HIGH Ni ALLOY STEEL PLATE WITH SUPERIOR HOT WORKABILITY AND HIGH-TEMPERATURE CREEP STRENGTH

By using W and V to strengthen high Ni alloy steels, the challenges of achieving both high hot workability and creep strength are addressed, resulting in improved manufacturability and reduced costs for high-temperature applications.

JP2024137740APending Publication Date: 2024-10-07NIPPON STEEL STAINLESS STEEL CORP

Patent Information

Application Number
JP2024021654
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-02-16
Publication Date
2024-10-07

AI Technical Summary

Technical Problem

Existing high Ni alloy steels face challenges in achieving both high hot workability and high-temperature creep strength, particularly due to issues like edge cracking during rolling and susceptibility to embrittlement, which are exacerbated by elements like Mo and B, and require costly high-temperature heat treatments that strain furnace equipment.

Method used

Incorporating W and V as solid solution strengthening elements, along with optimized alloy compositions and heat treatment conditions, to enhance both hot workability and creep strength within the capacity of standard heat treatment equipment, while minimizing grain boundary segregation and embrittlement.

Benefits of technology

The solution results in a high Ni alloy steel sheet with improved manufacturability, reduced furnace maintenance costs, and enhanced creep strength suitable for high-temperature applications, such as chemical plant reaction vessels, without compromising hot workability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137740000001_ABST
    Figure 2024137740000001_ABST
Patent Text Reader

Abstract

To provide a high alloy containing Nb and N with superior hot workability and creep strength.SOLUTION: A high Ni alloy steel plate with superior hot workability and high-temperature creep strength contains, in mass%, Cr: 20-30%, Ni: 30-50%, B: 0.0002-0.0030%, N: 0.12-0.30%, W: 0.01-3.0%, Nb: 0.30-0.90%, V: 0.01-0.50%, and Ca: 0.0001-0.0050%, and features an alloy component and an average grain size that satisfy A value≤95 and B value≥60 as defined separately and C value≥350 as defined below. C value=0.65×average grain size (μm)+350×(W(%)+Mo(%))+850×V(%)+550×Ta(%)+5,000×(C(%)-0.03)-1,500×|Nb(%)×N(%)-0.07|SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a high Ni alloy steel sheet which is manufactured by a process including a hot rolling process and a heat treatment, and which has excellent hot workability and high-temperature creep strength and is used in high-temperature applications requiring high-temperature creep strength. [Background technology]

[0002] A typical commercial alloy of high Ni alloy steel used for heat-resistant applications is Alloy 800H (ASTM N08010, N08011). In recent years, demand has been expanding in developing countries, and technological development is required to supply products that are inexpensive and have good surface quality and usability. For this reason, the manufacturing method is being converted from the conventional steel ingot method to the continuous casting method. Since high Ni alloy steel is highly susceptible to internal cracks in the slab during casting, edge cracks during hot working, and surface defects in the product, the design of the alloy's chemical composition, and improvements and development of smelting, casting, and hot working technologies have been promoted from the viewpoint of improving manufacturability in the continuous casting method.

[0003] On the other hand, in the high-temperature reaction vessels of chemical plants, which are the main application of this material, it is often used at high temperatures of 600°C or higher, and also under high pressure to improve the efficiency of chemical reactions. In these applications, the higher the creep strength, the thinner the material can be used, so in recent years, there has been an increase in the use of materials such as ASTM N08120 that contain Nb and N and use precipitation strengthening due to Nb carbonitride precipitates.

[0004] As for high Ni-based alloys utilizing precipitation strengthening by adding Nb and N, there are prior art documents such as Patent Documents 1 and 2. As mentioned above, all of these alloys are designed to utilize precipitation strengthening by carbonitride precipitates such as Nb, solid solution strengthening by adding Mo, and grain boundary strengthening by adding B in a composite manner. However, these alloys have a problem in manufacturing steel sheets in that they do not take into consideration hot workability, which is a problem in manufacturing high Ni alloy steel sheets. For example, as described in Patent Document 1, hot rolling must be performed at 1000°C or higher, but this is due to the increased sensitivity to II region embrittlement (ductility reduction around 900 to 1000°C) caused by the addition of Mo. Furthermore, Patent Document 2 has a tendency to perform heat treatment at high temperatures, with the heat treatment conditions ranging from 1180°C to 1300°C. In order to increase creep strength, it is desirable to heat at an ultra-high temperature range such as 1250°C to 1300°C as suggested in Patent Document 1, but heat treatment above 1250°C causes great damage to the furnace body, leading to increased maintenance costs for the furnace. In addition, there are only a limited number of steel plate manufacturers that are equipped with equipment with such capabilities as standard, and it is necessary to design the composition according to the capabilities of the manufacturing equipment. Thus, there is a need for the development of a high-Ni alloy that combines hot workability and high-temperature creep strength and is compatible with the capabilities of heat treatment equipment. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 6675846 [Patent Document 2] Patent No. 7174192 Summary of the Invention [Problem to be solved by the invention]

[0006] The present inventors aimed to obtain alloy components and metal structures that can be hot-rolled without defects such as edge cracking at 1200°C to 900°C, which is the temperature range during rolling of normal austenitic stainless steel, and can ensure a reduction in area RA of 60% or more during hot tension and a high-temperature creep strength of 250 hours or more to break under conditions of 800°C and 100 MPa, when a high-Ni alloy steel sheet containing Nb and N is actually used. In order to achieve this goal, if solid solution strengthening by adding Mo is relied upon as in conventional knowledge, the above-mentioned II region embrittlement susceptibility and I region embrittlement susceptibility (embrittlement at around 1200°C, which affects not only hot workability but also hot cracking susceptibility during welding) will increase, and further, the addition of B and the increase in the amounts of C, Si, etc. will significantly increase the I region embrittlement susceptibility, making it difficult to reach the above target level.

[0007] The present invention aims to provide a high Ni alloy steel plate that is excellent in hot workability and high-temperature creep strength, and that satisfies both hot workability and high-temperature creep strength and can be manufactured within the capacity range of ordinary heat treatment equipment. [Means for solving the problem]

[0008] In order to elucidate the causes and solve the above problems, the inventors selected W as a solid solution strengthening element, which has less grain boundary segregation than Mo, the main cause of region II embrittlement. Furthermore, in order to find the effect of precipitation strengthening by nitrides even when heat treatment is performed at 1200 to 1220°C to reduce the load on the furnace body, the inventors attempted to achieve both hot workability and creep strength by effectively utilizing Ta as necessary in addition to V in order to find the effect of precipitation strengthening by nitrides even when heat treatment is performed at 1200 to 1220°C in order to reduce the load on the furnace body.

[0009] In steels containing both Nb and N, coarse carbonitrides remain in an amount exceeding the solubility product of Nb and C or N at the heat treatment temperature, and these undissolved carbonitrides contribute little to precipitation strengthening, but rather act to reduce creep strength. In order to exceed the solubility limit of Nb and N during heat treatment at 1200 to 1220°C, we discovered that further improvement in creep strength can be expected by utilizing a third element that is dissolved in this temperature range and precipitates by aging in the operating temperature range as a precipitation strengthening element, and by taking into consideration the effect of crystal grains on creep strength and the effect of Si, B, etc. on hot workability, we obtained a high-Ni alloy steel plate that combines high levels of hot workability and high-temperature creep strength.

[0010] That is, the gist of the present invention is as follows. (1) containing, by mass%, C: 0.15% or less, Si: 0.05-1.0%, Mn: 0.05-1.5%, P: 0.030% or less, S: 0.0015% or less, Cr: 20-30%, Ni: 30-50%, Al: 0.02-0.30%, B: 0.0002-0.0030%, N: 0.12-0.30%, O: 0.006% or less, W: 0.01-3.0%, Nb: 0.30-0.90%, V: 0.01-0.50%, Ca: 0.0001-0.0050%, and the remainder being Fe and impurities; The A, B, and C values ​​defined below are A value ≦ 95, B value ≧ 60, and C value ≧ 350, respectively. A high Ni alloy steel sheet having excellent hot workability and high temperature creep strength, characterized by having an alloy composition and average crystal grain size that satisfy the above. however, A value = 12,000 x B (%) + 1,000 x C (%) + 10 x Mn (%) - 30 x Nb (%) +20×Si(%)+W(%)+10×V(%) B value = 115-35 x (C(%) + N(%))-25 x Nb(%)-45 x V(%)-20 x W(%) C value=0.65×average grain size (μm)+350×W(%)+850×V(%) +5,000×(C(%)-0.03)-1,500×|Nb(%)×N(%)-0.07|. In the above formula, "element symbol (%)" means the content (mass %) of the corresponding element. (2) The high Ni alloy steel plate excellent in hot workability and high-temperature creep strength according to (1), further comprising, in mass%, one or more of Mo: 0.01 to 0.80%, Ta: 0.001 to 0.50%, Cu: 0.01 to 0.50%, Co: 0.01 to 1.0%, Ti: 0.001 to 0.10%, Sn: 0.001 to 0.05%, Zn+Pb+Bi: 0.0010% or less, Mg: 0.0050% or less, Zr: 0.001 to 0.10%, Hf: 0.001 to 0.10%, and La+Ce+Nd+Pr: 0.001 to 0.050%, in place of a part of the Fe. However, in this case, A value, B value, and C value are respectively, A value = 12,000 x B (%) + 1,000 x C (%) + 10 x Mn (%) - 30 x Nb (%) +20×Si(%)+W(%)+10×V(%)+12×Mo(%) B value = 115-35 x (C(%) + N(%))-25 x Nb(%)-45 x V(%)-20 x W(%) -45×Mo(%) -40×Ta(%) C value = 0.65 x average grain size (μm) + 350 x (W (%) + Mo (%)) + 850 x V (%) + 550 x Ta (%) +5,000×(C(%)-0.03)-1,500×|Nb(%)×N(%)-0.07|. In the above formula, "element symbol (%)" means the content (mass %) of the corresponding element. Effect of the Invention

[0011] According to the present invention, the hot workability of Nb-containing high-N, high-Ni alloy steel sheets, which have been difficult to manufacture, can be improved without impairing creep strength, and the cost of expanding the capacity of heat treatment furnaces and the maintenance cost can be significantly reduced by designing the components according to the furnace capacity. Since Nb-containing high-N high alloy steels are used in applications requiring high levels of high-temperature creep strength and high-temperature corrosion resistance, such as reaction vessels in chemical plants such as polycrystalline silicon manufacturing equipment, they are expected to make a significant contribution to the development of the chemical and semiconductor industries. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a graph showing the relationship between the reduction in area at 1200° C. and the A value of the limiting formula A. [Diagram 2] FIG. 1 is a graph showing the relationship between the reduction in area at 900° C. and the B value of the limiting formula B. [Diagram 3] FIG. 1 is a graph showing the relationship between creep rupture time and the C value of the limiting formula C under conditions of 800° C. and 100 MPa. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] First, the reasons for limiting the contents of the essential component elements of the present invention will be described below. The contents of each component are expressed in mass %. <Component composition>

[0014] C: 0.15% or less C is added to high-temperature materials and heat-resistant alloys to ensure their strength at room temperature and high temperature. It is preferably added at 0.015% or more, more preferably at 0.03% or more, but the upper limit is limited to a content of 0.15% or less. In this alloy, C exists in the alloy as Cr carbide or Nb carbide, but if it is added at more than 0.15%, Cr carbide will be excessively formed, deteriorating high-temperature properties, weld hot cracking susceptibility, hot workability, and corrosion resistance. It is preferably 0.10% or less, more preferably 0.085% or less.

[0015] Silicon: 0.05 to 1.0% Silicon is added at 0.05% or more to improve deoxidation and oxidation resistance. However, it is also an element that lowers the melting point of steel, so adding more than 1.0% of silicon reduces hot ductility near 1200°C and solidification cracking sensitivity and liquation cracking sensitivity during welding. In addition, intermetallic compounds are more likely to precipitate, deteriorating high-temperature properties. Therefore, the upper limit is limited to 1.0%. The preferred upper limit is 0.7%, and the more preferred upper limit is 0.5%.

[0016] Mn: 0.05 to 1.5% Mn has the effect of increasing the stability of the austenite phase and improving heat resistance. For this reason, it is preferable to add Mn positively to the alloy of the present invention. To improve heat resistance, 0.05% or more is added. However, adding more than 1.5% makes intermetallic compounds more likely to precipitate, deteriorating heat resistance and adversely affecting solidification cracking susceptibility. Therefore, the upper limit is set at 1.5%. The preferred upper limit is 1.3%, and the more preferred upper limit is 1.0%.

[0017] P:0.030% or less P is an element that is inevitably mixed in from the raw materials and has the effect of increasing solidification cracking susceptibility, so its content is limited to 0.030% or less, preferably 0.025% or less.

[0018] S: 0.0015% or less S is an element that is inevitably mixed in from the raw materials, and since it also deteriorates hot workability and oxidation resistance, it is limited to 0.0015% or less, preferably 0.0010% or less. Although the S content can be reduced by refining, an extreme reduction in the content increases costs. For this reason, it is preferable to set the lower limit of the S content to 0.0001%.

[0019] Cr: 20~30% Cr is an essential element for the oxidation resistance and high-temperature corrosion resistance of heat-resistant alloys as high-temperature materials, and is contained at 20% or more, preferably 22% or more. On the other hand, if it is contained at more than 30%, the high-temperature structural stability decreases even if a large amount of Ni is contained, and intermetallic compounds are precipitated, deteriorating the heat resistance characteristics, so the upper limit is set to 30%. The preferable upper limit is 28%, and the more preferable upper limit is 26%.

[0020] Ni: 30~50% Ni is contained at 30% or more, preferably 32% or more, and more preferably more than 35% in order to stabilize the austenitic structure at high temperatures and to improve corrosion resistance and toughness against various acids. By increasing the Ni content, it becomes possible to contain more Cr, W, and Al, which are necessary to ensure heat resistance. On the other hand, Ni is an expensive alloy, and the upper limit of Ni content in the steel of the present invention is set to 50% or less from the viewpoint of cost.

[0021] Al: 0.02 to 0.30% Al is a deoxidizing element and also has the effect of forming an NiAl ordered phase in high Ni alloys to increase high-temperature strength. In the present invention, in order to promote deoxidation and desulfurization and improve hot workability, the content must be 0.02% or more, preferably 0.03% or more. On the other hand, if the Al content exceeds 0.30%, AlN precipitates, impairing manufacturability and heat resistance. For this reason, the upper limit of the Al content is set at 0.30%. The preferred upper limit is 0.15%.

[0022] B: 0.0002~0.0030% B is actively added to improve high-temperature creep strength, especially in applications where the steel will be used in high-temperature environments. Although the mechanism by which B improves creep strength is unclear, it is said to enhance grain boundary strength by segregating to grain boundaries. The improvement effect of hot tensile strength due to the inclusion of B is manifested at 0.0002% or more, so the lower limit of B addition is set to 0.0002%. On the other hand, since B is an element that lowers the melting point of steel and is prone to segregation, excessive addition of B promotes solidification cracking and liquation cracking, and has a significant adverse effect on hot workability, especially in the I-region embrittlement region (near 1200°C). Therefore, the upper limit of the content is set at 0.0030%. The preferable upper limit is 0.0025%.

[0023] N: 0.12~0.30% N is an important element that contributes greatly to improving high-temperature strength, and is an essential element in this steel along with Nb, V, and W. In addition to solid solution strengthening, N is an element that significantly improves creep strength by forming fine nitrides with Cr, Nb, V, and Ta over time in the operating temperature range, resulting in aging precipitation strengthening. In order to ensure the creep strength required for this steel, it is necessary to add 0.12% or more. On the other hand, excessive addition of more than 0.30% can cause bubbles to form during refining, so the upper limit is set at 0.30%. The preferred upper limit is 0.25%.

[0024] O: 0.006% or less Oxygen forms oxide-based inclusions with Ca, Mg, Al, and Ti in the alloy of the present invention. The oxygen content corresponds to the total amount of oxide-based inclusions and is an important indicator of the deoxidation state of the alloy. If the oxygen content exceeds 0.006%, the desired deoxidation equilibrium is not satisfied, and nozzle clogging during continuous casting and surface defects due to inclusions are likely to occur. For this reason, the upper limit of the oxygen content is set to 0.006%. On the other hand, reducing the oxygen content is advantageous in suppressing nozzle clogging and hot welding cracking by reducing oxide-based inclusions, but it generates excess Ca and excess Mg in the alloy, which causes a decrease in hot workability. For this reason, the oxygen content is preferably 0.0002% or more.

[0025] W: 0.01 to 3.0% W is an element that enhances the high-temperature strength and high-temperature corrosion resistance of heat-resistant alloys, and in particular, it significantly improves creep strength. In terms of raw material cost, the difference is such that the superiority or inferiority is reversed depending on the market situation. Its mechanism and strengthening ability are almost the same as Mo, which is known as a solid solution strengthening element. In addition, it was found that W is significantly less sensitive than Mo to the melting point reduction of steel and to I-region embrittlement and II-region embrittlement. Therefore, in the present invention, W is an essential additive element instead of Mo in order to ensure high-temperature creep strength and hot workability at a high level. W exerts its effect when added at 0.01% or more. It is preferably added at 0.05%, and more preferably added at 0.1% or more. On the other hand, excessive addition leads to a decrease in hot workability and an increase in alloy cost, so the upper limit is set to 3.0% in the steel of the present invention. The preferred upper limit is 2.5%, and the more preferred upper limit is 2.0%.

[0026] Nb: 0.30-0.90% Nb is an essential element in the present invention, and in addition to its high solid solution strengthening ability, it has the effect of improving the high-temperature strength of steel, especially the high-temperature creep strength, by finely precipitating carbides and nitrides at the operating temperature. For this reason, 0.30% or more is added. On the other hand, Nb is also an element that is prone to grain boundary segregation, and excessive addition increases the II region embrittlement susceptibility and adversely affects hot workability, so the upper limit in this chemical system is set at 0.90%.

[0027] V: 0.01 to 0.50% V is also an essential element in the present invention. Like Nb, V has the effect of improving the high-temperature strength of steel, especially the high-temperature creep strength, by finely precipitating carbides and nitrides at the operating temperature. This aging precipitation strengthening is effective when the metal elements and nitrogen that are in solid solution during heat treatment age and precipitate as nitrides at the operating temperature. However, in the case of Nb, the solid solubility limit at which it can be dissolved without forming carbonitrides during heat treatment is small, so even if it is added in excess of its solid solubility product at the heat treatment temperature, the creep strength improvement effect cannot be obtained. As a solution to this problem, we focused on the combined addition of Nb and V. When Nb and V are combined in high-N steel, the total solid solubility of Nb and V is greater than the solid solubility of Nb alone at the heat treatment temperature, and as a result, the amount of nitrides that are aged and precipitated in the operating temperature range is increased. For this reason, we found that the creep life is significantly increased by adding Nb in combination with V rather than by adding Nb alone. Like Nb, excessive addition of V increases the II region embrittlement susceptibility and adversely affects hot workability, so the upper limit of this chemical composition is set at 0.50%, with the preferred upper limit being 0.40%.

[0028] Ca: 0.0001 to 0.0050% Ca is an important element for improving the hot workability and weld hot cracking susceptibility of the alloy, and is contained to fix S in the alloy as CaS and improve hot workability. This reaction is as follows. Ca combines with oxygen in the alloy to produce CaO and CaO-Al2O3, and after the dissolved oxygen (free oxygen) in the alloy is reduced to almost zero, the remaining Ca reacts with S in the alloy to produce CaS. For this purpose, the alloy of the present invention contains Ca at 0.0001% or more, preferably 0.0003% or more, and more preferably 0.0005% or more. On the other hand, excessive Ca addition reduces hot ductility around 1100°C. For this reason, the upper limit of the Ca content is set to 0.0050%. The desirable upper limit of the Ca content is 0.0045%.

[0029] <Limited formula A> A value = 12,000 x B (%) + 1,000 x C (%) + 10 x Mn (%) - 30 x Nb (%) +20×Si(%)+W(%)+10×V(%) A value ≦ 95 The limiting formula A is defined as an index of hot workability in the temperature range (near 1200°C) where I-region embrittlement occurs in the composition range of the alloy of the present invention. The hot reduction of area (RA) in a hot tensile test is generally used as an index to judge whether or not a steel sheet can be hot rolled. It is known that if this value is ≥ 60%, the steel sheet can be rolled well without edge cracks at the end surface during hot rolling. The alloying elements that affect I-region embrittlement in the composition range of the alloy of the present invention are B, C, Mn, Nb, Si, and V. It is considered that these elements mainly lower the melting point of the steel or segregate to the final solidification portion to lower the grain boundary strength or grain boundary ductility, thereby increasing the susceptibility to I-region embrittlement. The result of examining the influence of these multiple alloying elements is as shown in the limiting formula A, and by adjusting the amount of alloying elements so that the A value of the limiting formula A is 95 or less, RA ≥ 60% at 1200°C can be satisfied and the maximum temperature in hot rolling can be 1200°C or higher. In particular, the adverse effects of B are significant, limiting the amount that can be added. On the other hand, W has a smaller adverse effect than other elements, and can be added more actively than other extracted elements.

[0030] <Limited formula B> B value = 115-35 x (C(%) + N(%))-25 x Nb(%)-45 x V(%)-20 x W(%) B value ≧60 Limiting formula B is defined as an index of hot workability in the temperature range (near 900°C) where II region embrittlement occurs in the composition range of the alloy of the present invention. In Limiting formula B, RA ≧ 60% at 900°C is the criterion. In the claimed scope of the alloy of the present invention, the alloying elements that affect II region embrittlement are C, N, Nb, V, and W. These elements strengthen the intragranular strength of crystal grains, but on the other hand, they do not contribute to strengthening the grain boundary strength, or they reduce the grain boundary strength by segregation to the grain boundary, etc. Therefore, it is considered that the strength difference between the intragranular strength and the grain boundary increases, and the hot ductility of the steel is reduced. However, W has a smaller adverse effect than the other extracted elements, and can be added more actively. The result of examining the influence of these multiple alloying elements is as shown in Limiting formula B, and by adjusting the amount of alloying elements so that the value of Limiting formula B is 60 or more, RA ≧ 60% at 900°C can be satisfied and the minimum rolling temperature in hot rolling can be 900°C or lower.

[0031] <Limited expression C> C value=0.65×average grain size (μm)+350×W(%)+850×V(%) +5,000×(C(%)-0.03)-1,500×|Nb(%)×N(%)-0.07| C value ≧ 350 The limiting formula C is defined as an index of creep strength within the composition range of the alloy of the present invention. In the present invention, the time to rupture at 800°C and 100 MPa is set as the standard as an index of creep strength. In order to improve creep strength, it is effective to (1) increase the average grain size and (2) actively add alloying elements that contribute to strengthening, but (1) is restricted by the heat treatment conditions, and as for (2), it has become clear that the creep strength does not increase as the amount of Nb and N added among the strengthening elements increases, and that the addition of an amount corresponding to the solubility product of Nb and N at the heat treatment temperature is effective, and any addition beyond that is rather harmful to creep strength. The contribution of these factors to the creep rupture life is as shown in the limiting formula C, and if this value is 350 or more, the creep rupture life at 800°C and 100 MPa exceeds 250 hours. The contribution of crystal grains is 0.65 x average grain size (μm), and the alloying elements that contribute to strengthening are W, V, and C, each of which contributes to extending the fracture life depending on its coefficient. The contribution of Nb and N reaches a maximum when the product of the amounts added is 0.07, and the contribution decreases if it is smaller or larger than that. The preferred C value is C value ≧ 400. The following formula can also be used as limiting formula C. C value=0.6×average grain size (μm)+350×W(%)+550×V(%) +10,000×(C(%)-0.04)-1,100×|Nb(%)×N(%)-0.09|

[0032] The composition of the high Ni alloy of the present invention contains the above-mentioned components, with the remainder being Fe and impurities. Next, the reasons for limiting the selective elements of the present invention will be described. Furthermore, instead of a part of the Fe, the following components (mass%) can be selectively contained.

[0033] Mo: 0.01 to 0.80% Mo, like W, is an element that improves the high-temperature strength and high-temperature corrosion resistance of the alloy, and can be added at 0.01% or more as necessary to improve these properties. However, as described below, Mo has a greater adverse effect on hot workability than W, so the upper limit of the amount of Mo added is lower than that of W, and in the present invention, the upper limit is set to 0.80%. The preferred upper limit is 0.65%, and the more preferred upper limit is 0.45%.

[0034] Ta: 0.001 to 0.50% Ta, like V and Nb, has the effect of improving the high-temperature strength of steel, especially the high-temperature creep strength, by finely precipitating carbides and nitrides at the temperature of use, so it can be added at 0.001% or more, preferably 0.01% or more, as necessary. Like V, Ta and Nb are added in combination to increase the amount of nitrides that precipitate during aging in the temperature range of use compared to when Nb is added alone. Note that, like V and Nb, excessive addition of Ta increases the sensitivity to region II embrittlement and adversely affects hot workability, so the upper limit is set at 0.50% in this chemical system. The preferred upper limit is 0.40%.

[0035] When Mo or Ta is added, the limiting formulas A to C are as follows: <Limited formula A> A value = 12,000 x B (%) + 1,000 x C (%) + 10 x Mn (%) - 30 x Nb (%) +20×Si(%)+W(%)+10×V(%)+12×Mo(%) A value ≦ 95 <Limited formula B> B value = 115-35 x (C(%) + N(%))-25 x Nb(%)-45 x V(%)-20 x W(%) -45×Mo(%) -40×Ta(%) B value ≧60 <Limited expression C> C value = 0.65 x average grain size (μm) + 350 x (W (%) + Mo (%)) + 850 x V (%) + 550 x Ta (%) +5,000×(C(%)-0.03)-1,500×|Nb(%)×N(%)-0.07| C value ≧ 350 It becomes. The following formula can also be used as limiting formula C. C value = 0.6 x average grain size (μm) + 350 x (W (%) + Mo (%)) + 550 x (V (%) + Ta (%)) +10,000×(C(%)-0.04)-1,100×|Nb(%)×N(%)-0.09|

[0036] Cu: 0.01 to 0.50% Cu is an element that increases the alloy's resistance to acid corrosion and dew-point corrosion resistance, which is often a problem in high-temperature equipment, and also has the effect of improving high-temperature strength and structural stability, so it can be added as necessary. To improve these heat resistance and corrosion resistance, the content is set to 0.01% or more, preferably 0.02% or more, and more preferably 0.05% or more. On the other hand, if the content exceeds 0.50%, embrittlement occurs during solidification, so the upper limit is set to 0.50%.

[0037] Co: 0.01 to 1.0% Co is an effective element for improving the high-temperature structural stability and corrosion resistance of the alloy, and in order to improve these properties, it is contained at 0.01% or more, preferably at 0.02% or more, and more preferably at 0.1% or more. If it is contained at more than 1.0%, it is an expensive element and the effect commensurate with the cost is not obtained, so the upper limit is set at 1.0%. The preferred upper limit of Co is 0.8%, and the more preferred upper limit is 0.50%.

[0038] Ti: 0.001 to 0.10% In high alloys containing N, Ti is not essential because it forms coarse TiN and adversely affects manufacturability and the surface quality of the steel. However, Ti is also an element with high deoxidizing and desulfurizing properties, so it can be added as a deoxidizing and desulfurizing agent as necessary, from a lower limit of 0.001% to an upper limit of 0.10%. The preferred upper limit is 0.07%, and the more preferred upper limit is 0.05%.

[0039] Sn: 0.001 to 0.05% Sn is an element that improves the corrosion resistance and high-temperature creep strength of steel when added at 0.001% or more, preferably 0.005% or more, and can be added as necessary. However, since the addition of more than 0.05% reduces hot workability, the upper limit is set at 0.05%.

[0040] Zn+Pb+Bi:0.0010% or less Zn, Pb, and Bi also significantly reduce the hot workability of austenitic single-phase alloys, so their upper limits must be strictly defined. The preferred limits are Pb≦0.0010%, Zn≦0.0010%, and Bi≦0.0010%, with the total content of Pb, Zn, and Bi being 0.0010%.

[0041] Mg: 0.0050% or less Since Mg is an element that exhibits a desulfurization effect, even a small amount of Mg can improve the hot workability of the alloy, but if added in excess, it significantly reduces the hot workability at temperatures around 900°C. Therefore, in the present invention, when Mg is added, the upper limit of the content is set to 0.0050%. The preferred upper limit is 0.0040%, and the more preferred upper limit is 0.0030%.

[0042] Zr: 0.001 to 0.10% Hf: 0.001~0.10% Addition of 0.001% or more, preferably 0.005% or more, of Zr and Hf fixes P and S, thereby improving the solidification cracking susceptibility, hot workability, and high-temperature oxidation resistance of steel, and can be added as needed. On the other hand, addition of a large amount exceeding 0.10% forms coarse nitrides, adversely affecting manufacturability. Therefore, the upper limit of the addition amount of these elements is set at 0.10%.

[0043] La+Ce+Nd+Pr: 0.001-0.050% Adding La, Ce, Nd, and Pr in a total amount of 0.001% or more, preferably 0.005% or more, fixes P and S and improves the oxidation resistance and hot workability of steel, but adding more than 0.050% in total generates coarse oxides and nitrides, which significantly impair manufacturability, causing nozzle clogging during refining and increasing surface defects. Therefore, the upper limit of the content is set at 0.050% in total for these elements. Methods for adding these elements include adding them as individual metals or alloys, or adding them as misch metal. EXAMPLES

[0044] Examples are described below. The inventors melted high Ni alloys in MgO crucibles using a 50 kg vacuum melting furnace, added Al, Ti, Ca, and Mg as necessary, and cast them into 25 kg square molds to obtain high Ni alloys with the compositions shown in Tables 1-1 and 1-2. For the components shown in Table 1-2, blanks indicate impurity levels. Numerical values ​​outside the range of the present invention and the preferred quality range of the present invention are underlined, including those in Table 2 described below.

[0045] [Table 1-1]

[0046] [Table 1-2]

[0047] The slabs cast from the molten material were tapered, measuring approximately 105mm square to 90mm square, and had a height of approximately 280mm. Round bar tensile test pieces measuring 60mmφ×110mm in the height direction were prepared from the chilled crystal part near the surface of the slab, and hot tensile tests were carried out. The test conditions were to hold at 1220℃ for 30 seconds, then rapidly cool to 1200℃ or 900℃, hold at the specified temperature for 30 seconds, and then tensile to fracture at 20mm / s. The cross-sectional area was measured before and after the test to determine the reduction in area (RA).

[0048] The hot tensile test specimen was removed from the cast strip of about 70 mm thickness, which was heated at 1250°C for 1 hour, rolled to a thickness of 16 mm in the temperature range of 1200°C to 900°C, and then heat-treated at 1200°C to 1260°C (individual conditions are shown in the table). From the hot-rolled annealed sheet, creep test specimens with a measurement part of 6 mmφ, length of 80 mm, and fixed part of 12 mmφ were prepared parallel to the rolling direction. The creep test was performed in accordance with JIS Z 2271, and the time to fracture was measured under conditions of 800°C and 100 MPa. A part of the steel sheet used for the creep test was cut out and subjected to short-term aging treatment at 800°C for 100 hours, after which the cross section was etched using cerium nitrate electrolyte and the metal structure was observed using an optical microscope, and the average crystal grain size was calculated by the section method. The heat treatment conditions, hot tensile test results, and creep test results are summarized in Table 2. The relationship between the reduction in area at 1200°C and the A value of the constraint formula A is shown in Figure 1, the relationship between the reduction in area at 900°C and the B value of the constraint formula B is shown in Figure 2, and the relationship between the creep rupture time and the C value of the constraint formula C is shown in Figure 3.

[0049] [Table 2]

[0050] As shown in Table 2 and Figures 1 to 3, Steel Nos. 1 to 3, 4-3, 4-4, and 5 to 16, which satisfy all of the ranges of the composition and the A-C values ​​of the limiting formulas A to C, all satisfied the RA at 1200°C ≥ 60%, the RA at 900°C ≥ 60%, and the creep rupture time at 800°C and 100 MPa ≥ 250 hours. On the other hand, Steel Nos. 4-1, 4-2, 24, and 25, which did not satisfy the C value ≥ 350, had creep rupture times of less than 250 hours, and Steel Nos. 17 to 21 and Steel Nos. 23 and 26, which did not satisfy the B value ≥ 60, had RAs of less than 60% at 900°C. Furthermore, Steel Nos. 21 to 23, which did not satisfy the A value ≤ 95, had RAs of less than 60% at 1200°C.

[0051] As can be seen from the above examples, the present invention clarifies the manufacturing conditions for a steel sheet having creep strength exceeding 250 hours at 800°C and 100 MPa and exhibiting good hot workability at 1200°C to 900°C. [Industrial Applicability]

[0052] The present invention makes it possible to suitably manufacture high alloys containing Nb and N for applications requiring high-temperature creep strength, and is expected to improve design freedom and reduce steel plate manufacturing costs. Furthermore, these alloys can be widely used not only for high-temperature applications, but also for structures used in high-corrosion-resistant applications. This will enable the provision of stable quality and manufacturability to meet the expanding demand for high-Ni alloys, which will make an enormous contribution to the development of the industry.

Claims

1. The composition contains, by mass%, C: 0.15% or less, Si: 0.05 to 1.0%, Mn: 0.05 to 1.5%, P: 0.030% or less, S: 0.0015% or less, Cr: 20 to 30%, Ni: 30 to 50%, Al: 0.02 to 0.30%, B: 0.0002 to 0.0030%, N: 0.12 to 0.30%, O: 0.006% or less, W: 0.01 to 3.0%, Nb: 0.30 to 0.90%, V: 0.01 to 0.50%, Ca: 0.0001 to 0.0050%, and the balance being Fe and impurities; The A value, B value, and C value defined below are A value ≦ 95, B value ≧ 60, and C value ≧ 350, respectively. The high Ni alloy steel sheet has excellent hot workability and high temperature creep strength, and is characterized by having an alloy composition and average crystal grain size that satisfy the above. however, A value = 12,000 x B (%) + 1,000 x C (%) + 10 x Mn (%) - 30 x Nb (%) +20×Si(%)+W(%)+10×V(%) B value = 115 - 35 x (C (%) + N (%)) - 25 x Nb (%) - 45 x V (%) - 20 x W (%) C value = 0.65 x average grain size (μm) + 350 x W (%) + 850 x V (%) +5,000 × (C (%) − 0.03) − 1,500 × |Nb (%) × N (%) − 0.07|. In the above formula, "element symbol (%)" means the content (mass %) of the corresponding element.

2. The high Ni alloy steel plate according to claim 1, further comprising, in place of a part of the Fe, one or more of the following, in mass %, Mo: 0.01 to 0.80%, Ta: 0.001 to 0.50%, Cu: 0.01 to 0.50%, Co: 0.01 to 1.0%, Ti: 0.001 to 0.10%, Sn: 0.001 to 0.05%, Zn + Pb + Bi: 0.0010% or less, Mg: 0.0050% or less, Zr: 0.001 to 0.10%, Hf: 0.001 to 0.10%, and La + Ce + Nd + Pr: 0.001 to 0.050%. In this case, the A, B, and C values ​​are as follows: A value = 12,000 x B (%) + 1,000 x C (%) + 10 x Mn (%) - 30 x Nb (%) +20×Si(%)+W(%)+10×V(%)+12×Mo(%) B value = 115 - 35 x (C (%) + N (%)) - 25 x Nb (%) - 45 x V (%) - 20 x W (%) -45 x Mo (%) -40 x Ta (%) C value = 0.65 x average grain size (μm) + 350 x (W (%) + Mo (%)) + 850 x V (%) + 550 x Ta (%) +5,000 × (C (%) − 0.03) − 1,500 × |Nb (%) × N (%) − 0.07|. In the above formula, "element symbol (%)" means the content (mass %) of the corresponding element.

Citation Information

Patent Citations

  • Fe-Cr-Ni alloy with excellent high-temperature strength

    JP6675846B2

  • Fe-Cr-Ni alloy with excellent workability and high-temperature strength

    JP7174192B1

Cited By

  • Creep-resistant laser melting flange chassis and preparation method thereof

    CN122625664A

  • Austenite alloy material

    WO2026094928A1

  • Austenitic alloy material

    WO2026182044A1