Cured product and producing method thereof

A cured body is produced using concrete sludge and controlled curing reactions to address the high cost and environmental impact of natural concretion production, achieving cost-effective and eco-friendly manufacturing.

JP2024139001APending Publication Date: 2024-10-09MITSUBISHI UBE CEMENT CORP

Patent Information

Application Number
JP2023049760
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

The production of cured bodies using natural concretions is costly and may increase carbon dioxide emissions due to the high cost of raw materials and environmental burden.

Method used

A hardened body is produced using concrete sludge, cement, aggregate, glycerol carbonate, dimethyl carbonate, glycerin, and water, with specific ratios of calcium hydroxide and glycerin to control the curing reaction and reduce carbon emissions.

Benefits of technology

The method allows for the production of a cured body at a lower cost while reducing carbon dioxide emissions, utilizing waste materials effectively.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139001000001_ABST
    Figure 2024139001000001_ABST
Patent Text Reader

Abstract

To provide a cured product which can be produced at a low cost by utilizing waste and having the exhaust of carbon dioxide suppressed, and a producing method thereof.SOLUTION: There is provided a cured product obtained by curing a mixture of concrete sludge, cement, aggregate, glycerol carbonate, dimethyl carbonate, glycerin, and water, in which the amount of calcium hydroxide contained in the mixture is 5 pts.mass or more and 80 pts.mass or less based on 100 pts.mass of the total amount of glycerin and glycerol carbonate, and the content of the glycerin is 20 pts.mass or more and 80 pts.mass or less based on 100 pts.mass of the total amount of the glycerin and the glycerol carbonate.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cured product and a method for producing the cured product. [Background technology]

[0002] Natural concretions are spherical rock masses formed by localized concentration of carbonates in marine facies. Since concretions often contain well-preserved fossils, the field of paleontology has pointed out the relationship between the decomposition reactions of living organisms and the formation of concretions (see Patent Document 1 and Non-Patent Document 1). According to these documents, the fatty acids in the remains of living organisms decompose to produce bicarbonate ions (HCO3 - This bicarbonate ion is converted into carbonate ion CO3 by the change in pH at the interface between the dead organisms and seawater. 2- This carbonate ion CO3 2- and calcium ion Ca 2+ reacts to form CaCO3. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2020 / 040243 Brochure [Non-patent literature]

[0004] [Non-Patent Document 1] Scientific Reports volume 5, Article number: 14123 (2015) Summary of the Invention [Problem to be solved by the invention]

[0005] Natural concretions grow while incorporating marine sediment such as silica sand, and it has been reported that they can grow to a diameter of 14 to 37 mm in a few weeks to a few months. Natural concretions are formed when CaCO3 grows under water pressure and earth pressure in the deep sea, resulting in a dense structure in which CaCO3 fills the gaps in the silica sand. This gives natural concretions extremely high compressive strength. Thus, natural concretions are of great interest as a high-strength structural material that contributes to low carbonization.

[0006] However, when natural concretion is used to produce a hardened body, the raw materials are expensive, which increases the production cost of the hardened body. In addition, depending on the raw material, carbon dioxide emissions increase, which increases the environmental load.

[0007] Therefore, the present invention aims to provide a hardened body that utilizes natural concretion and waste materials, which is low-cost and suppresses carbon dioxide emissions, and a method for producing the same. [Means for solving the problem]

[0008] As a result of intensive research conducted by the present inventors to solve the above problems, they discovered that by using concrete sludge as a raw material in the production of a hardened body using natural concretion, a hardened body that is low cost and reduces carbon dioxide emissions can be obtained.

[0009] The present invention has been made based on the above findings, and provides a hardened body obtained by hardening a mixture of concrete sludge, cement, aggregate, glycerol carbonate, dimethyl carbonate, glycerin, and water, the amount of calcium hydroxide contained in the mixture is 5 parts by mass or more and 80 parts by mass or less per 100 parts by mass of the total amount of the glycerin and the glycerol carbonate, The present invention provides a hardened body having a glycerin content of 20 parts by mass or more and 80 parts by mass or less per 100 parts by mass of the total amount of the glycerin and the glycerol carbonate.

[0010] The present invention also relates to a powder component package including concrete sludge powder, cement, and aggregate; A kit for producing a hardened body, comprising a combination of glycerol carbonate, dimethyl carbonate, and a liquid component package containing glycerin and water, the amount of calcium hydroxide contained in the powder component package is 5 parts by mass or more and 80 parts by mass or less per 100 parts by mass of the total amount of the glycerin and the glycerol carbonate contained in the liquid component package, The kit for producing a hardened body is provided, in which the content of the glycerin contained in the liquid component package is 20 parts by mass or more and 80 parts by mass or less per 100 parts by mass of the total amount of the glycerin and the glycerol carbonate.

[0011] The present invention further provides a method for producing a hardened body by mixing concrete sludge, cement, aggregate, glycerol carbonate, dimethyl carbonate, glycerin, and water and hardening the mixture, comprising the steps of: The amount of calcium hydroxide contained in the mixture is 5 parts by mass or more and 80 parts by mass or less per 100 parts by mass of the total amount of the glycerin and the glycerol carbonate, The present invention provides a method for producing a hardened body, in which the content of the glycerin is 20 parts by mass or more and 80 parts by mass or less per 100 parts by mass of the total amount of the glycerin and the glycerol carbonate.

[0012] The present invention further provides a method for producing a hardened body, comprising the steps of: mixing powders together to produce a powder mixture; mixing liquids together to produce a liquid mixture; and mixing and hardening the powder mixture and the liquid mixture, The powder includes concrete sludge powder, cement, and aggregate, The liquid includes glycerol carbonate, dimethyl carbonate, glycerin, and water; The amount of calcium hydroxide contained in the powder mixture is 5 parts by mass or more and 80 parts by mass or less per 100 parts by mass of the total amount of the glycerin and the glycerol carbonate contained in the liquid mixture, The present invention provides a method for producing a hardened body, in which the content of the glycerin contained in the liquid mixture is 20 parts by mass or more and 80 parts by mass or less per 100 parts by mass of the total amount of the glycerin and the glycerol carbonate. Effect of the Invention

[0013] According to the present invention, there are provided a hardened body that can be produced at low cost using waste materials and that suppresses carbon dioxide emissions, and a method for producing the same. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is an X-ray diffraction diagram of the reproduced concrete sludge powder used in the examples and comparative examples. [Diagram 2] FIG. 2 is an X-ray diffraction diagram of the actual concrete sludge powder used in the examples. [Diagram 3] FIG. 3 is an X-ray diffraction diagram of the cement used in the examples. [Figure 4] FIG. 4 is an X-ray diffraction diagram of the hardened body (air-cured) obtained in Example 1. [Diagram 5] FIG. 5 is an X-ray diffraction diagram of the hardened body (cured in water) obtained in Example 1. [Figure 6] FIG. 6 is an X-ray diffraction diagram of the hardened body (air-cured) obtained in Reference Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The present invention will now be described based on its preferred embodiments. The present invention relates to a hardened body. The hardened body of the present invention is produced by mixing a powder component and a liquid component and hardening the powder component based on a hardening mechanism that applies concretion. In detail, the hardened body of the present invention is produced by hardening a mixture of concrete sludge, cement, aggregate, glycerol carbonate, dimethyl carbonate, glycerin, and water. In other words, the hardened body of the present invention is specified by its manufacturing method. The reason for this is that the hardened body of the present invention is not amenable to direct specification by the components constituting the hardened body, their contents, or physical property values ​​representative of the hardened body, and such specification is not realistic, and there are impossible circumstances that make it necessary to use such expressions.

[0016] The powder component used to produce the hardened body of the present invention is a powder mixture prepared by mixing multiple types of powders together, while the liquid component is a liquid mixture prepared by mixing multiple types of liquids together.

[0017] The powder mixture used in producing the hardened body of the present invention contains concrete sludge powder, cement, and aggregate. On the other hand, the liquid mixture used in producing the hardened body of the present invention contains 1,2-glycerol carbonate (hereinafter, when simply referred to as "glycerol carbonate", it means 1,2-glycerol carbonate), dimethyl carbonate, glycerin, and water.

[0018] In the following description, the term "concrete sludge powder" refers to concrete sludge that has been dried and turned into a powder. The term "concrete sludge" refers to concrete sludge powder in a water-containing state or concrete sludge powder itself, depending on the context.

[0019] In the present invention, the inventors believe that the hardening mechanism of the powder mixture and liquid mixture involves (i) hydrolysis of glycerol carbonate and dimethyl carbonate, (ii) a reaction (interaction) between the glycerin thus produced and calcium ions in the concrete sludge powder, and (iii) the production of calcium carbonate.

[0020] The inventors believe that the hydrolysis of glycerol carbonate and dimethyl carbonate in (i) above occurs due to the reaction of water with glycerol carbonate and dimethyl carbonate in the presence of concrete sludge, which is one of the powder components contained in the powder mixture. The reaction formulas are as shown in (I) and (II) below. This reaction produces glycerin in the system.

[0021] [ka]

[0022] The reaction of the glycerin in the above (ii) with calcium ions in the concrete sludge is carried out by reacting the glycerin produced by the above hydrolysis with calcium ions (Ca 2+ The inventors speculate that the interaction between the two compounds causes a complex formation reaction or a reaction similar to the above. The substance (complex) formed by this reaction is believed to contribute to the strength of the cured body.

[0023] From the viewpoints of (i) and (ii) above, in a mixture obtained by mixing the powder mixture and the liquid mixture, the total amount of glycerol carbonate and dimethyl carbonate per 100 parts by mass of calcium hydroxide contained in the mixture is preferably more than 100 parts by mass, more preferably 200 parts by mass or more and 1,300 parts by mass or less, and even more preferably 300 parts by mass or more and 1,000 parts by mass or less.

[0024] The amount of calcium hydroxide contained in the mixture of the powder mixture and the liquid mixture is measured in accordance with the Cement Association standard test method JCASI-01:1997 "Quantitative method for free calcium oxide". The obtained amount of free calcium oxide is converted to calcium hydroxide.

[0025] In the present invention, as described above, glycerol carbonate and dimethyl carbonate are used in combination as liquid components contained in the liquid mixture. The technical advantages of using both in combination are as follows. When glycerol carbonate is used alone and dimethyl carbonate is not used, an excessive amount of glycerin derived from glycerol carbonate may be generated. The reason for this is that in order to knead the powder mixture and the liquid mixture with good workability, it is necessary to use a relatively large amount of the liquid mixture relative to the amount of the powder mixture used. The excessive amount of glycerin remains in the hardened body during the progress of concretion and / or after the completion of concretion, and leaks onto the surface of the hardened body. The leaked glycerin is one of the factors that impair the appearance of the hardened body. In addition, the leaked glycerin is one of the factors that reduce the strength of the hardened body. Therefore, in the present invention, in order to eliminate the above-mentioned inconvenience when glycerol carbonate is used alone, dimethyl carbonate is also used in addition to glycerol carbonate to suppress the generation of an excessive amount of glycerin. Note that dimethyl carbonate generates methanol by its hydrolysis, but since methanol volatilizes faster than glycerin, methanol is less likely to be exposed to the surface of the hardened body. In this way, in the present invention, by using glycerol carbonate and dimethyl carbonate in combination, it is possible to realize kneading of the powder mixture and the liquid mixture with good workability while suppressing the production of an excessive amount of glycerin. When dimethyl carbonate was used alone without glycerol carbonate, the material appeared to harden, but it was merely a matter of the material being held together, and the compressive strength was 1N / mm 2 Not even that.

[0026] In order to make the advantage of using glycerol carbonate and dimethyl carbonate in combination more prominent, the amount of dimethyl carbonate is preferably 15 parts by mass or more and 70 parts by mass or less, more preferably 25 parts by mass or more and 65 parts by mass or less, and even more preferably 35 parts by mass or more and 60 parts by mass or less, per 100 parts by mass of the total amount of glycerol carbonate and dimethyl carbonate.

[0027] By the way, concrete sludge is the sludge that comes from the washing water used to wash mixer trucks after transporting ready-mix concrete. Concrete sludge is an industrial waste that is disposed of after being dehydrated and dried. In the present invention, concrete sludge, which has been treated as industrial waste up until now, is effectively utilized as a material, thereby reducing the environmental load by reducing carbon dioxide emissions.

[0028] Concrete sludge may be a hardened product of cement itself, or a hardened product of cement and aggregate. In either case, the chemical composition of concrete sludge differs from that of cement depending on whether or not a hydration reaction has occurred.

[0029] Since the amount of calcium contained in concrete sludge, in other words the amount of Ca(OH)2, is not large, the hardening reaction may not occur easily. Therefore, in the present invention, water is used as one of the liquid components contained in the liquid mixture, as described above. By using water, the elution of calcium components from Ca(OH)2 is promoted, and the reaction with glycerin generated by hydrolysis of glycerol carbonate is promoted. However, by using water, the hydrolysis of glycerol carbonate may progress rapidly, and the reaction between glycerin generated by hydrolysis and calcium components may also progress rapidly. These phenomena cause the problem of unintended hardening during the mixing process of the powder mixture and the liquid mixture, and the problem of interference with the subsequent molding work. In order to solve this problem, the present inventors have conducted extensive research and found that by replacing a portion of glycerol carbonate with glycerin (this glycerin is not a hydrolysis product of glycerol carbonate), i.e., by using glycerol carbonate and glycerin together as liquid components, it is possible to control the hydrolysis reaction of glycerol carbonate, and thereby the reaction between glycerin and the calcium component. The present inventors believe that the reason for this is that by replacing a portion of glycerol carbonate with glycerin, the viscosity of the liquid mixture increases, and it takes time to uniformly mix the liquid mixture with the powder mixture, which delays the reaction. The replacement of glycerol carbonate with glycerin is also significant from the standpoint of reducing carbon dioxide emissions (when glycerin derived from plant photosynthesis is used).

[0030] From the above viewpoints, the degree of substitution of glycerol carbonate with glycerin is preferably 20 parts by mass or more and 80 parts by mass or less, more preferably 25 parts by mass or more and 75 parts by mass or less, and even more preferably 30 parts by mass or more and 70 parts by mass or less, relative to 100 parts by mass of the total amount of glycerin (G) and glycerol carbonate (GC). In this specification, this value is also referred to as the "GC substitution rate". The GC substitution rate (%) is defined as G / (GC+G)×100.

[0031] As a result of investigation, the inventors have confirmed that the properties of glycerin blended for the purpose of partially replacing glycerol carbonate are different from those of glycerin produced by hydrolysis of glycerol carbonate, and that the latter contributes more to the hardened body.

[0032] As described above, in the present invention, the reaction between calcium components derived from concrete sludge and glycerin is utilized. From this viewpoint, the amount of glycerol carbonate and glycerin used is related to the amount of calcium components derived from concrete sludge. From the viewpoint of successfully progressing the hardening reaction, in the mixture obtained by mixing the powder mixture and the liquid mixture, the amount of calcium hydroxide (Ca(OH)2) contained in the mixture is preferably 5 parts by mass or more and 80 parts by mass or less, more preferably 5 parts by mass or more and 75 parts by mass or less, and even more preferably 8 parts by mass or more and 70 parts by mass or less, relative to 100 parts by mass of the total amount of glycerin (G) and glycerol carbonate (GC). In this specification, this value is also referred to as the "Ca content." The Ca content (%) is defined as (Ca(OH)2) / (GC+G)×100. The amount of calcium hydroxide used to calculate the Ca content is determined by the method described above.

[0033] The powder mixture contains cement as well as concrete sludge powder as a material containing calcium components. Cement produces calcium hydroxide as a by-product during the hydration reaction. However, the hydration reaction of cement proceeds gradually and is slower than the hardening speed when producing the hardened body of the present invention (usually hardening in 10 to 30 minutes from the start of mixing), so it is considered that the calcium hydroxide used to calculate the Ca content is mainly derived from the concrete sludge powder.

[0034] In addition, the inventors conducted experiments using organic compounds such as 1,3-propanediol, 1,4-butanediol, triethanolamine, and 1,1,1-tris(hydroxymethyl)propane, which have multiple polar functional groups similar to glycerin, instead of glycerol carbonate, and found that either no hardening occurred or, although hardening occurred, the hardened body did not have sufficient strength. Based on this fact, the advantage of using glycerol carbonate in the present invention is clear.

[0035] The calcium carbonate (iii) is considered to be generated by the calcium component contained in the concrete sludge absorbing carbon dioxide. The source of carbon dioxide is considered to be the carbon dioxide generated by the hydrolysis of the glycerol carbonate and dimethyl carbonate (i) while concretion is in progress. On the other hand, after the completion of concretion, it is considered that carbon dioxide in the air becomes the source of calcium carbonate. In the present invention, it is considered that, as in natural concretion, the generated calcium carbonate involves the powder components present around it, forming a hardened body that is solidified to a high strength. The present inventors have confirmed that the hardened body of the present invention generates more calcium carbonate when it is left in water than when it is left in the air. The reason for this is considered to be that the carbon dioxide dissolved in the water acts on the hardened body. When the hardened body of the present invention is left in the air, its strength initially decreases, but then tends to increase. The reason for the decrease in strength is believed to be that the growth of calcium carbonate causes the hardened body to expand, resulting in defects inside the body. The reason for the increase in strength is believed to be that the growth of calcium carbonate continues, filling in the defects.

[0036] In this way, concrete sludge is used to produce calcium carbonate, which is the main component of concretion, and is further used to hydrolyze glycerol carbonate and dimethyl carbonate and form complexes with glycerin. Furthermore, when hardening experiments were carried out using magnesium hydroxide, sodium hydroxide and potassium hydroxide instead of concrete sludge, which are substances that, like concrete sludge, give off cations in water and become alkaline, the inventors confirmed that the strength of the hardened body was the highest when concrete sludge was used. Based on this fact, the superiority of using concrete sludge in the present invention is clear.

[0037] The average particle size of the concrete sludge powder is preferably 3 μm or more and 400 μm or less from the viewpoint of improving the strength of the hardened body. From this viewpoint, the average particle size of the concrete sludge powder is more preferably 4 μm or more and 200 μm or less, and even more preferably 5 μm or more and 100 μm or less.

[0038] The average particle size of the concrete sludge powder is measured using a laser diffraction particle size distribution measuring device (e.g., SALD-2200 manufactured by Shimadzu Corporation). In this specification, the term "average particle size" refers to the volume-weighted arithmetic mean particle size measured by this method.

[0039] In the production of the hardened body of the present invention, in addition to the above-mentioned concrete sludge powder, cement is also used as a powder component contained in the powder mixture. As a result of the inventor's investigation, it was found that cement contributes to suppressing the decrease in strength of the hardened body of the present invention when it is left in water.

[0040] In order to make the above-mentioned advantages arising from blending cement with the powder components contained in the powder mixture more pronounced, the amount of cement added is preferably 10 parts by mass or more and 30 parts by mass or less, more preferably 12 parts by mass or more and 25 parts by mass or less, and even more preferably 14 parts by mass or more and 20 parts by mass or less, per 100 parts by mass of the powder mixture. It is believed that the strong basicity of the cement promotes the hydrolysis of glycerol carbonate, and therefore it is possible to adjust the hardening rate by controlling the amount of cement added.

[0041] There is no particular limitation on the type of cement that can be used in the present invention. Examples of cement that can be used include portland cement, alumina cement, and blast furnace cement. Examples of Portland cement include ordinary Portland cement, high-early-strength Portland cement, extra-high-early-strength Portland cement, low-heat Portland cement, moderate-heat Portland cement, and sulfate-resistant Portland cement. These cements may be used alone or in combination of two or more. In particular, it is preferable to use Portland cement or alumina cement from the viewpoint of production costs. In addition, the Blaine specific surface area is one of the typical indicators of the characteristics of cement. There is no particular restriction on the Blaine specific surface area of ​​the cement used in the present invention, and a typical Blaine specific surface area of ​​cement used in the production of concrete or mortar can be used.

[0042] The cement preferably has an average particle size of 5 μm or more and 20 μm or less, from the viewpoint of improving the strength of the hardened body, particularly the strength when the hardened body is placed in water. From this viewpoint, the average particle size of the cement is more preferably 10 μm or more and 18 μm or less, and even more preferably 12 μm or more and 16 μm or less.

[0043] As described above, the underwater stability of the hardened body of the present invention is improved by using cement as one of the powder components contained in the powder mixture, and the inventors' investigations have revealed that the underwater stability of the hardened body of the present invention is further improved by further including silica fume in the powder mixture. The applicant speculates that the reason why the underwater stability of the hardened body of the present invention is further improved by using silica fume is as follows. The first reason is that a pozzolanic reaction occurs between cement and silica fume, producing a pozzolanic reaction product. The second reason is the microfiller effect of silica fume. The microfiller effect in cement is the effect of improving the dispersibility and filling property of the material by fine silica fume filling the gaps between cement particles. That is, in the present invention, when a powder mixture and a liquid mixture are mixed and hardened, it is considered that the silica fume penetrates not only into the cement but also into the gaps between other powders (for example, aggregate, which will be described later), improving the filling property and dispersibility. It is considered that the improvement in the filling property and dispersibility in the hardened body contributes to improving the strength of the hardened body.

[0044] In conventional structures such as concrete and mortar, micro defects occur and grow, causing destruction. In contrast, in the present invention, even if micro defects occur in the hardened body, the addition of silica fume improves the dispersibility of the powder components, and the above-mentioned complex is formed and calcium carbonate grows at the location where the defect occurs. The inventors presume that the defect is repaired and the strength of the hardened body is maintained or improved.

[0045] The type of silica fume used in the present invention is not particularly limited. Silica fume is a by-product obtained by collecting dust in exhaust gas generated during the production of metal silicon, ferrosilicon, electrofused zirconia, etc. The main component of silica fume is amorphous SiO2 that dissolves in an alkaline solution, and its content is generally about 90 to 98 mass%. The average particle size and fineness of silica fume are not particularly limited, but are preferably within the ranges specified in JIS A 6207, for example.

[0046] In order to make the above-mentioned advantages arising from the powder mixture containing silica fume more pronounced, the amount of silica fume used, in relation to the amount of concrete sludge powder used, is preferably 200 parts by mass or more and 1,500 parts by mass or less, more preferably 300 parts by mass or more and 1,300 parts by mass or less, and even more preferably 400 parts by mass or more and 1,200 parts by mass or less, per 100 parts by mass of silica fume. From a similar viewpoint, the amount of silica fume used, in relation to the amount of cement used, is preferably 100 parts by mass or more and 700 parts by mass or less, more preferably 150 parts by mass or more and 600 parts by mass or less, and even more preferably 200 parts by mass or more and 500 parts by mass or less, per 100 parts by mass of silica fume.

[0047] In the present invention, the powder mixture further contains aggregate. The aggregate mainly contributes to improving the aerial stability of the hardened body of the present invention. As the aggregate, the same aggregate as that contained in concrete or mortar can be used without any particular limitation. For example, fine aggregate and coarse aggregate can be used. Furthermore, calcium carbonate can be used. In particular, when limestone is used as the calcium carbonate, a hardened body having an excellent appearance similar to natural concretion can be obtained.

[0048] Examples of the fine aggregate that can be used include river sand, land sand, mountain sand, sea sand, crushed sand, silica sand, limestone aggregate, blast furnace slag fine aggregate, copper slag fine aggregate, electric furnace oxidized slag fine aggregate, etc. These fine aggregates can be used alone or in combination of two or more kinds.

[0049] As the coarse aggregate, for example, gravel, crushed stone, limestone aggregate, blast furnace slag coarse aggregate, electric furnace oxidizing slag coarse aggregate, etc. can be used.

[0050] In particular, it is preferable to use calcium carbonate or silica sand as the aggregate from the viewpoint of further improving the strength of the hardened body.

[0051] In any of the above cases, the average particle size of the aggregate is preferably 50 μm or more and 1000 μm or less from the viewpoint of improving the strength of the hardened body. To make this advantage more prominent, the average particle size of the aggregate is more preferably 60 μm or more and 500 μm or less, and even more preferably 75 μm or more and 300 μm or less. When the powder mixture contains the above-mentioned silica fume, it is preferable that the average particle size of the aggregate is larger than the average particle size of the silica fume in order to fully exert the microfiller effect of the silica fume.

[0052] The average particle size and median size of aggregates can be measured, for example, by sieving. For example, sieves with mesh sizes of 10 mm, 14 mm, 20 mm, 28 mm, 35 mm, 48 mm, 65 mm, 100 mm, 150 mm, 200 mm, and 270 mm can be used in accordance with JIS A1102-2006 "Sieving Test Method for Aggregates." Hereinafter, the "average particle size" and "median size" of aggregates refer to the average particle size measured by this method.

[0053] When a combination of two or more aggregates having different particle sizes is used as the aggregate, it is preferable that the aggregate contains a first aggregate having an average particle size of 25 μm or more and smaller than 250 μm and a second aggregate having an average particle size of 250 μm or more and smaller than 1000 μm from the viewpoint of further improving the strength of the hardened body. It is more preferable that the aggregate contains a first aggregate having an average particle size of 50 μm or more and smaller than 200 μm and a second aggregate having an average particle size of 250 μm or more and smaller than 500 μm. When a combination of two or more aggregates having different particle sizes is used as the aggregate, it is preferable that the aggregate contains a first aggregate having a median diameter (D50) of 25 μm or more and smaller than 250 μm and a second aggregate having a median diameter (D50) of 250 μm or more and 1000 μm or less, from the viewpoint of further improving the strength of the hardened body. It is more preferable that the aggregate contains a first aggregate having a median diameter of 50 μm or more and smaller than 200 μm and a second aggregate having a median diameter of 250 μm or more and 500 μm or less. The first aggregate and the second aggregate may be the same or different in type, and it is particularly preferred that both the first aggregate and the second aggregate are silica sand. The mixing ratio of the first aggregate and the second aggregate can be set widely as long as the average particle size of the mixed aggregate after mixing them is within the above-mentioned range. From the viewpoint of further improving the strength of the hardened body, the first aggregate is preferably contained in an amount of 50 parts by mass or more, more preferably 60 parts by mass or more and 95 parts by mass or less, and even more preferably 70 parts by mass or more and 90 parts by mass or less, per 100 parts by mass of the first aggregate and the second aggregate combined.

[0054] To manufacture the hardened body of the present invention, concrete sludge, cement, aggregate, glycerol carbonate, dimethyl carbonate, glycerin, and water are mixed and hardened. For this purpose, a powder component package containing concrete sludge powder, cement, and aggregate, and a liquid component package containing glycerol carbonate, dimethyl carbonate, glycerin, and water are prepared, and a hardened body manufacturing kit having a combination of these packages can be used. The mixing ratio of each powder contained in the powder component package in this kit is as described above. Similarly, the mixing ratio of each liquid contained in the liquid component package in the kit is also as described above. Specifically, the amount of calcium hydroxide contained in the powder component package is preferably 5 parts by mass or more and 80 parts by mass or less per 100 parts by mass of the total amount of glycerin and glycerol carbonate contained in the liquid component package. The content of glycerin in the liquid component package is preferably 20 parts by mass or more and 80 parts by mass or less per 100 parts by mass of the total amount of glycerin and glycerol carbonate.

[0055] If necessary, ingredients other than the various ingredients mentioned above can be added to the powder ingredient package and / or the liquid ingredient package. For example, a water reducing agent can be added to the powder ingredient package, such as nitrohumates, lignin sulfonates, citric acid, polycarboxylic acids, naphthalene, and the like. On the other hand, carbonate esters other than the above-mentioned glycerol carbonate and dimethyl carbonate can also be added to the liquid component package, such as ethylene carbonate, propylene carbonate, 1,3-dioxan-2-one, 4-fluoro-1,3-dioxolan-2-one, 4-chloro-1,3-dioxolan-2-one, 4-vinyl-1,3-dioxolan-2-one, 4-methoxy-1,3-dioxolan-2-one, and vinylene carbonate.

[0056] In the kit, it is preferable to use 10 parts by mass or more and 40 parts by mass or less of the liquid component package per 100 parts by mass of the powder component package, from the viewpoint of being able to mix the two packages uniformly and with good workability, and it is even more preferable to use 15 parts by mass or more and 30 parts by mass or less of the liquid component package.

[0057] For mixing the two packages, various conventionally known mixers can be used without any particular restrictions. Examples of the mixer that can be used include a vacuum kneader, a planetary centrifugal mixer, and a paddle mixer. Among these mixers, it is preferable to use a paddle mixer, since it is easy to obtain a cured product with high strength. When a paddle mixer is used as the mixer, a leaf-shaped or hook-shaped stirrer can be used. Among these stirrers, the use of a hook-shaped stirrer is preferred because it applies high shear force to the mixture in both packages, allowing the components to be mixed thoroughly and uniformly, making it easier to obtain a hardened product with high strength.

[0058] In mixing both packages, the better the dispersibility of each component, the higher the compressive strength of the resulting hardened product tends to be. On the other hand, hardening may progress as each component is mixed. Considering these factors, a kneader with a high shear force is preferable, which can improve the dispersibility of each component even after hardening has started.

[0059] In contrast to the setting of cement, the setting of the mixture of both packages occurs immediately. For example, the set life of the present invention is approximately 15 minutes, whereas the set life of concrete is approximately one day. The set of both packages may be heated to control the setting time.

[0060] Both packages can be mixed while cooling. This also suppresses hardening during mixing and increases the pot life. The cooling temperature is not limited, but may be, for example, -50°C or higher, preferably -30°C or higher, more preferably -20°C or higher, even more preferably -10°C or higher, even more preferably 0°C or higher, and most preferably 5°C or higher. The cooling temperature can be, for example, 25°C or lower, 20°C or lower, or 10°C or lower.

[0061] When both packages are sufficiently mixed, the mixture is filled into a mold to obtain the desired hardened body. In this case, the hardened body may be dried as necessary. The temperature conditions for drying are not limited, but may be, for example, 60°C or higher, 80°C or higher, or 100°C or higher. The drying time may be, for example, 1 hour or more, 10 hours or more, 24 hours or more, or 72 hours or more. Drying may be performed under reduced pressure. Depending on the formulation, glycerin may seep out from the hardened body, but the drying process has the advantage of being able to remove it.

[0062] The hardened body can be removed from the formwork after, for example, one to three hours at room temperature. The hardened body thus obtained can be used, for example, as secondary products for river bank protection, called environmental blocks or environmental protection blocks. Secondary products for river bank protection include products for land and products for underwater. Products for land function as greening blocks for rivers and have a structure that prevents soil from flowing out due to repeated increases and decreases in the river water level. Products for underwater use are structured so that they can be filled with boulders or pebbles. The hardened product of the present invention can also be used as a waterproofing material in emergency construction works, which are preferably used in the case of overflow caused by river flooding, burst water supply and sewerage pipes, etc. The hardened material of the present invention can also be used as a solidification material for soil improvement, etc. In this case, it is preferable because the hardened material can be generated in the ground by the growth of calcium carbonate, similar to natural concretions. The hardened product of the present invention can also be used for interlocking blocks, which have traditionally required steam curing for their production, but the present invention is advantageous in that steam curing is not required. Furthermore, the hardened product of the present invention can be used to repair damaged areas on the surface of concrete structures or mortar structures. Specifically, the mixture of the two packages can be applied to damaged areas such as cracks on the surface of the structure to fill and repair the area. In this case, the damaged area is self-repaired by the growth of calcium carbonate, as in the case of natural concretions.

[0063] Although the present invention has been described based on the preferred embodiment, the present invention is not limited to the above embodiment.

[0064] The present invention will be described in more detail below with reference to examples. However, the scope of the present invention is not limited to such examples. Unless otherwise specified, "%" means "% by mass".

[0065] In the examples, comparative examples and reference examples, the following powder components and liquid components were used. - Reproduced concrete sludge powder (normal Portland cement (same brand as normal Portland cement below) was prepared into a slurry with a W / C (water-cement ratio) of 300%, stirred continuously at 23°C for 72 hours, dried at 40°C for 72 hours, and then crushed in a test ball mill) Actual concrete sludge powder (sludge generated after transporting ready-mix concrete manufactured by Hagimori Kosan Co., Ltd., dried at 40°C for 24 hours, then crushed in a test ball mill for 1 hour) Cement (ordinary Portland cement, manufactured by UBE Mitsubishi Cement Corporation, density 3.16g / cm 3 , average particle size 15μm) Silica fume (SKW, density 3.16g / cm 3 , average particle size 2μm) Aggregate 1 (silica sand, N70, made by Hyōya, density 2.60g / cm 3, average particle size 155μm, median diameter 158μm) Aggregate 2 (silica sand, N60, made by Hyōya, density 2.60g / cm 3 , average particle size 249μm, median diameter 247μm) Aggregate 3 (silica sand, No. 6, made by Ube Sand, density 2.60 g / cm 3 , average particle size 308μm, median diameter 302μm) Hydrated lime (Calbrid, manufactured by Ube Materials, density 2.21 g / cm 3 , average particle size 6.5μm) Glycerol carbonate (UBE Corporation) Dimethyl carbonate (UBE Corporation) Glycerin (manufactured by Fujifilm Wako Co., Ltd.) The X-ray diffraction patterns of the reproduced concrete sludge powder, the actual concrete sludge powder, and cement are shown in Figures 1 to 3.

[0066] [Examples 1 to 6 and Comparative Examples 1 and 2] (1) Preparation of powder component packages The replica concrete sludge powder, cement, aggregate and silica fume were mixed in the proportions (g) shown in Table 1 to prepare a powder component package.

[0067] (2) Preparation of liquid component packages A liquid ingredient package was prepared by mixing glycerol carbonate (GC), dimethyl carbonate (DMC), glycerin (G) and water in the proportions (g) shown in Table 1.

[0068] (3) Mixing both packages The powder and liquid component packages were placed into a mortar mixer equipped with a hook-type agitator and mixed at 23°C and 70% RH until hardening was observed.

[0069] (4) Pouring into formwork The mixture of both packages was poured into a mold measuring 10 mm in length, 60 mm in width, and 10 mm in depth, and then hardened by keeping it at 23°C and 70% RH for 3 hours. In this way, a hardened body was obtained.

[0070] [Examples 7 to 9] Actual concrete sludge powder was used as the concrete sludge powder. Also, a powder component package and a liquid component package having the compositions shown in Table 1 were used. A hardened body was produced in the same manner as in Example 1 except for the above.

[0071] [Reference example 1] In this reference example, the powder component package does not contain concrete sludge powder, but contains hydrated lime instead, and the liquid component package does not contain glycerin or water. A hardened body was produced in the same manner as in Example 1, except that a powder component package and a liquid component package having the compositions shown in Table 1 were used.

[0072] 〔evaluation〕 The cured products obtained in the Examples, Comparative Examples, and Reference Examples were evaluated for moldability during production. Products with a pot life of more than 30 minutes were rated as moldable, and products with a pot life of 30 minutes or less were rated as not moldable. The pot life refers to the time from mixing the two packages to the start of curing. Furthermore, X-ray diffraction measurements were performed on the hardened bodies (air-cured and water-cured) obtained in Example 1. The results are shown in Figures 4 and 5. Furthermore, X-ray diffraction measurements were performed on the hardened bodies (air-cured) obtained in Reference Example 1. The results are shown in Figure 6.

[0073] [Table 1]

[0074] As is clear from the results shown in Table 1, when the GC substitution rate is increased in the order of Comparative Example 1, Comparative Example 2, Example 1, Example 2, and Example 3, it is found that a cured body can be molded when the GC substitution rate is in the range of 30% to 70%. It can be seen that even in Examples 4 to 6 in which the Ca content was different from that in Examples 1 to 3, it was possible to mold a hardened body when the GC substitution rate was in the range of 30% to 70%. As is clear from a comparison of Figures 4 and 5 with Figure 6, the hardened body obtained in Example 1 and the hardened body obtained in Reference Example 1, which used a liquid component package that did not contain glycerin or water, have different chemical compositions. The hardened body obtained in Reference Example 1 can be molded into a hardened body as in the other Examples, but since hydrated lime is used instead of concrete sludge powder as the raw material, it does not meet the objective of the present invention, which is to make effective use of waste materials.

Claims

1. A hardened body obtained by hardening a mixture of concrete sludge, cement, aggregate, glycerol carbonate, dimethyl carbonate, glycerin, and water, the amount of calcium hydroxide contained in the mixture is 5 parts by mass or more and 80 parts by mass or less per 100 parts by mass of the total amount of the glycerin and the glycerol carbonate, A hardened body, wherein the content of the glycerin is 20 parts by mass or more and 80 parts by mass or less per 100 parts by mass of the total amount of the glycerin and the glycerol carbonate.

2. The hardened body according to claim 1 , wherein the cement is Portland cement or alumina cement.

3. The hardened body according to claim 1, which is a hardened body obtained by hardening a mixture of the concrete sludge, the cement, the aggregate, the glycerol carbonate, the dimethyl carbonate, the glycerin, the water, and silica fume.

4. The hardened body according to claim 1 , which is used as a secondary product for river bank protection, a water-stopping material, or a ground improvement material.

5. a powder component package including concrete sludge powder, cement, and aggregate; A kit for producing a hardened body, comprising a combination of glycerol carbonate, dimethyl carbonate, and a liquid component package containing glycerin and water, the amount of calcium hydroxide contained in the powder component package is 5 parts by mass or more and 80 parts by mass or less per 100 parts by mass of the total amount of the glycerin and the glycerol carbonate contained in the liquid component package, A kit for producing a hardened body, wherein the content of the glycerin contained in the liquid component package is 20 parts by mass or more and 80 parts by mass or less per 100 parts by mass of the total amount of the glycerin and the glycerol carbonate.

6. A method for producing a hardened body by mixing concrete sludge, cement, aggregate, glycerol carbonate, dimethyl carbonate, glycerin, and water and hardening the mixture, comprising the steps of: The amount of calcium hydroxide contained in the mixture is 5 parts by mass or more and 80 parts by mass or less per 100 parts by mass of the total amount of the glycerin and the glycerol carbonate, The method for producing a hardened body, wherein the content of the glycerin is 20 parts by mass or more and 80 parts by mass or less per 100 parts by mass of the total amount of the glycerin and the glycerol carbonate.

7. A method for producing a hardened body, comprising the steps of: mixing powders together to produce a powder mixture; mixing liquids together to produce a liquid mixture; and mixing and hardening the powder mixture and the liquid mixture, The powder includes concrete sludge powder, cement, and aggregate, The liquid includes glycerol carbonate, dimethyl carbonate, glycerin, and water; The amount of calcium hydroxide contained in the powder mixture is 5 parts by mass or more and 80 parts by mass or less per 100 parts by mass of the total amount of the glycerin and the glycerol carbonate contained in the liquid mixture, A method for producing a hardened body, wherein the content of the glycerin contained in the liquid mixture is 20 parts by mass or more and 80 parts by mass or less per 100 parts by mass of the total amount of the glycerin and the glycerol carbonate.

8. The method according to claim 6, further comprising mixing silica fume.

9. The method of claim 7 , wherein the powder mixture further comprises silica fume.

10. The method according to claim 6 or 7, wherein the cement is Portland cement or alumina cement.

Citation Information

Patent Citations

  • Cement composition

    JP1999029349A

  • Method for desulfurizing tail gas in cement production

    JP2009234859A

  • Method for producing glycerin carbonate

    JP2010202624A

  • Hydraulic composition, method of producing hydraulic composition, molding, hardened material, and method of producing hardened material

    JP2022040900A

  • Curable composition and cured body

    JP2022144016A

Cited By

  • Method for producing powder for concrete and composition for concrete

    JP7762828B1