Aluminum-based alloy material, aluminum-based alloy wiring, and sputtering target
By adding Ge and rare earth elements to form intermetallic compounds, the aluminum-based alloy addresses the challenge of achieving heat resistance and low electrical resistivity while maintaining surface smoothness, suitable for display device wiring.
Patent Information
- Application Number
- JP2023222845
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2023-12-28
- Publication Date
- 2024-10-07
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing aluminum alloy films for display device wiring struggle to achieve both heat resistance and low electrical resistivity, and often suffer from surface roughness issues due to hillock formation during high-temperature processing.
Incorporating Ge and rare earth elements, particularly NdAlGe or NdAl2Ge2, into the aluminum-based alloy to form intermetallic compounds that provide both heat resistance and low electrical resistivity while maintaining surface smoothness.
The alloy achieves both heat resistance and low electrical resistivity, with improved surface smoothness even under high-temperature processing conditions, reducing the risk of hillock formation and ensuring reliable electrical connections.
Smart Images

Figure 2024137694000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an aluminum-based alloy material, an aluminum-based alloy wiring, and a sputtering target. [Background technology]
[0002] In recent years, flat panel displays such as liquid crystal displays and organic electro-luminescence (EL) displays have come to be widely used in smartphones, tablets, laptop computers, monitors, televisions, etc. Thin film transistors (TFTs) are used to drive each pixel of a flat panel display.
[0003] Conventionally, amorphous silicon (a-Si) has been used as the semiconductor film that constitutes this thin-film transistor. However, the operating speed of the TFT in high-definition displays is also becoming faster, which makes it difficult for amorphous silicon to keep up with. For this reason, low-temperature polysilicon (LTPS), which has a carrier mobility 300 times higher than that of conventional amorphous silicon, is becoming more and more popular.
[0004] Since the process temperature of amorphous silicon thin-film transistors is 400°C or less, aluminum alloy wiring, which has both heat resistance and electrical resistivity, has been the mainstream for gate wiring. In contrast, in the manufacturing process of low-temperature polysilicon thin-film transistors, high temperatures of 400°C or more are applied to the gate wiring, so wiring made of high-melting point metal materials such as Mo is used. However, this wiring has an electrical resistivity of about 12 μΩcm or more, which is higher than the electrical resistivity of aluminum alloy wiring (about 4 μΩcm to 5 μΩcm), and therefore has the problem of high resistance.
[0005] In view of this problem, techniques for achieving both heat resistance and low electrical resistivity have been investigated (see Patent Document 1). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 09-228035 Summary of the Invention [Problem to be solved by the invention]
[0007] Patent Document 1 describes an Al alloy film containing 2 at% or less Zr and 2 at% or less of one or more of W, Nb, and Mo, with the total amount of these being 0.2 to 2 at%. However, the Al alloy film described in Patent Document 1 is not sufficient in terms of achieving both heat resistance and low electrical resistivity. In addition, the Al alloy film described in Patent Document 1 has an increased number of hillocks when the electrical resistivity is reduced, making it difficult to maintain sufficient smoothness of the wiring surface.
[0008] The present disclosure has been made in light of the above circumstances, and has an object to provide an aluminum-based alloy material that is capable of achieving both heat resistance and low electrical resistivity, and also has excellent surface smoothness. [Means for solving the problem]
[0009] The inventors have added Ge and rare earth elements to aluminum to achieve a predetermined content, and have produced NdAlGe or NdAl 2 Ge 2 It has been found that by incorporating the above-mentioned compound, it is possible to achieve both the heat resistance and low electrical resistivity required for a wiring material for a display device while maintaining surface smoothness, and thus the present invention has been completed.
[0010] The aluminum-based alloy material according to one embodiment of the present disclosure is an aluminum-based alloy material for a display device, which contains Ge: 0.6 at% or more and 2.0 at% or less, rare earth elements: 0.3 at% or more and 1.0 at% or less, and is selected from NdAlGe or NdAl 2 Ge 2 Includes. Effect of the Invention
[0011] The aluminum-based alloy material according to one embodiment of the present disclosure is capable of achieving both heat resistance and low electrical resistivity, and is also excellent in surface smoothness. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a schematic cross-sectional view of a top-gate type TFT substrate according to an embodiment of the present disclosure. [Diagram 2] Figure 2 shows the results of the X-ray diffraction spectrum analysis of sample No. 1. [Diagram 3] FIG. 3 shows the results of the X-ray diffraction spectrum analysis of sample No. 9. [Figure 4] FIG. 4 shows the results of the X-ray diffraction spectrum analysis of sample No. 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] [Description of the embodiments of the present disclosure] First, the embodiments of the present disclosure will be listed and described.
[0014] (1) An aluminum-based alloy material according to one embodiment of the present disclosure is an aluminum-based alloy material for a display device, comprising Ge: 0.6 at% or more and 2.0 at% or less, rare earth elements: 0.3 at% or more and 1.0 at% or less, and is selected from NdAlGe or NdAl 2 Ge 2 Includes.
[0015] The aluminum-based alloy material contains Ge and rare earth elements in the above ranges, and is NdAlGe or NdAl 2 Ge 2 By including this, it is possible to achieve both heat resistance and low electrical resistivity, and also to achieve excellent surface smoothness.
[0016] (2) In the above (1), the ratio of the number of rare earth element atoms to the number of Ge atoms is preferably 0.5 to 1.0. By making the ratio of the number of rare earth element atoms to the number of Ge atoms 0.5 to 1.0 in this manner, the heat resistance can be further improved.
[0017] (3) In the above (1), it is preferable to include at least one of Ta: 0.05 at% to 0.5 at% and Nb: 0.05 at% to 0.5 at%. In this way, by including at least one of Ta: 0.05 at% to 0.5 at% and Nb: 0.05 at% to 0.5 at% or less, it is possible to further improve low electrical resistance and surface smoothness.
[0018] (4) In the above (2), it is preferable to include at least one of Ta: 0.05 at% to 0.5 at% and Nb: 0.05 at% to 0.5 at%. In this way, by including at least one of Ta: 0.05 at% to 0.5 at% and Nb: 0.05 at% to 0.5 at% or less, it is possible to further improve low electrical resistance and surface smoothness.
[0019] (5) An aluminum-based alloy wiring according to another aspect of the present disclosure is made of any one of the aluminum-based alloy materials (1) to (4) described above.
[0020] The aluminum-based alloy wiring is made of the above-mentioned aluminum-based alloy material, and therefore has both heat resistance and low electrical resistivity, and is excellent in surface smoothness.
[0021] (6) A sputtering target according to yet another aspect of the present disclosure is used for forming an aluminum-based alloy material according to any one of (1) to (4) above.
[0022] The sputtering target can provide the above-mentioned aluminum-based alloy material having both heat resistance and low electrical resistivity and excellent surface smoothness. The sputtering target can also be used to form the above-mentioned aluminum-based alloy wiring.
[0023] In this disclosure, "base alloy" refers to the metal element that is most abundant in the alloy in terms of atomic number. That is, "aluminum-base alloy material" refers to the alloy material that has the most aluminum content in terms of atomic number, and "aluminum-base alloy wiring" refers to the alloy wiring that has the most aluminum content in terms of atomic number. "At%" refers to atomic %.
[0024] [Details of the embodiment of the present disclosure] Hereinafter, the embodiments of the present disclosure will be described in detail with reference to the drawings as appropriate. Note that, for the numerical values described in this specification, only one of the upper limit value and the lower limit value described can be adopted, or the upper limit value and the lower limit value can be arbitrarily combined. Also, FIG. 1 is a schematic view, and may not match the actual dimensions, shape, etc.
[0025] <Aluminum-based alloy materials> The aluminum-based alloy material is an aluminum-based alloy material for display devices, containing Ge: 0.6 at% or more and 2.0 at% or less, rare earth elements: 0.3 at% or more and 1.0 at% or less, and is NdAlGe or NdAl 2 Ge 2 Includes.
[0026] The display device includes a flat panel display such as a liquid crystal display, an organic electroluminescence display, and an LED display. The aluminum-based alloy material is used, for example, as a wiring material for a thin film transistor mounted on the display device. The use of the aluminum-based alloy material is not limited to the wiring material for the thin film transistor. The aluminum-based alloy material can also be used, for example, as an electrode material for a thin film transistor. The aluminum-based alloy material may also be used as an electrode and wiring material in a field emission display (FED), an electrode and wiring material in a vacuum fluorescent tube (VFD), an electrode and wiring material in a plasma display (PDP), and an electrode material in an inorganic EL.
[0027] The aluminum-based alloy material contains Ge and Nd, and is therefore called NdAlGe or NdAl 2 Ge 2 The composition may include NdAlGe or NdAl 2 Ge 2 is produced as an intermetallic compound of Nd, Al and Ge by, for example, heat treatment. The aluminum-based alloy material is NdAlGe or NdAl 2 Ge 2 By including the above, it is possible to achieve both heat resistance and low electrical resistivity, and also to have excellent surface smoothness. More specifically, the aluminum-based alloy material may be subjected to heat treatment at 400°C or higher, or 450°C or higher, during the process of mounting the material on the display device. For example, in the manufacturing process of low-temperature polysilicon thin-film transistors, high temperatures of 400°C or higher are applied to the gate wiring. Even in such cases, the aluminum-based alloy material is able to achieve both heat resistance and low electrical resistivity, and maintain surface smoothness while suppressing the occurrence of abnormal grain growth called hillocks.
[0028] The reason why this aluminum-based alloy material is able to achieve heat resistance, low electrical resistivity, and surface smoothness is presumed to be as follows. For example, when wiring using pure Al (aluminum) is subjected to heat treatment at about 150°C or higher, the surface becomes rough and hillocks occur. It is thought that these hillocks are caused by Al diffusing to the surface to relieve the compressive stress caused by the heat treatment. When hillocks occur, the smoothness of the wiring surface is impaired, increasing the risk of short-circuiting with the upper and lower layers. Although the addition of only Nd can suppress stress relaxation to a certain extent when compressive stress is applied, hillocks occur when heated to a temperature of 250°C or higher. In contrast, by adding Ge together with Nd, an intermetallic compound of Al, Nd, and Ge (NdAlGe or NdAl 2 Ge 2 ) is generated during heat treatment, and this intermetallic compound acts as a stress reliever. As a result, stress can be released without changing the surface morphology, so the surface smoothness can be maintained. In addition, the precipitation of Ge and Nd as the above intermetallic compound can reduce the electrical resistivity after heat treatment.
[0029] [Al] The aluminum-based alloy material is mainly composed of Al. The lower limit of the content of Al in the aluminum-based alloy material is preferably 90 at%, more preferably 92 at%. On the other hand, the upper limit of the content of Al in the aluminum-based alloy material can be set according to the above-mentioned contents of Ge and Nd and the contents of other elements that may be contained, and is preferably 95 at%. The aluminum-based alloy material may further contain elements other than Al, Ge, and Nd, or may be composed of Al, Ge, Nd, and unavoidable impurities.
[0030] [Ge] Ge improves heat resistance and surface smoothness. More specifically, Ge, when added together with Nd, generates an intermetallic compound with Al and Nd during the heat treatment process, thereby suppressing the occurrence of hillocks. Ge also reduces the electrical resistivity after heat treatment by precipitating as an intermetallic compound with Nd. The lower limit of the Ge content in the aluminum-based alloy material is 0.6 at% and preferably 0.8 at% from the viewpoint of promoting surface smoothness and low electrical resistance after heat treatment. On the other hand, the upper limit of the Ge content is 2.0 at% and preferably 1.6 at% from the viewpoint of suppressing the precipitation of simple Ge due to an excessive Ge content.
[0031] [Rare earth elements] The aluminum-based alloy material includes a rare earth element. The rare earth element may be a lanthanoid element (a total of 15 elements from La (lanthanum) with atomic number 57 to Lu (lutetium) with atomic number 71 in the periodic table) in addition to Sc (scandium) and Y (yttrium). The aluminum-based alloy material may include a plurality of rare earth elements. However, the aluminum-based alloy material preferably includes only one type of rare earth element so that the desired quality can be easily obtained. When the aluminum-based alloy material includes only one type of rare earth element, the rare earth element is Nd. When the rare earth element is Nd, the desired intermetallic compound can be easily generated with Al and Ge by heat treatment.
[0032] The rare earth element improves heat resistance and surface smoothness. More specifically, the rare earth element is added together with Ge to generate an intermetallic compound with Al and Ge during the heat treatment process, thereby suppressing the occurrence of hillocks. The rare earth element also reduces the electrical resistivity after heat treatment by precipitating as an intermetallic compound with Ge. The lower limit of the content of the rare earth element in the aluminum-based alloy material is 0.3 at% and preferably 0.4 at% from the viewpoint of promoting surface smoothness and low electrical resistance after heat treatment. On the other hand, the upper limit of the content of the rare earth element in the aluminum-based alloy material is 1.0 at% and preferably 0.8 at% from the viewpoint of suppressing the generation of coarse precipitates and enhancing surface smoothness. In addition, when the aluminum-based alloy material contains multiple rare earth elements, the total content of these multiple rare earth elements may be within the above range. However, in the aluminum-based alloy material, the content of Nd is preferably within the above range. When the Nd content is within the above range, the heat resistance, the electrical resistance and the surface smoothness can be easily improved.
[0033] The lower limit of the ratio of the number of rare earth element atoms to the number of Ge atoms is preferably 0.5 from the viewpoint of suppressing a decrease in surface smoothness due to precipitation of simple Ge caused by an excess of Ge relative to the rare earth element. On the other hand, the above ratio is preferably 0.5 from the viewpoint of suppressing a decrease in surface smoothness due to an excess of rare earth element relative to Ge caused by coarse precipitates (e.g., Al 4 From the viewpoint of suppressing the decrease in surface smoothness due to the precipitation of rare earth elements, the ratio is preferably 1.0 or less, more preferably less than 1.0, and even more preferably 0.8 or less. By setting the ratio of the number of rare earth elements to the number of Ge atoms within the above range, the aluminum-based alloy material can be heat-treated at 300° C. or more to form a desired intermetallic compound (e.g., NdAlGe or NdAl 2 Ge 2 ) can be precipitated, and the heat resistance can be easily improved.
[0034] (Other elements) The aluminum-based alloy material may contain at least one of Ta (tantalum) and Nb (niobium). For example, the aluminum-based alloy material may be composed of Al, Ge, and Nd, at least one of Ta and Nb, and unavoidable impurities.
[0035] [Ta] Ta suppresses changes in surface morphology when compressive stress is applied. The lower limit of the Ta content in the aluminum-based alloy material is preferably 0.05 at% and more preferably 0.1 at% from the viewpoint of more reliably suppressing changes in surface morphology. On the other hand, the upper limit of the Ta content in the aluminum-based alloy material is preferably 0.5 at% and more preferably 0.4 at% from the viewpoint of suppressing an increase in electrical resistivity.
[0036] [Nb] Nb suppresses changes in surface morphology when compressive stress is applied. The lower limit of the Nb content in the aluminum-based alloy material is preferably 0.05 at% and more preferably 0.1 at% from the viewpoint of more reliably suppressing changes in surface morphology. On the other hand, the upper limit of the Nb content in the aluminum-based alloy material is preferably 0.5 at% and more preferably 0.4 at% from the viewpoint of suppressing an increase in electrical resistivity.
[0037] <Aluminum-based alloy wiring> Next, an aluminum-based alloy wiring made of the above-mentioned aluminum-based alloy material will be described. The aluminum-based alloy wiring can be used as wiring for a thin-film transistor mounted on a display device, for example. In this case, the aluminum-based alloy wiring can be used as a gate wiring, a source wiring, a drain wiring, or the like. In the following, referring to FIG. 1, a case where the aluminum-based alloy wiring is used as wiring for a top-gate thin-film transistor 10 will be described as an example of use of the aluminum-based alloy wiring. However, the aluminum-based alloy wiring may be used as wiring for a bottom-gate thin-film transistor. The aluminum-based alloy wiring can also be used as wiring for a field emission display, a fluorescent vacuum tube, a plasma display, or the like. Furthermore, in the following, a form in which the aluminum-based alloy wiring constitutes one wiring by itself will be described, but it is also possible to use the aluminum-based alloy wiring with other layers laminated thereon as one wiring.
[0038] <Top-gate thin-film transistor> 1 is a polysilicon thin-film transistor. More specifically, the thin-film transistor 10 is a low-temperature polysilicon thin-film transistor.
[0039] The thin-film transistor 10 includes a substrate 1, a semiconductor film 2 disposed on the substrate 1, a gate insulating film 3 disposed on the semiconductor film 2, a gate electrode 4 disposed on the gate insulating film 3, a first interlayer insulating film 5a disposed on the gate insulating film 3 and the gate electrode 4, a source electrode 6 and a drain electrode 7 disposed in a conductorized region of the semiconductor film 2, a second interlayer insulating film 5b disposed on the source electrode 6 and the drain electrode 7, and a pixel electrode 8 connected to the drain electrode 7. The gate electrode 4 is formed integrally with the gate wiring. The source electrode 6 is formed integrally with the source wiring. The drain electrode 7 is formed integrally with the drain wiring.
[0040] (substrate) The substrate 1 is not particularly limited, but examples thereof include a glass substrate and a silicon substrate. Examples of glass used for the glass substrate include non-alkali glass, high strain point glass, soda lime glass, etc. In addition, the substrate 1 may be a metal substrate such as a stainless steel thin film, or a resin substrate such as a polyethylene terephthalate (PET) film.
[0041] (Semiconductor film) The semiconductor film 2 is, for example, a first polysilicon film (poly-Si) that is not doped with phosphorus, and a second polysilicon film (n + The semiconductor film 2 is obtained, for example, by forming a first polysilicon film, forming a gate insulating film 3, forming a gate electrode 4, partially implanting ions into the first polysilicon film to form a second polysilicon film, and then performing a heat treatment at 450° C. to 500° C. for activation.
[0042] (Gate insulating film) The gate insulating film 3 may be, for example, a silicon oxide film, a silicon nitride film, a silicon oxynitride film, or an Al 2 O 3 Or Y 2 O 3 and the like. The gate insulating film 3 can be formed by using a CVD method, a PECVD method, or the like. The gate insulating film 3 may be a single layer body or a multilayer body having two or more layers. A contact hole is formed in the gate insulating film 3 by photolithography or the like.
[0043] (gate electrode) As described above, the gate electrode 4 is formed integrally with the gate wiring. This gate wiring is an aluminum-based alloy wiring made of the above-mentioned aluminum-based alloy material. In other words, the gate electrode 4 and the gate wiring are entirely made of the aluminum-based alloy material. The composition of the aluminum-based alloy wiring is the same as that of the aluminum-based alloy material. In other words, the aluminum-based alloy wiring contains Ge: 0.6 at% or more and 2.0 at% or less, rare earth elements: 0.3 at% or more and 1.0 at% or less, and is NdAlGe or NdAl 2 Ge 2 The gate wiring is made of the aluminum-based alloy wiring, and therefore has both heat resistance and low electrical resistivity, and has excellent surface smoothness. Therefore, even if the above-mentioned heat treatment is performed in the process of forming the semiconductor film 2, the excellent quality can be maintained.
[0044] (Interlayer insulating film) The interlayer insulating film 5 includes a first interlayer insulating film 5a and a second interlayer insulating film 5b. The first interlayer insulating film 5a and the second interlayer insulating film 5b are made of, for example, a silicon oxide film, a silicon nitride film, a silicon oxynitride film, an Al 2 O 3 Or Y 2 O 3 The first interlayer insulating film 5a and the second interlayer insulating film 5b can be formed by using a CVD method, a PECVD method, or the like. After the first interlayer insulating film 5a is formed, a contact hole is formed by photolithography or the like. The contact hole formed in the gate insulating film 3 and the contact hole formed in the first interlayer insulating film 5a are in communication with each other.
[0045] (Source and drain electrodes) The source electrode 6 and the drain electrode 7 cover a part of the first interlayer insulating film 5a and fill the contact holes. With this configuration, the source electrode 6 and the drain electrode 7 are electrically connected to the second polysilicon film of the semiconductor film 2.
[0046] As described above, the source electrode 6 is formed integrally with the source wiring, and the drain electrode 7 is formed integrally with the drain wiring. The source electrode 6 and the drain electrode 7 may be made of, for example, a metal with low electrical resistivity such as Al or Cu, a high melting point metal with high heat resistance such as Mo, Cr or Ti, or an alloy thereof. In addition, one or both of the source electrode 6 and the drain electrode 7 may be made of the aluminum-based alloy material. That is, one or both of the source wiring and the drain wiring may be the aluminum-based alloy wiring. By making one or both of the source wiring and the drain wiring out of the aluminum-based alloy wiring, it is possible to achieve both heat resistance and low electrical resistivity, and also to have excellent surface smoothness.
[0047] (Pixel electrode) The pixel electrode 8 is formed of a conductive oxide film, such as an indium tin oxide (ITO) film.
[0048] The thin film transistor 10 may include other configurations than those described above. For example, the thin film transistor 10 may include a barrier layer, a cap layer, or the like on any of the gate wiring, the source wiring, and the drain wiring. Examples of materials constituting the barrier layer include TiN, Mo, Ti, and W. The thin film transistor 10 may also include a buffer layer between the substrate 1 and the semiconductor film 2.
[0049] <Manufacturing method> The aluminum-based alloy material and the aluminum-based alloy wiring can be formed by inkjet coating, vacuum deposition, sputtering, etc. Among these, sputtering is preferred from the viewpoints of ease of alloying, productivity, film thickness uniformity, etc.
[0050] (Sputtering target) In order to form an aluminum-based alloy material and an aluminum-based alloy wiring by a sputtering method, a sputtering target having the same composition as the aluminum-based alloy material and the aluminum-based alloy wiring may be used. That is, the sputtering target used to form the aluminum-based alloy material or the aluminum-based alloy wiring contains elements such as Al, Nd, and Ge in the same content as the obtained aluminum-based alloy material and the aluminum-based alloy wiring. That is, the sputtering target contains Ge: 0.6 at% or more and 2.0 at% or less, and rare earth elements: 0.3 at% or more and 1.0 at% or less. The sputtering target is one aspect of the present disclosure. The sputtering target can achieve both heat resistance and low electrical resistivity, and can form the aluminum-based alloy material and the aluminum-based alloy wiring having excellent surface smoothness.
[0051] The preferred range of the content of each element in the sputtering target can be the same as the range described above for the aluminum-based alloy material.
[0052] The shape of the sputtering target can be appropriately set according to the shape and structure of the sputtering device. For example, the shape of the target can be a square plate, a circular plate, a cylindrical plate, etc. The sputtering target may be an aluminum alloy target having the same composition as the aluminum-based alloy material, or a composite target in which pure metals of other alloy elements are disposed on a pure aluminum target or an aluminum alloy target.
[0053] The sputtering target can be produced by a vacuum melting method, a powder sintering method, etc. Among them, the vacuum melting method is preferred from the viewpoint of improving the uniformity of the composition and structure within the target surface.
[0054] The lower limit of the substrate temperature in the sputtering method is preferably 25° C. from the viewpoint of suppressing the adsorption of moisture and gas onto the substrate, while the upper limit of the temperature is preferably 200° C., more preferably 150° C., from the viewpoint of ensuring the smoothness of the surfaces of the aluminum-based alloy material and the aluminum-based alloy wiring.
[0055] (Sputtering target materials) The sputtering target can be formed by processing an intermediate (preform) made of an aluminum-based alloy, or by arranging metal chips made of pure metals of other alloy elements on a pure aluminum target or an aluminum alloy target. The intermediate, the combination of the pure aluminum target or the aluminum alloy target with the metal chips, etc., are configured as a sputtering target material for forming the sputtering target. The sputtering target material is one aspect of the present disclosure. By using the sputtering target material, it is possible to achieve both heat resistance and low electrical resistivity, and to form the above-mentioned aluminum-based alloy material and aluminum-based alloy wiring that are excellent in surface smoothness.
[0056] The sputtering target material includes Al, Ge, and Nd. The elements included in the sputtering target material are the same as the elements constituting the above-mentioned sputtering target. The content of each element in the sputtering target material may be the same as the content in the above-mentioned sputtering target. In this case, the preferred range of the content of each element may be the same as the range described above for the aluminum-based alloy material.
[0057] [Other embodiments] The above-mentioned embodiment does not limit the configuration of the present invention. Therefore, the above-mentioned embodiment may omit, replace or add components of each part of the above-mentioned embodiment based on the description in this specification and common technical knowledge, and it should be construed that all of these are within the scope of the present invention. EXAMPLES
[0058] Hereinafter, the present disclosure will be described in detail based on examples, but the present disclosure should not be construed as being limited based on the description of these examples.
[0059] <Sample Preparation> An aluminum-based alloy layer having a thickness of 250 nm and the composition shown in Table 1 was formed on a glass substrate (Corning's "eagleXG") by DC magnetron sputtering. The content [at%] of each element in Table 1 was calculated from the target composition used for simultaneous discharge in film formation and the film formation rate of each target. The target composition was determined by XRF (X-ray fluorescence analysis). The sputtering conditions by DC magnetron sputtering are as follows: Atmosphere gas: Argon gas Film forming pressure: 0.26Pa Substrate temperature: Room temperature (no heating) Coating power: 3W / cm 2 -12W / cm 2 Target: 4 inch diameter alloy or composite target
[0060] [Table 1] In addition, in the contents in Table 1, "-" indicates that it is not contained. In addition, in Table 1, elements other than Ge, Nd, Ta, and Nb are Al and unavoidable impurities.
[0061] (Electrical resistivity test) For samples No. 1 to No. 13, heat treatment was performed for 1 hour at 450°C in a nitrogen atmosphere using an infrared lamp heat treatment furnace, and then the electrical resistivity [μΩcm] was measured by the four-probe method. The measurement results are shown in Table 2.
[0062] (Heat resistance test) For samples No. 1 and No. 3 to No. 13, heat treatment was performed for 1 hour at 450°C in a nitrogen atmosphere using an infrared lamp heat treatment furnace, and the surfaces of the samples were visually observed with an optical microscope at a magnification of 1000 times, and the heat resistance was evaluated according to the following criteria. For No. 2, heat treatment was performed in the same manner as above, except that the heat treatment temperature was 500°C, and the surfaces of the samples were visually observed with an optical microscope at a magnification of 1000 times, and the heat resistance was evaluated according to the following criteria. The results are shown in Table 2. The analysis results of the X-ray diffraction spectrum of No. 1 after the above heat treatment are shown in Figure 2, the analysis results of the X-ray diffraction spectrum of No. 9 after the above heat treatment are shown in Figure 3, and the analysis results of the X-ray diffraction spectrum of No. 3 after the above treatment are shown in Figure 4. Furthermore, the analysis results of the crystal phases after the above heat treatment by X-ray diffraction spectrum for No. 1, No. 2, No. 3, No. 8, No. 9, and No. 12 are shown in Table 2. A: No black or white spots are visible. B: Black and white spots are visible.
[0063] (comprehensive evaluation) Based on the above-mentioned electrical resistivity test and heat resistance test, a comprehensive evaluation was made according to the following criteria. The results are shown in Table 2. A: Electrical resistivity is 6μΩcm or less and heat resistance is rated A. B: At least one of the following is not satisfied: electrical resistivity is 6 μΩcm or less and heat resistance does not meet the A rating.
[0064] [Table 2] In Table 2, "-" indicates that the analysis was not performed.
[0065] <Evaluation Results> As shown in Tables 1 and 2, Ge: 0.6 at% to 2.0 at% and rare earth elements: 0.3 at% to 1.0 at% are included, and NdAlGe or NdAl 2 Ge 2No. 1 to No. 3, which include NdAl, are excellent in both electrical resistivity and heat resistance. In addition, the crystal phase of No. 4 to No. 6 has not been analyzed, but the analysis shows that it is NdAl 2 Ge 2 It is highly likely that they contain. Furthermore, as shown in Table 2, when No. 1, No. 3 to No. 6 were heat-treated for 1 hour at 450°C, and No. 2 was heat-treated for 1 hour at 500°C, no black or white spots were visible when viewed under an optical microscope at 1000x magnification. This means that No. 1 to No. 6 have no visible protrusions on their surfaces, and it can be inferred that no protrusions with a diameter of 1 μm or more exist. Therefore, No. 1 to No. 6 have excellent surface smoothness after heat treatment. [Industrial Applicability]
[0066] As described above, the aluminum-based alloy material according to one embodiment of the present disclosure is capable of achieving both heat resistance and low electrical resistivity, and also has excellent surface smoothness, and is therefore suitable for use in wiring for display devices. [Explanation of symbols]
[0067] 1 Board 2. Semiconductor film 3. Gate insulating film 4. Gate electrode 5 Interlayer insulating film 5a First interlayer insulating film 5b Second interlayer insulating film 6 Source Electrode 7 Drain electrode 8 Pixel electrode 10 Top-gate thin-film transistor
Claims
1. An aluminum-based alloy material for a display device, comprising: Ge: 0.6 at% or more and 2.0 at% or less, Rare earth elements: 0.3 at% or more and 1.0 at% or less Including, NdAlGe or NdAl 2 Ge 2 4. An aluminum-based alloy material comprising:
2. 2. The aluminum-based alloy material according to claim 1, wherein the ratio of the number of rare earth element atoms to the number of Ge atoms is 0.5 or more and 1.0 or less.
3. Ta: 0.05 at% or more and 0.5 at% or less, and Nb: 0.05 at% or more and 0.5 at% or less The aluminum-based alloy material according to claim 1, comprising at least one of the following:
4. Ta: 0.05 at% or more and 0.5 at% or less, and Nb: 0.05 at% or more and 0.5 at% or less The aluminum-based alloy material according to claim 2, comprising at least one of the following:
5. An aluminum-based alloy wiring made of the aluminum-based alloy material according to any one of claims 1 to 4.
6. A sputtering target used for forming the aluminum-based alloy material according to any one of claims 1 to 4.
Citation Information
Patent Citations
Al ALLOY FILM FOR WIRING FILM AND SPUTTERING TARGET MATERIAL FOR FORMING WIRING FILM
JP2005171378A
Aluminum alloy film for display device, display device and sputtering target
JP2009280911A
Al ALLOY FILM FOR DISPLAY, THIN FILM TRANSISTOR SUBSTRATE AND DISPLAY
JP2010238800A
Thin-film transistor substrate and display device
JP2011035153A
Al ALLOY FILM FOR DISPLAY DEVICE
JP2011190531A