Cement admixture

A cement admixture with calcium silicate and Al2O3 fixes carbon dioxide, addressing the environmental impact of cement production by reducing emissions and enhancing cement properties.

JP2024136385APending Publication Date: 2024-10-04TAIHEIYO CEMENT CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023047491
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing cement production methods contribute significantly to carbon dioxide emissions, and there is a need for a more sustainable approach that utilizes waste materials effectively while maintaining cement strength and fluidity.

Method used

A cement admixture containing pulverized carbonated cement clinker, composed of calcium silicate and Al2O3, is used to fix carbon dioxide, reducing emissions and enhancing the properties of mixed cement.

Benefits of technology

The admixture effectively reduces carbon dioxide emissions during cement production, promotes the use of waste as a raw material, and maintains or improves the strength and fluidity of mixed cement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024136385000001
    Figure 2024136385000001
  • Figure 2024136385000002
    Figure 2024136385000002
  • Figure 2024136385000003
    Figure 2024136385000003
Patent Text Reader

Abstract

To provide a cement admixture capable of reducing carbon intensity of mixed cement including the admixture when used as an admixture since cement clinker is used as a raw material and carbon dioxide has been fixated.SOLUTION: A cement admixture includes a pulverized product of carbonated cement clinker obtained by carbonating cement clinker including calcium silicate and Al2O3-containing mineral phase as a mineral composition. The cement clinker is a burned material, which preferably contains belite as the calcium silicate and gehlenite as the Al2O3-containing mineral phase and satisfies the following conditions (1) and (2): (1) the amount of the gehlenite relative to 100 pts.mass of the belite is 10-100 pts.mass; and (2) the cement clinker includes no aluminate phase, or 15 pts.mass or less relative to 100 pts.mass of the belite.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cement admixture. [Background technology]

[0002] Currently, reducing carbon dioxide emissions has become an important issue in order to curb global warming. As a method for fixing carbon dioxide contained in exhaust gases in a cementitious hardened body to reduce carbon dioxide emissions into the atmosphere, for example, Patent Document 1 describes a method for fixing carbon dioxide, which includes a contacting step of contacting a carbon dioxide-containing gas having a temperature of 350°C or higher with a cementitious hardened body to fix the carbon dioxide contained in the carbon dioxide-containing gas in the cementitious hardened body. Furthermore, Patent Document 2 describes a fine powder cement in which fine powder generated as a by-product during the production of recycled aggregate from waste concrete is reused as part of the cement raw material, and which is characterized by the addition of a small amount of fine powder of waste concrete containing almost no calcium hydroxide to cement clinker. This fine powder cement is a material in which carbonation has progressed. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2020-131074 A [Patent Document 2] JP 2010-254503 A Summary of the Invention [Problem to be solved by the invention]

[0004] Cement clinker is made using a large amount of waste as a raw material, and the production and use of cement clinker has an important role in contributing to a recycling-oriented society. An object of the present invention is to provide a cement admixture which uses cement clinker as a raw material and has carbon dioxide fixed therein, and which, when used as an admixture, can reduce the carbon dioxide emission unit of a mixed cement containing the admixture. [Means for solving the problem]

[0005] As a result of intensive research to solve the above problems, the present inventors have found that the above objects can be achieved by a cement admixture containing a pulverized carbonated cement clinker obtained by carbonating a cement clinker containing calcium silicate and an Al2O3-containing mineral phase, and have completed the present invention. That is, the present invention provides the following [1] to [9]. [1] A cement admixture comprising ground carbonated cement clinker obtained by carbonating cement clinker containing calcium silicate and an Al2O3-containing mineral phase as a mineral composition. [2] The cement admixture according to [1], wherein the cement clinker contains, as a mineral composition by the XRD-Rietveld method, 40% by mass or more of the calcium silicate and 0.1% by mass or more of the Al2O3-containing mineral phase. [3] The cement admixture according to [1] or [2], wherein the carbon content of the cement admixture is 0.5 to 10 mass %. [4] The cement admixture according to any one of [1] to [3], wherein the calcium silicate is one or more selected from alite and belite, and the Al2O3-containing mineral phase is one or more selected from an aluminate phase, a ferrite phase, gehlenite, hauyne, and CaAl2O4. [5] The cement admixture according to any one of [1] to [4], wherein the cement clinker contains belite as the calcium silicate and gehlenite as the Al2O3-containing mineral phase, and is a fired product that satisfies the following conditions (1) and (2): (1) The amount of the gehlenite per 100 parts by mass of the belite is 10 to 100 parts by mass. (2) The cement clinker does not contain an aluminate phase or contains an aluminate phase in an amount of 15 parts by mass or less per 100 parts by mass of the belite.

[0006] [6] A mixed cement comprising the cement admixture according to any one of [1] to [5] above and cement, wherein the proportion of the cement admixture in the mixed cement is 5 to 60 mass %. [7] A method for producing the cement admixture according to any one of the above [1] to [5], comprising a first carbonation curing step of obtaining the cement admixture by carbonating and curing the coarsely crushed material obtained by crushing the cement clinker, or by carbonating and curing the crushed material obtained by crushing the cement clinker, [8] A method for producing the cement admixture according to any one of [1] to [5] above, comprising: a kneading step of kneading a pulverized product obtained by pulverizing the cement clinker with water to obtain a paste; a paste carbonation step of carbonating and curing the paste to obtain a hardened paste; and a grinding step of grinding the hardened product to obtain the cement admixture. [9] The method for producing the cement admixture according to [8], further comprising a second carbonation curing step of carbonating the cement admixture obtained in the grinding step. Effect of the Invention

[0007] Since the cement admixture of the present invention fixes carbon dioxide, the carbon dioxide emission unit of a mixed cement containing the cement admixture can be reduced compared to the carbon dioxide emission unit of a cement not containing the cement admixture, and the amount of carbon dioxide emitted during the production of cement can be reduced. In addition, since the cement clinker is used as a raw material, the amount of cement clinker used in the mixed cement containing the cement admixture of the present invention can be maintained at the same level as that of the cement not containing the cement admixture, and the effective use of waste as a raw material for cement clinker can be promoted. Furthermore, the cement admixture of the present invention can provide a blended cement containing the cement admixture with sufficient strength development and fluidity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The cement admixture of the present invention contains ground carbonated cement clinker obtained by carbonating cement clinker containing calcium silicate and an Al2O3-containing mineral phase as a mineral composition. Examples of calcium silicates include alite (3CaO·SiO2: also called "C3S") and belite (2CaO·SiO2: also called "C2S"), etc. These may be contained alone or in combination of two or more kinds. Examples of Al2O3-containing mineral phases include aluminate phase (3CaO·Al2O3: also called "C3A"), ferrite phase (4CaO·Al2O3·Fe2O3: also called "C4AF"), gehlenite (2CaO·Al2O3·SiO2: also called "C2AS"), hauyne (3CaO·3Al2O3·CaSO4), CaAl2O4 (also called "CA"), etc. These may be contained alone or in combination of two or more. In addition, the mineral phase may contain components such as Na, Mg, Al, Si, P, S, Cl, K, Fe, Si, and Cr in solid solution.

[0009] The proportion of calcium silicate in the cement clinker is preferably 40% by mass or more, more preferably 45% by mass or more, even more preferably 50% by mass or more, even more preferably 55% by mass or more, even more preferably 60% by mass or more, and particularly preferably 65% ​​by mass or more, as a mineral composition by the XRD-Rietveld method, from the viewpoint of increasing the amount of carbon dioxide fixed in the cement clinker and from the viewpoint of ease of production, etc., the above proportion is preferably 98% by mass or less, more preferably 95% by mass or less, even more preferably 93% by mass or less, even more preferably 85% by mass or less, even more preferably 80% by mass or less, and particularly preferably 75% by mass or less, as a mineral composition by the XRD-Rietveld method. In addition, when the cement clinker contains a plurality of types of mineral compositions as calcium silicate, the above ratio is the total ratio of the plurality of types of mineral compositions.

[0010] When the cement clinker contains alite as calcium silicate, the proportion of alite in the cement clinker is preferably 80 mass % or less, more preferably 10 to 70 mass %, and particularly preferably 25 to 65 mass %, from the viewpoints of the strength development of the mixed cement containing the cement admixture of the present invention and the fluidity of the mixed cement before hardening. When the cement clinker contains belite as a calcium silicate, the proportion of belite in the cement clinker is preferably 5 to 95 mass%, more preferably 10 to 90 mass%, further preferably 15 to 88 mass%, and particularly preferably 20 to 85 mass%, from the viewpoints of the strength development of a mixed cement containing the cement admixture of the present invention and the fluidity of the mixed cement before hardening.

[0011] From the viewpoint of increasing the amount of carbon dioxide fixed in the cement clinker, the proportion of the Al2O3-containing mineral phase in the cement clinker, as a mineral composition by the XRD-Rietveld method, is preferably 0.1 mass% or more, more preferably 0.5 mass% or more, even more preferably 1.0 mass% or more, even more preferably 1.2 mass% or more, even more preferably 8.0 mass% or more, even more preferably 15 mass% or more, even more preferably 20 mass% or more, and particularly preferably 25 mass% or more. In addition, from the viewpoint of increasing the proportion of calcium silicate relatively to further improve the strength development of the mixed cement containing the cement admixture of the present invention and the fluidity of the mixed cement before hardening, the above proportion is preferably 50 mass% or less, more preferably 45 mass% or less, and particularly preferably 40 mass% or less, in terms of the mineral composition by the XRD-Rietveld method. In addition, when the cement clinker contains a plurality of types of mineral compositions as the Al2O3-containing mineral phase, the above ratio is the total ratio of the plurality of types of mineral compositions.

[0012] When the cement clinker contains an aluminate phase as an Al2O3-containing mineral phase, the ratio of the aluminate phase in the cement clinker is preferably 0.1 to 20 mass%, more preferably 0.2 to 15 mass%, even more preferably 0.3 to 10 mass%, even more preferably 0.5 to 8 mass%, and particularly preferably 0.7 to 5 mass%. If the ratio is 0.1 mass% or more, the carbonation of the cement clinker is easily promoted, and a large amount of carbon dioxide can be fixed in the cement clinker. If the ratio is 20 mass% or less, the fluidity of the mixed cement containing the cement admixture of the present invention before hardening is further improved.

[0013] When the cement clinker contains gehlenite as an Al2O3-containing mineral phase, the proportion of gehlenite in the cement clinker is preferably 0.1 to 40 mass%, more preferably 10 to 35 mass%, further preferably 20 to 32 mass%, and particularly preferably 25 to 30 mass%. If the proportion is 0.1 mass% or more, the carbonation of the cement clinker is likely to proceed, and a large amount of carbon dioxide can be fixed in the cement clinker. If the proportion is 40 mass% or less, the amount of calcium silicate (e.g., belite) is relatively large, and the strength development of the cement containing the cement admixture of the present invention is further improved. When the cement clinker contains auyne as an Al2O3-containing mineral phase, the ratio of auyne in the cement clinker is preferably 0.1 to 40 mass%, more preferably 10 to 35 mass%, further preferably 20 to 32 mass%, and particularly preferably 25 to 30 mass%. If the ratio is 40 mass% or less, the amount of calcium silicate (e.g., belite) becomes relatively large, so that the strength development of the cement containing the cement admixture of the present invention is further improved.

[0014] When the cement clinker contains CaAl2O4 as an Al2O3-containing mineral phase, the ratio of CaAl2O4 in the cement clinker is preferably 0.1 to 10 mass%, more preferably 0.2 to 5 mass%, further preferably 0.3 to 3 mass%, and particularly preferably 0.4 to 1 mass%. If the ratio is 10 mass% or less, the amount of calcium silicate (e.g., belite) becomes relatively large, and the strength development of the cement containing the cement admixture of the present invention is further improved.

[0015] The mineral composition of the cement clinker (proportion of belite, etc.) can be quantified, for example, by using the XRD (X-ray diffraction)-Rietveld method for the cement clinker. Specifically, the mineral composition can be quantified by fitting the theoretical profile of each mineral to the powder X-ray diffraction chart (actually measured profile) of the cement clinker. For the quantification, commercially available analysis software can be used. The mineral composition can also be quantified by microscopic observation or point counting using electron backscatter diffraction.

[0016] From the viewpoint of obtaining a cement admixture in which a larger amount of carbon dioxide is fixed in a short carbonation curing time (a cement admixture containing pulverized carbonated cement clinker in which a larger amount of carbon dioxide is fixed), it is preferable that the above-mentioned cement clinker is a fired product that contains belite as a calcium silicate and gehlenite as an Al2O3-containing mineral phase and satisfies the following conditions (1) and (2). (1) The amount of gehlenite per 100 parts by mass of belite is 10 to 100 parts by mass. (2) The fired product does not contain an aluminate phase, or contains an aluminate phase in an amount of 15 parts by mass or less per 100 parts by mass of the belite.

[0017] In the fired product satisfying the conditions (1) and (2), the amount of gehlenite relative to 100 parts by mass of belite is 10 to 100 parts by mass, preferably 20 to 80 parts by mass, more preferably 25 to 70 parts by mass, even more preferably 30 to 60 parts by mass, and particularly preferably 40 to 50 parts by mass. In the pulverized product of the fired product (pulverized cement clinker) in which the amount is less than 10 parts by mass, carbonation does not proceed easily, and the amount of carbon dioxide fixed in the cement clinker is reduced. When the amount exceeds 100 parts by mass, the amount of belite is relatively reduced, and the strength development of the mixed cement containing the cement admixture of the present invention is reduced. When the fired product contains an aluminate phase, the amount of the aluminate phase relative to 100 parts by mass of belite is 15 parts by mass or less, preferably 0.1 to 10 parts by mass, more preferably 0.5 to 5 parts by mass, and particularly preferably 1 to 3 parts by mass. It is difficult to produce a fired product with the amount exceeding 15 parts by mass. In addition, if the amount is 15 parts by mass or less, the fluidity of the mixed cement containing the cement admixture of the present invention before hardening is further improved.

[0018] The above-mentioned cement clinker can be produced, for example, by preparing the raw material from one or more materials selected from industrial waste, general waste, construction waste soil, etc. so as to have the target mineral composition, chemical composition, etc. of the fired product, and then firing the raw material at, for example, 1,000 to 1,400°C (preferably 1,200 to 1,400°C, and more preferably 1,300 to 1,400°C). In addition, if it is difficult to adjust the mineral composition of the cement clinker to the target values ​​using only the above raw materials, raw materials such as a calcium raw material (e.g., limestone), a silicon raw material, an aluminum raw material, and an iron raw material may be used. The obtained cement clinker (burned product) is usually crushed appropriately using a crusher such as a ball mill or a rod mill. When the cement admixture contains gypsum or limestone, the cement clinker and the lump-shaped gypsum or limestone may be crushed and mixed at the same time. The crushed product obtained by crushing the cement clinker (hereinafter also referred to as "cement clinker crushed product") preferably has a Blaine specific surface area of ​​1,000 to 10,000 cm. 2 / g, more preferably 2,000 to 8,000 cm 2 / g, and particularly preferably 3,000 to 6,000 cm 2 / g. The above Blaine specific surface area is 1,000 cm 2 / g or more, the amount of carbon dioxide fixed in the cement clinker by carbonation curing is increased. Also, the strength development of the blended cement containing the cement admixture of the present invention is improved. 2 / g or less, the fluidity of the mixed cement containing the cement admixture of the present invention before hardening is further improved.

[0019] The cement admixture of the present invention contains a pulverized product of carbonated cement clinker (hereinafter also referred to as "pulverized carbonated cement clinker") obtained by carbonating the above-mentioned cement clinker. The carbonation of cement clinker is carried out, for example, by carbonation curing. Note that "carbonation" refers to the absorption and fixation of carbon dioxide. The method of carbonation curing is not particularly limited, and examples thereof include (i) a method of exposing a crushed material (crushed cement clinker) obtained by crushing cement clinker to carbon dioxide for carbonation curing, (ii) a method of exposing a crushed material (crushed cement clinker) obtained by crushing cement clinker to carbon dioxide for carbonation curing (described later), (iii) a method of exposing a hardened body of a hydraulic composition (e.g., paste) containing crushed cement clinker and water to carbon dioxide for carbonation curing (described later), (iv) a method of injecting carbon dioxide into a slurry obtained by mixing crushed cement clinker and water, followed by dehydration and drying, and (v) a method of injecting carbon dioxide into a hydraulic composition (e.g., paste) containing crushed cement clinker and water when kneading the hydraulic composition. In the above method (i), the crushed cement clinker after carbonation curing is usually crushed to obtain a pulverized carbonated cement clinker. Examples of methods for exposing the object to carbon dioxide include a method in which the object to be carbonation cured is left standing in an atmosphere of a gas containing carbon dioxide (gaseous carbon dioxide) (hereinafter also referred to as a "carbon dioxide-containing gas"). The carbon content of the cement admixture is preferably 0.5 to 10 mass%, more preferably 0.8 to 8 mass%, further preferably 1 to 6 mass%, and particularly preferably 2 to 5 mass%. If the carbon content is 0.5 mass% or more, the amount of carbon dioxide emitted during the production of a mixed cement containing the cement admixture of the present invention can be further reduced. If the carbon content is 10 mass% or less, the strength development of the mixed cement containing the cement admixture of the present invention can be further improved. The proportion of carbon in a cement admixture can be measured, for example, using a commercially available carbon / sulfur analyzer.

[0020] The cement admixture of the present invention may contain gypsum. When the cement admixture contains gypsum, it is possible to save the trouble of adjusting the amount of gypsum contained in the mixed cement when preparing a mixed cement containing the cement admixture and cement. Examples of the type of gypsum are not particularly limited, and include, for example, natural gypsum dihydrate, flue gas desulfurized gypsum (flue gas desulfurized gypsum), phosphate gypsum, titanic gypsum, hydrofluoric gypsum, etc. These may be used alone or in combination of two or more. Examples of the form of gypsum (whether it is a hydrate or not) include gypsum dihydrate, gypsum hemihydrate, and anhydrous gypsum. These may consist of only one type, or may include two or more types. The proportion of gypsum in the cement admixture is preferably 0.1-4.0 mass%, more preferably 0.3-3.5 mass%, and particularly preferably 0.5-3.0 mass%, calculated as SO3. If the proportion is 0.1 mass% or more, the usable time before hardening (the time during which good fluidity can be maintained) of the mixed cement containing the cement admixture of the present invention is increased. If the proportion is 4.0 mass% or less, the strength development of the mixed cement containing the cement admixture of the present invention is improved. The gypsum (usually gypsum powder) may be prepared by mixing the ground cement clinker with gypsum before carbonating the ground cement clinker, or by mixing the carbonated ground cement clinker with gypsum after carbonating the ground cement clinker.

[0021] The Blaine specific surface area of ​​the cement admixture is preferably 2,000 to 20,000 cm 2 / g, more preferably 2,500 to 15,000 cm 2 / g. Particularly preferably, 3,000 to 13,000 cm 2 / g. The above Blaine specific surface area is 2,000 cm 2 / g or more, the strength development of a mixed cement containing the cement admixture of the present invention is further improved. 2 / g or less, the fluidity of the mixed cement containing the cement admixture of the present invention before hardening is further improved.

[0022] As a method for producing the above-mentioned cement admixture, for example, there can be mentioned a method including a first carbonation curing step of obtaining a cement admixture containing a pulverized product of carbonated cement clinker by carbonating and curing the coarsely crushed product obtained by coarsely crushing the above-mentioned cement clinker, or by carbonating and curing the pulverized product obtained by crushing the above-mentioned cement clinker. An example of the carbonation curing method is a method in which cement clinker is coarsely crushed and then the obtained coarsely crushed material, or cement clinker is crushed and then the obtained crushed material is allowed to stand under an atmosphere of carbon dioxide-containing gas. According to this method, compared to a method in which precast concrete or the like is carbonation cured to fix carbon dioxide in concrete, the equipment can be made smaller and the costs associated with the equipment can be reduced. Another example of the carbonation curing method is a method in which cement clinker is pulverized, and then the pulverized material is brought into contact with a carbon dioxide-containing gas to effect continuous carbonation.

[0023] From the viewpoint of increasing the amount of carbon dioxide fixed in the cement clinker, the carbon dioxide concentration of the carbon dioxide-containing gas is preferably 1 vol% or more, more preferably 10 vol% or more, even more preferably 50 vol% or more, and particularly preferably 60 vol% or more. Also, from the viewpoint of reducing costs for curing equipment, etc., the carbon dioxide gas concentration is preferably 95 vol% or less, more preferably 85 vol% or less, even more preferably 50 vol% or less, and particularly preferably 30 vol% or less. The temperature in the carbonation curing is preferably 5 to 300° C., more preferably 10 to 250° C., even more preferably 20 to 200° C., still more preferably 40 to 150° C., and particularly preferably 50 to 130° C. If the temperature is 5° C. or higher, the efficiency of carbonation is further improved. If the temperature is 300° C. or lower, the energy cost required for the carbonation curing can be further reduced. The relative humidity in the carbonation curing is preferably 20 to 90%, more preferably 30 to 80%, and particularly preferably 40 to 70%. If the relative humidity is 20% or more, the efficiency of carbonation is further improved. If the relative humidity is 90% or less, the cost required for curing equipment can be further reduced.

[0024] Another example of the method for producing a cement admixture includes a kneading step of kneading water with a pulverized product obtained by pulverizing cement clinker to obtain a paste, a paste carbonation step of carbonating and curing the paste to obtain a hardened paste, and a grinding step of grinding the hardened product to obtain a cement admixture containing a pulverized product of carbonated cement clinker. In the kneading step, gypsum may be further kneaded. The method of kneading each material is not particularly limited. The device used for kneading is also not particularly limited, and for example, a conventional mixer such as an omni mixer, a pan type mixer, a twin-shaft mixer, or a tilting mixer can be used.

[0025] The carbonation curing method in the paste carbonation step may include a method in which the paste is allowed to stand under an atmosphere of a carbon dioxide-containing gas. The carbon dioxide concentration of the carbon dioxide-containing gas, the temperature in the carbonation curing, and the relative humidity in the carbonation curing are similar to the carbon dioxide concentration of the carbon dioxide-containing gas in the first carbonation curing step described above. Alternatively, the paste before hardening may be poured into a formwork, and after the paste in the formwork has hardened, the hardened paste may be removed from the formwork and allowed to stand in an atmosphere of carbon dioxide-containing gas. The method for applying the paste is not particularly limited, and a conventional method such as pouring can be used. The method of curing the mixture after it is poured into the formwork until it is demolded is not particularly limited, and for example, general curing methods such as air curing, moist air curing, underwater curing, sealed curing, steam curing, etc. Carbonation curing may also be used as the curing method until it is demolded.

[0026] In the pulverization step, the method for pulverizing the hardened body is not particularly limited, and examples thereof include a method in which the hardened body is pulverized using a pulverizing means such as a disk mill, a vibration mill, an impact crusher, or a cone crusher. Moreover, the above-mentioned kneading step and paste carbonation step may be carried out again using the pulverized material obtained in the pulverization step instead of the pulverized material obtained by pulverizing the cement clinker.

[0027] After the above-mentioned pulverization step, a second carbonation curing step may be provided in which the cement admixture obtained in the pulverization step is further carbonated and cured. By further carbonating and curing the cement admixture obtained in the pulverization step, a larger amount of carbon dioxide can be fixed in the cement admixture (particularly, the pulverized carbonated cement clinker contained in the cement admixture). In addition, further pulverization may be performed in this step. The carbonation curing method in the second carbonation curing step is the same as the carbonation curing method in the first carbonation curing step described above. In addition, for the purpose of further carbonation curing the cement admixture obtained in the second carbonation curing step, one or more carbonation curing steps (steps similar to the above-mentioned second carbonation curing step) may be provided after the second carbonation curing step. The number of added carbonation curing steps is preferably 1 or more, more preferably 1 to 2. By performing the carbonation curing step multiple times, the proportion of carbon in the cement admixture can be increased.

[0028] The blended cement of the present invention contains the above-mentioned cement admixture and cement. The cement is not particularly limited, and examples thereof include various types of Portland cement such as ordinary Portland cement, high-early-strength Portland cement, moderate-heat Portland cement, low-heat Portland cement, and sulfate-resistant Portland cement; cement containing admixtures such as blast-furnace cement and fly ash cement (mixed cement); ecocement, white cement, and ultra-fast-hardening cement. These may be used alone or in combination of two or more. The ratio of the cement admixture in the mixed cement is preferably 5 to 60% by mass, more preferably 8 to 55% by mass, even more preferably 10 to 50% by mass, even more preferably 15 to 40% by mass, and particularly preferably 18 to 30% by mass. If the ratio is 5% by mass or more, the carbon dioxide emission intensity of the mixed cement containing the cement admixture can be further reduced, and the carbon dioxide emission when producing the same amount of the mixed cement can be further reduced compared to the cement not containing the cement admixture. If the ratio is 60% by mass or less, the strength development of the mixed cement can be further improved. EXAMPLES

[0029] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. [Production of cement clinker A] Sewage sludge, construction soil, limestone, and clay were used as raw materials, and the raw materials were mixed to obtain the target chemical composition range including the chemical composition shown in Table 1 (actual values ​​measured in accordance with "JIS R 5204:2019 (Method for X-ray fluorescence analysis of cement)"), and the raw materials were prepared for firing. This raw material for firing was then fired at 1,370°C in a rotary kiln to obtain cement clinker A (fired product). In addition to heavy oil, waste oil and waste plastic were used as fuel for firing. The powder X-ray diffraction (XRD) pattern of the obtained cement clinker A was obtained using an X-ray diffractometer (manufactured by Bruker Japan, product name "D8 ADVANCE A-25 type"). The measurement conditions of the powder X-ray diffraction were as follows: target: CuKα, tube condition: 40 kV-40 mA, scanning range: 2θ = 5 to 65 °, step width: 0.023 ° / step, and measurement time: 0.13 seconds / step. The obtained powder XRD pattern was qualitatively analyzed using analysis software (manufactured by Bruker Japan, product name "DIFFRAC.EVA"), and peaks of C2S (β-C2S), C2AS, C3A, and CA were observed. Next, the mineral composition of cement clinker A was measured by fitting the theoretical profiles of each mineral, C2S (β-C2S), C2AS, C3A, and CA, to the measured profiles obtained from the powder XRD results by the Rietveld method using analytical software (manufactured by Bruker Japan, product name "DIFFRAC.TOPAS ver.6"). The results are shown in Table 2.

[0030] [Materials used] (1) Cement clinker A: obtained by the above-mentioned manufacturing method (2) Ordinary Portland Cement: Manufactured by Taiheiyo Cement Corporation; Dihydrate gypsum content: 0.9% by mass (SO3 equivalent); Hemihydrate gypsum content: 1.7% by mass (SO3 equivalent); Limestone (CaCO3) content: 4.0% by mass; Cement clinker contained in ordinary Portland cement has the chemical composition shown in Table 3 and the mineral composition shown in Table 4 (The chemical composition was measured in accordance with "JIS R 5204: 2019 (Method for X-ray fluorescence analysis of cement)". The mineral composition was measured in the same manner as the above-mentioned cement clinker A, except that the mineral settings in the analysis software were changed to the types of minerals shown in Table 4.), Carbon dioxide emission intensity (the amount of carbon dioxide emitted when producing 1 ton of ordinary Portland cement): 824.2 kg / ton; Blaine specific surface area: 3,160 cm 2 / g (3) Low-heat Portland cement; manufactured by Taiheiyo Cement Corporation; proportion of gypsum dihydrate: 1.2% by mass (SO3 equivalent); proportion of gypsum hemihydrate: 1.6% by mass (SO3 equivalent); cement clinker contained in the low-heat Portland cement has the chemical composition shown in Table 5 and the mineral composition shown in Table 6 (the chemical composition and mineral composition were measured in the same manner as for ordinary Portland cement clinker); carbon dioxide emission unit (amount of carbon dioxide emitted in producing 1 ton of low-heat Portland cement): 824.2 kg / ton; Blaine specific surface area: 3,160 cm 2 / g (4) Gypsum: Exhausted gypsum dihydrate (SO3 content: 44.9% by mass) (5) Fine aggregate: Cement Association standard sand (6) Water: Tap water The carbon dioxide emission intensity of ordinary Portland cement and low-heat Portland cement is based on the value of carbon dioxide generated during the production of Portland cement (weighted average of all Portland cement) listed in "Summary of LCI Data for Cement, General Incorporated Association, Japan Cement Association, March 16, 2022: https: / / www.jcassoc.or.jp / cement / 4pdf / jg1i_01.pdf."

[0031] [Table 1]

[0032] [Table 2]

[0033] [Table 3]

[0034] [Table 4]

[0035] [Table 5]

[0036] [Table 6]

[0037] [Example 1] Ordinary Portland cement was left to stand for 4 days under an atmosphere of a carbon dioxide-containing gas with a temperature of 65°C, a relative humidity of 60°C, and a carbon dioxide content of 80% by volume (hereinafter also referred to as "carbonation curing condition A"), and then left to stand for a further 7 days under an atmosphere of a temperature of 65°C, a relative humidity of 60°C, and a carbon dioxide-containing gas with a carbon dioxide content of 20% by volume (hereinafter also referred to as "carbonation curing condition B") to perform carbonation curing, thereby obtaining a cement admixture A. The gypsum proportion and Blaine specific surface area (represented as "Blaine" in Table 7) of the obtained cement admixture are shown in Table 7. The carbon content of the resulting cement admixture A was measured according to the following method.

[0038] [Carbon ratio] The carbon content of the resulting cement admixture (hereinafter also referred to as "carbonated cement admixture") was measured using a carbon / sulfur analyzer (manufactured by Horiba, product name "EMIA-Step") at a temperature of 1,250°C for 120 seconds. [Amount of carbon dioxide fixed in the cement admixture before carbonation (referred to as "CO2 fixed amount" in Table 7)] The amount of carbon dioxide fixed per ton of the cement admixture before carbonation (ordinary Portland cement in Example 1) was determined using a carbon-sulfur analyzer. Specifically, the carbon amount of the cement admixture before carbonation and the cement admixture after carbonation (cement admixture A in Example 1) was analyzed using a carbon-sulfur analyzer and then converted into CO2. This converted value was determined to be due to decarbonation of calcium carbonate contained in the cement admixture before carbonation or the cement admixture after carbonation, and the amount of carbon dioxide fixed per ton of the cement admixture before carbonation was determined using the following formula (1). Amount of carbon dioxide fixed (kg / ton) = a / (100-b) × (100 / (100-c) × 1000-(d / 100) × 1000 (1) (In formula (1), a represents the proportion of carbon dioxide in the cement admixture after carbonation (% by mass), b represents the ignition loss in the cement admixture after carbonation (% by mass), c represents the ignition loss in the cement admixture before carbonation (% by mass), and d represents the proportion of carbon dioxide in the cement admixture before carbonation (% by mass).)

[0039] [Carbon dioxide emission intensity (referred to as "CO2 emission intensity" in Table 7)] The carbon dioxide emission intensity of the carbonated cement admixture (the amount of carbon dioxide emitted during the production of the carbonated cement admixture) was calculated using the following formula (2). Carbon dioxide emission intensity (kg / ton) = (ef) × 1000 / (1000+f+g) (2) (In formula (2), e is the carbon dioxide emission unit of the cement admixture before carbonation (kg / ton), f is the amount of carbon dioxide fixed in the cement admixture before carbonation (kg / ton), and g is the increase in water in the cement admixture after carbonation compared to the cement admixture before carbonation (kg / ton)) The increase in water content of the cement admixture after carbonation relative to the cement admixture before carbonation (represented as "increased water content" in Table 7) was calculated using the following formula (3). Increase in water volume (kg / ton) = (h + i × 1000 / 100) / j × 100 - 1000 - h (3) (In the above formula (3), h is the amount of carbon dioxide fixed in the cement admixture before carbonation (kg / ton), i is the carbon dioxide content in the cement admixture before carbonation (mass%), and j is the carbon dioxide content in the cement admixture after carbonation (mass%).

[0040] [Carbon dioxide reduction rate (referred to as "CO2 reduction rate" in Table 7)] The carbon dioxide reduction rate (%) due to the carbonation of cement clinker was calculated using the following formula (4). Carbon dioxide reduction rate = (kl) / k × 100% (4) (In equation (4), k is the carbon dioxide emission unit of ordinary Portland cement (kg / ton), and l is the carbon dioxide emission unit of the cement admixture after carbonation (kg / ton).

[0041] [Example 2] Cement clinker A and dehydrated gypsum were mixed and ground in amounts such that the mass ratio was 95.67:4.33, to obtain a mixture of ground cement clinker A and ground dehydrated gypsum. The carbon dioxide emission intensity of the above mixture (the amount of carbon dioxide emitted during the production of the above mixture) was 615 kg / ton. The mixture was subjected to carbonation curing in the same manner as in Example 1 to obtain a cement admixture B. The carbon content of the obtained cement admixture B and other properties were measured in the same manner as in Example 1.

[0042] [Example 3] Ordinary Portland cement and water were put into a container in an amount such that the mass ratio of water to cement (water / cement) was 50 / 100, and the mixture was kneaded for 3 minutes using a hand mixing spoon as specified in "JIS R 5201:2015 (Physical Testing Methods for Cement)" to prepare a paste. The obtained paste was left in the container for 4 days under carbonation curing condition A. After leaving it, the dried hardened paste was removed from the container and crushed for 30 seconds using a vibrating disc mill under a condition of 100 g / batch, and then the obtained crushed material and water were used in an amount such that the mass ratio of water to crushed material (water / crushed material) was 50 / 100 to prepare a paste in the same manner as the above paste, and the paste was left to stand for 7 days under carbonation curing condition B. After leaving it to stand, the dried hardened paste was removed from the container and crushed for 30 seconds using a vibrating disc mill under a condition of 100 g / batch to obtain a cement admixture C. The carbon content of the obtained cement admixture C was measured in the same manner as in Example 1. [Example 4] A cement admixture D was obtained in the same manner as in Example 3, except that the mixture prepared in Example 2 (a mixture of ground cement clinker A and ground dehydrated gypsum) was used instead of ordinary Portland cement. The carbon content of the obtained cement admixture D and other properties were measured in the same manner as in Example 1.

[0043] [Example 5] Ordinary Portland cement was left to stand for 7 days under an atmosphere of a carbon dioxide-containing gas with a temperature of 30°C, a relative humidity of 60°C, and a carbon dioxide content of 80% by volume (hereinafter also referred to as "carbonation curing condition C") to carry out carbonation curing, and cement admixture E was obtained. The carbon percentage and other properties of the obtained cement admixture E were calculated in the same manner as in Example 1. [Example 6] A cement admixture F was obtained in the same manner as in Example 5, except that the above mixture prepared in Example 2 was used instead of ordinary Portland cement. The carbon percentage and other properties of the obtained cement admixture F were calculated in the same manner as in Example 1. [Example 7] Ordinary Portland cement and water were mixed in amounts such that the mass ratio of water to cement (water / cement) was 50 / 100 to prepare a paste. The obtained paste was left to stand for one day under carbonation curing conditions C. The hardened paste after standing was pulverized using a vibrating disk mill to obtain a cement admixture G. The carbon percentage of the obtained cement admixture G and the like were calculated in the same manner as in Example 1. [Example 8] A cement admixture H was obtained in the same manner as in Example 7, except that the above mixture prepared in Example 2 was used instead of ordinary Portland cement. The carbon percentage of the obtained cement admixture H and the like were calculated in the same manner as in Example 1.

[0044] [Example 9] Ordinary Portland cement and water were mixed in amounts such that the mass ratio of water to cement (water / cement) was 50 / 100 to prepare a paste. The obtained paste was left to stand for 7 days under carbonation curing condition C. The hardened paste after standing was pulverized using a vibrating disk mill to obtain cement admixture I. The carbon percentage and other properties of the obtained cement admixture I were calculated in the same manner as in Example 1. [Example 10] A cement admixture J was obtained in the same manner as in Example 9, except that the above mixture prepared in Example 2 was used instead of ordinary Portland cement. The carbon percentage of the obtained cement admixture J was calculated in the same manner as in Example 1.

[0045] [Example 11] In the same manner as in Example 9, a cement admixture K having a different Blaine specific surface area from that of the cement admixture I was obtained. The obtained admixture K differs from the cement admixture I only in the Blaine specific surface area, so the carbon ratio of the cement admixture J was the same as that of Example 9. [Example 12] In the same manner as in Example 10, a cement admixture L having a different Blaine specific surface area from that of the cement admixture J was obtained. The obtained admixture L differed from the cement admixture J only in the Blaine specific surface area, so the carbon ratio of the cement admixture J was the same as that of Example 10. [Example 13] A cement admixture M was obtained in the same manner as in Example 9, except that low-heat Portland cement was used instead of ordinary Portland cement. The carbon ratio and the like of the obtained cement admixture M were calculated in the same manner as in Example 1. The results are shown in Table 7.

[0046] [Table 7]

[0047] [Examples 14 to 36] Ordinary Portland cement was mixed with the types of cement admixtures shown in Table 8 in the proportions shown in Table 8 to prepare blended cements. Using the prepared mixed cement, water, and fine aggregate, test specimens were prepared in accordance with "JIS R 5201:2015 (Physical testing methods for cement)" and the mortar compressive strength was measured at ages of 3 days, 7 days, and 28 days. The amount of water mixed was set so that the mass ratio of water to mixed cement (water / mixed cement) was 50 / 100, and the amount of fine aggregate mixed was set so that 300 parts by mass per 100 parts by mass of mixed cement.

[0048] In addition, the carbon dioxide emission intensity of the blended cement (the amount of carbon dioxide emitted when producing 1 ton of blended cement; represented as "CO2 emission intensity" in Table 8) was calculated using the following formula (5). Carbon dioxide emission intensity of blended cement (kg / ton) = m × n + o × p (5) (In formula (5), m is the carbon dioxide emission unit of ordinary Portland cement (kg / ton), n is the mixing ratio of ordinary Portland cement in the blended cement (mass ratio of ordinary Portland cement to blended cement (ordinary Portland cement / blended cement)), o is the carbon dioxide emission unit of the cement admixture after carbonation (kg / ton), and p is the mixing ratio of the cement admixture after carbonation in the blended cement (mass ratio of the cement admixture after carbonation to the blended cement (cement admixture after carbonation / blended cement)). In addition, the carbon dioxide reduction rate (referred to as "CO2 reduction rate" in Table 8) was calculated using the following formula (6). Carbon dioxide reduction rate = (carbon dioxide emission intensity of ordinary Portland cement) - carbon dioxide emission intensity of blended cement) / carbon dioxide emission intensity of ordinary Portland cement × 100% (6) Furthermore, for the mortars of Examples 15, 17, 19, and 21, the mortar flow values ​​(0 hits and 15 hits) were measured in accordance with "JIS R 5201:2015 (Physical testing methods for cement)".

[0049] [Comparative Example 1] Mortar was prepared in the same manner as in Example 14, except that ordinary Portland cement was used instead of the blended cement, and the mortar compressive strength and mortar flow values ​​(0 strokes, 15 strokes) were measured. The results are shown in Tables 8 and 9.

[0050] [Table 8]

[0051] [Table 9]

[0052] From Table 7, it can be seen that carbon dioxide is fixed in the cement admixtures A to M. In addition, from Tables 8 to 9, the carbon dioxide emission intensity (534 to 819 kg / ton) of the blended cements of Examples 14 to 36 is smaller than the carbon dioxide emission intensity (824 kg / ton) of the ordinary Portland cement of Comparative Example 1, and it is understood that according to the present invention, the carbon dioxide emission intensity of the blended cement can be reduced. In addition, the mortar compressive strength at ages of 3 and 7 days (age of 3 days: 9.2 to 26.9 N / mm 2 , material age 7 days: 15.7~44.1N / mm 2 ) is, for example, the compressive strength of mortar (3 days old: 7.5 N / mm2), which is one of the qualities of fly ash cement type C specified in "JIS R 5210:2009 (Portland cement)". 2 Above, material age 7 days: 15.0N / mm 2 The compressive strength of the mortar at 28 days of use in Examples 14 to 22 and 24 to 36 (at 28 days of use: 32.6 to 63.2 N / mm 2 ) is one of the qualities of the above fly ash cement type C, and is the compressive strength of the mortar (28 days old: 32.5N / mm 2 or above). It can also be seen that the mortar flow values ​​of Examples 15, 17, 19, and 21 (average value for 0 hits: 104-108 mm, average value for 15 hits: 198-213 mm) are similar to the mortar flow value of Comparative Example 1 (average value for 0 hits: 107 mm, average value for 15 hits: 214 mm).

Claims

1. The mineral composition is calcium silicate and Al. 2 O 3 A cement admixture comprising ground carbonated cement clinker obtained by carbonating cement clinker containing a mineral phase.

2. The cement clinker has a mineral composition according to the XRD-Rietveld method, the calcium silicate being present in an amount of 40 mass% or more, and the Al 2 O 3 2. The cement admixture according to claim 1, which contains the mineral phase in an amount of 0.1 mass% or more.

3. The cement admixture according to claim 1, wherein the carbon content of the cement admixture is 0.5 to 10 mass %.

4. The calcium silicate is at least one selected from alite and belite, and the Al 2 O 3 The mineral phases contained are aluminate phase, ferrite phase, gehlenite, auin, and CaAl 2 O 4 2. The cement admixture according to claim 1, which is one or more selected from the following:

5. The cement clinker contains belite as the calcium silicate, and the Al 2 O 3 2. The cement admixture according to claim 1, which is a fired product containing gehlenite as a contained mineral phase and which satisfies the following conditions (1) and (2): (1) The amount of the gehlenite is 10 to 100 parts by mass per 100 parts by mass of the belite. (2) The cement clinker does not contain an aluminate phase, or contains an aluminate phase in an amount of 15 parts by mass or less per 100 parts by mass of the belite.

6. A mixed cement comprising the cement admixture according to any one of claims 1 to 5 and cement, The mixed cement has a ratio of the cement admixture of 5 to 60 mass %.

7. A method for producing the cement admixture according to any one of claims 1 to 5, comprising: a first carbonation curing step of obtaining the cement admixture by carbonating and curing the coarsely crushed material obtained by crushing the cement clinker, or by carbonating and curing the pulverized material obtained by crushing the cement clinker; A method for producing a cement admixture comprising the steps of:

8. A method for producing the cement admixture according to any one of claims 1 to 5, comprising: a kneading step of kneading the pulverized material obtained by pulverizing the cement clinker with water to obtain a paste; a paste carbonation step of carbonating the paste to obtain a hardened paste; A grinding step of grinding the hardened body to obtain the cement admixture; A method for producing a cement admixture comprising the steps of:

9. The method for producing a cement admixture according to claim 8, further comprising a second carbonation curing step of carbonating and curing the cement admixture obtained in the grinding step.

Citation Information

Patent Citations

  • Fine powder cement

    JP2010254503A

  • Immobilization method of carbon dioxide

    JP2020131074A