Method for producing soft nitrided component

The cold working and nitriding process enhances bending fatigue properties of nitrocarburized parts by optimizing steel composition and processing, addressing cost and environmental concerns while maintaining high performance.

JP2024137532AActive Publication Date: 2024-10-07JFE STEEL CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023049081
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-07
Estimated Expiration
2043-03-24

Smart Images

  • Figure 2024137532000003
    Figure 2024137532000003
  • Figure 2024137532000001
    Figure 2024137532000001
  • Figure 2024137532000002
    Figure 2024137532000002
Patent Text Reader

Abstract

To provide a cost-efficient method for producing a soft nitrided component with superior bending fatigue characteristics.SOLUTION: A method for producing a soft nitrided component includes a cold working step where raw steel material is subjected to cold working, thereby producing a precursor with a maximum strength value in the reverse pole figure intensity distribution of 1.5 or more; and a nitriding step where the precursor is nitrided.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a nitrocarburized component. [Background technology]

[0002] In order to address environmental issues such as reducing carbon dioxide emissions, there is a demand for weight reduction in various industrial product parts. Nitriding is a heat treatment that improves the fatigue properties of steel parts while having the advantage of less heat treatment distortion compared to carburizing and quenching. Nitriding is applied to various steel parts, including vehicle gears. Improving fatigue properties allows steel parts to be made smaller, thereby realizing weight reduction in industrial products such as vehicles. Therefore, improving fatigue properties is desired for steel parts.

[0003] Patent Document 1 discloses a structural steel for soft nitriding. This structural steel for soft nitriding contains, by weight, 0.20-0.50% C, 0.03-0.50% Si, 0.30-3.00% Mn, 0.10-1.00% Cr, 0.03-1.00% Mo, 0.01-0.10% Al, 0.03-0.50% V, 0.015-0.070% S, 0-0.040% Pb, and 15 ppm or less O, with the balance being Fe and unavoidable impurities. In this structural steel for soft nitriding, a predetermined relationship is specified between the contents of S, Pb, and oxygen and the target material hardness and the target core hardness. This structural steel for soft nitriding is said to have excellent fatigue strength and machinability, so that it can be used after being machined in the as-rolled, as-forged, normalized, etc. state, and then subjected to soft nitriding and shot peening.

[0004] Patent Document 2 describes a steel for soft nitriding that has excellent bending fatigue strength. This steel for soft nitriding contains, in mass %, the following alloying elements: C: 0.01% to 0.15%, Si: 0.01% to 1.5%, Mn: 0.15% to 2%, Cu: 0.5% to 2%, N: limited to less than 0.005%, and contains one or more of Ti: 0.01% to 0.5%, Nb: 0.005% to 0.5%, and V: 0.05% to 0.5%, with C+N≦Ti / 4.0+Nb / 7.7+V / 4.3, and may further contain, as necessary, one or more of Ni: 0.5% to 2% or less, Cr: 0.1% to 2%, Al: 0.05% to 0.5% or less, S: 0.03% to 0.1%, and Pb: 0.005% to 0.3%, with the balance being Fe and unavoidable impurities. The area ratio of ferrite is 90% or more, and the remainder is made up of carbides and pearlite structures. The average size of pearlite is 20 μm or less. In this soft nitriding steel, Cu is an element that contributes to the age hardening of the core hardness during soft nitriding, and is considered to be essential for obtaining high fatigue strength. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 09-227992 [Patent Document 2] JP 2002-069572 A Summary of the Invention [Problem to be solved by the invention]

[0006] For example, if the addition of a large amount of Cu is required as in the steel for soft nitriding disclosed in Patent Document 2, not only will the manufacturing cost of the steel increase, but it will also lead to high-temperature embrittlement of the steel, which may lead to a decrease in yield due to an increase in cracks after continuous casting and an increase in additional costs due to maintenance. If the addition of a rare metal such as V is required as in the steel for soft nitriding disclosed in Patent Document 1, it may lead to an increase in the manufacturing cost of the steel and an increase in the environmental load. Therefore, it is desired to propose a manufacturing method for soft-nitrided parts that are low-cost and have excellent bending fatigue properties.

[0007] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a method for producing a soft nitrided part having excellent bending fatigue properties at low cost. [Means for solving the problem]

[0008] In order to achieve the above object, a method for producing a nitrided part according to the present invention is as follows.

[0009] [1] A cold working process in which a raw steel material is cold worked to obtain a precursor having a maximum strength value of 1.5 or more in an inverse pole figure intensity distribution; and a nitriding step of nitriding the precursor.

[0010] [2] The method for producing a nitrided part according to the above item [1], wherein the cold working includes at least one element of cold stretching, drawing, and forging.

[0011] [3] The method for producing a soft nitrided part according to the above [1] or [2], wherein in the cold working step, a portion in which the maximum value is 1.5 or more is formed in the precursor.

[0012] [4] The method for producing a nitrided part according to any one of [1] to [3], wherein the cold working step comprises performing the cold working two or more times.

[0013] [5] A method for producing a soft nitrided part described in any one of [1] to [4], wherein in the cold working step, the cold working is repeated until the maximum value becomes 1.5 or more. Effect of the Invention

[0014] According to the present invention, it is possible to provide a method for producing a soft nitrided part having excellent bending fatigue properties at low cost. [Brief description of the drawings]

[0015] [Figure 1] FIG. 2 is a schematic diagram showing the shape of a test piece. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The method for producing a nitrided component according to this embodiment will be described below.

[0017] First, an outline of the method for manufacturing a nitrided component according to this embodiment will be described.

[0018] The manufacturing method of the soft nitrided part according to this embodiment includes a cold working step of cold working a raw steel material to obtain a precursor having a maximum intensity value of 1.5 or more in the inverse pole figure intensity distribution, and a nitriding step of nitriding the precursor.

[0019] According to the manufacturing method of the soft-nitrided component according to the present embodiment, it is possible to provide a soft-nitrided component having excellent bending fatigue characteristics at low cost.

[0020] Hereinafter, the method for manufacturing a nitrided component according to the present embodiment and the nitrided component realized by this manufacturing method will be described in detail.

[0021] An example of a soft-nitrided part realized by the manufacturing method for a soft-nitrided part according to this embodiment (hereinafter referred to as the soft-nitrided part according to this embodiment) is a part that forms a vehicle such as an automobile. Examples of parts in the automobile field include engine crankshafts, timing gears, etc., transmission gears, ring gears, sun gears, planetary gears, etc., of a transmission, steering pinions, worms, etc., of a suspension, and worms for power windows in an interior.

[0022] Nitriding includes both a nitriding treatment in which only nitrogen is introduced into steel, and a soft nitriding treatment in which nitrogen and carbon are introduced into steel at the same time, and both are treatments that do not cause martensitic transformation of steel. Of these, nitriding in this embodiment refers to soft nitriding.

[0023] In the manufacturing method of the nitrocarburized part according to the present embodiment, as described above, the raw steel material is nitrided to manufacture the nitrocarburized part. That is, the main body of the nitrocarburized part according to the present embodiment has a surface layer in which steel is nitrided. As an example, this surface layer is about 0.5 mm from the surface of the main body. This embodiment also includes cases in which the thickness of this surface layer is greater than 0.5 mm. Hereinafter, the raw steel material may be simply referred to as steel.

[0024] The soft-nitrided component according to the present embodiment may be a component in which the main body is combined with another structure that is made of a metal or a metal alloy and has a non-nitrided surface. The soft-nitrided component according to the present embodiment may be a component in which the main body is combined with another structure that is not made of metal.

[0025] The steel used in the manufacturing method of the soft-nitrided part according to the present embodiment may contain Fe (iron) as a main component, and C (carbon), Si (silicon), Mn (manganese), P (phosphorus), S (sulfur), and impurities as other component compositions. It is not excluded that this steel further contains optional components described later.

[0026] This steel may contain, as an optional component, one or more selected from Al (aluminum), N (nitrogen), Cr (chromium), Ti (titanium), Nb (niobium), V (vanadium), Hf (hafnium), Ta (tantalum), Sn (tin), Sb (antimony), Se (selenium), Ca (calcium), Pb (lead), and Bi (bismuth).

[0027] An example of a steel that can be used in the method for producing a soft-nitrided component according to this embodiment is carbon steel for machine construction (S45C) specified in JIS G4051.

[0028] In the following, the contents and effects of each component in particularly suitable steels among the steels that can be used in the manufacturing method of the soft-nitrided component according to the present embodiment will be described in detail. In the following description, when the content is simply stated, it means the content (mass%) in the steel. Note that the steels that can be used in the manufacturing method of the soft-nitrided component according to the present embodiment are not limited to the steels described below.

[0029] The steel that can be used in the manufacturing method of the soft nitrided part according to this embodiment may preferably contain, as a component composition (chemical composition), C: 0.04 mass% or more and 0.35 mass% or less, Si: 0.01 mass% or more and 1.20 mass% or less, Mn: 0.30 mass% or more and 1.80 mass% or less, P: 0.1 mass% or less, S: 0.5 mass% or less, Al: 0.010 mass% or more and 0.300 mass% or less, and N: 0.0250 mass% or less, with the remainder being Fe (iron) and impurities.

[0030] This steel may contain, as optional components, one or more selected from the group consisting of 2.0 mass% or less of Cr (chromium), 1.0 mass% or less of Mo (molybdenum), 1.0 mass% or less of Cu (copper), 1.0 mass% or less of Ni (nickel), and 0.01 mass% or less of B (boron).

[0031] In addition, this steel may contain, as an optional component composition, one or more selected from the group consisting of 0.1 mass% or less of Ti (titanium), 0.1 mass% or less of Nb (niobium), 0.2 mass% or less of V (vanadium), 0.1 mass% or less of Hf (hafnium), and 0.1 mass% or less of Ta (tantalum).

[0032] Furthermore, this steel may contain, as an optional component, at least one selected from the group consisting of 0.1 mass % or less of Sn (tin) and 0.1 mass % or less of Sb (antimony).

[0033] In addition, this steel may contain, as an optional component, one or more selected from the group consisting of 0.3 mass% or less of Se (selenium), 0.1 mass% or less of Ca (calcium), 0.3 mass% or less of Pb (lead), and 0.3 mass% or less of Bi (bismuth).

[0034] The C content may be 0.04% by mass or more and 0.35% by mass or less. In order to increase the central hardness after nitriding, the C content is preferably 0.04% by mass or more. If the C content exceeds 0.35% by mass, the load during cold working increases, which may shorten the life of the die. The C content is preferably 0.05% by mass or more and 0.27% by mass or less, more preferably 0.10% by mass or more and 0.25% by mass or less.

[0035] The Si content may be 0.01% by mass or more and 1.20% by mass or less. In nitriding steel, Si serves as a deoxidizer. Excessive Si content in steel may reduce the cold workability of the steel material and may reduce the fatigue strength through a reduction in the toughness of the steel. The Si content is preferably 0.05% by mass or more and 0.70% by mass or less, more preferably 0.10% by mass or more and 0.50% by mass or less.

[0036] The Mn content may be 0.30% by mass or more and 1.80% by mass or less. Mn improves hardenability and strengthens the pre-nitriding structure of steel, thereby strengthening the post-nitriding structure (nitrided steel). In order to obtain sufficient fatigue strength, the Mn content should be 0.30% by mass or more. If the steel contains excessive Mn, it may lead to an increase in deformation resistance. The Mn content is preferably 0.40% by mass or more and 1.70% by mass or less, and more preferably 0.50% by mass or more and 1.30% by mass or less.

[0037] The P content may be 0.1 mass% or less. Since P segregates at the grain boundaries of nitrided steel and reduces toughness, the lower the P content, the more desirable it is. The P content is permitted up to 0.1 mass%. The P content is preferably 0.02 mass% or less. Although there is no problem if the lower limit of the P content is not particularly limited, since the inclusion of P is usually unavoidable, unnecessary reduction in P content may increase the refining time and the refining cost. Therefore, it is reasonable and preferable to set the P content to 0.003 mass% or more.

[0038] The S content may be 0.5% by mass or less. S exists as sulfide-based inclusions and is an element effective in improving machinability. Excessive S inclusion in steel may lead to a decrease in cold workability. There is no particular limit to the S content, but since the inclusion of S is usually unavoidable, excessive reduction in S content may increase refining costs. Therefore, it is reasonable to set the S content to 0.003% by mass or more. The S content is preferably 0.004% by mass or more and 0.3% by mass or less, and more preferably 0.005% by mass or more and 0.09% by mass or less.

[0039] The Al content may be 0.010% by mass or more and 0.300% by mass or less. Al forms oxides and is an element effective in deoxidizing nitrided steel. Furthermore, Al has the effect of suppressing the formation of coarse oxide-based inclusions in nitrided steel. If the Al content is less than 0.010% by mass, these effects may not be obtained. Excessive Al inclusion in steel may lead to an increase in inclusions (Al oxides), which may increase the starting points of fatigue fracture and cause low fatigue strength.

[0040] The N content may be 0.0250% by mass or less. N combines with Al to form nitride (AlN). Finely precipitated AlN has the effect of increasing the hardness of steel after nitriding (nitrided steel). Excessive N inclusion in steel may lead to surface cracking of the steel billet after casting. There is no particular limit to the N content, but since the inclusion of N is usually unavoidable, excessive reduction in N content may increase refining costs. The N content is 0.0010% by mass or more, preferably 0.0015% by mass or more. The N content is preferably 0.0180% by mass or less, more preferably 0.0020% by mass or more and 0.0150% by mass or less.

[0041] The Cr content may be 2.0 mass% or less. Cr contributes to improving hardenability and temper softening resistance, and is also a useful element for promoting spheroidization of carbides. If the Cr content exceeds 2.0 mass%, the Cr nitride layer formed on the surface after soft nitriding becomes thick, which may hinder the penetration of N into the inside and lead to insufficient hardness. The Cr content is preferably 0.40 mass% or more and 1.90 mass% or less, and more preferably 0.70 mass% or more and 1.75 mass% or less.

[0042] The Mo content may be 1.0 mass% or less. Mo improves hardenability and strengthens the pre-nitriding structure, thereby strengthening the post-nitriding structure. However, if the Mo content is 1.0 mass% or more, the hardenability becomes excessive, the hardness after rolling increases, and the workability and machinability may decrease. In order to realize the effect of Mo in improving the strength of the steel material, it is preferable to contain Mo in an amount of 0.01 mass% or more in the steel. The Mo content is more preferably 0.03 mass% or more and 0.50 mass% or less, and further preferably 0.05 mass% or more and 0.25 mass% or less.

[0043] The Cu content may be 1.0 mass% or less. Cu improves hardenability and strengthens the pre-nitriding structure, thereby strengthening the post-nitriding structure. In order to obtain this effect, it is preferable to contain Cu in an amount of 0.01 mass% or more in the steel. If the Cu content exceeds 1.0 mass%, the surface of the rolled material may become rough, and there is a concern that these may remain as defects. The Cu content is more preferably 0.015 mass% or more and 0.5 mass% or less, and even more preferably 0.03 mass% or more and 0.3 mass% or less.

[0044] The Ni content may be 1.0 mass% or less. Ni is an element useful for improving toughness. In order to obtain these effects, it is preferable to contain Ni in an amount of 0.01 mass% or more in the steel. Even if the Ni content in the steel exceeds 1.0 mass%, the above effects are saturated. The Ni content is more preferably 0.015 mass% or more and 0.5 mass% or less, and further preferably 0.03 mass% or more and 0.3 mass% or less.

[0045] The content of B may be 0.01% by mass or less. B segregates at grain boundaries and inhibits diffusion-type transformation, which is effective in improving hardenability, and also has the effect of strengthening grain boundaries, inhibiting the occurrence and progression of fatigue cracks, and improving fatigue strength. In order to obtain this effect of B, it is preferable to contain B in steel at 0.0003% by mass or more. If the content of B exceeds 0.01% by mass, the toughness of the steel decreases, so the content of B is preferably 0.01% by mass or less. The content of B is more preferably 0.0005% by mass or more and 0.005% by mass or less, and even more preferably 0.0007% by mass or more and 0.002% by mass or less.

[0046] The Ti content may be 0.1 mass% or less. Ti improves the strength of the steel by combining with carbon and nitrogen to form fine precipitates during soft nitriding. However, even if the Ti content in the steel exceeds 0.1 mass%, the effect is saturated. The Ti content is preferably 0.005 mass% or more and 0.08 mass% or less, and more preferably 0.01 mass% or more and 0.06 mass% or less.

[0047] The Nb content may be 0.1 mass% or less. Nb improves the strength of the steel by combining with carbon and nitrogen to form fine precipitates during soft nitriding. However, even if the Nb content in the steel exceeds 0.1 mass%, the effect is saturated. The Nb content is preferably 0.005 mass% or more and 0.08 mass% or less, and more preferably 0.01 mass% or more and 0.06 mass% or less.

[0048] The V content may be 0.2 mass% or less. V combines with carbon and nitrogen to form fine precipitates during soft nitriding, thereby improving the strength of the steel. In order to obtain this effect of V, it is preferable to contain at least 0.003 mass% or more of V in the steel. If the V content in the steel exceeds 0.2 mass%, the alloy cost will increase and the effect will saturate. The V content is more preferably 0.005 mass% or more and 0.15 mass% or less, and further preferably 0.01 mass% or more and 0.10 mass% or less.

[0049] The Hf content may be 0.1 mass% or less. Hf improves the strength of steel by combining with carbon and nitrogen and forming fine precipitates during soft nitriding. In order to obtain this effect of Hf, it is preferable to contain at least 0.003 mass% or more of Hf in the steel. If the Hf content in the steel exceeds 0.1 mass%, coarse precipitates may be generated during casting and solidification, which may lead to deterioration of fatigue strength. The Hf content is more preferably 0.005 mass% or more and 0.06 mass% or less, and even more preferably 0.01 mass% or more and 0.05 mass% or less.

[0050] The Ta content may be 0.1% by mass or less. Ta improves the strength of steel by combining with carbon and nitrogen to form fine precipitates during soft nitriding. In order to obtain this effect of Ta, it is preferable to contain Ta in steel at least 0.003% by mass or more. On the other hand, if the Ta content exceeds 0.1% by mass, cracks are likely to occur during casting and solidification, and defects may remain even after rolling and forging. The Ta content is more preferably 0.005% by mass or more and 0.06% by mass or less, and even more preferably 0.01% by mass or more and 0.05% by mass or less.

[0051] The Sb content may be 0.1 mass% or less. Sb is an element effective in suppressing decarburization of the steel surface and preventing a decrease in surface hardness. In order to realize this effect, it is preferable to contain Sb in the steel at 0.0003 mass% or more. If an excessive amount of Sb is contained in the steel, the workability of the steel decreases. The Sb content is more preferably 0.001 mass% or more and 0.05 mass% or less, and further preferably 0.0015 mass% or more and 0.035 mass% or less.

[0052] The Sn content may be 0.1 mass% or less. Sn is an element effective for improving the corrosion resistance of the steel surface. From the viewpoint of improving the corrosion resistance, it is preferable that the steel contains 0.003 mass% or more of Sn. If the steel contains an excessive amount of Sn, the workability decreases. The Sn content is more preferably 0.0010 mass% or more and 0.050 mass% or less, and further preferably 0.0015 mass% or more and 0.035 mass% or less.

[0053] The Se content may be 0.3 mass% or less. Se improves machinability by combining with Mn and Cu and dispersing as precipitates in the steel. To obtain this effect, it is preferable to contain at least 0.001 mass% Se in the steel. Even if the Se content in the steel exceeds 0.3 mass%, the effect is saturated. The Se content is more preferably 0.005 mass% to 0.1 mass%, and further preferably 0.008 mass% to 0.09 mass%.

[0054] The Ca content may be 0.1% by mass or less. Ca improves machinability by combining with S and dispersing in the steel as sulfides. To obtain this effect, it is preferable to contain at least 0.0005% by mass of Ca in the steel. If the Ca content in the steel exceeds 0.1% by mass, the effect is saturated. The Ca content is more preferably 0.0010% by mass or more and 0.0500% by mass or less, and further preferably 0.0015% by mass or more and 0.0300% by mass or less.

[0055] The Pb content may be 0.3% by mass or less. Pb has the effect of refining chips during cutting. Addition of Pb is effective when it is desired to improve chip disposability. To obtain this effect, it is preferable to contain 0.01% by mass or more of Pb in the steel. Even if excessive Pb is contained in the steel, the effect of improving chip disposability becomes saturated. The Pb content is preferably 0.01% by mass or more and 0.2% by mass or less, and more preferably 0.01% by mass or more and 0.1% by mass or less.

[0056] The Bi content may be 0.3 mass% or less. Bi has the effect of refining chips during cutting. Addition of Bi is effective when it is desired to improve chip disposability. To obtain this effect, it is preferable to contain Bi at 0.01 mass% or more. Even if an excessive amount of Bi is contained in the steel, the effect of improving chip disposability becomes saturated. The Bi content is preferably 0.01 mass% or more and 0.2 mass% or less, and more preferably 0.01 mass% or more and 0.1 mass% or less.

[0057] The balance other than the above-described elements is Fe and impurities. The impurities are substances that are mixed in from raw materials such as ore and scrap, or from the manufacturing environment during industrial production of steel material, and are allowed within a range that does not adversely affect the characteristics of this embodiment.

[0058] When steel is cold worked, crystal orientation rotation occurs according to the working style. As the amount of working increases, the crystal orientation rotation becomes more pronounced, and the accumulation of crystal orientations progresses. The inverse pole figure intensity distribution obtained by EBSD (electron backscatter diffraction) is a representative index showing the degree of accumulation of crystal orientations. When the maximum value of strength in the inverse pole figure intensity distribution is 1.5 or more, the fatigue strength of the steel is improved. To sufficiently improve the fatigue strength of steel, the maximum value of strength in the inverse pole figure intensity distribution is preferably 1.7 or more, and more preferably 2.0 or more.

[0059] In the soft nitrided component of this embodiment, the maximum strength value in the inverse pole figure intensity distribution measured in a direction parallel to the component surface at a depth of 0.5 mm from the surface of the body is 1.5 or more.

[0060] The cold working in this embodiment includes working including at least one element of cold tensile working (cold tensile working), cold drawing, and cold forging (cold forging). Specifically, for example, gear forming, spline forming, drawing (diameter reduction) forming, forward extrusion forming, backward extrusion forming, gear forming by cold rolling, and spline forming are also included in the cold working in this embodiment.

[0061] There is no limit to the number of cold working steps that the steel may undergo, for example, the steel may be cold worked only once to provide a maximum strength value of 1.5 or more in the inverse pole figure intensity distribution of the precursor.

[0062] Also, for example, the steel may be subjected to cold working multiple times (two or more times) to make the maximum strength value in the inverse pole figure intensity distribution of the precursor 1.5 or more.

[0063] Also, using the maximum value of the strength in the inverse pole figure intensity distribution of the precursor as a guideline, cold working may be repeated until this maximum value becomes 1.5 or more.

[0064] When cold working steel, the amount of deformation per cold working step is arbitrary.

[0065] The crystal orientation rotation due to cold working occurs regardless of the composition and structure of the steel, and the orientation accumulation behavior depends on the processing mode. Therefore, the manufacturing method of the soft-nitrided part according to the present embodiment is applicable to all steel materials as the raw steel material, and is not limited to the example of the present embodiment. EXAMPLES

[0066] Hereinafter, the steel according to the present embodiment will be described based on examples, but the steel according to the present embodiment is not limited to these examples.

[0067] Example 1 Carbon steel for machine construction (S45C) specified in JIS G4051 was formed into a round bar (an example of raw steel material) with a diameter of 20 mm by hot rolling.

[0068] Next, this round bar was subjected to cold drawing (an example of cold working) to produce a round bar-shaped precursor. As shown in Table 1, the precursors were produced by changing the number of cold drawing processes from one to three, and by changing the diameter of the die used in the cold drawing process (precursor Nos. 2 to 6). As a comparison control for the precursors produced by cold drawing, a round bar that was not cold drawn was secured (precursor No. 1).

[0069] Fifteen of each of precursors No. 1 to 6 were prepared.

[0070] The diameters of precursors No. 2 to 6 and the cumulative area reduction (%) in repeated cold drawing are shown in Table 1. The cumulative area reduction is the reduction rate of the cross-sectional area intersecting the axial direction when a round bar with a diameter of 20 mm is processed into a precursor.

[0071] Next, a part of each of these round bars or precursors (precursor Nos. 1 to 6) was cut to obtain Ono-type rotating bending fatigue test pieces (hereinafter simply referred to as test pieces) having a parallel part with a diameter of 10 mm.

[0072] FIG. 1 shows a schematic diagram of the shape of the test piece. The test piece is linear along the axis G, and the cross section perpendicular to the axis G is a circular rod shape whose center overlaps with the axis G. Both ends of the test piece in the direction along the axis G are gripping parts 1,1 described later. A parallel part 2 is disposed between the gripping parts 1,1 in the direction along the axis G. In this embodiment, the diameter of the parallel part 2 shown in FIG. 1 is 10 mm. Also, the diameter of the gripping parts 1,1 is 12 mm. The length between the gripping parts 1,1 including the parallel part 2 is 30 mm. Both ends of the parallel part 2 in the direction along the axis G are narrowed into a curved shape of R15 from the end of the gripping part 1 to the center in the axial direction.

[0073] [Table 1]

[0074] Next, five randomly selected test pieces from the 15 test pieces corresponding to each precursor were measured by the EBSD method to obtain the inverse pole figure intensity distribution and the maximum strength value of each test piece. Then, the average value of the maximum strength values ​​of the five test pieces corresponding to each precursor (hereinafter, sometimes referred to as the average strength value) was obtained. The inverse pole figure intensity distribution was obtained for a cross section overlapping with the central axis (axis center G shown in FIG. 1) of the cross section perpendicular to the longitudinal direction at the gripping part of the test piece.

[0075] The cross section was measured by cutting the gripping portion in the longitudinal direction to expose the cross section.

[0076] The calculation of the inverse pole figure intensity distribution based on the measurement results by the EBSD method was performed using the crystal orientation analysis software OIM manufactured by TSL, Inc. For the measurement by the EBSD method, a scanning electron microscope (manufactured by JEOL Ltd., model: JSM-7001F) was used.

[0077] The measurement field of view for the EBSD method was a square region with one side measuring 0.5 mm, and the inverse pole figure intensity distribution was analyzed in the direction along the central axis (axis center G) mentioned above (the same as the tensile axis direction in the fatigue test described below) using the spherical harmonics method under the conditions of Series Rank: 13, Gaussian Smoothing: 5.0°, and Sample Symmetry: Triclinic.

[0078] Next, of the 15 test pieces corresponding to each precursor, the remaining 10 test pieces were subjected to a gas soft-nitriding heat treatment (nitriding) at 570°C for 3 hours to obtain post-treatment test pieces (an example of a soft-nitrided part) (an example of a nitriding process). The nitriding treatment was carried out in a mixed gas containing ammonia and carbon monoxide.

[0079] Next, the treated test pieces corresponding to each precursor were subjected to a rotating bending fatigue test at a stress amplitude of 500 MPa, and the fatigue fracture life (times) was measured as the fatigue strength of each, and the average fatigue fracture life (average fatigue strength, times) of 10 treated test pieces corresponding to each precursor was calculated. Note that the larger the average fatigue fracture life, the better the bending fatigue properties, which is preferable. The average fatigue fracture life for each precursor is also shown in Table 1.

[0080] Furthermore, the improvement rate of fatigue fracture life due to cold drawing was calculated for each of the treated test pieces corresponding to precursor Nos. 2 to 6. The improvement rate of fatigue fracture life due to cold drawing is the average value of the fatigue fracture life of precursor Nos. 2 to 6 divided by the average value of the fatigue fracture life of the round bar (precursor No. 1). The larger the improvement rate of fatigue fracture life, the better the bending fatigue properties, which is preferable. The improvement rate of fatigue fracture life corresponding to each precursor is also shown in Table 1.

[0081] When the fatigue fracture life of the treated test specimen (nitrocarburized part) is extended (i.e., when the fatigue fracture life improvement rate exceeds 1) compared with the fatigue fracture life of the treated test specimen (precursor No. 1) that was nitrided without cold drawing, it can be said that the bending fatigue properties of the treated test specimen are superior.

[0082] As shown in Table 1, the improvement rate of fatigue fracture life increases as the average strength value of the test piece (precursor) increases. Therefore, it can be seen that the bending fatigue properties of the test piece (nitrocarburized part) after treatment become excellent as the average strength value increases.

[0083] Among these, when the fatigue fracture life of the treated test piece (nitrogen-nitrided part) is more than twice as long as the fatigue fracture life of the treated test piece (precursor No. 1) that was nitrided without cold drawing (i.e., the fatigue fracture life improvement rate is 2 or more), it can be said that the bending fatigue properties of the treated test piece are particularly excellent.

[0084] As shown in Table 1, when the average strength value of the test piece (precursor) is 1.5 or more, the fatigue fracture life improvement rate is 2 or more. Therefore, it can be seen that when the average strength value is 1.5 or more, the bending fatigue properties of the treated test piece (nitrocarburized part) are excellent. It can also be seen that the larger the average strength value of the test piece (precursor), the more the fatigue fracture life improvement rate improves, and that the larger the average strength value of the test piece (precursor), the more excellent the bending fatigue properties of the treated test piece (nitrocarburized part).

[0085] Example 2 First, steels (steels No. 1 to 31) having the chemical compositions shown in Table 2 were melted and formed into round bars (examples of raw steel materials) having a diameter of 20 mm by hot rolling.

[0086] Then, this round bar was subjected to cold tensile processing (an example of cold processing) to produce a round bar-shaped precursor with a diameter of 16 mm (an example of a cold processing process), and then a portion of this precursor was cut to obtain an Ono-type rotating bending fatigue test specimen (hereinafter simply referred to as the test specimen) with a parallel portion diameter of 10 mm.

[0087] In this example, the test piece has the same shape as the test piece according to Example 1 (see FIG. 1).

[0088] [Table 2]

[0089] The specimen was then subjected to EBSD measurement to obtain the inverse pole figure strength distribution and the maximum strength value. The inverse pole figure strength distribution was obtained for a cross section overlapping with the central axis (axis G shown in Figure 1) of the cross section perpendicular to the longitudinal direction at the gripping part of the specimen.

[0090] The cross section was measured by cutting the gripping portion in the longitudinal direction to expose the cross section.

[0091] The calculation of the inverse pole figure intensity distribution based on the measurement results by the EBSD method was performed in the same manner as in Example 1.

[0092] The measurement field of view range in the EBSD method and the analysis conditions for the inverse pole figure intensity distribution were also the same as in Example 1.

[0093] Next, this test piece was subjected to gas soft-nitriding heat treatment (nitriding) at 570℃ for 3 hours to obtain a post-treatment test piece (an example of a soft-nitrided part) (an example of a nitriding process). The nitriding treatment was carried out in a mixed gas containing ammonia and carbon monoxide.

[0094] Next, for the treated test pieces of each component composition, the treated test pieces were separated into those with a maximum strength value of 1.5 or more in the inverse pole figure strength distribution and those without. Then, the treated test pieces with a maximum strength value of 1.5 or more in the pole figure strength distribution and those without were subjected to a rotating bending fatigue test, and the fatigue limits (1×10 7 The equivalent stress (stress) was evaluated.

[0095] As shown in Table 2, it can be seen that the post-processing test pieces (nitrogen-nitrided parts, with a maximum strength value of 1.5 or more in the pole figure intensity distribution) manufactured by the manufacturing method of a soft-nitrided part according to this embodiment have significantly superior bending fatigue properties compared to those manufactured by a manufacturing method not according to this embodiment.

[0096] Thus, the steel forming the test piece (main body of the soft-nitrided part) after treatment according to this embodiment has excellent fatigue properties, despite being low cost and not requiring the inclusion of large amounts of relatively expensive metals such as Cu.

[0097] Moreover, the steel forming the post-treatment test piece (main body of the soft-nitrided part) according to this embodiment does not require the addition of a rare metal such as V, is low cost, and yet has excellent fatigue properties.

[0098] The treated test specimens were measured using the EBSD method to determine the inverse pole figure intensity distribution and the maximum strength value. The maximum strength value of the inverse pole figure intensity distribution of each treated test specimen was the same as the maximum strength value of the inverse pole figure intensity distribution of the corresponding test specimen before nitriding (the state of each treated test specimen before nitriding).

[0099] The inverse pole figure strength distribution was obtained for a portion 0.5 mm deep from the surface of the gripped portion of the treated test piece. The measurement of the portion 0.5 mm deep from the surface of the gripped portion of the treated test piece was performed by cutting a part of the surface of the gripped portion (position 3 in Figure 1 as an example) 0.5 mm below the surface to expose that portion.

[0100] That is, the maximum intensity value of the inverse pole figure intensity distribution inside the test piece (in this embodiment, a portion 0.5 mm deep from the surface) was the same before and after nitriding the test piece.

[0101] In this manner, a method for producing a soft nitrided part having excellent bending fatigue properties at low cost can be provided.

[0102] It should be noted that the embodiments disclosed in this specification are merely examples, and the present invention is not limited to these embodiments, and can be modified as appropriate without departing from the scope of the present invention. [Industrial Applicability]

[0103] The present invention can be applied to a method for manufacturing a soft nitrided part. [Explanation of symbols]

[0104] 1: Grip part 2: Parallel section G: Axial center

Claims

1. a cold working step of cold working a raw steel material to obtain a precursor having a maximum intensity value of 1.5 or more in an inverse pole figure intensity distribution; and a nitriding step of nitriding the precursor.

2. The method for producing a nitrided part according to claim 1, wherein the cold working includes at least one element of cold stretching, drawing, and forging.

3. The method for producing a soft nitrided part according to claim 1 , wherein in the cold working step, a portion in which the maximum value is 1.5 or more is formed in the precursor.

4. The method for producing a soft nitrided part according to claim 2 , wherein in the cold working step, a portion in which the maximum value is 1.5 or more is formed in the precursor.

5. The method for producing a soft nitrided part according to any one of claims 1 to 4, wherein in the cold working step, the cold working is performed two or more times.

6. The method for producing a soft nitrided part according to any one of claims 1 to 4, wherein in the cold working step, the cold working is repeated until the maximum value becomes 1.5 or more.

7. The method for producing a soft nitrided part according to claim 5 , wherein in the cold working step, the cold working is repeated until the maximum value becomes 1.5 or more.

Citation Information

Patent Citations

  • Steel for soft-nitriding

    JP1997071841A

  • Steel for cold forging / nitriding, steel material for cold forging / nitriding and cold-forged / nitrided component

    JP2012087361A

  • Rolled steel for cold forging / nitriding

    JP2013159794A

  • Cold forging and nitriding steel, cold forging and nitriding steel material, and cold forged and nitrided component

    JP2013185186A

  • Soft-nitriding steel for structural purpose

    JP1997227992A