Producing method of carbon-based product

By configuring a heating furnace with specific resistance zones, the method integrates firing and graphitization steps, addressing energy inefficiencies and lead times in carbon-based product manufacturing, enhancing operational efficiency.

JP2024139057APending Publication Date: 2024-10-09IBIDEN CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023049842
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

The high energy consumption and lengthy lead times associated with the graphitization process of carbon-based products, particularly graphite materials, are hindered by the need for large amounts of energy to sinter and dispose of packed powder, limiting operational efficiency.

Method used

A method involving a heating furnace with specific resistance configurations, where a carbonaceous block is positioned between electrodes, surrounded by regions of differing resistance values, allowing for gradual heating and combining firing and graphitization steps into one process, reducing energy loss and shortening manufacturing time.

Benefits of technology

This approach enables efficient heating and graphitization without the need for additional powder refilling, thus reducing energy consumption and shortening the overall manufacturing process duration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139057000001_ABST
    Figure 2024139057000001_ABST
Patent Text Reader

Abstract

To provide a producing method of a carbon-based product, which can contribute not only to graphitization (heating) using an Acheson furnace but also to shortening of a lead time and reduction of thermal energy loss in the whole production process.SOLUTION: A producing method of a carbon-based product comprises a heating step of: preparing a heating furnace which has original blocks disposed between a pair of electrodes, a stuffing powder region where stuffing powder surrounding the original block is placed, and a heat insulating layer surrounding the stuffing powder region; and applying electrical current to the electrodes to heat the original block. The original block is composed of carbonaceous particles and a binder formed of a carbon precursor for binding the carbonaceous particles to each other. The stuffing powder region is composed of a first region adjacent to the original block in an energization direction in which the electrical current is applied to the electrodes and a second region surrounding the original block and the first region along the axis in the energization direction. In the initial stage of the heating step, a resistivity value ρ1 of the original block and a resistivity value ρ2 of the stuffing powder region satisfy ρ1>ρ2, therefore, a calorific value per volume of the second region is larger than that of the first region.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a carbon-based product. [Background technology]

[0002] Carbon products, including graphite materials, require high-temperature heat treatment during the manufacturing process. Graphite materials require a large amount of energy to be produced by sintering a carbon precursor compact and then graphitizing it at around 3000°C, making it necessary to reduce costs and shorten lead times. In particular, in the graphitization process, a large amount of input power is required to heat the pack material, and a large amount of pack material needs to be removed and disposed of after the high-temperature treatment, which is an obstacle to improving operability through continuous operation.

[0003] Patent Document 1 describes a graphite block manufacturing method capable of reducing the cost and shortening the lead time of the graphitization step by eliminating the filling of pack material which causes such undesirable phenomena, in which an original block formed containing at least a carbon material aggregate and a binder is made electrically conductive and held between electrodes, and the original block is electrically heated in an atmosphere having less oxygen than the air and in the absence of pack material around the original block and the electrodes to perform a graphitization treatment, thereby forming a graphite block. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2003-292375 A Summary of the Invention [Problem to be solved by the invention]

[0005] Graphite blocks are manufactured by kneading coke as an aggregate and pitch as a binder, then crushing the mixture appropriately, and going through the processes of molding, firing, and graphitization. The invention described in Patent Document 1 is an invention related to reducing costs and shortening lead times only in the graphitization process, and does not take into consideration overall cost reductions and lead times, including processes before firing.

[0006] The present invention aims to provide a method for producing carbon-based products that not only involves graphitization (heating) using an Acheson furnace, but also contributes to shortening lead times and reducing thermal energy loss throughout the entire manufacturing process. [Means for solving the problem]

[0007] In order to solve the above problems, the method for producing a carbon-based product of the present invention is as follows.

[0008] (1) preparing a heating furnace having an original block disposed between a pair of electrodes, a pack material region surrounding the original block and in which a pack material is disposed, and a heat insulating layer further surrounding the pack material region; A method for producing a carbon-based product, comprising a heating step of passing an electric current through the electrodes to heat the original block, The original block includes carbonaceous particles and a binder made of a carbon precursor that binds the carbonaceous particles together, The pack material area comprises: a first region adjacent to the original block in a current flow direction, which is a direction in which a current is passed through the electrode; a second region surrounding the original block and the first region along the axis of the current flow direction; It consists of: A method for producing a carbon-based product, characterized in that, in an initial stage of the heating step, ρ1>ρ2, and the second region has a greater amount of heat per volume than the first region. ρ1: Resistivity of the original block ρ2: Specific resistance of the packing material area

[0009] The method for producing a carbon-based product of the present invention preferably has the following aspects.

[0010] (2) During the heating process of the original block, ρ1<ρ2 holds, and the amount of heat generated per unit volume in the first region is greater than that in the second region.

[0011] (3) The pore size at which the cumulative pore volume of the carbon-based product, as measured by mercury intrusion porosimetry, is 50 to 500 μm.

[0012] (4) In the original block, the carbonaceous particles and the binder form secondary particles, and the average particle size of the secondary particles is 50 to 1000 μm.

[0013] (5) The original block is a rectangular parallelepiped and is placed with its longest direction facing the current flow direction.

[0014] (6) The method for producing the carbon-based product described above comprises the steps of: a kneading step of kneading the carbonaceous particles and the binder to obtain a carbon precursor; a molding step of molding the carbon precursor to obtain the original block; and a heating step of heating the original block. Effect of the Invention

[0015] According to the method for producing a carbon-based product of the present invention, in the initial stage of the heating process, when ρ1>ρ2, the amount of heat generated per volume in the second region is greater than that in the first region, and the original block can be heated slowly from the second region. In addition, as the raw block is gradually fired, the electrical conductivity of the raw block increases due to carbonization, and the block can be moved to a higher temperature heating process (graphitization process) in the same way as in a normal Acheson furnace. In other words, the firing process and graphitization process can be carried out in a single process. This eliminates the need for the process of cooling the original block after sintering and the reheating process during graphitization, reducing energy loss. In addition, the conventional sintering and graphitization processes can be carried out in a single process, eliminating the need for repacking the packing powder. This makes it possible to shorten the lead time for the entire manufacturing process. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a plan view of the inside of an Acheson furnace used in a method for producing a carbon-based product according to a first embodiment of the present invention. [Diagram 2] FIG. 2 is an enlarged view of one repeat unit around the original block of FIG. [Diagram 3] FIG. 3(a) is an explanatory diagram showing the current flow in the initial stage of the heating process, and FIG. 3(b) is an explanatory diagram showing the current flow in the final stage of the heating process. [Figure 4] 4(a) is an oblique view of the original block of FIG. 2 and the area around the original block, FIG. 4(b) is a cross-sectional view taken along the direction of current flow, and FIG. 4(c) is a cross-sectional view taken from the side of the current flow. [Diagram 5] FIG. 5 is a circuit diagram showing an equivalent circuit around the original block in FIG. [Figure 6] FIG. 6(a) is a flow diagram showing steps of a method for producing a carbon-based product according to the first embodiment of the present invention, and FIG. 6(b) is a flow diagram showing steps of a conventional method for producing a carbon-based product. [Figure 7] Figure 7(a) is a plan view of the inside of an Acheson furnace used in a method for producing a carbon-based product in embodiment 2 of the present invention, Figure 7(b) is a plan view of the inside of an Acheson furnace used in a method for producing a carbon-based product in embodiment 3 of the present invention, and Figure 7(c) is a plan view of the inside of an Acheson furnace used in a method for producing a carbon-based product in embodiment 4 of the present invention. [Figure 8] FIG. 8 is a cross-sectional view of the structure of the original block in accordance with the first embodiment of the present invention. [Figure 9] FIG. 9 is a scatter diagram showing the relationship between the heating temperature and the specific resistance of the original block in the first embodiment of the present invention. [Figure 10] FIG. 10 is a perspective view of the inside of an Acheson furnace used in the manufacturing method of a carbon-based product according to the embodiment. [Figure 11] FIG. 11 is a photograph showing the appearance of the carbon-based product obtained in the example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] In the present invention, the carbon-based product is not particularly limited as long as it is a product mainly made of carbon. For example, it includes graphite products that have been subjected to a graphitization process in which the product is heated at about 3000°C, carbonaceous products that have been subjected to a sintering process in which the product is heated at about 1000°C and carbonized, and various carbon-based products that have been heat-treated in the intermediate temperature range.

[0018] In the present invention, the carbonaceous particles constituting the original block are not particularly limited. In addition to resin-based carbonaceous particles that become glassy carbon, coke-based carbonaceous particles that are easily graphitized, graphite carbonaceous particles, etc. can be used. As the coke-based carbonaceous particles, needle coke, petroleum-based coke, and coal-based coke can be used. In the present invention, any organic material that is liquid or softens when heated can be used as a binder made of a carbon precursor. Pitch, resin, etc. can be used as the binder. The original block is obtained by adjusting the raw materials by binding the carbonaceous particles with a binder and molding them. In the original block, the carbonaceous particles and the binder form secondary particles, and the average particle diameter of the secondary particles is preferably 50 to 1000 μm. If the average particle diameter of the secondary particles is 50 μm or more, the pyrolysis gas generated in the heating process can be quickly discharged outside the original block, and swelling and cracking can be prevented. If the average particle diameter of the secondary particles is 1000 μm or less, the connection points between the secondary particles can be sufficiently secured, so that the strength is high and cracking is unlikely to occur during the heating process. The average particle size of the secondary particles can be measured using a laser diffraction particle size distribution measuring device.

[0019] When the original block is heated by the heating step of the present invention, the organic components condense and low molecular weight hydrocarbons, moisture, sulfur-containing components, and nitrogen-containing components are eliminated to give a carbonaceous or graphitic product. Hereinafter, the present invention will be described based on an embodiment.

[0020] First Embodiment The first embodiment of the present invention comprises a kneading step, a molding step, and a heating step. The process flow is shown in Fig. 6(a). In the conventional method for producing a carbon-based product (Fig. 6(b)), a carbon-based product is obtained through the kneading step, molding step, firing step, and graphitization step, whereas in the present embodiment, the firing step and graphitization step can be carried out together as a heating step.

[0021] <Kneading process> The raw block can be obtained by molding the raw material obtained by kneading coal-based coke powder and coal-based pitch. Since pitch is solid at room temperature, it can be heated to melt it and kneaded with coke powder using a kneader.

[0022] The average particle size of the coke powder used is not particularly limited, but is, for example, 5 to 500 μm. The type of coke powder used is not particularly limited, but for example, petroleum coke, coal coke, needle coke, etc. can be used.

[0023] The softening point of the pitch used is not particularly limited. For example, pitch with a softening point of 50 to 200°C can be used. If the softening point of the pitch is 200°C or less, the temperature required for kneading is low, and the rate of polycondensation reaction caused by heating during kneading can be slowed down, and kneading can be stabilized. Also, if the softening point is 50°C or more, the volatile components are small, so the carbonization yield can be increased, and sufficient binder components remain after the heating process, making it possible to obtain a carbon-based product with high strength.

[0024] The temperature during kneading is not particularly limited, but is preferably higher than the softening point of pitch in order to melt the pitch as a binder. For example, 100° C. or higher is preferable, and 150° C. or higher is more preferable. The upper limit of the temperature during kneading is not particularly limited, but is preferably 350° C. or lower, and more preferably 300° C. or lower, in order to prevent excessive polycondensation of the pitch.

[0025] In the kneading process, the kneader kneads the coke powder and pitch, creating a granulation effect. As the kneading process progresses, the volatile matter in the pitch is removed and the polycondensation reaction progresses, increasing the binding force and coarsening the particles (Figure 8). FIG. 8 shows a schematic diagram of a binder 70 and carbonaceous particles 80. As shown in FIG. The particles granulated in the kneading step may be molded as they are in the subsequent molding step as a raw material, or may be crushed appropriately to adjust the particle size and then molded as a raw material.

[0026] <Forming process> In the molding step, the raw material obtained in the kneading step is molded to obtain a base block. The molding method is not particularly limited, but can be performed by methods such as embossing, CIP molding, and extrusion molding.

[0027] The molding process may be cold molding at room temperature, or hot molding in which the raw materials are heated and molded. The temperature of the hot molding is not particularly limited, but is preferably higher than 70°C. In addition, the temperature is preferably 300°C or lower, more preferably 250°C or lower, so as not to excessively promote polycondensation of the raw materials. By performing hot molding, the adhesiveness of the raw materials can be increased, and molding can be performed at a low pressure.

[0028] <Heating process> In the heating step of the present embodiment, the original block obtained in the molding step can be heated by being placed in a heating furnace and energized. The heating temperature is not particularly limited, but can be appropriately adjusted depending on the application of the carbon-based product. In the heating step of the present embodiment, prior to the heating step, a heating furnace is prepared in which the original block is placed between a pair of electrodes, the heating furnace has a pack material region in which the pack material is placed surrounding the original block, and a heat-insulating layer further surrounding the pack material region.

[0029] FIG. 1 is a plan view of the inside of an Acheson furnace used in a method for producing a carbon-based product according to a first embodiment of the present invention. An original block 10, a pack material 20, a heat insulating layer 30, and an electrode 40 are arranged in an Acheson furnace 100, which is a heating furnace. The original block 10, the pack material 20, and the heat insulating layer 30 are arranged inside a housing 50 of the Acheson furnace 100, and the surface of the electrode 40 is exposed from the housing 50 because electricity is applied from the outside. The pack material 20 is divided into a first region 21 and a second region 22 depending on the region in which it is arranged.

[0030] FIG. 2 is an enlarged view of one repeat unit around the original block of FIG. 2 shows one repeat unit of the original block 10 embedded in the pack material 20. A first region 21 of the pack material area is adjacent to the original block 10 in the current-flow direction. A second region 22 surrounds the original block and the first region along the axis of the current-flow direction. In a cross-sectional view taken along the current-flow direction (cross-sectional view in the direction of FIG. 4(b)), the cross-sectional area of ​​the original block 10 and the cross-sectional area of ​​the electrode 40 are equal.

[0031] In the Acheson furnace 100, a master block 10 is placed between a pair of electrodes 40, a pack material region in which pack material 20 is placed surrounding the master block 10, and a heat insulating layer 30 surrounding the pack material region are also arranged, and the master block 10 can be heated by passing a current through the electrodes 40.

[0032] 4(a) is an oblique view of the original block of FIG. 2 and the area around the original block, FIG. 4(b) is a cross-sectional view taken along the direction of current flow, and FIG. 4(c) is a cross-sectional view taken from the side of the current flow. Carbonaceous pack material has an appropriate resistance value, so it can be resistively heated by passing a current through the electrodes. The resistance value between the electrodes is determined by the resistivity and arrangement of the pack material and original block.

[0033] The resistivity of the original block decreases as the firing process progresses. Therefore, the area through which the current flows changes in accordance with the change in the original block's resistivity. In the early stages of the heating process, the original block's resistivity is high, and the current flows mainly through the second region (Figure 3(a)). As the temperature of the furnace rises and the original block is carbonized, the current begins to flow through the original block and the first region (Figure 3(b)). In addition, Figures 3(a) and 3(b) show one original block 10 between a pair of electrodes 40, and the amount of current i1 flowing through the first region and the amount of current i2 flowing through the second region are shown diagrammatically by the thickness of the arrows.

[0034] As shown in Figures 4(a), 4(b), and 4(c), respectively, the cross-sectional area of ​​the original block 10 perpendicular to the current-flow direction is S1, the cross-sectional area of ​​the second region 22 of the pack material 20 is S2, the length of the original block 10 along the current-flow direction is L1, the length of the first region 21 of the pack material 20 is L2, the specific resistance of the original block 10 is ρ1, and the specific resistance of the pack material 20 is ρ2. In one repeat unit of the original block 10 embedded in the pack material 20, the resistance value of the first region 21 is R1, the resistance value of the second region 22 is R2, and the resistance value of the original block 10 is R3. B Let us assume that.

[0035] FIG. 5 is a circuit diagram showing an equivalent circuit around the original block in FIG. R1, R2, R B The equivalent circuit for one repeating unit was set as shown in Figure 5. Since there is a sufficient distance between the original block and the thermal insulation layer, it was assumed that there was no current flowing in the first region or between the original block and the second region. Total resistance of the equivalent circuit R total is as follows.

number

number

number

[0036] The amount of heat generated per volume (V1) of the first region is as follows:

number

number

number

[0037] The amount of heat generated per volume (V2) of the second region is

number

number

[0038] Volume of the original block (V B The heat generated per

number

number

[0039] The difference in heat generation per volume between the second region and the first region is:

number

[0040] In the initial stage of this embodiment (before the original block is fired), the resistivity of the original block is overwhelmingly large, and the current passing through the second region 22 is dominant as shown in FIG. 3( a), and heat is generated by the resistance of the pack material 20 in the second region 22, so that the original block 10 can be warmed up little by little.

[0041] As the heat of the pack material 20 is transferred to the original block 10 and carbonization of the original block 10 progresses, the resistivity of the original block 10 becomes lower than that of the pack material 20, and the current passing through the first region 21 and the original block 10 becomes dominant as shown in Figure 3(b), and heat is generated by the resistance of the pack material 20 in the first region 21, heating the original block 10. At this stage, a carbon-based product can be obtained by heating in the same way as in an Acheson furnace for normal graphitization.

[0042] The heat insulating layer 30 is not particularly limited, but it is preferable to use carbon black since it has high heat resistance and heat insulating properties, and is a carbonaceous material that does not contain impurities.

[0043] The heating furnace may have one or more original blocks. Carbonaceous pack material is placed in a first region between the electrode and the original block and in a second region between the multiple original blocks. Carbonaceous pack material is placed in a second region between the electrode and the insulating layer on the side of the original block, similar to the first region.

[0044] The power supply for energizing an Acheson furnace has rated values ​​for both voltage and current. The maximum voltage that can be supplied is determined by the primary voltage and the winding ratio of the transformer, and the actual voltage applied is the voltage minus the internal resistance of the power supply and wiring. The rated current is generally determined by the current capacity of the control semiconductor.

[0045] The maximum energy can be input into an Acheson furnace when the product of the voltage and current actually applied between the electrodes, minus the internal resistance of the power supply, is maximized, and the power supply's capacity can be utilized to the maximum when the resistance between the electrodes is [voltage actually applied between the electrodes] / [current]. Therefore, when attempting to heat the product to a high temperature, the resistance between the electrodes is adjusted by adjusting the gap between the original blocks, and mainly by adjusting the thickness of the pack material in the first area.

[0046] The average particle size of the carbonaceous pack powder is not particularly limited, but is preferably, for example, 1 to 20 mm. The material of the carbonaceous pack powder is not particularly limited, but is preferably coke, graphite, or the like. Graphite has low resistivity and is easy to conduct electricity, and when placed around the original block, it generates heat and can promote heating. Coke may be used instead of graphite. When the coke is heated in the Acheson furnace, it is graphitized to become graphite, and can promote heating in the same way as the graphite pack powder. The average particle size of the carbon black used in the heat insulating layer is not particularly limited, but is preferably 2 to 1000 nm. Carbon black has an extremely small particle size, and the spherical crystals are oriented concentrically, and while the electrical conductivity is good within the particles, the resistance between the particles is high, so that almost no current flows on the heat insulating layer side, and the current is concentrated on the pack powder side, thereby suppressing heat generation on the heat insulating layer side.

[0047] The pore diameter at which the cumulative pore volume in the mercury intrusion method of the carbon-based product obtained by the method for producing a carbon-based product of the present invention is 50 to 500 μm is preferably 50 to 500 μm. If the pore diameter at which the cumulative pore volume of a carbon-based product in the mercury intrusion porosimetry is 50% of the total pore volume is 50 μm or more, the decomposition gas generated in the heating process can be quickly discharged outside the original block, and a carbon-based product without bulging or cracking can be obtained. If the pore diameter at which the cumulative pore volume of a carbon-based product in the mercury intrusion porosimetry is 500 μm or less, the connection points between secondary particles can be sufficiently secured, making the product strong and less likely to crack in the heating process. Note that, in the mercury intrusion porosimetry, measurements are performed at a mercury pressure range of 7 kPa to 220 MPa. A pressure of 7 kPa corresponds to a pore diameter of 211 μm, and 220 MPa corresponds to 6.8 nm.

[0048] Second Embodiment FIG. 7(a) is a plan view of the inside of an Acheson furnace used in a method for producing a carbon-based product according to a second embodiment of the present invention. In the second embodiment, in the heating step of the first embodiment, an electrode 40 having a larger cross-sectional area than the original block 10 is disposed. Since an electrode with a cross-sectional area larger than that of the original block is arranged, current can be sent evenly to the second region, making it less likely for localized heat to occur and for the original block to crack during the heating process.

[0049] Third Embodiment FIG. 7(b) is a plan view of the inside of an Acheson furnace used in the method for producing a carbon-based product according to the third embodiment of the present invention. In the third embodiment, in the heating step of the first embodiment, a dummy electrode 60 made of graphite and having a larger cross-sectional area than the original block 10 in the direction perpendicular to the current flow is disposed between the electrode 40 and the original block 10. Since a dummy electrode having a larger cross-sectional area than the master block is arranged, current can be sent to the second region without being biased, making it difficult for localized heat to occur and making it difficult for the master block to crack during the heating process. Furthermore, the size of the electrodes can be made smaller, so that the amount of heat diffusing to the outside of the furnace through the electrodes can be reduced.

[0050] Fourth Embodiment FIG. 7(c) is a plan view of the inside of an Acheson furnace used in the method for producing a carbon-based product according to the fourth embodiment of the present invention. In the fourth embodiment, rectangular original blocks 10 are used, and multiple rows are arranged with the longest direction of the rectangular parallelepiped in the current flow direction. With this configuration, the area receiving heat is large in the initial stage of the heating process, and heat can be efficiently received from the second region, making it possible to prevent cracking in the initial stage. Note that the pack material region sandwiched between original blocks 10 in the current flow direction becomes second region 22. Therefore, multiple arranged original blocks 10 can be heated from both sides in the thickness direction, making it possible to reduce the internal temperature difference and make the blocks less likely to crack.

[0051] The present specification discloses the following:

[0052] The present disclosure (1) provides a method for preparing a heating furnace having a pack material region in which an original block is disposed between a pair of electrodes and a pack material is disposed surrounding a periphery of the original block, and a heat insulating layer further surrounding the pack material region, A method for producing a carbon-based product, comprising a heating step of passing an electric current through the electrodes to heat the original block, The original block includes carbonaceous particles and a binder made of a carbon precursor that binds the carbonaceous particles together, The pack material area comprises: a first region adjacent to the original block in a current flow direction, which is a direction in which a current is passed through the electrode; a second region surrounding the original block and the first region along the axis of the current flow direction; It consists of: This is a method for producing a carbon-based product, characterized in that in an initial stage of the heating step, ρ1>ρ2, and the second region has a larger amount of heat per volume than the first region. ρ1: Resistivity of the original block ρ2: Specific resistance of the packing material area

[0053] The present disclosure (2) is a method for producing a carbon-based product as described in the present disclosure (1), characterized in that during the heating process of the original block, ρ1<ρ2, and the first region has a greater amount of heat per volume than the second region.

[0054] The present disclosure (3) is the method for producing a carbon-based product according to the present disclosure (1) or (2), characterized in that the pore diameter at which the cumulative pore volume of the carbon-based product in a mercury intrusion porosimetry is 50% of the total pore volume is 50 to 500 μm.

[0055] The present disclosure (4) is the method for producing a carbon-based product according to any one of the present disclosures (1) to (3), characterized in that in the original block, the carbonaceous particles and the binder form secondary particles, and the average particle diameter of the secondary particles is 50 to 1000 μm.

[0056] The present disclosure (5) is a method for producing a carbon-based product according to any one of the present disclosures (1) to (4), characterized in that the original block is a rectangular parallelepiped and is arranged with its longest direction facing the current flow direction.

[0057] The present disclosure (6) relates to a method for producing the carbon-based product described above, a kneading step of kneading the carbonaceous particles and the binder to obtain a carbon precursor; a molding step of molding the carbon precursor to obtain the original block; A heating step according to claim 1 or 2, in which the original block is heated; The method for producing a carbon-based product according to any one of the present disclosures (1) to (5) is characterized by comprising: EXAMPLES

[0058] 《Kneading process》 75 parts by weight of coal-based coke with an average particle size of 350 μm and 25 parts by weight of pitch with a softening point of 130°C were heated to 270°C and kneaded using a kneader. A carbon precursor granulated into granules was prepared during the kneading. The average particle size of the granulated particles was 200 μm.

[0059] 《Molding process》 The carbon precursor obtained in the kneading process was filled into a heated mold and pressed to obtain a base block. The size of the mold opening was 610 mm x 320 mm, the temperature of the mold was 100°C, and the surface pressure of the press molding was 1 MPa. Since the kneading process and the molding process were performed consecutively, the carbon precursor was used while still warm and was not reheated during molding. The size of the obtained original block was 610 mm x 320 mm x 80 mm, and the weight was 20 kg.

[0060] 《Heating process》 FIG. 10 is a perspective view of the inside of an Acheson furnace used in the manufacturing method of a carbon-based product according to the embodiment. Four original blocks were placed in an Acheson furnace, and electricity was passed through the electrodes at both ends of the lined-up original blocks to heat them. The original blocks were stacked in the thickness direction and arranged between the electrodes. Two dummy electrodes (four on each side) were placed between the original blocks to prevent bias in the current. In this case, smaller electrodes could be used, which reduced the amount of heat diffusing through the electrodes and improved thermal efficiency. The cross section of the packing area is 800 mm wide and 750 mm high, the cross section of the original block is 320 mm wide and 610 mm high, and the cross-sectional area S1 of the original block is 0.195 m 2 The cross-sectional area of ​​the packing material region S2 is 0.6m 2 It was. The distance between the electrode and the block and between the blocks was 70 mm (0.07 m). The length of the repeating unit in the direction of current flow was 0.15 m (150 mm), and the length of the block was 0.08 m (80 mm). The dummy electrode was 400 mm x 400 mm x 100 mm, and was loaded into the furnace in such a position that it protruded 210 mm above the original block (see FIG. 10). The resistivity ρ2 of the pack material was 0.002 Ωm. The resistivity ρ1 of the original block as a function of its thermal history, which was measured separately, is shown in Figure 9. Before heating (only thermal history during kneading), it was 5 Ωm, at 700°C it was 360 μΩm, at 900°C it was 100 μΩm, and at 2500°C it was 15 μΩm. The resistance value of each element in each temperature range was calculated based on the resistivity of the original block.

[0061] [Table 2] Furthermore, the current ratio to the total current in each temperature range was calculated.

[0062] [Table 3] The heat generation amount of each resistance element was calculated based on each current ratio and resistance value. Note that since the current ratio is used, the current value is made dimensionless.

[0063] The resistance value of each resistance element was multiplied by the square of the non-dimensional current value to calculate the heat generation amount. The actual heat generation amount is calculated by multiplying each value and the current (i1 + i2). 2 The product of this is the actual amount of heat generated. [Table 4] Furthermore, the heat generation ratio of each resistance element in each temperature range was calculated.

[0064] [Table 5] The amount of heat generated per volume of each resistance element in each temperature range was calculated.

[0065] [Table 6] Before heating, the second region generates more heat per unit volume, and the original block is heated from the second region. The original block is fired at 700°C, and the resistivity ρ1 decreases. As the resistivity ρ1 of the original block decreases, the heat generation per unit volume becomes greater in the first region, and the Acheson furnace can be energized using normal resistance heating.

[0066] In this embodiment, the heating process was completed at 1230°C. FIG. 11 is a photograph of the appearance of the carbon-based product obtained in the example. The obtained carbon-based product had been sintered. The carbon-based product had a portion facing the dummy electrode and a protruding portion. Cracks were observed at the boundary area. It was confirmed that the area where a uniform current was flowing from the dummy electrode was fired without cracks.

[0067] The pore distribution of the obtained carbonaceous product was measured by mercury intrusion porosimetry. The pore diameter at which the cumulative pore volume was 50% of the total pore volume was 76 μm. The bulk density is 1.23 g / cm 3 , and the resistivity was 97 μΩm. The master block of this Example has sufficiently large pores, so that even if the initial stage of the pack material was heated by resistance heating of the second region using an Acheson furnace, the decomposition gases were easily diffused and the heat treatment could be performed. [Explanation of symbols]

[0068] 10 Original Block 20 Packing Flour 21 The First Area 22 The Second Area 30 Thermal insulation layer 40 electrodes 50 Case 60 Dummy Electrode 70 Binder 80 Carbonaceous particles 100 Acheson Furnace (heating furnace)

Claims

1. a heating furnace is provided, the heating furnace including: an original block disposed between a pair of electrodes; a pack material region surrounding the original block and in which a pack material is disposed; and a heat insulating layer further surrounding the pack material region; A method for producing a carbon-based product, comprising a heating step of passing an electric current through the electrodes to heat the original block, The original block includes carbonaceous particles and a binder made of a carbon precursor that binds the carbonaceous particles together, The pack material area comprises: a first region adjacent to the original block in a current flow direction, which is a direction in which a current is passed through the electrode; a second region surrounding the original block and the first region along the axis of the current flow direction; It consists of: In the initial stage of the heating step, ρ 1 >ρ 2 wherein the second region has a greater amount of heat per volume than the first region. ρ 1 : Resistivity of the original block ρ 2 : Specific resistance of packing area

2. During the heating process of the raw block, ρ 1 <ρ 2 2. The method for producing a carbon-based product according to claim 1, wherein the first region generates a larger amount of heat per unit volume than the second region.

3. 3. The method for producing a carbon-based product according to claim 1, wherein the pore size at which the cumulative pore volume of the carbon-based product in a mercury intrusion method is 50% of the total pore volume is 50 to 500 μm.

4. 3. The method for producing a carbon-based product according to claim 1, wherein the carbonaceous particles and the binder in the original block form secondary particles, and the average particle size of the secondary particles is 50 to 1000 μm.

5. 3. The method for producing a carbon-based product according to claim 1, wherein the original block is a rectangular parallelepiped and is arranged with its longest direction facing the current flow direction.

6. The method for producing the carbon-based product described above comprises the steps of: a kneading step of kneading the carbonaceous particles and the binder to obtain a carbon precursor; a molding step of molding the carbon precursor to obtain the original block; A heating step according to claim 1 or 2, in which the original block is heated; A method for producing a carbon-based product, comprising: