High strength steel member and manufacturing method thereof

The high-strength steel member with a Zn-based plating layer and controlled Fe-Zn alloy thickness addresses appearance corrosion and weld cracking issues, enhancing durability in corrosive environments.

JP2024137398AActive Publication Date: 2024-10-07JFE STEEL CORP

Patent Information

Application Number
JP2023048909
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-07
Estimated Expiration
2043-03-24

AI Technical Summary

Technical Problem

Conventional hot-pressed steel members using Al-based or Zn-based plated steel sheets face issues with insufficient appearance corrosion resistance and a high risk of resistance weld cracking, along with a potential for delayed fracture in corrosive environments.

Method used

A high-strength steel member with a Zn-based plating layer on its surface, controlled Fe-Zn alloy layer thickness, and a natural immersion potential of -1100 to -800 mV, combined with optional Fe-Al alloy and oxide management, to enhance corrosion resistance and reduce weld cracking.

Benefits of technology

The solution provides excellent appearance corrosion resistance, low risk of resistance weld cracking, and reduced risk of delayed fracture, ensuring durability in corrosive environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137398000001
    Figure 2024137398000001
  • Figure 2024137398000002
    Figure 2024137398000002
Patent Text Reader

Abstract

To provide a high strength steel member excellent in appearance corrosion resistance and resistance welding crack characteristics and with a little risk of delayed fracture in a corrosive environment.SOLUTION: A high strength steel member comprises a hot-pressed member and a Zn-based plating layer on at least one surface of the hot-pressed member. A thickness of an Fe-Zn alloy layer between the hot-pressed member and the Zn-based plating layer is 0 to 1.0 μm. Natural immersion potential in 0.5 mass% NaCl aqueous solution air-saturated at 25°C is -1100 to -800 mV in silver- silver chloride-saturated potassium chloride electrode standard, and Vickers hardness is 400 or above.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a high-strength steel member, in particular to a high-strength steel member having excellent appearance corrosion resistance and resistance weld cracking properties and a low risk of delayed fracture in a corrosive environment, and to a method for manufacturing the high-strength steel member. [Background technology]

[0002] In recent years, the use of high-strength steel sheets has been increasing in the automotive industry, as the demand for lighter weight steel sheets has increased while improving their performance. However, as the strength of steel sheets increases, press formability generally decreases, making it difficult to produce complex part shapes.

[0003] In light of this, the use of hot pressing technology, which forms steel hot rather than cold, is increasing. Hot pressing is a forming method in which steel sheets are heated to the austenite single phase temperature range (around 900°C), then pressed while still at high temperature, and then rapidly cooled (quenched) by contact with a die. Press forming is performed in the heated and softened state, and then the strength is increased by quenching, so hot pressing makes it possible to manufacture components with high strength while ensuring press formability. In addition, since hot press forming generates almost no residual stress in the processed area, the risk of delayed fracture due to corrosion is significantly smaller than that of cold press formed products of the same strength.

[0004] On the other hand, automotive components are also required to have high corrosion resistance. The corrosion resistance required for automotive components can be broadly divided into corrosion resistance against perforation corrosion (perforation corrosion resistance) and corrosion resistance against appearance corrosion (appearance corrosion resistance). Perforation corrosion is, as the name suggests, corrosion that forms through holes in the steel material that constitutes the component. On the other hand, appearance corrosion is corrosion that impairs the appearance, such as the generation of red rust or paint blistering due to corrosion.

[0005] In the field of hot pressing, it is common to use Al-based plated steel sheets to impart rust resistance to hot pressed parts. By using Al-based plated steel sheets as the material, the puncture corrosion resistance of the hot pressed parts is significantly improved.

[0006] However, hot-pressed members obtained using general Al-plated steel sheets have a problem that, although they have excellent perforation corrosion resistance, they have poor appearance corrosion resistance. That is, hot-pressed members obtained by hot-pressing Al-plated steel sheets have an intermetallic compound phase and a diffusion layer on the surface, mainly consisting of Al, which is a constituent component of the plating, and Fe diffused from the base steel sheet. However, these phases have a small potential difference with the base material (steel), so they have a small anodic corrosion protection effect on the base material. Therefore, in places such as cut edges where there is no plating layer and the upper coating film is thin, the base material corrodes early and red rust occurs. In addition, since the intermetallic compound itself contains a high concentration of Fe, red rust may occur even during the anodic protection process regardless of whether the base material is corroded or not.

[0007] As described above, conventional hot-pressed members using general Al-based plated steel sheets have excellent perforation corrosion resistance, but their appearance corrosion resistance is insufficient compared to pressed members manufactured by cold pressing zinc-based plated steel sheets.

[0008] One of the reasons for the insufficient appearance corrosion resistance is poor chemical conversion treatability. That is, in the manufacture of general automotive parts, hot-pressed parts are subjected to zinc phosphate-based chemical conversion treatment as a base treatment, and then painted. Since a chemically stable Al oxide film is formed on the outermost surface of the Al-plated steel sheet after hot pressing, almost no zinc phosphate-based chemical conversion film is formed during the chemical conversion treatment.

[0009] Against this background, various technologies have been proposed to improve various properties, such as the appearance and corrosion resistance, of hot-pressed members using Al-based plated steel sheets.

[0010] For example, Patent Document 1 proposes a technique of using a plated steel sheet having an Al plating layer and a surface coating layer containing ZnO formed on the Al plating layer as a steel sheet for hot pressing.

[0011] Moreover, Patent Document 2 proposes a method in which a plated steel sheet having an Al-based plating layer is heated in an atmosphere in which the hydrogen concentration and dew point are controlled, and then hot-pressed. [Prior art documents] [Patent documents]

[0012] [Patent Document 1] International Publication No. 2009 / 131233 [Patent Document 2] JP 2006-051543 A Summary of the Invention [Problem to be solved by the invention]

[0013] However, as a result of the inventors' investigations, it was found that the conventional techniques proposed in the above Patent Documents 1 and 2 still provide insufficient appearance corrosion resistance at the painted end faces of hot-pressed members.

[0014] For example, Patent Document 1 reports that forming a coating containing ZnO, a wurtzite compound, improves post-painting corrosion resistance. However, in Patent Document 1, the post-painting corrosion resistance is evaluated based only on the width of the paint blister, and the occurrence of red rust is not taken into consideration. In actual automotive parts, it is required to suppress not only paint blistering but also the occurrence of red rust, which greatly affects the appearance. With the technology of Patent Document 1, the paint blistering is suppressed as a result of improving the chemical conversion treatability, but the red rust resistance is not sufficient.

[0015] On the other hand, as described in Patent Document 1, Zn-based plated steel sheets may be used as steel sheets for hot pressing. When Zn-based plated steel sheets are subjected to hot pressing, Zn in the plated layer and Fe in the base material are mutually diffused during the heating process, and an intermetallic compound phase or solid solution phase containing Zn and Fe is formed in the surface layer of the member. In this case, by adjusting the heating conditions, an intermetallic compound phase containing a high concentration of Zn can be formed on the outermost surface of the member. The hot-pressed member obtained in this manner has the same level of corrosion resistance as that obtained by cold pressing a galvannealed steel sheet.

[0016] However, since the intermetallic compound phase inevitably contains Fe, the Fe may corrode and cause a corroded appearance with red rust mixed in. Therefore, the hot-pressed member obtained by hot pressing the Zn-based plated steel sheet does not have sufficient external corrosion resistance compared to an electrogalvanized steel sheet and a hot-dip galvanized steel sheet that is not subjected to an alloying treatment.

[0017] Even when using Zn-based plated steel sheets, the appearance corrosion resistance can be improved to some extent by adjusting the heating conditions. For example, if the temperature is raised in a short time and the holding time at high temperature is very short, the Zn-rich phase that does not contain Fe remains, improving the appearance corrosion resistance.

[0018] However, when hot pressing is performed while the Zn-rich phase that does not contain Fe remains as described above, the risk of liquid metal embrittlement (LME) cracking increases significantly, so it is not realistic to adopt the heating conditions described above when hot pressing Zn-based coated steel sheets.

[0019] Furthermore, as a result of the inventors' investigations, it was found that when an intermetallic compound phase or solid solution phase containing Zn and Fe is present in the surface layer of a component, especially directly on the base steel sheet, cracks are likely to occur in the resistance weld. Although the detailed mechanism is unclear, it is speculated that Zn melted or vaporized during the rapid heating process during resistance welding acts on the base material, causing a phenomenon similar to liquid metal embrittlement.

[0020] As described above, it is difficult to achieve both excellent corrosion resistance and prevention of liquid metal embrittlement cracking during forming in hot-pressed members using Zn-based plated steel sheets. In addition, hot-pressed members using Zn-based plated steel sheets have a high risk of resistance weld cracking.

[0021] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide a high-strength steel member which has excellent appearance corrosion resistance, a low risk of resistance weld cracking, and a low risk of delayed fracture in a corrosive environment. [Means for solving the problem]

[0022] The present invention has been made to solve the above problems, and the gist of the present invention is as follows.

[0023] 1. A high-strength steel component having a hot-pressed component and a Zn-based plating layer on at least one surface of the hot-pressed component, the thickness of the Fe-Zn alloy layer between the hot press member and the Zn-based plating layer is 0 to 1.0 μm; The natural immersion potential in an air-saturated 0.5% by mass NaCl aqueous solution at 25°C is -1100 to -800 mV based on a silver-silver chloride-saturated potassium chloride electrode, and A high-strength steel component with a Vickers hardness of 400 or more.

[0024] 2. The amount of Zn deposited on each side of the hot-pressed member is 5 to 100 g / m 2 2. The high strength steel member according to claim 1,

[0025] 3. The high-strength steel member according to 1 or 2 above, further comprising an Fe—Al alloy layer between the hot-pressed member and the Zn-based plating layer.

[0026] 4. The high-strength steel member according to any one of the above 1 to 3, wherein a coverage rate of an Fe oxide layer having a thickness of 1 μm or more between the hot-pressed member and the Zn-based plating layer is 10% or less.

[0027] 5. A heating process for heating the steel plate for hot pressing; a hot pressing step of hot pressing the heated steel plate to obtain a hot pressed member; and a Zn-based plating step of forming a Zn-based plating layer having a Zn content of 70 atomic % or more on at least one surface of the hot-pressed member at a temperature of 250°C or less.

[0028] 6. The method for producing a high-strength steel member according to 5 above, wherein the steel sheet for hot press use is an aluminized steel sheet.

[0029] 7. A method for producing a high-strength steel member as described in 5 or 6 above, further comprising, between the hot pressing step and the Zn-based plating step, an oxide removal step of removing oxides present on the surface of the hot-pressed member. Effect of the Invention

[0030] According to the present invention, it is possible to provide a high-strength steel member which has excellent appearance corrosion resistance, a low risk of resistance weld cracking, and a low risk of delayed fracture in a corrosive environment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0031] Hereinafter, the embodiment of the present invention will be specifically described. Note that the following description shows a preferred embodiment of the present invention, and the present invention is not limited to the following description. Furthermore, "%" used as a unit of content represents "% by mass" unless otherwise specified.

[0032] [High strength steel parts] A high-strength steel member according to one embodiment of the present invention has a hot-pressed member as a base material and a Zn-based plating layer on at least one surface of the hot-pressed member. The high-strength steel member satisfies the following conditions. The thickness of the Fe-Zn alloy layer between the hot-pressed member and the Zn-based plating layer is 0 to 1 μm. The natural immersion potential in an air-saturated 0.5% by mass NaCl aqueous solution at 25°C is -1100 to -800 mV relative to a silver-silver chloride-saturated potassium chloride electrode. -Vickers hardness is 400 or more.

[0033] (Hot press parts) The high-strength steel member of the present invention includes a hot-pressed member as a base material. The hot-pressed member is a member obtained by press-forming a steel plate in a state where the strength is reduced by heating the steel plate to a high temperature. Therefore, springback does not occur and the shape fixability is excellent. In addition, the hot-pressed member hardly generates residual stress in the processed portion. Since the residual stress is small, the risk of delayed fracture is significantly smaller in the hot-pressed member than in a cold-press-formed member having the same strength.

[0034] In the present invention, the above-mentioned problems are solved by controlling the thickness of the Fe-Zn alloy layer and the natural immersion potential as described below. Therefore, the hot-pressed member is not particularly limited and any hot-pressed member can be used.

[0035] However, in order to make the Vickers hardness of the high-strength steel member 400 or more, it is desirable to increase the Vickers hardness of the hot-pressed member used as the base material. In order to increase the Vickers hardness of the hot-pressed member, it is preferable that the hot-pressed member has the following composition.

[0036] In mass%, C: 0.1 to 0.5%, Si: 0.1 to 5.0%, Mn: 0.1-5.0%, P: 0.02% or less, S: 0.01% or less, Al: 0.1% or less, and N: Contains 0.01% or less, The balance is Fe and unavoidable impurities.

[0037] The composition of the components may further be optionally Nb: 0.05% or less, Ti: 0.05% or less, B: 0.0050% or less, Cr: 20% or less, and Sb: 0.03% or less The composition may contain at least one selected from the group consisting of:

[0038] The effects and preferred contents of each element in the above-mentioned preferred composition will be described below.

[0039] C: 0.1 to 0.5% C is an element that has the effect of improving strength by forming a structure such as martensite. From the viewpoint of increasing the Vickers hardness, it is preferable that the C content is 0.1% or more. On the other hand, if the C content exceeds 0.5%, the toughness of the spot welded portion deteriorates. Therefore, it is preferable that the C content is 0.5% or less.

[0040] Si: 0.1 to 5.0% Silicon is an effective element for strengthening steel and obtaining good material properties. In order to obtain the above effect, the silicon content is preferably 0.1% or more. On the other hand, if the silicon content exceeds 5.0%, ferrite is stabilized, and hardenability is reduced. Therefore, the silicon content is preferably 5.0% or less.

[0041] Mn: 0.1-5.0% Mn is an element effective in increasing the strength of steel. From the viewpoint of ensuring excellent mechanical properties and strength, it is preferable that the Mn content be 0.1% or more. On the other hand, if the Mn content is excessive, surface segregation during annealing increases, which affects the adhesion of the Zn-based plating layer to the hot-pressed member. Therefore, from the viewpoint of improving adhesion, it is preferable that the Mn content be 5.0% or less.

[0042] P:0.02% or less If the P content is excessive, local ductility is deteriorated due to grain boundary embrittlement caused by P segregation to the austenite grain boundaries during casting. As a result, the balance between strength and ductility of the hot press member is reduced. Therefore, from the viewpoint of improving the balance between strength and ductility, it is preferable that the P content is 0.02% or less. On the other hand, the lower limit of the P content is not particularly limited and may be 0%. However, since an excessive reduction leads to an increase in manufacturing costs, it is preferable that the P content is 0.001% or more.

[0043] S: 0.01% or less S becomes inclusions such as MnS, which causes deterioration of impact resistance and cracks along the metal flow of the weld. Therefore, it is desirable to reduce the S content as much as possible, and specifically, it is preferable to set it to 0.01% or less. From the viewpoint of ensuring good stretch flangeability, it is more preferable to set it to 0.005% or less. On the other hand, the lower limit of the S content is not particularly limited and may be 0%. However, since excessive reduction leads to an increase in manufacturing costs, it is preferable that the S content is 0.0001% or more.

[0044] Al: 0.1% or less Al is an element that acts as a deoxidizer. However, if the Al content exceeds 0.1%, the hardenability decreases. Therefore, the Al content is preferably 0.1% or less. On the other hand, although there is no particular lower limit for the Al content, from the viewpoint of enhancing the effect as a deoxidizer, the Al content is preferably 0.01% or more.

[0045] N: 0.01% or less If the N content exceeds 0.01%, AlN is generated during heating before hot pressing, and hardenability is reduced. Therefore, the N content is preferably 0.01% or less. On the other hand, the lower limit of the N content is not particularly limited and may be 0%. However, since excessive reduction leads to an increase in manufacturing costs, the N content is preferably 0.001% or more.

[0046] Nb: 0.05% or less Nb is an effective component for strengthening steel, but if it is contained in excess, shape fixability decreases. Therefore, when Nb is added, the Nb content is preferably 0.05% or less. On the other hand, the lower limit of the Nb content is not particularly limited and may be 0%.

[0047] Ti: 0.05% or less Ti, like Nb, is an effective component for strengthening steel, but if it is contained in excess, shape fixability decreases. Therefore, when Ti is added, the Ti content is preferably 0.05% or less. On the other hand, the lower limit of the Ti content is not particularly limited and may be 0%.

[0048] B: 0.0050% or less B is an element that has the effect of suppressing the formation and growth of ferrite from the austenite grain boundaries. However, the addition of excessive B significantly impairs formability. Therefore, when B is added, from the viewpoint of improving formability, the B content is preferably 0.0050% or less. On the other hand, although there is no lower limit for the B content, from the viewpoint of enhancing the effect of adding B, it is preferably 0.0002% or more.

[0049] Cr:20% or less Cr is a useful element for strengthening steel and improving hardenability. However, since Cr is an expensive element, when Cr is added, the Cr content is preferably 20% or less in order to reduce alloy costs. On the other hand, the lower limit of the Cr content is not particularly limited and may be 0%, but from the viewpoint of enhancing the effect of adding Cr, it is preferably 0.1% or more.

[0050] Sb: 0.03% or less Sb is an element that has the effect of preventing decarburization of the surface layer of a steel sheet during hot pressing. However, excessive Sb leads to an increase in rolling load, which reduces productivity. Therefore, when Sb is added, the Sb content is preferably 0.03% or less from the viewpoint of further improving productivity. On the other hand, the lower limit of the Sb content is not particularly limited and may be 0%, but from the viewpoint of enhancing the effect of adding Sb, it is preferably 0.003% or more.

[0051] The hot-pressed member can be manufactured by hot-pressing a steel plate for hot pressing, as described below. Therefore, the hot-pressed member can be said to be a hot-pressed steel plate. The hot-pressed member having the above-mentioned composition can be obtained by hot-pressing a steel plate for hot pressing having the same composition.

[0052] (Zn-based plating layer) The high-strength steel member of the present invention has a Zn-based plating layer on the surface of a hot-pressed member as a base material. The Zn-based plating layer may be provided on at least one surface of the hot-pressed member, and may be provided on both surfaces. The Zn-based plating layer may be provided on the entire surface of the hot-pressed member, or may be provided on a part of the surface. In other words, the high-strength steel member may have a portion that is not covered with the Zn-based plating layer. In the present invention, the "Zn-based plating layer" is defined as a plating layer containing 50 atomic % or more of Zn.

[0053] In the present invention, the desired corrosion resistance is achieved by controlling the natural immersion potential as described below. Therefore, the composition of the Zn-based plating layer is not particularly limited, and may be any composition containing 50 atomic % or more of Zn. The Zn-based plating layer may be a layer containing one or both of an intermetallic compound and an alloy (solid solution), or may be a layer consisting of one or both of an intermetallic compound and an alloy (solid solution). Examples of the intermetallic compound include Ni2Zn 11 , Co2Zn 11, MgZn2, etc. The solid solution may be, for example, a solid solution in which Zn is dissolved in one or both of Fe and Al. The Zn-based plating layer may be a Zn plating layer.

[0054] From the viewpoint of corrosion resistance, the Zn content in the Zn-based plating layer is preferably 60 atomic % or more, more preferably 80 atomic % or more, and even more preferably 90 atomic % or more. On the other hand, the upper limit of the Zn content is not particularly limited and may be 100%. In other words, the Zn-based plating layer may be a plating layer consisting of Zn and unavoidable impurities.

[0055] If the Zn-based plating layer contains 10 atomic % or more of Fe, the corrosion products will show a red color due to Fe oxides, and the appearance corrosion resistance will deteriorate. Therefore, from the viewpoint of further improving the appearance corrosion resistance, it is preferable that the Fe content in the Zn-based plating layer is 10 atomic % or less.

[0056] The amount of Zn coating in the high strength steel member of the present invention is not particularly limited. However, the amount of Zn coating is preferably 5 g / m 2 If the amount of Zn is less than 5g / m, the period during which the effect of preventing red rust formation can be obtained will be shortened. 2 It is preferable that the content is 10 g / m or more. 2 More preferably, it is 20 g / m or more. 2 It is more preferable that the Zn coating weight is 100 g / m or more. 2 If the coating weight exceeds 100 g / m, cracks may occur in the weld even if no Fe-Zn alloy layer is present. Therefore, from the viewpoint of further improving resistance weld crack resistance, it is recommended to use a coating weight of Zn of 100 g / m 2 It is preferable that the thickness is less than 80 g / m 2 It is more preferable to set it as follows:

[0057] The amount of Zn attached can be measured by subjecting the high-strength steel member to anodic electrolysis to dissolve Zn, and quantifying the amount of dissolved Zn by inductively coupled plasma-mass spectrometry (ICP-MS). Specifically, first, constant current anodic electrolysis is performed in a 3% sodium hydroxide-1% aluminum chloride aqueous solution, with the high-strength steel member as the working electrode and a platinum mesh electrode as the counter electrode. The current density in the anodic electrolysis is 4 mA / cm. 2 During anodic electrolysis, the electrolysis is stopped at the point where the potential becomes increasingly noble. This allows all of the Zn to be dissolved in the aqueous solution. The amount of Zn in the aqueous solution is then quantitatively analyzed by ICP-MS to determine the total amount of dissolved Zn. The amount of Zn attached can be determined by dividing the total amount of Zn obtained by the surface area of ​​the high-strength member.

[0058] [Fe-Zn alloy layer] In the present invention, it is important that the thickness of the Fe-Zn alloy layer between the hot-pressed member and the Zn-based plating layer is 0 to 1.0 μm. In other words, in the high-strength steel member of the present invention, there is no Fe-Zn alloy layer between the hot-pressed member and the Zn-based plating layer, or even if there is an Fe-Zn alloy layer, the thickness of the Fe-Zn alloy layer is 1.0 μm.

[0059] If the Fe-Zn alloy layer is present directly on the steel sheet, the Zn may melt or evaporate during resistance welding, causing resistance weld cracks in the surface layer of the steel material, which may deteriorate the strength and fatigue properties of the weld. Therefore, in order to avoid weld cracks, the thickness of the Fe-Zn alloy layer is set to 1.0 μm or less.

[0060] The Fe-Zn alloy layer is a layered phase having a Zn concentration of 15% or more and a total concentration of Fe and Zn of 80% or more, when the cross section of a high-strength steel member is observed and analyzed by SEM-EDX.

[0061] The Fe-Zn alloy layer is formed by forming an Fe-Zn-based plating layer after hot press forming. Alternatively, when a Zn-based plating layer is present on the surface of a steel sheet for hot press forming before hot press forming, i.e., directly on an alloy mainly composed of Fe, alloying of Fe and Zn proceeds during the heating process, and the Fe-Zn alloy layer is formed. Regardless of the method for forming the Fe-Zn alloy layer that affects the weld cracking properties, it is preferable that the manufacturing method of the high strength steel member of the present invention does not go through any of the above steps.

[0062] [Fe-Al alloy layer] The high strength steel member of the present invention may further have an Fe-Al alloy layer at the interface between the hot press member and the Zn-based plating layer.

[0063] The solid solubility limit of Zn in the Fe-Al alloy layer is lower than that of Zn in Fe. Therefore, during resistance welding, the Fe-Al alloy layer acts as a barrier against molten Zn that is generated when the Zn-based plating layer melts. Therefore, by providing an Fe-Al alloy layer, the risk of resistance weld cracking can be further reduced.

[0064] Furthermore, the Fe-Al alloy layer has a low anodic dissolution rate in a corrosive environment and a low oxygen reduction reaction rate, which is the main cathodic reaction. Therefore, the Fe-Al alloy layer has a low corrosion rate of the Fe-Al alloy layer itself and a low galvanic corrosion rate with the upper Zn-based plating layer. Therefore, by providing the Fe-Al alloy layer, it is possible to obtain even better corrosion resistance.

[0065] In the present invention, when a cross section of a high-strength steel member is observed and analyzed by SEM-EDX, a layer having a thickness of 1 μm or more and consisting of a phase having an Fe concentration of 15% or more, a total concentration of Fe and Al of 80% or more, and a Zn concentration of less than 10% is defined as an "Fe-Al alloy layer."

[0066] The Fe-Al alloy layer is not particularly limited and any layer can be used as long as it meets the above definition. That is, in the present invention, the components constituting the Fe-Al alloy layer are not limited to alloys in the narrow sense, and may be intermetallic compounds or metal layers containing solid solutions. Examples of the intermetallic compounds include Fe2Al5, Fe4Al 13 , FeAl, etc. Furthermore, an example of a metal phase containing a solid solution is α-Fe containing Al as a solid solution.

[0067] The thickness of the Fe-Al alloy layer is not particularly limited, but from the viewpoint of enhancing the effect of reducing resistance weld cracking, it is preferably 1 μm or more, more preferably 5 μm or more, and even more preferably 10 μm or more, while from the viewpoint of adhesion of the plating layer, the thickness of the Fe-Al alloy layer is preferably 30 μm or less, more preferably 25 μm or less, and even more preferably 20 μm or less.

[0068] The thickness of the Fe-Al alloy layer can be measured by observing and analyzing a cross section of the high strength steel member by SEM-EDX, more specifically, by the method described in the examples.

[0069] The method for forming the Fe-Al alloy layer is not particularly limited, but it is economically advantageous to provide an Al-based plating layer on the surface of the steel sheet for hot press forming before hot press forming, i.e., directly on the alloy mainly composed of Fe, and allow alloying of Fe and Al to proceed during the heating process. The method for forming the Al-based plating layer on the steel sheet for hot press forming is also not particularly limited, and examples include hot-dip plating, electroplating using a non-aqueous solvent or molten salt, physical vapor deposition, and clad rolling, but hot-dip plating is preferred from the viewpoints of manufacturability and economy.

[0070] [Fe oxide layer] The high-strength steel member of the present invention may have an Fe oxide layer at the interface between the hot-pressed member and the Zn-based plating layer. In the present invention, the Fe oxide layer is defined as a layer in which the O concentration is 20% or more and the sum of the concentrations of Fe and O is 80% or more when a cross section of the high-strength steel member is observed and analyzed by SEM-EDX. The Fe-based oxide constituting the Fe oxide layer is not particularly limited, and examples thereof include Fe2O3, FeO, and Fe3O4.

[0071] However, if a large amount of Fe oxide exists between the hot-pressed member and the Zn-based plating layer, the resistance weld cracking properties may be deteriorated. That is, Fe oxide has a higher electrical resistance than the hot-pressed member, which is the base material, the Zn-based plating layer, and the Fe-Al alloy layer. Therefore, if a large amount of Fe oxide exists, the current path during resistance welding is restricted, which causes localized heat generation. As a result, the resistance weld cracking properties are deteriorated.

[0072] Therefore, it is desirable that the amount of Fe oxide present between the hot-pressed member and the Zn-based plating layer is small. Specifically, it is preferable that the coverage of the Fe oxide layer having a thickness of 1 μm or more between the hot-pressed member and the Zn-based plating layer is 10% or less. On the other hand, the lower the coverage, the better, and it is preferable that the coverage is 0%. In the following description, when the term "coverage of the Fe oxide layer" is used, it means "coverage of the Fe oxide layer having a thickness of 1 μm or more."

[0073] The coverage of the Fe oxide layer can be measured by observing the cross section of the high-strength steel member with SEM-EDX. Specifically, the cross section of the high-strength steel member is observed with an SEM under conditions of an acceleration voltage of 5 kV and a magnification of 1000 times to obtain a backscattered electron image. Next, the coverage can be calculated by dividing the length of the backscattered electron image where Fe oxide having a thickness of 1 μm or more exists by the total width observed.

[0074] The Fe oxide layer is formed when non-plated steel sheets are hot-pressed. By adjusting the heating conditions and the chemical composition of the steel sheet, the coverage of the Fe oxide layer can be reduced to 10% or less.

[0075] A specific method for reducing the coverage of the Fe oxide layer is, for example, to perform heating before hot pressing by direct electrical heating and shorten the heating time. In addition, using a steel sheet containing 1% or more of Cr as the steel sheet for hot pressing is also effective in reducing the coverage of the Fe oxide layer.

[0076] On the other hand, when a general hot press steel sheet, for example, Mn-B steel 22MnB5 according to the DIN standard, is used, the coverage of the Fe oxide layer is nearly 100%. Even in such a case, the coverage of the Fe oxide layer can be reduced by providing an oxide removal process for removing oxides present on the surface of the hot press member between the hot press process and the Zn-based plating process. A specific method for removing the oxides will be described later.

[0077] [Surface oxide layer] The high-strength steel member of the present invention may further have an oxide layer on the surface of the Zn-based plating layer. Here, the oxide layer is referred to as a surface oxide layer to distinguish it from the Fe oxide layer between the hot-pressed member and the Zn-based plating layer. The oxide contained in the surface oxide layer is not particularly limited, but examples thereof include Zn oxide and composite oxides containing Zn and Al, Mg, Ti, Cr, Mn, Fe, Ni, etc.

[0078] If the surface oxide layer is too thick, there is a risk of reduced adhesion when painted, and therefore the thickness of the surface oxide layer is preferably 5 μm or less.

[0079] (natural immersion potential) In the present invention, it is important that the natural immersion potential of the high strength steel member is -1100 to -800 mV based on a silver-silver chloride-saturated potassium chloride electrode (SSE). By setting the natural immersion potential within the above range, the cathodic protection performance of the hot pressed member, which is the base material, becomes the best, and excellent appearance corrosion resistance can be obtained. In addition, delayed fracture caused by hydrogen generated with corrosion can be reduced.

[0080] If the natural immersion potential is more noble (positive) than -800mV, the potential difference between the steel material and the coating layer is small, and the cathodic protection performance is insufficient, resulting in inferior appearance corrosion resistance. Therefore, the natural immersion potential is set to -800mV or less, preferably -900mV or less, and more preferably -950mV or less. On the other hand, if the natural immersion potential is more noble (negative) than -1100mV, the effect of improving appearance corrosion resistance is saturated. In addition, the amount of hydrogen generated by corrosion becomes excessive, increasing the risk of delayed fracture. Therefore, the natural immersion potential is set to -1100mV or more, preferably -1075mV or more, and more preferably -1050mV or more.

[0081] The natural immersion potential in the present invention refers to the natural immersion potential in an air-saturated 0.5 mass% NaCl aqueous solution at 25°C, expressed based on a silver-silver chloride-saturated potassium chloride electrode. In measuring the natural immersion potential, a 10 mmφ area in any flat part of the hot-pressed member having an area of ​​10 mmφ or more is used as the working electrode. The average value of the immersion potential from 60 seconds to 600 seconds after the working electrode is immersed in the NaCl aqueous solution is taken as the natural immersion potential of the hot-pressed member. In the measurement, the temperature of the NaCl aqueous solution is adjusted to 25±5°C.

[0082] Although the mechanical properties of the high-strength steel member of the present invention are not particularly limited, it is preferable that the residual stress measured by X-ray diffraction at any point of the high-strength steel member is less than 600 MPa. When trimming or piercing is performed after hot press forming, if cold working is performed, residual stress is generated at the point, increasing the risk of delayed fracture. In order to reduce the risk of delayed fracture, it is preferable not to perform cold working after hot press forming, and to use a laser processing device for trimming and piercing.

[0083] (Vickers hardness) The Vickers hardness of the high-strength steel member of the present invention is 400 or more. That is, in the present invention, "high strength" means that the Vickers hardness is 400 or more. The high-strength steel member of the present invention having a Vickers hardness of 400 or more can be suitably used for applications such as automotive frame members. The Vickers hardness is measured on a flat portion of the cross section of the high-strength steel member. The high-strength steel member of the present invention may have a Vickers hardness of 400 or more at least in a part thereof. For example, in order to impart a function, other hot-pressed members having different strengths can be joined to a part of the high-strength steel member. In addition, in the cooling process after hot pressing, cooling can be performed with different thermal histories depending on the part of the hot-pressed member. In such a case, the Vickers hardness of the high-strength steel member finally obtained may be 400 or more in a part thereof and less than 400 in the other parts.

[0084] On the other hand, if the Vickers hardness of the high-strength steel member is too high, the resistance to delayed fracture may decrease. Therefore, the Vickers hardness of the high-strength steel member is preferably 800 or less, more preferably 700 or less, and even more preferably 600 or less.

[0085] The Vickers hardness of the high-strength steel member is determined by the Vickers hardness of the hot-pressed member as the base material. Therefore, in order to obtain a high-strength steel member having the above Vickers hardness, it is sufficient to use a hot-pressed member having the same Vickers hardness as the base material.

[0086] In the present invention, as described above, the strength of the member is defined based on the Vickers hardness. Therefore, the tensile strength of the high-strength steel member is not particularly limited. However, in general, when the Vickers hardness is 400 or more, the tensile strength of the high-strength steel member is about 1180 MPa or more.

[0087] [Manufacturing method] Next, a preferred method for producing the high strength steel member of the present invention will be described.

[0088] A method for producing a high-strength steel member according to one embodiment of the present invention includes the following steps (1) to (3). (1) Heating process for heating steel sheets for hot pressing (2) A hot pressing process in which the heated steel plate for hot pressing is hot pressed to form a hot pressed member. (3) A Zn-based plating step of forming a Zn-based plating layer having a Zn content of 70 atomic % or more on at least one surface of the hot-pressed member at a temperature of 250° C. or less.

[0089] The hot press steel sheet is not particularly limited and any steel sheet can be used. The suitable composition of the steel sheet is the same as the suitable composition of the steel material of the hot press member described above. The hot press steel sheet is preferably a hot-rolled steel sheet or a cold-rolled steel sheet.

[0090] As the hot press steel sheet, a steel sheet having no plating layer can be used, but a steel sheet having a plating layer (plated steel sheet) can also be used. Examples of the plated steel sheet include an Al-plated steel sheet and a Ni-plated steel sheet.

[0091] The Al-plated steel sheet is a steel sheet having an Al-plated layer, the Al content of which is 50 mass % or more, on at least one surface of the steel sheet.

[0092] An interface alloy layer containing 50 mass% or more of an Fe-Al based intermetallic compound may be provided between the Al plating layer and the base steel sheet. The components of the Al plating layer are not limited as long as it is an Al alloy containing 50 mass% or more of Al, but may optionally contain Si. More preferably, the Al plating layer has a component composition consisting of Si: 0.1-13%, Mg: 0-10%, and Fe: 0-5%.

[0093] The Ni-plated steel sheet is a steel sheet having a plating layer on at least one surface of the steel sheet, the Ni content of which is 50 mass% or more. The composition of the plating layer is not limited as long as it is a Ni alloy mainly composed of Ni, but may optionally contain Ti, Cr, Fe, Co, Mo, and W.

[0094] Furthermore, if the Al plating layer or the Ni plating layer contains Zn, an Fe-Zn alloy layer may be formed after hot pressing. Therefore, from the viewpoint of suppressing the formation of an Fe-Zn alloy layer, it is preferable that the Zn concentration of the Al plating layer or the Ni plating layer is 50% or less.

[0095] The plating of the base steel sheet can be carried out by any method, but from the viewpoint of economy, it is preferably carried out by an electroplating method or a hot-dip galvanizing method. Hereinafter, the case of producing an Al-plated steel sheet by a hot-dip galvanizing method will be described.

[0096] First, prior to hot-dip galvanization, the base steel sheet is annealed. Next, the base steel sheet after the annealing is immersed in a hot-dip galvanizing bath to obtain a hot-dip galvanized steel sheet having a hot-dip galvanized layer on the surface of the base steel sheet. The hot-dip galvanizing bath may contain Al, Zn, and Fe flowing out from the base material or bath-immersed equipment. The hot-dip galvanizing bath may further contain Si. More preferably, the hot-dip galvanizing bath has a component composition of Si: 0.1-13%, Mg: 0-10%, Fe: 0-5%, and the balance being Al and unavoidable impurities.

[0097] The coating weight of the hot-dip coating layer is not particularly limited, but is preferably 20 g / m per one side of the steel sheet. 2 It is preferable that the thickness is 30 g / m or more. 2 More preferably, it is 50 g / m or more. 2 It is more preferable that the coating weight of the hot-dip coating layer is 300 g / m2 or more per one side of the steel sheet. 2 It is preferable that the thickness is less than 250 g / m 2 More preferably, it is 200 g / m or less. 2 It is more preferable that the coating weight of the plating layer is not more than 100%. As described above, when hot pressing is performed, the coating weight of the plating layer increases due to the diffusion of Fe from the base steel sheet. Therefore, by setting the coating weight of the hot-dip plating layer on the hot-dip plated steel sheet before hot pressing to the above range, the coating weight of the plating layer on the hot-pressed member can be set to the above-mentioned preferable range.

[0098] The coating weight per side of the hot-dip plating layer is determined by the following method. First, the hot-dip plating steel sheet to be evaluated is punched to obtain three samples of 48 mmφ. Then, one side of each sample (the side opposite to the side on which the coating weight is measured) is masked. Each sample is immersed in a 17% hydrochloric acid solution containing 1 mL of hexamethylenetetramine as an inhibitor for 20 minutes to dissolve the hot-dip plating layer, and the weight of each sample is measured again. The difference in mass before and after dissolution of the hot-dip plating layer is divided by the area of ​​the sample to calculate the coating weight per unit area of ​​each sample. The average value of the coating weights of the three samples is then taken as the coating weight per side of the hot-dip plating layer of the hot-dip plating steel sheet.

[0099] (Heating process) Prior to the hot pressing step, the steel sheet for hot pressing is heated (heating step). In the heating step, it is preferable to raise the temperature from room temperature to a heating temperature between the Ac3 transformation point of the base steel sheet and 1100°C in a temperature-raising time of 10 seconds or more and 300 seconds or less in an atmosphere with an oxygen concentration of 0.1 to 22 volume %, and to further hold the steel sheet for hot pressing after the temperature-raising step at the heating temperature for a holding time of 5 seconds or more and 900 seconds or less in the atmosphere.

[0100] The atmosphere in the heating step preferably has an oxygen concentration of 0.1 to 22% by volume. When a non-plated steel sheet is used, it is preferable to reduce the thickness and coverage of the Fe oxide layer, and for this purpose, the oxygen concentration is preferably 22% by volume or more, more preferably 10% by volume or less, and even more preferably 1% by volume or less. On the other hand, even if the oxygen concentration is less than 0.1% by volume, no particular effect is obtained and the operating costs increase, so the oxygen concentration is preferably 0.1% by volume or more.

[0101] If the heating temperature is lower than the Ac3 transformation point, the strength required for the hot press member may not be obtained, whereas if the heating temperature exceeds 1100°C, the operating costs increase.

[0102] The lower limit of the time for the steel sheet for hot pressing to reach the heating temperature from room temperature is not particularly limited, but is preferably 10 seconds or more from the viewpoint of the operational stability of the hot press. The upper limit of the time for the steel sheet for hot pressing to reach the heating temperature from room temperature is not particularly limited, but is preferably 300 seconds or less, because an excessively long heating time leads to a deterioration in productivity.

[0103] The lower limit of the holding time after reaching the heating temperature is not particularly limited, but it is preferably 5 seconds or more from the viewpoint of operational stability of hot pressing. On the other hand, if the holding time exceeds 900 seconds, a stable oxide film is formed on the surface of the steel sheet for hot pressing, which is difficult to remove, so that the holding time is preferably 900 seconds or less.

[0104] (Hot pressing process) Next, the steel plate heated in the heating step is subjected to hot pressing to obtain a hot pressed member (hot pressing step). In the hot pressing, the steel plate for hot pressing is formed into a desired shape and cooled by a metal mold, water, etc. In the present invention, the hot pressing conditions are not particularly limited, but it is preferable to perform pressing at a general hot pressing temperature range of 600 to 800°C.

[0105] (Zn-based plating process) Next, a Zn-based plating layer is formed on at least one surface of the obtained hot-pressed member (Zn-based plating step). If the temperature when forming the Zn-based plating layer (hereinafter sometimes referred to as "film-forming temperature") exceeds 250°C, the hot-pressed member is tempered, and the desired hardness cannot be obtained. Therefore, in the step of forming the Zn-based plating layer, the film-forming temperature is set to 250°C or less. Here, the temperature when forming the Zn-based plating layer (film-forming temperature) refers to the maximum temperature reached by the hot-pressed member when the Zn-based plating layer is formed. The film-forming temperature is preferably 150°C or less, more preferably 100°C or less.

[0106] The Zn content of the Zn-based plating layer is 70 atomic % or more. If the Zn content is less than 70 atomic %, that is, if the total content of elements other than Zn exceeds 30 atomic %, the natural immersion potential in an air-saturated 0.5 mass % NaCl aqueous solution at 25°C may be outside the range of -1100 to -800 mV based on a silver-silver chloride-saturated potassium chloride electrode standard, and the desired corrosion resistance cannot be obtained. More specifically, if the potential is excessively base, the potential difference with the base steel is large, and the paint blistering rate may increase. In addition, if the potential is excessively noble, red rust due to corrosion of the base material may become noticeable. By controlling the Zn content of the Zn-based plating layer to 70 atomic % or more, stable performance against both paint blistering and red rust can be obtained. In order to stabilize the corrosion resistance, the Zn content of the Zn-based plating layer is preferably 80 atomic % or more, more preferably 90 atomic % or more.

[0107] The method for forming the Zn-based plating layer is not particularly limited, and either wet plating or dry plating can be used. Usually, the plating method can be selected according to the type of Zn-based plating layer to be formed.

[0108] For example, when the Zn-based plating layer is pure Zn, Zn-Ni plating, Zn-Ni-Co plating, Zn-Cr plating, or Zn-Mn plating, it is preferable to form the film by electroplating. When the coating layer is a composition that is difficult to electrolytically deposit from an aqueous solution, such as Zn-Ti plating or Zn-Mg plating, it is preferable to form the film by PVD. Note that when forming a Zn-based plating layer by hot-dip plating, the temperature exceeds 250°C, so hot-dip plating is not used.

[0109] Regardless of the method used to form the coating layer, the conditions can be adjusted so that the coating layer on one side (front side) of the steel sheet and the other side (back side) of the steel sheet have the desired thickness. For example, in the case of electroplating, the thickness of the coating layer on each side can be adjusted by changing either or both of the current density and current flow time on each side. In addition, by adjusting the arrangement of the electrodes and controlling the current density, it is possible to intentionally provide a distribution in the plating deposition weight within the same surface.

[0110] (Surface oxide removal process) As described above, when a non-plated steel sheet is hot-pressed, an Fe oxide layer is formed on the surface of the hot-pressed part. Therefore, in order to reduce the coverage of the Fe oxide layer in the finally obtained high-strength steel part, it is preferable to remove the oxides present on the surface of the hot-pressed part after hot pressing and before Zn-based plating (oxide removal step).

[0111] The method for removing oxides in the oxide removing step is not particularly limited and any method can be used. Suitable oxide removing methods include physical methods such as shot blasting, sand blasting, and dry ice blasting, optical methods such as laser cleaning, chemical methods such as pickling, and combinations thereof. Any acid solution can be used for the pickling without any particular limitation.

[0112] In addition, when an Al-plated steel sheet is used as a steel sheet for hot pressing, a thin Al-based oxide is generated on the surface of the hot-pressed member. When the Al-based oxide is present, the adhesion between the Zn-based plating layer and the base steel sheet is reduced. Therefore, even when an Al-plated steel sheet is used, it is preferable to remove the Al-based oxide by carrying out the oxide removal step. There is no particular limitation on the method for removing the Al-based oxide. However, the plating layer of the hot-pressed Al-plated steel sheet dissolves in an acidic solution. Therefore, in order to remove the Al-based oxide while preventing the plating layer from dissolving, it is preferable to remove the oxide by immersing the steel sheet in an alkaline solution of pH 11 or more. EXAMPLES

[0113] The functions and effects of the present invention will be described below based on examples, although the present invention is not limited to the following examples.

[0114] A high-strength steel member was manufactured by hot pressing a steel plate for hot pressing according to the following procedure.

[0115] As the steel sheets for hot pressing, the following steel sheets (A) to (F) were used.

[0116] (A) A cold-rolled steel sheet having a thickness of 1.4 mm, containing, by mass%, C: 0.34%, Si: 0.25%, Mn: 1.2%, Cr: 0.2%, P: 0.005%, S: 0.001%, Al: 0.03%, N: 0.004%, Nb: 0.02%, Ti: 0.01%, B: 0.002%, Sb: 0.01%, with the remainder being Fe and unavoidable impurities.

[0117] (B) A cold-rolled steel sheet having a thickness of 1.4 mm, containing, by mass%, C: 0.34%, Si: 0.50%, Mn: 0.6%, Cr: 1.0%, P: 0.005%, S: 0.001%, Al: 0.03%, N: 0.004%, Nb: 0.02%, Ti: 0.01%, B: 0.002%, Sb: 0.01%, with the balance being Fe and unavoidable impurities.

[0118] (C) A cold rolled steel sheet having a thickness of 1.4 mm and containing, by mass%, C: 0.34%, Si: 1.0%, Mn: 1.0%, Cr: 11%, P: 0.005%, S: 0.001%, Al: 0.03%, N: 0.004%, Nb: 0.02%, Ti: 0.01%, B: 0.002%, Sb: 0.01%, with the remainder being Fe and unavoidable impurities.

[0119] (D) A cold-rolled steel sheet having a thickness of 1.6 mm and containing, by mass%, C: 0.21%, Si: 0.2%, Mn: 1.3%, Cr: 0.18%, P: 0.005%, S: 0.001%, Al: 0.03%, N: 0.004%, B: 0.002%, with the remainder being Fe and unavoidable impurities.

[0120] (E) A cold-rolled steel sheet having a thickness of 1.8 mm and containing, by mass%, C: 0.42%, Si: 0.25%, Mn: 1.0%, Cr: 0.12%, P: 0.005%, S: 0.001%, Al: 0.03%, N: 0.004%, Nb: 0.02%, Ti: 0.01%, B: 0.002%, Sb: 0.01%, with the remainder being Fe and unavoidable impurities.

[0121] (F) A cold rolled steel sheet having a thickness of 1.2 mm and containing, by mass%, C: 0.49%, Si: 0.2%, Mn: 1.2%, Cr: 0.18%, P: 0.005%, S: 0.001%, Al: 0.03%, N: 0.004%, Nb: 0.02%, Ti: 0.01%, B: 0.002%, Sb: 0.01%, with the remainder being Fe and unavoidable impurities.

[0122] In some examples, the plated steel sheet obtained by plating the surface of the above steel sheet was used as the hot press steel sheet. The combination of the steel sheet and the plating layer used is shown in Table 1. Each plating layer was formed under the following conditions.

[0123] (Electrolytic zinc plating) The steel sheet was used as the cathode and the iridium oxide-coated titanium sheet was used as the anode to perform electroplating under the following conditions to form a Zn plating layer. The thickness of the Zn plating layer was adjusted by changing the current application time. Plating solution composition: Zinc sulfate heptahydrate 240g / L pH: 2.0 ·Temperature: 50℃ ·Current density: 40A / dm 2

[0124] (Electrolytic Zn-12%Ni alloy plating) The steel sheet was used as the cathode and the iridium oxide-coated titanium sheet was used as the anode to perform electroplating under the following conditions to form a Zn-12%Ni alloy plating layer. The thickness of the Zn-12%Ni alloy plating layer was adjusted by changing the current application time. Plating solution composition: Nickel sulfate hexahydrate 240g / L Zinc sulfate heptahydrate 20g / L pH: 2.0 ·Temperature: 50℃ ·Current density: 40A / dm 2

[0125] (Ni alloy electric plating) The steel sheet was used as the cathode and the iridium oxide-coated titanium sheet was used as the anode to perform electroplating under the following conditions to form a Ni plating layer. The thickness of the Ni plating layer was adjusted by changing the current application time. Plating solution composition: Nickel sulfate hexahydrate 240g / L Boric acid 30g / L pH: 3.0 ·Temperature: 50℃ ·Current density: 40A / dm 2

[0126] (Hot-dip plating) In some examples, hot-dip galvanized steel sheets were used for comparison. The hot-dip galvanized steel sheets were prepared by immersing the steel sheets in a hot-dip galvanizing bath. After the steel sheets were pulled out of the hot-dip galvanizing bath, N2 gas wiping was performed to adjust the coating weight of the plating layer. The following three types of hot-dip galvanizing baths were used. ·Zn-0.2%Al hot-dip plating bath (bath temperature 460℃) ·Al-10%Si hot-dip plating bath (bath temperature 660℃) ·Al-10%Si-1%Mg hot-dip plating bath (bath temperature 660℃)

[0127] ·Heating process Next, a test piece of 200 × 300 mm was taken from the obtained hot-dip plated steel sheet, and the test piece was heated to 900 ° C under the conditions (heating method and temperature rise time) shown in Table 1. After the temperature was raised to 900 ° C, it was held for 1 minute.

[0128] Hot pressing process As described above, after holding at 900°C for 1 minute, the test piece was hot pressed to obtain a hat-shaped high-strength steel member. Specifically, the test piece was transferred to a press device installed adjacent to the heating device and immediately hot pressed. A hat-shaped die was used for the hot pressing, and the forming start temperature was 700°C. The shape of the obtained high-strength steel member was such that the flat portion of the upper surface had a length of 100 mm, the flat portion of the side surface had a length of 50 mm, and the flat portion of the lower surface had a length of 50 mm. In addition, the bending R of the die was 7R for both shoulders of the upper surface and both shoulders of the lower surface.

[0129] ·Oxide removal process In some examples, an oxide removal process was performed to remove oxides from the surface of the hot-pressed parts by shot blasting, pickling, or alkaline immersion. The methods used for the oxide removal process are shown in Table 1.

[0130] In the shot blasting, steel balls with an average grain size of 0.5 mm were used as the blasting material, and the blasting material was sprayed against the surface of the hot-pressed part at an angle of 60° and with an air pressure of 0.2 MPa. For comparison, in Example No. 5, the shot blasting treatment time was half that of the other examples, and the amount of remaining oxide was intentionally increased.

[0131] The pickling solution used was a 10% HCl aqueous solution containing 1 g / L of hexamethylenetetramine as an inhibitor. The temperature of the pickling solution was 50° C., and the immersion time was 60 seconds.

[0132] For the alkali immersion, a 50% NaOH aqueous solution at 80° C. was used. The hot-pressed part was immersed in the NaOH aqueous solution for 60 seconds to remove oxides.

[0133] ·Zn-based plating process Next, a Zn-based plating layer was formed on the surface of the hot-pressed member by the method shown in Table 1. Each of the methods used is described below. For comparison, in some examples, the Zn-based plating layer was not formed.

[0134] (Electroplating) The formation of the Zn-based plating layer by electroplating was carried out under the following conditions. In each case, electrolysis was carried out using the hot-pressed member as the cathode and the iridium oxide-coated titanium plate as the anode, and the thickness of the coating layer was adjusted by changing the current flow time. The anode was of the same shape as the hot-pressed member, and the anode was placed on both sides of the hot-pressed member to carry out plating.

[0135] (1) Zn plating Plating solution composition: Zinc sulfate heptahydrate 240g / L pH: 2.0 ·Temperature: 50℃ ·Current density: 40A / dm 2

[0136] (2) Zn-12%Ni alloy plating Plating solution composition: Nickel sulfate hexahydrate 240g / L Zinc sulfate heptahydrate 20g / L pH: 2.0 ·Temperature: 50℃ ·Current density: 40A / dm 2

[0137] (3) Zn-18%Ni alloy plating Plating solution composition: Nickel sulfate hexahydrate 240g / L Zinc sulfate heptahydrate 20g / L pH: 2.0 ·Temperature: 50℃ ·Current density: 60A / dm 2

[0138] (4) Zn-30%Ni alloy plating Plating solution composition: Nickel sulfate hexahydrate 360g / L Zinc sulfate heptahydrate 20g / L pH: 2.0 ·Temperature: 50℃ ·Current density: 100A / dm 2

[0139] (5) Zn-8%Cr alloy plating Plating solution composition: Chromium(III) sulfate hexahydrate 100 g / L Zinc sulfate heptahydrate 200 g / L Sodium sulfate 100g / L Polyethylene glycol 1g / L pH: 2.0 ·Temperature: 50℃ ·Current density: 50A / dm 2

[0140] (6) Zn-40%Mn alloy plating Plating solution composition: Manganese(II) sulfate 70g / L Zinc sulfate heptahydrate 30 g / L Sodium citrate 180 g / L pH: 5.6 ·Temperature: 50℃ ·Current density: 20A / dm 2

[0141] (7) Zn-Fe alloy plating Plating solution composition: Iron(II) sulfate heptahydrate 240g / L Zinc sulfate heptahydrate 20g / L pH: 2.0 ·Temperature: 50℃ ·Current density: 40A / dm 2

[0142] (PVD) The formation of the Zn-based plating layer by PVD was carried out by ion plating. For the ion plating, a batch-type radio frequency (RF) excitation type ion plating device manufactured by Showa Vacuum Co., Ltd. was used. The film formation conditions were as follows: temperature of the hot pressed member: 100°C, pressure: 3 Pa, bias voltage: -20 V. The composition of the plating layer was controlled by adjusting the composition of the metal used as the deposition source. The thickness of the plating layer was also controlled by adjusting the deposition time.

[0143] (Hot-dip plating method) In some comparative examples, the Zn-based plating layer was formed by hot-dip plating using a flux. The flux was a mixture of ammonium chloride and zinc chloride. The hot-dip plating bath had a temperature of 460°C, a composition of Zn-0.2%Al, and an immersion time of 60 seconds.

[0144] (natural immersion potential) The natural immersion potential of the high-strength steel member obtained by the above procedure was measured by the following procedure. First, three samples with a diameter of 16 mm were taken by punching from the flat part of the upper surface of the hot-pressed member formed into a hat shape. The immersion potential was measured in an air-saturated 0.5 mass% NaCl aqueous solution at 25±5°C, using a 10 mm diameter area in the center of the sample as the working electrode and a silver-silver chloride-saturated potassium chloride electrode (SSE) as the reference electrode. The time average of the immersion potential from 60 seconds to 600 seconds after the working electrode was immersed in the NaCl aqueous solution was taken as the natural immersion potential of the sample. The average value of the natural immersion potential of the three different samples was taken as the natural immersion potential of the hot-pressed member to be evaluated. The measurement results are shown in Table 2.

[0145] Furthermore, for each of the obtained high-strength steel members, the Vickers hardness, the thickness of the Fe-Zn alloy layer, the Zn coating weight, the thickness of the Fe-Al alloy layer, and the coverage rate of the Fe oxide layer were measured by the following methods. The measurement results are shown in Table 2.

[0146] (Vickers hardness) A test piece was cut out from the top plate of the obtained high-strength steel member by a laser cutting machine, and then the cross section of the test piece was mirror-polished. Thereafter, the Vickers hardness of the test piece was measured at a position of 1 / 4 of the plate thickness. The measurement was performed at 10 points at intervals of 200 μm in a direction perpendicular to the rolling direction of the steel plate, and the average value was taken as the Vickers hardness of the high-strength steel member. The measurement conditions for the Vickers hardness were a test force of 100 g and a holding time of 5 seconds.

[0147] (Fe-Zn alloy layer thickness) The thickness of the Fe-Zn alloy layer was evaluated by observing and analyzing the cross section of the high-strength steel member by SEM-EDX according to the following procedure. The cross section of the mirror-finished high-strength steel member was observed using a SEM to obtain a backscattered electron image at a magnification of 5000 times at an acceleration voltage of 5 kV. If an alloy layer was observed at the interface between the Zn-based plating layer and the base steel sheet, its composition was analyzed by EDX to determine whether it was an Fe-Zn alloy layer with a Zn concentration of 15% or more and a total concentration of Fe and Zn of 80% or more. If it was an Fe-Zn alloy layer, its thickness was measured from the cross section at any 10 points within the observation field. The above observation was performed in any 10 fields of view, and the average value was taken as the thickness of the Fe-Zn alloy layer.

[0148] (Zn phase adhesion amount) The amount of the Zn phase attached was measured by subjecting the high-strength steel member to anodic electrolysis to dissolve Zn, and quantifying the amount of dissolved Zn by inductively coupled plasma-mass spectrometry (ICP-MS). Specifically, first, constant current anodic electrolysis was performed in a 3% sodium hydroxide-1% aluminum chloride aqueous solution, with the high-strength steel member as the working electrode and a platinum mesh electrode as the counter electrode. The current density in the anodic electrolysis was 4 mA / cm. 2 During the anodic electrolysis, all of the Zn was dissolved in the aqueous solution by stopping the electrolysis at the point where the potential became steeply noble. Then, the amount of Zn in the aqueous solution was quantitatively analyzed by ICP-MS to determine the total amount of dissolved Zn. The amount of Zn attached was calculated by dividing the total amount of Zn obtained by the surface area of ​​the high-strength member.

[0149] (Fe-Al alloy layer thickness) The thickness of the Fe-Al alloy layer was evaluated by observing and analyzing the cross section of the high-strength steel member by SEM-EDX according to the following procedure. The cross section of the mirror-finished high-strength steel member was observed using a SEM to obtain a backscattered electron image at a magnification of 5000 times at an acceleration voltage of 5 kV. If an alloy layer was observed at the interface between the Zn-based plating layer and the base steel sheet, its composition was analyzed by EDX to determine whether it was an Fe-Al alloy layer with an Fe concentration of 15% or more and a total concentration of Fe and Al of 80% or more. If it was an Fe-Al alloy layer, its thickness was measured from the cross section at any 10 points within the observation field. The above observation was performed in any 10 fields of view, and the average value was taken as the thickness of the Fe-Al alloy layer.

[0150] (Fe oxide layer thickness and coverage) The cross section of the high-strength steel member was observed by SEM-EDX to measure the coverage of the Fe oxide layer having a thickness of 1 μm or more. Specifically, the cross section of the high-strength steel member was observed by SEM under conditions of an acceleration voltage of 5 kV and a magnification of 1000 times to obtain a backscattered electron image. Next, the coverage was calculated by dividing the length of the Fe oxide having a thickness of 1 μm or more in the backscattered electron image by the total width observed.

[0151] When an oxide layer was found at the interface between the Zn-based plating layer and the hot-pressed part, its composition was analyzed by EDX. If the O concentration was 20% or more and the sum of the concentrations of Fe and O was 80% or more, it was determined to be an Fe oxide layer.

[0152] The coverage of the Fe oxide layer in the observation field was measured by measuring the length of the area in the plate plane where the Fe oxide layer was 1 μm or more thick, and dividing the length where the Fe oxide layer was 1 μm or more thick by the total width of the observation field. The above measurement was performed in 10 arbitrary fields of view, and the average value was taken as the coverage of the Fe oxide layer.

[0153] (Exterior corrosion resistance) Next, in order to evaluate the appearance and corrosion resistance of the obtained high strength steel members, the coating blister from the painted edge and the occurrence of red rust from the painted edge were tested according to the following procedure.

[0154] First, a 70 mm wide region was cut out of the obtained hat-shaped high-strength steel member using a laser cutter, and the test piece was subjected to zinc phosphate-based conversion treatment and electrodeposition coating to obtain a corrosion resistance test piece. The zinc phosphate-based conversion treatment was performed under standard conditions using PB-SX35 manufactured by Nihon Parkerizing Co., Ltd. The electrodeposition coating was performed using Electron GT-100 manufactured by Kansai Paint Co., Ltd. so that the coating film thickness was 5 μm. The baking condition for the electrodeposition coating was to hold for 20 minutes after reaching 170°C.

[0155] The obtained corrosion resistance test pieces were subjected to a cyclic corrosion test (SAE-J2334) without masking, and the corrosion condition after 40 cycles was evaluated. The appearance corrosion resistance of the painted edge was judged based on the width of the paint blister from the edge and the occurrence of red rust on the cut edge, according to the following criteria. A rating of 1 or 2 for both the paint blister width and the red rust area rate on the edge was considered to be pass. The evaluation results are shown in the table. Note that when the paint blister width was more than 1 mm, red rust had occurred in the cross-cut scratches. 1: Paint blister width ≦1mm and no red rust in cross-cut scratches 2: Paint blister width ≦1mm and red rust present in cross-cut scratches 3: 1mm<paint blister width≦3mm 4: Paint blister width > 3mm

[0156] (resistance weld crack resistance) Furthermore, in order to evaluate the resistance weld cracking resistance of the obtained high strength steel members, resistance spot welding was performed according to the following procedure, and the occurrence of cracks in the welds was evaluated.

[0157] First, a test piece was cut out from the top plate of a high-strength steel member. On the other hand, a mating member to be used for welding was cut out from a galvannealed steel sheet. The galvannealed steel sheet has a tensile strength of 980 MPa and a coating weight of the zinc coating layer of 50 g / m2. 2 , plate thickness t: 1.6 mm.

[0158] Next, the test piece and the mating material were resistance spot welded together. The conditions of the resistance spot welding were: impact angle θ: 5°, pressure: 3.5 kN, hold time: 0.12 seconds, 0.18 seconds, or 0.24 seconds. The welding current and welding time were adjusted so that the nugget diameter d was 5.9 mm.

[0159] The cross section of the weld formed by the resistance spot welding was observed, and the resistance weld crack resistance of the weld was evaluated according to the following criteria. If the evaluation was 1 to 3, it was determined that the resistance weld crack resistance of the weld was excellent. The results are shown in Table 2. 1: No cracks longer than 0.1 mm were observed with a hold time of 0.12 seconds. 2: Cracks longer than 0.1 mm were observed at a hold time of 0.12 seconds, but no cracks longer than 0.1 mm were observed at a hold time of 0.18 seconds. 3: Cracks longer than 0.1 mm were observed at a hold time of 0.18 seconds, but no cracks longer than 0.1 mm were observed at a hold time of 0.24 seconds. 4: A crack longer than 0.1 mm was observed at a hold time of 0.24 seconds.

[0160] As can be seen from the results shown in Table 2, the high-strength steel members satisfying the conditions of the present invention were excellent in appearance corrosion resistance and resistance weld cracking properties.

[0161] [Table 1]

[0162] [Table 2]

Claims

1. A high-strength steel member having a hot-pressed member and a Zn-based plating layer on at least one surface of the hot-pressed member, The thickness of the Fe-Zn alloy layer between the hot press member and the Zn-based plating layer is 0 to 1.0 μm; The natural immersion potential in an air-saturated 0.5% by mass NaCl aqueous solution at 25° C. is −1100 to −800 mV based on a silver-silver chloride-saturated potassium chloride electrode, and A high-strength steel member having a Vickers hardness of 400 or more.

2. The amount of Zn deposited on one side of the hot-pressed member is 5 to 100 g / m 2 2. The high strength steel member according to claim 1, wherein

3. 3. The high strength steel member according to claim 1, further comprising an Fe-Al alloy layer between the hot press member and the Zn-based plating layer.

4. The high strength steel member according to any one of claims 1 to 3, wherein a coverage of an Fe oxide layer having a thickness of 1 µm or more between the hot press member and the Zn-based plating layer is 10% or less.

5. A heating step of heating the hot press steel plate; a hot pressing step of hot pressing the heated steel plate to obtain a hot pressed member; and forming a Zn-based plating layer having a Zn content of 70 atomic % or more on at least one surface of the hot-pressed member at a temperature of 250° C. or less.

6. The method for producing a high strength steel member according to claim 5, wherein the steel sheet for hot press use is an Al-plated steel sheet.

7. 7. The method for producing a high-strength steel member according to claim 5 or 6, further comprising, between the hot pressing step and the Zn-based plating step, an oxide removing step of removing oxides present on a surface of the hot-pressed member.

Citation Information

Patent Citations

  • Hot press method for high strength automotive member made of cold rolled or hot rolled steel sheet, or al-based plated or zn-based plated steel sheet, and hot pressed parts

    JP2006051543A

  • Hot press member and method for manufacturing the same

    JP2011246801A

  • Hot-press-molded article and production method for same, and plated steel sheet for use in hot-press molding

    WO2016006232A1

  • Hot-pressed member and steel sheet for hot-pressing, and manufacturing method for hot-pressed member

    WO2022091480A1

  • Plated steel sheet and method of hot-pressing plated steel sheet

    WO2009131233A1

Cited By

  • Steel plate, hot stamping component, manufacturing process therefor, and use thereof

    WO2026223833A1