Gelling agent, liquid composition, and hydrogel

Cellulose oligomers with specific polymerization ranges interact with polysaccharides to form hydrogels, addressing the lack of effective hydrogel formation in existing technologies and providing stable, temperature-responsive gels for cell culture and drug delivery.

JP2024137125APending Publication Date: 2024-10-07TOKYO INST OF TECH +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023048520
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-07

AI Technical Summary

Technical Problem

Existing technologies do not effectively utilize cellulose oligomers to form hydrogels with polysaccharides, particularly in the context of cell culture media and drug delivery systems.

Method used

A gelling agent comprising cellulose oligomers with an average degree of polymerization of 5 to 20, which interacts with polysaccharides like hyaluronic acid to form hydrogels through neutralization with an acid, creating a crosslinked structure.

Benefits of technology

The solution enables the formation of stable hydrogels that can be used as scaffolds for cell culture and drug delivery systems, with temperature-responsive gelling properties and long-term stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137125000001_ABST
    Figure 2024137125000001_ABST
Patent Text Reader

Abstract

To provide a novel gelling agent and a gellable novel liquid composition and hydrogel using the same.SOLUTION: A gelling agent according to an embodiment is intended for gelling a polysaccharide such as hyaluronic acid, the gelling agent comprising a cellulose oligomer with an average degree of polymerization of 5-20 inclusive. A gellable liquid composition according to an embodiment comprises a cellulose oligomer with an average degree of polymerization of 5-20 inclusive, a polysaccharide, and water.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a gelling agent, a gellable liquid composition, and a hydrogel formed by gelling the liquid composition. [Background technology]

[0002] Gels are known that are formed by compositions that contain cellulose or its derivatives and polysaccharides such as hyaluronic acid.For example, Patent Document 1 discloses that an aqueous solution containing hyaluronic acid and carboxymethylcellulose with a pH of 3.5 or less is frozen and then thawed to produce a co-crosslinked gel composition that is made of hyaluronic acid and carboxymethylcellulose.

[0003] On the other hand, Patent Document 2 discloses the use of a cellulose oligomer having an average degree of polymerization of 5 to 20 as a medium additive added to a medium for culturing cells. The cellulose oligomer is an oligosaccharide having a structure in which glucose is linked by β-1,4-glycosidic bonds. Patent Document 2 discloses that the cellulose oligomer is added to suspend cells in the medium, and does not disclose gelation by combining the cellulose oligomer with a polysaccharide. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2003-019194 A [Patent Document 2] Patent Publication No. 2021-069339 Summary of the Invention [Problem to be solved by the invention]

[0005] In the course of investigating new applications of the above-mentioned cellulose oligomer, the present inventors discovered that the cellulose oligomer forms a hydrogel through interaction with a polysaccharide such as hyaluronic acid.

[0006] Embodiments of the present invention are based on the above findings, and have an object to provide a novel gelling agent capable of gelling polysaccharides, a gellable liquid composition containing a polysaccharide, and a hydrogel formed by gelling the liquid composition. [Means for solving the problem]

[0007] The present invention includes the embodiments set forth below. [1] A gelling agent for gelling a polysaccharide, comprising a cellulose oligomer having an average degree of polymerization of 5 or more and 20 or less. [2] A gellable liquid composition comprising a cellulose oligomer having an average degree of polymerization of 5 or more and 20 or less, a polysaccharide, and water. [3] The liquid composition according to [2], which is an alkaline aqueous solution containing the cellulose oligomer and the polysaccharide and can be gelled by neutralizing with an acid. [4] The liquid composition according to [2], wherein the cellulose oligomer is precipitated by neutralizing an alkaline aqueous solution containing the cellulose oligomer and the polysaccharide with an acid. [5] The liquid composition described in [2] or [3], wherein the polysaccharide is a non-cellulosic polysaccharide. [6] The liquid composition described in [2] or [3], wherein the polysaccharide is at least one type selected from the group consisting of glycosaminoglycans and water-soluble polysaccharides composed only of glucose and / or glucose derivatives polymerized by α-1,4-glycosidic bonds and α-1,6-glycosidic bonds. [7] The liquid composition according to any one of [2] to [6], wherein the cellulose oligomer is contained in an amount of 0.5 to 100 parts by mass per 100 parts by mass of the polysaccharide. [8] A hydrogel obtained by gelling the liquid composition described in any one of [2] to [7]. Effect of the Invention

[0008] According to embodiments of the present invention, it is possible to provide a novel gelling agent capable of gelling a polysaccharide, a gellable liquid composition containing a polysaccharide, and a hydrogel formed by gelling the liquid composition. [Brief description of the drawings]

[0009] [Figure 1] A conceptual diagram for explaining a presumed mechanism of gelation according to one embodiment. [Diagram 2] Photographs showing the state of Examples 1 to 3 and Comparative Examples 1 to 4 after 24 hours of inversion DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] [Gelling agent] The gelling agent according to the embodiment is a gelling agent for gelling polysaccharides, and contains a cellulose oligomer having an average degree of polymerization of 5-20.

[0011] Cellulose oligomers are oligosaccharides in which glucose units are linked by β-1,4-glycosidic bonds, and are also called cellooligosaccharides. Cellulose oligomers may have no substituents or may have a substituent at the anomeric position of the reducing end.

[0012] In this embodiment, the cellulose oligomer used has an average degree of polymerization (DP) (average number of glucose units present in one molecule) of 5 to 20. From the viewpoint of forming a more uniform gel, the average degree of polymerization (DP) is preferably 5 to 18, more preferably 6 to 15, even more preferably 6 to 10, and even more preferably 7 to 9. The average degree of polymerization of the cellulose oligomer is a weighted average value of the degrees of polymerization according to the mass ratio of the cellulose oligomer. The cellulose oligomer is usually a mixture of compounds having different degrees of polymerization, and may include, for example, one having a degree of polymerization of 4 to 20, one having a degree of polymerization of 5 to 18, or one having a degree of polymerization of 5 to 13.

[0013] As the cellulose oligomer, it is preferable to use a compound represented by the following general formula (1). [ka]

[0014] In formula (1), R represents a hydrogen atom or a substituent introduced in place of a hydrogen atom. The wavy line in the bond between the carbon at position 1 (anomeric carbon) of the reducing end and the OR group indicates that the configuration of the OR group is α, β, or a mixture of α and β. The configuration of the OR group is preferably β.

[0015] In formula (1), n ​​is the average degree of polymerization and is a number from 5 to 20. n is preferably 5 to 18, more preferably 6 to 15, even more preferably 6 to 10, and still more preferably 7 to 9.

[0016] The synthesis method of the cellulose oligomer is not particularly limited. For example, a method of reacting α-glucose-1-phosphate (hereinafter sometimes referred to as αG1P) with at least one primer selected from the group consisting of glucose, cellobiose and their derivatives with cellodextrin phosphorylase (hereinafter sometimes referred to as CDP) can be mentioned. This reaction is a synthesis method utilizing the reverse reaction of CDP, in which αG1P is used as a glucose donor, and at least one primer selected from the group consisting of glucose, cellobiose and their derivatives is used as a primer (i.e., glucose acceptor), and these are reacted with CDP, whereby αG1P is sequentially polymerized as a monomer with respect to the primer. Note that by replacing the hydrogen atom of the hydroxyl group at the anomeric position in the primer with a substituent, cellulose oligomers having various substituents can be synthesized.

[0017] The cellulose oligomer may be synthesized using CDP as described above and used as it is, or may be dissolved in an aqueous alkaline solution and used, or may be self-assembled.

[0018] The self-assembled cellulose oligomer can be prepared as follows. That is, an aqueous solution is prepared by dissolving the cellulose oligomer in an alkaline aqueous solution, and the obtained aqueous solution is neutralized with an acid. As a result, the cellulose oligomer becomes insoluble and precipitates, and at that time, the cellulose oligomer self-assembles by incubating with stirring, shaking, etc. or in a stationary state. That is, the molecules of the cellulose oligomer are aligned to form a cellulose oligomer assembly having a cellulose II type crystal structure. In one embodiment, the cellulose oligomer may be a cellulose oligomer assembly having a cellulose II type crystal structure, which contains a compound represented by formula (1) as a constituent component.

[0019] The cellulose oligomer assembly may have a sheet-like structure (cellulose nanosheet). Here, the sheet-like structure is a concept that includes a long and thin ribbon-like structure (cellulose nanoribbon).

[0020] In one embodiment, the gelling agent may be an aqueous dispersion of the cellulose oligomer. That is, the gelling agent may be a dispersion in which the cellulose oligomer aggregate is dispersed in water. Alternatively, in one embodiment, the gelling agent may be an aqueous solution in which the cellulose oligomer is dissolved in an alkaline aqueous solution. Alternatively, in one embodiment, the gelling agent may be in the form of a powder obtained by drying an aqueous dispersion or solution of the cellulose oligomer by freeze-drying or the like.

[0021] When the gelling agent is the above-mentioned aqueous dispersion, the content (concentration) of the cellulose oligomer is not particularly limited and is, for example, preferably 0.10 to 15% (w / v), more preferably 0.12 to 5.0% (w / v), and even more preferably 0.12 to 1.0% (w / v).

[0022] When the gelling agent is the above aqueous solution, the content (concentration) of the cellulose oligomer is not particularly limited, and is, for example, preferably 0.12 to 1.3% (w / v), more preferably 0.14 to 0.70% (w / v).

[0023] In this specification, "% (w / v)" refers to a mass volume percent concentration, which is the mass (g) of the subject substance contained in a volume of 100 mL.

[0024] The gelling agent may contain a cellulose oligomer and water as a dispersion medium or solvent, as well as various additives such as an alkali agent, a buffer agent, and an inorganic salt.

[0025] Examples of the alkaline agent include sodium hydroxide, potassium hydroxide, and lithium hydroxide.

[0026] Examples of the buffer include phosphate buffered saline (PBS), 2-morpholinoethanesulfonic acid (MES) buffer, trishydroxymethylaminomethane (Tris) buffer, 3-morpholinopropanesulfonic acid (MOPS) buffer, and 4-(2-hydroxyethyl)-1-piperazineethanesulfonic acid (HEPES) buffer.

[0027] Examples of inorganic salts include sodium chloride, potassium chloride, and lithium chloride.

[0028] The gelling agent is used to gel polysaccharides. As the polysaccharide, non-cellulosic polysaccharides are preferably used. More preferably, as the polysaccharide, there are (A) glycosaminoglycans and (B) water-soluble polysaccharides composed only of glucose and / or glucose derivatives polymerized by α-1,4-glycosidic bonds and α-1,6-glycosidic bonds, and any one of these may be used alone or in combination of two or more. Many of these are constituent polysaccharides of the extracellular matrix, and are preferably used in this embodiment.

[0029] The glycosaminoglycan (A) is a polysaccharide having an amino sugar in which the hydroxyl group of the sugar is replaced with an amino group. Examples of glycosaminoglycans include hyaluronic acid, chondroitin sulfate, heparin, keratan sulfate, and heparan sulfate.

[0030] The water-soluble polysaccharide (B) above is a polysaccharide having a structure in which glucose and / or glucose derivatives are polymerized via α-1,4-glycosidic bonds and α-1,6-glycosidic bonds, and examples thereof include dextran and its derivatives (e.g., carboxymethyldextran (CM-Dex)), pullulan, etc.

[0031] In this specification, the above-mentioned polysaccharides, when they have anionic groups, are a concept that also encompasses salts thereof such as sodium salts.

[0032] In one embodiment, the polysaccharide is preferably at least one selected from the group consisting of hyaluronic acid, chondroitin sulfate, heparin, carboxymethyldextran, and pullulan.

[0033] [Liquid composition] The liquid composition according to the embodiment contains the above-mentioned gelling agent, and is therefore a gellable liquid composition that contains a cellulose oligomer having an average degree of polymerization of 5 or more and 20 or less, a polysaccharide, and water.

[0034] In the liquid composition, the cellulose oligomer and the polysaccharide are as described above, and therefore a detailed description thereof will be omitted.

[0035] In the liquid composition, the content of the cellulose oligomer is preferably 0.5 to 100 parts by mass relative to 100 parts by mass of the polysaccharide. Since the cellulose oligomer is used as a gelling agent for gelling an aqueous solution of the polysaccharide, the content of the cellulose oligomer is preferably equal to or less than the content of the polysaccharide. The content of the cellulose oligomer is preferably 1 to 80 parts by mass relative to 100 parts by mass of the polysaccharide, more preferably 2 to 70 parts by mass, even more preferably 3 to 60 parts by mass, and even more preferably 4 to 50 parts by mass.

[0036] In one embodiment, when hyaluronic acid is used as the polysaccharide, the content of the cellulose oligomer is preferably 5 to 100 parts by mass, more preferably 8 to 80 parts by mass, even more preferably 10 to 60 parts by mass, and even more preferably 15 to 40 parts by mass, per 100 parts by mass of hyaluronic acid.

[0037] In the liquid composition, the content (concentration) of the cellulose oligomer is not particularly limited, and is, for example, preferably 0.10 to 1.0% (w / v), more preferably 0.12 to 0.50% (w / v), even more preferably 0.15 to 0.40% (w / v), even more preferably 0.18 to 0.35% (w / v), and even more preferably 0.20 to 0.30% (w / v).

[0038] In the liquid composition, the content (concentration) of the polysaccharide is not particularly limited, and may be, for example, 0.30 to 10.0% (w / v), 0.50 to 8.0% (w / v), 0.60 to 6.0% (w / v), or 0.80 to 5.0% (w / v). In one embodiment, when hyaluronic acid is used as the polysaccharide, the content (concentration) of hyaluronic acid in the liquid composition is not particularly limited, but is preferably 0.50 to 1.5% (w / v), more preferably 0.60 to 1.3% (w / v), and even more preferably 0.80 to 1.2% (w / v).

[0039] In the liquid composition, the cellulose oligomer may be contained in a form dissolved in an alkaline aqueous solution, or may be contained in a form dispersed in water as a cellulose oligomer aggregate.

[0040] For example, in one embodiment, the liquid composition may be an alkaline aqueous solution containing cellulose oligomers and polysaccharides, which can then be gelled by neutralizing with an acid.

[0041] In one embodiment, the liquid composition may contain a cellulose oligomer aggregate dispersed in water and a polysaccharide dissolved in water. In this case, the gellable liquid composition is obtained by precipitating the cellulose oligomer by neutralizing an alkaline aqueous solution containing the cellulose oligomer and the polysaccharide with an acid.

[0042] The liquid composition may contain, in addition to the cellulose oligomer, polysaccharide, and water, various additives such as an alkaline agent, a buffering agent, an inorganic salt, an organic low molecular weight compound, a protein, etc. The alkaline agent, the buffering agent, and the inorganic salt are as described above, and therefore the description thereof will be omitted.

[0043] [Hydrogel] The liquid composition can form a hydrogel by gelling. Therefore, the hydrogel according to the embodiment is formed by gelling the liquid composition. Therefore, the hydrogel contains the cellulose oligomer, the polysaccharide, and water, and may further contain various additives contained in the liquid composition. The contents of the cellulose oligomer and the polysaccharide in the hydrogel and the ratio of the two are as described above in the liquid composition, and therefore the explanation is omitted.

[0044] Here, the hydrogel refers to a dispersion in which water is the dispersion medium and has lost its fluidity and solidified. In detail, in the gelation evaluation test described later, if the dispersion does not flow down to the bottom of the vial at all after 10 minutes from the inversion of the vial, but is entirely retained at the top of the vial, it is judged that the dispersion has gelled (i.e., a hydrogel has been formed).

[0045] The liquid composition has a temperature responsive gelling ability, i.e., the liquid composition can be gelled (or can be caused to gel faster than in a low temperature environment) by heating, and can maintain the gel state even when subsequently cooled.

[0046] The hydrogel is formed by the interaction between the cellulose oligomer and the polysaccharide to form a complex. In detail, the cellulose oligomer is contained in the hydrogel as a cellulose oligomer aggregate formed by self-assembly, and it is considered that the aggregation of the cellulose oligomer aggregate functions as a crosslinking agent (physical crosslinking) that connects between the molecular chains of the polysaccharide.

[0047] As a method for forming a hydrogel, for example, a cellulose oligomer may be self-assembled to prepare an aqueous dispersion of cellulose oligomer aggregates, and then the aqueous dispersion may be mixed with a polysaccharide or an aqueous solution thereof. However, it is preferable to precipitate the cellulose oligomer by neutralizing an alkaline aqueous solution containing the cellulose oligomer and the polysaccharide with an acid. This allows a more uniform hydrogel to be formed.

[0048] FIG. 1 is a conceptual diagram showing a speculated mechanism of gelation according to one embodiment. Here, a case where an alkaline aqueous solution is neutralized to form a hydrogel will be described. An acid is added to an alkaline aqueous solution in which a cellulose oligomer and a polysaccharide are dissolved to neutralize (neutralize the pH). At this time, a buffering agent may be added to the acid. When the neutralized aqueous solution is placed in a high-temperature environment (e.g., 37°C) for a predetermined time (e.g., 24 hours), the fluidity of the aqueous solution is lost and a hydrogel is formed. In contrast, when the neutralized aqueous solution is placed in a low-temperature environment (e.g., 4°C) for a predetermined time (e.g., 24 hours), the aqueous solution maintains its fluidity and a sol is formed. Then, when the sol is placed in a high-temperature environment (e.g., 37°C) for a predetermined time (e.g., 24 hours), the fluidity is lost and a hydrogel is formed.

[0049] The mechanism of gelation is presumed to be as follows. By neutralizing the alkaline aqueous solution, the cellulose oligomer becomes insoluble and precipitates, and self-assembles to form a cellulose oligomer aggregate. At that time, since polysaccharides are present in the aqueous solution, as shown in Figure 1, an interaction occurs between the self-assembly of the cellulose oligomer and the molecular chains of the polysaccharide, and the cellulose oligomer aggregates aggregate in a high-temperature environment, and the aggregates act as cross-linking agents connecting the molecular chains of the polysaccharide. Therefore, a hydrogel with a three-dimensional network is formed by the molecular chains of the polysaccharide and the aggregates.

[0050] On the other hand, in a low-temperature environment, although interactions occur between the cellulose oligomer aggregates and the polysaccharide molecular chains, the cellulose oligomer aggregates do not aggregate (or the aggregation rate is so slow that sufficient aggregation to lose fluidity does not occur within a specified time), and it is believed that a sol with fluidity is formed. When the sol is placed in a high-temperature environment, it is believed that the aggregation of the cellulose oligomer aggregates is promoted, a cross-linked structure that connects the polysaccharide molecular chains is formed, and a hydrogel with a three-dimensional network is formed.

[0051] The temperature at which the liquid composition is gelled is not particularly limited, and may be, for example, 15° C. or higher, 20° C. or higher, or 25° C. or higher. The upper limit of the gelling temperature is also not particularly limited, and may be, for example, 60° C. or lower, or 50° C. or lower. The time period during which the liquid composition is gelled is not particularly limited, and may be 10 hours or longer, 15 hours or longer, or 18 hours or longer.

[0052] [Application] The uses of the hydrogel according to the embodiment are not particularly limited, and examples thereof include a scaffold for cell culture, and a drug delivery system for controlling the distribution of drugs or useful proteins in the body by placing them in the hydrogel. EXAMPLES

[0053] The present invention will be further explained below with reference to examples, but is not limited to these.

[0054] [Synthesis of cellulose oligomers] According to the method described in T. Serizawa et al., Polym. J., 2016, 48, 539-544 (using D-glucose as a primer), a cellulose oligomer (derived from glucose) with an average degree of polymerization of 9 (n = 9) was synthesized as shown in the following formula. Also, according to the method described in T. Serizawa et al., Langmuir, 2017, 33, 13415-13422 (using cellobiose as a primer), a cellulose oligomer (derived from cellobiose) with an average degree of polymerization of 7 (n = 7) was synthesized as shown in the following formula. [ka]

[0055] In detail, 200 mmol / L αG1P, 50 mmol / L D-glucose or cellobiose, and 0.2 U / mL cellodextrin phosphorylase (CDP) were mixed in 500 mmol / L 2-[4-(2-hydroxyethyl)-1-piperazinyl]ethanesulfonic acid (HEPES) buffer (pH 7.5) and incubated for 3 days at 60 ° C. The reaction solution containing the product was centrifuged (15000 rpm, 10 minutes or more, 4 ° C.), the supernatant was removed, and then ultrapure water was added to redisperse the product. The centrifugation (same conditions) was repeated until the replacement rate of the supernatant was 99.999% or more, and cellulose oligomers were obtained.

[0056] The average degree of polymerization of the product was measured by a proton nuclear magnetic resonance (NMR) device. The sample was prepared by dissolving 12 mg or more of the freeze-dried product in 600 μL of 4 mass% sodium deuterium hydroxide deuterium oxide solution. The NMR device used was an ADVANCE III HD500 (Bruker Biospin, magnetic field strength: 500 MHz, number of accumulations: 16). The average degree of polymerization was calculated based on the integral value of the protons at the anomeric positions (δ~5.1, 4.5) of the reducing end of the cellulose oligomer and the other anomeric positions (δ~4.3).

[0057] [Polysaccharide] The polysaccharides used in the examples are as follows: Hyaluronic acid: Nacalai Tesque CM-Dex: Tokyo Chemical Industry Co., Ltd. Chondroitin sulfate C sodium: manufactured by Nacalai Tesque Heparin sodium: manufactured by Nacalai Tesque

[0058] [Test Example 1: Examples 1 to 3, Comparative Examples 1 to 4] A 1 mL mighty vial was used as the container. A 1 mol / L NaOH aqueous solution in which cellulose oligomer and hyaluronic acid were dissolved was neutralized with a 1 mol / L HCl aqueous solution to prepare a 300 μL aqueous solution. At that time, a phosphate buffer component was added to the HCl aqueous solution so that the aqueous solution after neutralization became a phosphate buffered saline solution (PBS, [NaCl] 137 mmol / L). The concentrations of the cellulose oligomer and hyaluronic acid in the aqueous solution after neutralization were as shown in Table 1 below. The types of cellulose oligomers are as shown in Table 1. The obtained aqueous solution was left to stand in an atmosphere of 25°C for 24 hours, and then gelation evaluation was performed.

[0059] The gelation evaluation was carried out by inverting the vial after standing, and 10 minutes after inversion, if none of the aqueous solution (dispersion system) had flowed down to the bottom of the vial and was entirely retained at the top of the vial, it was judged that gelation had occurred. In Table 1, gelled samples are indicated as "gels" and non-gelled samples are indicated as "sols."

[0060] [Table 1]

[0061] The results are shown in Table 1. No gelation occurred in Comparative Example 1, which did not contain a cellulose oligomer. No gelation occurred in Comparative Examples 2 and 3, which did not contain hyaluronic acid, and Comparative Example 4. In contrast, gelation occurred in Examples 1 to 3, which used a combination of cellulose oligomer and hyaluronic acid, and a hydrogel was obtained in which the cellulose oligomer and hyaluronic acid were combined due to their interaction.

[0062] 2 is a photograph showing the state 24 hours after inversion, and the gel state was maintained without flowing even after 24 hours in Examples 1 to 3. When comparing the types of cellulose oligomer, Examples 1 and 2, which used a cellobiose-derived cellulose oligomer, formed a more transparent and uniform gel than Example 3, which used a glucose-derived cellulose oligomer.

[0063] [Test Example 2: Comparative Examples 5 and 6] In a 1 mL mighty vial, 300 μL of an aqueous solution was prepared by dissolving sodium carboxymethylcellulose (manufactured by Nacalai Tesque) and hyaluronic acid. At that time, the concentration of sodium carboxymethylcellulose in the aqueous solution was 0.20% (w / v) in Comparative Example 5, and 0.30% (w / v) in Comparative Example 6. The concentration of hyaluronic acid was 1.0% (w / v) in both Comparative Examples 5 and 6. The obtained aqueous solution was left to stand in an atmosphere of 25° C. for 24 hours, and then gelation evaluation was performed in the same manner as in Test Example 1.

[0064] As a result, in Comparative Examples 5 and 6, in which sodium carboxymethylcellulose was used instead of cellulose oligomer, the aqueous solution was observed to flow down 10 minutes after the vials were inverted after standing still, and no gelation occurred.

[0065] [Test Example 3: Examples 4 to 6] The concentration of hyaluronic acid in the aqueous solution after neutralization was set to 0.40% (w / v) in Example 4, 0.60% (w / v) in Example 5, and 0.80% (w / v) in Example 6, and the rest was the same as in Example 1 to obtain an aqueous solution after neutralization, and after standing for 24 hours in an atmosphere of 25°C, gelation evaluation was performed. As a result, in Examples 4 to 6, the aqueous solution did not flow down and gelled 10 minutes after the vial after standing was inverted. In addition, in Examples 4 to 6, the aqueous solution did not flow down even after 24 hours had passed since inversion, and the gel state was maintained.

[0066] [Test Example 4: Examples 7 to 9, Comparative Examples 7 to 12: Stationary Temperature Dependence] In a 1mL mighty vial, 1mol / L NaOH aqueous solution in which cellulose oligomer and hyaluronic acid were dissolved was neutralized with 1mol / L HCl aqueous solution to which phosphate buffer components were added, and 300μL of aqueous solution was prepared in which the aqueous solution after neutralization was phosphate buffered saline (PBS, [NaCl] 137mmol / L). At that time, the concentration of cellulose oligomer (derived from cellobiose) in the aqueous solution after neutralization was 0.20% (w / v), and the concentration of hyaluronic acid was 1.0% (w / v). The obtained aqueous solution was left for 24 hours in an atmosphere of 4°C in Example 7, in an atmosphere of 25°C in Example 8, and in an atmosphere of 37°C in Example 9, and then gelation evaluation was performed in the same manner as in Test Example 1.

[0067] In Comparative Examples 7 to 9, no cellulose oligomer was added, and otherwise the aqueous solutions were prepared in the same manner as in Examples 7 to 9. The obtained aqueous solutions were allowed to stand for 24 hours in an atmosphere of 4°C in Comparative Example 7, in an atmosphere of 25°C in Comparative Example 8, and in an atmosphere of 37°C in Comparative Example 9, and then a gelation evaluation was performed in the same manner as in Test Example 1.

[0068] In Comparative Examples 10 to 12, hyaluronic acid was not added, and otherwise aqueous solutions were prepared in the same manner as in Examples 7 to 9. The obtained aqueous solutions were allowed to stand for 24 hours in an atmosphere of 4°C in Comparative Example 10, in an atmosphere of 25°C in Comparative Example 11, and in an atmosphere of 37°C in Comparative Example 12, and then a gelation evaluation was performed in the same manner as in Test Example 1.

[0069] The results are shown in Table 2 below. Comparative Examples 7 to 9, which contained only hyaluronic acid without adding cellulose oligomer, did not gel when left at 4°C, 25°C, or 37°C. Similarly, Comparative Examples 10 to 12, which contained only cellulose oligomer without adding hyaluronic acid, did not gel when left at 4°C, 25°C, or 37°C. In contrast, when cellulose oligomer and hyaluronic acid were mixed, Example 7, which was left at 4°C, did not gel, but Examples 8 and 9, which were left at 25°C and 37°C, maintained a gel state not only 10 minutes after inversion but also 24 hours after inversion. This shows that gelation can be controlled by the temperature at which it is left. In addition, there was a tendency for the gel to become more opaque as the temperature at which it is left at rest increased. This suggests that the aggregation of cellulose oligomer aggregates may contribute to gelation.

[0070] The vial containing the sol of Example 7 that did not gel was placed upright and left to stand for 24 hours in an atmosphere at 37°C, after which a similar gelation evaluation was performed. The sol was gelled and the gel state was maintained even 24 hours after inversion. Furthermore, when the vial in this gel state was placed upright and left to stand for 24 hours in an atmosphere at 4°C, and then inverted, the gel state was maintained even 24 hours after inversion. Thus, it was found that the liquid product (sol) obtained by standing at 4°C was gelled by standing at 37°C. Moreover, after gelling in this way, it did not return to a liquid state even when returned to 4°C. In other words, it was found that the gel once formed was stable against temperature changes. This suggests that the cellulose oligomer aggregates that have aggregated once do not disperse even when the temperature is lowered. [Table 2]

[0071] [Test Example 5: Standing Time Dependence] A neutralized aqueous solution (hyaluronic acid concentration: 1.0% (w / v), cellulose oligomer (derived from cellobiose) concentration: 0.20% (w / v), NaCl concentration: 137 mmol / L (PBS condition)) was prepared in the same manner as in Example 1. The obtained neutralized aqueous solutions were allowed to stand in an atmosphere of 25°C for the standing times shown in Table 3 below, and gelation evaluation was performed in the same manner as in Test Example 1.

[0072] The results are shown in Table 3 below, and it was found that gelation occurred when left to stand for 18 hours or more in the formulation of Example 1. Since the time required for self-assembly of the cellulose oligomer is considered to be shorter, this supports the possibility that aggregation of cellulose oligomer aggregates contributes to gelation.

[0073] [Table 3]

[0074] [Test Example 6: Evaluation of hydrogel stability] A neutralized aqueous solution (hyaluronic acid concentration: 1.0% (w / v), cellulose oligomer (derived from cellobiose) concentration: 0.20% (w / v), NaCl concentration: 137 mmol / L (PBS condition)) was prepared in the same manner as in Example 1 above, and the obtained neutralized aqueous solution was left to stand for 24 hours in an atmosphere of 25 ° C. to prepare the hydrogel of Example 10. In addition, the cellulose oligomer concentration was set to 1.0% (w / v), and the rest was the same as in Example 10 to prepare the hydrogel of Example 11. Next, 600 μL of ultrapure water was injected into each vial of Examples 10 and 11, and a layer of ultrapure water was formed on each hydrogel, and then the vials were left to stand in an atmosphere of 25 ° C., and the state of the hydrogel was observed from immediately after the start of the standing until 60 days had passed.

[0075] As a result, in both Examples 10 and 11, the hydrogel maintained a gel state for at least two months after the addition of ultrapure water. In Example 11, in which the cellulose oligomer concentration was 1.0% (w / v), the hydrogel was observed floating up in the vial about six days after the start of standing. This suggested that in Example 11, the salt inside was flowing out due to osmotic pressure. However, the shape of the hydrogel itself was maintained without change. Therefore, it was suggested that the hydrogels of Examples 10 and 11 were stable in ultrapure water, and that a network structure strong enough not to collapse when immersed in ultrapure water was constructed.

[0076] [Test Example 7: Example 12: Low-temperature long-term standing] A neutralized aqueous solution (hyaluronic acid concentration: 1.0% (w / v), cellulose oligomer (derived from cellobiose) concentration: 0.20% (w / v), NaCl concentration: 137 mmol / L (PBS condition)) was prepared in the same manner as in Example 7 above, and the obtained neutralized aqueous solution was left standing for 24 hours in an atmosphere at 4 ° C. When this was inverted and inverted, the aqueous solution flowed down and did not gel. After leaving it standing for 24 hours at 4 ° C. while inverted, the aqueous solution accumulated in the mouth of the vial was dropped, and the vial was placed in an upright position again and left standing in an atmosphere at 4 ° C. Then, it was observed that it became cloudy when it was left standing for a total of 2 weeks after neutralization. Therefore, when this was inverted and gelation evaluation was performed, it was gelled after 10 minutes without flowing down. When it was further left standing for 24 hours at 25 ° C. while inverted, the gel state was maintained even after 24 hours had passed. This indicates that gelation occurs when the standing time is extended, even when the solution is left at 4°C. This is thought to be because it takes a long time for the cellulose oligomer aggregates to aggregate in a low-temperature environment of 4°C.

[0077] [Test Example 8: Examples 13 to 17 and Comparative Examples 13 to 15] According to Table 4 below, instead of hyaluronic acid 1.0% (w / v), CM-Dex, chondroitin sulfate C sodium, and heparin sodium were used at a concentration of 5.0% (w / v), and the concentration of cellulose oligomer (derived from cellobiose) was as shown in Table 4. The rest of the procedure was the same as in Test Example 1, and a neutralized aqueous solution was prepared. The obtained aqueous solution was allowed to stand in an atmosphere of 25°C for 24 hours, and then a gelation evaluation was performed.

[0078] The results are shown in Table 4. When CM-Dex, sodium chondroitin sulfate C, or sodium heparin was used as the polysaccharide, gelation did not occur in Comparative Examples 13 to 15, which did not contain a cellulose oligomer. In contrast, in Examples 13 to 17, which contained a cellulose oligomer along with these polysaccharides, the aqueous solution did not flow off and gelled 10 minutes after inversion.

[0079] [Table 4]

[0080] In addition, the various numerical ranges described in the specification can be arbitrarily combined with their upper and lower limits, and all such combinations are considered to be preferred numerical ranges described in the specification. In addition, a numerical range described as "X to Y" means from X to Y.

[0081] Although several embodiments of the present invention have been described above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the gist of the invention. These embodiments and their omissions, substitutions, modifications, etc. are included in the scope and gist of the invention as well as the invention and its equivalents described in the claims.

Claims

1. A gelling agent for gelling a polysaccharide, comprising a cellulose oligomer having an average degree of polymerization of 5 or more and 20 or less.

2. A gellable liquid composition comprising a cellulose oligomer having an average degree of polymerization of 5 or more and 20 or less, a polysaccharide, and water.

3. The liquid composition according to claim 2 , which is an alkaline aqueous solution containing the cellulose oligomer and the polysaccharide and can be gelled by neutralizing with an acid.

4. The liquid composition according to claim 2 , wherein the cellulose oligomer is precipitated by neutralizing an alkaline aqueous solution containing the cellulose oligomer and the polysaccharide with an acid.

5. The liquid composition of claim 2 , wherein the polysaccharide is a non-cellulosic polysaccharide.

6. 3. The liquid composition according to claim 2, wherein the polysaccharide is at least one selected from the group consisting of glycosaminoglycans and water-soluble polysaccharides composed only of glucose and / or glucose derivatives polymerized through α-1,4-glycosidic bonds and α-1,6-glycosidic bonds.

7. The liquid composition according to claim 2, comprising 0.5 to 100 parts by mass of the cellulose oligomer per 100 parts by mass of the polysaccharide.

8. A hydrogel formed by gelling the liquid composition according to any one of claims 2 to 7.

Citation Information

Patent Citations

  • Co-crosslinked gel composition comprising hyaluronic acid and carboxymethyl cellulose

    JP2003019194A

  • Medium additive for suspension culture, medium composition and culture method

    JP2021069339A