AI Technical Summary
【0013】 分散機を用いて導電材を溶媒に分散して導電材分散液を製造する際、本発明の方法を採用することによって、品質値の制御された導電材分散液を継続して取得することができる。 特に、品質値として導電材分散液の粘度を採用した場合、導電材分散液の分散状態を良好に制御することができ、当該導電材分散液から得られる電池材料の物理特性を好適に制御することができる。
Smart Images

Figure 2024139160000001 
Figure 2024139160000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a conductive material dispersion containing at least a conductive material and a solvent. The conductive material dispersion produced by the present invention can be used as a slurry for a lithium ion secondary battery plate. [Background technology]
[0002] Various methods are known for producing slurries for lithium ion secondary battery plates and for producing carbon black dispersions for lithium ion secondary batteries.
[0003] For example, Patent Document 1 discloses a method for producing a positive electrode slurry for a lithium ion secondary battery, which contains a positive electrode active material for a lithium ion secondary battery, a binder, a conductive material, and an organic solvent, and includes the following step (1): mixing at least the positive electrode active material for a lithium ion secondary battery, the binder, and the organic solvent at a predetermined temperature at which the storage elastic stress of a binder solution for measuring storage elastic stress, which contains the binder and the organic solvent, satisfies a predetermined reduction range, from when at least a part of the positive electrode active material for a lithium ion secondary battery, at least a part of the binder, and at least a part of the organic solvent are initially mixed until when at least all of the positive electrode active material for a lithium ion secondary battery and all of the binder are mixed. The present invention discloses a method for producing a positive electrode slurry for a lithium ion secondary battery, comprising the steps of:
[0004] Patent Document 2 describes a method for producing a carbon black dispersion for batteries, which contains carbon black, N-methyl-2-pyrrolidone, a polyvinylidene fluoride polymer, and a dispersant, in which the carbon black content is 10 to 30 parts by mass relative to 100 parts by mass of the dispersion, the dispersant content is 1 to 6 parts by mass relative to 100 parts by mass of the carbon black, and the polyvinylidene fluoride polymer content x is 20 parts by mass or less relative to 100 parts by mass of the carbon black, and x=a / Mw (where a is 11×10 5 ≦a≦22×10 6where Mw is the weight average molecular weight of the polyvinylidene fluoride polymer), and the carbon black dispersion for batteries is dispersed using a shear type disperser so that the viscosity of the dispersion has a minimum viscosity value of 0.1 to 3 Pa s within a shear rate range of 1 / s or more and less than 100 / s. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2017-174535 A (claims, etc.) [Patent Document 2] JP 2017-135062 A (claims, etc.) Summary of the Invention [Problem to be solved by the invention]
[0006] In order to disperse fine particles in water, a dispersant is generally used and the mixture is stirred with a stirrer, but a mixed liquid containing a conductive material is viscous and difficult to disperse. In particular, when the mixed liquid becomes highly concentrated, it is not easy to continuously produce a homogeneous dispersion even with a high-performance stirrer.
[0007] In the process of obtaining a dispersion of fine particles, in order to achieve the desired physical properties, it is common to adjust the operating conditions of the process equipment based on the dispersion composition, experiments, experience, etc., and then measure and confirm the physical properties of the final dispersion. However, the physical properties of the final dispersion may not match those of the target, and it is therefore necessary to control the physical properties of the dispersion in parallel with the production.
[0008] In addition, if the dispersion liquid has a high viscosity, it is difficult to deliver the liquid, and production (dispersion) must be performed at a low speed, making quality control extremely difficult. If one tries to complete the dispersion in a short time, excessive pressure and power load will be applied to the entire process equipment, increasing the risk of breakdowns, which is not desirable.
[0009] If the dispersion liquid is highly viscous and highly concentrated and tends to solidify, accurate measurement using this confirmation method is difficult, so there is a need to find a method that allows measurement and confirmation without releasing the dispersion liquid from the sealed process.
[0010] An object of the present invention is to provide a method for obtaining a conductive material dispersion having a controlled quality value when a conductive material dispersion is produced by dispersing a conductive material in a solvent. [Means for solving the problem]
[0011] The inventors discovered that by providing a sensor for measuring quality values within the process, particularly in the outlet line of the disperser, and measuring the quality value of the dispersion within the outlet line, it is possible to accurately predict the time at which the dispersion will approach the target quality from the measured quality value, and thus completed the present invention.
[0012] That is, the present invention provides a method for producing a conductive material dispersion, which comprises continuously supplying a conductive material mixed liquid containing at least a conductive material and a solvent to a disperser, dispersing the conductive material, and continuously discharging the obtained conductive material dispersion from the disperser, A sensor is installed on the outlet line of the disperser to measure the quality value of the conductive material dispersion liquid discharged from the disperser at predetermined time intervals; Calculate the increase or decrease trend of the quality value from the quality value measurements of the most recent multiple points, The supply speed of the conductive material mixture to the disperser and / or the power of the disperser are adjusted according to the calculated increase / decrease tendency. The present invention relates to a method for producing a conductive material dispersion liquid, Effect of the Invention
[0013] When a conductive material dispersion is produced by dispersing a conductive material in a solvent using a disperser, by employing the method of the present invention, a conductive material dispersion with controlled quality values can be continuously obtained. In particular, when the viscosity of the conductive material dispersion is used as the quality value, the dispersion state of the conductive material dispersion can be well controlled, and the physical properties of the battery material obtained from the conductive material dispersion can be suitably controlled. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] In the present invention, a conductive material mixture containing at least a conductive material and a solvent is continuously supplied to a disperser and dispersed to obtain a conductive material dispersion. The conductive material mixture is a mixture in which at least a conductive material and a solvent are simply mixed by a mixer such as a disperser or a planetary mixer. The conductive material mixture is continuously supplied to the disperser using a pump or the like and is finely dispersed by the action of the disperser. Dispersion by the disperser is preferably performed in a closed system.
[0015] As the dispersing machine, a device having a strong beating ability such as a homomixer under high speed rotation, a high pressure homogenizer, an ultra-high pressure homogenizer, an ultrasonic dispersion processor, a planetary mixer, a combimix, a kneader, a centrifugal mixer, a Henschel mixer, a ball mill, a bead mill, a thin film rotating type high speed agitator, a screw type mixer, a paddle mixer, a dispersing type mixer, a turbine type mixer, a propeller mixer, a blender, an ultrasonic homogenizer, a colloid mill, a pebble mill, a beater, a disk type refiner, a conical type refiner, a double disk type refiner, a grinder, etc. Such a dispersing machine is preferable because it performs defibration or crushing of the conductive material in parallel with the affinity between the conductive material and the solvent. Two or more types of dispersing machines may be used in combination.
[0016] In the present invention, the conductive material dispersion obtained through dispersion by the disperser is continuously discharged from the disperser, and the discharged conductive material dispersion is led to a storage tank or a next process device through an outlet line. The operation of discharging the conductive material dispersion is preferably carried out using a pump or the like capable of controlling the dispersion flow rate. In addition, the discharge operation is preferably carried out in a state where the conductive material dispersion is sealed without being exposed to the outside.
[0017] During the discharge operation, the quality value of the conductive material dispersion discharged from the disperser is measured at predetermined time intervals using a sensor installed in the outlet line of the conductive material dispersion. The quality value of the conductive material dispersion may be continuously measured, and the measured values may be collected at a predetermined time interval. The measurement interval is approximately 1 / 100 of the residence time T of the conductive material dispersion in the disperser. Then, the increase / decrease tendency of the quality value of the conductive material dispersion is calculated from the most recent measured values at multiple points. The most recent five or more measured values may be used for the calculation.
[0018] Next, the supply speed of the conductive material and the solvent to the disperser is adjusted according to the calculated increase / decrease tendency. In particular, the quality value after 2 to 4 times the residence time T from the measurement is adjusted to approach the target value. This controls the residence time in the disperser until the conductive material dispersion passes through the disperser. Alternatively, in addition to or instead of this, the power of the disperser, for example, the rotation speed of the stirring blade of the disperser, is adjusted. When the power of the disperser is increased, the rotation speed of the stirring blade increases and the dispersion of the conductive material dispersion increases. This controls the dispersibility of the conductive material dispersion by the action of the disperser.
[0019] It is preferable to continuously perform a series of operations, consisting of measuring the quality value of the conductive material dispersion discharged from the disperser, calculating the increase / decrease tendency from the measured quality value, and adjusting the supply rate of the conductive material dispersion to the disperser in accordance with the calculated increase / decrease tendency, using an automated device. Alternatively, in addition to or instead of this, it is preferable to continuously perform a series of operations consisting of measuring the quality value of the conductive material dispersion discharged from the disperser, calculating the increase / decrease tendency from the measured quality value, and adjusting the power of the disperser in accordance with the calculated increase / decrease tendency using an automated device.
[0020] The automatic control device includes at least the steps of measuring a quality value of the conductive material dispersion liquid discharged from the disperser, calculating an increase / decrease trend of the quality value from the measured quality value, and adjusting the supply speed of the conductive material mixed liquid to the disperser in accordance with the calculated increase / decrease trend.
[0021] Alternatively, the automatic control device may additionally or instead include at least the steps of measuring a quality value of the conductive material dispersion liquid discharged from the disperser, calculating an increase / decrease trend of the quality value from the measured quality value, and adjusting the power of the disperser in accordance with the calculated increase / decrease trend. This makes it possible to appropriately control the quality of the conductive material dispersion.
[0022] The quality value of the conductive material dispersion liquid includes various physical properties, but it is particularly preferable to use viscosity. The case where viscosity is used as the quality value will be described below.
[0023] As a device for measuring viscosity, an in-line type viscosity sensor is preferably used. The in-line type viscosity sensor is installed in the outlet line of the conductive material dispersion liquid and measures the viscosity of the conductive material dispersion liquid. An example of the in-line type viscosity sensor is the MV type in-line viscosity sensor (manufactured by MAKE Co., Ltd.).
[0024] The viscosity is measured at a predetermined time interval. The viscosity may be measured continuously, and the measured values may be collected at each predetermined time interval. The interval at which the viscosity is measured is approximately 1 / 100 of the residence time of the conductive material dispersion in the disperser. The tendency of the viscosity of the conductive material dispersion to increase or decrease is then calculated from the most recent viscosity measurement values at multiple points. The most recent five or more viscosity measurement values may be used for the calculation.
[0025] Next, the supply rate of the conductive material mixture to the disperser and / or the power of the disperser are adjusted according to the calculated increase / decrease tendency, thereby controlling the residence time of the conductive material dispersion in the disperser until it passes through the disperser.
[0026] Specifically, if the viscosity of the conductive material dispersion tends to increase, the supply speed of the conductive material mixture is decreased and / or the power of the disperser is increased to lengthen the residence time of the conductive material dispersion in the disperser and / or to increase the energy to the conductive material dispersion, which results in an increase in the dispersing action of the disperser of the conductive material dispersion and a decrease in the viscosity of the conductive material dispersion.
[0027] Conversely, if the viscosity of the conductive material dispersion tends to decrease, the supply speed of the conductive material mixture is increased and / or the power of the disperser is reduced to shorten the residence time of the conductive material dispersion in the disperser and / or to reduce the energy to the conductive material dispersion, which results in a decrease in the dispersing action of the disperser of the conductive material dispersion and an increase in the viscosity of the conductive material dispersion. In this way, the viscosity of the conductive material dispersion liquid can be controlled.
[0028] A method for controlling the viscosity of a conductive material dispersion will be described using as an example a process in which the viscosity of the conductive material dispersion discharged from a disperser is measured with an in-line viscometer, and the supply speed of the conductive material dispersion to the disperser is automatically adjusted by a pump based on the viscosity transition.
[0029] In the process of dispersing a conductive material mixture using an agitator such as a thin film swirling high-speed agitator, the viscosity, which is the quality value of the dispersion, is measured at regular time intervals using an in-line viscometer placed at the outlet line of the agitator. At this time, the slope a (e.g., mPa·s / sec) and intercept b (the latest viscosity value) of the viscosity transition of the dispersion are obtained from the most recent multiple viscosity measurement values, and the supply speed of the mixture is adjusted so that the predicted viscosity value Y after a specified time approaches the target viscosity value.
[0030] When the predicted value Y is greater than the target value, the pump is adjusted to further disperse the conductive material dispersion and reduce the viscosity by decreasing the supply speed of the mixed liquid or increasing the peripheral speed of the rotation speed of the disperser. Conversely, when the predicted value Y is smaller than the target value, the pump is adjusted to suppress dispersion of the conductive material dispersion and increase the viscosity by increasing the supply speed of the mixed liquid or decreasing the peripheral speed of the rotation speed of the disperser. The greater the deviation between the target value and the predicted value Y, the greater the change in the supply speed of the mixed liquid.
[0031] By programming the operation of calculating the predicted viscosity value Y after a certain time from the measured viscosity value and feeding it back to the pump that supplies the dispersion, it is possible to automate the adjustment of the viscosity of the dispersion. The correlation coefficient used to calculate the slope of the most recent viscosity change of the dispersion can also be used as a criterion for determining the amount of change in the supply speed of the mixed liquid. This makes it possible to improve the accuracy of viscosity control of the dispersion when the measurement values vary greatly due to noise, etc.
[0032] This makes it possible to control the dispersion state of the conductive material dispersion, and even if the mixed state of the mixed liquid supplied to the disperser fluctuates, the viscosity and other physical properties of the conductive material dispersion can be controlled. The method of the present invention controls the residence time of the conductive material mixed liquid in the disperser and / or the dispersing action of the disperser due to the mechanical force applied to the conductive material mixed liquid, using the viscosity of the conductive material dispersion as an index.
[0033] The conductive material may be carbon nanotubes, a combination of carbon nanotubes and flat graphite, graphene, etc. The conductive material is preferably supplied to the disperser as a mixed liquid in which it is preliminarily mixed with a fluid medium.
[0034] <Carbon nanotubes> The carbon nanotube (CNT) used in the present invention is not particularly limited as long as it has a shape formed by essentially rolling one surface of graphite into a cylindrical shape, and either a single-walled CNT in which one surface of graphite is rolled into one layer, or a multi-walled CNT in which two or more layers are rolled, can be used.
[0035] Furthermore, examples of the form of carbon nanotubes include, but are not limited to, graphite whiskers, filamentous carbon, graphite fibers, ultrafine carbon tubes, carbon tubes, carbon fibrils, carbon microtubes, and carbon nanofibers, and these may be used alone or in combination of two or more types (hereinafter simply referred to as "at least one type").
[0036] Furthermore, from the viewpoints of the viscosity, conductivity, and stability of the dispersion, the average outer diameter of the carbon nanotubes is preferably 1 nm or more and 90 nm or less, more preferably 3 nm or more and 30 nm or less, and even more preferably 3 nm or more and 15 nm or less.
[0037] In the present invention, the average outer diameter of carbon nanotubes refers to the arithmetic mean value of the outer diameters of a sufficient number n measured using an image at a magnification of 100,000 or more with a transmission electron microscope. The purity of the carbon nanotubes used in the present invention is preferably 90 to 100% by mass, and particularly preferably 95 to 100% by mass. The purity of the carbon nanotubes is calculated based on the amount of impurities, with ash content measured according to JIS K 1469 or JIS K 6218 being taken as the impurity.
[0038] Specific examples of carbon nanotubes that can be used include NC7000 (average outer diameter: 10 nm) manufactured by Nanocyl, Baytubes C150P (average outer diameter: 11 nm) manufactured by Bayer, FloTube 9000 (average outer diameter: 19 nm), FloTube 7320 (average outer diameter: 9 nm), FloTube 7010 (average outer diameter: 9 nm), FloTube 6810 (average outer diameter: 8 nm), FloTube 6120 (average outer diameter: 8 nm), FloTube 6100 (average outer diameter: 8 nm), FloTube 2020 (average outer diameter: 4 nm) manufactured by Cnano, and MEIJO eDIPS manufactured by Meijo Nano Carbon Co., Ltd. At least one of EC2.0 (average outer diameter 2.0 nm), KORBON-A7 (average outer diameter 1.2 nm) manufactured by KORBON Co., Ltd., NFT-7 (average outer diameter 30 nm) manufactured by Koatsu Gas Kogyo Co., Ltd., and NFT-15 (average outer diameter 30 nm) manufactured by Koatsu Gas Kogyo Co., Ltd. can be used.
[0039] The solvent in the dispersion of the present invention may be water, a water-soluble solvent, or a mixture thereof. As the water, tap water, distilled water, ion-exchanged water, etc. may be used.
[0040] Examples of the water-soluble solvent include ethylene glycol, triethylene glycol, tetraethylene glycol, propylene glycol, dipropylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 2,3-butanediol, 1,3-butanediol, 1,4-butanediol, 1,2-pentanediol, 1,5-pentanediol, 2,5-hexanediol, 3-methyl-1,3-butanediol, 2-methylpentane-2,4-diol, 3-methylpentane-1,3,5-triol, 1,2,3 At least one of alkylene glycols such as 2-hexanetriol, polyalkylene glycols such as polyethylene glycol and polypropylene glycol, glycerols such as glycerol, diglycerol and triglycerol, lower alkyl ethers of glycols such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether and diethylene glycol mono-n-butyl ether, N-methyl-2-pyrrolidone, and 1,3-dimethyl-2-imidalidinone can be used.
[0041] Other water-soluble solvents that can be used include amides such as dimethylformamide and dimethylacetamide, and ketones such as acetone. When water and a water-soluble solvent are mixed, the content of the water-soluble solvent is preferably 0.1 to 10% by mass, and more preferably 0.5 to 5% by mass, based on the total amount of the mixed solvent, from the viewpoint of storage stability of the dispersion.
[0042] The content of the carbon nanotubes in the dispersion can be set to a suitable value depending on the application. When used in conductive pastes, electrode pastes for secondary batteries, electrodes for secondary batteries, etc., the carbon nanotube content is preferably 0.1 to 15.0 mass% relative to the total amount of the dispersion, more preferably 0.1 to 10.0 mass%, even more preferably 0.5 to 8.0 mass%, particularly preferably 1.0 to 6.0 mass%, and most preferably 2.0 to 5.0 mass%, from the viewpoints of achieving both high stability and conductive performance and viscosity during dispersion production. The present invention can be suitably applied to carbon nanotube dispersions with such concentrations.
[0043] By making the carbon nanotube content 0.1 mass % or more relative to the total amount of the dispersion, good conductivity can be ensured when the battery is made, while by making it 15.0 mass % or less, the stability of the dispersion can be ensured.
[0044] The carbon nanotubes can also be combined with flat graphite. In this case, a synergistic effect with the carbon nanotubes can be obtained by making the amount of flat graphite 10% by mass or more relative to the amount of carbon nanotubes, and the stability of the dispersion can be ensured by making the amount 200% by mass or less.
[0045] The dispersion of the present invention may further contain cellulose nanofibers (CeNFs). As the cellulose nanofibers, oxidized cellulose nanofibers obtained by carboxylating cellulose with TEMPO can be preferably used as a dispersant for carbon nanotubes.
[0046] The oxidized cellulose nanofibers used preferably have cellulose type I crystals. The oxidized cellulose nanofibers preferably have a crystallinity of less than 70% as measured by X-ray diffraction. The crystallinity is more preferably 25% or more and less than 70%. If the crystallinity is less than 70%, the carbon nanotubes are oxidized and defibrated to a suitable degree, resulting in good dispersibility.If the crystallinity is more than 70%, the carbon nanotubes are likely to be insufficiently defibrated or crushed, resulting in insufficient dispersibility.
[0047] The fiber length of the oxidized cellulose nanofibers blended in the dispersion is preferably such that 85% or more of the total have a fiber length of 50 nm to 250 nm, and more preferably 30% or more of the total have a fiber length of 100 nm to 150 nm. Furthermore, the oxidized cellulose nanofibers blended in the carbon nanotube dispersion preferably have a number average fiber length L of 100 nm to 150 nm, and a ratio of the number average fiber length L to the length-weighted average fiber length Ll (Ll / L) of 1.0 to 1.4.
[0048] When the fiber length of the oxidized cellulose nanofibers is within the above range, the dispersibility of the carbon nanotubes is good. Although the mechanism behind this is unclear, it is presumed to be related to the permeability of the oxidized cellulose nanofibers into the carbon nanotubes.
[0049] Furthermore, the oxidized cellulose nanofibers used have a certain amount of remaining alcoholic hydroxyl groups, which allows stronger hydrogen bonding between molecules and structural restoration. When the dispersion is applied, the viscosity decreases during application, making it easier to apply evenly, and the viscosity recovers after application, allowing the material to maintain a uniform state thereafter. In addition, the recovery (increase) of viscosity after application makes the material less likely to aggregate and warp when drying. Alcoholic hydroxyl groups are detected by infrared spectroscopy.
[0050] The dispersion of the present invention may contain graphene. Graphene is a single-atom-thick sp 2 It is a sheet-like material of bonded carbon atoms arranged in a honeycomb-like hexagonal lattice structure made up of carbon atoms and their bonds.
[0051] In the present invention, a series of operations are performed, including measuring the quality value of the conductive material dispersion discharged from the disperser, calculating the increase / decrease tendency from the measured quality value, and adjusting the supply speed of the conductive material mixed liquid to the disperser and / or the power of the disperser in accordance with the calculated increase / decrease tendency. It is preferable to perform the series of operations using an automated device. In this case, the method for producing the conductive material dispersion is preferably one in which the quality value to be controlled is viscosity. EXAMPLES
[0052] Examples 1 to 9 <Preparation of Conductive Dispersion Liquid> The conductive material, dispersant, and ion-exchanged water were mixed in the compositions and ratios shown in Table 1, Examples 1 to 9, and stirred for 1 hour in a mixer (Combimix; manufactured by Primix Corporation) to obtain a mixed solution. Next, the mixed solution was put into a 1.5 L capacity Dyno Mill (manufactured by Willy & Bachofen, bead mill; zirconia beads φ1.0 mm) and dispersed at a circumferential speed of a rotating disk of 10 m / s. Furthermore, the mixed solution was continuously supplied to and discharged from the disperser using a metering pump capable of controlling the flow rate. The initial condition for the bead mill residence time of the mixed solution, i.e., the dispersion treatment time, was set to 15 minutes.
[0053] At that time, an in-line viscosity sensor (FEM-1000V-ST, Sekonic Corporation) installed on the outlet line of the disperser was used to measure the viscosity of the conductive material dispersion discharged from the disperser at 1 second intervals, and when the slope of the viscosity change of the conductive material dispersion from the most recent 20 measurement values was taken as a (mPa s / sec) and the most recent viscosity value was taken as the intercept b, the pump frequency was adjusted to control the supply speed of the conductive material mixture to the disperser so that the predicted viscosity value Y (= 200 × a + b) after 200 seconds became the target viscosity value.
[0054] When the predicted value Y is greater than the target viscosity value, the supply speed of the mixed liquid is decreased or the peripheral speed of the rotation speed of the disperser is increased to further advance the dispersion of the conductive material dispersion and to decrease the viscosity. When the predicted value Y is smaller than the target viscosity value, the supply speed of the mixed liquid is increased or the peripheral speed of the rotation speed of the disperser is decreased to suppress the dispersion of the conductive material dispersion and to increase the viscosity. The above operations were automatically controlled by a program.
[0055] In accordance with the calculated viscosity increase / decrease tendency, the supply flow rate of the conductive material mixture liquid was automatically controlled in real time in Examples 1-2 and 5-9, the peripheral speed of the disperser rotation speed in Production Example 4, and both in Production Example 3. By following the above procedure, a homogeneous conductive material dispersion with an almost constant viscosity was continuously obtained from the beginning to the end of production, even though the mixing state of the mixed liquid supplied to the disperser changed from time to time and the viscosity of the mixed liquid fluctuated.
[0056] <Preparation of negative electrode slurry> Conductive material dispersions of Examples 1 to 9 containing at least one conductive material selected from spherical graphite, acetylene black, carbon nanotubes, graphite (flake-like), and graphene as active materials, and carboxymethyl cellulose (CMC) and styrene butadiene rubber (SBR) as binders were prepared in the proportions shown in Examples 1 to 9 in Table 2. After mixing the spherical graphite and CMC using a planetary mixer, the conductive material dispersion was added until the mixture had a suitable hardness for kneading. After kneading for 3 hours, the remaining conductive material dispersion was added little by little, and when the mixture became uniform and fluid, SBR was added to prepare a negative electrode slurry.
[0057] <Preparation of negative electrode> The negative electrode slurry obtained by the above method was applied to a copper foil having a thickness of 20 μm by a die coater in a coating amount of 4.0 mg / cm. 2 After coating with the coating solution, the negative electrode was dried with hot air to obtain a sheet-like negative electrode. The following evaluations were carried out using the obtained negative electrode sheet. The results are shown in Table 2.
[0058] <Electrode evaluation> Electrode restoration evaluation The negative electrode sheet was pressed with a press to make the coating density 1.60 g / cm 3 After leaving the film at room temperature under atmospheric pressure for 7 days, the density was measured and evaluated according to the following criteria. The density was calculated from the film thickness. ◎: Density 1.55g / cm 3 less than 〇: Density 1.55g / cm 3 More than 1.60g / cm 3 less than ×: Density 1.60g / cm 3 As it is
[0059] Output characteristics and battery characteristics uniformity evaluation Twenty disks were randomly punched out from the negative electrode sheet to produce 20 coin cells (CR2032). DC resistance was measured using each coin cell, and the output characteristics were evaluated according to the following criteria. In addition, the standard deviation of the measured DC resistance values was calculated, and the uniformity of the battery characteristics was evaluated according to the following criteria. The results are shown in Table 1. Output Characteristics ◎: The average DC resistance of 20 coin cells is less than 30 Ω ○: The average DC resistance of 20 coin cells is 30 Ω or more and less than 40 Ω ×: The average DC resistance of 20 coin cells is 40 Ω or more. Uniformity of battery characteristics 〇: The standard deviation of the DC resistance measurements of 20 coin cells is less than 0.5 Ω ×: The standard deviation of the DC resistance measurements of 20 coin cells is 0.5 Ω or more.
[0060] Comparative Examples 1 to 4 <Preparation of Conductive Dispersion Liquid> A conductive material dispersion was obtained in the same manner as in Example 1, except that the components of the dispersion were combined in the compositions and ratios shown in Comparative Examples 1 to 4 in Table 1, and neither the supply speed of the conductive material mixture to the disperser nor the power of the disperser was adjusted, but manual control was performed based on offline measured values.
[0061] <Preparation of negative electrode slurry> Conductive material dispersions of Comparative Examples 1 to 4 containing at least one conductive material selected from spherical graphite, acetylene black, carbon nanotubes, graphite (flake-like), and graphene as active materials, and carboxymethyl cellulose (CMC) and styrene butadiene rubber (SBR) as binders were prepared in the proportions shown in Table 2, Comparative Examples 1 to 4. After mixing the spherical graphite and CMC using a planetary mixer, the conductive material dispersion was added until it reached a suitable consistency for kneading, and after kneading for 3 hours, the remaining conductive material dispersion was added little by little, and when it became uniform and fluid, SBR was added to prepare a negative electrode slurry.
[0062] <Preparation of negative electrode> Using the negative electrode slurry obtained by the above method, a negative electrode sheet was obtained in the same manner as in Example 1. The electrode recovery, output characteristics, and battery characteristic uniformity of the obtained negative electrode sheet were evaluated according to the above criteria. The results are shown in Table 2.
[0063] [Table 1]
[0064] [Table 2] [Industrial Applicability]
[0065] According to the method for producing a conductive material dispersion of the present invention, a conductive material dispersion that can be used as a slurry for electrode plates of lithium ion secondary batteries can be continuously produced.
Claims
1. A method for producing a conductive material dispersion, comprising continuously supplying a conductive material mixed liquid containing at least a conductive material and a solvent to a disperser, dispersing the conductive material, and continuously discharging the obtained conductive material dispersion from the disperser, A sensor is installed on the outlet line of the disperser to measure the quality value of the conductive material dispersion liquid discharged from the disperser at predetermined time intervals; Calculate the increase or decrease trend of the quality value from the quality value measurements of the most recent multiple points, The supply speed of the conductive material mixture to the disperser and / or the power of the disperser are adjusted according to the calculated increase / decrease tendency.
4. The method for producing a conductive material dispersion comprising the steps of:
2. The method for producing a conductive material dispersion liquid according to claim 1 , wherein the quality value is a viscosity.
3. The method for producing a conductive material dispersion liquid according to claim 1 , wherein the conductive material is a carbon nanotube.
4. 2. The method for producing a conductive material dispersion according to claim 1, wherein the conductive material is a combination of carbon nanotubes and flat graphite.
5. The method for producing a conductive material dispersion liquid according to claim 1 , wherein the conductive material is graphene.
6. The method for producing a conductive material dispersion according to claim 1 , wherein the dispersion further contains cellulose nanofibers.
7. The method for producing the conductive material dispersion liquid according to any one of claims 1 to 6, wherein a series of operations consisting of measuring the quality value of the conductive material dispersion liquid discharged from a disperser, calculating the increase / decrease tendency from the measured quality value, and adjusting the supply speed of the conductive material mixed liquid to the disperser and / or the power of the disperser according to the calculated increase / decrease tendency are continuously performed using an automated device.
Citation Information
Patent Citations
Method for manufacturing carbon black dispersion for lithium ion secondary battery
JP2017135062A
Manufacturing method of cathode slurry for lithium ion secondary battery
JP2017174535A