Manufacturing method of faraday rotator and optical isolator

The method of immersing Faraday rotator chips in a hot phosphoric acid solution effectively removes particles, ensuring high-quality anti-reflection film formation on Faraday rotators.

JP2024138931AInactive Publication Date: 2024-10-09SHIN ETSU CHEMICAL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023049660
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for cleaning Faraday rotators are inefficient in removing particles generated during cutting and polishing, leading to incomplete removal and subsequent damage to anti-reflection films.

Method used

Immersing the Faraday rotator chips in a hot phosphoric acid solution with specific concentration and temperature ranges to dissolve and remove particles, followed by vapor deposition of anti-reflection films.

Benefits of technology

Achieves complete removal of particles, enabling high-quality anti-reflection film deposition without defects.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide a manufacturing method of a Faraday rotator capable of efficiently removing particles before and after vapor deposition, especially before the vapor deposition, to address such a problem that, although an antireflection film is vapor-deposited on both light transmission surfaces of a chip used as a Faraday rotator, when particles remain on the light transmission surfaces, the antireflection film after the vapor deposition is deteriorated.SOLUTION: A manufacturing method of a Faraday rotator includes: a cutting step of cutting out a substantially rectangular flat plate to be used as a Faraday rotator from a single crystal circular wafer; a step of cleaning the substantially rectangular flat plate; and an antireflection film forming step of forming an antireflection film on light transmission surfaces of the substantially rectangular flat plate. In the step of cleaning the substantially rectangular flat plate, the substantially rectangular flat plate is immersed in a hot phosphoric acid solution to dissolve and remove attached particles.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an optical isolator used in optical communications, and more particularly to a method for manufacturing a Faraday rotator used in an optical isolator. [Background technology]

[0002] In laser light sources used in optical processing machines, optical measuring instruments, and optical communications, if the emitted laser light is reflected by the surface of a component installed along the transmission path and part of the reflected light returns to the laser light source and enters it, the laser oscillation becomes unstable. In order to block such reflected light, an optical isolator is used that uses a Faraday rotator that rotates the polarization plane of the reflected light non-reciprocally.

[0003] An optical isolator is primarily composed of a polarizer, an analyzer, a Faraday rotator, and a permanent magnet that magnetizes the Faraday rotator to induce a Faraday rotation angle. It is installed between a light source and an optical transmission component, and transmits only the light traveling toward the optical transmission component and blocks the reflected light returning toward the light source.

[0004] For example, the structure of a polarization-dependent optical isolator is such that a polarizer is provided on the input side and an analyzer is provided on the output side. That is, a Faraday rotator is placed between the polarizer and the analyzer, and rotates the polarization axis of the incident light by 45 degrees. The polarizer and the analyzer are also placed so that the relative angle between their transmission polarization axes is 45 degrees.

[0005] The light that enters the optical isolator passes through the polarizer and the Faraday rotator, where its polarization plane is rotated by 45 degrees. This rotation causes the polarization plane of the light to match that of the analyzer, allowing the light to pass through the analyzer. Meanwhile, the reflected light reaches the optical isolator from the opposite direction, passes through the analyzer, and then the Faraday rotator, but the polarization plane of the light is further rotated by 45 degrees by the Faraday rotator, making it perpendicular to the polarization plane of the polarizer, and therefore unable to pass through the polarizer. Therefore, the reflected light cannot return to the laser light source, and does not adversely affect laser oscillation.

[0006] In optical communications, magnetic materials such as bismuth-substituted rare earth iron garnet single crystals are used as the Faraday rotators of optical isolators, so extremely advanced cleaning is required to remove fine particles from these materials.

[0007] In the manufacture of Faraday rotators, a circular wafer after single crystal growth is cut into square chips with dimensions determined according to the required specifications, typically 11 to 15 mm on a side, using a cutting device such as a dicing saw. In the subsequent processing step, an anti-reflective coating is formed on both sides of the chip, but in order to form a high-quality anti-reflective coating, it is extremely important to completely remove particles adhering to the surface of the chip by cleaning before depositing the anti-reflective coating.

[0008] In the cutting process, a dicing machine is usually used, but when cutting with a blade with diamond grains embedded, cutting powder from the work itself is generated, and also when lapping or polishing, fine powder from the work itself is generated, and these particles adhere to the surface of the chip. As a method for cleaning the chip, it is common to attach a large number of chips to a cleaning tool and clean them in an ultrasonic cleaning device using polyethylene alkaline detergent or pure water.

[0009] To address the above-mentioned problems, Patent Document 1 describes a method of cleaning a Faraday rotator with an ultrasonic cleaner by applying ultrasonic waves while the rotator is placed in a magnetic field with a magnetic flux density of 500 G (gauss) or more. However, even if ultrasonic waves are applied in such a magnetic field for cleaning, it is difficult to completely remove particles, and therefore it is difficult to deposit and form a high-quality anti-reflection film.

[0010] Patent Document 2 describes a method of cleaning a side surface of a Faraday rotator processed into a chip shape with a resin layer, which is then cleaned with an ultrasonic cleaner. However, although this method can prevent particles from adhering to the side surface, it is not possible to completely remove particles adhering to other surfaces by ultrasonic cleaning, making it difficult to deposit and form a high-quality anti-reflection coating. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] JP 2007-121992 A [Patent Document 2] Patent No. 2849655 Summary of the Invention [Problem to be solved by the invention]

[0012] Since the material of the Faraday rotator itself is an insulator, particles from the workpiece itself generated during the cutting process, polishing process, etc. tend to adhere to the chip, but the ultrasonic cleaning method described above is unable to completely remove the particles that were attached before cleaning from the chip. If an anti-reflective film is evaporated onto the chip in such a situation where the particles are not completely removed, the anti-reflective film is applied on top of the attached particles, which causes a major problem in that the anti-reflective film is damaged when the particles fall off for some reason.

[0013] In addition, cleaning of Faraday rotators cannot be completed by ultrasonic cleaning equipment alone, and it is necessary to wipe off particles with a cotton swab or cleaning paper soaked in a solvent, etc., which results in poor work efficiency. Therefore, there is a demand for an improvement in the efficiency of the cleaning work of Faraday rotators.

[0014] The present invention has been made in consideration of the above-mentioned problems, and has an object to provide a method for manufacturing a Faraday rotator that is capable of depositing and forming a high-quality anti-reflection film when the anti-reflection film is deposited on the Faraday rotator. [Means for solving the problem]

[0015] The inventors discovered that by immersing a Faraday rotator tip in a hot phosphoric acid solution to dissolve and remove particles, it is possible to remove particles that were incompletely removed by an ultrasonic cleaner, and that a high-quality anti-reflection film can be obtained by the subsequent deposition of an anti-reflection film, thus completing the present invention.

[0016] Therefore, the present invention provides the following Faraday rotator and method for manufacturing an optical isolator. [1] A method for manufacturing a Faraday rotator, comprising: a cutting step of cutting a substantially square flat plate to be used as a Faraday rotator from a single crystal circular wafer; a cleaning step of cleaning the substantially square flat plate; and an anti-reflection film forming step of forming an anti-reflection film on a light transmitting surface of the substantially square flat plate, 4. A method for manufacturing a Faraday rotator, wherein the cleaning step includes immersing the approximately rectangular flat plate in a hot phosphoric acid solution. [2] The method for producing a Faraday rotator according to [1] above, wherein the hot phosphoric acid solution has a concentration of 50 to 89 mass % and a temperature of 100°C to 170°C. [3] The method for producing a Faraday rotator according to [2] above, wherein the temperature of the hot phosphoric acid solution is 120°C to 150°C. [4] The method for producing a Faraday rotator according to [1] above, wherein the approximately rectangular plate is immersed in the hot phosphoric acid solution for 1 to 10 minutes. [5] The method for producing a Faraday rotator according to any one of [1] to [4] above, wherein the substantially rectangular plate is immersed in the hot phosphoric acid solution at least once before the anti-reflection film forming step is performed. [6] A method for manufacturing an optical isolator including a polarizer, a Faraday rotator, and an analyzer, comprising the steps of: A method for producing an optical isolator, comprising the steps of: [7] The method for producing an optical isolator according to [6] above, wherein the hot phosphoric acid solution has a concentration of 50 to 89 mass % and a temperature of 100°C to 170°C. [8] The method for producing an optical isolator according to [7] above, wherein the temperature of the hot phosphoric acid solution is 120°C to 150°C. [9] The method for producing an optical isolator according to [6] above, wherein the approximately square plate is immersed in the hot phosphoric acid solution for 1 to 10 minutes.

[10] The method for manufacturing an optical isolator according to any one of [6] to [9] above, wherein the approximately rectangular flat plate is immersed in the hot phosphoric acid solution at least once before carrying out the anti-reflection film forming step. Effect of the Invention

[0017] According to the method for manufacturing a Faraday rotator of the present invention, it is possible to remove particles of the workpiece itself that are attached to the Faraday rotator, and it is possible to obtain a Faraday rotator on which a high-quality anti-reflection film is deposited and formed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] A first aspect of the present invention is a method for manufacturing a Faraday rotator, comprising the steps of: cutting a substantially square flat plate to be used as a Faraday rotator from a single crystal circular wafer; cleaning the substantially square flat plate; and forming an anti-reflection film on a light transmitting surface of the substantially square flat plate, This is a method for producing a Faraday rotator, characterized in that the cleaning step includes immersing the approximately square plate in a hot phosphoric acid solution (a heated phosphoric acid solution).

[0019] In the above-mentioned manufacturing method, the Faraday rotator to be manufactured is not particularly limited. For example, YFeO 12 (YIG), Y3Al5O 12 (YAG), Tb3Ga5O 12The Faraday rotator is made of a single crystal of bismuth-substituted rare earth iron garnet such as TGG. Antireflection films are often applied to both light transmitting surfaces of the Faraday rotator, and the manufacturing method of the present invention is preferably applied to such cases.

[0020] The manufacturing method is characterized in that in one of the cleaning steps for cleaning an approximately square flat plate to be used as a Faraday rotator, the approximately square flat plate is immersed in a hot phosphoric acid solution to dissolve and remove particles of the workpiece itself that are generated and attached to the chip surface by cutting, polishing, etc.

[0021] The temperature of the hot phosphoric acid solution when the approximately square flat plate is immersed in the hot phosphoric acid solution is usually 100°C to 170°C, preferably 110°C to 160°C, and more preferably 120°C to 150°C. If the temperature of the hot phosphoric acid solution exceeds 170°C, boiling becomes intense, the approximately square flat plate dissolves faster, and it becomes difficult to adjust the film thickness. On the other hand, if the temperature is less than 100°C, the particle dissolution rate becomes slow, and the workability is likely to deteriorate.

[0022] The hot phosphoric acid solution has a phosphoric acid (H3PO4) concentration of usually 50 to 89 mass%, preferably 70 to 89 mass%, and more preferably 80 to 89 mass%. If the hot phosphoric acid solution has a concentration of more than 89 mass%, the dissolution rate of the approximately square plate increases, making it difficult to adjust the film thickness. On the other hand, if the hot phosphoric acid solution has a concentration of less than 50 mass%, the dissolution rate of particles decreases, increasing the possibility of deteriorating workability.

[0023] The time for immersing the approximately square plate in the hot phosphoric acid solution is usually 1 to 10 minutes, preferably 2 to 8 minutes, and more preferably 3 to 6 minutes. If it exceeds 10 minutes, the approximately square plate may be dissolved too much. On the other hand, if it is less than 1 minute, the particles may not be dissolved sufficiently.

[0024] The solvent of the hot phosphoric acid solution is typically water, but a solvent such as alcohol (e.g., methanol, ethanol, isopropanol, butanol, ethylene glycol) can also be used. These solvents may be used alone or in combination of two or more.

[0025] In the manufacturing method, it is preferable to immerse the substantially rectangular flat plate in the hot phosphoric acid solution at least once before carrying out the anti-reflection film forming step. After the anti-reflection film is formed on the light transmitting surface of the substantially rectangular flat plate, the particles are not sufficiently dissolved, and the effect of the present invention cannot be fully obtained.

[0026] A second aspect of the present invention is a method for manufacturing an optical isolator including a polarizer, a Faraday rotator, and an analyzer, comprising the steps of: A method for producing an optical isolator, wherein the Faraday rotator is produced by the method according to the first aspect of the present invention.

[0027] In the method for manufacturing an optical isolator, the optical isolator to be manufactured is not particularly limited, and generally includes a polarizer, an analyzer, a Faraday rotator, and a permanent magnet for magnetically saturating the Faraday rotator.

[0028] In the method for producing the optical isolator, a Faraday rotator is obtained by applying the above-mentioned method for producing a Faraday rotator of the present invention, and then an optical isolator is produced according to a conventional method. As an example of a specific embodiment, for example, an optical isolator is produced as follows. That is, the Faraday rotator chip cut from the wafer by a dicing machine into a square with a side of 11 mm to 15 mm is fabricated as a Faraday rotator after undergoing various processes including the cleaning process based on the first embodiment of the present invention described above. Then, a square polarizer with a side of the same size as the Faraday rotator and an analyzer are stacked on both sides of the light transmission direction, and the chip is further engraved by a dicing machine into a square with a side of 0.5 mm, for example. Then, a magnet is placed so as to apply a magnetic field parallel to the light transmission direction. In addition, elements such as a wave plate and a filter are added as necessary, and the chip is usually placed in a housing to manufacture an optical isolator as a device.

[0029] The polarizer and analyzer are linear polarizing plates, usually glass plates with metal particles dispersed in them, and their polarization mechanism is due to the resonance absorption of the conduction electrons in the metal particles. In addition, the polarizer and analyzer are generally made of the same material and shape, and are called polarizers when placed on the light incident side and analyzers when placed on the reflection or transmission side. There are no particular limitations on the magnets, but for example, SmCo magnets and NdFeB magnets are used. The magnets are usually hollow and cylindrical, and a monolith magnet may be used, or multiple magnets may be used to create the desired shape. EXAMPLES

[0030] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0031] [Example 1] A bismuth-substituted rare earth iron garnet single crystal film was grown on a circular Ca, Mg, Zr, etc.-substituted gadolinium-gallium-garnet substrate (SGGG substrate: manufactured by Saint-Gobain) with a diameter of 3 inches by liquid phase epitaxy. Then, the thickness of the bismuth-substituted rare earth iron garnet single crystal film was set to 0.4 mm by double-sided polishing, and both sides were mirror-finished. Next, cutting was performed with a 0.1 mm thick diamond blade (#600) in a peripheral blade dicing device, and 20 chips measuring 11 mm square were obtained from one bismuth-substituted rare earth iron garnet single crystal film.

[0032] The obtained chip was immersed in a hot phosphoric acid aqueous solution at 120°C (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., product code 162-02177, concentration: phosphoric acid (H3PO4) 85.0% by mass, pure water 15.0% by mass) for 5 minutes to dissolve and remove the cutting and polishing powder adhering to the chip, and then ultrasonic cleaning was performed. After that, it was set in a vacuum deposition device, and an anti-reflection film was deposited on the chip surface to produce a Faraday rotator. The deposited anti-reflection film was then observed with an optical microscope, and the number (average) of missing parts of the anti-reflection film was found to be 0.

[0033] [Example 2] A Faraday rotator was produced in the same manner as in Example 1, except that the temperature of the hot phosphoric acid solution was set to 100° C. Thereafter, the deposited antireflection film was observed under an optical microscope, and the number (average number) of missing portions of the antireflection film was found to be 1.

[0034] [Example 3] A Faraday rotator was produced in the same manner as in Example 1, except that the temperature of the hot phosphoric acid solution was set to 100° C. and the immersion time was set to 6 minutes. Thereafter, the deposited antireflection film was observed under an optical microscope, and the number (average value) of missing portions of the antireflection film was found to be zero.

[0035] [Example 4] A Faraday rotator was produced in the same manner as in Example 1, except that the temperature of the hot phosphoric acid solution was set to 150° C. and the immersion time was set to 3 minutes. Thereafter, the deposited antireflection film was observed with an optical microscope, and the number (average value) of missing portions of the antireflection film was found to be zero.

[0036] [Example 5] A Faraday rotator was produced in the same manner as in Example 1, except that after an antireflection film was deposited and formed on the chip surface, it was immersed for 5 minutes in a hot phosphoric acid solution at 120° C. Thereafter, the deposited antireflection film was observed under an optical microscope, and the number (average number) of missing portions of the antireflection film was found to be 3.

[0037] [Comparative Example 1] A Faraday rotator was produced in the same manner as in Example 1, except that the step of immersing the chip obtained by cutting in a hot phosphoric acid solution at 120° C. was not performed. Thereafter, the deposited antireflection film was observed with an optical microscope, and the number (average number) of missing portions of the antireflection film was found to be 10.

[0038] [Comparative Example 2] A Faraday rotator was produced in the same manner as in Example 1, except that a phosphoric acid solution at 14° C. that had been left without heating was used instead of the hot phosphoric acid solution. Thereafter, the deposited antireflection film was observed under an optical microscope, and the number (average number) of missing portions of the antireflection film was found to be 8.

[0039] (Results / Discussion) In Examples 1 to 4, the Faraday rotator chip was immersed in a hot phosphoric acid solution before the anti-reflection coating was deposited, and the cutting powder and polishing powder adhering to the chip were dissolved and removed, thereby suppressing the occurrence of defects due to the loss of the anti-reflection coating after deposition. Moreover, Example 5 revealed that the cutting powder and polishing powder adhering to the chip could be dissolved and removed by immersing the Faraday rotator in a hot phosphoric acid solution after the anti-reflection coating was deposited.

[0040] On the other hand, in Comparative Example 1, in which ultrasonic cleaning was only performed without immersion in a hot phosphoric acid solution, and in Comparative Example 2, in which a phosphoric acid solution other than a hot phosphoric acid solution was used, the number of defects due to chipping of the antireflective film after deposition of the antireflective film was large, and the results were inferior to those of Examples 1 to 4.

[0041] As described above, it was found that by immersing the chip in a hot phosphoric acid solution to dissolve and remove cutting and polishing powder adhering to the chip before depositing an antireflective film on the light-transmitting surface of the chip to be used as a Faraday rotator, a high-quality antireflective film can be formed without any missing parts after deposition.

[0042] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention.

Claims

1. A method for manufacturing a Faraday rotator, comprising: a cutting step of cutting a substantially square flat plate to be used as a Faraday rotator from a single crystal circular wafer; a cleaning step of cleaning the substantially square flat plate; and an anti-reflection film forming step of forming an anti-reflection film on a light transmitting surface of the substantially square flat plate, 4. A method for manufacturing a Faraday rotator, wherein the cleaning step includes immersing the approximately rectangular flat plate in a hot phosphoric acid solution.

2. 2. The method for manufacturing a Faraday rotator according to claim 1, wherein the hot phosphoric acid solution has a concentration of 50 to 89 mass % and a temperature of 100° C. to 170° C.

3. 3. The method for manufacturing a Faraday rotator according to claim 2, wherein the temperature of the hot phosphoric acid solution is 120° C. to 150° C.

4. 2. The method for manufacturing a Faraday rotator according to claim 1, wherein the approximately rectangular plate is immersed in the hot phosphoric acid solution for 1 to 10 minutes.

5. 5. The method for manufacturing a Faraday rotator according to claim 1, wherein the substantially rectangular flat plate is immersed in the hot phosphoric acid solution at least once before the anti-reflection film forming step is performed.

6. A method for manufacturing an optical isolator including a polarizer, a Faraday rotator, and an analyzer, comprising the steps of:

2. A method for producing an optical isolator, comprising the steps of: forming said Faraday rotator by the method of claim 1;

7. 7. The method for producing an optical isolator according to claim 6, wherein the hot phosphoric acid solution has a concentration of 50 to 89 mass % and a temperature of 100° C. to 170° C.

8. 8. The method for producing an optical isolator according to claim 7, wherein the temperature of the hot phosphoric acid solution is 120° C. to 150° C.

9. 7. The method for producing an optical isolator according to claim 6, wherein the approximately rectangular plate is immersed in the hot phosphoric acid solution for 1 to 10 minutes.

10. 10. The method for producing an optical isolator according to claim 6, wherein the substantially rectangular flat plate is immersed in the hot phosphoric acid solution at least once before the anti-reflection film forming step is performed.

Citation Information

Patent Citations

  • Faraday rotator using square hysteresis, and its manufacturing method

    JP2004125840A

  • Method and apparatus for cleaning optical component, and method and apparatus for spin-drying optical component after cleaning, and optical component holding parts

    JP2007121992A

  • Optical isolator manufacturing method