natural shellac resin), was dissolved in isopropanol to prepare a resin composition with a resin component concentration of 30 mass %.
[0045] (Formation of protective film) The prepared resin composition was applied to a polyethylene terephthalate substrate (PET substrate) using a bar coater, and the coating was dried at 85° C. Thus, a protective film was formed on the PET substrate. The PET substrate corresponds to the separator of the present disclosure, and the protective film corresponds to the wafer protective film of the present disclosure.
[0046] (Protective film treatment) As back grinding tape (BGT), ICROS tape manufactured by Mitsui Chemicals Tocello Co., Ltd. TM The PET substrate on which the protective film was formed was then laminated with the BGT at room temperature using a laminator. This produced a laminate in which the BGT, protective film, and PET substrate were arranged in this order. It was visually confirmed that there were no voids at the interface between the BGT and the protective film. The laminate corresponds to the wafer protection member of the present disclosure. Next, the PET substrate was peeled off to expose the protective film. The exposed protective film and the glass substrate were laminated using a laminator at 80° C. It was confirmed by an optical microscope that there were no voids at the interface between the protective film and the glass substrate. After lamination with the glass substrate, the BGT was peeled off by irradiating UV light from the BGT side using a metal halide lamp. At this time, the condition of the protective film was observed using an optical microscope to confirm that the protective film had not peeled off from the glass substrate. The glass substrate with the protective film obtained by peeling off the BGT was used to evaluate the water resistance and cleanability (the alcohol cleaning speed and alcohol cleaning rate described below) shown below.
[0047] (water resistance) The glass substrate with the protective film was immersed in pure water at room temperature for 30 minutes. After that, the glass substrate was taken out of the pure water, and the appearance of the glass substrate was confirmed with an optical microscope. The solubility of the protective film in water was evaluated based on the following evaluation criteria. If the evaluation was A, the dissolution of the protective film in water was suppressed, and it was determined that the water resistance was good. -Evaluation criteria- A: No defects were found in the protective film. B: Defects in the protective film, such as dissolution of the protective film or peeling of the protective film from the glass substrate, were confirmed. The results are shown in Table 1.
[0048] (Alcohol cleaning speed) The glass substrate with the protective film was immersed in alcohol (1-butanol) at room temperature for 10 minutes. After that, the glass substrate was removed from the alcohol, and the appearance of the glass substrate was observed using an optical microscope. The alcohol cleaning speed was evaluated based on the following evaluation criteria. If the evaluation was A, it was determined that the protective film could be cleaned in a relatively short time and that the alcohol cleaning speed was good. -Evaluation criteria- A: No residue of the protective film was found on the glass substrate. B: A small amount of residue was found on the glass substrate, but the glass substrate could still be used. C: Residue was observed to the extent that the glass substrate could not be used. The results are shown in Table 1.
[0049] (Alcohol cleaning rate) The glass substrate with the protective film was immersed in alcohol (1-butanol) at room temperature for 30 minutes. Thereafter, the glass substrate was removed from the alcohol, and the appearance of the glass substrate was observed using an optical microscope. The alcohol cleaning rate was evaluated based on the following evaluation criteria. If the evaluation was A, it was determined that the protective film could be cleaned and the alcohol cleaning rate was good. Furthermore, if the evaluation was B for (alcohol cleaning speed) but A for (alcohol cleaning rate), it was evaluated that although it was difficult to clean the protective film in a relatively short time, the alcohol cleaning rate was high. -Evaluation criteria- A: No residue of the protective film was found on the glass substrate. B: A small amount of residue was found on the glass substrate, but the glass substrate could still be used. C: Residue was observed to the extent that the glass substrate could not be used. The results are shown in Table 1.
[0050] [Example 2] A resin composition with a resin component concentration of 30% by mass was prepared by dissolving 24 parts by mass of a base resin, shellac resin (purified shellac resin, manufactured by Gifu Shellac Manufacturing Co., Ltd.), and 6 parts by mass of poly(2-ethyl-2-oxazoline) (PEOX, manufactured by Sigma-Aldrich Corporation, weight average molecular weight: approximately 50,000) in isopropanol.
[0051] [Example 3] A resin composition with a resin component concentration of 30% by mass was prepared by dissolving 24 parts by mass of a base resin, shellac resin (purified shellac resin, manufactured by Gifu Shellac Manufacturing Co., Ltd.), and 6 parts by mass of poly(2-ethyl-2-oxazoline) (PEOX, manufactured by Sigma-Aldrich, weight average molecular weight: approximately 500,000) in isopropanol.
[0052] [Example 4] A resin composition with a resin component concentration of 28% by mass was prepared by dissolving 24 parts by mass of a base resin, shellac resin (purified shellac resin, manufactured by Gifu Shellac Manufacturing Co., Ltd.), and 4 parts by mass of polyvinyl butyral (product name: Mowital B45H, manufactured by Kuraray Co., Ltd.) in isopropanol.
[0053] [Comparative Example 1] A base resin, polyvinyl alcohol (PVA, product name: Kuraray Poval 5-74, manufactured by Kuraray Co., Ltd.), was dissolved in isopropanol to prepare a resin composition with a resin component concentration of 20 mass %.
[0054] [Comparative Example 2] A base resin, polyvinylpyrrolidone (PVP, product name: PVP K-30, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), was dissolved in isopropanol to prepare a resin composition with a resin component concentration of 30 mass %.
[0055] [Comparative Example 3] A base resin, polyvinylpyrrolidone (PVP, product name: PVP K-90, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), was dissolved in isopropanol to prepare a resin composition with a resin component concentration of 20 mass %.
[0056] [Comparative Examples 4 and 5] The base resin, poly(2-ethyl-2-oxazoline) (PEOX, manufactured by Sigma-Aldrich Corporation, weight average molecular weight: approximately 50,000) or poly(2-ethyl-2-oxazoline) (PEOX, manufactured by Sigma-Aldrich Corporation, weight average molecular weight: approximately 500,000), was dissolved in isopropanol to prepare a resin composition with a resin component concentration of 30 mass%.
[0057] [Comparative Example 6] A base resin, polyvinyl butyral (product name: Mowital B45H, manufactured by Kuraray Co., Ltd.), was dissolved in isopropanol to prepare a resin composition with a resin component concentration of 20 mass %.
[0058] For each of the Examples and Comparative Examples, the alcohol cleaning speed, alcohol cleaning rate, and water resistance were evaluated in the same manner as in Example 1. The results are shown in Tables 1 and 2.
[0059] [Table 1]
[0060] [Table 2]
[0061] As shown in Tables 1 and 2, in Examples 1 to 4, both the alcohol cleansing rate and the water resistance were evaluated as being good. On the other hand, in Comparative Examples 1 to 6, at least one of the alcohol cleaning rate and water resistance was evaluated as poor. In Examples 2 to 4, the alcohol cleaning rate was improved by adding an alcohol-soluble resin as an additive.
Claims
1. Shellac resin, An organic solvent; A resin composition for protecting a wafer comprising the above compound.
2. The resin composition according to claim 1 , further comprising an alcohol-soluble resin.
3. The resin composition according to claim 2, wherein the content of the alcohol-soluble resin is 5% by mass to 40% by mass based on the total amount of the shellac resin.
4. The resin composition according to claim 3 , wherein the alcohol-soluble resin comprises at least one of polyoxazoline and polyvinyl butyral.
5. A wafer protective film formed from the resin composition according to any one of claims 1 to 4.
6. A substrate; The wafer protective film according to claim 5 formed on the substrate; A wafer protection member comprising:
7. Protecting a wafer using the wafer protective film according to claim 5; removing the wafer protective film from the wafer or from chips obtained by dicing the wafer; A method for removing a wafer protective film comprising the steps of:
Citation Information
Patent Citations
Method and apparatus for forming reference surface of wafer
JP2007134371A
Easily-adhesive agent composition, multilayer polyester resin film, and solar cell back sheet
JP2014136730A
Adhesive for temporary adhesion and part production method
JP2019019331A
Adhesive for temporary stopping water system, manufacturing method of adhesive for temporary stopping water system, and manufacturing method of various members or components using the adhesive for temporary stopping water system
JP2019163485A
Backside protective sheet for solar cell module, backside protective sheet roll body, and solar cell module