Method for manufacturing eye joint with whirl-stop pin

By spot welding a detent pin made of carbon steel with a specific carbon content and subsequent annealing, the method addresses the inefficiencies and high costs of conventional eye joint manufacturing, enhancing the strength and simplifying the process.

JP2024137678APending Publication Date: 2024-10-07NICHIRIN CO LTD +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023214546
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-23
Filing Date
2023-12-20
Publication Date
2024-10-07

AI Technical Summary

Technical Problem

Conventional methods for manufacturing eye joints with detent pins are time-consuming and increase manufacturing costs due to the need for complex processes like forming a recess and brazing, which do not effectively improve welding strength.

Method used

A method involving spot welding a detent pin made of carbon steel with a carbon content of 0.42% to 0.48% to the outer peripheral surface of an eye joint, followed by an annealing process to enhance the toughness of the welded part, thereby simplifying the coupling process and reducing costs.

Benefits of technology

The method improves the strength of the welded part by using carbon steel with specific carbon content and annealing, allowing for a simpler and more cost-effective manufacturing process while maintaining the integrity of the eye joint.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137678000001_ABST
    Figure 2024137678000001_ABST
Patent Text Reader

Abstract

To provide a method for manufacturing an eye joint with a whirl-stop pin, capable of reducing a manufacturing cost.SOLUTION: A manufacturing method for an eye joint with a whirl-stop pin, which is formed by combining an eye joint 1 having a socket 11 at one end part and an annular part 12 with a whirl-stop pin 2, comprises: a welding process for spot-welding the whirl-stop pin 2 to an outer peripheral surface of the annular part 12 using carbon steel with a carbon content of 0.42 wt.% or more and 0.48 wt.% or less as a material for the whirl-stop pin 2; and an annealing process for annealing the eye joint 1 to which the whirl-stop pin 2 is spot-welded.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing an eye joint with a locking pin. [Background technology]

[0002] For example, the brakes of an automobile are activated when the pedal force is converted into hydraulic pressure, and the brake oil that transmits the hydraulic pressure is sent to the brake caliper through the brake hose. Such brake hoses generally have an eye joint attached to the end, and are connected to the brake caliper via the eye joint.

[0003] An eye joint is generally fixed with a bolt that is inserted into its annular portion. To prevent the eye joint from rotating when fixed with the bolt, it is known to provide a locking pin on the annular portion of the eye joint (for example, Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2019-027464 A Summary of the Invention [Problem to be solved by the invention]

[0005] In order to connect the anti-rotation pin to the annular part of the eye joint, a recess is generally formed on the side of the annular part, and the anti-rotation pin is press-fitted into the recess and brazed. For example, the eye joint of Patent Document 1 does not have a recess, but in order to improve the welding strength of the anti-rotation pin, the joint part with the eye joint is curved for the anti-rotation pin, and a protrusion is provided on the curved surface for welding. However, the above conventional method is time-consuming and increases the manufacturing cost.

[0006] SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to provide a method for manufacturing an eye joint with a rotation-prevention pin that can reduce manufacturing costs. [Means for solving the problem]

[0007] The manufacturing method of the eye joint with a rotation prevention pin of the present invention is a manufacturing method of an eye joint with a rotation prevention pin, which is formed by combining an eye joint having a cylindrical portion at an end and a circular portion, and a rotation prevention pin, The material of the anti-rotation pin is carbon steel having a carbon content of 0.42% by weight or more and 0.48% by weight or less, a welding step of spot welding the anti-rotation pin to an outer peripheral surface of the annular portion; an annealing process for annealing the eye joint to which the anti-rotation pin is spot-welded; Equipped with. Effect of the Invention

[0008] According to the present invention, a locking pin is spot welded to the eye joint. Even if the locking pin hardens and becomes brittle due to the heat of spot welding, reducing the strength of the welded portion, the strength of the welded portion can be improved by using carbon steel with a carbon content of 0.42% by weight to 0.48% by weight as the material for the locking pin and by performing an annealing process thereafter, thereby increasing the toughness of the welded portion. As a result, a simple method can be used to connect the locking pin to the eye joint, reducing manufacturing costs. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a perspective view showing an example of an eye joint 100 with a locking pin. [Diagram 2] FIG. 2 is a vertical cross-sectional side view showing an example of an eye joint 100 with a rotation-stop pin. [Diagram 3] FIG. 2 is a schematic diagram showing how anti-rotation pin 2 is spot-welded to eye joint 1. [Figure 4]1 is a diagram showing the state in which the anti-rotation pin eye joint 100 is installed on the jig 3 when measuring the strength of the anti-rotation pin. FIG. [Diagram 5] FIG. 2 is an explanatory diagram showing another example of the eye joint 1. [Figure 6] 2 is an exploded perspective view of a welding jig and an explanatory diagram showing the positions of an eye joint 10 and a locking pin 2 relative to the welding jig in a welding process. FIG. [Figure 7] 2 is a cross-sectional view of the welding jig body 40 showing the positional relationship between a first cavity 61, a second cavity 62, and a third cavity 63 in the welding jig body 40. FIG. [Figure 8] 13 is a schematic diagram for explaining the positioning of anti-rotation pin 2 relative to eye joint 10 using pin jig 50. FIG. [Figure 9] 1 is an explanatory diagram showing the positional relationship among a welding jig, an eye joint 10, a locking pin 2, and welding electrodes during welding. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.

[0011] (Configuration of the eye joint 100 with anti-rotation pin) As shown in FIG. 1, an eye joint with a rotation prevention pin 100 of this embodiment is formed by combining an eye joint 1 and a rotation prevention pin 2.

[0012] (Eye Joint 1) As shown in FIGS. 1 and 2, the eye joint 1 has a socket 11 as a cylindrical portion, an annular portion 12, a neck portion 13, and a nipple 14.

[0013] The socket 11 is provided at one end of the eye joint 1. The socket 11 has an insertion portion 11a provided therein (see FIG. 2). The insertion portion 11a provided therein has a tubular shape. The socket 11 and the insertion portion 11a have the same axis.

[0014] The annular portion 12 is provided at the other end of the eye joint 1. The annular portion 12 is an annular member having a through hole 12b through which a bolt for fixing is inserted. The annular portion 12 is provided with a driving hole 12a (see FIG. 2) penetrating the side wall surface of the annular portion 12 at approximately the center between its upper and lower surfaces. The tip of the neck portion 13 is driven into the driving hole 12a, and the corresponding parts are joined by copper brazing.

[0015] Neck portion 13 is formed integrally with socket 11, has a cylindrical shape thinner than socket 11, and has a communication hole 13a (see FIG. 2) formed therein. As described above, the tip of neck portion 13 is driven into driving hole 12a of annular portion 12, whereby socket 11 and annular portion 12 are connected to each other.

[0016] The nipple 14 is a cylindrical member whose outer diameter is formed to match the communication hole 13a, and a fluid hole 14a is formed inside. The tip of the nipple 14 is driven into the communication hole 13a, and this part is joined by copper brazing. As a result, the fluid hole 14a of the nipple 14 is communicated with the through hole 12b formed in the annular portion 12 via the communication hole 13a. In addition, since the socket 11 is configured into a socket type by joining the nipple 14, it is possible to insert and connect, for example, a brake hose or the like into the insertion portion 11a.

[0017] The socket 11, the annular portion 12, the neck portion 13 and the nipple 14 are configured so that the axis of the insertion portion 11a provided in the socket 11, the axis of the driving hole 12a provided in the annular portion 12 and the axis of the communicating hole 13a provided in the neck portion 13, and the axis of the fluid hole 14a provided in the nipple 14 coincide with each other.

[0018] The shape of eye joint 1 is not limited as long as it does not cause any problems in practical use of the hydraulic brake system. Also, the material of eye joint 1 may be any material as long as it does not cause any problems in practical use of the hydraulic brake system.

[0019] In this embodiment, the material of the eye joint 1 is, for example, carbon steel. Specifically, the material of the eye joint 1 is carbon steel containing 0.10% by weight or more and 0.15% by weight or less of carbon. More specifically, the material of the eye joint 1 is cold heading carbon steel SWCH12A or SWCH12R.

[0020] (Anti-rotation pin 2) The anti-rotation pin 2 is provided on the outer circumferential surface of the annular portion 12. In this embodiment, the anti-rotation pin 2 is provided at a position facing the socket 11, but is not limited to this. The anti-rotation pin 2 may be provided at any other position on the outer circumferential surface of the annular portion 12, or may be provided at multiple positions. In addition, the shape of the anti-rotation pin 2 in this embodiment is cylindrical, but is not limited to this, and may be L-shaped, etc.

[0021] In this embodiment, the material of the anti-rotation pin 2 is carbon steel containing 0.42% by weight or more and 0.48% by weight or less of carbon. More specifically, the material of the anti-rotation pin 2 is SWCH45K, a cold heading carbon steel. In this way, the anti-rotation pin 2 is made of carbon steel containing a larger amount of carbon than the eye joint 1.

[0022] (Manufacturing method of eye joint 100 with anti-rotation pin: welding process) First, a welding process is performed in which the anti-rotation pin 2 is spot-welded to the eye joint 1. As shown in Fig. 3, the anti-rotation pin 2 preferably has a tapered portion 2a that is machined into a tapered shape at the end on the side to be spot-welded. This increases the electrical resistance of the anti-rotation pin 2, so that the heat generated by spot welding can be concentrated more on the tapered portion 2a to melt it. In this way, in this embodiment, no welding material is used, and the tapered portion 2a of the anti-rotation pin 2 is melted and joined to the eye joint 1.

[0023] In this manner, anti-rotation pin 2 is spot welded to eye joint 1. Since anti-rotation pin 2 is made of carbon steel with a carbon content of 0.42% by weight or more and 0.48% by weight or less, it is believed that the heat of the spot welding causes changes in the mechanical properties of anti-rotation pin 2, such as hardening and embrittlement.

[0024] The above-mentioned eye joint 1 is attached to the end of a brake hose (not shown). For example, the end of the brake hose is inserted into the socket 11, and while the brake hose is held by a nipple 14 provided inside the socket 11, the socket 11 is tightened to reduce the diameter, thereby attaching the eye joint 1 to the end of the brake hose.

[0025] The eye joint 1 is not limited to the above-mentioned eye joint 1 for mounting a brake hose, and may be, for example, an eye joint 10 for connecting a pipe. Specifically, the present invention may be applied to a manufacturing method of an eye joint 100 with a rotation stop pin using the eye joint 10 for connecting a pipe shown in FIG. 5. As shown in FIG. 5, the eye joint 10 has a circular ring portion 12 and a cylindrical pipe connection portion 15. One end of the pipe connection portion 15 is integrally formed with the circular ring portion 12, and the other end is connected to the pipe 16. The pipe connection portion 15 and the pipe 16 are connected, for example, by brazing. The pipe 16 is, for example, a double-wrapped steel pipe. In addition, when connecting a socket to the end of the pipe 16, for example, a method described in Japanese Patent No. 6906230 can be used.

[0026] In the following, a specific example of the welding process will be described using the eye joint 10 shown in the example of FIG.

[0027] (Specific examples of welding processes) For example, a welding jig is used to perform a welding process in which the anti-rotation pin 2 is spot-welded to the annular portion 12. As shown in Fig. 6, the welding jig is composed of a welding jig body 40 and a pin jig 50. The welding jig body 40 is used to fix the annular portion 12 and the pipe connection portion 15 in the welding process. The pin jig 50 is used to position the anti-rotation pin 2 with respect to the annular portion 12 in the welding process.

[0028] (Example of welding process: welding jig body 40) The welding jig body 40 has therein a first cavity 61, a second cavity 62, and a third cavity 63. The first cavity 61 is a space for arranging the annular portion 12 and the pipe connection portion 15. The second cavity 62 is a space for arranging the pin jig 50. The third cavity 63 (see FIG. 7) is a space for arranging an electrode for spot welding (for example, an annular portion side electrode rod 70 described with reference to FIG. 9).

[0029] As shown in FIG. 6, the welding jig body 40 is a split-shaped jig and includes a first welding jig body 41 and a second welding jig body 42. The first welding jig body 41 and the second welding jig body 42 have symmetrical fitting holes formed in their respective abutment surfaces 40a that are in abutment with each other. When the first welding jig body 41 and the second welding jig body 42 are in abutment with each other, the symmetrical fitting holes form a first cavity 61 and a second cavity 62. In this embodiment, the welding jig body 40 is formed in a split shape having the first welding jig body 41 and the second welding jig body 42, but is not limited thereto as long as the shape is such that the annular portion 12 and the pipe connection portion 15 can be disposed therein.

[0030] The first welding jig body 41 and the second welding jig body 42 have abutment surfaces 40a that abut against each other. The annular portion 12 and the pipe connection portion 15 are disposed in a first cavity 61 formed in the abutment surfaces 40a. The annular portion 12 and the pipe connection portion 15 are disposed in the first cavity 61 such that the axial direction of the through hole 12b in the annular portion 12 coincides with the direction in which the first welding jig body 41 and the second welding jig body 42 abut against each other.

[0031] Hereinafter, the direction in which the first welding jig body 41 and the second welding jig body 42 are abutted is defined as the front-rear direction X. In the front-rear direction X, the side on which the first welding jig body 41 is located is defined as the front side X1, and the side on which the second welding jig body 42 is located is defined as the rear side X2. The axial direction of the cylindrical pipe connection part 15 of the eye joint 10 is defined as the up-down direction Z. In the up-down direction Z, the direction from the pipe connection part 15 to the annular part 12 in the up-down direction Z is defined as the upper side Z1, and the opposite side is defined as the lower side Z2. The direction perpendicular to each of the front-rear direction X and the up-down direction Z is defined as the lateral direction Y.

[0032] As shown in the upper left part of FIG. 6, the fitting hole of the welding jig body 40 forms a first cavity 61 and a second cavity 62 communicating with the upper side Z1 of the first cavity 61. The annular part 12 and the pipe connection part 15 are fitted into the first cavity 61. When the annular part 12 and the pipe connection part 15 are fitted into the first cavity 61, a part of the upper side Z1 of the annular part 12 protrudes into the second cavity 62. The pin jig 50 is placed in the second cavity 62. The second cavity 62 penetrates the upper side Z1 of the welding jig body 40 so that the pin jig 50 can be placed from the upper side Z1 of the welding jig body 40. Note that only one hole (the fitting hole of the first welding jig body 41) of a pair of fitting holes having a symmetrical shape is shown in the upper left part of FIG. 6 and FIG. 7.

[0033] On contact surface 40a, first welding jig body 41 has a pin hole 412, and second welding jig body 42 has a positioning pin 422 at the opposing position. By inserting positioning pin 422 into pin hole 412, first welding jig body 41 and second welding jig body 42 can be easily joined together.

[0034] 7, the welding jig body 40 is formed with a third cavity 63 penetrating the welding jig body 40 in the front-rear direction X. The third cavity 63 is formed to intersect with a portion where the annular portion 12 is disposed when the annular portion 12 is disposed in the first cavity 61. In this embodiment, the cross-sectional shape of the third cavity 63 is formed to substantially match the cross-sectional shape of the through-hole 12b of the annular portion 12, but is not limited thereto. A ring-side electrode bar 70 (described later) is inserted into the third cavity 63.

[0035] (Example of welding process: pin jig 50) As described above, the pin jig 50 is used to position the anti-rotation pin 2 with respect to the annular portion 12 in the welding process. The pin jig 50 is made of an insulating material, for example, ceramic. As shown in FIG. 8, the pin jig 50 has an annular portion fitting hole 51 and a tubular hole 52. The annular portion fitting hole 51 is formed on the lower side Z2 of the pin jig 50. The annular portion fitting hole 51 is a fitting hole into which a portion of the annular portion 12 protruding into the second hollow portion 62 is fitted. That is, the annular portion fitting hole 51 matches the shape of the annular portion 12 protruding into the second hollow portion 62. The tubular hole 52 communicates with the annular portion fitting hole 51 and is located on the upper side Z1 of the annular portion fitting hole 51. When the anti-rotation pin 2 is disposed in the cylindrical hole 52, the tip portion of the lower side Z2 of the anti-rotation pin 2 comes into contact with the outer circumferential surface of the annular portion 12.

[0036] 8, the cylindrical hole 52 is formed with an escape cavity 52a. The escape cavity 52a is an enlarged portion with an enlarged diameter at the tip portion of the lower side Z2 of the cylindrical hole 52. This allows the melted material of the end portion of the lower side Z2 of the anti-rotation pin 2 to escape to the escape cavity 52a, making it possible to prevent the melted material of the anti-rotation pin 2 from leaking out of the cylindrical hole 52. The escape cavity 52a is formed with a smaller diameter than the thickness of the annular portion 12 in the front-rear direction X. This makes it possible to prevent the melted material of the end portion of the anti-rotation pin 2 from leaking out to the annular portion 12 via the escape cavity 52a.

[0037] (A specific example of a welding process) The welding process includes the following first to third steps. As shown in Fig. 9, in the first step, the annular portion 12 and the pipe connection portion 15 are placed in the first cavity 61. For example, the annular portion 12 and the pipe connection portion 15 are fitted into the first welding jig body 41. Then, the second welding jig body 42 is abutted against the first welding jig body 41 into which the annular portion 12 and the pipe connection portion 15 are fitted, while being positioned by the pin hole 412 and the positioning pin 422.

[0038] In the second step, the pin jig 50 is fitted into the second hollow portion 62. Then, the anti-rotation pin 2 is placed in the cylindrical hole 52 of the pin jig 50, as shown in FIG.

[0039] In the third step, the anti-rotation pin 2 disposed in the cylindrical hole 52 is spot-welded to the outer circumferential surface of the annular portion 12 disposed in the first hollow portion 61. First, as shown in Fig. 9, for example, an annular portion-side electrode rod 70, which is an electrode for spot welding, is inserted into the third hollow portion 63 from the front side X1. As a result, the annular portion-side electrode rod 70 is inserted into the through hole 12b of the annular portion 12 and is electrically connected to the annular portion 12.

[0040] The pin-side electrode 71 is then brought into contact with the anti-rotation pin 2 arranged in the pin jig 50. Then, while applying pressure to the lower side Z2 of the anti-rotation pin 2 with the pin-side electrode 71, a current is applied from a battery (not shown) to perform spot welding. When spot welding is performed, the anti-rotation pin 2 is melted from its tapered tip portion on the lower side Z2 and joined to the outer circumferential surface of the annular portion 12. At this time, the molten material of the anti-rotation pin 2 spreads into the relief cavity 52a, preventing the molten material from leaking out of the cylindrical hole.

[0041] (Manufacturing method of eye joint with anti-rotation pin 100: Annealing process) Next, an annealing process is performed to anneal the eye joint 1 to which the anti-rotation pin 2 is spot welded. The annealing process includes a heating process and a cooling process using, for example, a continuous furnace. Specifically, in the annealing process, the anti-rotation pin eye joint 100 is transported on a belt conveyor at a speed of several tens of mm per minute, and is annealed by passing through a heating furnace and a cooling facility.

[0042] The heating furnace is set at a temperature of, for example, 900° C. to 1150° C., preferably 950° C. to 1120° C., and is preferably filled with a gas atmosphere such as methane or propane to prevent oxidation. The cooling equipment is configured to cool the internal gas from the outside with water, for example. Note that the continuous furnace may have a plurality of heating furnaces and a plurality of cooling equipment.

[0043] In this way, by annealing the anti-rotation pin 2 whose strength has been reduced due to hardening and embrittlement, it is possible to improve the toughness of the welded portion of the anti-rotation pin 2.

[0044] In this annealing process, copper brazing may be performed simultaneously on the above-mentioned places where the neck 13 is driven into the driving hole 12a and the nipple 14 is driven into the communication hole 13a. In this case, by placing a copper ring (not shown) made of a copper wire shaped into a ring near the above-mentioned driving places of the neck 13 and the nipple 14, the copper ring melts due to heat treatment in the annealing process, and the molten copper enters the gap where the neck 13 is driven into the driving hole 12a and the gap where the nipple 14 is driven into the communication hole 13a by capillary action, and is brazed. In this way, the neck 13 is joined to the annular portion 12, and the nipple 14 is joined to the socket 11.

[0045] In the case of performing copper brazing as described above, for example, the heating furnace may be configured as a two-layer structure. Specifically, a heating furnace that heats to a temperature (e.g., 900°C, etc.) lower than the melting point of copper (1083°C) is provided as the first layer. Then, a heating furnace that heats to a temperature (e.g., 1150°C, etc.) higher than the melting point of copper (1083°C) is provided as the second layer. This allows the entire anti-rotation pin-equipped eye joint 100 to be heated evenly in the first layer, and the second layer to be heated to a temperature exceeding the melting point of copper, thereby improving the permeability of the molten copper.

[0046] In this way, in the case of eye joint 1 that requires a brazing process, the brazing process can be carried out simultaneously in the process of annealing eye joint with anti-rotation pin 100.

[0047] The above describes a method for manufacturing the anti-rotation pin eye joint 100 according to one embodiment of the present invention. The above description has disclosed the following technical features regarding the method for manufacturing the anti-rotation pin eye joint 100.

[0048] The manufacturing method of the eye joint with anti-rotation pin 100 of this embodiment is a manufacturing method of an eye joint with an anti-rotation pin formed by combining an eye joint 1 having a socket 11 at an end and a ring portion 12 with an anti-rotation pin 2, and includes a welding process of spot welding the anti-rotation pin 2 to the outer peripheral surface of the ring portion 12 using carbon steel having a carbon content of 0.42% by weight or more and 0.48% by weight or less as the material for the anti-rotation pin 2, and includes an annealing process of annealing the eye joint 1 to which the anti-rotation pin 2 has been spot welded.

[0049] According to the above configuration, the anti-rotation pin 2 is spot welded to the eye joint 1. At this time, even if the heat of the spot welding hardens and embrittles the anti-rotation pin 2, reducing the strength of the welded portion, the use of carbon steel with a carbon content of 0.42% by weight to 0.48% by weight as the material for the anti-rotation pin 2 and subsequent annealing treatment increase the toughness of the welded portion, making it possible to improve the strength of the welded portion. As a result, a simple method can be used to connect the anti-rotation pin 2 to the eye joint 1, reducing manufacturing costs.

[0050] In addition, in the manufacturing method of the eye joint with anti-rotation pin 100 of this embodiment, the welding process includes a first process, a second process, and a third process. In the first process, the annular portion 12 and the pipe connection portion 15 are arranged in the first cavity portion 61 of the welding jig body 40. In the second process, the pin jig 50 made of an insulating material is fitted into the second cavity portion 62 of the welding jig body 40, which is connected to the first cavity portion 61, and the anti-rotation pin 2 is arranged in the cylindrical hole 52 of the pin jig 50. In the third process, the anti-rotation pin 2 arranged in the cylindrical hole 52 is spot-welded to the outer circumferential surface of the annular portion 12 arranged in the first cavity portion 61. The cylindrical hole 52 of the pin jig 50 is provided with an escape cavity portion 52a. The escape cavity portion 52a prevents the melt of the end of the anti-rotation pin 2 from leaking out of the cylindrical hole. The relief cavity 52 a has a diameter smaller than the thickness of the annular portion 12 .

[0051] According to the above configuration, the annular portion 12 and the pipe connection portion 15 are positioned by the welding jig body 40, and the anti-rotation pin 2 is positioned relative to the annular portion 12 by the pin jig 50. Also, an escape cavity 52a is provided in the cylindrical hole 52 of the pin jig 50 in which the anti-rotation pin 2 is positioned. This allows the annular portion 12 and the anti-rotation pin 2 to be positioned by the welding jig body 40 and the pin jig 50, and further allows for the leakage of the molten material to the outside during spot welding to be suppressed.

[0052] Furthermore, in the manufacturing method of the eye joint with anti-rotation pin 100 of this embodiment, a third cavity 63 is formed in the welding jig body 40, which intersects with a portion of the first cavity 61 where the annular portion 12 is disposed. The annular portion side electrode rod 70 is inserted into the third cavity 63. In a third step, the annular portion side electrode rod 70 is inserted into the through hole 12b of the annular portion 12 disposed in the first cavity 61 and spot welded.

[0053] According to the above configuration, the annular portion side electrode rod 70 is inserted into the third hollow portion 63 of the welding jig body 40, and is also inserted into the through hole 12b of the annular portion 12. This allows the annular portion side electrode rod 70 to establish an electrical connection with the annular portion 12, and also makes it possible to suppress misalignment between the welding jig body 40 and the annular portion 12.

[0054] Although the examples of the present invention have been described above, they are merely illustrative examples and do not limit the present invention, and the specific configurations and the like can be appropriately modified in design. Furthermore, the actions and effects described in the embodiments of the invention are merely a list of the most preferable actions and effects resulting from the present invention, and the actions and effects of the present invention are not limited to those described in the embodiments of the present invention. EXAMPLES

[0055] (Pin strength of anti-rotation pin 2 after annealing) Next, the pin strength of anti-rotation pin 2 in anti-rotation pin eye joint 100 will be specifically described using a comparative example and an example of anti-rotation pin eye joint 100 according to this embodiment.

[0056] As shown in Table 1, in Comparative Examples 1 to 6, SWCH12A, which has a carbon content of 0.10% by weight or more and 0.15% by weight or less according to the JIS standard, was used as the material for the anti-rotation pin 2. In contrast, in Examples 1 to 3 and Comparative Examples 7 to 9, SWCH45K, which has a carbon content of 0.42% by weight or more and 0.48% by weight or less according to the JIS standard, was used as the material for the anti-rotation pin 2. The pin diameter of the anti-rotation pin 2 used in all cases was 5 mm. Furthermore, SWCH12A was used as the material for the eye joint 1 in all cases.

[0057] [Table 1]

[0058] In addition, the eye joint 100 with the anti-rotation pin 2 spot-welded thereto was annealed under the following conditions. Specifically, in the annealing process, the eye joint 100 with the anti-rotation pin was heated and cooled by moving it on a belt conveyer at a speed of 35 mm / min in a continuous furnace with a length of about 20 m. The temperature inside the heating furnace was set to about 950°C to 1100°C, and the eye joint 100 with the anti-rotation pin was moved at the above speed over a distance of about 4 m. The cooling equipment was a type in which the interior was cooled by circulating cooling water through a cooling tower, and the eye joint 100 with the anti-rotation pin was cooled by moving it over a distance of about 9 m. The temperature of the drainage water used to cool the cooling equipment was about 25°C to 50°C.

[0059] In addition, a jig 3 as shown in FIG. 4 was used to measure the pin strength of the anti-rotation pin 2. Specifically, the jig 3 has an installation stand 33 on which the anti-rotation pin eye joint 100 is installed, a fitting part 31 that fits into the through hole of the annular part 12 of the anti-rotation pin eye joint 100 on the installation stand 33, and a stop part 32 that stops the rotation of the anti-rotation pin eye joint 100. The anti-rotation pin eye joint 100 fitted into the fitting part 31 is made rotatable. The anti-rotation pin eye joint 100 that is rotated comes into contact with the stop part 32 and the anti-rotation pin 2 at a predetermined position, and the rotation is stopped. In this state, a torque is applied in the stopping direction by the stop part 32 of the anti-rotation pin eye joint 100 of the comparative example and the example, and the strength when the state of the pin changes is measured. Three samples were prepared for each example and comparative example (Examples 1 to 3, Comparative Examples 1 to 9). For Comparative Examples 7 to 9 and Comparative Examples 1 to 3, the above measurements were taken at a stage before the annealing process (stage at which anti-rotation pin 2 was spot welded to eye joint 1). Note that for Comparative Examples 7 to 9 and Comparative Examples 1 to 3, brazing of neck portion 13 to annular portion 12 and brazing of nipple 14 to socket 11 had not yet been performed. Also, for Examples 1 to 3 and Comparative Examples 4 to 6, the above measurements were taken at a stage after the annealing process.

[0060] [Table 2]

[0061] As a result, as shown in Table 2, the pin strength of anti-rotation pin 2 before annealing was 20, 25, and 28 N·m in Comparative Examples 7 to 9, and 38, 45, and 50 N·m in Comparative Examples 1 to 3, respectively. On the other hand, the pin strength of anti-rotation pin 2 after annealing was 61, 64, and 66 N·m in Examples 1 to 3, and 34, 35, and 36 N·m in Comparative Examples 4 to 6, respectively. It was thus found that the pin strength of anti-rotation pin 2 in the Examples was greatly improved by annealing. Also, in the Comparative Examples, it was found that anti-rotation pin 2 was deformed after annealing, and the pin itself was softened.

[0062] In this way, even if the anti-rotation pin is simply joined by spot welding, the pin strength of the anti-rotation pin 2 can be improved by using carbon steel with a carbon content of 0.42% by weight or more and 0.48% by weight or less as the material for the anti-rotation pin 2 and performing annealing after spot welding. [Explanation of symbols]

[0063] 1,10 Eye Joint 2 Anti-rotation pin 2a Tapered section 3. Jig 11 Socket (cylindrical part) 11a Insertion part 12 Circular Ring 12a Driving hole 13 Neck 13a Communication hole 14 Nipples 14a Fluid hole 15 Pipe connection 16 Pipes 31 Fitting part 32 Stop part 33 Installation stand 40 Welding jig body 40a Contact surface 41 First welding jig body 42 Second welding jig body 50 pin jig 51 Circular ring fitting hole 52 Cylindrical hole 52a Relief cavity 61 1st cavity 62 Second cavity 63 Third cavity 70 Ring side electrode 71 Pin side electrode 100 Eye joint with anti-rotation pin 412 Pin hole 422 Locating pin

Claims

1. A method for manufacturing an eye joint with a rotation prevention pin, which is formed by combining an eye joint having a cylindrical portion or a pipe connection portion at an end and a circular portion with a rotation prevention pin, The material of the anti-rotation pin is carbon steel having a carbon content of 0.42% by weight or more and 0.48% by weight or less, a welding step of spot welding the anti-rotation pin to an outer peripheral surface of the annular portion; an annealing process for annealing the eye joint to which the anti-rotation pin is spot-welded; Equipped with Manufacturing method for eye joint with anti-rotation pin.

2. In the annealing step, the eye joint to which the anti-rotation pin is spot-welded is heated at a temperature of 900° C. or more and 1150° C. or less. A method for manufacturing the anti-rotation pin eye joint according to claim 1.

3. The welding step includes: A first step of disposing the annular portion in a first cavity of a welding jig body; a second step of fitting a pin jig made of an insulating material into a second cavity of the welding jig body, the second cavity being in communication with the first cavity, and arranging the anti-rotation pin in a cylindrical hole of the pin jig; a third step of spot-welding the anti-rotation pin disposed in the cylindrical hole to an outer circumferential surface of the annular portion disposed in the first hollow portion; having a recess for preventing a molten material of the end of the anti-rotation pin from leaking out of the cylindrical hole of the pin jig, the recess having a diameter smaller than a thickness of the annular portion is provided in the cylindrical hole of the pin jig; A method for manufacturing an eye joint with a rotation prevention pin according to claim 1 or 2.

4. a third cavity portion is formed in the welding jig body, the third cavity portion intersecting a portion of the first cavity portion in which the annular portion is disposed, the third cavity portion being into which an electrode rod is inserted; In the third step, the electrode rod is inserted into the annular portion disposed in the first cavity portion and spot-welded. A method for manufacturing the anti-rotation pin eye joint according to claim 3.

Citation Information

Patent Citations

  • Joint and manufacturing method of joint

    JP2019027464A