Cellulose nanofiber manufacturing apparatus and method for manufacturing cellulose nanofiber

By employing a high-pressure homogenizer with specific stainless steel components and controlled flow velocity, the wear issues of downstream parts are mitigated, enhancing the longevity and efficiency of cellulose nanofiber production.

JP2024136432APending Publication Date: 2024-10-04NIPPON PAPER IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023047548
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

High-pressure homogenizers used for producing cellulose nanofibers experience rapid wear and breakdown due to fatigue failure and cavitation jets, necessitating frequent replacement of downstream piping components.

Method used

The use of a single-hole nozzle-type high-pressure homogenizer with downstream piping, fittings, and plugs made from stainless steel containing specific compositions of Cr, Ni, and optionally chromium molybdenum steel or titanium, along with surface treatments like solution heat treatment, precipitation hardening, or hard chrome plating, and controlling the average flow velocity in the downstream piping to less than 5.0 m/s.

Benefits of technology

This configuration extends the lifespan of downstream piping components by reducing wear, ensuring consistent production of high-quality cellulose nanofibers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024136432000001_ABST
    Figure 2024136432000001_ABST
Patent Text Reader

Abstract

To provide a cellulose nanofiber manufacturing apparatus capable of extending component life of a high-pressure homogenizer and a method for manufacturing a cellulose nanofiber.SOLUTION: A cellulose nanofiber manufacturing apparatus is equipped with a single-hole nozzle-type high-pressure homogenizer 2 that performs a micronization process on pulp fibers, and has a single-hole nozzle 4 and a downstream pipe equipped with a pipe 6, a joint 7, and a plug 8 that are arranged downstream of the single-hole nozzle, and the pipe, joint, plug, etc. are made of stainless steel containing 15.0 mass% to 17.5 mass% of Cr, 3.0 mass% to 5.0 mass% of Ni, and 3.0 mass% to 5.0 mass% of Cu, or chromium-molybdenum steel or titanium containing 0.9 mass% to 1.2 mass% of Cr and 0.25 mass% or less of Ni.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cellulose nanofiber production apparatus equipped with a high-pressure homogenizer and a cellulose nanofiber production method using the high-pressure homogenizer. [Background technology]

[0002] Nanotechnology, a technique for freely controlling matter in the nanometer range, that is, on the scale of atoms and molecules, is expected to give rise to a variety of convenient new materials and devices. In particular, nano-order fibers (nanofibers) have attracted a great deal of attention because making fibers as thin as possible gives rise to completely new physical properties not found in conventional fibers. It is expected that the application of nanofibers will lead to the realization of purification devices with high-performance filters that do not allow even the smallest foreign particles to pass through, increased strength of synthetic fibers, high-performance clothing, and increased efficiency of fuel cells.

[0003] Cellulose nanofibers are fibers with a nano-level fiber diameter of 1000 nm or less, and can generally be obtained by defibrating chemically modified cellulose fibers with the mechanical shear force of a high-pressure homogenizer. For example, a high-pressure homogenizer (Microfluidizer manufactured by Powrex Corporation) equipped with a Y-shaped interaction chamber (Y-shaped nozzle) has been used to defibrate the chemically modified cellulose fibers (see Non-Patent Document 1). [Prior art documents] [Non-patent literature]

[0004] [Non-Patent Document 1] POWREX Corporation Product information https: / / www.powrex.co.jp / microfluidizer Summary of the Invention [Problem to be solved by the invention]

[0005] However, when operating a high-pressure homogenizer, extremely high pressures are repeatedly applied, and it is known that parts can wear out and break in a short period of time due to metal fatigue failure and abrasion caused by cavitation jets, resulting in the problem of having to replace expensive parts frequently.

[0006] The present invention aims to provide a cellulose nanofiber production apparatus and a cellulose nanofiber production method that can extend the life of downstream piping components, consisting of piping, fittings, and plugs, arranged downstream of a single-hole nozzle when a highly durable single-hole nozzle is equipped as the fiber-defibrating nozzle of a high-pressure homogenizer. [Means for solving the problem]

[0007] The present invention provides the following (1) to (9). (1) A cellulose nanofiber production apparatus equipped with a single-hole nozzle-type high-pressure homogenizer that performs a micronization process on pulp fibers, comprising a single-hole nozzle and a downstream pipe equipped with piping, fittings, and plugs arranged downstream of the single-hole nozzle, wherein the downstream pipe equipped with the piping, fittings, and plugs is made of stainless steel containing 15.0% by mass or more and 17.5% by mass or less of Cr, 3.0% by mass or more and 5.0% by mass or less of Ni, and 3.0% by mass or more and 5.0% by mass or less of Cu, or chromium molybdenum steel or titanium containing 0.9% by mass or more and 1.2% by mass or less of Cr and 0.25% by mass or less of Ni. (2) The cellulose nanofiber production apparatus according to (1), wherein the piping, fittings, and plugs are subjected to a surface treatment. (3) The cellulose nanofiber production apparatus according to (2), characterized in that the surface treatment is solution heat treatment (heat treatment symbol S), precipitation hardening heat treatment (heat treatment symbol H), or hard chrome plating treatment. (4) The cellulose nanofiber production apparatus according to (1), wherein the inner diameter of the downstream pipe is 2.0 mm or more. (5) A cellulose nanofiber production apparatus equipped with a single-hole nozzle type high-pressure homogenizer that performs micronization of pulp fibers, the cellulose nanofiber production apparatus comprising a single-hole nozzle and a downstream pipe equipped with piping, fittings, and a plug that is arranged downstream of the single-hole nozzle, the inner diameter of the downstream pipe being 2.0 mm or more. (6) The cellulose nanofiber production apparatus according to (1) or (5), characterized in that the hole diameter φ of the single-hole nozzle is 0.1 mm or more and 0.8 mm or less. (7) A method for producing cellulose nanofibers, comprising a defibration step using a single-hole nozzle-type high-pressure homogenizer for finely refining pulp fibers, the high-pressure homogenizer having a single-hole nozzle and a downstream pipe equipped with pipes, joints, and plugs arranged downstream of the single-hole nozzle, wherein the pipes, joints, and plugs are made of stainless steel containing 15.0% by mass or more and 17.5% by mass or less of Cr, 3.0% by mass or more and 5.0% by mass or less of Ni, and 3.0% by mass or more and 5.0% by mass or less of Cu, or chromium-molybdenum steel or titanium containing 0.9% by mass or more and 1.2% by mass or less of Cr and 0.25% by mass or less of Ni. (8) The method for producing cellulose nanofibers according to (7), wherein the average flow velocity in the downstream pipe is less than 5.0 m / s. (9) A method for producing cellulose nanofibers, comprising a defibration step using a single-hole nozzle-type high-pressure homogenizer for finely refining pulp fibers, characterized in that the average flow velocity in a downstream pipe located downstream of the single-hole nozzle of the high-pressure homogenizer is less than 3.0 m / s. Effect of the Invention

[0008] According to the present invention, when a highly durable single-hole nozzle is equipped as the fiber-defibrating nozzle of a high-pressure homogenizer, a cellulose nanofiber production apparatus and a cellulose nanofiber production method can be provided that can extend the life of downstream piping components, including piping, fittings, and plugs, that are arranged downstream of the single-hole nozzle. [Brief description of the drawings]

[0009] [Figure 1] FIG. 2 is a diagram showing a configuration of a high-pressure homogenizer according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, a cellulose nanofiber production apparatus and a cellulose nanofiber production method according to an embodiment of the present invention will be described.

[0011] The cellulose nanofiber production apparatus according to the first embodiment of the present invention is a cellulose nanofiber production apparatus equipped with a single-hole nozzle-type high-pressure homogenizer 2 that performs a micronization process on pulp fibers, as shown in Figure 1, and has a single-hole nozzle (orifice) 4, a downstream pipe 6 arranged downstream of the single-hole nozzle 4, and a fitting 7 and a plug 8 attached to the downstream pipe 6, and the materials used for the downstream pipe 6, the fitting 7 and the plug 8 are stainless steel containing 15.0 mass% or more and 17.5 mass% or less of Cr, 3.0 mass% or more and 5.0 mass% or less of Ni, and 3.0 mass% or more and 5.0 mass% or less of Cu, or chromium molybdenum steel or titanium containing 0.9 mass% or more and 1.2 mass% or less of Cr and 0.25 mass% or less of Ni, respectively.

[0012] The single-hole nozzle 4 used in this single-hole nozzle type high-pressure homogenizer 2 has a hole diameter φ of 0.1 mm or more and 0.8 mm or less. The downstream pipe 6, joint 7, and plug 8 are subjected to surface treatment such as solution heat treatment (heat treatment symbol S), precipitation hardening heat treatment (heat treatment symbol H), or hard chrome plating. In the precipitation hardening heat treatment, all known heat treatments such as H900, H1025, H1075, and H1150 can be applied. In the cellulose nanofiber production method using this cellulose nanofiber production apparatus, the average flow velocity in the downstream pipe 6 of the high-pressure homogenizer 2 is less than 5.0 m / s.

[0013] According to this cellulose nanofiber production apparatus and cellulose nanofiber production method, the materials used for the downstream piping 6, fitting 7, and plug 8 are stainless steel containing 15.0 to 17.5 mass% Cr, 3.0 to 5.0 mass% Ni, and 3.0 to 5.0 mass% Cu, or chrome molybdenum steel or titanium containing 0.9 to 1.2 mass% Cr and 0.25 mass% Ni, and further, the downstream piping components have been subjected to surface treatment such as solution heat treatment (heat treatment symbol S), precipitation hardening heat treatment (heat treatment symbol H), or hard chrome plating. Therefore, even when the high-pressure homogenizer 2 is equipped with a single-hole nozzle 4 which has excellent durability, the amount of wear of the downstream piping 6, fitting 7, and plug 8 can be reduced, and the lifespan of the downstream piping 6, fitting 7, and plug 8 can be extended.

[0014] A cellulose nanofiber production apparatus according to a second embodiment of the present invention is a cellulose nanofiber production apparatus equipped with a single-hole nozzle type high-pressure homogenizer 2 that performs micronization of pulp fibers, similar to the cellulose nanofiber production apparatus according to the first embodiment shown in Fig. 1, and has a single-hole nozzle 4, a downstream pipe 6 arranged downstream of the single-hole nozzle 4, and a joint 7 and a plug 8 attached to the downstream pipe, and the inner diameter of the downstream pipe 6 is 2.0 mm or more and 100 mm or less, preferably 5.0 mm or more and 50 mm or less. In a cellulose nanofiber production method using this cellulose nanofiber production apparatus, the average flow velocity in the downstream pipe 6 of the high-pressure homogenizer 2 is less than 3.0 m / s.

[0015] According to this cellulose nanofiber production apparatus and cellulose nanofiber production method, the inner diameter of the downstream piping 6 is 2.0 mm or more and 100 mm or less, preferably 5.0 mm or more and 50 mm or less, and the average flow velocity in the downstream piping 6 is less than 3.0 m / s, so that even when the high-pressure homogenizer 2 is equipped with a single-hole nozzle 4 that has excellent durability, it is possible to reduce the amount of wear on the downstream piping 6, fitting 7, and plug 8, and to extend the lifespan of the downstream piping 6, fitting, and plug 8. Furthermore, by setting an upper limit on the inner diameter of the downstream piping 6, it is possible to suppress an increase in the amount of raw material remaining in the downstream piping 6 and prevent any effects on the quality of the cellulose nanofiber produced.

[0016] (Method of manufacturing cellulose nanofiber) The cellulose nanofiber production method of the present invention includes a defibration step in which a cellulose raw material is defibrated by applying a mechanical shear force using the high-pressure homogenizer according to the first or second embodiment. In the present invention, it is possible to use chemically modified cellulose as the cellulose raw material, and in that case, it is preferable to carry out a step of dehydrating and washing the dispersion of chemically modified cellulose and a step of adjusting the concentration of the dispersion of chemically modified cellulose before subjecting it to the defibration step.

[0017] (Cellulose nanofiber) Cellulose nanofibers are materials produced by finely breaking down plant fibers to the nano level, and are generally fine fibers with an average fiber diameter of about 3 to 500 nm and an average aspect ratio of 50 or more. The average fiber diameter and average fiber length of cellulose nanofibers can be obtained by averaging the fiber diameters and fiber lengths obtained from the observation of each fiber using a field emission scanning electron microscope (FE-SEM). The aspect ratio can be calculated using the following formula. Aspect ratio = average fiber length / average fiber diameter

[0018] (Cellulose raw material) In the present invention, the cellulose raw material refers to various forms of materials mainly composed of cellulose, and examples thereof include natural cellulose such as pulp (bleached or unbleached wood pulp, bleached or unbleached non-wood pulp, refined linters, pulp derived from herbs such as jute, Manila hemp, and kenaf), cellulose produced by microorganisms such as acetic acid bacteria, regenerated cellulose spun after dissolving cellulose in a solvent such as a cuprammonium solution or a morpholine derivative, and fine cellulose obtained by depolymerizing the cellulose raw material by subjecting the cellulose to hydrolysis, alkali hydrolysis, enzymatic decomposition, explosion treatment, mechanical treatment such as a vibrating ball mill, or the like.

[0019] In the present invention, when a sheet-like cellulose raw material is used, it is preferable to roughly crush it to a size of about 0.5 to 5 cm square. By roughly crushing it to the above size, the cellulose raw material can be efficiently and uniformly modified in the next reaction step. The method of roughly crushing is not particularly limited, but a single-shaft rotary shear type grinder, a double-shaft rotary shear type grinder, a multi-shaft screw type grinder, a shredder, a guillotine cutter, etc. can be used. Among these, the use of a single-shaft rotary shear type grinder or a shredder is preferable from the viewpoint of rough crushing.

[0020] Cellulose has three hydroxyl groups per glucose unit and can be chemically modified in various ways. In the present invention, a cellulose raw material obtained by chemical modification (chemically modified cellulose) may be used. Examples of chemical modifications include oxidation (carboxylation), carboxymethylation, cationization, and esterification. Among these, oxidation (carboxylation) and carboxymethylation are more preferred.

[0021] (Chemical modification of cellulose) (Oxidation) In the present invention, the oxidation of the cellulose raw material can be carried out using a known method and is not particularly limited, but it is preferable to adjust the amount of carboxyl groups to 0.5 mmol / g to 3.0 mmol / g relative to the bone dry mass of the cellulose nanofiber.

[0022] As an example, cellulose can be obtained by oxidizing it in water using an oxidizing agent in the presence of an N-oxyl compound and a compound selected from the group consisting of bromides, iodides, or a mixture thereof. This oxidation reaction selectively oxidizes the primary hydroxyl group at the C6 position of the glucopyranose ring on the cellulose surface, and a cellulose-based fiber having an aldehyde group and a carboxyl group or a carboxylate group on the surface can be obtained. The concentration of cellulose during the reaction is not particularly limited, but is preferably 5% by mass or less. The N-oxyl compound refers to a compound that can generate nitroxy radicals. Any compound can be used as the N-oxyl compound as long as it promotes the desired oxidation reaction.

[0023] The amount of the N-oxyl compound used is not particularly limited as long as it is a catalytic amount capable of oxidizing the raw cellulose. For example, the amount is preferably 0.01 to 10 mmol, more preferably 0.02 to 1 mmol, and even more preferably 0.05 to 0.5 mmol per 1 g of bone dry cellulose. The amount is preferably about 0.1 to 4 mmol / L relative to the reaction system.

[0024] Bromides are compounds containing bromine, examples of which include alkali metal bromides that can dissociate and ionize in water. Also, iodides are compounds containing iodine, examples of which include alkali metal iodides. The amount of bromide or iodide used can be selected within a range that can promote the oxidation reaction. The total amount of bromide and iodide is, for example, preferably 0.1 to 100 mmol, more preferably 0.1 to 10 mmol, and even more preferably 0.5 to 5 mmol, per 1 g of bone-dry cellulose.

[0025] The oxidizing agent may be a known one, such as halogen, hypohalous acid, halous acid, perhalogen acid or their salts, halogen oxide, peroxide, etc. Among them, sodium hypochlorite is preferable because it is inexpensive and has a low environmental impact. The appropriate amount of the oxidizing agent to be used is, for example, preferably 0.5 to 500 mmol, more preferably 0.7 to 50 mmol, even more preferably 1 to 25 mmol, and most preferably 3 to 10 mmol, per 1 g of bone-dry cellulose. Also, for example, 1 to 40 mol is preferable per 1 mol of the N-oxyl compound.

[0026] The cellulose oxidation process can proceed efficiently even under relatively mild conditions. Therefore, the reaction temperature is preferably 4 to 40°C, or may be room temperature of about 15 to 30°C. As the reaction proceeds, carboxyl groups are generated in the cellulose, and a decrease in the pH of the reaction solution is observed. In order to efficiently proceed with the oxidation reaction, it is preferable to add an alkaline solution such as an aqueous sodium hydroxide solution to maintain the pH of the reaction solution at about 8 to 12, preferably 10 to 11. The reaction medium is preferably water, because it is easy to handle and does not easily cause side reactions.

[0027] The reaction time in the oxidation reaction can be appropriately set according to the degree of progress of the oxidation, and is usually about 0.5 to 6 hours, for example, about 1 to 4 hours. The oxidation reaction may be carried out in two stages. For example, the oxidized cellulose obtained by filtering after the completion of the first stage reaction is oxidized again under the same or different reaction conditions, thereby enabling efficient oxidation without reaction inhibition by table salt produced as a by-product in the first stage reaction.

[0028] Another example of the carboxylation (oxidation) method is a method in which a cellulose raw material is oxidized by contacting it with an ozone-containing gas. This oxidation reaction oxidizes at least the hydroxyl groups at positions 2 and 6 of the glucopyranose ring, and decomposes the cellulose chain. The ozone concentration in the ozone-containing gas is 50 to 250 g / m 3 It is preferable that the thickness is 70 to 220 g / m 3It is more preferable that the ozone is added to the cellulose raw material in an amount of 0.1 to 30 parts by mass, and more preferably 5 to 30 parts by mass, based on 100 parts by mass of the solid content of the cellulose raw material. The ozone treatment temperature is preferably 0 to 50°C, and more preferably 20 to 50°C. The ozone treatment time is not particularly limited, but is about 1 to 360 minutes, and preferably about 30 to 300 minutes. When the ozone treatment conditions are within these ranges, it is possible to prevent cellulose from being excessively oxidized and decomposed, and the yield of oxidized cellulose is good. After the ozone treatment, an oxidizing agent may be used to perform a post-oxidation treatment. The oxidizing agent used in the post-oxidation treatment is not particularly limited, but examples thereof include chlorine-based compounds such as chlorine dioxide and sodium chlorite, oxygen, hydrogen peroxide, persulfuric acid, and peracetic acid. For example, these oxidizing agents are dissolved in a polar organic solvent such as water or alcohol to prepare an oxidizing agent solution, and the cellulose raw material is immersed in the solution to perform the post-oxidation treatment.

[0029] The amount of carboxyl groups, carboxylate groups, and aldehyde groups in the cellulose fiber can be adjusted by controlling the amount of oxidizing agent added and the reaction time. The amount of carboxyl groups can be measured, for example, by preparing 60 mL of a 0.5% by mass slurry (aqueous dispersion) of oxidized cellulose, adding a 0.1 M aqueous hydrochloric acid solution to adjust the pH to 2.5, then dropping a 0.05 N aqueous sodium hydroxide solution to measure the electrical conductivity until the pH reaches 11, and calculating the amount of carboxyl groups using the following formula from the amount of sodium hydroxide (a) consumed in the neutralization stage of the weak acid, where the change in electrical conductivity is gradual. Carboxyl group amount [mmol / g oxidized cellulose or cellulose nanofiber] = a (mL) x 0.05 / mass of oxidized cellulose (g)

[0030] (Carboxymethylation) In the present invention, the carboxymethylation of the cellulose raw material can be carried out using a known method, and is not particularly limited, but it is preferable to adjust the degree of carboxymethyl group substitution per anhydrous glucose unit of cellulose to 0.01 to 0.50. One example of the method is the following production method, but it may be synthesized by a conventionally known method or a commercially available product may be used. Cellulose is used as the raw material, and 3 to 20 times by mass of water and / or lower alcohol, specifically methanol, ethanol, N-propyl alcohol, isopropyl alcohol, N-butanol, isobutanol, tertiary butanol, etc., or a mixture of two or more of them is used as a solvent. The mixing ratio of the lower alcohol is 60 to 95% by mass. As the mercerizing agent, 0.5 to 20 times the moles of an alkali metal hydroxide, specifically sodium hydroxide or potassium hydroxide, per anhydrous glucose residue of the raw material is used. The starting material, solvent, and mercerizing agent are mixed, and a mercerization treatment is carried out at a reaction temperature of 0 to 70° C., preferably 10 to 60° C., for a reaction time of 15 minutes to 8 hours, preferably 30 minutes to 7 hours. Then, a carboxymethylating agent is added at 0.05 to 10.0 times the moles per glucose residue, and an etherification reaction is carried out at a reaction temperature of 30 to 90° C., preferably 40 to 80° C., for a reaction time of 30 minutes to 10 hours, preferably 1 hour to 4 hours.

[0031] The degree of carboxymethyl substitution per glucose unit can be measured, for example, by the following method. That is, 1) Approximately 2.0 g of carboxymethylated cellulose fiber (bone dry) is weighed out and placed in a 300 mL Erlenmeyer flask with a stopper. 2) 100 mL of a solution of 1000 mL of nitric acid methanol and 100 mL of special-grade concentrated nitric acid is added, and the mixture is shaken for 3 hours to convert carboxymethyl cellulose salt (carboxymethylated cellulose) into hydrogenated carboxymethylated cellulose. 3) 1.5 to 2.0 g of hydrogenated carboxymethylated cellulose (bone dry) is weighed out and placed in a 300 mL Erlenmeyer flask with a stopper. 4) The hydrogenated carboxymethylated cellulose is moistened with 15 mL of 80% methanol, 100 mL of 0.1 N NaOH is added, and the mixture is shaken at room temperature for 3 hours. 5) Using phenolphthalein as an indicator, 1.1 N H 2 SO 4Back-titrate the excess NaOH with 6) Calculate the degree of carboxymethyl substitution (DS) using the following formula. A = [(100 × F'-(0.1N H 2 SO 4 )(mL)×F)×0.1] / (absolute dry mass of hydrogenated carboxylated cellulose (g) DS = 0.162 x A / (1-0.058 x A) A: The amount of 1N NaOH required to neutralize 1 g of hydrogenated carboxymethyl cellulose (mL) F': 0.1N H 2 SO 4 Factor F: Factor of 0.1N NaOH

[0032] (cationization) In the present invention, the cationization of the cellulose raw material can be carried out using a known method, and the cationization can result in the cellulose molecule having, for example, ammonium, phosphonium, sulfonium, or a group having these ammonium, phosphonium, or sulfonium, but a group having ammonium is preferred, and a group containing quaternary ammonium is particularly preferred. The specific cationization method is not particularly limited, but as an example, a cationization agent such as glycidyl trimethyl ammonium chloride, 3-chloro-2 hydroxypropyl trialkyl ammonium hydride, or a halohydrin type thereof, and an alkali metal hydroxide (sodium hydroxide, potassium hydroxide, etc.) as a catalyst can be reacted with the cellulose raw material in the presence of water and / or an alcohol having 1 to 4 carbon atoms to obtain a cationically modified cellulose having a group containing quaternary ammonium.

[0033] In this method, the degree of cationic substitution per glucose unit of the cationically modified cellulose obtained can be adjusted by controlling the amount of the cationizing agent to be reacted and the composition ratio of water and / or alcohol having 1 to 4 carbon atoms. The degree of substitution here refers to the number of substituents introduced per unit structure (glucopyranose ring) constituting cellulose. In other words, it is defined as "the value obtained by dividing the number of moles of the introduced substituents by the total number of moles of hydroxyl groups in the glucopyranose ring." Pure cellulose has three substitutable hydroxyl groups per unit structure (glucopyranose ring), so the theoretical maximum value of the degree of substitution of the cellulose fiber of the present invention is 3 (the minimum value is 0).

[0034] In the present invention, the cationic substitution degree per glucose unit of the cationized cellulose is preferably 0.01 to 0.40. By introducing cationic substituents into cellulose, the celluloses are electrically repelled from each other. Therefore, cellulose into which cationic substituents have been introduced can be easily nanofibrillated. If the cationic substitution degree per glucose unit is less than 0.01, sufficient nanofibrillation cannot be achieved. On the other hand, if the cationic substitution degree per glucose unit is more than 0.40, the cellulose may swell or dissolve, making it impossible to maintain the fiber form, and may not be obtained as nanofibers.

[0035] The degree of cationic substitution per glucose unit can be calculated by the following formula after drying the sample (cationically modified cellulose) and measuring the nitrogen content with a total nitrogen analyzer TN-10 (Mitsubishi Chemical). The degree of substitution here refers to the average value of the number of moles of substituents per mole of anhydrous glucose unit. Degree of cation substitution = (162 x N) / (1-151.6 x N) N: Nitrogen content

[0036] (Esterification) The method for esterifying a cellulose raw material or defibrated cellulose fibers to obtain esterified cellulose fibers or esterified cellulose nanofibers is not particularly limited, but an example of the method is to react the cellulose raw material or defibrated cellulose fibers with compound A. Compound A will be described later.

[0037] Examples of methods for reacting compound A with the cellulose raw material or defibrated cellulose fibers include a method of mixing a powder or an aqueous solution of compound A with the cellulose raw material or defibrated cellulose fibers, a method of adding an aqueous solution of compound A to a slurry of the cellulose raw material or defibrated cellulose fibers, etc. Of these, the method of mixing an aqueous solution of compound A with the cellulose raw material or defibrated cellulose fibers or a slurry thereof is preferred because it increases the uniformity of the reaction and increases the efficiency of esterification.

[0038] Examples of compound A include phosphoric acid compounds (e.g., phosphoric acid, polyphosphoric acid), phosphorous acid, phosphonic acid, polyphosphonic acid, and esters thereof. Compound A may be in the form of a salt. Among the above, phosphoric acid compounds are preferred because they are low cost, easy to handle, and can be introduced into cellulose of a cellulose raw material (e.g., pulp fiber) to improve defibration efficiency. The phosphoric acid compound may be any compound having a phosphoric acid group, and examples thereof include phosphoric acid, sodium dihydrogen phosphate, disodium hydrogen phosphate, trisodium phosphate, sodium pyrophosphate, sodium metaphosphate, potassium dihydrogen phosphate, dipotassium hydrogen phosphate, tripotassium phosphate, potassium pyrophosphate, potassium metaphosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, triammonium phosphate, ammonium pyrophosphate, and ammonium metaphosphate. The phosphoric acid compounds used may be one type or a combination of two or more types. Among these, from the viewpoints of high efficiency of introduction of phosphate groups, ease of defibration in the defibration step described below, and ease of industrial application, phosphoric acid, sodium salts of phosphoric acid, potassium salts of phosphoric acid, and ammonium salts of phosphoric acid are preferred, sodium salts of phosphoric acid are more preferred, and sodium dihydrogen phosphate and disodium hydrogen phosphate are even more preferred. In addition, it is preferable to use an aqueous solution of a phosphoric acid compound in the esterification, since this increases the uniformity of the reaction and the efficiency of introduction of the phosphate group. The pH of the aqueous solution of the phosphoric acid compound is preferably 7 or less, since this increases the efficiency of introduction of the phosphate group. A pH of 3 to 7 is more preferred from the viewpoint of suppressing hydrolysis of the pulp fibers.

[0039] Examples of the esterification method include the following methods. Compound A is added to a suspension (for example, solid content concentration 0.1 to 10% by mass) of cellulose raw material or defibrated cellulose fiber while stirring to introduce phosphate groups into cellulose. When the cellulose raw material or defibrated cellulose fiber is 100 parts by mass, and compound A is a phosphoric acid compound, the amount of compound A added is preferably 0.2 parts by mass or more, more preferably 1 part by mass or more, in terms of phosphorus element amount. This can further improve the yield of esterified cellulose fiber or esterified cellulose nanofiber. The upper limit is preferably 500 parts by mass or less, more preferably 400 parts by mass or less. This can efficiently obtain a yield commensurate with the amount of compound A used. Therefore, 0.2 to 500 parts by mass is preferable, and 1 to 400 parts by mass is more preferable.

[0040] When compound A is reacted with the cellulose raw material or defibrated cellulose fibers, compound B may also be added to the reaction system. Examples of methods for adding compound B to the reaction system include adding compound B to a slurry of the cellulose raw material or defibrated cellulose fibers, an aqueous solution of compound A, or a slurry of the cellulose raw material or defibrated cellulose fibers and compound A.

[0041] Compound B is not particularly limited, but is preferably a basic compound, and is more preferably a nitrogen-containing compound that is basic. "Basic" usually means that an aqueous solution of compound B exhibits pink to red color in the presence of a phenolphthalein indicator, and / or that the pH of the aqueous solution of compound B is greater than 7. The nitrogen-containing compound that is basic is not particularly limited as long as it exhibits the effects of the present invention, but is preferably a compound having an amino group. Examples of compounds having an amino group include urea, methylamine, ethylamine, trimethylamine, triethylamine, monoethanolamine, diethanolamine, triethanolamine, pyridine, ethylenediamine, and hexamethylenediamine. Among these, urea is preferred because of its low cost and ease of handling. The amount of compound B added is preferably 2 to 1000 parts by mass, more preferably 100 to 700 parts by mass. The reaction temperature is preferably 0 to 95°C, more preferably 30 to 90°C. The reaction time is not particularly limited, but is usually about 1 to 600 minutes, and is preferably 30 to 480 minutes. When the esterification reaction conditions are within any of these ranges, it is possible to prevent the cellulose from being excessively esterified and becoming easily soluble, and it is possible to improve the yield of phosphated cellulose.

[0042] After reacting the cellulose raw material or defibrated cellulose fibers with compound A, a suspension of esterified cellulose fibers or esterified cellulose nanofibers is usually obtained. The suspension of esterified cellulose fibers or esterified cellulose nanofibers is dehydrated as necessary. It is preferable to carry out a heat treatment after dehydration. This can suppress hydrolysis of the cellulose raw material or defibrated cellulose fibers. The heating temperature is preferably 100 to 170°C, and it is more preferable to heat at 130°C or less (more preferably 110°C or less) while water is contained during the heat treatment, and then heat at 100 to 170°C after removing the water.

[0043] In phosphated cellulose, a phosphate group substituent is introduced into cellulose, and cellulose particles repel each other electrically. Therefore, phosphated cellulose fibers can be easily defibrated to cellulose nanofibers (defibration performed to obtain cellulose nanofibers is also called nanodefibration). The degree of phosphate substitution per glucose unit of phosphated cellulose fibers is preferably 0.001 or more. This allows sufficient defibration (e.g. nanodefibration) to be performed. The upper limit of the degree of phosphate substitution per glucose unit of phosphated cellulose fibers is preferably 0.40 or less. This can suppress swelling or dissolution of phosphated cellulose fibers, and can suppress the occurrence of a situation in which cellulose nanofibers cannot be obtained. Therefore, the degree of phosphate substitution per glucose unit of phosphated cellulose fibers is preferably 0.001 to 0.40. In addition, the degree of phosphate substitution per glucose unit of cellulose nanofibers modified by phosphate esterification (phosphated cellulose nanofibers) is preferably 0.001 or more. The upper limit is preferably 0.40 or less. Therefore, the degree of phosphate substitution per glucose unit of the phosphated cellulose nanofiber is preferably 0.001 to 0.40. It is preferable that the phosphated cellulose fiber is subjected to a washing treatment such as boiling and then washing with cold water. This allows efficient defibration.

[0044] The reaction tank used in the process of chemically modifying the cellulose raw material to obtain modified cellulose is not particularly limited, but examples include a tank equipped with stirring blades, a pulper, a kneader, a ribbon-type mixer, a screw-type mixer, etc. Among these, when the reaction is carried out at a raw material concentration of approximately 3% or less, it is preferable to use a tank or a pulper equipped with stirring blades that can stir liquids or liquid-like slurries. Furthermore, when the reaction is carried out under conditions where the raw material concentration exceeds approximately 3%, since the reactants are not in a liquid form but are solid, it is preferable to use a kneader, ribbon-type mixer, or screw-type mixer that can mix and stir them.

[0045] (Cleaning process) In the present invention, the obtained dispersion of chemically modified cellulose is subjected to a dehydration treatment and then washed with water, and this process makes it possible to obtain cellulose nanofibers with few impurities.

[0046] In this step, dehydration devices of the centrifugal separation type, vacuum dehydration type, and pressurized dehydration type can be used. Specifically, centrifugal separation type (Tanabe Willtec centrifuge, Kokusan centrifuge, etc.), vacuum dehydration type (drum type vacuum dehydrator, Tsukishima Kikai horizontal belt filter, etc.), pressurized dehydration type (filter press, tube press), centrifugal separation type (Tanabe Willtec centrifuge, Kokusan centrifuge, etc.), and vacuum dehydration type (drum type vacuum dehydrator, Tsukishima Kikai horizontal belt filter) are preferred, since they can perform dehydration without applying strong shear force to the dehydrated raw material. In addition, a combination of these types can also be used.

[0047] (Concentration adjustment process for chemically modified cellulose) In the present invention, in order to efficiently carry out the subsequent defibration step, it is preferable to adjust the concentration of the dispersion of chemically modified cellulose to 0.1% by mass to 10% by mass. If the concentration is less than 0.1% by mass, the presence of too little modified pulp will result in insufficient defibration. On the other hand, if the concentration exceeds 10% by mass, the viscosity of the modified pulp dispersion increases as defibration proceeds, making it impossible to apply sufficient force to the modified pulp, resulting in insufficient defibration.

[0048] (defibration process) In the present invention, the high-pressure homogenizer according to the first or second embodiment is used to defibrate the chemically modified cellulose. Defibration using a high-pressure homogenizer is performed by applying a pressure of 50 MPa or more to the aqueous dispersion and applying a strong shear force. The pressure applied is more preferably 100 MPa or more, and even more preferably 140 MPa or more. Furthermore, prior to defibration and dispersion treatment using the high-pressure homogenizer, the cellulose nanofibers can be subjected to a preliminary treatment, if necessary, using a known mixing, stirring, emulsifying, or dispersing device such as a high-speed shear mixer.

[0049] When defibrating by the above treatment, the solids concentration of the cellulose fiber raw material is 0.1% by mass or more, preferably 0.2% by mass or more, particularly 0.3% by mass or more, and 10% by mass or less, particularly 6% by mass or less. If the solids concentration is too low, the amount of liquid will be too large for the amount of cellulose fiber raw material to be treated, resulting in poor efficiency, and if the solids concentration is too high, the fluidity will be poor. EXAMPLES

[0050] (Wet atomization treatment to measure wear) When the high-pressure homogenizer had been operated a cumulative 1,000 times, the weight loss of the downstream member (plug) was measured as the degree of wear. Wear degree (weight loss degree, g / 1,000 shot) = plug mass before use (g / piece) - plug mass (g / piece) *The closer the wear level is to 0, the less wear there is and the longer the life.

[0051] [Example 1] (Production of cellulose nanofibers) Bleached unbeaten kraft pulp (85% brightness, bone dry state) derived from coniferous trees was added to an aqueous solution (100 ml of aqueous solution per 1 g of bone dry cellulose) in which TEMPO (Sigma Aldrich, 0.05 mmol per 1 g of bone dry cellulose) and sodium bromide (1.0 mmol per 1 g of bone dry cellulose) were dissolved, and the mixture was stirred until the pulp was uniformly dispersed. An aqueous solution of sodium hypochlorite was added to the reaction system so that the sodium hypochlorite concentration was 5.5 mmol / g, and the oxidation reaction was started at room temperature. The pH of the system decreased during the reaction, but 3M aqueous solution of sodium hydroxide was added successively to adjust the pH to 10. The reaction was terminated when the sodium hypochlorite was consumed and the pH of the system no longer changed.

[0052] The reaction mixture was filtered through a glass filter to separate the pulp, which was then thoroughly washed with water to obtain oxidized pulp (carboxylated cellulose). The pulp yield was 90%, the oxidation reaction took 90 minutes, and the amount of carboxyl groups was 1.4 mmol / g. Water was added to the reaction mixture to adjust the concentration to 3.0% by weight (w / v), and the mixture was treated 42 times with a high-pressure homogenizer (20°C, 150 MPa) to obtain an oxidized cellulose nanofiber dispersion.

[0053] The high-pressure homogenizer used had a downstream pipe made of SUS630s, with an inner diameter of φ3.18 mm and a length of 102 mm, downstream of a single-hole nozzle (nozzle diameter φ0.26 mm) that promotes atomization, followed by a 3 / 8 (inch) size tee and a plug made of SUS630s, with a flow path that bends at 90°. The material SUS630s is SUS630 that has been heat-treated to become a solid solution. The single-hole nozzle should be replaced after approximately 1 million shots.

[0054] The average velocity of the fluid passing through the downstream pipe located downstream of the single-hole nozzle was 3.5 m / s, and the average fiber diameter and average fiber length of the obtained cellulose nanofibers were 3.9 nm and 620 nm, respectively. The abrasion degree measured by abrasion degree measurement using wet atomization treatment was 2.1 mg. [Example 2] The high pressure homogenizer of Example 1 was changed to one using SUS630H900 as the material for the downstream pipe and plug. The material SUS630H900 was obtained by subjecting SUS630 to a solution heat treatment and then a precipitation hardening heat treatment. The degree of wear measured by a wet atomization treatment was 0.1 mg. [Example 3] The high-pressure homogenizer in Example 1 was changed to one in which titanium was used as the material for the downstream pipe and plug. The degree of wear measured by the wear measurement by wet atomization treatment was 0.1 mg. [Example 4] The high pressure homogenizer of Example 1 was changed to one using SUS630s+Cr as the material for the downstream pipe and plug. The material SUS630s+Cr was obtained by subjecting SUS630 to solution heat treatment and hard chrome plating. The degree of wear measured by the wear measurement after wet atomization treatment was 0.9 mg. [Example 5] The high pressure homogenizer of Example 1 was changed to one using SCM440Cr as the material for the downstream pipe and plug. The material SCM440Cr was obtained by applying hard chrome plating to SCM440. The degree of wear measured by the wear measurement by wet atomization treatment was 0.6 mg. [Example 6] The high-pressure homogenizer of Example 1 was modified to use SUS316 for the downstream piping and plug, with the tee plug size changed to 9 / 16 inch and the inner diameter of the downstream piping changed to 6.4 mm. The flow velocity in the piping was 0.9 m / s, and the degree of wear measured by abrasion measurement using wet atomization treatment was 1.1 mg. [Example 7] The high-pressure homogenizer of Example 1 was modified to use SUS630s for the downstream piping and plug, with the tee plug size changed to 9 / 16 inch and the inner diameter of the downstream piping changed to 6.4 mm. The flow velocity in the piping was 0.9 m / s, and the degree of wear measured by abrasion measurement using wet atomization treatment was 0.5 mg. [Example 8] The high-pressure homogenizer of Example 1 was modified to use SUS630H900 as the material for the downstream pipe and plug, with the tee plug size changed to 9 / 16 inch and the inner diameter of the downstream pipe changed to 6.4 mm. The flow velocity in the pipe was 0.9 m / s, and the degree of wear measured by the wear measurement by wet atomization treatment was 0.0 mg.

[0055] [Comparative Example 1] The high-pressure homogenizer in Example 1 was changed to one using SUS329-J4L as the material for the downstream pipe and plug. The degree of wear measured by the wear measurement by wet atomization treatment was 3.3 mg. [Comparative Example 2] The high-pressure homogenizer in Example 1 was changed to one using SUS316Cr as the material for the downstream pipe and plug. The degree of wear measured by the wear measurement after wet atomization treatment was 4.0 mg.

[0056] [Table 1]

[0057] It was shown that in Examples 1 to 8, the degree of wear measured by the wear measurement after wet atomization treatment was smaller than that in the comparative example, and the life of the plug was longer. [Explanation of symbols]

[0058] 2...High pressure homogenizer, 4...Single hole nozzle, 6...Downstream piping, 7...Fitting, 8...Plug

Claims

1. A cellulose nanofiber production apparatus equipped with a single-hole nozzle type high-pressure homogenizer for finely refining pulp fibers, A single-hole nozzle and a downstream pipe having a pipe, a joint, and a plug disposed downstream of the single-hole nozzle, The downstream piping including the piping, fittings, and plugs is made of stainless steel containing 15.0% by mass or more and 17.5% by mass or less of Cr, 3.0% by mass or more and 5.0% by mass or less of Ni, and 3.0% by mass or more and 5.0% by mass or less of Cu, or chromium-molybdenum steel containing 0.9% by mass or more and 1.2% by mass or less of Cr and 0.25% by mass or less of Ni, characterized in that the material used is titanium.

2. The cellulose nanofiber production apparatus according to claim 1, characterized in that the piping, the joints, and the plugs are surface-treated.

3. The cellulose nanofiber production apparatus according to claim 2, characterized in that the surface treatment is a solution heat treatment (heat treatment symbol S), a precipitation hardening heat treatment (heat treatment symbol H), or a hard chrome plating treatment.

4. The cellulose nanofiber production apparatus according to claim 1, characterized in that the inner diameter of the downstream piping is 2.0 mm or more.

5. A cellulose nanofiber production apparatus equipped with a single-hole nozzle type high-pressure homogenizer for finely refining pulp fibers, A single-hole nozzle and a downstream pipe having a pipe, a joint, and a plug disposed downstream of the single-hole nozzle, A cellulose nanofiber production apparatus, characterized in that the inner diameter of the downstream piping is 2.0 mm or more.

6. The cellulose nanofiber production apparatus according to claim 1 or claim 5, characterized in that the hole diameter φ of the single-hole nozzle is 0.1 mm or more and 0.8 mm or less.

7. A method for producing cellulose nanofibers, comprising a defibration step using a single-hole nozzle type high-pressure homogenizer for finely pulp fiber, The high pressure homogenizer has a single-hole nozzle and a downstream pipe having a pipe, a fitting, and a plug disposed downstream of the single-hole nozzle; A method for producing cellulose nanofibers, characterized in that the material used for the downstream piping including the piping, fittings, and plugs is stainless steel containing 15.0 to 17.5% by mass of Cr, 3.0 to 5.0% by mass of Ni, and 3.0 to 5.0% by mass of Cu, or chromium molybdenum steel or titanium containing 0.9 to 1.2% by mass of Cr and 0.25% by mass of Ni.

8. The method for producing cellulose nanofibers according to claim 7, characterized in that the average flow velocity in the downstream piping is less than 5.0 m / s.

9. A method for producing cellulose nanofibers, comprising a defibration step using a single-hole nozzle type high-pressure homogenizer for finely pulp fiber, A method for producing cellulose nanofibers, characterized in that the average flow velocity in a downstream pipe located downstream of the single-hole nozzle of the high-pressure homogenizer is less than 3.0 m / s.