Cathode active material for non-aqueous electrolyte secondary battery and cathode for the non-aqueous electrolyte secondary battery
By integrating tungsten and boron compounds into lithium-containing transition metal oxides, the reaction resistance of lithium ion secondary battery positive electrodes is reduced, improving the output characteristics of non-aqueous electrolyte secondary batteries.
Patent Information
- Application Number
- JP2024114661
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-05-16
- Filing Date
- 2024-07-18
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2040-03-09
AI Technical Summary
Existing methods for reducing the reaction resistance of lithium ion secondary battery positive electrodes, such as those using lithium tungstate compounds, are insufficient, limiting the output characteristics of non-aqueous electrolyte secondary batteries.
A positive electrode active material for non-aqueous electrolyte secondary batteries is formulated by incorporating a lithium-containing transition metal oxide with specific amounts of tungsten and boron compounds, where tungsten is distributed between primary particles and boron is predominantly on the surface, promoting lithium ion conductivity and reducing resistance.
The synergistic effect of tungsten and boron compounds significantly lowers the reaction resistance of the positive electrode, enhancing the output characteristics of the battery.
Smart Images

Figure 2024138527000001 
Figure 2024138527000002 
Figure 2024138527000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a positive electrode active material for a non-aqueous electrolyte secondary battery and a positive electrode for a non-aqueous electrolyte secondary battery. [Background technology]
[0002] Lithium-containing transition metal oxides are used as positive electrode active materials in lithium ion secondary batteries, which are non-aqueous electrolyte secondary batteries. For example, Patent Document 1 describes a lithium-containing transition metal oxide having the general formula Li z Ni 1-x-y Co x M y A method for increasing the output of a lithium-ion secondary battery is disclosed in which a lithium tungstate compound is attached to the surface of primary particles of a lithium-containing transition metal oxide represented by O2 (0≦x≦0.35, 0≦y≦0.35, 0.95≦z≦1.30, M is at least one element selected from Mn, V, Mg, Mo, Nb, Ti, and Al) to reduce the reaction resistance of the positive electrode. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2016-127004 A Summary of the Invention
[0004] However, the method described in Patent Document 1 cannot sufficiently reduce the reaction resistance of the positive electrode, and there is still room for improvement.
[0005] Therefore, an object of the present disclosure is to provide a nonaqueous electrolyte secondary battery having a lower reaction resistance of the positive electrode and improved output characteristics than conventional batteries by reducing the resistance of the positive electrode active material.
[0006] A positive electrode active material for a non-aqueous electrolyte secondary battery according to one embodiment of the present disclosure includes a lithium-containing transition metal oxide having secondary particles formed by aggregation of primary particles, and a tungsten compound and a boron compound present at least between the primary particles, the tungsten compound being 0.1 to 0.38 mass% in terms of elemental tungsten relative to the mass of the lithium-containing transition metal oxide, the boron compound being 0.006 to 0.17 mass% in terms of elemental boron relative to the mass of the lithium-containing transition metal oxide, the amount of elemental tungsten eluted when the positive electrode active material is washed for 5 minutes with a 0.01 mol / L aqueous sodium hydroxide solution is 60% or less of the amount of elemental tungsten detected when the positive electrode active material is dissolved in a mixed acid containing hydrofluoric acid, nitric acid, and hydrochloric acid, and the amount of elemental boron eluted when the positive electrode active material is washed for 1 minute with ion-exchanged water is 80% or more of the amount of elemental boron detected when the positive electrode active material is dissolved in hydrochloric acid.
[0007] A positive electrode for a non-aqueous electrolyte secondary battery according to one embodiment of the present disclosure is characterized by comprising a positive electrode mixture layer containing the positive electrode active material and a conductive material in an amount of 1 mass % or less relative to the mass of the positive electrode active material.
[0008] According to one embodiment of the present disclosure, a low-resistance positive electrode active material for a nonaqueous electrolyte secondary battery is obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] In lithium-containing transition metal oxides, if a phenomenon called cation mixing occurs in which a transition metal such as nickel enters the site for insertion and desorption of lithium ions during charging and discharging, the resistance of the positive electrode increases, and high output cannot be obtained. For example, Patent Document 1 describes z Ni 1-x-y Co x M yA method has been disclosed in which a lithium tungstate compound is formed on the surface of primary particles of a lithium-containing transition metal oxide represented by the formula: O2 (where 0≦x≦0.35, 0≦y≦0.35, 0.95≦z≦1.30, and M is at least one element selected from Mn, V, Mg, Mo, Nb, Ti, and Al), thereby forming a conductive path for lithium ions at the interface with the electrolyte, thereby reducing the resistance of the positive electrode. However, as a result of intensive studies by the present inventors, it has been found that the resistance of the positive electrode cannot be sufficiently reduced by simply securing a conductive path for lithium ions by adding tungsten. Therefore, the inventors conducted further studies and found that a positive electrode active material can be prepared by adding a tungsten compound and a boron compound to a lithium-containing transition metal oxide, and that the resistance of the positive electrode active material can be reduced if the amount of tungsten element eluted when the positive electrode active material is washed with a 0.01 mol / L aqueous sodium hydroxide solution for 5 minutes is 60% or less of the amount of tungsten element detected when the positive electrode active material is dissolved in a mixed acid containing hydrofluoric acid, nitric acid, and hydrochloric acid, and the amount of boron element eluted when the positive electrode active material is washed with ion exchanged water for 1 minute is 80% or more of the amount of boron element detected when the positive electrode active material is dissolved in hydrochloric acid.
[0010] Hereinafter, the lithium-containing transition metal oxide, the tungsten compound, and the boron compound constituting the positive electrode active material according to this embodiment, and the method for producing the positive electrode active material will be described in detail.
[0011] [Lithium-containing transition metal oxides] The lithium-containing transition metal oxide has secondary particles formed by agglomeration of primary particles. In other words, the lithium-containing transition metal oxide is composed of primary particles and secondary particles formed by agglomeration of the primary particles, and it is preferable that the secondary particles have voids and grain boundaries through which the electrolyte can penetrate, in terms of improving the output characteristics of the non-aqueous electrolyte secondary battery. The average particle size of the primary particles is, for example, preferably 500 nm or less, more preferably in the range of 50 nm to 300 nm. The average particle size of the primary particles is the average value of the major axes of 10 primary particles obtained by obtaining a backscattered electron image (hereinafter sometimes referred to as SEM image) of the cross section of the particle. The median particle size (D50) of the secondary particles is, for example, preferably in the range of 1 μm to 50 μm, more preferably in the range of 5 μm to 20 μm. Here, the median particle size means the median particle size (D50) at which the volume integrated value is 50% in the particle size distribution measured by the laser diffraction scattering method.
[0012] The composition of the lithium-containing transition metal oxide is represented by the general formula Li α Ni 1-w-x-y-z Co w Al x Mn y M z O2 (wherein 0.95≦α≦1.05, 0≦w≦0.09, 0≦x≦0.06, 0≦y≦0.1, 0≦z≦0.01, and M is at least one element selected from Mg, Sr, Si, Y, Mo, V, Ti, Fe, Zr, and Nb). From the viewpoint of increasing the energy density of the nonaqueous electrolyte secondary battery, a large Ni content is preferable, and therefore the sum of w, x, y, and z in the general formula is preferably 0≦w+x+y+z≦0.15, and more preferably 0≦w+x+y+z≦0.12.
[0013] The content of Co contained in the lithium-containing transition metal oxide can be 0≦w≦0.03. In this case, the resistance value of the lithium-containing transition metal oxide increases as the content of Co decreases, and therefore the effect of reducing resistance by adding tungsten and boron becomes more pronounced.
[0014] The lithium-containing transition metal oxide can be synthesized as follows. (1) Formation of transition metal complex oxides First, a transition metal composite hydroxide such as nickel-cobalt-aluminum composite hydroxide obtained by coprecipitation is heat-treated to obtain a transition metal composite oxide. (2) Synthesis of transition metal composite oxides and lithium compounds Next, the transition metal composite oxide is mixed with a lithium compound such as lithium hydroxide or lithium carbonate, and the mixture is heat-treated and then pulverized to obtain lithium-containing transition metal oxide particles.
[0015] [Tungsten compounds] Examples of tungsten compounds (hereinafter, sometimes referred to as W compounds) include tungsten oxide (WO3), lithium tungstate (Li2WO4, Li4WO5, Li6W2O9), and ammonium tungstate. At least a part of the W compounds is present between the primary particles of the lithium-containing transition metal oxide. From an SEM image of a cross section of a secondary particle of the lithium-containing transition metal oxide contained in the positive electrode active material, it can be confirmed that tungsten elements are present between the primary particles constituting the secondary particles. In addition, the W compound is 0.1 to 0.38 mass% in terms of tungsten element with respect to the mass of the lithium-containing transition metal oxide. If the amount of the W compound is within this range, the resistance value of the positive electrode active material can be reduced.
[0016] The amount of tungsten element dissolved when the positive electrode active material is washed with 0.01 mol / L sodium hydroxide solution for 5 minutes is 60% or less of the amount of tungsten element detected when the positive electrode active material is dissolved with a mixed acid containing hydrofluoric acid, nitric acid, and hydrochloric acid (hereinafter, this value may be referred to as the tungsten dissolution rate (W dissolution rate)). If the W dissolution rate is within this range, it is presumed that most of the W compounds are in a state in which they are present between the primary particles of the lithium-containing transition metal oxide, and the resistance of the positive electrode active material is significantly reduced due to the synergistic effect with the distribution state of the boron compound described later.
[0017] Specifically, the W elution rate is calculated as follows. (1) Measurement of the amount of elution into an alkaline aqueous solution 1 g of the positive electrode active material is immersed in 10 mL of 0.01 M NaOH aqueous solution at room temperature, and after stirring for 5 minutes at 200 rpm using a magnetic stirrer, the solution and the positive electrode active material are separated by suction filtration. The separated filtrate is subjected to ICP analysis to measure the amount of tungsten dissolved in the alkaline aqueous solution (NaOH). (2) Calculation of W elution rate (amount eluted in alkaline aqueous solution / total amount) Add 10mL of a 1:1:1 mixture of 46% hydrofluoric acid, 60% nitric acid, and 35% hydrochloric acid to 1g of positive electrode active material, heat at 80℃ for 2 hours to dissolve, and perform ICP analysis of the solution to measure the total amount of tungsten. The W elution rate is calculated by dividing the amount of tungsten eluted into the alkaline aqueous solution by the total amount of tungsten.
[0018] [Boron compounds] Examples of boron compounds (hereinafter sometimes referred to as B compounds) include boric acid (H3BO3), metaboric acid (HBO2), tetraboric acid (H2B4O7), etc. The B compound may be boric acid.
[0019] At least a part of the compound B is present between the primary particles of the lithium-containing transition metal oxide. The amount of the compound B is 0.006 to 0.17% by mass, and preferably 0.006 to 0.11% by mass in terms of boron element, relative to the mass of the lithium-containing transition metal oxide.
[0020] The amount of boron element dissolved when the positive electrode active material is washed with ion-exchanged water for 1 minute is 80% or more of the amount of boron element detected when the positive electrode active material is dissolved with hydrochloric acid (hereinafter, this value may be referred to as the boron dissolution rate (B dissolution rate)). If the B dissolution rate is within this range, it is assumed that most of the B compounds are present on the surface of the secondary particles of the lithium-containing transition metal oxide, and the resistance of the positive electrode active material is significantly reduced due to the synergistic effect with the distribution state of the W compounds. Since the B compounds have Li-ion conductivity, they promote the exchange of Li ions between the electrolyte and the positive electrode active material on the secondary particle surface, and the presence of the B compounds between the primary particles also makes it easier to transfer the Li ions received on the secondary particle surface to the primary particle surface. In addition, the presence of the W compounds on the primary particle surface allows the Li ions to be transferred smoothly.
[0021] The B elution rate is more preferably 93% to 98%, and further preferably 95% to 98%. When the W elution rate is 60% or less, the reaction resistance can be further reduced by setting the B elution rate in the above range.
[0022] Specifically, the B elution rate is calculated as follows. (1) Measurement of the amount of elution into water 1 g of the positive electrode active material was immersed in 30 mL of ion-exchanged water at room temperature and stirred at 200 rpm for 1 minute using a magnetic stirrer, after which the solution and the positive electrode active material were separated by suction filtration. The separated filtrate was subjected to ICP analysis to measure the amount of boron dissolved in the ion-exchanged water. (2) Calculation of B dissolution rate (amount dissolved in water / total amount) Add 10 mL of 6 mol / L hydrochloric acid to 0.5 g of the positive electrode active material, heat at 80°C for 2 hours to dissolve, and perform ICP analysis of the solution to measure the total amount of boron. The B dissolution rate is calculated by dividing the amount of boron dissolved in the ion-exchanged water by the total amount of boron.
[0023] [Method of manufacturing positive electrode active material] <Cleaning process> First, the lithium-containing transition metal oxide is washed with water and dehydrated to obtain a cake-like composition. The lithium-containing transition metal oxide may be particulate material obtained in the synthesis step. By washing with water, it is possible to remove unreacted lithium compounds added in the synthesis step of the lithium-containing transition metal oxide and impurities other than the lithium compounds. When washing with water, for example, 300 g to 5000 g of the lithium-containing transition metal oxide can be added per 1 L of water. The washing with water can be repeated multiple times. Dehydration after washing with water can be performed, for example, with a filter press. By dehydration, the water content of the cake-like composition after washing can be reduced to 10 mass% or less. The water content of the cake-like composition is preferably 2 mass% to 10 mass%, more preferably 4 mass% to 8 mass%, from the viewpoint of facilitating the spreading of the tungsten compound or tungsten-containing solution to be added later on the surface of the lithium-containing transition metal oxide. The moisture content of the cake-like composition is calculated by drying 10 g of the cake-like composition by leaving it in a vacuum at 120° C. for 2 hours, and dividing the change in weight of the cake-like composition before and after drying by the weight of the cake-like composition before drying. The moisture content of the tungsten additive described later is calculated in the same manner.
[0024] <Tungsten addition process> Next, a tungsten compound or a tungsten-containing solution is added to the cake-like composition to obtain a tungsten additive. Even after washing, a part of the lithium compound remains in the cake-like composition, and the remaining lithium compound is dissolved in the water contained in the cake-like composition on the surface of the lithium-containing transition metal oxide contained in the cake-like composition to generate an alkaline aqueous solution.
[0025] When a tungsten compound is added to the cake-like composition, the tungsten compound dissolves in an alkaline aqueous solution and spreads over the entire surface of the lithium-containing transition metal oxide. Examples of the tungsten compound that is directly added to the cake-like composition include tungsten oxide (WO3), lithium tungstate (Li2WO4, Li4WO5, Li6W2O9), etc.
[0026] A tungsten-containing solution may also be added to the cake-like composition. The tungsten concentration in the tungsten-containing solution is, for example, 0.05 mol / L or more, and preferably 0.1 mol / L to 1 mol / L. The tungsten-containing solution is not particularly limited as long as it contains tungsten, but is preferably a solution in which a tungsten compound that is easily soluble in an alkaline solution, such as tungsten oxide, lithium tungstate, or ammonium tungstate, is dissolved in an aqueous solution of lithium hydroxide. In order not to increase the water content of the tungsten additive, it is preferable to add a tungsten compound to the cake-like composition rather than a tungsten-containing solution.
[0027] Furthermore, the tungsten additive may be dried at 150 to 200°C. By drying, the moisture content of the tungsten additive can be adjusted. The drying atmosphere may be, for example, a vacuum. The drying time is not particularly limited, but may be 0.5 to 10 hours. After drying, it may be cooled in a drying furnace or the like.
[0028] <Boron addition process> Next, boron is added to the tungsten additive. By adding boron to the tungsten additive, the conductive path of lithium ions can be secured by the synergistic effect of tungsten and boron, so that the resistance of the positive electrode active material can be further reduced. In addition, tungsten and boron are attached to the surface of the lithium-containing transition metal oxide to coat it, so that the surface structure of the lithium-containing transition metal oxide can be maintained during charging and discharging.
[0029] Examples of the boron compound added directly to the tungsten additive include boric acid (H3BO3), metaboric acid (HBO2), and tetraboric acid (H2B4O7). The particle size of the boron compound is not particularly limited, but from the viewpoint of dispersibility, it is preferably 100 μm or less, more preferably 50 μm or less, and particularly preferably 10 μm or less. A boron-containing solution can also be added to the tungsten additive. The boron concentration in the boron-containing solution is, for example, 0.05 mol / L to 2 mol / L, and preferably 0.1 mol / L to 1 mol / L. The boron-containing solution is not particularly limited as long as it contains boron, but examples include boric acid, metaboric acid, and tetraboric acid, and it is preferable to add lithium hydroxide (LiOH), lithium carbonate (Li2CO3), or the like to make the pH of the boron-containing solution 7 or more. In this case, it is possible to prevent the surface of the tungsten additive from being deteriorated by the acid.
[0030] The tungsten additive to which the boron compound is added may be dried at 150 to 200°C. By drying, the amount of boron present between the secondary particles of the lithium-containing transition metal oxide can be increased. The drying atmosphere can be, for example, a vacuum. The drying time is not particularly limited, but is preferably 0.5 to 10 hours in order to diffuse the boron. The heating rate up to the predetermined heat treatment temperature is preferably 1°C / min to 10°C / min.
[0031] Next, the tungsten additive to which the boron compound is added is heat-treated at a temperature of from 180°C to 330°C to prepare a positive electrode active material. By heat-treating at a temperature of from 180°C to 330°C, which is higher than the melting point of the boron compound, the boron compound or the boron-containing solution can melt and spread over the entire surface of the lithium-containing transition metal oxide. The heat treatment time is not particularly limited, but is preferably 0.5 hours to 15 hours in order to sufficiently melt the boron compound or the boron-containing solution.
[0032] After the heat treatment step, a cooling step can be performed. The boron-containing compound melted by the heat treatment can be reprecipitated by the cooling step. The cooling step is not particularly limited as long as it is a step that can lower the temperature of the tungsten additive, but for example, rapid cooling can be performed to lower the temperature of the tungsten additive to 100°C or less in 30 minutes after the heat treatment step.
[0033] A non-aqueous electrolyte secondary battery to which the above-mentioned positive electrode active material is applied can be obtained by, for example, housing an electrode assembly, in which electrodes (positive electrode, negative electrode) and a separator are laminated or wound, together with a non-aqueous electrolyte in a housing such as a battery can or a laminate. The positive electrode, negative electrode, separator, and non-aqueous electrolyte in this embodiment are, for example, as follows.
[0034] [Positive electrode] The positive electrode includes a positive electrode current collector such as a metal foil and a positive electrode composite layer formed on the positive electrode current collector. The positive electrode current collector may be a foil of a metal such as aluminum that is stable in the potential range of the positive electrode, or a film having the metal disposed on its surface.
[0035] The positive electrode mixture layer preferably contains a positive electrode active material, a conductive material, a binder, etc. The conductive material is preferably 1 mass% or less with respect to the mass of the positive electrode active material. The positive electrode can be produced, for example, by applying a positive electrode mixture slurry containing a positive electrode active material, a conductive material, a binder, etc., onto a positive electrode current collector, drying the coating, and then rolling to form a positive electrode mixture layer on both sides of the positive electrode current collector.
[0036] As the conductive material, carbon powder such as carbon black, acetylene black, ketjen black, graphite, and carbon nanotubes may be used alone or in combination of two or more kinds.
[0037] Examples of the binder include fluorine-based polymers, rubber-based polymers, etc. For example, examples of the fluorine-based polymers include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), or modified versions thereof, and examples of the rubber-based polymers include ethylene-propylene-isoprene copolymers, ethylene-propylene-butadiene copolymers, etc. These may be used alone or in combination of two or more kinds.
[0038] [Negative electrode] The negative electrode includes a negative electrode current collector such as a metal foil, and a negative electrode composite layer formed on the negative electrode current collector. For the negative electrode current collector, a foil of a metal such as copper that is stable in the potential range of the negative electrode, a film with the metal disposed on the surface layer, or the like can be used. The negative electrode composite layer contains a negative electrode active material, and preferably also contains a thickener, a binder, and the like. The negative electrode can be produced, for example, by applying a negative electrode composite slurry in which a negative electrode active material, a thickener, and a binder are dispersed in water at a predetermined weight ratio onto the negative electrode current collector, drying the coating, and then rolling to form a negative electrode composite layer on both sides of the negative electrode current collector.
[0039] As the negative electrode active material, a carbon material capable of absorbing and releasing lithium ions can be used, and in addition to graphite, non-graphitizable carbon, graphitizable carbon, fibrous carbon, coke, carbon black, etc. Furthermore, as a non-carbon-based material, silicon, tin, and alloys and oxides mainly containing these can be used.
[0040] As the binder, PTFE or the like can be used as in the case of the positive electrode, but styrene-butadiene copolymer (SBR) or its modified form may also be used. As the thickener, carboxymethyl cellulose (CMC) or the like can be used.
[0041] [Non-aqueous electrolyte] As the non-aqueous solvent (organic solvent) of the non-aqueous electrolyte, carbonates, lactones, ethers, ketones, esters, etc. can be used, and two or more of these solvents can be mixed and used. For example, cyclic carbonates such as ethylene carbonate, propylene carbonate, butylene carbonate, chain carbonates such as dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, mixed solvents of cyclic carbonates and chain carbonates, etc. can be used.
[0042] The electrolyte salt of the non-aqueous electrolyte may be LiPF6, LiBF4, LiCF3SO3, or a mixture thereof. The amount of electrolyte salt dissolved in the non-aqueous solvent may be, for example, 0.5 to 2.0 mol / L.
[0043] [Separator] The separator may be a porous sheet having ion permeability and insulation. Specific examples of the porous sheet include a microporous thin film, a woven fabric, and a nonwoven fabric. The separator may be made of an olefin resin such as polyethylene or polypropylene, or cellulose. The separator may be a laminate having a cellulose fiber layer and a thermoplastic resin fiber layer such as an olefin resin. The separator may also be a multilayer separator including a polyethylene layer and a polypropylene layer, and may have a material such as an aramid resin or ceramic applied to the surface of the separator. EXAMPLES
[0044] The present disclosure will be further described below with reference to examples, but the present disclosure is not limited to these examples.
[0045] [Preparation of positive electrode active material] <Example 1> A positive electrode active material was prepared according to the following procedure.
[0046] (1) Preparation of lithium-containing transition metal oxide Ni obtained by coprecipitation 0.91 Co 0.05 Al0.04 Nickel-cobalt-aluminum composite hydroxide represented by (OH)2 was heat-treated at 500°C to obtain an oxide. LiOH and the oxide were mixed in an Ishikawa-type mortar so that the molar ratio of Li to the total transition metals was 1.02:1 to obtain a mixture. The mixture was placed in a sintering furnace and heated under an oxygen flow with an oxygen concentration of 95% (10 cm 3 The mixture was sintered at a temperature rise rate of 2.0°C / min from room temperature to 650°C, and then at a temperature rise rate of 0.5°C / min from 650°C to 710°C, at a flow rate of 2 mL / min per kg of mixture and 5 L / min per kg of mixture. 1.01 Ni 0.91 Co 0.05 Al 0.04 Particles of lithium nickel cobalt aluminum composite oxide (lithium-containing transition metal oxide) represented by O2 were obtained. The composition of the lithium-containing transition metal oxide particles was measured using an ICP emission spectrometer.
[0047] (2) Cleaning process 800 g of pure water was added to 1000 g of the lithium nickel cobalt aluminum composite oxide particles, stirred, filtered, separated, and dehydrated to obtain a cake-like composition after a washing step. The water content of the cake-like composition was 4% by mass.
[0048] (3) Tungsten addition process Next, 0.19% by mass of WO3 powder was added to the above cake-like composition in terms of tungsten element relative to the lithium-containing transition metal oxide, and the mixture was heated to 180°C in a vacuum and dried for 3 hours, and then cooled to room temperature in a furnace to obtain a tungsten additive with a moisture content of 0.08% by mass.
[0049] (4) Boron addition process To the tungsten additive, boric acid was added in an amount of 0.01 mass% in terms of boron element relative to the lithium-containing transition metal oxide, and heat treatment was performed for 3 hours in an air atmosphere at 250° C. After the heat treatment process, the tungsten additive was cooled to 100° C. or less within 30 minutes to obtain the positive electrode active material of Example 1. The W elution rate of the obtained positive electrode active material was 55%, and the B elution rate was 100%.
[0050] <Example 2> A positive electrode active material was produced in the same manner as in Example 1, except that in the boron addition step, after the addition of boric acid and before the heat treatment, the temperature was raised to 180°C in a vacuum and drying was performed for 4 hours. The W elution rate of the obtained positive electrode active material was 53%, and the B elution rate was 97%. Since the drying was performed in a vacuum, more boric acid was present between the primary particles than in Example 1, and therefore the B elution rate was lower than that in Example 1.
[0051] <Examples 3 to 7> A positive electrode active material was produced in the same manner as in Example 1, except that the amounts of WO3 powder and boric acid added were changed as shown in Table 1. The W elution rate and B elution rate were as shown in Table 1.
[0052] <Example 8> A positive electrode active material was prepared in the same manner as in Example 1 except for the boron addition step. In the boron addition step, a boron-containing aqueous solution was added to the tungsten additive instead of boric acid. The boron-containing aqueous solution was prepared by adding 0.045 g of boric acid to an aqueous solution in which 0.15 g of lithium hydroxide (LiOH) was dissolved in 10.5 g of pure water, and stirring the solution while heating at 60 ° C. The prepared boron-containing aqueous solution was added to the tungsten additive so that the boron element content was 0.01 mass % relative to the lithium-containing transition metal oxide. The tungsten additive to which the boron-containing aqueous solution was added was held in a vacuum at room temperature for 24 hours, then heated to 180 ° C. and dried for 3 hours, and then cooled to room temperature in a furnace to obtain a tungsten additive with a water content of 0.08 mass %. Thereafter, a heat treatment was performed in an air atmosphere at 250 ° C. for 3 hours, and the mixture was cooled to 100 ° C. or less within 30 minutes to obtain a positive electrode active material of Example 8. The resulting positive electrode active material had a W elution rate of 57% and a B elution rate of 81%. By adding boric acid in the form of an aqueous solution and further holding the material in a vacuum at room temperature, more boric acid was present between the primary particles than in Example 2, and therefore the B elution rate was lower than that in Example 2.
[0053] <Comparative Example 1> Except for not carrying out the boron addition step, a positive electrode active material was produced in the same manner as in Example 1. The W elution rate of the obtained positive electrode active material was 60%.
[0054] <Comparative Example 2> A positive electrode active material was produced in the same manner as in Example 1, except that the tungsten addition step was not carried out, and instead the temperature was raised to 180° C. in a vacuum, drying was carried out for 3 hours, and then the boron addition step was carried out after cooling in a furnace to room temperature. The B elution rate of the obtained positive electrode active material was 100%.
[0055] <Comparative Example 3> A positive electrode active material was produced in the same manner as in Example 1, except that the tungsten addition step and the boron addition step were not performed, and instead the temperature was raised to 180° C. in a vacuum, dried for 3 hours, and then cooled in a furnace to room temperature to obtain a cake-like composition with a moisture content of 0.08 mass %.
[0056] <Comparative Examples 4 to 5> A positive electrode active material was produced in the same manner as in Example 1, except that the amounts of WO3 powder and boric acid added were changed as shown in Table 1. The W elution rate and B elution rate were as shown in Table 1.
[0057] <Comparative Example 6> In the same manner as in Example 1, a washing step was carried out after the preparation of the lithium-containing transition metal oxide. Then, a boron-containing aqueous solution was added to the cake-like composition. The boron-containing aqueous solution was prepared by adding 0.045 g of boric acid to an aqueous solution in which 0.15 g of lithium hydroxide (LiOH) was dissolved in 10.5 g of pure water, and stirring the solution while heating at 60°C. The prepared boron-containing aqueous solution was added to the cake-like composition so that the boron-containing aqueous solution was 0.01 mass% in terms of boron element relative to the lithium-containing transition metal oxide. The cake-like composition to which the boron-containing aqueous solution was added was kept in a vacuum at room temperature for 24 hours, then heated to 180°C and dried for 3 hours, and then cooled in a furnace to room temperature to obtain a boron additive with a water content of 0.08 mass%. Then, a heat treatment was carried out in an air atmosphere at 250°C for 3 hours.
[0058] Next, the tungsten-containing aqueous solution was sprayed onto the boron additive at 200°C or higher. The tungsten-containing aqueous solution was prepared by adding 2.4g of WO3 powder to an aqueous solution in which 1g of lithium hydroxide (LiOH) was dissolved in 20g of pure water, and stirring the solution while heating at 60°C. The prepared tungsten-containing aqueous solution was added to the boron additive so that the tungsten-containing aqueous solution was 0.19% by mass in terms of tungsten element relative to the lithium-containing transition metal oxide. The boron additive to which the tungsten-containing aqueous solution was added was heated to 180°C in a vacuum, dried for 3 hours, and then cooled in a furnace to room temperature to obtain a positive electrode active material of Comparative Example 6. The W elution rate of the obtained positive electrode active material was 100%, and the B elution rate was 72%. By adding boric acid in the form of an aqueous solution and further holding it at room temperature in a vacuum, more boric acid was present between the primary particles than in Example 2, and therefore the B elution rate was lower than that in Example 2. In addition, by spraying tungsten onto the boron additive at 200°C or higher, the water evaporated in a short time and the tungsten compound remained on the secondary particle surface, resulting in a higher W elution rate than in Example 1.
[0059] <Comparative Example 7> In the same manner as in Example 1, a washing step was carried out after the preparation of the lithium-containing transition metal oxide. Thereafter, the temperature was raised to 180°C in a vacuum, and the mixture was dried for 3 hours, and then cooled to room temperature in a furnace to obtain a cake-like composition with a moisture content of 0.08% by mass. Boric acid was added to the cake-like composition in an amount of 0.01% by mass in terms of boron element relative to the lithium-containing transition metal oxide, and a boron additive was obtained by performing a heat treatment for 3 hours in an air atmosphere at 250°C. Next, a tungsten-containing aqueous solution was sprayed onto the boron additive in a state of 200°C or higher. The tungsten-containing aqueous solution was prepared by adding 2.4g of WO3 powder to an aqueous solution in which 1g of lithium hydroxide (LiOH) was dissolved in 20g of pure water, and stirring the solution while heating at 60°C. The prepared tungsten-containing aqueous solution was added to the boron additive so that the amount was 0.19% by mass in terms of tungsten element relative to the lithium-containing transition metal oxide. The boron additive to which the tungsten-containing aqueous solution was added was heated to 180°C in a vacuum, dried for 3 hours, and then cooled to room temperature in a furnace to obtain a positive electrode active material of Comparative Example 7. The W elution rate of the obtained positive electrode active material was 100%, and the B elution rate was 96%. The W elution rate was higher than that of Example 1 for the same reason as in Comparative Example 6. The B elution rate was slightly lower than that of Example 1 because more tungsten was present on the surface of the secondary particles than in Example 1.
[0060] [Preparation of positive electrode] The positive electrode active materials prepared in Examples 1 to 8 and Comparative Examples 1 to 7, acetylene black, and polyvinylidene fluoride were mixed in a mass ratio of 40:2:1, and were kneaded using an agate mortar and pestle to form thin pellets. After that, the mixture was rolled to a predetermined thickness using a roller, and then punched into a predetermined circular shape to form a positive electrode.
[0061] [Preparation of non-aqueous electrolyte] Ethylene carbonate (EC), methyl ethyl carbonate (MEC), and dimethyl carbonate (DMC) were mixed in a volume ratio of 20:5:75. Lithium hexafluorophosphate (LiPF6) was dissolved in the mixed solvent to a concentration of 1.2 mol / L to prepare a non-aqueous electrolyte.
[0062] [Preparation of test cell] The positive electrode and the negative electrode made of lithium metal were stacked facing each other with a separator interposed therebetween to prepare an electrode body. The electrode body and the non-aqueous electrolyte were then inserted into an aluminum coin-shaped exterior body and sealed by crimping with a press machine to prepare a test cell. Test cells were prepared in the same manner as in the other examples and comparative examples.
[0063] [Measurement of reaction resistance] The above test cell was charged at a constant current of 0.7 mA under a temperature condition of 25° C. until the cell voltage reached 4.3 V, and then charged at a constant voltage of 4.3 V until the current value reached 0.07 mA. Subsequently, a constant current discharge was performed at 0.7 mA until the cell voltage reached 2.5 V. Thereafter, again under a temperature condition of 25° C., a constant current charge was performed at 0.7 mA until the cell voltage reached 4.3 V, and then a constant voltage charge was performed at 4.3 V until the current value reached 0.07 mA. Next, the test cell was measured for AC impedance at 20 kHz to 0.01 Hz using an AC impedance measuring device, and a Cole-Cole plot was drawn from the measured data, and the reaction resistance was calculated from the size of the arc between 10 Hz and 0.1 Hz. The reaction resistance shown in Table 1 is expressed relatively to the reaction resistance of the test cell containing the positive electrode active material of Comparative Example 1, which is set to 100, and the reaction resistance of the other test cells.
[0064] [Table 1]
[0065] <Example 9> By changing the composition of the nickel-cobalt-aluminum composite hydroxide, the composition of the lithium-containing transition metal oxide can be changed to Li 1.01 Ni 0.88 Co 0.09 Al 0.03 Except for changing to O2, a positive electrode active material was produced in the same manner as in Example 1. The W elution rate of the obtained positive electrode active material was 59%, and the B elution rate was 100%.
[0066] <Comparative Example 8> By changing the composition of the nickel-cobalt-aluminum composite hydroxide, the composition of the lithium-containing transition metal oxide can be changed to Li 1.01 Ni 0.88 Co 0.09 Al 0.03 Except for changing to O2, a positive electrode active material was produced in the same manner as in Comparative Example 1. The W elution rate of the obtained positive electrode active material was 55%.
[0067] <Comparative Example 9> By changing the composition of the nickel-cobalt-aluminum composite hydroxide, the composition of the lithium-containing transition metal oxide can be changed to Li 1.01 Ni 0.88 Co 0.09 Al 0.03 A positive electrode active material was produced in the same manner as in Comparative Example 3, except that O2 was used.
[0068] Using the positive electrode active materials obtained in Example 9 and Comparative Examples 8 and 9, test cells were prepared and the reaction resistance was measured in the same manner as in Example 1. The reaction resistance shown in Table 2 is expressed relatively to the reaction resistance of the test cell containing the positive electrode active material of Comparative Example 8, which is set to 100, and the reaction resistances of the other test cells.
[0069] [Table 2]
[0070] <Example 10> By changing the composition of the nickel-cobalt-aluminum composite hydroxide, the composition of the lithium-containing transition metal oxide can be changed to Li 1.01 Ni 0.92 Co 0.05 Al 0.03 Except for changing to O2, a positive electrode active material was produced in the same manner as in Example 1. The W elution rate of the obtained positive electrode active material was 58%, and the B elution rate was 100%.
[0071] <Comparative Example 10> By changing the composition of the nickel-cobalt-aluminum composite hydroxide, the composition of the lithium-containing transition metal oxide can be changed to Li 1.01 Ni 0.92 Co 0.05 Al 0.03 Except for changing to O2, a positive electrode active material was produced in the same manner as in Comparative Example 1. The W elution rate of the obtained positive electrode active material was 57%.
[0072] Using the positive electrode active materials obtained in Example 10 and Comparative Example 10, test cells were prepared and the reaction resistance was measured in the same manner as in Example 1. The reaction resistance shown in Table 3 is a relative expression of the reaction resistance of the test cell containing the positive electrode active material of Example 10, with the reaction resistance of the test cell containing the positive electrode active material of Comparative Example 10 taken as 100.
[0073] [Table 3]
[0074] <Comparative Example 11> By changing the composition of the nickel-cobalt-aluminum composite hydroxide, the composition of the lithium-containing transition metal oxide can be changed to Li 1.01 Ni 0.82 Co 0.15 Al 0.03 Except for changing to O2, a positive electrode active material was produced in the same manner as in Example 1. The W elution rate of the obtained positive electrode active material was 52%, and the B elution rate was 100%.
[0075] <Comparative Example 12> By changing the composition of the nickel-cobalt-aluminum composite hydroxide, the composition of the lithium-containing transition metal oxide can be changed to Li 1.01 Ni 0.82 Co 0.15 Al 0.03 Except for changing to O2, a positive electrode active material was produced in the same manner as in Comparative Example 1. The W elution rate of the obtained positive electrode active material was 58%.
[0076] <Comparative Example 13> By changing the composition of the nickel-cobalt-aluminum composite hydroxide, the composition of the lithium-containing transition metal oxide can be changed to Li 1.01 Ni 0.82 Co 0.15 Al 0.03 A positive electrode active material was produced in the same manner as in Comparative Example 3, except that O2 was used.
[0077] Using the positive electrode active materials obtained in Comparative Examples 11 to 13, test cells were prepared and the reaction resistance was measured in the same manner as in Example 1. The reaction resistance shown in Table 4 is expressed relatively to the reaction resistance of the test cell containing the positive electrode active material of Comparative Example 11, which is set to 100, and the reaction resistances of the other test cells.
[0078] [Table 4]
[0079] <Example 11> By changing the composition of the nickel-cobalt-aluminum composite hydroxide, the composition of the lithium-containing transition metal oxide can be changed to Li 1.01 Ni 0.92 Co 0.02 Al 0.02 Mn 0.04 Except for changing to O2, a positive electrode active material was produced in the same manner as in Example 1. The W elution rate of the obtained positive electrode active material was 56%, and the B elution rate was 100%.
[0080] <Comparative Example 14> By changing the composition of the nickel-cobalt-aluminum composite hydroxide, the composition of the lithium-containing transition metal oxide can be changed to Li 1.01 Ni 0.92 Co 0.02 Al 0.02 Mn 0.04 Except for changing to O2, a positive electrode active material was produced in the same manner as in Comparative Example 1. The W elution rate of the obtained positive electrode active material was 54%.
[0081] Using the positive electrode active materials obtained in Example 11 and Comparative Example 14, test cells were prepared and the reaction resistance was measured in the same manner as in Example 1. The reaction resistance shown in Table 5 is a relative expression of the reaction resistance of the test cell containing the positive electrode active material of Example 11, with the reaction resistance of the test cell containing the positive electrode active material of Comparative Example 14 taken as 100.
[0082] [Table 5]
[0083] In Examples 1 to 11, it was confirmed that by adding not only tungsten but also boron and setting the W elution rate and B elution rate within a predetermined range, the reaction resistance was lower than that of Comparative Example 1. On the other hand, in Comparative Examples 2 to 7, the reaction resistance was higher than that of Comparative Example 1.
[0084] Moreover, it was confirmed from Examples 1, 9, 10, and 11 that the effect of adding boron is greater as the amount of Co contained in the lithium-containing transition metal oxide is smaller. On the other hand, from Comparative Examples 11 and 12, no effect of adding boron was obtained when the amount of Co was 15 mol%.
Claims
1. a lithium-containing transition metal oxide having secondary particles formed by aggregation of primary particles; A positive electrode active material for a non-aqueous electrolyte secondary battery, comprising a tungsten compound and a boron compound present at least between the primary particles, The tungsten compound is present in an amount of 0.1 to 0.38 mass% in terms of elemental tungsten relative to the mass of the lithium-containing transition metal oxide, The boron compound is present in an amount of 0.006 to 0.17% by mass in terms of boron element relative to the mass of the lithium-containing transition metal oxide, an amount of tungsten element eluted when the positive electrode active material is washed with a 0.01 mol / L aqueous sodium hydroxide solution for 5 minutes is 60% or less of an amount of tungsten element detected when the positive electrode active material is dissolved in a mixed acid containing hydrofluoric acid, nitric acid, and hydrochloric acid; a positive electrode active material for a non-aqueous electrolyte secondary battery, wherein an amount of elemental boron eluted when the positive electrode active material is washed with ion-exchanged water for one minute is 80% or more of an amount of elemental boron detected when the positive electrode active material is dissolved in hydrochloric acid.
2. The composition of the lithium-containing transition metal oxide is represented by the general formula Li α Ni 1-w-x-y-z Co w A x Mn y M z O 2 2. The positive electrode active material for a nonaqueous electrolyte secondary battery according to claim 1, represented by the formula: (wherein 0.95≦α≦1.05, 0≦w≦0.09, 0≦x≦0.06, 0≦y≦0.1, 0≦z≦0.01, and M is at least one element selected from Mg, Sr, Si, Y, Mo, V, Ti, Fe, Zr, and Nb).
3. 3. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 2, wherein the content of Co contained in the lithium-containing transition metal oxide satisfies 0≦w≦0.
03.
4. 4. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein the boron compound contains boric acid.
5. The positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 4, wherein the boron compound is present in an amount of 0.006 to 0.11 mass% in terms of boron element relative to the mass of the lithium-containing transition metal oxide.
6. The amount of boron element eluted when the positive electrode active material is washed with ion-exchanged water for 1 minute is 93% to 98% of the amount of boron element detected when the positive electrode active material is dissolved with hydrochloric acid. The positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 5.
7. A positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 6, a conductive material in an amount of 1% by mass or less relative to the mass of the positive electrode active material;
Citation Information
Patent Citations
Method of manufacturing positive electrode active material, and positive electrode active material
JP2010040383A
Positive electrode active material for nonaqueous electrolyte secondary battery and method of producing the same
JP2015133318A
Positive electrode active substance for non-aqueous electrolyte secondary battery and method for producing same, positive electrode mixture paste for non-aqueous electrolyte secondary battery, and non-aqueous electrolyte secondary battery
WO2018043515A1
Positive electrode active material for nonaqueous electrolyte secondary battery, manufacturing method thereof, and nonaqueous electrolyte secondary battery arranged by use of positive electrode active material
JP2016127004A