Sustained-release coating composition
Cellulose acetate with a soluble plasticizer addresses manufacturing limitations of existing sustained-release membranes by allowing broader temperature ranges and eliminating curing, enhancing process flexibility and efficiency.
Patent Information
- Application Number
- JP2023048196
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-04
AI Technical Summary
Existing sustained-release membrane materials, such as ethyl cellulose and ethyl acrylate/methyl methacrylate copolymer, impose strict manufacturing process limitations due to temperature control requirements and particle adhesion issues, necessitating the use of lubricants like talc.
Employing cellulose acetate with a high melting point and a plasticizer soluble at 25°C, eliminating the need for a curing process and allowing a broader temperature range in the coating process, thus easing manufacturing restrictions.
The use of cellulose acetate with a soluble plasticizer enables the formation of sustained-release membranes without curing, expanding temperature tolerance and reducing the need for lubricants, thereby simplifying the manufacturing process.
Smart Images

Figure 2024136895000006 
Figure 2024136895000001 
Figure 2024136895000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a sustained-release coating composition, a sustained-release granule using the same, and a method for producing the sustained-release granule. [Background technology]
[0002] Formulations designed to adjust the dissolution rate of the active pharmaceutical ingredient (API) and ensure stable dissolution of the API for a long period of time are called sustained-release formulations. Sustained-release formulations are widely used because they have many advantages, such as reducing the number of times the drug is taken and stabilizing the blood concentration of the API. Sustained-release formulations are classified into matrix type and reservoir type based on the release control mechanism. Of these, reservoir-type sustained-release formulations have a structure in which tablets or granules containing the drug are coated with a sustained-release polymer film.
[0003] Ethyl cellulose is widely used as a material for the sustained release polymer coating in reservoir-type sustained release preparations. For example, Patent Document 1 discloses a method for producing a solid dosage form, which includes a step of coating a tablet or the like containing a drug with an aqueous dispersion containing a water-soluble pore-forming substance and ethyl cellulose, and then curing the tablet. Ethyl acrylate-methyl methacrylate copolymer is also used as a material for the sustained release polymer coating. For example, Patent Document 2 discloses the use of an aqueous dispersion containing ethyl acrylate-methyl methacrylate copolymer and talc as a material for the sustained release layer in a particulate composition. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2005-538105 A [Patent Document 2] JP 2018-8917 A Summary of the Invention [Problem to be solved by the invention]
[0005] When preparing a sustained-release film using a dispersion of ethyl cellulose, in order to impart sustained-release function to the film, a process of densifying the film by performing curing as described in Patent Document 1 is essential. However, since the curing conditions are directly related to the state of the film and thus the performance of sustained release, it is difficult to control the conditions such as temperature during curing to obtain the desired sustained release, and there is a problem that the restrictions on the manufacturing process are too strict. Although Patent Document 1 proposes some ideas to deal with this problem, the difficulty of controlling the conditions such as temperature during curing is an essential problem, so the restrictions on the manufacturing process are still strict.
[0006] In addition, when a sustained-release film is prepared using a dispersion containing ethyl acrylate-methyl methacrylate copolymer, the glass transition point of the polymer is extremely low, so the temperature must be kept low in the coating process to prevent adhesion of particles to each other due to melting of the film, which places strict limitations on the manufacturing process. Another limitation on the manufacturing process is the need to use a large amount of a lubricant or flow agent such as talc to prevent adhesion of particles to each other in the coating process, as shown in Patent Document 2.
[0007] As described above, the sustained-release film materials that have been used so far have a problem in that they have strict limitations on their manufacturing process. Therefore, an object of the present disclosure is to provide a sustained-release film material that can further relax the limitations on its manufacturing process. [Means for solving the problem]
[0008] The present inventors came up with the idea of selecting cellulose acetate, which has a high melting point, as a material for the sustained-release membrane. Cellulose acetate is well known as a material for semipermeable membranes, and is used as a coating agent for osmotic tablets by utilizing its unique property of semipermeability. However, cellulose acetate is used as a coating agent for osmotic tablets in the form of a solution dissolved in an organic solvent. Since organic solvents are volatile and inevitably involve manufacturing restrictions such as temperature control to ensure safety, cellulose acetate cannot be used in the same form as a coating agent for osmotic tablets for the above purpose.
[0009] As a result of extensive research, the present inventors have found that by using cellulose acetate together with a plasticizer that is soluble in cellulose acetate at 25°C, it is possible to impart the function of forming a sustained-release film, while eliminating the need for organic solvents and lubricants, eliminating the need for a curing process, and making it possible to expand the allowable temperature in the coating process, thereby significantly relaxing restrictions on the manufacturing process.
[0010] That is, the present disclosure provides the inventions of the following aspects. Item 1. A sustained-release coating composition for a granular drug, comprising cellulose acetate and mixed with a plasticizer when used, A sustained release coating composition, wherein the plasticizer is a plasticizer that can dissolve the cellulose acetate at 25°C. Item 2. A sustained-release coating composition for a granular drug, comprising cellulose acetate and a plasticizer capable of dissolving the cellulose acetate at 25°C. Item 3. The sustained-release coating composition according to Item 1 or 2, wherein the cellulose acetate is in the form of particles having an average particle size of 6 μm or less. Item 4. The sustained-release coating composition according to any one of Items 1 to 3, wherein the plasticizer is triacetin and / or triethyl citrate. Item 5. The sustained-release coating composition according to any one of Items 1 to 4, wherein the amount of the plasticizer is 10 parts by weight or more relative to 100 parts by weight of the total of the cellulose acetate and the plasticizer. Item 6. The sustained-release coating composition according to any one of Items 1 to 5, which is substantially free of organic solvents. Item 7. The sustained-release coating composition according to any one of Items 1 to 6, which is substantially free of a lubricant and / or a fluidizing agent. Item 8. The sustained release coating composition according to any one of Items 1 to 7, which is a water suspension. Item 9. A sustained-release granule comprising elementary granules containing an active ingredient and a sustained-release membrane coating the elementary granules, the sustained-release membrane being composed of a mixture containing a plasticizer in which cellulose acetate is soluble at 25°C and the cellulose acetate dissolved in the plasticizer. Item 10. A method for producing sustained-release granules, comprising a coating step of spraying the sustained-release coating composition according to any one of Items 2 to 8 onto uncoated granules containing an active ingredient, and not including a curing step. Item 11. The method according to item 10, wherein the coating step is carried out at 38 to 100° C. Effect of the Invention
[0011] According to the present disclosure, a sustained-release membrane material is provided that can reduce manufacturing restrictions. [Brief description of the drawings]
[0012] [Figure 1] 1 shows the results of testing the sustained release properties of the sustained release granules of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] 1. Sustained release coating composition The sustained-release coating composition of the present disclosure includes a sustained-release coating composition for granular drugs (hereinafter also referred to as "first sustained-release coating composition") that contains cellulose acetate and is mixed with a plasticizer (hereinafter also referred to as "predetermined plasticizer") that can dissolve the cellulose acetate at 25° C. when used, and a sustained-release coating composition for granular drugs (hereinafter also referred to as "second sustained-release coating composition") that contains cellulose acetate and a plasticizer that can dissolve the cellulose acetate at 25° C. Hereinafter, the first sustained-release coating composition and the second coating composition will be collectively referred to as "sustained-release coating composition".
[0014] 1-1.Cellulose acetate The sustained release coating composition of the present disclosure includes cellulose acetate. There is no particular limitation on the cellulose acetate that can be used in the present disclosure.
[0015] The acetyl group content of cellulose acetate is not particularly limited, but may be, for example, 29% or more, preferably 33% or more, more preferably 36% or more, and even more preferably 38% or more. The upper limit of the acetyl group residual content is not particularly limited, but may be, for example, 45% or less, preferably 42% or less, and more preferably 41% or less. The acetyl group content is a value measured by the acetyl group content quantitative method described in the "Content of Acetyl" section of the "Cellulose Acetate" section of the United States Pharmacopeia (USP) and National Formulary (NF) Compendium (hereinafter referred to as "USP-NF").
[0016] The degree of polymerization of cellulose acetate is not particularly limited, and the 6% viscosity is, for example, 80 mPa·s or more, preferably 85 mPa·s or more, and more preferably 87 mPa·s or more. The upper limit of the 6% viscosity is also not particularly limited, and for example, 300 mPa·s or less, preferably 200 mPa·s or less, more preferably 150 mPa·s or less, and even more preferably 100 mPa·s or less. The 6% viscosity is the viscosity of a 6 w / v% solution at 25°C.
[0017] The shape of cellulose acetate is not particularly limited, and any shape such as particulate, flake, fiber, etc. is acceptable. When particulate cellulose acetate is used, the size of the cellulose acetate particles is not particularly limited, but from the viewpoint of improving the sustained release property of the film, the average particle diameter is, for example, 6 μm or less, preferably 4 μm or less, more preferably 2 μm or less, even more preferably 1.5 μm or less, and even more preferably 1 μm or less. The average particle diameter is not particularly limited in its lower limit, but may be, for example, 0.05 μm or more, 0.1 μm or more, 0.2 μm or more, 0.3 μm or more, 0.4 μm or more, 0.5 μm or more, 0.6 μm or more, 0.7 μm or more, 0.8 μm or more, or 0.9 μm or more. In this specification, the average particle diameter is the particle diameter (D50) at 50% cumulative value in the particle size distribution obtained by the laser diffraction / scattering method.
[0018] The amount of cellulose acetate contained in the first sustained-release coating composition of the present disclosure can be determined according to the form at the time of use (i.e., the second sustained-release coating composition). The amount of cellulose acetate contained in the first sustained-release coating composition of the present disclosure is not particularly limited, but may be, for example, 0.5% by weight or more, preferably 1% by weight or more, more preferably 2% by weight or more, and even more preferably 2.5% by weight or more. The amount of cellulose acetate contained in the first sustained-release coating composition of the present disclosure is not particularly limited in its upper limit, but may be, for example, 20% by weight or less, preferably 10% by weight or less, more preferably 8% by weight or less, and even more preferably 7% by weight or less. The amount of cellulose acetate contained in the second sustained-release coating composition of the present disclosure is not particularly limited, but may be, for example, 0.5% by weight or more, preferably 1% by weight or more, more preferably 2% by weight or more, and even more preferably 2.5% by weight or more. The amount of cellulose acetate contained in the first sustained-release coating composition of the present disclosure is not particularly limited in its upper limit, but may be, for example, 15% by weight or less, preferably 7.5% by weight or less, and even more preferably 3.8% by weight or less.
[0019] 1-2.Prescribed plasticizers The first sustained-release coating composition of the present disclosure does not contain a specific plasticizer, but is mixed with a specific plasticizer when used. The second sustained-release coating composition of the present disclosure contains a specific plasticizer.
[0020] The predetermined plasticizer is a plasticizer that dissolves the cellulose acetate at 25°C. As such a plasticizer, any known pharmaceutical acceptable plasticizer can be used without any particular limitation. Specific examples of the predetermined plasticizer include triacetin and triethyl citrate. The predetermined plasticizer may be used alone or in combination of two or more kinds.
[0021] The amount of the predetermined plasticizer mixed in the first sustained-release coating composition of the present disclosure when used, and the amount of the predetermined plasticizer contained in the second sustained-release coating composition of the present disclosure can be appropriately set based on the content of cellulose acetate, the size of the cellulose acetate particles, and / or the desired degree of sustained release. For example, the amount of the predetermined plasticizer relative to the total of 100 parts by weight of cellulose acetate and the predetermined plasticizer is, for example, 10 parts by weight or more or 20 parts by weight or more, preferably 25 parts by weight or more, more preferably 30 parts by weight or more, even more preferably 35 parts by weight or more, even more preferably 40 parts by weight or more, even more preferably 43 parts by weight or more, 47 parts by weight or more, 50 parts by weight or more, or 53 parts by weight or more. The amount of the predetermined plasticizer is not particularly limited in its upper limit, and may be, for example, 70 parts by weight or less, 65 parts by weight or less, 60 parts by weight or less, or 57 parts by weight or less.
[0022] The specific amount of the specified plasticizer contained in the second sustained-release coating composition of the present disclosure is determined depending on the content of cellulose acetate and the ratio of the specified plasticizer, but is preferably 0.3 to 18 wt %, more preferably 0.7 to 13 wt %, and even more preferably 1 to 8 wt %.
[0023] 1-3.Other ingredients The sustained-release coating composition of the present disclosure may contain other components as appropriate within the scope of not impairing the effects of the present invention. Examples of other components include water, surfactants, preservatives, pH adjusters, thickeners, etc. These other components may be used alone or in combination.
[0024] The water content in the sustained release coating composition of the present disclosure is not particularly limited, and can be, for example, 60 to 99 wt%, preferably 70 to 98 wt%, more preferably 80 to 97.5 wt%, even more preferably 85 to 97 wt%, even more preferably 90 to 96.5 wt%, and even more preferably 92 to 96 wt%.
[0025] In addition, the sustained-release coating composition of the present disclosure does not completely exclude the inclusion of an organic solvent, a lubricant, and / or a fluidizing agent, but preferably does not substantially contain an organic solvent, a lubricant, and / or a fluidizing agent, and more preferably does not substantially contain both an organic solvent and a lubricant and / or a fluidizing agent. The organic solvent is a liquid organic compound having a boiling point of 150° C. or less (preferably 100° C. or less). "Substantially free of organic solvent" means that the content of the organic solvent is 0 to 1% by weight (preferably 0 to 0.1% by weight, more preferably 0% by weight). Examples of the lubricant and / or fluidizing agent include those commonly used in pharmaceuticals, such as talc, glycerin monostearate, magnesium stearate, calcium stearate, stearic acid, sucrose fatty acid ester, silicon dioxide, macrogol, etc. "Substantially free of lubricant and / or fluidizing agent" means that the total amount of the lubricant and the fluidizing agent is 0 to 1% by weight (preferably 0 to 0.1% by weight, more preferably 0% by weight).
[0026] 1-4.Form The specific form of the sustained release coating composition of the present disclosure is not particularly limited and can be appropriately determined depending on the blended components. Preferably, the sustained release coating composition of the present disclosure is in the form of an aqueous suspension.
[0027] 1-5.Applications The sustained-release coating composition of the present disclosure is used as a material for the sustained-release film of sustained-release granules. The first sustained-release coating composition is mixed with a specific plasticizer at the time of use to prepare a second sustained-release coating composition, which is then subjected to the manufacturing method described in "3. Manufacturing method of sustained-release granules". The second sustained-release coating composition is directly subjected to the manufacturing method described in "3. Manufacturing method of sustained-release granules".
[0028] 2.Sustained release granules The sustained-release granules of the present disclosure comprise elementary granules containing an active ingredient and a sustained-release membrane that coats the elementary granules, and are characterized in that the sustained-release membrane is composed of a mixture containing a plasticizer that dissolves cellulose acetate at 25°C and the cellulose acetate dissolved in the plasticizer.
[0029] The components of the elementary granules can be appropriately selected from active pharmaceutical ingredients (API) depending on the application. The active pharmaceutical ingredient may be any active ingredient that is blended into an oral drug and is desired to have a sustained action, such as vasodilators, antiplatelet drugs, antihypertensives, antiasthmatics (bronchodilators), antiemetics, cardiac stimulants, analgesics, anti-inflammatory drugs, antiulcer drugs, antineoplastic drugs, antirheumatic drugs, antibiotics, antidepressants, antipsychotics, antianxiety drugs, antiallergic drugs, and antiepileptic drugs. These active pharmaceutical ingredients may be used alone or in combination of two or more.
[0030] The size of the elementary granules is not particularly limited, but may be, for example, 100 μm or more, preferably 150 μm or more, more preferably 200 μm or more, even more preferably 250 μm or more, and even more preferably 300 μm or more in terms of average particle diameter (D50). The upper limit of the average particle diameter is also not particularly limited, but may be, for example, 800 μm or less, preferably 650 μm or less, and more preferably 500 μm or less.
[0031] The sustained-release film is composed of a mixture containing a specific plasticizer and the cellulose acetate dissolved in the specific plasticizer. In this sustained-release film, the cellulose acetate particles are impregnated with the plasticizer and are compatible and integrated, thereby bonding the particles together.
[0032] The thickness of the sustained release film may be appropriately determined according to the desired sustained release. The thickness of the sustained release film is, for example, 5 to 40 parts by weight, preferably 10 to 30 parts by weight, more preferably 15 to 25 parts by weight, and even more preferably 18 to 22 parts by weight, of the total amount of cellulose acetate and a predetermined plasticizer constituting the sustained release film, relative to 100 parts by weight of the elementary granules. The specific thickness of the sustained release film is, for example, 2 to 40 μm, preferably 3 to 25 μm, more preferably 5 to 20 μm, even more preferably 6 to 16 μm, and even more preferably 7 to 13 μm.
[0033] The pharmaceutical classification of the sustained-release granules of the present disclosure includes reservoir-type sustained-release granules, specifically pH-independent sustained-release granules and pH-dependent sustained-release granules. Among these, the preferred pharmaceutical classification of the sustained-release granules of the present disclosure is pH-independent sustained-release granules.
[0034] The sustained release granules of the present disclosure are prepared by the manufacturing method described in "3. Manufacturing method of sustained release granules".
[0035] 3. Manufacturing method of sustained release granules The method for producing sustained-release granules of the present disclosure is characterized in that it includes a coating step of spraying the second sustained-release coating composition described in "1. Sustained-release coating composition" above onto elementary granules containing an active ingredient to coat them, and does not include a curing step.
[0036] While the mechanism by which conventional sustained-release film materials, such as ethyl cellulose or ethyl acrylate-methyl methacrylate copolymer, form a sustained-release film is the melting of the resin material, the mechanism by which the second sustained-release coating composition described in "1. Sustained-release coating composition", which is the sustained-release film material in the manufacturing method of the present disclosure, forms a sustained-release film is the dissolution of cellulose acetate. Therefore, in the manufacturing method of the present disclosure, a sustained-release film can be formed without a curing step that melts the coated material, despite the high melting point of cellulose acetate.
[0037] As a specific method for the coating step, a typical wet coating method (also called a fluidized bed coating method) can be used.
[0038] Furthermore, in the manufacturing method of the present disclosure, since the melting point of cellulose acetate is high, the temperature conditions in the coating step are widely acceptable. Therefore, in the manufacturing method of the present disclosure, a relatively high temperature that was not acceptable in the coating of conventional sustained-release films is also acceptable. Specifically, the temperature conditions in the coating composition include, for example, 38 to 100°C, preferably 40 to 100°C, preferably 45 to 100°C, more preferably 50 to 100°C, 55 to 100°C, 60 to 100°C, 50 to 80°C, 50 to 70°C, or 50 to 75°C. The temperature can be set as the dry gas temperature in the wet coating method.
[0039] Conditions other than temperature in the coating step (for example, dry gas volume, spray speed, spray gas volume, etc.) can be appropriately determined depending on the size and amount of the elementary granules, etc.
[0040] Each feature disclosed herein may be combined with any other feature disclosed herein. EXAMPLES
[0041] The present invention will be described in more detail below with reference to examples, but each configuration and their combinations in each embodiment are merely examples, and addition, omission, substitution, and other modifications of the configurations are possible as appropriate within the scope of the present invention. The present disclosure is not limited by the embodiments, but is limited only by the scope of the claims.
[0042] [Test Example 1] (1) Cellulose acetate (1-1) Acetyl group content The acetyl group content of the cellulose acetate used in this test example was measured according to the method described in the quantitative method in USP-NF and was found to be 39.5%.
[0043] (1-2)6% viscosity The 6% viscosity of the cellulose acetate used in this test example was measured as follows and was found to be 89 mPa·s.
[0044] 3.00g of dry cellulose acetate and 39.90g of 95v / v% acetone aqueous solution were placed in an Erlenmeyer flask, sealed, and stirred for about 1.5 hours. Then, the flask was shaken for about 1 hour on a rotary shaker to completely dissolve the solution. The resulting 6w / v% solution was transferred to the designated mark of an Ostwald viscometer and allowed to warm to 25°C for about 15 minutes. The flow time between the time marks was measured, and the 6% viscosity was calculated using the following formula.
number
[0045] The viscometer coefficient was calculated from the following formula by measuring the flow time in the same manner as above using a standard solution for calibrating the viscometer.
number
[0046] (2) Preparation of the first sustained release coating composition (2-1) Example 1-1 Using a high-pressure homogenizer, the aqueous suspension containing cellulose acetate was treated 20 times at a treatment pressure of 50 MPaG, and then further treated 30 times at a treatment pressure of 150 MPaG. This resulted in a first sustained-release coating composition being obtained as an aqueous suspension (Example 1-1). The average particle size of the cellulose acetate (6% by weight) contained in this aqueous suspension (Example 1-1) was confirmed with a laser diffraction particle size distribution analyzer, and the D50 was 6 μm.
[0047] (2-2) Example 1-2 Using a bead mill (A-LABO), an aqueous suspension containing cellulose acetate was circulated under the conditions of a bead diameter of Φ0.8 mm and a peripheral speed of 8 m. As a result, a first sustained-release coating composition was obtained as an aqueous suspension (Example 1-2). The average particle diameter of the cellulose acetate (6 wt%) contained in this aqueous suspension (Example 1-2) was confirmed by a laser diffraction particle size distribution analyzer, and the D50 was 0.4 μm.
[0048] (3) Preparation of second sustained release coating composition (Examples 2-1 and 2-2) To the aqueous suspension of Example 1-1, an aqueous triacetin solution (6% by weight) was added so that the amount of triacetin was 55 parts by weight per 100 parts by weight of the total amount of cellulose acetate and triacetin, to obtain an aqueous suspension containing cellulose acetate and triacetin (Example 2-1). To the aqueous suspension of Example 1-2, the same ratio of triacetin was added, to obtain an aqueous suspension containing cellulose acetate and triacetin (Example 2-2). The amount of cellulose acetate in the aqueous suspensions (Examples 2-1 and 2-2) was 2.7% by weight, the amount of triacetin was 3.3% by weight, and the amount of water was 94% by weight.
[0049] (4) Preparation of sustained release granules (Examples 3-1 and 3-2) Acetaminophen (AAP) (product name: Pyretinol, Iwaki Pharmaceutical Co., Ltd.) was used as the API. The AAP was sieved through a 355 μm mesh sieve until 20% of the total amount passed through, and the remaining portion was used as the base granules.
[0050] 150 g of the raw granules were placed in a fluidized bed coating device (FL-LABO, Freund Corporation), and fluidized bed coating was performed by spraying each of the sustained release coating compositions of Example 2-1 and Example 2-2. The fluidized bed coating conditions were as follows.
[0051] [Table 1]
[0052] Coating was terminated when the total amount of cellulose acetate and triacetin in the sustained-release coating composition used reached 30 g (20 parts by weight per 100 parts by weight of the uncoated granules). In this way, sustained-release granules (Example 3-1) using the sustained-release coating composition of Example 2-1 and sustained-release granules (Example 3-2) using the sustained-release coating composition of Example 2-2 were obtained. The recovered sustained-release granules were sieved through a sieve with 1 mm openings, and the undersieve was subjected to a dissolution test.
[0053] (5) Dissolution test (sustained release test) The dissolution test was carried out according to the rotating basket method of the Japanese Pharmacopoeia. Purified water was used as the test liquid. The obtained dissolution rates are shown in Figure 1. In Figure 1, the results of AAP not coated with a sustained-release membrane are shown as Comparative Example 1.
[0054] As shown in Figure 1, the sustained release properties were confirmed for all sustained release granules (Examples 3-1 and 3-2). In addition, it was confirmed that the sustained release performance of the sustained release granules of Example 3-2 using cellulose acetate with an average particle size of 0.4 μm is significantly superior to that of the sustained release granules of Example 3-1 using cellulose acetate with an average particle size of 6 μm.
[0055] [Test Example 2] Sustained-release granules (Examples 4 and 5) were prepared and subjected to a dissolution test in the same manner as in Example 3-2 of Test Example 1, except that the amount of triacetin added to the sustained-release coating composition of Example 1-2 was changed as shown in Table 2. The dissolution rate (%) at a dissolution time of 60 minutes is shown in Table 2. Table 2 also shows the results of Example 3-2.
[0056] [Table 2]
[0057] As shown in Table 2, it was confirmed that the same sustained release properties were obtained for all sustained release granules.
[0058] [Reference example] (1) Preparation of the second sustained release coating composition Sustained-release coating compositions (Example 6 and Comparative Examples 2 and 3) were prepared in the same manner as in Example 2-2, except that the plasticizer added to the sustained-release coating composition of Example 1-2 (aqueous suspension of cellulose acetate) was changed to that shown in Table 3.
[0059] (2) Film formation evaluation 5 g of each sustained-release coating composition was dispensed into a glass petri dish and dried at 40° C. for 48 hours. The resulting dried product was visually observed and the degree of film formation was evaluated based on the following criteria. The results are shown in Table 3. ◯: The cellulose acetate particles are impregnated with the plasticizer and are compatible and integrated. Δ: The affinity between the cellulose acetate particles and the plasticizer is insufficient, so that the particles are not sufficiently integrated with each other. ×: The cellulose acetate particles and the plasticizer are separated, so that the particles are not integrated.
[0060] [Table 3]
[0061] As shown in Table 3, when a plasticizer capable of dissolving cellulose acetate at 25°C was used (Examples 2-2 and 2-6), a film was formed without curing. As shown in Test Examples 1 and 2, sustained release was confirmed in sustained-release granules in which elementary granules were coated with the sustained-release coating composition of Example 2-2, and therefore it can be reasonably assumed that the sustained-release coating composition of Example 6, which was formed into a film in the same manner as the sustained-release coating composition of Example 2-2, can also coat elementary granules with a sustained-release film. On the other hand, when a plasticizer incapable of dissolving cellulose acetate at 25°C was used (Comparative Examples 2 and 3), film formation was not possible, and therefore it was obvious that the elementary granules could not be coated with a sustained-release film.
Claims
1. A sustained release coating composition for a granular drug, comprising cellulose acetate, which is mixed with a plasticizer when used, A sustained release coating composition, wherein the plasticizer is a plasticizer that can dissolve the cellulose acetate at 25°C.
2. A sustained release coating composition for a granular drug, comprising cellulose acetate and a plasticizer capable of dissolving said cellulose acetate at 25°C.
3. 3. The sustained-release coating composition according to claim 1, wherein the cellulose acetate is in the form of particles having an average particle size of 6 μm or less.
4. 3. The sustained release coating composition according to claim 1 or 2, wherein the plasticizer is triacetin and / or triethyl citrate.
5. 3. The sustained-release coating composition according to claim 1, wherein the amount of the plasticizer is 10 parts by weight or more relative to 100 parts by weight of the total of the cellulose acetate and the plasticizer.
6. 3. The sustained release coating composition of claim 1 or 2, which is substantially free of organic solvents.
7. 3. The sustained release coating composition according to claim 1 or 2, which is substantially free of lubricants and / or flow agents.
8. The sustained release coating composition according to claim 1 or 2, which is an aqueous suspension.
9. The present invention comprises elementary granules containing an active ingredient and a sustained-release membrane that covers the elementary granules, The sustained-release granules, wherein the sustained-release film is composed of a mixture containing a plasticizer capable of dissolving cellulose acetate at 25°C and the cellulose acetate dissolved in the plasticizer.
10. A method for producing sustained-release granules, comprising a coating step of spraying the sustained-release coating composition according to claim 2 onto elementary granules containing an active ingredient, and not including a curing step.
11. The method according to claim 10, wherein the coating step is carried out at 38 to 100°C.
Citation Information
Patent Citations
Method for producing a solid dosage form coated with two layers consisting of a water-insoluble polymer and a water-soluble pore-forming substance
JP2005538105A
Intestinal release particulate composition
JP2018008917A