Method for producing carbon-coated lithium iron phosphate material

By controlling slurry temperature with a liquid-cooled jacket during the carbon-coating process, the method stabilizes carbon content and improves the quality of lithium iron phosphate materials by preventing oxidation and ensuring uniform solubility.

JP2024137679AActive Publication Date: 2024-10-07ADVANCED LITHIUM ELECTROCHEMISTRY CO LTD

Patent Information

Application Number
JP2023215069
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-21
Filing Date
2023-12-20
Publication Date
2024-10-07
Estimated Expiration
2043-12-20

Smart Images

  • Figure 2024137679000001_ABST
    Figure 2024137679000001_ABST
Patent Text Reader

Abstract

To provide a method for producing a carbon-coated lithium iron phosphate material in which a slurry temperature is controlled in order to ensure a carbon content of the carbon-coated lithium iron phosphate material and to improve the stability of product quality at the same time.SOLUTION: A method for producing a carbon-coated lithium iron phosphate material includes the following steps. Step (a): a first slurry, a carbon source and a lithium source are provided, and the first slurry is formed of an iron source and a phosphorus source. Step (b): the first slurry, the carbon source, and the lithium source are mixed to form a second slurry, and the second slurry is ground in a barrel at a first temperature to form a third slurry, and the first temperature is 25°C to 40°C. Step (c): the third slurry is dried and sintered to form a carbon-coated lithium iron phosphate material, the carbon-coated lithium iron phosphate material comprising a core layer and a coating layer, the coating layer coating the core layer, the core layer comprising the lithium source, the iron source, and the phosphorus source, and the coating layer comprising the carbon source.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for making positive electrode materials, and in particular to a method for making carbon-coated lithium iron phosphate materials. [Background technology]

[0002] Lithium-ion batteries are widely used in the field of energy storage due to their good cycle charge / discharge characteristics and high energy density. In particular, lithium-ion batteries using lithium iron phosphate (LiFePO4) as the positive electrode material are characterized by low material costs and high safety, and are attracting attention as batteries with great development potential. However, due to the olivine structure of lithium iron phosphate, the diffusivity of lithium ions and electronic conductivity are low, limiting the applications of lithium iron phosphate.

[0003] Considering the above drawbacks, most of the current industries carbon-coat lithium iron phosphate to improve its performance. In the conventional carbon-coating process, the lithium-containing slurry is alkaline and the temperature rises during the grinding process, so that the carbon source is easily oxidized and decomposed in this alkaline and high-temperature environment, and the carbon content of the finally formed carbon-coated lithium iron phosphate material decreases. In addition, the solubility of the lithium salt in the slurry also changes due to the temperature difference during grinding, which reduces the quality stability of the carbon-coated lithium iron phosphate material produced. Therefore, the carbon-coated lithium iron phosphate material produced by the conventional carbon-coating process often has insufficient carbon content and is unstable in quality.

[0004] The present invention has been made in consideration of the above circumstances, and provides a method for producing a carbon-coated lithium iron phosphate material in which the slurry temperature is controlled in order to ensure the carbon content of the carbon-coated lithium iron phosphate material and at the same time improve the stability of product quality. Summary of the Invention [Problem to be solved by the invention]

[0005] The object of the present invention is to provide a method for producing carbon-coated lithium iron phosphate material by controlling the slurry temperature so as to ensure the carbon content of the carbon-coated lithium iron phosphate material and at the same time improve the stability of the product quality. First, a first slurry formed of a carbon source (material), a lithium source (material), an iron source (material) and a phosphorus source (material) is provided. Next, the first slurry, the carbon source (material) and the lithium source (material) are mixed to form a second slurry, and the second slurry is ground in a barrel at 25°C to 40°C to form a third slurry. Finally, the third slurry is dried and sintered to form the carbon-coated lithium iron phosphate material. By controlling the slurry temperature within a certain temperature range, the uniformity (consistency) of the solubility of the lithium source in the slurry can be ensured, and at the same time, the carbon source in the slurry is prevented from being oxidized and decomposed in a high-temperature environment, so that the carbon content of the carbon-coated lithium iron phosphate material can be ensured and the stability of the product quality can be improved. In addition, the slurry temperature is controlled, for example, by liquid cooling via a cooling water jacket. The cooling water jacket is arranged to surround the internal space of the barrel that contains the slurry, and the temperature rise and fall can be controlled smoothly and uniformly, further improving the stability of product quality.

[0006] In order to achieve the above-mentioned object, the present invention provides a method for producing a carbon-coated lithium iron phosphate material, which includes the steps of: (a) providing a first slurry, a carbon source, and a lithium source, the first slurry being formed from an iron source and a phosphorus source; (b) mixing the first slurry, the carbon source, and the lithium source to form a second slurry, and grinding the second slurry in a barrel at a first temperature to form a third slurry, the first temperature being 25°C to 40°C; and (c) drying and sintering the third slurry to form a carbon-coated lithium iron phosphate material, the carbon-coated lithium iron phosphate material having a core layer and a coating layer, the coating layer coating the core layer, the core layer being formed from a lithium source, an iron source, and a phosphorus source, and the coating layer being formed from a carbon source.

[0007] In one embodiment, the first temperature is maintained by a liquid cooling system.

[0008] In one embodiment, the barrel comprises a first space and a cooling water jacket, the first space is configured to contain the second slurry and the third slurry, the cooling water jacket is configured to surround the first space, and the liquid cooling is performed via the cooling water jacket.

[0009] In one embodiment, the cooling water jacket comprises at least two flow paths and a second space, the second space being in communication between the at least two flow paths and surrounding the first space, and the at least two flow paths being arranged to allow liquid to flow in and out of the second space.

[0010] In one embodiment, the carbon source, the lithium source, and the first slurry are ground using a ball mill.

[0011] In some embodiments, the second slurry and the third slurry are alkaline.

[0012] In one embodiment, the iron source is iron powder, the phosphorus source is an aqueous phosphoric acid solution, and the first slurry is formed by reacting the iron powder with the aqueous phosphoric acid solution.

[0013] In one embodiment, the third slurry is dried by spray drying.

[0014] In one embodiment, the third slurry is sintered at a sintering temperature, and the sintering temperature is between 550°C and 750°C.

[0015] In some embodiments, the third slurry is sintered in a non-oxidizing atmosphere.

[0016] In one embodiment, the carbon-coated lithium iron phosphate material has a carbon content of 1.0% to 1.6%. [Brief description of the drawings]

[0017] [Figure 1] 1 is a flowchart showing a method for producing a carbon-coated lithium iron phosphate material according to an embodiment of the present invention. [Figure 2A]FIG. 2 is a conceptual diagram of the three-dimensional structure of a barrel in an embodiment of the present invention. [Figure 2B] 2B is a cross-sectional view of the present invention taken along line AA' in FIG. 2A. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Some exemplary embodiments showing the features and advantages of the present invention will be described in detail in the following description. It should be understood that the present invention can be modified in various ways in different aspects without departing from the scope of the present invention, and that the description and drawings are used for illustrative purposes in nature and are not intended to limit the present invention. Although the broad ranges and parameters of the present invention are all approximate, in specific cases, the numerical values ​​are described as precisely as possible. Terms such as "first", "second", and "third" may be used to describe different components in the claims, but it should be understood that these components should not be limited by these terms, and that these components described in the embodiments are represented by different component symbols. These terms are used to distinguish different components. For example, the first component can be referred to as the second component, and similarly, the second component can be referred to as the first component, without departing from the scope of the embodiment. In addition, the term "and / or" in the specification means any one or combination of one or more related features. In addition, the term "about" refers to an average value within a standard error range generally accepted by those skilled in the art. Unless expressly defined in the embodiments relating to operation / operation, all numerical ranges, amounts, values, percentages, etc. described herein (e.g., angles, durations, temperatures, operating conditions, ratios and corresponding percentages, etc.) should be understood in all embodiments by the terms "about" or "substantially". Unless otherwise stated in the content, all numerical values ​​in the present invention and claims can be taken as approximations that can be varied as necessary. For example, each parameter may be interpreted in light of at least the number of significant digits described, applying ordinary rounding rules. Also, numerical ranges herein can be expressed as ranges from one endpoint to the other endpoint or between two endpoints. It should be noted that all ranges described herein include the endpoints unless otherwise defined.

[0019] Please refer to FIG. 1 to FIG. 2B. FIG. 1 is a flow chart of a method for producing a carbon-coated lithium iron phosphate material in an embodiment of the present invention. FIG. 2A is a conceptual diagram of the three-dimensional structure of a barrel in an embodiment of the present invention. FIG. 2B is a cross-sectional view of the A-A' line in FIG. 2A. In this embodiment, the method for producing a carbon-coated lithium iron phosphate material includes the following steps. First, as shown in step S1, a first slurry, a carbon source, and a lithium source are provided (prepared). The first slurry is formed from an iron source and a phosphorus source. In this embodiment, the iron source is, for example, iron powder, the phosphorus source is, for example, phosphoric acid (H3PO4), and the first slurry is formed by reacting, for example, iron powder with an aqueous phosphoric acid solution. To form a more stable first slurry, the reaction time is, for example, 17 hours to 24 hours. Examples of the carbon source include water-soluble sugars such as glucose, fructose, galactose, sucrose, maltose, or lactose, but the present invention is not limited thereto. The lithium source may be, for example, a lithium salt such as lithium hydroxide (LiOH), lithium carbonate (Li2CO3), lithium nitrate (LiNO3) or lithium chloride (LiCl), but the invention is not limited thereto. Note that the lithium source may be, for example, a combination of multiple different lithium salts, but the invention is not limited thereto.

[0020] Next, as shown in step S2, the first slurry, the carbon source, and the lithium source are mixed to form a second slurry, and the second slurry in the barrel 1 is pulverized at a first temperature to form a third slurry. Here, the first temperature is 25°C to 40°C, and preferably 27°C to 35°C. In this embodiment, the carbon source, the lithium source, and the first slurry are mixed and reacted at a second temperature to form a second slurry. The second temperature is, for example, 50°C or less, and preferably 30°C to 50°C. The second slurry is pulverized for 9 hours to 12 hours using, for example, a ball mill method to form a third slurry. The median particle size (D50) of the third slurry is, for example, 1.0 μm. The second slurry and the third slurry are alkaline. The pulverization conditions and the median particle size (D50) of the third slurry of the present invention are not limited to these and can be adjusted according to actual demand.

[0021] In this embodiment, the barrel 1 includes a first space 10 and a cooling water jacket 20. The first space 10 is provided to accommodate the second slurry and the third slurry. The cooling water jacket 20 is provided to surround the first space 10. The first temperature can be maintained by the cooling water jacket 20 in a liquid-cooling manner. The cooling water jacket 20 includes a second space 21, a first flow path 22, and a second flow path 23. The second space 21 is connected between the first flow path 22 and the second flow path 23, and surrounds the first space 10. In this embodiment, the second space 21 is, for example, a spiral flow path that is concentric with the first space 10 and annularly surrounds the first space 10. The first flow path 22 and the second flow path 23 are configured to allow liquid to flow into and out of the second space 21. In this embodiment, the liquid flows into the second space 21 along the first flow path 22, and the heat of the second slurry is transferred from the first space 10 to the second space 21 and absorbed by the liquid in the second space 21. The liquid that absorbs the heat flows out along the second flow path 23. The temperature of the second slurry in the barrel 1 is maintained through the liquid flow in the cooling water jacket 20 of the barrel 1. In addition, the second space 21 through which the liquid flows is installed so as to surround the first space 10 that contains the slurry, and the rise and fall of the temperature can be controlled smoothly and uniformly, ensuring the uniformity (consistency) of the solubility of the lithium source in the slurry, and at the same time, preventing the oxidative decomposition of the carbon source in the slurry in a high-temperature environment. In this embodiment, the first flow path 22 and the second flow path 23 are arranged at the upper and lower parts of the barrel 1 along, for example, the vertical direction (Z-axis direction). In another embodiment, the first flow path 22 is configured to allow liquid to flow into the second space 21 and the second flow path 23 is configured to allow liquid to flow out of the second space 21, and the first flow path 22 and the second flow path 23 are both disposed, for example, in an upper portion of the barrel 1. In another embodiment, the first flow path 22 is configured to allow liquid to flow into the second space 21 and the second flow path 23 is configured to allow liquid to flow out of the second space 21, and the first flow path 22 and the second flow path 23 are both disposed, for example, in a lower portion of the barrel 1.In another embodiment, the first flow path 22 is configured to allow liquid to flow into the second space 21, and the second flow path 23 is configured to allow liquid to flow out of the second space 21, and the two first flow paths 22 are arranged at the top and bottom of the barrel (upper space and lower space of the barrel) along the vertical direction (Z-axis direction), respectively, and the two second flow paths 23 are also arranged at the top and bottom of the barrel (upper space and lower space of the barrel) along the vertical direction (Z-axis direction), but details thereof are omitted. In the present invention, the number and configuration of the flow paths for flowing liquid into and out of the second space 21 are not limited, and details thereof are omitted. In this embodiment, the barrel 1 includes, for example, a supply port 30, a discharge port 40, and a cover member 50, and the supply port 30 and the discharge port 40 are each connected to the first space 10. A grinding assembly (not shown) is connected to, for example, the supply port 30 and the discharge port 40 to communicate with the first space 10. In the mixing and grinding process, the second slurry is discharged from the first space 10 through the discharge port 40, fed to the grinding assembly, ground in the grinding step, and then discharged from the grinding assembly through the feed port 30 and fed to the first space 10 for mixing and cooling. This allows the slurry to be continuously cooled during the mixing and grinding process, the temperature is smoothly and uniformly controlled, and the stability of the product quality is improved. The cover member 50 is, for example, disposed above the first space 10 to shield the first space 10 from the vertical direction (Z-axis direction), thereby preventing impurities and foreign matter from being mixed into the slurry during the process. In this embodiment, the cover member 50 further includes, for example, a through hole 51, which is used to introduce solid lithium salt into the first space 10. The through hole 51 may be provided in a plurality of holes, such as for introducing lithium salt into the first space 10 or for inserting a thermometer into the first space 10 to measure the temperature of the internal slurry, and may have a diameter. The present invention is not limited thereto. The carbon source, the lithium source and the first slurry may be mixed and reacted in the barrel 1 to form the second slurry, for example, so that the second temperature is controlled to 50° C. or less.

[0022] Finally, as shown in step S3, the third slurry is dried and sintered to form a carbon-coated lithium iron phosphate material. The carbon-coated lithium iron phosphate material includes a core layer and a coating layer, the coating layer coating the core layer, the core layer being composed of a lithium source, an iron source, and a phosphorus source, and the coating layer being composed of a carbon source. In this embodiment, the product of the previous step is dried, for example, by a spray drying method, and sintered, for example, in a non-oxidizing atmosphere and at a temperature of 550°C to 750°C for 7 hours to 15 hours. The carbon content of the carbon-coated lithium iron phosphate material is, for example, 1.0% to 1.6%. Note that the drying method, sintering conditions, and carbon content of the carbon-coated lithium iron phosphate material of the present invention are not limited thereto, and can be adjusted according to actual needs.

[0023] The manufacturing process and effects of the carbon-coated lithium iron phosphate material of the present invention will be described in detail below with reference to examples.

[0024] First Example: Provide a first slurry, a carbon source, and a lithium source. The first slurry is formed by reacting 5585g of iron powder, 11529g of 85% phosphoric acid aqueous solution, and 40L of deionized water in a barrel for 20 hours. In this embodiment, the target weight of the carbon-coated lithium iron phosphate material is 1578g, the target carbon content ratio (target carbon weight content) is 1.30%, and the carbon weight in the carbon-coated lithium iron phosphate material is 50% of the carbon weight in the third slurry (i.e., 50% of the carbon weight is lost in the sintering process), so 41.0g of carbon needs to be added. In this embodiment, the carbon source is glucose, and the mass ratio of carbon atoms in the molecule is 40%, so 102.5g of glucose needs to be provided to meet the 41.0g carbon weight. The lithium source is 1197g of lithium hydroxide (LiOH) and 1847g of lithium carbonate (Li2CO3). 5585g of iron powder contains 100 moles of iron, 11529g of 85% aqueous phosphoric acid contains 100 moles of phosphorus, 1197g of lithium hydroxide and 1847g of lithium carbonate contain a total of 100 moles of lithium, which can produce 100 moles of lithium iron phosphate (LiFePO4).

[0025] Next, 102.5 g of glucose, 1197 g of lithium hydroxide, and 1847 g of lithium carbonate are added to the stirred first slurry and reacted to form a second slurry. The second slurry is milled to form a third slurry by ball milling. During milling, the temperature of the second slurry is liquid-cooled and maintained at 25° C. by a cooling water jacket on the barrel. The third slurry has a median particle size of 1.0 μm.

[0026] Finally, the third slurry is dried and sintered to form a carbon-coated lithium iron phosphate material. The carbon-coated lithium iron phosphate material is formed by drying using a spray drying method and sintering in a nitrogen atmosphere at a temperature of 550°C to 750°C for 10 hours. The carbon-coated lithium iron phosphate material of the first embodiment is analyzed by a BET specific surface area measurement method and found to have a specific surface area of ​​9.60 cm. 2 When the carbon-coated lithium iron phosphate of the first example was analyzed with an elemental analyzer, it was found that the carbon content was 1.15%.

[0027] First Comparative Example: The manufacturing process of the first comparative example is generally the same as that of the first embodiment, except that the temperature of the second slurry of the first comparative example is maintained at 45° C. during mixing and grinding. The carbon-coated lithium iron phosphate of the first comparative example was analyzed by the BET specific surface area measurement method and found to have a specific surface area of ​​8.58 cm 2 When the carbon-coated lithium iron phosphate of the first comparative example was analyzed with an elemental analyzer, it was found that the carbon content was 1.02%.

[0028] Please refer to Table 1. Table 1 shows the slurry temperature (°C) and the specific surface area (cm) of the carbon-coated lithium iron phosphate formed in the first embodiment and the first comparative example. 2The graph shows the carbon content (carbon weight content, %) and the carbon content (carbon weight content, %). Compared with the target carbon content ratio of 1.30%, it was found that the carbon content loss rate of the carbon-coated lithium iron phosphate formed in the first embodiment was 11.5%, and the carbon content loss rate of the carbon-coated lithium iron phosphate formed in the first comparative example was 21.5%. This shows that the carbon loss level of the first embodiment, in which the slurry temperature is 25°C, is smaller than that of the first comparative example, in which the slurry temperature is 45°C, and the specific surface area of ​​the carbon-coated lithium iron phosphate of the first embodiment is larger than that of the first comparative example. In other words, by controlling the slurry temperature to 25°C to 40°C using a liquid cooling method using a cooling water jacket, the uniformity (consistency) of the solubility of the lithium source in the slurry can be ensured, and at the same time, the oxidative decomposition of the carbon source in the slurry in a high-temperature environment can be prevented, the carbon content of the carbon-coated lithium iron phosphate material can be ensured, and the stability of the product quality can be improved. JPEG2024137679000002.jpg34164

[0029] Example 2: A first slurry, a carbon source, and a lithium source are provided. The first slurry was formed by reacting 5585 g of iron powder, 11529 g of 85% phosphoric acid aqueous solution, and 40 L of deionized water in a barrel for 20 hours. In this example, the target weight of the carbon-coated lithium iron phosphate material is 1578 g, the target carbon content ratio (target carbon weight content) is 1.40%, and the carbon weight in the carbon-coated lithium iron phosphate material is 50% of the carbon weight in the third slurry (i.e., 50% of the carbon weight is lost during the sintering process), so 44.2 g of carbon needs to be added. In addition, the carbon source in this example is glucose, and the mass ratio of carbon atoms in the molecule is 40%, so 110.5 g of glucose needs to be provided to meet the carbon weight of 44.2 g. The lithium sources are 1197 g of lithium hydroxide (LiOH) and 1847 g of lithium carbonate (Li2CO3). 5585g of iron powder contains 100 moles of iron, 11529g of 85% aqueous phosphoric acid contains 100 moles of phosphorus, 1197g of lithium hydroxide and 1847g of lithium carbonate contain a total of 100 moles of lithium, which can produce 100 moles of lithium iron phosphate (LiFePO4).

[0030] Next, 110.5 g of glucose, 1197 g of lithium hydroxide, and 1847 g of lithium carbonate are added to the stirred first slurry and reacted to form a second slurry. The second slurry is milled by ball milling to form a third slurry. During milling, the temperature of the second slurry is maintained at 27° C. by liquid cooling via the cooling water jacket of the barrel. The third slurry has a median particle size of 1.0 μm.

[0031] Finally, the third slurry is dried and sintered to form a carbon-coated lithium iron phosphate material. The material is dried by spray drying and sintered for 10 hours at a temperature of 550°C to 750°C in a nitrogen atmosphere to form a carbon-coated lithium iron phosphate material. The carbon-coated lithium iron phosphate of the second embodiment is analyzed by a BET specific surface area measurement method and found to have a specific surface area of ​​9.40 cm. 2When the carbon-coated lithium iron phosphate of the second example was analyzed by an elemental analyzer, it was found that the carbon content ratio (carbon weight content) was 1.25%.

[0032] Second Comparative Example: The manufacturing process of the second comparative example was almost the same as that of the second example, except that the temperature of the second slurry of the second comparative example was maintained at 45° C. during mixing and grinding. The carbon-coated lithium iron phosphate of the second comparative example was analyzed by the BET specific surface area measurement method and found to have a specific surface area of ​​9.04 cm 2 When the carbon-coated lithium iron phosphate of the second comparative example was analyzed by an elemental analyzer, it was found that the carbon content ratio (carbon weight content) was 1.11%.

[0033] Please refer to Table 2. Table 2 shows the slurry temperature (°C) and the specific surface area (cm) of the carbon-coated lithium iron phosphate formed in the second embodiment and the second comparative example. 2 The graph shows the carbon content (carbon weight content, %) and the carbon content (carbon weight content, %). Compared to the target carbon content ratio (target carbon weight content) of 1.40%, the carbon content loss rate of the carbon-coated lithium iron phosphate formed in the second embodiment is 10.7%, and the carbon content loss rate of the carbon-coated lithium iron phosphate formed in the second comparative example is 20.7%. As a result, the carbon loss level of the second embodiment, in which the slurry temperature is 27° C., is smaller than that of the second comparative example, in which the slurry temperature is 45° C., and the specific surface area of ​​the carbon-coated lithium iron phosphate of the second embodiment is larger than that of the second comparative example. In addition, the carbon loss level of the second embodiment, in which the slurry temperature is 27° C., is smaller than that of the first embodiment, in which the slurry temperature is 25° C. In other words, by controlling the slurry temperature at 27°C to 40°C using a liquid cooling method with a cooling water jacket, the uniformity (consistency) of the solubility of the lithium source in the slurry can be ensured, and at the same time, the oxidative decomposition of the carbon source in the slurry in a high-temperature environment can be prevented, the carbon content of the carbon-coated lithium iron phosphate material can be ensured, and the stability of the product quality can be improved. JPEG2024137679000003.jpg35164

[0034] Example 3: Provide a first slurry, a carbon source, and a lithium source. The first slurry was formed by reacting 5585g of iron powder, 11529g of 85% phosphoric acid aqueous solution, and 40L of deionized water in a barrel for 20 hours. In this example, the target weight of the carbon-coated lithium iron phosphate material is 1578g, the target carbon content ratio (target carbon weight content) is 1.40%, and the carbon weight in the carbon-coated lithium iron phosphate material is 50% of the carbon weight in the third slurry (i.e., 50% carbon weight was lost during the sintering process), so 44.2g of carbon needs to be added. In addition, the carbon source in this example is glucose, and the mass ratio of carbon atoms in the molecule is 40%, so 110.5g of glucose needs to be provided to meet the 44.2g carbon weight. The lithium source is 1197g of lithium hydroxide (LiOH) and 1847g of lithium carbonate (Li2CO3). 5585g of iron powder contains 100 moles of iron, 11529g of 85% aqueous phosphoric acid contains 100 moles of phosphorus, 1197g of lithium hydroxide and 1847g of lithium carbonate contain a total of 100 moles of lithium, which can produce 100 moles of lithium iron phosphate (LiFePO4).

[0035] Next, 110.5 g of glucose, 1197 g of lithium hydroxide, and 1847 g of lithium carbonate were added to the stirred first slurry and reacted to form a second slurry. The second slurry was milled to form a third slurry by ball milling. During milling, the temperature of the second slurry was maintained at 25° C. by liquid cooling via a cooling water jacket on the barrel. The third slurry had a median particle size of 1.0 μm.

[0036] Finally, the third slurry is dried and sintered to form a carbon-coated lithium iron phosphate material. The material is dried by spray drying and sintered in a nitrogen atmosphere at a temperature of 550°C to 750°C for 10 hours to form a carbon-coated lithium iron phosphate material. The carbon-coated lithium iron phosphate of the third embodiment is analyzed by a BET specific surface area measurement method and found to have a specific surface area of ​​9.82 cm. 2When the carbon-coated lithium iron phosphate of the third example was analyzed by an elemental analyzer, the carbon content was found to be 1.24%.

[0037] Example 4: The manufacturing process of the fourth embodiment is generally the same as that of the third embodiment, except that the temperature of the second slurry of the fourth embodiment was maintained at 35° C. during mixing and grinding. The carbon-coated lithium iron phosphate of the fourth embodiment was analyzed by the BET specific surface area measurement method and found to have a specific surface area of ​​10.08 cm 2 When the carbon-coated lithium iron phosphate of the fourth example was analyzed by an elemental analyzer, it was found that the carbon content was 1.28% (carbon weight content).

[0038] Please refer to Table 3. Table 3 shows the slurry temperature (°C) and the specific surface area (cm) of the formed carbon-coated lithium iron phosphate for the third and fourth examples. 2 The carbon content (carbon weight content, %) is shown. Compared with the target carbon content ratio (target carbon weight content) of 1.40%, the carbon content loss rate of the carbon-coated lithium iron phosphate formed in the third embodiment is 11.4%, and the carbon content loss rate of the carbon-coated lithium iron phosphate formed in the fourth embodiment is 8.6%. Thus, the carbon loss level of the fourth embodiment, in which the slurry temperature is 35°C, is smaller than that of the third embodiment, in which the slurry temperature is 25°C, and the specific surface area of ​​the carbon-coated lithium iron phosphate of the fourth embodiment is larger than that of the third embodiment. In other words, by controlling the slurry temperature to 27°C to 35°C using a liquid cooling method using a cooling water jacket, the uniformity (consistency) of the solubility of the lithium source in the slurry is ensured, and at the same time, the oxidative decomposition of the carbon source in the slurry in a high-temperature environment is prevented, the carbon content of the carbon-coated lithium iron phosphate material is ensured, and the stability of the product quality is improved. JPEG2024137679000004.jpg35164

[0039] Fifth Example: Provide a first slurry, a carbon source, and a lithium source. The first slurry was formed by reacting 5585g of iron powder, 11529g of 85% aqueous phosphoric acid solution, and 40L of deionized water in a barrel for 20 hours. In this embodiment, the target weight of the carbon-coated lithium iron phosphate material is 1578g, the target carbon content ratio (target carbon weight content) is 1.20%, and the carbon weight in the carbon-coated lithium iron phosphate material is 50% of the carbon weight in the third slurry (i.e., 50% carbon weight was lost during the sintering process), so 37.9g ​​of carbon needs to be added. In addition, the carbon source in this embodiment is glucose, and the mass ratio of carbon atoms in the molecule is 40%, so 94.7g of glucose needs to be provided to meet the 37.9g ​​carbon weight. The lithium source is 1197g of lithium hydroxide (LiOH) and 1847g of lithium carbonate (Li2CO3). 5585g of iron powder contains 100 moles of iron, 11529g of 85% aqueous phosphoric acid contains 100 moles of phosphorus, 1197g of lithium hydroxide and 1847g of lithium carbonate contain a total of 100 moles of lithium, which can produce 100 moles of lithium iron phosphate (LiFePO4).

[0040] Next, 94.7 g of glucose, 1197 g of lithium hydroxide, and 1847 g of lithium carbonate are added to the stirred first slurry and reacted to form a second slurry. The second slurry is milled to form a third slurry by ball milling. During milling, the temperature of the second slurry is maintained at 25° C. by liquid cooling using a cooling water jacket on the barrel. The third slurry has a median particle size of 1.0 μm.

[0041] Finally, the third slurry is dried and sintered to form a carbon-coated lithium iron phosphate material. The carbon-coated lithium iron phosphate material is formed by drying using a spray drying method and sintering for 10 hours at a temperature of 550°C to 750°C in a nitrogen atmosphere. The carbon-coated lithium iron phosphate material of the fifth embodiment is analyzed by a BET specific surface area measurement method and found to have a specific surface area of ​​8.97 cm. 2When the carbon-coated lithium iron phosphate of the fifth example was analyzed by an elemental analyzer, it was found that the carbon content was 1.10%.

[0042] Sixth Example: The manufacturing process of the sixth embodiment is generally the same as that of the fifth embodiment, except that the temperature of the second slurry of the sixth embodiment was maintained at 35° C. during mixing and grinding. The carbon-coated lithium iron phosphate of the sixth embodiment was analyzed by the BET specific surface area measurement method and found to have a specific surface area of ​​9.34 cm 2 When the carbon-coated lithium iron phosphate of Example 6 was analyzed by an elemental analyzer, it was found that the carbon content was 1.11%.

[0043] Please refer to Table 4. Table 4 shows the slurry temperature (°C) and the specific surface area (cm) of the carbon-coated lithium iron phosphate formed in the fifth and sixth examples. 2 The carbon content (carbon weight content, %) is shown. Compared with the target carbon content ratio of 1.20%, the carbon content loss rate of the carbon-coated lithium iron phosphate formed in the fifth embodiment is 8.3%, and the carbon content loss rate of the carbon-coated lithium iron phosphate formed in the sixth embodiment is 7.5%. Thus, the carbon loss degree of the sixth embodiment in which the slurry temperature is 35°C is smaller than that of the fifth embodiment in which the slurry temperature is 25°C, and the specific surface area of ​​the carbon-coated lithium iron phosphate of the sixth embodiment is larger than that of the fifth embodiment. In other words, by controlling the slurry temperature to 27°C to 35°C using a liquid cooling method with a cooling water jacket, the uniformity (consistency) of the solubility of the lithium source in the slurry is ensured, and at the same time, the oxidative decomposition of the carbon source in the slurry in a high-temperature environment is prevented, the carbon content of the carbon-coated lithium iron phosphate material is ensured, and the stability of the product quality is improved. JPEG2024137679000005.jpg35164

[0044] As described above, the present invention provides a method for producing carbon-coated lithium iron phosphate material by controlling the slurry temperature to ensure the carbon content of the carbon-coated lithium iron phosphate material and improve the stability of the product quality. First, a first slurry formed of a carbon source, a lithium source, an iron source and a phosphorus source is provided. Next, the first slurry, the carbon source and the lithium source are mixed to form a second slurry, and the second slurry is ground in a barrel at 25°C to 40°C to form a third slurry. Finally, the third slurry is dried and sintered to form the carbon-coated lithium iron phosphate material. By controlling the slurry temperature within a specific temperature range, the uniformity (consistency) of the solubility of the lithium source in the slurry can be ensured, and at the same time, the carbon source in the slurry can be prevented from being oxidized and decomposed in a high-temperature environment, ensuring the carbon content of the carbon-coated lithium iron phosphate material and improving the stability of the product quality. In addition, the slurry temperature is controlled, for example, by liquid cooling via a cooling water jacket. The cooling water jacket is arranged to surround the internal space of the barrel that contains the slurry, and the temperature rise and fall can be controlled smoothly and uniformly, thereby further improving the stability of product quality.

[0045] The present invention may be modified in various ways by those skilled in the art, without departing from the scope thereof as defined by the claims. [Explanation of symbols]

[0046] 1: Barrel 10: 1st space 20: Cooling water jacket 21:Second space 22: First flow path 23: Second flow path 30: Supply port 40: Outlet 50: Lid material A-A': Line S1, S2, S3: Step X, Y, Z: Axes

Claims

1. 1. A method for producing a carbon-coated lithium iron phosphate material, comprising the steps of: (a) providing a first slurry, a carbon source, and a lithium source, the first slurry being formed of an iron source and a phosphorus source; (b) mixing the first slurry, the carbon source, and the lithium source to form a second slurry, and mixing and grinding the second slurry in a barrel at a first temperature to form a third slurry, wherein the first temperature is between 25° C. and 40° C.; and (c) drying and sintering the third slurry to form the carbon-coated lithium iron phosphate material, the carbon-coated lithium iron phosphate material having a core layer and a coating layer, the coating layer coating the core layer, the core layer being composed of the lithium source, the iron source and the phosphorus source, and the coating layer being composed of the carbon source.

2. 2. The method of claim 1, wherein the first temperature is maintained by a liquid cooling method.

3. 3. The method for producing a carbon-coated lithium iron phosphate material according to claim 2, wherein the barrel comprises a first space and a cooling water jacket, the first space is configured to accommodate the second slurry and the third slurry, the cooling water jacket is configured to surround the first space, and the liquid cooling method is cooling via the cooling water jacket.

4. 4. The method for producing a carbon-coated lithium iron phosphate material according to claim 3, wherein the cooling water jacket comprises at least two flow paths and a second space, the second space being in communication with the at least two flow paths and surrounding the first space, and the at least two flow paths are arranged so that liquid flows into or out of the second space.

5. 2. The method for producing a carbon-coated lithium iron phosphate material according to claim 1, wherein the carbon source, the lithium source, and the first slurry are pulverized by a ball mill method.

6. 2. The method of claim 1, wherein the second slurry and the third slurry are alkaline.

7. 2. The method of claim 1, wherein the iron source is iron powder, the phosphorus source is an aqueous phosphoric acid solution, and the first slurry is formed by reacting the iron powder with the aqueous phosphoric acid solution.

8. 2. The method for producing a carbon-coated lithium iron phosphate material according to claim 1, wherein the third slurry is dried by a spray drying method.

9. 2. The method for producing the carbon-coated lithium iron phosphate material according to claim 1, wherein the third slurry is sintered at a sintering temperature of 550°C to 750°C.

10. 2. The method of claim 1, wherein the third slurry is sintered in a non-oxidizing atmosphere.

11. 2. The method for producing a carbon-coated lithium iron phosphate material according to claim 1, wherein the carbon weight content of the carbon-coated lithium iron phosphate material is 1.0% to 1.6%.

Citation Information

Patent Citations

  • Preparation method for lithium iron phosphate modified by doping graphene

    CN103579617A

  • Preparation method of three-layer carbon-coated composite lithium iron phosphate cathode material

    CN109920989A

  • Organic carbon coated lithium iron phosphate positive electrode material and preparation method thereof

    CN113651304A

  • Thin wire gripping mechanism

    JP1994079677A

  • Lithium secondary battery cathode active material and its manufacturing method, and precursor of the same and its manufacturing method

    JP2012155916A

Cited By

  • Multi-media structures containing growth enhancement additives

    US12371655B2