Semiconductor wafer with protective film, semiconductor chip with protective film, protection method for semiconductor wafer, manufacturing method of semiconductor wafer with protective film, and composite sheet

A protective film for semiconductor wafers with a specific cross-sectional shape between bumps addresses warping and protective performance issues, ensuring strong bump protection and efficient production by adhering to predefined height and distance relationships.

JP2024139197APending Publication Date: 2024-10-09LINTEC CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023050030
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Semiconductor wafers with protective films face challenges in suppressing warping and maintaining strong protective performance as they become larger and thinner, with existing methods either increasing resin amount or reducing protective performance.

Method used

The protective film is designed with a specific cross-sectional shape between adjacent bumps, adhering to predefined height and distance relationships to ensure strong bump protection and minimize warping, achieved by forming a protective film with a curable resin that satisfies certain mathematical relationships.

Benefits of technology

The solution enhances shear strength and environmental stability of bumps while reducing the overall resin amount, minimizing warping and enabling efficient, cost-effective production of semiconductor wafers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139197000001_ABST
    Figure 2024139197000001_ABST
Patent Text Reader

Abstract

To provide a semiconductor wafer with a protective film, etc., of which the bumps are firmly protected regardless of an environmental change and which is capable of suppressing occurrence of warpage.SOLUTION: A semiconductor wafer with a protective film comprises: a semiconductor wafer provided with a bump-formed face including a plurality of bumps; and a protective film (X) of a cured resin covering a side face of each bump, a face positioned at a lower side of the side face, and the bump-formed face. The plurality of bumps include a first bump and a second bump which are adjacent to each other. In a planar view of the first bump and the second bump, on a cross section passing through the inside of a circle of a predetermined size including a center of the first bump and the inside of a circle of a predetermined size passing through a center of the second bump, the protective film (X) includes: a first shoulder part in contact with the first bump and most separated from the bump-formed face; a second shoulder part in contact with the second bump and most separated from the bump-formed face; and a valley part which is positioned between the first and second shoulder parts. A height h1a of the first shoulder part, a height h1b of the second shoulder part, and a smallest height h2 of the valley part satisfy a predetermined relation.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a semiconductor wafer with a protective film, a semiconductor chip with a protective film, a method for protecting a semiconductor wafer, a method for manufacturing a semiconductor wafer with a protective film, and a composite sheet. [Background technology]

[0002] In recent years, semiconductor devices have been manufactured using a mounting method known as the face-down method, in which a semiconductor chip having bumps on its circuit surface and a substrate for mounting the semiconductor chip are stacked such that the circuit surface of the semiconductor chip faces the substrate, thereby mounting the semiconductor chip on the substrate. Incidentally, the semiconductor chips are usually obtained by dicing a semiconductor wafer having bumps on its circuit surface.

[0003] A semiconductor wafer having bumps may be provided with a protective film for the purpose of protecting the bonded portion between the bump and the semiconductor wafer (hereinafter also referred to as a "bump neck"). For example, in Patent Documents 1 and 2, a laminate in which a support substrate, an adhesive layer, and a thermosetting resin layer are laminated in this order is pressed and attached to a bump-forming surface of a semiconductor wafer having bumps with the thermosetting resin layer as a bonding surface, and then the thermosetting resin layer is heated and cured to form a protective film. Note that Patent Documents 1 and 2 illustrate that the surface of the protective film between two adjacent bumps is flat. Furthermore, Patent Document 3 describes that when a protective film is formed by curing a curable resin film, the weight-average molecular weight of the curable component contained in the curable resin film is optimized in order to prevent a large concave distortion from occurring in the protective film formed between two adjacent bumps. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2015-092594 A [Patent Document 2] JP 2012-169484 A [Patent Document 3] Patent No. 6229222 Summary of the Invention [Problem to be solved by the invention]

[0005] Incidentally, as semiconductor processes become more complicated and semiconductor wafers become larger and thinner, suppression of warpage in semiconductor wafers with protective films is now more stringently required than ever before. According to the inventor's research, it was found that if valleys are prevented from being formed in the protective film, as in Patent Document 3, the total amount of resin on the semiconductor wafer with the protective film increases, and this makes it more likely for warping to occur, for example, when a thin semiconductor wafer is used or when the back surface of the semiconductor wafer with the protective film is ground to make it thinner. It was also found that simply reducing the thickness of the protective film in order to suppress warping would reduce the protective performance of the protective film in the first place, making it unable to provide strong protection for the bumps, and that the reduction in the protective performance of the protective film would become more pronounced, for example, when exposed to a high-temperature environment.

[0006] The present invention has been made in consideration of the above problems, and has an object to provide a semiconductor wafer with a protective film, a semiconductor chip with a protective film, a method for protecting a semiconductor wafer, a method for manufacturing a semiconductor wafer with a protective film, and a composite sheet, which can firmly protect bumps regardless of environmental changes and suppress the occurrence of warping. [Means for solving the problem]

[0007] As a result of intensive research into solving the above problems, the inventors discovered that the above problems could be solved by making the cross-sectional shape of the protective film between a pair of adjacent bumps a predetermined shape, and thus completed the present invention.

[0008] That is, the present invention relates to the following. [1] A semiconductor wafer having a bump-forming surface with a plurality of bumps; a protective film (X) including a cured resin that covers a side surface of each of the bumps, a surface located below the side surface, and the bump formation surface, The plurality of bumps include a first bump and a second bump adjacent to each other, When the first and second bumps are viewed in plan, in a vertical cross section passing through a circle having a diameter 10% of the maximum diameter of the first bump and having the same center as the center of the first bump, and a circle having a diameter 10% of the maximum diameter of the second bump and having the same center as the center of the second bump, the protective film (X) has a first shoulder portion which is a portion in contact with the first bump and is the farthest from the bump-forming surface, a second shoulder portion which is a portion in contact with the second bump and is the farthest from the bump-forming surface, and a valley portion located between the first shoulder portion and the second shoulder portion, A semiconductor wafer with a protective film, wherein a height h1a of the first shoulder portion from the bump-forming surface, a height h1b of the second shoulder portion from the bump-forming surface, and a minimum height h2 of the valley portion from the bump-forming surface satisfy the relationship of the following formula (1). 0.75≧[h2 / {(h1a+h1b) / 2}]≧0...Equation (1) [2] The semiconductor wafer with a protective film according to the above [1], wherein a minimum height h2 of the valley portion from the bump-forming surface, a height BMha of the first bump from the bump-forming surface, and a height BMhb of the second bump from the bump-forming surface satisfy the relationship of the following formula (2). 0.37≧[h2 / {(BMha+BMhb) / 2}]≧0...Equation (2) [3] A semiconductor wafer with a protective film according to the above [1] or [2], wherein in the vertical cross section, a length L in a direction along the bump-forming surface of a region of the valley portion having a height that is 80% or less of the arithmetic mean value h1 of a height h1a of the first shoulder portion from the bump-forming surface and a height h1b of the second shoulder portion from the bump-forming surface, and a distance w between the first bump and the second bump in the vertical cross section satisfy the relationship of the following formula (3). 0.90≧[L / w]≧0...Equation (3) [4] A semiconductor wafer with a protective film according to any one of the above [1] to [3], wherein a height h1a of the first shoulder portion from the bump forming surface and a height Bha of the first bump from the bump forming surface satisfy the relationship of the following formula (4), and a height h1b of the second shoulder portion from the bump forming surface and a height Bhb of the second bump from the bump forming surface satisfy the relationship of the following formula (5). [h1a / Bha]≧0.20 Equation (4) [h1b / Bhb]≧0.20...Equation (5) [5] The semiconductor wafer with a protective film according to any one of the above [1] to [4], wherein the height BMh of the plurality of bumps from the bump-forming surface is 15 to 300 μm. [6] The semiconductor wafer with a protective film according to any one of the above [1] to [5], wherein the surface of the semiconductor wafer opposite to the surface on which the bumps are formed is a ground surface. [7] A semiconductor wafer with a protective film according to any one of the above [1] to [6], wherein grooves serving as planned division lines are formed on the bump formation surface so as not to reach the rear surface. [8] A semiconductor chip with a protective film, which is an individual product of the semiconductor wafer with a protective film according to any one of [1] to [7] above, a protective film (X) having the first bump, the second bump, the first shoulder, the second shoulder, and the valley; A semiconductor chip with a protective film, the semiconductor chip having a cut surface formed in a direction intersecting the bump formation surface. [9] A semiconductor chip with a protective film, which is an individual product of the semiconductor wafer with a protective film according to any one of [1] to [7] above, a cut surface formed in a direction intersecting the bump formation surface, A semiconductor chip with a protective film, in which a height h1a of the first shoulder portion from the bump-forming surface and a height h2' of a surface of the protective film (X) from the bump-forming surface at a position where the vertical cross section and the cut surface intersect satisfy the relationship of the following formula (6). 0.75≧[h2' / h1a]≧0...Equation (6)

[10] A method for protecting a semiconductor wafer having a bump-forming surface having a plurality of bumps, comprising: a step of attaching a curable resin film (x) of a composite sheet having a laminated structure of a curable resin film (x) and a release sheet (Y) so that the curable resin film (x) is in contact with the bump-forming surface, and pressing the release sheet (Y) toward the bump-forming surface with a pressing body, thereby covering the side surfaces of each bump included in the plurality of bumps, the surfaces located below the side surfaces, and the bump-forming surface with the curable resin film (x); and a step of curing the curable resin film (x) to form a protective film (X) containing a cured resin, The plurality of bumps include a first bump and a second bump adjacent to each other, When the first and second bumps are viewed in plan, in a vertical cross section passing through a circle including the center of the first bump and having a diameter that is 10% of the diameter of the first bump, and a circle including the center of the second bump and having a diameter that is 10% of the diameter of the second bump, the protective film (X) has a first shoulder portion that is a portion in contact with the first bump and is the farthest from the bump-forming surface, a second shoulder portion that is a portion in contact with the second bump and is the farthest from the bump-forming surface, and a valley portion located between the first shoulder portion and the second shoulder portion, A method for protecting a semiconductor wafer, wherein a height h1a of the first shoulder portion from the bump-forming surface, a height h1b of the second shoulder portion from the bump-forming surface, and a minimum height h2 of the valley portion from the bump-forming surface satisfy the relationship of the following formula (1): 0.75≧[h2 / {(h1a+h1b) / 2}]≧0...Equation (1)

[11] A method for producing a semiconductor wafer with a protective film according to any one of the above [1] to [7], comprising the following steps (S1) and (S2): Step (S1): A step of attaching a composite sheet having a laminated structure of a curable resin film (x) and a release sheet (Y) to the bump-forming surface while pressing the curable resin film (x) as an attachment surface. · Step (S2): Forming a protective film (X) containing a cured resin having the first shoulder portion, the second shoulder portion, and the valley portion by curing a curable resin film (x). A method for manufacturing a semiconductor wafer with a protective film, which includes this step.

[12] A composite sheet having a laminated structure of a release sheet (Y) and a curable resin film (x), which is used to form a protective film (X) on the bump formation surface of a semiconductor wafer having a plurality of bumps, and satisfies the following requirement (α). · Requirement (α): When the first bump and the second bump adjacent to each other among the plurality of bumps are viewed in plan view, in a vertical cross-section passing through a circle with a diameter of 10% of the maximum diameter of the first bump and including the center of the first bump, and a circle with a diameter of 10% of the maximum diameter of the second bump and including the center of the second bump, the protective film (X) has a first shoulder portion which is a portion in contact with the first bump and is the portion farthest from the bump formation surface, a second shoulder portion which is a portion in contact with the second bump and is the portion farthest from the bump formation surface, and a valley portion located between the first shoulder portion and the second shoulder portion. The height h1a of the first shoulder portion from the bump formation surface, the height h1b of the second shoulder portion from the bump formation surface, and the thickness dx of the curable resin film (x) satisfy the following formula (α1). 0 < dx / [(h1a + h1b) / 2] ≦ 0.70 ··· Formula (α1)

[13] A composite sheet having a laminated structure of a release sheet (Y) and a curable resin film (x), which is used to form a protective film (X) on the bump formation surface of a semiconductor wafer having a plurality of bumps, and satisfies the following requirement (β). · Requirement (β): The total thickness dc of the composite sheet and the thickness dx of the curable resin film (x) satisfy the following formula (β1). 0 < (dx / dc) ≦ 0.100 ··· Formula (β1)

[14] A composite sheet having a laminated structure of a release sheet (Y) and a curable resin film (x), It is used to form a protective film (X) on the bump formation surface of a semiconductor wafer having a plurality of bumps, A composite sheet that satisfies the following requirements (α) and (β). · Requirement (α): When the first bump and the second bump adjacent to each other among the plurality of bumps are viewed in plan view, within a circle having a diameter of 10% of the maximum diameter of the first bump and including the center of the first bump, and within a circle having a diameter of 10% of the maximum diameter of the second bump and including the center of the second bump, in a vertical cross-section passing through, the protective film (X) has a first shoulder portion that is a portion in contact with the first bump and is the portion farthest from the bump formation surface, a second shoulder portion that is a portion in contact with the second bump and is the portion farthest from the bump formation surface, and a valley portion located between the first shoulder portion and the second shoulder portion, The height h1a of the first shoulder portion from the bump formation surface, the height h1b of the second shoulder portion from the bump formation surface, and the thickness dx of the curable resin film (x) satisfy the following formula (α1). 0 < dx / [(h1a + h1b) / 2] ≦ 0.70 ··· Formula (α1) · Requirement (β): The total thickness dc of the composite sheet and the thickness dx of the curable resin film (x) satisfy the following formula (β1). 0 < [dx / dc] ≦ 0.100 ··· Formula (β1)

Advantages of the Invention

[0009] According to the present invention, it is possible to provide a semiconductor wafer with a protective film, a semiconductor chip with a protective film, a method for protecting a semiconductor wafer, a method for manufacturing a semiconductor wafer with a protective film, and a composite sheet in which the bumps are firmly protected regardless of environmental changes and the occurrence of warpage can be suppressed.

Brief Description of the Drawings

[0010] [Figure 1] It is a schematic diagram of a semiconductor wafer with a protective film according to an embodiment of the present invention. [Diagram 2] It is a schematic partial cross-sectional view showing an example of a semiconductor wafer with a protective film. [Diagram 3]1A to 1C are schematic diagrams illustrating examples of vertical cross sections that define shoulders and valleys of a protective film. [Figure 4] FIG. 11 is an explanatory diagram showing a procedure for setting a vertical cross section. [Diagram 5] 11 is a schematic partial cross-sectional view showing another example of a semiconductor wafer with a protective film. FIG. [Figure 6] 11 is a schematic partial cross-sectional view showing still another example of a semiconductor wafer with a protective film. FIG. [Figure 7] 11 is a schematic partial cross-sectional view showing still another example of a semiconductor wafer with a protective film. FIG. [Figure 8] 11 is a schematic partial cross-sectional view showing still another example of a semiconductor wafer with a protective film. FIG. [Figure 9] 11 is a schematic partial cross-sectional view showing still another example of a semiconductor wafer with a protective film. FIG. [Figure 10] 1 is a schematic diagram showing an example of a planned dividing line for a semiconductor wafer with a protective film; [Figure 11] 1 is a schematic cross-sectional view showing an example of a semiconductor chip with a protective film. [Figure 12] 11 is a schematic diagram showing another example of the planned dividing lines for the semiconductor wafer with a protective film. FIG. [Figure 13] 11 is a schematic cross-sectional view showing another example of a semiconductor chip with a protective film. FIG. [Figure 14] FIG. 2 is a schematic cross-sectional view showing an example of the configuration of a composite sheet. [Figure 15] 1A to 1C are explanatory views showing an example of a manufacturing process for a semiconductor wafer with a protective film. [Figure 16] 1A to 1C are explanatory views showing an example of a manufacturing process for a semiconductor wafer with a protective film. [Figure 17] 1A to 1C are explanatory views showing an example of a manufacturing process for a semiconductor wafer with a protective film. [Figure 18] 1A to 1C are explanatory views showing an example of a manufacturing process for a semiconductor wafer with a protective film. [Figure 19] 1A to 1C are explanatory views showing an example of a manufacturing process for a semiconductor wafer with a protective film. [Figure 20] 1 is an explanatory diagram of a method for measuring the shear properties of a semiconductor chip with a protective film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] In this specification, the term "active ingredient" refers to the components contained in the target composition excluding water and diluting solvents such as organic solvents. In addition, in this specification, "(meth)acrylic acid" refers to both "acrylic acid" and "methacrylic acid", and the same applies to other similar terms. In this specification, the weight average molecular weight and number average molecular weight are polystyrene equivalent values ​​measured by gel permeation chromatography (GPC). In this specification, the lower limit and upper limit described in stages for the preferred numerical range (e.g., the range of the content, etc.) can be independently combined. For example, the description "preferably 10 to 90, more preferably 30 to 60" can be combined with the "preferable lower limit (10)" and the "more preferable upper limit (60)" to form "10 to 60."

[0012] [Semiconductor wafer with protective film] A semiconductor wafer with a protective film according to an embodiment of the present invention includes a semiconductor wafer having a bump-forming surface having a plurality of bumps, and a protective film (X) including a cured resin that covers the side surfaces and surfaces located below the side surfaces of each of the bumps included in the plurality of bumps, as well as the bump-forming surface, the plurality of bumps include a first bump and a second bump adjacent to each other, and when the first and second bumps are viewed in plan, a circle including the center of the first bump and having a diameter that is 10% of the maximum diameter of the first bump and a circle including the center of the second bump and having a diameter that is 10% of the maximum diameter of the second bump are formed on the semiconductor wafer with a protective film (X). In a vertical cross section passing through a circle having a diameter that is 10% of the maximum diameter of the bump, the protective film (X) has a first shoulder that contacts the first bump and is the farthest from the bump-forming surface, a second shoulder that contacts the second bump and is the farthest from the bump-forming surface, and a valley located between the first shoulder and the second shoulder, and a height h1a of the first shoulder from the bump-forming surface, a height h1b of the second shoulder from the bump-forming surface, and a minimum height h2 of the valley from the bump-forming surface satisfy the relationship of the following formula (1). 0.75≧[h2 / {(h1a+h1b) / 2}]≧0...Equation (1) If the arithmetic average value of h1a and h1b is h1, the above formula (1) can be expressed as follows. 0.75≧[h2 / h1]≧0...Equation (1) In the following description, h1 may be referred to as the "average height of the shoulder."

[0013] In the semiconductor wafer with protective film, the protective film (X) between two adjacent bumps satisfies the relationship of formula (1) above, and thus the shear strength of the bumps is improved and the decrease in the shear strength is suppressed even when the bumps are subjected to environmental changes such as temperature rise, so that the bumps are strongly protected regardless of environmental changes. In addition, the protective film (X) satisfies the relationship of formula (1) above, so that the total amount of the protective film (X) on the semiconductor wafer can be reduced, and thus the occurrence of warpage in the semiconductor wafer with protective film is suppressed. Since the warpage of the semiconductor wafer with the protective film is small, it is easy to subject it to a fully automated manufacturing process, thereby increasing productivity. Furthermore, since the amount of the resin composition used to form the protective film (X) is small, the cost is reduced and it is possible to provide a semiconductor wafer with a protective film which is environmentally friendly.

[0014] In the following, the "height h1a of the first shoulder from the bump forming surface" may be referred to as the "height h1a of the first shoulder," the "height h1b of the second shoulder from the bump forming surface" may be referred to as the "height h1b of the second shoulder," and the "minimum height h2 of the valley from the bump forming surface" may be referred to as the "height h2 of the valley." The "position farthest from the bump-forming surface" for defining each of the above shoulders is determined within the region where the protective film (X) formed on the bump-forming surface is continuously present. Therefore, for example, the "position farthest from the bump-forming surface" is not determined from the contact portion between the protective film (X) and the bump, which is partially present on the top of the bump and is removed by the exposure process (plasma etching process) described later.

[0015] FIG. 1 is a schematic diagram showing an example of a semiconductor wafer with a protective film according to an embodiment of the present invention, where FIG. 1(a) is a plan view and FIG. 1(b) is a cross-sectional view taken along line IB-IB in FIG. 1(a). 1 has a semiconductor wafer 41. The semiconductor wafer 41 has a bump-forming surface 41a on which a plurality of bumps BM are regularly formed. A protective film (X) containing a cured resin is formed on the bump formation surface 41a. The protective film (X) is provided so as to cover the side surfaces of each bump BM, the surfaces positioned below the side surfaces, and the bump formation surface 41a.

[0016] <Semiconductor wafer> The semiconductor wafer will be described below. In the following description, a "semiconductor wafer having bumps" will also be referred to as a "wafer with bumps." Also, a "semiconductor wafer" will also be referred to simply as a "wafer."

[0017] The wafer 41 has circuits such as wiring, capacitors, diodes, and transistors formed on the surface thereof. The material of the wafer is not particularly limited, and examples thereof include a silicon wafer, a silicon carbide wafer, a compound semiconductor wafer, a sapphire wafer, and a glass wafer.

[0018] The size of wafer 41 is not particularly limited, but from the viewpoint of improving batch processing efficiency, it is usually 8 inches (diameter 200 mm) or more, and preferably 12 inches (diameter 300 mm) or more. The shape of the wafer is not limited to a circle, and may be a polygonal shape such as a square or a rectangle. In the case of a polygonal wafer, the size of wafer 41 is preferably such that the length of the longest side is equal to or greater than the above size (diameter), from the viewpoint of improving batch processing efficiency.

[0019] The thickness of the wafer 41 is not particularly limited, but from the viewpoint of easily suppressing warping of the wafer 41 caused by curing the curable resin film (x), it is preferably 100 μm to 1,000 μm, more preferably 200 μm to 900 μm, and even more preferably 300 μm to 800 μm.

[0020] The shape of the bump BM is not particularly limited, and may be any shape as long as it can be fixed in contact with an electrode or the like on a chip mounting substrate. For example, although the bump BM is ball-shaped in Fig. 1, the bump BM may be a spheroid. The spheroid may be, for example, a spheroid stretched in a direction perpendicular to the bump formation surface 41a of the wafer 41, or a spheroid stretched in a direction horizontal to the bump formation surface 41a of the wafer 41. Moreover, the bump BM may be in a pillar shape. The bumps BM may be made of, for example, solder.

[0021] From the viewpoint of ensuring reliable connection to the wiring board, the height BMh of the plurality of bumps from the bump-forming surface is preferably 15 to 300 μm, more preferably 18 to 280 μm, and even more preferably 20 to 260 μm. The bump height BMh can be measured, for example, by observing, with an optical microscope, a cross section of a bumped semiconductor wafer cut in a direction perpendicular to the bump-formed surface and passing through the center of the bump.

[0022] The bump height BMh means, when focusing on one bump, the straight line distance between the contact point of the bump with the bump-forming surface and the part of the bump that is located farthest from the bump-forming surface. The bump height BMh can be measured, for example, by cutting a semiconductor wafer with a protective film (X) in a direction perpendicular to the bump-forming surface and passing through the center of the bump, and observing the cut cross section with an optical microscope.

[0023] <Protective film (X)> The protective film (X) contains a cured resin obtained by curing a curable resin film. The shape of the protective film (X) will be described below with reference to a cross-sectional view of a semiconductor wafer with the protective film. The material of the protective film (X) will be described later.

[0024] FIG. 2 is a schematic cross-sectional view showing an example of a semiconductor wafer with a protective film, and is a partially enlarged view. In a semiconductor wafer 50A with a protective film shown in FIG. 2, a bump formation surface 41a of the semiconductor wafer 41 is provided with a plurality of bumps BM including a first bump BMa and a second bump BMb adjacent to each other. The protective film (X) on the bump forming surface 41a between the first bump BMa and the second bump BMb has a first shoulder portion XSa which is in contact with the first bump BMa and is the farthest position from the bump forming surface 41a, a second shoulder portion XSb which is in contact with the second bump BMb and is the farthest position from the bump forming surface 41a, and a valley portion XV which is located between the first shoulder portion XSa and the second shoulder portion XSb. The first shoulder height h1a, the second shoulder height h1b, and the minimum height h2 of the valley satisfy the relationship of the above formula (1). The arithmetic mean value of the first shoulder height h1a and the second shoulder height h1b is also referred to as the "shoulder height h1." In the following description, the height of each shoulder, the height of each valley, the length of the region including the valley, etc. of the protective film (X) are all values ​​measured at 23°C.

[0025] FIG. 3 is a schematic diagram showing an example of a vertical cross section that defines the shoulder and valley of the protective film (X). In Fig. 3, nine bumps BMa1 to BMa3, BMb1 to BMb3, and BMc1 to BMc3 are arranged at equal intervals along the left-right direction (horizontal direction) and the up-down direction (vertical direction) of Fig. 3. As shown in Fig. 3, the vertical cross section defining the shoulder and valley of the protective film (X) may be any of a vertical cross section along a straight line CS1 that is parallel to the horizontal direction and passes through each bump, a vertical cross section along a straight line CS2 that is parallel to the vertical direction and passes through each bump, and a vertical cross section along a straight line CS3 that is obliquely intersecting the horizontal and vertical directions and passes through each bump.

[0026] From the viewpoint of easily preventing the height of the valleys from increasing, it is preferable that the relationship of the above formula (1) is satisfied in a vertical cross section along the direction in which the inter-bump distance is smallest. In the example shown in Fig. 3, the inter-bump distance w1 in the horizontal direction and the inter-bump distance w2 in the vertical direction are equal and smaller than the inter-bump distance w3 in the diagonal direction, so it is preferable that the relationship of the above formula (1) is satisfied in a vertical cross section along the straight line CS1 or straight line CS2. From the viewpoint of making it easier to prevent warpage of the wafer, the relationship of formula (1) above may be satisfied in vertical cross sections along all of the straight lines CS1, CS2, and CS3.

[0027] From the viewpoint of making it easier to prevent warpage of the wafer, the ratio of the number of the points of the protective film (X) that satisfy the relationship of the above formula (1) to the total number of points located between two adjacent bumps is preferably 50% or more, more preferably 60% or more, and even more preferably 70% or more. In the example of Fig. 3, the standard for the ratio of the number of the points that satisfy the relationship of the above formula (1) is 20, which is the total number of each point shown below. Between BMa1 and BMa2, between BMa2 and BMa3, Between BMb1 and BMb2, between BMb2 and BMb3, Between BMc1 and BMc2, between BMc2 and BMc3, Between BMa1 and BMb1, between BMa2 and BMb2, between BMa3 and BMb3, between BMb1 and BMc1, between BMb2 and BMc2, between BMb3 and BMc3, Between BMa1 and BMb2, between BMb2 and BMc3, Between BMa3 and BMb2, between BMb2 and BMc1, Between BMa2 and BMb1, between BMa2 and BMb3, and Between BMb1 and BMc2, between BMb3 and BMc2, The upper limit of the above ratio is not particularly limited and may be 100%, but from the viewpoint of ease of production, it can be, for example, 99% or less. In other words, it is preferably 50% to 100%, and more preferably 50% to 99%.

[0028] FIG. 4 is an explanatory diagram showing a procedure for setting a vertical cross section that defines the shoulder and valley of the protective film (X), and is an explanatory diagram when the semiconductor wafer with the protective film shown in FIG. 2 is taken as an example. The above-mentioned vertical cross section can be defined as a cross section obtained by cutting the semiconductor wafer perpendicularly so as to pass through the center BCa of the bump BMa and the center BCb of the bump BMb when each of the adjacent bumps BMa, BMb is viewed in a plane, as shown in FIG. Here, the vertical cross section does not necessarily have to pass through the centers of the two bumps, but only needs to pass through a circle Ca having a diameter that is 10% of the maximum diameter of the first bump BMa and having the same center as the center BCa of the first bump, and a circle Cb having a diameter that is 10% of the maximum diameter of the second bump BMb and having the same center as the center BCb of the second bump, when the first bump BMa and the second bump BMb are viewed in a plane.

[0029] From the viewpoint of reducing the amount of resin constituting the protective film (X), the value of [h2 / {(h1a+h1b) / 2}] is preferably 0.60 or less, more preferably 0.57 or less, even more preferably 0.55 or less, still more preferably 0.53 or less, still more preferably 0.50, still more preferably 0.48 or less, and particularly preferably 0.46 or less. In other words, it preferably satisfies the following relationship (1'). 0.60≧[h2 / {(h1a+h1b) / 2}]≧0...Equation (1')

[0030] It is preferable that the minimum height h2 of the valley portion from the bump-forming surface, the height BMha of the first bump from the bump-forming surface, and the height BMhb of the second bump from the bump-forming surface satisfy the relationship of the following formula (2). 0.37≧[h2 / {(BMha+BMhb) / 2}]≧0...Equation (2) By satisfying the above relationship, it becomes easier to form a valley portion having a height sufficiently smaller than the height of the shoulder portion.

[0031] From the viewpoint of easily suppressing warpage of the semiconductor wafer with a protective film, the value of [h2 / {(BMha+BMhb) / 2}] is preferably 0.30 or less, more preferably 0.29 or less, more preferably 0.28 or less, and even more preferably 0.27 or less. In other words, it preferably satisfies the following relationship (2'). 0.30≧[h2 / {(Bha+Bhb) / 2}]≧0...Equation (2')

[0032] From the standpoint of making it easier to form a valley portion, it is preferable that in the vertical cross section, the length L in a direction along the bump forming surface of a region of the valley portion having a height that is 80% or less of the arithmetic mean value h1 of the height h1a of the first shoulder portion from the bump forming surface and the height h1b of the second shoulder portion from the bump forming surface, and the distance w between the first bump and the second bump in the vertical cross section satisfy the relationship of the following formula (3). 0.90≧[L / w]≧0...Equation (3) L / g more preferably satisfies the following formula (3-1), and even more preferably satisfies the following formula (3-2). 0.75≧[L / w]≧0...Equation (3-1) 0.60≧[L / w]≧0...Equation (3-2)

[0033] From the standpoint of making it easier to ensure the protective performance of the bump, it is preferable that the height h1a of the first shoulder portion from the bump forming surface and the height Bha of the first bump from the bump forming surface satisfy the relationship of the following formula (4), and that the height h1b of the second shoulder portion from the bump forming surface and the height Bhb of the second bump from the bump forming surface satisfy the relationship of the following formula (5). [h1a / Bha]≧0.20 Equation (4) [h1b / Bhb]≧0.20...Equation (5) Each of [h1a / Bha] and [h1b / Bhb] is more preferably 0.30 or more, even more preferably 0.40 or more, and still more preferably 0.50 or more. The upper limit values ​​of [h1a / Bha] and [h1b / Bhb] are not particularly limited, but from the viewpoint of easily exposing the bump top from the protective film (X), they are preferably 1.0 or less, more preferably less than 1.0, even more preferably 0.90 or less, and even more preferably 0.80 or less. In other words, [h1a / Bha] and [h1b / Bhb] are preferably 0.30 to 1.0.

[0034] The surface (back surface) of the semiconductor wafer opposite to the bump-forming surface may be a ground surface. Grinding the back surface of the semiconductor wafer makes the semiconductor wafer thinner, thereby enabling the semiconductor wafer with a protective film to be miniaturized. On the other hand, the semiconductor wafer with a protective film becomes more prone to warping as the electronic components become thinner, but the occurrence of warping can be suppressed by having the first shoulder portion XSa and second shoulder portion XSb and the valley portion XV of the protective film (X) satisfy the relationship of formula (1) above.

[0035] In order to facilitate the division of the semiconductor wafer, grooves serving as division lines may be formed on the bump-forming surface so as not to reach the rear surface. By providing the grooves, warping of the semiconductor wafer with the protective film can be easily suppressed.

[0036] 5 to 9 are schematic partial cross-sectional views showing other examples of a semiconductor wafer with a protective film. In the semiconductor wafer 50B with protective film shown in Fig. 5, the minimum height h2 of the valley portion XV is zero (h2 = 0), that is, the bottom surface of the valley portion reaches the bump formation surface 41a. This allows the amount of resin constituting the protective film (X) to be reduced. In addition, since the protective film (X) satisfies the above formula (1), the bump neck of each bump is sufficiently protected. In addition, when the minimum height h2 of the valley is 0, the average height h1 of the shoulder is preferably 50 μm or more, more preferably 55 μm or more, even more preferably 60 μm or more, and even more preferably 65 μm or more, from the viewpoint of sufficiently ensuring the protection performance of the bump. There is no upper limit, but from the viewpoint of ease of manufacture, it is, for example, 85 μm. In other words, when the minimum height h2 of the valley is 0, the average height h1 of the shoulder is preferably 50 to 85 μm.

[0037] In the semiconductor wafer 50C with a protective film shown in FIG. 6, the shape of the protective film (X) in the vertical cross section is linear in both the region from the first shoulder portion XSa to the deepest part of the valley portion XV and the region from the second shoulder portion XSb to the deepest part of the valley portion XV. In the semiconductor wafer 50C with a protective film, the vicinity of the bump neck is protected by the pyramidal protective film (X), so that the protective performance of the bumps BMa, BMb can be easily improved.

[0038] In the semiconductor wafer 50D with a protective film shown in FIG. 7, the shape of the protective film (X) in the vertical cross section is such that the region from the first shoulder portion XSa to the valley portion XV and the region from the second shoulder portion XSb to the valley portion XV are both curved, and the valley portion XV is a straight line of uniform height. In the semiconductor wafer 50D with a protective film, since there are regions where the thickness of the protective layer (X) is constant, it is generally easy to achieve the intended physical properties and to suppress the amount of warpage within a desired range. Such a shape is likely to occur when the distance between the first bump BMa and the second bump BMb is large.

[0039] In the semiconductor wafer 50E with a protective film shown in FIG. 8, the region from the first shoulder portion XSa to the valley portion XV and the region from the second shoulder portion XSb to the valley portion XV are both linear, and the valley portion XV is also linear and of uniform height. The semiconductor wafer 50E with a protective film has the same advantages as the semiconductor wafer 50D with a protective film described above.

[0040] 9, grooves 41c are formed along the intended dividing lines without reaching the rear surface 41b on the bump-forming surface 41a of the semiconductor wafer 41. Valleys XV of the protective film (X) are formed at positions overlapping the grooves 41c in a direction perpendicular to the bump-forming surface 41a. By forming the groove portion 41c in the semiconductor wafer 41, the protective film (X) satisfies the relationship of formula (1), and in addition, the effect of shrinkage caused by the hardening of the curable resin film (x) can be mitigated to some extent on the wafer side, which is advantageous in reducing the amount of warping. When the above-mentioned groove portion is provided in the semiconductor wafer, the minimum height h2 of the valley portion means the height from an imaginary plane obtained by extending the bump formation surface onto the valley portion.

[0041] [Semiconductor chip with protective film] A first semiconductor chip with a protective film according to an embodiment of the present invention is an individualized product of any of the semiconductor wafers with a protective film described above, and has a protective film (X) having the first bump and the second bump, as well as the first shoulder portion, the second shoulder portion, and the valley portion, and has a cut surface formed in a direction intersecting the bump formation surface.

[0042] Fig. 10 is a schematic diagram showing an example of a division line of a semiconductor wafer with a protective film, and Fig. 11 is a schematic cross-sectional view showing an example of a semiconductor chip, which corresponds to a partial cross-sectional view taken along line X'-X' in Fig. 10. In the example shown in Fig. 10, the protective film-equipped semiconductor wafer 50 is diced along the planned division lines DL that are set so that the protective film-equipped semiconductor chips obtained after dicing include a plurality of bumps BM. This results in a protective film-equipped semiconductor chip CP1 having the configuration shown in Fig. 11. The semiconductor chip CP1 with a protective film has a first bump BMa and a second bump BMb, as well as a protective film (X) having a first shoulder portion XSa, a second shoulder portion XSb, and a valley portion XY, and has a cut surface CF formed in a direction perpendicular to the bump formation surface 41a.

[0043] In the semiconductor wafer CP1 with a protective film, the protective film (X) between two adjacent bumps BMa and BMb satisfies the relationship of the above formula (1), thereby improving the shear strength of each bump BMa and BMb and firmly protecting the bumps regardless of environmental changes. In addition, the protective film (X) satisfies the relationship of the above formula (1), so that the total amount of the protective film (X) on the semiconductor wafer can be reduced.

[0044] A second semiconductor chip with a protective film according to an embodiment of the present invention is an individual product of any one of the above-mentioned semiconductor wafers with a protective film, a cut surface formed in a direction intersecting the bump formation surface, A height h1a of the first shoulder portion from the bump-forming surface and a height h2' of the surface of the protective film (X) from the bump-forming surface at a position where the vertical cross section and the cut surface intersect satisfy the relationship of the following formula (6). 0.75≧[h2' / h1a]≧0...Equation (6)

[0045] Fig. 12 is a schematic diagram showing another example of the division lines of a semiconductor wafer with a protective film, and Fig. 13 is a schematic cross-sectional view showing an example of a semiconductor chip, which corresponds to a partial cross-sectional view taken along line XIII-XIII in Fig. 12. In the example shown in Fig. 12, the semiconductor wafer 50 with the protective film is diced along the planned division lines DL that are set so that one bump BMa is included in the semiconductor chip with the protective film obtained after dicing. This results in a semiconductor chip CP2 with the protective film having the configuration shown in Fig. 13. The semiconductor chip CP2 with a protective film has a first bump BMa, and in a vertical cross section passing through the center of the first bump BMa when the first bump BMa is viewed in a plan view, the semiconductor chip CP2 with a protective film has a protective film (X) having a first shoulder XSa, and has a cut surface CF formed in a direction perpendicular to the bump-forming surface 41a. The protective film (X) of the semiconductor chip CP2 with a protective film decreases in thickness toward the cut surface CF in the vertical cross section, and has a minimum height h2' from the bump-forming surface at the position where the vertical cross section and the cut surface CF intersect.

[0046] In the semiconductor wafer CP2 with a protective film, the protective film (X) satisfies the relationship of the above formula (6). This improves the shear strength of the first bump BMa, and the bump is strongly protected regardless of environmental changes. In addition, since the protective film (X) satisfies the relationship of the above formula (6), the total amount of the protective film (X) on the semiconductor wafer can be reduced.

[0047] [Method of protecting semiconductor wafers] A method for protecting a semiconductor wafer according to an embodiment of the present invention is a method for protecting a semiconductor wafer having a bump-forming surface having a plurality of bumps, comprising the steps of: a step of attaching a curable resin film (x) of a composite sheet having a laminated structure of a curable resin film (x) and a release sheet (Y) so that the curable resin film (x) is in contact with the bump-forming surface, and pressing the release sheet (Y) toward the bump-forming surface with a pressing body, thereby covering the side surfaces of each bump included in the plurality of bumps, the surfaces located below the side surfaces, and the bump-forming surface with the curable resin film (x); and a step of curing the curable resin film (x) to form a protective film (X) containing a cured resin, The plurality of bumps include a first bump and a second bump adjacent to each other, When the first and second bumps are viewed in plan, in a vertical cross section passing within a circle that includes the center of the first bump and has a diameter that is 10% of the diameter of the first bump, and within a circle that includes the center of the second bump and has a diameter that is 10% of the diameter of the second bump, the protective film (X) has a first shoulder that is a portion that contacts the first bump and is the farthest from the bump-forming surface, a second shoulder that is a portion that contacts the second bump and is the farthest from the bump-forming surface, and a valley that is located between the first shoulder and the second shoulder, A height h1a of the first shoulder portion from the bump-forming surface, a height h1b of the second shoulder portion from the bump-forming surface, and a minimum height h2 of the valley portion from the bump-forming surface satisfy the relationship of the following formula (1). 0.75≧[h2 / {(h1a+h1b) / 2}]≧0...Equation (1)

[0048] According to the above semiconductor wafer protection method, the protective film (X) between two adjacent bumps satisfies the relationship of the above formula (1), thereby improving the shear strength of the bumps and suppressing the decrease in the shear strength even when subjected to environmental changes such as temperature rise, so that the bumps are strongly protected regardless of environmental changes. In addition, since the protective film (X) satisfies the relationship of the above formula (1), the total amount of the protective film (X) on the semiconductor wafer can be reduced, and the occurrence of warpage is suppressed in the semiconductor wafer with the protective film. Since the warpage of the semiconductor wafer with the protective film is small, it is easy to subject it to a fully automated manufacturing process, thereby increasing productivity. Furthermore, since the amount of the resin composition used to form the protective film (X) is small, costs can be reduced, and it is possible to provide a semiconductor wafer with a protective film that is environmentally friendly.

[0049] [Method of manufacturing semiconductor wafer with protective film] The method for producing a semiconductor wafer with a protective film according to the embodiment of the present invention is carried out by using the above-mentioned composite sheet. Specifically, it includes the following steps (S1) and (S2). Step (S1): A step of attaching a composite sheet having a laminated structure of a curable resin film (x) and a release sheet (Y) to a bump-forming surface of a semiconductor wafer having a bump-forming surface on which a plurality of bumps are provided, while pressing the composite sheet against the bump-forming surface of the semiconductor wafer with the curable resin film (x) as an attachment surface. Step (S2): A step of forming a protective film (X) containing a cured resin having the first shoulder portion, the second shoulder portion, and the valley portion by curing the curable resin film (x). The composite sheet will be described first, and then each of the steps will be described.

[0050] [Composite sheet] The composite sheet used for forming the protective film (X) on the bump-forming surface of the electronic component will be described below. The composite sheet has a laminated structure of a curable resin film (x) and a release sheet (Y).

[0051] The above composite sheet preferably satisfies the following requirement (α), from the viewpoint of facilitating the formation of valleys having a height sufficiently lower than the height of the shoulders of the protective film (X). ·Requirement (α): When the first bump and the second bump adjacent to each other among the plurality of bumps are viewed in plan view, within a circle having a diameter of 10% of the maximum diameter of the first bump and including the center of the first bump, and within a circle having a diameter of 10% of the maximum diameter of the second bump and including the center of the second bump, in a vertical cross-section passing through, the protective film (X) has a first shoulder portion which is a portion in contact with the first bump and is the portion farthest from the bump formation surface, a second shoulder portion which is a portion in contact with the second bump and is the portion farthest from the bump formation surface, and a valley portion located between the first shoulder portion and the second shoulder portion. The height h1a of the first shoulder portion from the bump formation surface, the height h1b of the second shoulder portion from the bump formation surface, and the thickness dx of the curable resin film (x) satisfy the following formula (α1). 0 < dx / [(h1a + h1b) / 2] ≦ 0.70 ··· Formula (α1) Since (h1a + h1b) / 2 = h1, formula (α1) can also be expressed as follows. 0 < [dx / h1] ≦ 0.70 ··· Formula (α1)

[0052] In the above requirement (α), from the viewpoint of making it easier to form a valley portion having a height sufficiently lower than the height of the shoulder portion of the protective film (X), it is more preferable to satisfy the following formula (α2), and it is even more preferable to satisfy the following formula (α3). 0 < dx / [(h1a + h1b) / 2] ≦ 0.50 ··· Formula (α2) 0 < dx / [(h1a + h1b) / 2] ≦ 0.40 ··· Formula (α3) Incidentally, formulas (α2) and (α3) can also be expressed as follows. 0 < [dx / h1] ≦ 0.50 ··· Formula (α2) 0 < [dx / h1] ≦ 0.40 ··· Formula (α3)

[0053] From the viewpoint of making it easier to form a valley portion having a height sufficiently lower than the height of the shoulder portion of the protective film (X) in the above composite sheet, it is preferable to satisfy the following requirement (β). Requirement (β): The thickness dc of the entire composite sheet and the thickness dx of the curable resin film (x) satisfy the following formula (β1). 0<[dx / dc]≦0.100...Formula (β1)

[0054] In terms of the above requirement (β), from the viewpoint of making it easier to form valleys having a height sufficiently lower than the height of the shoulders of the protective film (X), it is more preferable that the following formula (β2) is satisfied, and it is even more preferable that the following formula (β3) is satisfied. 0<[dx / dc]≦0.080...Formula (β2) 0<[dx / dc]≦0.060...Formula (β3)

[0055] The above composite sheet preferably satisfies the above requirements (α) and (β) from the viewpoint of making it easier to form valleys having a height sufficiently lower than the height of the shoulders of the protective film (X).

[0056] <Composition of the composite sheet> An example of the structure of the above composite sheet is shown in FIG. FIG. 14 is a schematic cross-sectional view showing an example of the configuration of a composite sheet. The composite sheets 1a and 1b shown in FIG. 14(a) and FIG. 14(b) have a curable resin film (x) on one side of a release sheet (Y). By providing the curable resin film (x) on one side of the release sheet (Y), the curable resin film (x) is stably supported and protected when the curable resin film (x) is transported as a product package or when the curable resin film (x) is conveyed in a process. In FIG. 14, the symbol dx indicates the thickness of the curable resin film (x), and the symbol dc indicates the thickness of the entire composite sheet.

[0057] In the composite sheet 1a shown in FIG. 14(a), the release sheet (Y) is the substrate 11, and the substrate 11 is provided with a curable resin film (x) on one surface thereof. In the composite sheet 1a, the release sheet (Y) is an adhesive sheet in which a substrate 11 and a release layer 21 are laminated together, and the release layer 21 of the adhesive sheet is attached to the curable resin film (x).

[0058] The composite sheet 1b is an adhesive sheet in which a release sheet (Y) is laminated with a base material 11, an intermediate layer 31, and a release layer 21 in this order, and the release layer 21 of the adhesive sheet is laminated with a curable resin film (x). The adhesive sheet in which a base material 11, an intermediate layer 31, and a release layer 21 are laminated with each other in this order can be suitably used as a backgrind tape. That is, the composite sheet 1b shown in FIG. 14(b) has a backgrind tape as a release sheet (Y), and therefore can be suitably used when the curable resin film (x) of the composite sheet 1b is laminated with a bump-formed surface of a semiconductor wafer having a plurality of bumps, and then the surface of the semiconductor wafer opposite to the bump-formed surface is ground to thin the semiconductor wafer.

[0059] The composite sheets 1a and 1b include, in addition to the curable resin film (x), a release layer 21, or a release sheet (Y) including the release layer 21 and an intermediate layer 31. By including the release layer 21, or the release layer 21 and an intermediate layer 31, the release sheet (Y) has an appropriate degree of flexibility and can ensure a predetermined thickness that allows the curable resin film (x) to be embedded between a plurality of bumps when the composite sheets 1a and 1b are attached to the bump-forming surface of a semiconductor wafer.

[0060] The curable resin film (x) and the release sheet (Y) used in the composite sheet will be described below.

[0061] <Curable resin film (x)> The curable resin film (x) is a film for protecting the bump formation surface of a semiconductor wafer having a plurality of bumps, and forms a protective film (X) by curing through heating or energy ray irradiation. That is, the curable resin film (x) may be a thermosetting resin film (x1) that is cured by heating, or an energy ray curable resin film (x2) that is cured by energy ray irradiation. In this specification, the term "energy rays" refers to electromagnetic waves or charged particle beams that have an energy quantum. Examples of such beams include ultraviolet rays and electron beams, and preferably ultraviolet rays.

[0062] The physical properties of the curable resin film (x) can be adjusted by adjusting either or both of the types and amounts of the components contained in the curable resin film (x).

[0063] The thermosetting resin film (x1) and the energy ray-curable resin film (x2) will be described below.

[0064] (Thermosetting resin film (x1)) The thermosetting resin film (x1) of this embodiment forms a cured resin film by being cured by heating. The thermosetting resin film of the present embodiment contains a polymer component (A) and a thermosetting component (B). The thermosetting resin film (x1) of the present embodiment is formed, for example, from a thermosetting resin composition (x1-1) containing the polymer component (A) and the thermosetting component (B). The polymer component (A) is a component that can be considered to be formed by a polymerization reaction of a polymerizable compound. The thermosetting component (B) is a component that can undergo a curing (polymerization) reaction when triggered by heat. The curing (polymerization) reaction also includes a polycondensation reaction.

[0065] (Polymer component (A)) The thermosetting resin film (x1) and the thermosetting resin composition (x1-1) contain a polymer component (A). The polymer component (A) is a polymer compound for imparting film-forming properties, flexibility, etc. to the thermosetting resin film (x1). The polymer component (A) may be used alone or in combination of two or more. When two or more types of the polymer component (A) are used in combination, the combination and ratio thereof can be selected arbitrarily.

[0066] Examples of the polymer component (A) include acrylic resins, polyarylate resins, polyvinyl acetal, polyesters, urethane resins (resins having urethane bonds), acrylic urethane resins, silicone resins (resins having siloxane bonds), rubber resins (resins having a rubber structure), phenoxy resins, and thermosetting polyimides. Among these, acrylic resins, polyarylate resins, and polyvinyl acetals are preferred.

[0067] The acrylic resin may be a known acrylic polymer. The weight average molecular weight (Mw) of the acrylic resin is preferably from 10,000 to 2,000,000, more preferably from 300,000 to 1,500,000, and further preferably from 500,000 to 1,000,000. When the weight-average molecular weight of the acrylic resin is equal to or greater than the lower limit, the shape stability (stability over time during storage) of the thermosetting resin film (x1) is easily improved. Also, when the weight-average molecular weight of the acrylic resin is equal to or less than the upper limit, the thermosetting resin film (x1) is easily adapted to the uneven surface of the adherend, and for example, the occurrence of voids between the adherend and the thermosetting resin film is easily suppressed. Therefore, the covering property of the bump-forming surface of the semiconductor wafer is improved, and the embedding property in the grooves is also easily improved.

[0068] The glass transition temperature (Tg) of the acrylic resin is preferably from -60 to 70°C, more preferably from -40 to 50°C, and even more preferably from -30 to 30°C, from the viewpoint of application and handling of the thermosetting resin film (x1).

[0069] Examples of acrylic resins include polymers of one or more (meth)acrylic acid esters; copolymers of two or more monomers selected from (meth)acrylic acid, itaconic acid, vinyl acetate, acrylonitrile, styrene, and N-methylolacrylamide.

[0070] Examples of the (meth)acrylic acid ester constituting the acrylic resin include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, n-octyl (meth)acrylate, n-nonyl (meth)acrylate, and (meth)acrylic acid alkyl esters in which the alkyl group constituting the alkyl ester has a chain structure having 1 to 18 carbon atoms, such as isononyl acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate (lauryl (meth)acrylate), tridecyl (meth)acrylate, tetradecyl (meth)acrylate (myristyl (meth)acrylate), pentadecyl (meth)acrylate, hexadecyl (meth)acrylate (palmityl (meth)acrylate), heptadecyl (meth)acrylate, and octadecyl (meth)acrylate (stearyl (meth)acrylate); (meth)acrylic acid cycloalkyl esters such as isobornyl (meth)acrylate and dicyclopentanyl (meth)acrylate; (Meth)acrylic acid aralkyl esters such as benzyl (meth)acrylate; (Meth)acrylic acid cycloalkenyl esters such as (meth)acrylic acid dicyclopentenyl ester; (Meth)acrylic acid cycloalkenyloxyalkyl esters such as (meth)acrylic acid dicyclopentenyloxyethyl ester; (Meth)acrylic acid imide; glycidyl group-containing (meth)acrylic acid esters such as glycidyl (meth)acrylate; hydroxyl group-containing (meth)acrylic acid esters such as hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; Examples of such esters include (meth)acrylic acid esters containing a substituted amino group, such as N-methylaminoethyl (meth)acrylate. In this specification, the term "substituted amino group" refers to an amino group in which one or two hydrogen atoms have been replaced with a group other than a hydrogen atom. Among these, from the viewpoint of the film-forming properties of the thermosetting resin film (x1) and the attachability of the thermosetting resin film (x1) to the protective film-forming surface of the semiconductor chip, it is preferable that the alkyl group constituting the alkyl ester is a copolymer of a combination of a (meth)acrylic acid alkyl ester, a glycidyl group-containing (meth)acrylic acid ester, and a hydroxyl group-containing (meth)acrylic acid ester, each of which has a chain structure containing 1 to 18 carbon atoms; it is more preferable that the alkyl group constituting the alkyl ester is a copolymer of a combination of a (meth)acrylic acid alkyl ester, a glycidyl group-containing (meth)acrylic acid ester, and a hydroxyl group-containing (meth)acrylic acid ester, each of which has a chain structure containing 1 to 4 carbon atoms; and it is even ... copolymer is a combination of butyl acrylate, methyl acrylate, glycidyl acrylate, and 2-hydroxyethyl acrylate.

[0071] The acrylic resin may be, for example, a copolymer of one or more monomers selected from (meth)acrylic acid ester, (meth)acrylic acid, itaconic acid, vinyl acetate, acrylonitrile, styrene, N-methylolacrylamide, and the like.

[0072] The monomer constituting the acrylic resin may be used alone or in combination of two or more. When the monomer constituting the acrylic resin is two or more, the combination and ratio thereof can be selected arbitrarily.

[0073] The polyarylate resin in the polymer component (A) may be any known one, such as a resin having a basic structure formed by polycondensation of a dihydric phenol with a dibasic acid such as phthalic acid or carboxylic acid. Among these, a polycondensate of bisphenol A with phthalic acid, poly(4,4'-isopropylidenediphenylene terephthalate) / isophthalate copolymer, or derivatives thereof are preferred.

[0074] The polyvinyl acetal in the polymer component (A) may be any of the known polyvinyl acetals. Among them, preferred polyvinyl acetals include, for example, polyvinyl formal and polyvinyl butyral, with polyvinyl butyral being more preferred. Examples of polyvinyl butyral include those having structural units represented by the following formulas (i)-1, (i)-2, and (i)-3.

[0075] [ka]

[0076] (In the formula, l, m, and n each independently represent an integer of 1 or more.)

[0077] The weight-average molecular weight (Mw) of the polyvinyl acetal is preferably 5,000 to 200,000, more preferably 8,000 to 100,000. When the weight-average molecular weight of the polyvinyl acetal is equal to or greater than the above lower limit, the shape stability (stability over time during storage) of the thermosetting resin film (x1) is easily improved. When the weight-average molecular weight of the polyvinyl acetal is equal to or less than the above upper limit, the thermosetting resin film (x1) is easily adapted to the uneven surface of the adherend, and for example, the occurrence of voids between the adherend and the thermosetting resin film (x1) is easily suppressed. Therefore, the coverage of the bump-forming surface of the semiconductor wafer is improved, and the embedding property in the grooves is also easily improved.

[0078] The glass transition temperature (Tg) of the polyvinyl acetal is preferably 40 to 80°C, and more preferably 50 to 70°C, from the viewpoints of film-forming properties of the thermosetting resin film (x1) and exposing properties of the bump tops. In this specification, the term "exposure ability of the bump top portion" refers to the ability of the bump to penetrate the thermosetting resin film (x1) for forming a protective film when the thermosetting resin film (x1) is attached to a wafer with bumps, and is also referred to as the penetration ability of the bump top portion.

[0079] The ratio of the three or more monomers constituting the polyvinyl acetal can be selected arbitrarily.

[0080] The content of the polymer component (A) is preferably 2 to 30 mass%, more preferably 3 to 25 mass%, and further preferably 3 to 15 mass%, based on the total amount of the active ingredients of the thermosetting resin composition (x1-1).

[0081] The polymer component (A) may also correspond to the thermosetting component (B). In this embodiment, when the thermosetting resin composition (x1-1) contains a component that corresponds to both the polymer component (A) and the thermosetting component (B), the thermosetting resin composition (x1-1) is considered to contain both the polymer component (A) and the thermosetting component (B).

[0082] (Thermosetting component (B)) The thermosetting resin film (x1) and the thermosetting resin composition (x1-1) contain a thermosetting component (B). The thermosetting component (B) is a component for curing the thermosetting resin film (x1) to form a hard cured resin film. The thermosetting component (B) may be used alone or in combination of two or more. When the thermosetting component (B) is used in two or more types, the combination and ratio thereof can be selected arbitrarily.

[0083] Examples of the thermosetting component (B) include epoxy-based thermosetting resins, thermosetting polyimides, polyurethanes, unsaturated polyesters, and silicone resins. Among these, epoxy-based thermosetting resins are preferred. When the thermosetting component (B) is an epoxy-based thermosetting resin, it is possible to improve the protection of the cured resin film and the protruding property of the bump top, and also to suppress warping of the cured resin film.

[0084] The epoxy thermosetting resin comprises an epoxy resin (B1) and a thermosetting agent (B2). The epoxy-based thermosetting resin may be used alone or in combination of two or more. When two or more kinds of epoxy-based thermosetting resins are used, the combination and ratio thereof can be selected arbitrarily.

[0085] (Epoxy resin (B1)) The epoxy resin (B1) is not particularly limited, but from the viewpoint of making it easier to exert the effects of the present invention, it is preferable to use a combination of an epoxy resin that is solid at room temperature (hereinafter also referred to as a solid epoxy resin) and an epoxy resin that is liquid at room temperature (hereinafter also referred to as a liquid epoxy resin). In this specification, "room temperature" refers to 5 to 35°C, and preferably 15 to 25°C.

[0086] The liquid epoxy resin is not particularly limited as long as it is liquid at room temperature, and examples thereof include bisphenol A type epoxy resin, bisphenol F type epoxy resin, novolac type epoxy resin, glycidyl ester type epoxy resin, biphenyl type epoxy resin, phenylene skeleton type epoxy resin, etc. Among these, bisphenol A type epoxy resin is preferred. The liquid epoxy resin may be used alone or in combination of two or more. When two or more liquid epoxy resins are used, the combination and ratio thereof can be selected arbitrarily.

[0087] The epoxy equivalent of the liquid epoxy resin is preferably 200 to 600 g / eq, more preferably 250 to 550 g / eq, and further preferably 300 to 500 g / eq. The epoxy equivalent in this embodiment can be measured in accordance with JIS K 7236:2009.

[0088] The solid epoxy resin is not particularly limited as long as it is solid at room temperature, and examples thereof include biphenyl type epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, orthocresol novolac epoxy resin, dicyclopentadiene type epoxy resin, naphthalene type epoxy resin, anthracene type epoxy resin, fluorene type epoxy resin, etc. Among these, naphthalene type epoxy resin, dicyclopentadiene type epoxy resin, and fluorene type epoxy resin are preferred, and naphthalene type epoxy resin and dicyclopentadiene type epoxy resin are more preferred. The solid epoxy resin may be used alone or in combination of two or more. When the solid epoxy resin is used in combination of two or more kinds, the combination and ratio thereof can be selected arbitrarily.

[0089] The epoxy equivalent of the solid epoxy resin is preferably 150 to 450 g / eq, and more preferably 150 to 400 g / eq.

[0090] The ratio of the content of the liquid epoxy resin (xe) to the content of the solid epoxy resin (ye) [(xe) / (ye)] is preferably 0.01 to 10.0, more preferably 0.02 to 8.0, and even more preferably 0.03 to 6.0, in terms of mass ratio. When the ratio [(xe) / (ye)] is within the above range, the generation of cutting chips and the like can be suppressed when cutting the cured resin film with a dicing blade after curing, and the processability can be easily improved.

[0091] The number average molecular weight of the epoxy resin (B1) is not particularly limited, but from the viewpoints of the curability of the thermosetting resin film and the strength and heat resistance of the cured resin film after curing, it is preferably 300 to 30,000, more preferably 400 to 10,000, and even more preferably 500 to 3,000.

[0092] (Thermal hardener (B2)) The heat curing agent (B2) functions as a curing agent for the epoxy resin (B1). The thermosetting agent (B2) may be, for example, a compound having two or more functional groups in one molecule that can react with an epoxy group. Examples of the functional group include a phenolic hydroxyl group, an alcoholic hydroxyl group, an amino group, a carboxyl group, and an anhydride group of an acid group, and the like. The phenolic hydroxyl group, the amino group, or an anhydride group of an acid group is preferred, and the phenolic hydroxyl group or the amino group is more preferred.

[0093] Among the heat curing agents (B2), examples of phenolic curing agents having a phenolic hydroxyl group include polyfunctional phenolic resins, biphenols, novolac-type phenolic resins, dicyclopentadiene-based phenolic resins, and aralkylphenolic resins. Among the heat curing agents (B2), examples of amine-based curing agents having an amino group include dicyandiamide (hereinafter sometimes abbreviated as "DICY"). Among these, phenol-based curing agents having a phenolic hydroxyl group are preferred, and novolac-type phenolic resins are more preferred.

[0094] Of the thermosetting agents (B2), for example, the number average molecular weight of resin components such as polyfunctional phenol resins, novolac type phenol resins, dicyclopentadiene-based phenol resins, and aralkyl phenol resins is preferably 300 to 30,000, more preferably 400 to 10,000, and even more preferably 500 to 3,000. Of the thermosetting agent (B2), the molecular weight of the non-resin components, such as biphenol and dicyandiamide, is not particularly limited, but is preferably 60 to 500, for example.

[0095] The heat curing agent (B2) may be used alone or in combination of two or more. When two or more types of heat curing agents (B2) are used, the combination and ratio thereof can be selected arbitrarily.

[0096] In the thermosetting resin composition (x1-1), the content of the thermosetting agent (B2) is preferably 0.010 to 200 parts by mass, more preferably 0.020 to 150 parts by mass, even more preferably 0.050 to 100 parts by mass, and even more preferably 0.10 to 77 parts by mass, relative to 100 parts by mass of the epoxy resin (B1). When the content of the thermosetting agent (B2) is equal to or more than the above lower limit, the curing of the thermosetting resin film (x1) proceeds more easily. In addition, when the content of the thermosetting agent (B2) is equal to or less than the above upper limit, the moisture absorption rate of the thermosetting resin film is reduced, and the reliability of the package obtained by using the thermosetting resin film (x1) is further improved.

[0097] In the thermosetting resin composition (x1-1), the content of the thermosetting component (B) (the total content of the epoxy resin (B1) and the thermosetting agent (B2)) is preferably 200 to 10,000 parts by mass, more preferably 300 to 5,000 parts by mass, even more preferably 400 to 2,000 parts by mass, and even more preferably 500 to 1,000 parts by mass, per 100 parts by mass of the polymer component (A), from the viewpoint of improving the protective properties of the cured resin film.

[0098] (Cure accelerator (C)) The thermosetting resin film (x1) and the thermosetting resin composition (x1-1) may contain a curing accelerator (C). The curing accelerator (C) is a component for adjusting the curing rate of the thermosetting resin composition (x1-1). Preferred examples of the curing accelerator (C) include tertiary amines such as triethylenediamine, benzyldimethylamine, triethanolamine, dimethylaminoethanol, and tris(dimethylaminomethyl)phenol; imidazoles (imidazoles in which one or more hydrogen atoms are substituted with groups other than hydrogen atoms) such as 2-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, and 2-phenyl-4-methyl-5-hydroxymethylimidazole; organic phosphines (phosphines in which one or more hydrogen atoms are substituted with organic groups) such as tributylphosphine, diphenylphosphine, and triphenylphosphine; and tetraphenylboron salts such as tetraphenylphosphonium tetraphenylborate and triphenylphosphine tetraphenylborate. Among these, from the viewpoint of making it easier to exert the effects of the present invention, imidazoles are preferred, and 2-phenyl-4,5-dihydroxymethylimidazole is more preferred.

[0099] The curing accelerator (C) may be used alone or in combination of two or more. When two or more curing accelerators (C) are used, the combination and ratio thereof can be selected arbitrarily.

[0100] In the thermosetting resin composition (x1-1), when the curing accelerator (C) is used, the content of the curing accelerator (C) is preferably 0.001 to 10 parts by mass, more preferably 0.01 to 5 parts by mass, relative to 100 parts by mass of the content of the thermosetting component (B). When the content of the curing accelerator (C) is equal to or more than the above lower limit, the effect of using the curing accelerator (C) is more pronounced. In addition, when the content of the curing accelerator (C) is equal to or less than the above upper limit, for example, the effect of suppressing the highly polar curing accelerator (C) from migrating to the adhesive interface with the adherend in the thermosetting resin film (x1) and segregating under high temperature and high humidity conditions is enhanced, and the reliability of the package obtained using the thermosetting resin film (x1) is further improved.

[0101] (Filling material (D)) The thermosetting resin film (x1) and the thermosetting resin composition (x1-1) may contain a filler (D). By including the filler (D), it becomes easier to adjust the thermal expansion coefficient of the cured resin film obtained by curing the thermosetting resin film (x1) to an appropriate range, and the reliability of the package obtained by using the thermosetting resin film (x1) is further improved. In addition, by including the filler (D) in the thermosetting resin film (x1), it is also possible to reduce the moisture absorption rate of the cured resin film and improve the heat dissipation property.

[0102] The filler (D) may be either an organic filler or an inorganic filler, but is preferably an inorganic filler.Preferred inorganic fillers include, for example, powders of silica, talc, calcium carbonate, boron nitride, etc.; beads of these inorganic fillers that have been spherically shaped; surface-modified products of these inorganic fillers; single crystal fibers of these inorganic fillers; glass fibers, etc. Among these, the inorganic filler is preferably silica.

[0103] The filler (D) may be used alone or in combination of two or more kinds. When two or more types of filler (D) are used, their combination and ratio can be selected arbitrarily.

[0104] When the filler (D) is used, the content of the filler (D) is preferably 5 to 50 mass%, more preferably 7 to 40 mass%, and even more preferably 10 to 30 mass%, based on the total amount of the active ingredients of the thermosetting resin composition, from the viewpoint of suppressing peeling of the cured resin film from the chip due to thermal expansion and thermal contraction.

[0105] The average particle size of the filler (D) is preferably from 5 nm to 1000 nm, more preferably from 5 nm to 500 nm, and even more preferably from 10 nm to 300 nm. In this specification, the particle size of the filler (D) means the arithmetic mean particle size obtained by measuring the particle sizes of multiple randomly selected primary particles of the filler (D) observed under an electron microscope and calculating the average value.

[0106] (Energy ray curable resin (E)) The thermosetting resin film (x1) and the thermosetting resin composition (x1-1) may contain an energy ray-curable resin (E). Since the thermosetting resin film (x1) contains the energy ray-curable resin (E), the properties can be changed by irradiation with energy rays.

[0107] The energy ray curable resin (E) is obtained by polymerizing (curing) an energy ray curable compound. Examples of the energy ray curable compound include a compound having at least one polymerizable double bond in the molecule, and an acrylate compound having a (meth)acryloyl group is preferable.

[0108] Examples of the acrylate-based compound include chain-type acrylates such as trimethylolpropane tri(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol monohydroxypenta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,4-butylene glycol di(meth)acrylate, and 1,6-hexanediol di(meth)acrylate. Examples of the polyalkylene glycol (meth)acrylate include aliphatic skeleton-containing (meth)acrylates; dicyclopentanyl di(meth)acrylate and other cyclic aliphatic skeleton-containing (meth)acrylates; polyethylene glycol di(meth)acrylate and other polyalkylene glycol (meth)acrylates; oligoester (meth)acrylates; urethane (meth)acrylate oligomers; epoxy-modified (meth)acrylates; polyether (meth)acrylates other than the above polyalkylene glycol (meth)acrylates; and itaconic acid oligomers.

[0109] The weight average molecular weight of the energy ray-curable compound is preferably from 100 to 30,000, and more preferably from 300 to 10,000.

[0110] The energy ray curable compound used in the polymerization may be used alone or in combination of two or more. When two or more energy ray curable compounds are used in the polymerization, the combination and ratio thereof can be selected arbitrarily.

[0111] When the energy ray curable resin (E) is used, the content of the energy ray curable resin (E) is preferably 1 to 95 mass%, more preferably 5 to 90 mass%, and further preferably 10 to 85 mass%, based on the total amount of the active ingredients of the thermosetting resin composition (x1-1).

[0112] (Photopolymerization initiator (F)) When the thermosetting resin film (x1) and the thermosetting resin composition (x1-1) contain an energy ray curable resin (E), the thermosetting resin film (x1) and the thermosetting resin composition (x1-1) may contain a photopolymerization initiator (F) in order to efficiently proceed with the polymerization reaction of the energy ray curable resin (E).

[0113] Examples of the photopolymerization initiator (F) include benzophenone, acetophenone, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, benzoin benzoic acid, benzoin methyl benzoate, benzoin dimethyl ketal, 2,4-diethylthioxanthone, 1-hydroxycyclohexyl phenyl ketone, benzyl diphenyl sulfide, tetramethylthiuram monosulfide, azobisisobutyronitrile, benzyl, dibenzyl, diacetyl, 1,2-diphenylmethane, 2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, and 2-chloroanthraquinone.

[0114] The photopolymerization initiator (F) may be used alone or in combination of two or more. When the photopolymerization initiator (F) is used in combination of two or more kinds, the combination and ratio thereof can be selected arbitrarily.

[0115] In the thermosetting resin composition (x1-1), the content of the photopolymerization initiator (F) is preferably 0.1 to 20 parts by mass, more preferably 1 to 10 parts by mass, and further preferably 2 to 5 parts by mass, relative to 100 parts by mass of the energy ray-curable resin (E).

[0116] (Near infrared shielding particles (G)) From the viewpoint of easily improving the infrared shielding property, the thermosetting resin film (x1) and the thermosetting resin composition (x1-1) preferably contain near-infrared shielding particles (G). Examples of the near-infrared shielding particles (G) include precious metal particles such as gold and silver; tin-doped indium oxide particles (ITO particles); antimony-doped tin oxide particles; cesium-doped tungsten oxide particles; lanthanum hexaboride; dyes; pigments; alumina; and silicon carbide. Pigments are preferred from the viewpoint of availability and the like. Among pigments, black pigments are preferred because of their excellent near-infrared shielding performance. That is, the thermosetting resin film (x1) of this embodiment preferably contains a pigment, and among these, black pigments (G1) are preferred. Examples of black pigments include carbon black, copper oxide, iron oxide, manganese dioxide, aniline black, and activated carbon. Among these, carbon black is preferred from the viewpoint of availability and the like.

[0117] From the viewpoint of easily improving the near-infrared shielding properties, the content of the black pigment (G1) in the thermosetting resin film (x1) is preferably more than 0.5 mass%, more preferably 0.7 mass% or more, even more preferably 1.0 mass% or more, and still more preferably 1.5 mass% or more, based on the total amount of the thermosetting resin film (x1). From the viewpoint of ensuring the film-forming properties of the thermosetting resin film (x1), the content of the black pigment (G1) is preferably less than 35 mass %, more preferably 30 mass % or less, and even more preferably 25 mass % or less, based on the total amount of the curable resin film (x1).

[0118] In order to facilitate uniform dispersion of the black pigment (G1) in the thermosetting resin film (x1), the particle size of the black pigment (G1) is preferably 1 nm to 1 μm, more preferably 10 nm to 500 nm, and even more preferably 10 nm to 100 nm. In this specification, the particle size of the black pigment (G1) refers to the arithmetic mean particle size obtained by measuring the particle sizes of a plurality of randomly selected primary particles of the black pigment (G1) observed under an electron microscope and calculating the average value.

[0119] (Additive (H)) The thermosetting resin film (x1) and the thermosetting resin composition (x1-1) may contain an additive (H) within the range that does not impair the effects of the present invention. The additive (G) may be a known one and may be arbitrarily selected according to the purpose, and is not particularly limited. Preferred examples of the additive (H) include coupling agents, crosslinking agents, surfactants, plasticizers, antistatic agents, antioxidants, leveling agents, and gettering agents.

[0120] The additive (H) may be used alone or in combination of two or more. When the general-purpose additive (H) is used in two or more types, the combination and ratio thereof can be selected arbitrarily. The content of the additive (H) is not particularly limited and may be appropriately selected depending on the purpose.

[0121] (solvent) The thermosetting resin composition (x1-1) preferably further contains a solvent. The thermosetting resin composition (x1-1) containing a solvent has good handleability. The solvent is not particularly limited, but preferred examples include hydrocarbons such as toluene and xylene; alcohols such as methanol, ethanol, 2-propanol, isobutyl alcohol (2-methylpropan-1-ol), and 1-butanol; esters such as ethyl acetate; ketones such as acetone and methyl ethyl ketone; ethers such as tetrahydrofuran; and amides (compounds having an amide bond) such as dimethylformamide and N-methylpyrrolidone. The solvent may be used alone or in combination of two or more. When two or more solvents are used, the combination and ratio thereof can be selected arbitrarily. The solvent is preferably methyl ethyl ketone or the like, since the components contained in the thermosetting resin composition (x1-1) can be mixed more uniformly.

[0122] (Method for preparing thermosetting resin composition (x1-1)) The thermosetting resin composition (x1-1) is prepared by blending the respective components constituting the composition. The order of addition of each component when blending is not particularly limited, and two or more components may be added at the same time. When a solvent is used, the solvent may be used by mixing with any other blending components other than the solvent to dilute the blending components in advance, or the solvent may be used by mixing with any other blending components without diluting the other components in advance. The method for mixing the components during blending is not particularly limited, and may be appropriately selected from known methods such as a method of mixing by rotating a stirrer or stirring blade, a method of mixing using a mixer, a method of mixing by adding ultrasound, etc. The temperature and time during addition and mixing of each component are not particularly limited as long as the components do not deteriorate, and may be adjusted appropriately. A temperature of 15 to 30°C is preferred.

[0123] <Energy ray curable resin film (x2)> The energy ray-curable resin film (x2) contains an energy ray-curable component (a). The energy ray-curable resin film (x2) is formed, for example, from an energy ray-curable resin composition (x2-1) containing an energy ray-curable component (a). The energy ray-curable component (a) is preferably uncured and preferably has adhesive properties, and more preferably is uncured and has adhesive properties. In the following description of this specification, “the content of each component based on the total amount of active ingredients of the energy ray curable resin composition (x2-1)” is synonymous with “the content of each component of the energy ray curable resin film (x2) formed from the energy ray curable resin composition (x2-1)”.

[0124] (Energy ray curable component (a)) The energy ray-curable component (a) is a component that is cured by irradiation with energy rays, and is also a component that imparts film-forming properties, flexibility, and the like to the energy ray-curable resin film (x2). Examples of the energy ray curable component (a) include a polymer (a1) having an energy ray curable group and a weight average molecular weight of 80,000 to 2,000,000, and a compound (a2) having an energy ray curable group and a molecular weight of 100 to 80,000. The polymer (a1) may be at least partially crosslinked with a crosslinking agent, or may not be crosslinked.

[0125] (Polymer (a1)) An example of the polymer (a1) having an energy ray-curable group and a weight average molecular weight of 80,000 to 2,000,000 includes an acrylic resin (a1-1) obtained by polymerizing an acrylic polymer (a11) having a functional group capable of reacting with a group possessed by another compound, and an energy ray-curable compound (a12) having a group reactive with the functional group and an energy ray-curable group such as an energy ray-curable double bond.

[0126] Examples of functional groups that can react with groups possessed by other compounds include hydroxyl groups, carboxy groups, amino groups, substituted amino groups (groups in which one or two hydrogen atoms of an amino group are substituted with groups other than hydrogen atoms), and epoxy groups. However, from the viewpoint of preventing corrosion of circuits such as semiconductor wafers and semiconductor chips, it is preferable that the functional group is a group other than a carboxy group. Among these, it is preferable that the functional group is a hydroxyl group.

[0127] Acrylic polymer having functional groups (a11) The acrylic polymer (a11) having a functional group may be, for example, a copolymer of an acrylic monomer having a functional group and an acrylic monomer not having a functional group, and may further include a copolymer of a monomer other than the acrylic monomer (non-acrylic monomer) in addition to these monomers. The acrylic polymer (a11) may be a random copolymer or a block copolymer.

[0128] Examples of the acrylic monomer having a functional group include a hydroxyl group-containing monomer, a carboxyl group-containing monomer, an amino group-containing monomer, a substituted amino group-containing monomer, and an epoxy group-containing monomer.

[0129] Examples of hydroxyl group-containing monomers include hydroxyalkyl (meth)acrylates such as hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; and non-(meth)acrylic unsaturated alcohols (unsaturated alcohols not having a (meth)acryloyl skeleton) such as vinyl alcohol and allyl alcohol.

[0130] Examples of the carboxy group-containing monomer include ethylenically unsaturated monocarboxylic acids (monocarboxylic acids having an ethylenically unsaturated bond) such as (meth)acrylic acid and crotonic acid; ethylenically unsaturated dicarboxylic acids (dicarboxylic acids having an ethylenically unsaturated bond) such as fumaric acid, itaconic acid, maleic acid and citraconic acid; anhydrides of the above ethylenically unsaturated dicarboxylic acids; and (meth)acrylic acid carboxyalkyl esters such as 2-carboxyethyl methacrylate.

[0131] The acrylic monomer having a functional group is preferably a hydroxyl group-containing monomer or a carboxyl group-containing monomer, more preferably a hydroxyl group-containing monomer.

[0132] The acrylic monomer having a functional group constituting the acrylic polymer (a11) may be used alone or in combination of two or more. When the acrylic monomer having a functional group constituting the acrylic polymer (a11) is two or more, the combination and ratio thereof can be selected arbitrarily.

[0133] Examples of acrylic monomers having no functional group include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, n-octyl (meth)acrylate, n-nonyl (meth)acrylate, and isopropyl (meth)acrylate. Examples of (meth)acrylic acid alkyl esters include those in which the alkyl group constituting the alkyl ester has a chain structure having 1 to 18 carbon atoms, such as nonyl, decyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate (lauryl (meth)acrylate), tridecyl (meth)acrylate, tetradecyl (meth)acrylate (myristyl (meth)acrylate), pentadecyl (meth)acrylate, hexadecyl (meth)acrylate (palmityl (meth)acrylate), heptadecyl (meth)acrylate, and octadecyl (meth)acrylate (stearyl (meth)acrylate).

[0134] Examples of acrylic monomers not having a functional group include alkoxyalkyl group-containing (meth)acrylic acid esters such as methoxymethyl (meth)acrylate, methoxyethyl (meth)acrylate, ethoxymethyl (meth)acrylate, and ethoxyethyl (meth)acrylate; (meth)acrylic acid esters having an aromatic group, including (meth)acrylic acid aryl esters such as phenyl (meth)acrylate; non-crosslinkable (meth)acrylamide and derivatives thereof; and (meth)acrylic acid esters having a non-crosslinkable tertiary amino group, such as N,N-dimethylaminoethyl (meth)acrylate and N,N-dimethylaminopropyl (meth)acrylate.

[0135] The acrylic monomer having no functional group constituting the acrylic polymer (a11) may be used alone or in combination of two or more. When the acrylic monomer having no functional group constituting the acrylic polymer (a11) is two or more, the combination and ratio thereof can be selected arbitrarily.

[0136] Examples of non-acrylic monomers include olefins such as ethylene and norbornene; vinyl acetate; and styrene.

[0137] The non-acrylic monomer constituting the acrylic polymer (a11) may be used alone or in combination of two or more. When the non-acrylic monomer constituting the acrylic polymer (a11) is two or more, the combination and ratio thereof can be selected arbitrarily.

[0138] In the acrylic polymer (a11), the ratio (content) of the amount of the structural unit derived from the acrylic monomer having a functional group to the total mass of the structural units constituting the acrylic polymer (a11) is preferably 0.1 to 50 mass%, more preferably 1 to 40 mass%, and even more preferably 3 to 30 mass%. When the ratio is within such a range, the content of the energy ray curable group in the acrylic resin (a1-1) obtained by copolymerization of the acrylic polymer (a11) and the energy ray curable compound (a12) makes it possible to easily adjust the degree of curing of the protective film (X) to a preferred range.

[0139] The acrylic polymer (a11) constituting the acrylic resin (a1-1) may be used alone or in combination of two or more. When the acrylic polymer (a11) constituting the acrylic resin (a1-1) is two or more, the combination and ratio thereof can be selected arbitrarily.

[0140] The content of the acrylic resin (a1-1) is preferably 1 to 60 mass%, more preferably 3 to 50 mass%, and further preferably 5 to 40 mass%, based on the total amount of the active ingredients of the energy ray-curable resin composition (x2-1).

[0141] Energy ray curable compounds (a12) The energy ray-curable compound (a12) preferably has one or more groups selected from the group consisting of an isocyanate group, an epoxy group, and a carboxy group as a group reactive with the functional group of the acrylic polymer (a11), and more preferably has an isocyanate group as the group. When the energy ray-curable compound (a12) has, for example, an isocyanate group as the group, this isocyanate group easily reacts with the hydroxyl group of the acrylic polymer (a11) having a hydroxyl group as the functional group.

[0142] The energy ray-curable compound (a12) preferably has 1 to 5 energy ray-curable groups, and more preferably 1 or 2 energy ray-curable groups, in one molecule.

[0143] Examples of the energy ray curable compound (a12) include 2-methacryloyloxyethyl isocyanate, meta-isopropenyl-α,α-dimethylbenzyl isocyanate, methacryloyl isocyanate, allyl isocyanate, 1,1-(bisacryloyloxymethyl)ethyl isocyanate; an acryloyl monoisocyanate compound obtained by reacting a diisocyanate compound or a polyisocyanate compound with hydroxyethyl (meth)acrylate; an acryloyl monoisocyanate compound obtained by reacting a diisocyanate compound or a polyisocyanate compound with a polyol compound and hydroxyethyl (meth)acrylate, etc. Among these, the energy ray curable compound (a12) is preferably 2-methacryloyloxyethyl isocyanate.

[0144] The energy ray curable compound (a12) constituting the acrylic resin (a1-1) may be used alone or in combination of two or more. When the energy ray curable compound (a12) constituting the acrylic resin (a1-1) is two or more, the combination and ratio thereof can be selected arbitrarily.

[0145] In the acrylic resin (a1-1), the content ratio of the energy ray curable group derived from the energy ray curable compound (a12) to the content of the functional group derived from the acrylic polymer (a11) is preferably 20 to 120 mol%, more preferably 35 to 100 mol%, and even more preferably 50 to 100 mol%. When the content ratio is in such a range, the adhesive strength of the protective film (X) after curing is increased. When the energy ray curable compound (a12) is a monofunctional compound (having one of the above groups in one molecule), the upper limit of the content ratio is 100 mol%, but when the energy ray curable compound (a12) is a polyfunctional compound (having two or more of the above groups in one molecule), the upper limit of the content ratio may exceed 100 mol%.

[0146] The weight average molecular weight (Mw) of the polymer (a1) is preferably from 100,000 to 2,000,000, and more preferably from 300,000 to 1,500,000.

[0147] When the polymer (a1) is at least partially crosslinked with a crosslinking agent, the polymer (a1) may be crosslinked at the group reactive with the crosslinking agent by polymerization of a monomer which does not correspond to any of the above-mentioned monomers described as constituting the acrylic polymer (a11) and has a group reactive with the crosslinking agent, or may be crosslinked at a group reactive with the functional group derived from the energy ray-curable compound (a12).

[0148] The polymer (a1) may be used alone or in combination of two or more. When two or more types of polymer (a1) are used, the combination and ratio thereof can be selected arbitrarily.

[0149] (Compound (a2)) The energy ray-curable group contained in the compound (a2) having an energy ray-curable group and a weight average molecular weight of 100 to 80,000 includes a group containing an energy ray-curable double bond, and preferred examples thereof include a (meth)acryloyl group or a vinyl group.

[0150] The compound (a2) is not particularly limited as long as it satisfies the above conditions, and examples thereof include a low molecular weight compound having an energy ray-curable group, an epoxy resin having an energy ray-curable group, and a phenol resin having an energy ray-curable group.

[0151] Among the compounds (a2), examples of the low molecular weight compound having an energy ray-curable group include polyfunctional monomers or oligomers, and acrylate compounds having a (meth)acryloyl group are preferred. Examples of the acrylate compounds include 2-hydroxy-3-(meth)acryloyloxypropyl methacrylate, polyethylene glycol di(meth)acrylate, propoxylated ethoxylated bisphenol A di(meth)acrylate, 2,2-bis[4-((meth)acryloxypolyethoxy)phenyl]propane, ethoxylated bisphenol A di(meth)acrylate, 2,2-bis[4-((meth)acryloxydiethoxy)phenyl]propane, 9,9-bis[4-(2-(meth)acryloyloxyethoxy)phenyl]fluorene, 2,2-bis[4-((meth)acryloxypolypropoxy)phenyl]propane, tricyclodecane dimethanol di(meth)acrylate, 1,10-decane diol di(meth)acrylate, 1,10-decane diol di(meth)acrylate, 1,2-bis[4-((meth)acryloxydiethoxy)phenyl]propane, 1,2-bis[4-((meth)acryloxypolypropoxy)phenyl]propane, 1,3-dimethylphenyl dimethacrylate, 1,4-dimethylphenyl dimethacrylate, 1,5-dimethylphenyl dimethacrylate, 1,6-dimethylphenyl dimethacrylate, 1,7-dimethylphenyl dimethacrylate, 1,8-dimethylphenyl dimethacrylate, 1,9-dimethylphenyl dimethacrylate, 1,10-dimethylphenyl dimethacrylate, 1,2-dimethylphenyl dimethacrylate ... Bifunctional (meth)acrylates such as 6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, 2,2-bis[4-((meth)acryloxyethoxy)phenyl]propane, neopentyl glycol di(meth)acrylate, ethoxylated polypropylene glycol di(meth)acrylate, and 2-hydroxy-1,3-di(meth)acryloxypropane;Polyfunctional (meth)acrylates such as tris(2-(meth)acryloxyethyl)isocyanurate, ε-caprolactone-modified tris-(2-(meth)acryloxyethyl)isocyanurate, ethoxylated glycerin tri(meth)acrylate, pentaerythritol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, ethoxylated pentaerythritol tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol poly(meth)acrylate, and dipentaerythritol hexa(meth)acrylate; polyfunctional (meth)acrylate oligomers such as urethane (meth)acrylate oligomers;

[0152] Of the compounds (a2), examples of the epoxy resin having an energy ray-curable group and the phenol resin having an energy ray-curable group that can be used include those described in paragraph 0043 of JP 2013-194102 A.

[0153] The compound (a2) has a weight average molecular weight of preferably 100 to 30,000, and more preferably 300 to 10,000.

[0154] The compound (a2) may be used alone or in combination of two or more. When the compound (a2) is used in combination of two or more, the combination and ratio thereof can be selected arbitrarily.

[0155] (Polymer (b) having no energy ray-curable group) When the energy ray-curable resin composition (x2-1) and the energy ray-curable resin film (x2) contain the compound (a2) as the energy ray-curable component (a), it is preferable that they further contain a polymer (b) having no energy ray-curable group. The polymer (b) having no energy ray-curable group may be at least partially crosslinked with a crosslinking agent, or may not be crosslinked.

[0156] Examples of the polymer (b) having no energy ray curable group include acrylic polymers, phenoxy resins, urethane resins, polyesters, rubber resins, and acrylic urethane resins. Among these, the polymer (b) is preferably an acrylic polymer (hereinafter sometimes abbreviated as "acrylic polymer (b-1)").

[0157] The acrylic polymer (b-1) may be a known one, for example, a homopolymer of one kind of acrylic monomer, or a copolymer of two or more kinds of acrylic monomers. The acrylic polymer (b-1) may also be a copolymer of one or more kinds of acrylic monomers and one or more kinds of monomers other than the acrylic monomers (non-acrylic monomers).

[0158] Examples of the acrylic monomer constituting the acrylic polymer (b-1) include (meth)acrylic acid alkyl esters, (meth)acrylic acid esters having a cyclic skeleton, glycidyl group-containing (meth)acrylic acid esters, hydroxyl group-containing (meth)acrylic acid esters, and substituted amino group-containing (meth)acrylic acid esters.

[0159] Examples of the (meth)acrylic acid alkyl ester include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, n-octyl (meth)acrylate, n-nonyl (meth)acrylate, and isono (meth)acrylate. Examples of the alkyl (meth)acrylate ester include (meth)acrylic acid alkyl esters in which the alkyl group constituting the alkyl ester has a chain structure having 1 to 18 carbon atoms, such as ethyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate (lauryl (meth)acrylate), tridecyl (meth)acrylate, tetradecyl (meth)acrylate (myristyl (meth)acrylate), pentadecyl (meth)acrylate, hexadecyl (meth)acrylate (palmityl (meth)acrylate), heptadecyl (meth)acrylate, and octadecyl (meth)acrylate (stearyl (meth)acrylate).

[0160] Examples of (meth)acrylic acid esters having a cyclic skeleton include (meth)acrylic acid cycloalkyl esters such as isobornyl (meth)acrylate and dicyclopentanyl (meth)acrylate; (meth)acrylic acid aralkyl esters such as benzyl (meth)acrylate; (meth)acrylic acid cycloalkenyl esters such as dicyclopentenyl (meth)acrylate; and (meth)acrylic acid cycloalkenyloxyalkyl esters such as dicyclopentenyloxyethyl (meth)acrylate.

[0161] Examples of the glycidyl group-containing (meth)acrylic acid ester include glycidyl (meth)acrylate, etc. Examples of the hydroxyl group-containing (meth)acrylic acid ester include hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. The substituted amino group-containing (meth)acrylic acid ester may, for example, be N-methylaminoethyl (meth)acrylate.

[0162] Examples of non-acrylic monomers constituting the acrylic polymer (b-1) include olefins such as ethylene and norbornene; vinyl acetate; and styrene.

[0142] An example of the polymer (b) having no energy ray-curable group and at least a portion of which is crosslinked with a crosslinking agent is one in which a reactive functional group in the polymer (b) has reacted with a crosslinking agent. The reactive functional group is not particularly limited and may be appropriately selected depending on the type of crosslinking agent, etc. For example, when the crosslinking agent is a polyisocyanate compound, examples of the reactive functional group include a hydroxyl group, a carboxyl group, and an amino group, and among these, a hydroxyl group that is highly reactive with an isocyanate group is preferred. When the crosslinking agent is an epoxy compound, examples of the reactive functional group include a carboxy group, an amino group, and an amide group, and among these, a carboxy group, which has high reactivity with an epoxy group, is preferred. However, from the viewpoint of preventing corrosion of the circuits of the semiconductor wafer or semiconductor chip, it is preferable that the reactive functional group is a group other than a carboxy group.

[0163] Examples of the polymer (b) having a reactive functional group but not having an energy ray curable group include those obtained by polymerizing at least a monomer having a reactive functional group. In the case of the acrylic polymer (b-1), it is sufficient to use one or both of the acrylic monomer and the non-acrylic monomer listed as the monomers constituting the polymer (b-1) that have a reactive functional group. For example, examples of the polymer (b) having a hydroxyl group as a reactive functional group include those obtained by polymerizing a hydroxyl group-containing (meth)acrylic acid ester, and other examples include those obtained by polymerizing a monomer in which one or more hydrogen atoms in the acrylic monomer or non-acrylic monomer listed above are substituted with the reactive functional group.

[0164] In the polymer (b) having a reactive functional group, the ratio (content) of the amount of the structural unit derived from the monomer having a reactive functional group to the total mass of the structural units constituting the polymer (b) is preferably 1 to 20 mass%, more preferably 2 to 10 mass%. When the ratio is in such a range, the degree of crosslinking in the polymer (b) becomes a more preferable range.

[0165] The weight average molecular weight (Mw) of the polymer (b) having no energy ray-curable group is preferably 10,000 to 2,000,000, and more preferably 100,000 to 1,500,000, in terms of improving the film-forming property of the energy ray-curable resin composition (x2-1).

[0166] The polymer (b) having no energy ray curable group may be used alone or in combination of two or more. When the polymer (b) having no energy ray curable group is used in two or more types, the combination and ratio thereof can be selected arbitrarily.

[0167] The energy ray-curable resin composition (x2-1) may contain either or both of a polymer (a1) and a compound (a2). When the energy ray-curable resin composition (x2-1) contains the compound (a2), it is preferable that it further contains a polymer (b) having no energy ray-curable group, and in this case, it is also preferable that it further contains a polymer (a1). In addition, the energy ray-curable resin composition (x2-1) may not contain the compound (a2) and may contain both the polymer (a1) and the polymer (b) having no energy ray-curable group.

[0168] When the energy ray-curable resin composition (x2-1) contains the polymer (a1), the compound (a2), and the polymer (b) having no energy ray-curable group, the content of the compound (a2) is preferably 10 to 400 parts by mass, and more preferably 30 to 350 parts by mass, per 100 parts by mass of the total content of the polymer (a1) and the polymer (b) having no energy ray-curable group.

[0169] The total content of the energy ray curable component (a) and the polymer (b) having no energy ray curable group is preferably 5 to 90 mass%, more preferably 10 to 80 mass%, and even more preferably 20 to 70 mass%, based on the total amount of the active ingredients of the energy ray curable resin composition (x2-1). When the content of the energy ray curable component is in such a range, the energy ray curability of the energy ray curable resin film (x2) becomes better.

[0170] The energy ray curable resin composition (x2-1) may contain, in addition to the energy ray curable component, one or more selected from the group consisting of a thermosetting component, a photopolymerization initiator, a filler, a coupling agent, a crosslinking agent, and an additive, depending on the purpose. For example, by using an energy ray-curable resin composition (x2-1) containing an energy ray-curable component and a thermosetting component, the energy ray-curable resin film (x2) formed has improved adhesive strength to an adherend by heating, and the strength of the protective film (X) formed from this energy ray-curable resin film (x2) is also improved.

[0171] The thermosetting component, photopolymerization initiator, filler, coupling agent, crosslinking agent, and additives in the energy ray curable resin composition (x2-1) may be the same as the thermosetting component (B), photopolymerization initiator (H), filler (D), coupling agent (E), crosslinking agent (F), and additive (I) in the energy ray curable resin composition (x2-1), respectively.

[0172] In the energy ray curable resin composition (x2-1), the thermosetting component, the photopolymerization initiator, the filler, the coupling agent, the crosslinking agent and the additive may each be used alone or in combination of two or more. When using two or more in combination, the combination and ratio thereof can be selected arbitrarily. The contents of the thermosetting component, photopolymerization initiator, filler, coupling agent, crosslinking agent, and additives in the energy ray-curable resin composition (x2-1) may be appropriately adjusted depending on the purpose, and are not particularly limited.

[0173] The energy ray-curable resin composition (x2-1) preferably further contains a solvent because its handleability is improved by dilution. Examples of the solvent contained in the energy ray-curable resin composition (x2-1) include the same solvents as those in the thermosetting resin composition (x1-1). The solvent contained in the energy ray curable resin composition (x2-1) may be used alone or in combination of two or more. When two or more types are used in combination, the combination and ratio thereof can be selected arbitrarily.

[0174] (Other Ingredients) The energy ray curable resin composition (x2-1) may contain, in addition to the above-mentioned energy ray curable component, appropriate amounts of components other than the curable component, i.e., a curing accelerator (C), a filler (D), near-infrared shielding particles (G), an additive (H), etc., as in the case of the thermosetting resin film (x1) described above.

[0175] (Method for producing energy ray curable resin composition (x2-1)) The energy ray curable resin composition (x2-1) can be obtained by blending the components for constituting the composition. The order of addition of the components when blending is not particularly limited, and two or more components may be added at the same time. When a solvent is used, the solvent may be used by mixing it with any of the other ingredients to dilute the ingredients in advance, or the solvent may be used by mixing it with any of the other ingredients without diluting them in advance. The method for mixing the ingredients during mixing is not particularly limited, and may be appropriately selected from known methods such as a method of mixing by rotating a stirrer or agitator blades, a method of mixing using a mixer, a method of mixing by adding ultrasonic waves, etc. The temperature and time during addition and mixing of each component are not particularly limited as long as the components do not deteriorate, and may be adjusted appropriately. A temperature of 15 to 30°C is preferred.

[0176] (Thickness of the curable resin film (x)) The thickness of the curable resin film (x) is preferably 70 μm or less, more preferably less than 70 μm, even more preferably 65 μm or less, even more preferably 60 μm or less, even more preferably 55 μm or less, and particularly preferably 50 μm or less, from the viewpoint of easily forming a valley portion in the protective film (X). Also, from the viewpoint of easily forming a protective film (X) having good protective performance, it is preferably 15 μm or more, more preferably 20 μm or more, and even more preferably 25 μm or more. In other words, the thickness of the curable resin film (x) is preferably 15 μm to 70 μm.

[0177] The thickness of the curable resin film (x) can be adjusted based on the relationship between the thickness of the curable resin film (x) and the thickness of the protective film (X) formed by curing the curable resin film (x), and information such as the height of the bumps on the semiconductor wafer to be used.

[0178] From the viewpoint of forming a protective film having excellent coverage on both the bump-forming surface and the side surfaces of a semiconductor chip, the above-mentioned thermosetting resin film preferably satisfies the following requirement (I). <Requirement (I)> A strain is generated in a test piece of the thermosetting resin film having a diameter of 25 mm and a thickness of 1 mm under conditions of a temperature of 90°C and a frequency of 1 Hz, and the storage modulus of the test piece is measured. When the storage modulus of the test piece when the strain of the test piece is 1% is defined as Gc1 and the storage modulus of the test piece when the strain of the test piece is 300% is defined as Gc300, the value of X calculated by the following formula (i) is 10 or more and less than 10,000. X=Gc1 / Gc300...Formula (i)

[0179] The upper limit of the X value specified in the above requirement (I) is, from the viewpoint of forming a protective film having excellent covering properties, preferably 5,000 or less, more preferably 2,000 or less, even more preferably 1,000 or less, still more preferably 500 or less, even more preferably 400 or less, still more preferably 300 or less, even more preferably 100 or less, and particularly preferably 70 or less. From the viewpoint of improving the embedding property into the grooves of the wafer for producing semiconductor chips, the lower limit of the X value specified in the above requirement (I) is preferably 19 or more, more preferably 20 or more, even more preferably 30 or more, and particularly preferably 40 or more.

[0180] In the thermosetting resin film, Gc1 is not particularly limited as long as the X value defined in the requirement (I) is 10 or more and less than 10,000. However, from the viewpoint of making it easier to form a protective film with excellent covering properties, Gc1 is set to 1×10 2 ~1×10 6 Pa is preferred, and 2×10 3 ~7×10 5 Pa is more preferable, and 3×10 3 ~5×10 5 Pa is more preferred.

[0181] In the thermosetting resin film, Gc300 is not particularly limited as long as the X value is 10 or more and less than 10,000. However, from the viewpoint of improving the embeddability of the thermosetting resin film into the bump bases and into the grooves of the wafer for producing semiconductor chips after the bumps penetrate the thermosetting resin film, Gc300 is preferably 10 to 15,000 Pa, more preferably 30 to 10,000 Pa, and even more preferably 60 to 5,000 Pa.

[0182] <Release sheet (Y)> The release sheet (Y) functions as a support for supporting the curable resin film (x). The release sheet (Y) may be a laminate of a substrate 11 and a release layer 21 as shown in Fig. 14(a), or may be a laminate in which a substrate 11, an intermediate layer 31, and a release layer 21 are laminated in this order as shown in Fig. 14(b). A laminate in which a substrate 11, an intermediate layer 31, and a release layer 21 are laminated in this order is suitable for use as a backgrind tape.

[0183] The substrate contained in the release sheet (Y), and the release layer and intermediate layer that may be contained in the release sheet (Y) will be described below.

[0184] (base material) The substrate is in the form of a sheet or film, and examples of the constituent materials thereof include the following various resins. Examples of resins constituting the substrate include polyethylenes such as low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), and high-density polyethylene (HDPE); polyolefins other than polyethylene such as polypropylene, polybutene, polybutadiene, polymethylpentene, and norbornene resin; ethylene-based copolymers (copolymers obtained using ethylene as a monomer) such as ethylene-vinyl acetate copolymer, ethylene-(meth)acrylic acid copolymer, ethylene-(meth)acrylic acid ester copolymer, and ethylene-norbornene copolymer; and vinyl chloride-based resins (copolymers obtained using vinyl chloride as a monomer) such as polyvinyl chloride and vinyl chloride copolymer. resins obtained by subjecting the polyester to polymerization; polystyrene; polycycloolefins; polyesters such as polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, polyethylene isophthalate, polyethylene-2,6-naphthalenedicarboxylate, and wholly aromatic polyesters in which all of the constituent units have aromatic cyclic groups; copolymers of two or more of the above polyesters; poly(meth)acrylic acid esters; polyurethanes; polyurethane acrylates; polyimides; polyamides; polycarbonates; fluororesins; polyacetals; modified polyphenylene oxides; polyphenylene sulfides; polysulfones; and polyether ketones. In addition, examples of the resin constituting the substrate include polymer alloys such as mixtures of the polyester and other resins. The polymer alloys of the polyester and other resins preferably contain a relatively small amount of resin other than polyester. Examples of the resin constituting the substrate include crosslinked resins in which one or more of the resins exemplified above are crosslinked; and modified resins such as ionomers using one or more of the resins exemplified above.

[0185] The resin constituting the substrate may be one type used alone or two or more types used in combination. When the resin constituting the substrate is two or more types, the combination and ratio thereof can be selected arbitrarily.

[0186] The substrate may be one layer (single layer) or two or more layers. When the substrate is a multilayer substrate, the layers may be the same or different from each other, and the combination of the layers is not particularly limited.

[0187] The thickness of the substrate is preferably from 5 μm to 1,000 μm, more preferably from 10 μm to 500 μm, even more preferably from 15 μm to 300 μm, and even more preferably from 20 μm to 150 μm. Here, the "thickness of the substrate" means the thickness of the entire substrate. For example, the thickness of a substrate consisting of multiple layers means the total thickness of all layers constituting the substrate.

[0188] The substrate is preferably one having a high thickness accuracy, i.e., one having reduced thickness variation regardless of the location. Among the above-mentioned constituent materials, examples of materials having a high thickness accuracy that can be used to constitute the substrate include polyethylene, polyolefins other than polyethylene, polyethylene terephthalate, and ethylene-vinyl acetate copolymer.

[0189] In addition to the main constituent materials such as the resin, the substrate may contain various known additives such as fillers, colorants, antistatic agents, antioxidants, organic lubricants, catalysts, and softeners (plasticizers).

[0190] The substrate may be transparent or opaque, may be colored depending on the purpose, or may have other layers deposited thereon. In addition, when the curable resin film (x) is an energy ray curable resin film (x2) and when the release layer is an energy curable release layer, the substrate is preferably one that transmits energy rays.

[0191] The substrate can be produced by a known method. For example, a substrate containing a resin can be produced by molding a resin composition containing the resin.

[0192] (Release layer) The release layer has a function of imparting releasability to the release sheet, and is formed, for example, from a cured product of a release layer-forming composition that contains a release agent. The release agent is not particularly limited, and examples thereof include silicone resin, alkyd resin, acrylic resin, ethylene-vinyl acetate copolymer, etc. Among these, ethylene-vinyl acetate copolymer is preferred from the viewpoint of enhancing the protruding property of the top of the bump and from the viewpoint of peelability from the cured resin film.

[0193] The release layer may be one layer (single layer) or two or more layers. When the release layer is a multi-layer structure, the multi-layer structure may be the same or different from each other, and the combination of the multi-layer structure is not particularly limited.

[0194] The thickness of the release layer is preferably 3 μm to 50 μm, more preferably 3 μm to 45 μm, and even more preferably 3 μm to 40 μm. Here, the "thickness of the release layer" means the thickness of the entire release layer, and for example, the thickness of a release layer consisting of multiple layers means the total thickness of all layers constituting the release layer.

[0195] The release layer may be formed using an energy ray curable adhesive or a non-energy ray curable adhesive. The release layer formed using an energy ray curable adhesive can easily adjust the physical properties before and after curing.

[0196] (Middle class) The intermediate layer is in the form of a sheet or film, and its constituent material may be appropriately selected according to the purpose, and is not particularly limited. For example, when the purpose is to suppress the deformation of the protective film (X) by reflecting the shape of the bumps present on the semiconductor surface in the protective film covering the semiconductor surface, preferred constituent materials of the intermediate layer include urethane (meth)acrylate; resins containing constituent units derived from monomer components such as olefin monomers such as α-olefin, etc., from the viewpoint of improving the unevenness conformability, improving the bump penetration property, and further improving the attachment property of the intermediate layer.

[0197] The intermediate layer may be one layer (single layer) or two or more layers. When the intermediate layer is a multi-layer structure, the multi-layer structure may be the same or different from each other, and the combination of the multi-layer structure is not particularly limited.

[0198] The thickness of the intermediate layer can be adjusted appropriately depending on the height of the bumps on the semiconductor surface to be protected, but from the viewpoint of easily absorbing the effect of relatively high bumps, it is preferably 50 μm to 600 μm, more preferably 70 μm to 500 μm, and even more preferably 80 μm to 400 μm. Here, the "thickness of the intermediate layer" means the thickness of the entire intermediate layer, and for example, the thickness of an intermediate layer consisting of multiple layers means the total thickness of all layers that make up the intermediate layer.

[0199] (Manufacturing method of composite sheet) The composite sheet can be produced by laminating the above-mentioned layers in order so that they are in a corresponding positional relationship. For example, when manufacturing a release sheet, if a release layer or intermediate layer is laminated on a substrate, the release layer or intermediate layer can be laminated by applying a pressure-sensitive adhesive composition or a composition for forming an intermediate layer onto the substrate and drying it or irradiating it with energy rays as necessary. Examples of the coating method include spin coating, spray coating, bar coating, knife coating, roll coating, roll knife coating, blade coating, die coating, and gravure coating.

[0200] On the other hand, for example, when a curable resin film (x) is laminated on a release layer already laminated on a substrate, the curable resin film (x) can be directly formed by applying a thermosetting resin composition (x1-1) or an energy ray curable resin composition (x2-1) on the release layer. Similarly, when a release layer is laminated on top of an intermediate layer already laminated on a substrate, the release layer can be formed directly by applying a pressure-sensitive adhesive composition onto the intermediate layer.

[0201] In this way, when forming a continuous two-layer laminate structure using any of the compositions, it is possible to form a new layer by coating the composition on the layer formed from the composition. However, it is preferable that the layer to be laminated later among these two layers is formed in advance using the composition on another release film, and the exposed surface of the formed layer opposite to the side in contact with the release film is bonded to the exposed surface of the remaining layer already formed to form a continuous two-layer laminate structure. At this time, it is preferable that the composition is coated on the release-treated surface of the release film. After the formation of the laminate structure, the release film may be removed as necessary.

[0202] [Each step in the manufacturing process of a semiconductor wafer with a protective film] 15 to 19 are explanatory diagrams showing an example of a manufacturing process of a semiconductor wafer with a protective film. The explanatory diagrams used in the following description are examples in which the composite sheet 1b described above is used, but the present invention is not limited to this.

[0203] <Process (S1)> An outline of step (S1) is shown in FIGS. In step (S1), first, a semiconductor wafer having a bump-forming surface on which a plurality of bumps are provided is prepared. Next, the curable resin film (x) of the composite sheet 1b is placed facing the bump formation surface 41a of the semiconductor wafer 41 (see FIG. 15). Then, the composite sheet 1b is attached to the bump formation surface 41a of the semiconductor wafer 41 while being pressed, with the curable resin film (x) serving as the attachment surface. As a result, the bump formation surface 41a of the semiconductor wafer 41 is covered with the curable resin film (x), and the curable resin film (x) is also filled between the multiple bumps BM (see FIG. 16).

[0204] The pressing force applied when attaching the composite sheet 1b to the bump-forming surface 41a of the semiconductor wafer 41 is preferably 1 kPa to 200 kPa, more preferably 5 kPa to 150 kPa, and even more preferably 10 kPa to 100 kPa, from the viewpoint of effectively filling the spaces between the multiple bumps BM with the curable resin film (x). A valley portion is formed by pressing the curable resin film (x) through the release sheet (Y) with an appropriate pressing force. At this time, even if the thickness of the curable resin film (x) is relatively thin, the curable resin film (x) is pushed against and adheres to the side surface of the bump BM by pressing the curable resin film (x) with the release layer 21 or the release sheet (Y) including the release layer 21 and the intermediate layer 31, thereby forming a shoulder portion. By making the thickness of the curable resin film (x) thinner and increasing the pressing force, it is possible to appropriately form a shoulder portion while making the minimum height h2 of the valley portion zero, as in the semiconductor wafer 50B with a protective film shown in FIG. 5.

[0205] The pressure applied when attaching the composite sheet 1b to the bump-formed surface 41a of the semiconductor wafer 41 may be varied as appropriate from the beginning to the end of attachment. For example, from the viewpoint of better filling the spaces between the bumps BM with the curable resin film (x), it is preferable to lower the pressure applied in the beginning of attachment and gradually increase the pressure.

[0206] Furthermore, when the composite sheet 1b is attached to the bump formation surface 41a of the semiconductor wafer 41, if the curable resin film (x) is a thermosetting resin film (x1), it is preferable to heat the film in order to more effectively fill the spaces between the bumps BM with the curable resin film (x). If the curable resin film (x) is a thermosetting resin film (x1), the fluidity of the thermosetting resin film (x1) is temporarily increased by heating, and the film is hardened by continuing to heat the film. Thus, by heating the film within a range in which the fluidity of the thermosetting resin film (x1) is improved, the thermosetting resin film (x1) can easily spread between the bumps BM, and the filling property of the thermosetting resin film (x1) between the bumps BM is further improved. Specifically, the heating temperature (attaching temperature) is preferably 50°C to 150°C, more preferably 60°C to 130°C, and further preferably 70°C to 110°C. The heat treatment performed on the thermosetting resin film (x1) is not included in the curing treatment of the thermosetting resin film (x1).

[0207] Furthermore, the composite sheet 1b may be attached to the bump formation surface 41a of the semiconductor wafer 41 in a reduced pressure environment. This creates a negative pressure between the bumps BM, making it easier for the curable resin film (x) to spread between the bumps BM. As a result, the filling of the curable resin film (x) between the bumps BM is more likely to be improved. The specific pressure of the reduced pressure environment is preferably 0.001 kPa to 50 kPa, more preferably 0.01 kPa to 5 kPa, and even more preferably 0.05 kPa to 1 kPa.

[0208] <Process (BG)> In the method for manufacturing a semiconductor wafer with a protective film according to this embodiment, the step (S1) is followed by an optional back grinding step (step (BG)). The outline of the step (BG) is shown in FIGS. 17, in the process (BG), with the composite sheet 1b attached, the surface of the semiconductor wafer 41 opposite to the bump-formed surface 41a (i.e., the back surface 41b of the semiconductor wafer 41 in FIG. 16) is ground (back-grinding process) to thin the semiconductor wafer 41. As a result, a ground surface GS is formed on the back surface of the semiconductor wafer 41. In the above-mentioned method for producing a semiconductor wafer with a protective film, since the release sheet (Y) is a backgrind sheet, the backgrinding process of the back surface of the semiconductor wafer 41 can be performed satisfactorily. The back grinding process may be performed before the curable resin film (x) is cured, as in the manufacturing method of a semiconductor wafer with a protective film according to this embodiment, or may be performed after the curable resin film (x) is cured. After the step (BG) is completed, the release sheet (Y) is peeled off from the composite sheet 1b as shown in FIG.

[0209] <Process (S2)> After performing step (S1), step (BG) is performed as necessary, and then step (S2) is performed. Specifically, as shown in Fig. 19(a), a protective film (X) containing a cured resin is formed by curing a curable resin film (x), thereby obtaining a semiconductor wafer with a protective film. The protective film (X) formed by curing the curable resin film (x) is stronger than the curable resin film (x) at room temperature (23° C.). Therefore, by forming the protective film (X), the bump neck is well protected.

[0210] The curable resin film (x) can be cured by either heat curing or curing by irradiation with energy rays, depending on the type of curable component contained in the curable resin film (x). As for the conditions for thermal curing, the curing temperature is preferably 90° C. to 200° C., and the curing time is preferably 1 hour to 3 hours. The conditions for curing by irradiation with energy rays are appropriately set depending on the type of energy rays used. For example, when ultraviolet rays are used, the illuminance is preferably 170 mW / cm 2 ~250mw / cm 2 and the light dose is preferably 300 mJ / cm 2 ~3,000mJ / cm 2 It is.

[0211] Here, in the process of curing the curable resin film (x) to form the protective film (X), from the viewpoint of removing air bubbles and the like that may get in when the curable resin film (x) fills the spaces between the plurality of bumps BM in step (S2), the curable resin film (x) is preferably a thermosetting resin film (x1). That is, when the curable resin film (x) is a thermosetting resin film (x1), the fluidity of the thermosetting resin film (x1) temporarily increases when heated, and the film is cured by continuing to be heated. By utilizing this phenomenon, when the fluidity of the thermosetting resin film (x1) increases, air bubbles and the like that may get in when the thermosetting resin film (x1) fills the spaces between the plurality of bumps BM are removed, and the thermosetting resin film (x1) can be cured in a state in which the filling ability of the thermosetting resin film (x1) between the plurality of bumps BM is improved. From the viewpoint of shortening the curing time, the curable resin film (x) is preferably an energy ray-curable resin film (x1).

[0212] As described above, the release sheet (Y) is peeled off before the curable resin film (x) is cured, and the curable resin film (x) is cured to form the protective film (X), thereby obtaining a semiconductor wafer with a protective film. However, the present invention is not limited to such an embodiment, and the release sheet (Y) may be peeled off after the curable resin film (x) is cured to form the protective film (X), thereby obtaining a semiconductor wafer with a protective film.

[0213] <Process (EC)> As an optional step (EC), an etching process may be performed after the curable resin film (x) is cured. FIG. 19(b) shows an outline of step (EC). By performing the etching process, the valleys are mainly etched, resulting in valleys XV' having a height lower than the height of the original valleys XV shown by the dashed line in FIG. 19(b), and the height difference between the valleys and the shoulders can be increased. Also, by performing the etching process, the protective film (X) covering the tops of the bumps or the protective film (X) attached to part of the tops of the bumps can be removed to expose the tops of the bumps. The etching process may be, for example, a wet etching process or a dry etching process, and the dry etching process may be, for example, a plasma etching process.

[0214] [Method of manufacturing semiconductor chips with protective film] The method for producing a semiconductor chip with a protective film according to an embodiment of the present invention includes the following steps (T1) and (T2). Step (T1): A step of obtaining a semiconductor wafer with a protective film by carrying out the method for producing a semiconductor wafer with a protective film. Step (T2): A step of dividing the semiconductor wafer with the protective film into individual pieces.

[0215] <Process (T1)> In the step (T1), the above-mentioned method for producing a semiconductor wafer with a protective film of the present invention is carried out to obtain a semiconductor wafer with a protective film.

[0216] <Process (T2)> In the step (T2), the semiconductor wafer with the protective film obtained in the step (T1) is divided into individual pieces. The method of dicing is not particularly limited, and any known dicing method can be appropriately used, specifically, for example, laser dicing, blade dicing, and stealth dicing (registered trademark).

[0217] Before carrying out the step (T1), a step of forming a back surface protective film on the back surface (the surface opposite to the bump formation surface) of the protective film-coated semiconductor wafer may be included.

[0218] As a semiconductor wafer having a bump-forming surface with bumps, a wafer for manufacturing semiconductor chips may be used in which a plurality of grooves are formed on the bump-forming surface as planned division lines, the grooves not reaching the rear surface. In this case, the plurality of grooves are cut grooves formed when applying a blade-tip dicing method (dicing before grinding), and are formed to a depth shallower than the thickness of the semiconductor wafer, and the deepest part of the grooves is formed so as not to reach the rear surface of the semiconductor wafer. The plurality of grooves can be formed by dicing using a conventionally known wafer dicing device equipped with a dicing blade or the like. When using a wafer for producing semiconductor chips having the above-mentioned grooves formed therein, a method for producing a semiconductor chip with a protective film according to an embodiment of the present invention roughly includes a step (S1) of preparing a wafer for producing semiconductor chips and attaching a curable resin film, a step (S2) of curing the curable resin film, and a step (S3) of singulating, and further includes a step (S-BG) of grinding the back surface of the wafer for producing semiconductor chips.

[0219] In this case, in step (S2), the bump formation surface of the semiconductor chip fabrication wafer is covered with a curable resin film (x), and the curable resin film (x) is embedded in the grooves formed in the semiconductor chip fabrication wafer. Then, in step (S3), dicing is performed along the grooves to obtain semiconductor chips with a protective film. The semiconductor chip with protective film obtained through the above process has excellent strength because the bump-forming surface and side surfaces are covered with a cured resin film. In addition, because the bump-forming surface and side surfaces are continuously and seamlessly covered with the cured resin film, the bonding surface (interface) between the bump-forming surface and the cured resin film is not exposed on the side surfaces of the semiconductor chip. Since there is no exposed portion, peeling of the film from the exposed portion is unlikely to occur during the dicing process or after manufacturing.

[0220] The step (S-BG) is carried out after the step (S1) and before the step (S2), after the step (S2) and before the step (S3), or during the step (S3). The amount of grinding when grinding the back surface of the semiconductor chip production wafer having the above-mentioned grooves formed therein may be at least an amount that exposes the bottom of the grooves of the semiconductor chip production wafer, and further grinding may be performed to grind the curable resin film (x) or cured resin film embedded in the grooves together with the semiconductor chip production wafer.

[0221] [Semiconductor package manufacturing method] The method for manufacturing a semiconductor package according to the embodiment of the present invention includes the following steps (U1) to (U2). Step (U1): A step of obtaining a semiconductor chip with a protective film by carrying out the above-mentioned method for producing a semiconductor chip with a protective film. Step (U2): A step of electrically connecting the wiring board and the semiconductor chip with the protective film via the bumps.

[0222] <Process (U1)> In the step (U1), the above-mentioned method for producing a semiconductor chip with a protective film of the present invention is carried out to obtain a semiconductor chip with a protective film.

[0223] <Process (U2)> In the step (U2), the wiring board having wiring and the semiconductor chip with a protective film are electrically connected via bumps BM. More specifically, the bump formation surface of the protective film-attached semiconductor chip and the wiring formation surface of the wiring board are heated in a state in which they are opposed to each other via the bumps BM (hereinafter, also referred to as the "heat connection step"). This allows the tops of the bumps BM to be satisfactorily electrically connected to the wiring. The conditions for the heat connection step are, for example, a temperature of 250° C. to 270° C. and a time of 30 seconds to 5 minutes.

[0224] <Process (U3)> The method for producing a semiconductor package according to one aspect of the present invention further includes the following step (U3). Step (U3): A step of filling an underfill material between the wiring board and the semiconductor chip with the protective film. EXAMPLES

[0225] The present invention will now be described in detail with reference to examples, but the present invention is not limited to the following examples.

[0226] 1. Manufacturing of thermosetting resin films 1-1. Production Example 1 (Production of Thermosetting Resin Film (BSF-A)) (1) Raw materials for producing thermosetting resin compositions The raw materials used in the production of the thermosetting resin composition are shown below. Polymer component (A) (A)-1: An acrylic resin (weight average molecular weight 800,000, glass transition temperature -28°C) obtained by copolymerizing butyl acrylate (hereinafter abbreviated as "BA") (55 parts by mass), methyl acrylate (hereinafter abbreviated as "MA") (10 parts by mass), glycidyl methacrylate (hereinafter abbreviated as "GMA") (20 parts by mass), and 2-hydroxyethyl acrylate (hereinafter abbreviated as "HEA") (15 parts by mass). Epoxy resin (B1) (B1)-1: Liquid bisphenol F type epoxy resin ("YL983U" manufactured by Mitsubishi Chemical Corporation); weight average molecular weight = 340 (B1)-2: polyfunctional aromatic epoxy resin ("EPPN-502H" manufactured by Nippon Kayaku Co., Ltd.); weight average molecular weight = 1,000 (B1)-3: Dicyclopentadiene type epoxy resin ("EPICLON HP-7200" manufactured by DIC Corporation); weight average molecular weight = 600 ·Heat hardener (B2) (B2)-1: Novolac type phenolic resin ("BRG-556" manufactured by Showa Denko K.K.) Curing accelerator (C) (C)-1: 2-Phenyl-4,5-dihydroxymethylimidazole ("Curesol 2PHZ-PW" manufactured by Shikoku Chemical Industry Co., Ltd.) ·Filling material (D) (D)-1: Spherical silica modified with epoxy groups ("Admanano YA050C-MKK" manufactured by Admatechs Co., Ltd.); 0.05 μm (average particle size) The average particle size of the filler was determined by measuring the outer diameter of one particle at several points and calculating the arithmetic mean value.

[0227] (2) Production of thermosetting resin composition Polymer component (A)-1 (100 parts by mass), epoxy resin (B1)-1 (135 parts by mass), epoxy resin (B1)-2 (90 parts by mass), epoxy resin (B1)-3 (150 parts by mass), heat curing agent (B2)-1 (180 parts by mass), curing accelerator (C)-1 (1 part by mass), and filler (D)-1 (160 parts by mass) were dissolved or dispersed in methyl ethyl ketone and stirred at 23 ° C. to obtain a thermosetting resin composition having a total concentration of all components other than the solvent of 55% by mass. Note that the blending amounts of all components other than the solvent shown here are the blending amounts of the target product not including the solvent.

[0228] (3) Manufacturing of thermosetting resin film (BSF-A) A release film ("SP-PET381031" manufactured by Lintec Corporation, thickness 38 μm) made of polyethylene terephthalate film with one side treated for release by silicone treatment was used, and the thermosetting resin composition obtained above was applied to the release-treated surface, followed by drying at 100°C for 2 minutes to produce a thermosetting curable resin film (BSF-A) having a thickness of 100 μm.

[0229] 1-2. Production Example 2 (Production of Thermosetting Resin Film (BSF-B)) (1) Raw materials for producing thermosetting resin compositions The raw materials used in the production of the thermosetting resin composition are shown below. Polymer component (A) (A)-2: Phenoxy resin (Gabriel Phenoxies "PKHH")

[0230] Epoxy resin (B1) (B1)-4: Liquid modified bisphenol A type epoxy resin (DIC Corporation "Epicron EXA-4850-150", molecular weight 900, epoxy equivalent 450g / eq) (B1)-5: Dicyclopentadiene type epoxy resin (DIC Corporation "Epicron HP-7200HH", epoxy equivalent 254-264g / eq) ·Heat hardener (B2) (B2)-2: O-cresol type novolak resin (DIC Corporation "Phenolite KA-1160") ·Filling material (D) Filler (D)-1 shown in Production Example 1 above Additives (I) (I)-1: Rheology control agent (polyhydroxycarboxylic acid ester, BYK's "BYK-R606") Curing accelerator (C) Curing accelerator (C) shown in Production Example 1 above

[0231] (2) Production of thermosetting resin composition Polymer component (A)-1 (100 parts by mass), epoxy resin (B1)-1 (350 parts by mass), epoxy resin (B1)-4 (270 parts by mass), (B2)-1 (190 parts by mass), curing accelerator (C)-1 (2 parts by mass), filler (D)-1 (90 parts by mass) and additive (I)-1 (9 parts by mass) were dissolved or dispersed in methyl ethyl ketone and stirred at 23 ° C. to obtain a composition having a total concentration of all components other than the solvent of 45 mass % as a thermosetting resin composition. Note that the blending amounts of all components other than the solvent shown here are the blending amounts of the target product not including the solvent.

[0232] (3) Manufacturing of thermosetting resin film (BSF-B) A release film ("SP-PET381031" manufactured by Lintec Corporation, thickness 38 μm) made of polyethylene terephthalate film, one side of which had been treated for release by silicone treatment, was used. The thermosetting resin composition obtained above was applied to the release-treated surface, and the film was dried by heating at 120°C for 2 minutes to form thermosetting resin films (BSF-B) having thicknesses of 30 μm, 45 μm, and 70 μm, respectively.

[0233] 2. Preparation of backgrind tape The following two types of backgrind tape (BG tape) were prepared. BG tape (BG-A): Lintec Corporation's BG tape "E-3281B" (consists of a polyethylene terephthalate base material and two types of release layers. The total thickness is 287 μm.) BG tape (BG-B): Lintec Corporation's BG tape "E-8510HR" (consists of a polyethylene terephthalate base material, a urethane acrylate intermediate layer, and a release layer. The total thickness is 510 μm.)

[0234] 3. Bumped Wafer Preparation A bump wafer (Walts "WLP TEG M2", 0.4 mm pitch, Ball Grid Array (BGA)) was used as the electronic component. This bump wafer has spherical bumps with a diameter of 250 μm regularly arranged in a matrix on the bump-forming surface when viewed in plan. The thickness of the silicon wafer portion is 730 μm. The height of the bump-forming surface of each bump is 210 μm, and a passivation film with a thickness of 10 nm is provided on the areas of the bump-forming surface other than the bumps. In addition, there are no grooves along the planned division lines.

[0235] 4. Examples 1 to 4 and Comparative Examples 1 to 4 4-1. Example 1 A BG tape (BG-B) was attached to a thermosetting resin film (BSF-B) with the release layer as the attachment surface to obtain a laminate (composite sheet). The laminate was placed on the bump wafer with the thermosetting resin film facing the bump wafer, and the laminate was attached to the bump wafer using a bonding device (a roller-type laminator "RAD-3510F / 12" manufactured by Lintec Corporation) under conditions of a table temperature of 90°C, a bonding speed of 5 mm / sec, a bonding pressure of 0.5 MPa, and a roller bonding height of -400 μm. Next, after peeling off the BG tape, the thermosetting resin film was cured using a heat and pressure curing device ("RAD-9100" manufactured by Lintec Corporation) under conditions of a heating temperature of 130°C, a heating time of 4 hours, and a pressure of 0.5 MPa, thereby obtaining a semiconductor wafer with a protective film in which a protective film (X) was formed on the bump formation surface.

[0236] 4-2. Example 2 A semiconductor wafer with a protective film (X) formed on the bump-forming surface was produced in the same manner as in Example 1, except that the thickness of the thermosetting resin film (BSF-B) was changed to 30 μm, and that after the protective film was formed, the bump-forming surface of the bump wafer was irradiated with plasma for 15 minutes using a parallel plate reactive ion etching apparatus RIE-10NRT (manufactured by Samco Corporation) under conditions of output: 250 W, gas flow rate: CF4 = 10 sccm, O2 = 90 sccm.

[0237] 4-3. Example 3 A semiconductor wafer with a protective film, in which a protective film (X) was formed on the bump-forming surface, was produced in the same manner as in Example 2, except that the plasma exposure time was changed to 60 minutes.

[0238] 4-4. Example 4 A semiconductor wafer with a protective film was produced in which a protective film (X) was formed on the bump-forming surface of the bump wafer using the same procedure as in Example 1, except that after the protective film was formed, plasma was irradiated for 15 minutes under the same conditions as in Example 2 to the bump-forming surface of the bump wafer.

[0239] 4-5. Comparative Example 1 The BG tape (BG-B) was attached to the bump-formed surface of the bump wafer using an attachment device ("RAD-3510F / 12" manufactured by Lintec Corporation). The attachment conditions were the same as those in Example 1. Thereafter, the BG tape was peeled off to provide a sample for "measurement of shoulder height and valley height" described below.

[0240] 4-6. Comparative Example 2 A semiconductor wafer having a protective film formed on the bump-forming surface was produced using the same procedure as in Example 1, except that a 100 μm thick thermosetting resin film (BSF-A) was used, BG tape (BG-A) was used, and plasma was irradiated for 60 minutes under the same conditions as in Example 2 to the bump-forming surface after the protective film was formed.

[0241] 4-7. Comparative Example 3 A semiconductor wafer having a protective film formed on the bump-forming surface was produced using the same procedure as in Example 1, except that the thickness of the thermosetting resin film (BSF-B) was changed to 70 μm, BG tape (BG-A) was used, and plasma was irradiated for 60 minutes under the same conditions as in Example 2 to the bump-forming surface after the protective film was formed.

[0242] 4-8. Comparative Example 4 A semiconductor wafer having a protective film formed on the bump-forming surface was produced in the same manner as in Example 1, except that the thickness of the thermosetting resin film (BSF-B) was changed to 30 μm and BG tape (A) was used.

[0243] 5-1. Measurement of X value (Gc1 / Gc300) According to the procedure of the above-mentioned manufacturing example, 20 sheets of thermosetting resin film BSF-A and thermosetting resin film BSA-B, each having a thickness of 45 μm, were prepared. Next, these thermosetting resin films were laminated, and the obtained laminated film was cut into a disk shape having a diameter of 25 mm to prepare a test piece of thermosetting resin film having a thickness of 1 mm. The location where the test piece was to be placed in the viscoelasticity measuring device ("MCR301" manufactured by Anton Paar) was kept warm at 80°C in advance, and the test piece of the thermosetting resin film obtained above was placed on this location, and the test piece was fixed to the location by pressing a measuring tool against the upper surface of the test piece. Next, the strain generated in the test piece was increased stepwise in the range of 0.01% to 1,000% under the conditions of a temperature of 90°C and a measurement frequency of 1 Hz, and the storage modulus Gc of the test piece was measured. Then, the X value was calculated from the measured values ​​of Gc1 and Gc300. As a result, the X value of the thermosetting resin film BSF-A was 19. Also, the X value of the thermosetting resin film BSA-B was 30.

[0244] 5-2. Measurement of shoulder height and valley height A pair of adjacent bumps (first and second bumps) was arbitrarily selected from the semiconductor wafers with protective films obtained in the examples and comparative examples, and a portion including these bumps was cut out as a chip by dicing. Next, Epofix resin (manufactured by Marumoto Struers) and Epofix hardener (manufactured by Marumoto Struers) were mixed in a mass ratio of 25:3, and the cut-out chip was embedded and solidified. Then, the solidified chip was cross-polished together with the resin so that a vertical cross section passing through a circle including the center of the first bump and having a diameter 10% of the diameter of the first bump, and a circle including the center of the second bump and having a diameter 10% of the diameter of the second bump, is formed when the first and second bumps are viewed in a plane. Then, by observing the longitudinal section with a digital microscope manufactured by Keyence Corporation, the height h1a from the bump forming surface of the first shoulder portion which is in contact with the first bump and is the position furthest from the bump forming surface, the height h1b from the bump forming surface of the second shoulder which is in contact with the second bump and is the position furthest from the bump forming surface, and the minimum height h2 from the bump forming surface of the valley portion located between the first and second shoulder portions were measured. The results are shown in Table 1. In Table 1, "h1" is the arithmetic mean value of "h1a" and "h1b", and means "h1=(h1a+h1b) / 2". Since the height of each of the above-mentioned parts is measured within a very small cross section, the effect of warpage on the measurement is minor. Therefore, as described below, the height of each of the above-mentioned parts may be measured after grinding the back surface of each semiconductor wafer with the protective film. In the semiconductor wafer with the protective film of Comparative Example 4, the curable resin film (x) was thin, and since the BG tape (A) which was less flexible than the BG tape (B) was used, the thermosetting resin film could not be fully filled near the bump neck, and voids were generated, so the film peeled off during application and could not be applied, and the wafer could not be processed. For this reason, the shoulder height and valley height were not measured, and the various evaluations described below were not performed.

[0245] [Table 1]

[0246] As shown in Table 1, in the semiconductor wafers with protective films of Examples 1 to 4, the height h1 of the shoulder portion of the protective film and the minimum height h2 of the valley portion satisfy the relationship of formula (1), while in the semiconductor wafers with protective films of Comparative Examples 2 and 3, the height h1 of the shoulder portion of the protective film and the minimum height h2 of the valley portion do not satisfy the relationship of formula (1).

[0247] 6. Evaluation The following evaluations were performed using the semiconductor wafer with protective film obtained above. More specifically, for Examples 1 to 4 and Comparative Examples 2 and 3, the backside of the bump wafer to which the laminate obtained in each of the above-mentioned Examples and Comparative Examples was attached was ground, the curable resin film was cured, and then the amount of warpage and the process suitability were measured. After the semiconductor wafer with protective film after backside grinding was divided into individual pieces, the shear properties were evaluated using each of the semiconductor chips with protective film obtained. For Comparative Example 1, the backside of the bump wafer was ground using a bump wafer to which a BG tape was attached, and then the amount of warpage and the process suitability were measured. After the bump wafer after backside grinding was divided into individual pieces, the shear properties were evaluated using the semiconductor chips obtained. The results are shown in Table 2. In addition, the notation "-" in each evaluation item column in Table 2 means that the semiconductor chip with the protective film could not be evaluated.

[0248] 6-1. Amount of warping (Examples 1 to 4, Comparative Examples 2 and 3) As described above, a laminate of a thermosetting resin film and a BG tape was attached to a bump wafer, and the back surface of the bump wafer was ground using a grinding device (Disco Corporation, "DGP-8760") until the thickness of the silicon wafer portion was 250 μm. After grinding, the BG tape was peeled off. Thereafter, the thermosetting resin film was cured using a heating and pressure curing device ("RAD-9100" manufactured by Lintec Corporation) under conditions of a heating temperature of 130°C, a heating time of 4 hours, and a pressure of 0.5 MPa. Then, tape (manufactured by Nichiban Corporation, product name "Cellotape (registered trademark) LP-24", tape width 24 mm) was attached to positions (three positions) that were approximately equally divided into three on the outer periphery of the wafer having the cured thermosetting resin film, and the warpage at a predetermined position (the position with the largest warpage) was measured and recorded as the amount of warpage of the wafer. Note that if the amount of warpage was 5 mm or less, it was considered to be acceptable, and if it was more than 5 mm, it was considered to be unacceptable. Comparative Example 1 As described above, the back surface of the bump wafer with the BG tape (B) attached was ground using a grinding machine (DISCO Corporation, "DGP-8760") until the thickness of the silicon wafer portion was 250 μm. After grinding, the BG tape was peeled off. Thereafter, the amount of warpage of the wafer was measured in the same manner as in Examples 1 to 4 and Comparative Examples 2 and 3 above.

[0249] 6-2. Process suitability Each of the ground semiconductor wafers with protective film obtained in the above "3-1. Amount of warpage" was loaded onto a transfer device and subjected to a process for singulation, and the process suitability was evaluated based on the following criteria. - "VG": Can be transported without problems. "G": There is some warping, but it can be transported without any problems. "B": The warping is so great that it cannot be transported. - "VB": Cannot be pasted.

[0250] 6-3.Shear properties The ground semiconductor wafers with protective film after peeling off the BG tape obtained in "3-1. Amount of warpage" above were used to evaluate shear properties in the following manner. (Examples 1 to 4, Comparative Examples 1 to 3) The ground semiconductor wafer with protective film was mounted on a DC tape using a mounting device ("D-676H" manufactured by Lintec Corporation), and then diced into individual pieces using a blade dicer ("DFD-6361" manufactured by Disco Corporation, blade: ZH05-SD2000-N1-90-CC, rotation speed: 30,000 rpm, DC speed: 30 mm / s) to obtain semiconductor chips. Using a shear tester (Nordson Advanced Technology's "Dage 4000", load cell: BS250, shear tool: SHR-062-0250), the tool contact point was set to 100 μm from the passivation film, shear was applied at a movement speed of 0.1 mm / s, and the force at which the bump broke was measured.

[0251] Fig. 20 is an explanatory diagram of a method for measuring the shear properties of a semiconductor chip with a protective film. As shown in Fig. 20, the tip of the shear tool 100 was placed at a position lower than the height BMh of the bump, where the height g2 from the bump formation surface (more specifically, the passivation film formed on the bump formation surface) was approximately 100 μm, and where there was no protective film (X) (corresponding to a position where the height g1 from the surface of the valley of the protective film (X) was approximately 50 μm). Then, the shear tool was moved at a constant speed in the direction of the arrow in Fig. 20 (a direction horizontal to the bump formation surface 41a toward the center of the bump BM) and brought into contact with the side of the bump BM, thereby performing the measurement. The thickness a of the tip of the shear tool in the moving direction of the shear tool is 90 μm. Meanwhile, the semiconductor chips obtained in the examples and comparative examples were stored in a thermostatic chamber ("OFW-300B" manufactured by AS ONE Corporation) at 150°C for 1,000 hours. The same shear test as described above was carried out on the semiconductor chips after storage to check for any decrease in strength.

[0252] 6-4.Protection The protective properties were evaluated according to the following criteria based on the location of the bump destruction when the shear properties were measured using the method described above in "6-3. Shear Properties." "G": The bump is destroyed starting from a point other than the bump neck. "B": The bump is destroyed starting from the bump neck.

[0253] [Table 2]

[0254] As is clear from Table 2, the semiconductor chips with protective film of Examples 1 to 4, in which the shoulder height h1 and valley height h2 of the protective film (X) satisfy the relationship of formula (1), have high shear strength, are resistant to shear strength reduction even after durability testing, and the bumps are destroyed from the middle when the shear testing is performed, which shows that the protective film strongly protects the bumps and has high protective performance. Furthermore, the semiconductor wafers with protective film of Examples 1 to 4 have the amount of warping suppressed to a range of 2 to 3 mm, which shows that the process suitability is good.

[0255] On the other hand, the semiconductor chip of Comparative Example 1 does not have a protective film formed thereon, so its shear strength is lower than that of the semiconductor chip with protective film of the Example, and the shear strength is significantly reduced after the durability test. Furthermore, the bumps are broken from the bump neck portion during the shear strength measurement. From these facts, it is found that the semiconductor chip of Comparative Example 1 has inferior protective performance. In addition, the protective film-attached semiconductor chips of Comparative Examples 2 and 3, in which the shoulder height h1 and valley height h2 of the protective film (X) do not satisfy the relationship of formula (1), have good shear properties because the valley height of the protective film is higher than that of the Examples. However, the protective film-attached semiconductor wafers of Comparative Examples 2 and 3 have significantly larger warpage than the protective film-attached semiconductor wafers of the Examples, and are found to have poor process suitability. [Explanation of symbols]

[0256] 1a, 1b composite sheet x Curable resin film X Protective film Y Release Sheet 11 Base material 21 Peeling layer 31 Middle Class 41 Semiconductor Wafers 41a Bump forming surface 41b back side 41c Groove 50, 50A, 50B, 50C, 50D, 50E, 50F Semiconductor wafer with protective film 100 Share Tools BM, BMa1~BMa3, BMb1~BMb3, BMc1~BMc3 bumps BMa 1st Bump BMb 2nd bump BMh Bump height Center of BCa and BCb bumps Ca, Cb A circle containing the center of the bump and having a diameter of 10% of the maximum diameter of the bump CP1, CP2 Semiconductor chip with protective film CF cutting surface GS grinding surface CS1, CS2, CS3 Straight lines showing the cutting direction of the vertical section DL division line L Length of the area with a height of 80% or less of the average height h1 of the shoulder XSa 1st shoulder XSb 2nd shoulder XV, XV' Tanibe a Thickness of the tip of the shear tool dc Total thickness of composite sheet dx Thickness of the curable resin film h1a Height of first shoulder h1b Height of second shoulder h2 Minimum height of valley h2' Thickness of the protective film at the intersection of the vertical section and the cut surface g1 Height of the tip of the shear tool from the valley surface g2 Height of the tip of the shear tool from the bump forming surface w, w1, w2, w3 Distance between bumps

Claims

1. A semiconductor wafer having a bump-forming surface with a plurality of bumps; a protective film (X) including a cured resin that covers a side surface of each of the bumps, a surface located below the side surface, and the bump formation surface, The plurality of bumps include a first bump and a second bump adjacent to each other, When the first and second bumps are viewed in plan, in a vertical cross section passing through a circle having a diameter 10% of the maximum diameter of the first bump and having the same center as the center of the first bump, and a circle having a diameter 10% of the maximum diameter of the second bump and having the same center as the center of the second bump, the protective film (X) has a first shoulder portion which is a portion in contact with the first bump and is the farthest from the bump-forming surface, a second shoulder portion which is a portion in contact with the second bump and is the farthest from the bump-forming surface, and a valley portion located between the first shoulder portion and the second shoulder portion, A semiconductor wafer with a protective film, wherein a height h1a of the first shoulder portion from the bump forming surface, a height h1b of the second shoulder portion from the bump forming surface, and a minimum height h2 of the valley portion from the bump forming surface satisfy the relationship of the following formula (1): 0.75≧[h2 / {(h1a+h1b) / 2}]≧0...Formula (1)

2. 2. The semiconductor wafer with a protective film according to claim 1, wherein a minimum height h2 of the valley portion from the bump forming surface, a height BMha of the first bump from the bump forming surface, and a height BMhb of the second bump from the bump forming surface satisfy the relationship of the following formula (2). 0.37≧[h2 / {(BMha+BMhb) / 2}]≧0...Formula (2)

3. 3. The semiconductor wafer with a protective film according to claim 1, wherein in the vertical cross section, a length L in a direction along the bump forming surface of a region of the valley portion that has a height that is 80% or less of the arithmetic average value h1 of the height h1a of the first shoulder portion from the bump forming surface and the height h1b of the second shoulder portion from the bump forming surface, and a distance w between the first bump and the second bump in the vertical cross section satisfy the relationship of the following formula (3). 0.90≧[L / w]≧0...Formula (3)

4. 3. The semiconductor wafer with a protective film according to claim 1, wherein a height h1a of the first shoulder portion from the bump forming surface and a height Bha of the first bump from the bump forming surface satisfy the relationship of the following formula (4), and a height h1b of the second shoulder portion from the bump forming surface and a height Bhb of the second bump from the bump forming surface satisfy the relationship of the following formula (5). [h1a / Bha]≧0.20...Formula (4) [h1b / Bhb]≧0.20...Formula (5)

5. 3. The semiconductor wafer with a protective film according to claim 1, wherein a height BMh of said plurality of bumps from said bump-forming surface is 15 to 300 μm.

6. 3. The semiconductor wafer with a protective film according to claim 1, wherein a surface of the semiconductor wafer opposite to the bump-formed surface is a ground surface.

7. 3. The semiconductor wafer with a protective film according to claim 1, wherein grooves serving as intended dividing lines are formed on the bump-formed surface so as not to reach the rear surface.

8. A semiconductor chip with a protective film, which is an individual product of the semiconductor wafer with a protective film according to claim 1 or 2, a protective film (X) having the first bump, the second bump, the first shoulder, the second shoulder, and the valley; A semiconductor chip with a protective film, the semiconductor chip having a cut surface formed in a direction intersecting the bump formation surface.

9. A semiconductor chip with a protective film, which is an individual product of the semiconductor wafer with a protective film according to claim 1 or 2, a cut surface formed in a direction intersecting the bump formation surface, A semiconductor chip with a protective film, wherein a height h1a of the first shoulder portion from the bump-forming surface and a height h2' of a surface of the protective film (X) from the bump-forming surface at a position where the vertical cross section and the cut surface intersect satisfy the relationship of the following formula (6). 0.75≧[h2' / h1a]≧0...Formula (6)

10. A method for protecting a semiconductor wafer having a bump-formed surface having a plurality of bumps, comprising the steps of: a step of attaching a curable resin film (x) of a composite sheet having a laminated structure of a curable resin film (x) and a release sheet (Y) so that the curable resin film (x) is in contact with the bump-forming surface, and pressing the release sheet (Y) toward the bump-forming surface with a pressing body, thereby covering the side surfaces of each bump included in the plurality of bumps, the surfaces located below the side surfaces, and the bump-forming surface with the curable resin film (x); and a step of curing the curable resin film (x) to form a protective film (X) containing a cured resin, The plurality of bumps include a first bump and a second bump adjacent to each other, When the first and second bumps are viewed in a plan view, in a vertical cross section passing through a circle including the center of the first bump and having a diameter that is 10% of the diameter of the first bump, and a circle including the center of the second bump and having a diameter that is 10% of the diameter of the second bump, the protective film (X) has a first shoulder portion that is a portion in contact with the first bump and is the farthest from the bump-forming surface, a second shoulder portion that is a portion in contact with the second bump and is the farthest from the bump-forming surface, and a valley portion located between the first shoulder portion and the second shoulder portion, A method for protecting a semiconductor wafer, wherein a height h1a of the first shoulder portion from the bump forming surface, a height h1b of the second shoulder portion from the bump forming surface, and a minimum height h2 of the valley portion from the bump forming surface satisfy the relationship of the following formula (1): 0.75≧[h2 / {(h1a+h1b) / 2}]≧0...Formula (1)

11. 3. A method for producing a semiconductor wafer with a protective film according to claim 1, comprising the steps of: (S1) and (S2) as follows: Step (S1): A step of attaching a composite sheet having a laminated structure of a curable resin film (x) and a release sheet (Y) to the bump-forming surface while pressing the curable resin film (x) as an attachment surface. - Step (S2): A method for manufacturing a semiconductor wafer with a protective film, comprising a step of forming a protective film (X) containing a cured resin having the first shoulder portion, the second shoulder portion, and the valley portion by curing a curable resin film (x).

12. A composite sheet having a laminated structure of a release sheet (Y) and a curable resin film (x), It is used to form a protective film (X) on a bump-formed surface of a semiconductor wafer having a plurality of bumps, A composite sheet that satisfies the following requirement (α): Requirement (α): When a first bump and a second bump adjacent to each other and included in the plurality of bumps are viewed in a plan view, in a vertical cross section passing through a circle that includes the center of the first bump and has a diameter that is 10% of the maximum diameter of the first bump, and a circle that includes the center of the second bump and has a diameter that is 10% of the maximum diameter of the second bump, the protective film (X) has a first shoulder that is a portion that contacts the first bump and is the farthest from the bump-forming surface, a second shoulder that is a portion that contacts the second bump and is the farthest from the bump-forming surface, and a valley that is located between the first shoulder and the second shoulder, The height h1a of the first shoulder portion from the bump-forming surface, the height h1b of the second shoulder portion from the bump-forming surface, and the thickness dx of the curable resin film (x) satisfy the following formula (α1). 0<dx / [(h1a+h1b) / 2]≦0.70...Formula (α1)

13. A composite sheet having a laminated structure of a release sheet (Y) and a curable resin film (x), It is used to form a protective film (X) on a bump-formed surface of a semiconductor wafer having a plurality of bumps, A composite sheet that satisfies the following requirement (β): Requirement (β): The thickness dc of the entire composite sheet and the thickness dx of the curable resin film (x) satisfy the following formula (β1). 0<(dx / dc)≦0.100...Formula (β1)

14. A composite sheet having a laminated structure of a release sheet (Y) and a curable resin film (x), It is used to form a protective film (X) on a bump-formed surface of a semiconductor wafer having a plurality of bumps, A composite sheet that satisfies the following requirements (α) and (β): Requirement (α): When a first bump and a second bump adjacent to each other and included in the plurality of bumps are viewed in a plan view, in a vertical cross section passing through a circle including the center of the first bump and having a diameter that is 10% of the maximum diameter of the first bump, and a circle including the center of the second bump and having a diameter that is 10% of the maximum diameter of the second bump, the protective film (X) has a first shoulder portion that is a portion in contact with the first bump and is the farthest from the bump-forming surface, a second shoulder portion that is a portion in contact with the second bump and is the farthest from the bump-forming surface, and a valley portion located between the first shoulder and the second shoulder, The height h1a of the first shoulder portion from the bump-forming surface, the height h1b of the second shoulder portion from the bump-forming surface, and the thickness dx of the curable resin film (x) satisfy the following formula (α1). 0<dx / [(h1a+h1b) / 2]≦0.70...Formula (α1) Requirement (β): The thickness dc of the entire composite sheet and the thickness dx of the curable resin film (x) satisfy the following formula (β1). 0<[dx / dc]≦0.100...Formula (β1)

Citation Information

Patent Citations

  • Semiconductor device and its manufacturing method

    JP2002270721A

  • Semiconductor device manufacturing method

    JP2012169484A

  • Semiconductor device manufacturing method

    JP2017103362A

  • Electronic component, manufacturing method of electronic component, mounting structure, and manufacturing method of mounting structure

    JP2021052072A

  • Trap control circuit for satellite broadcast television receiver

    JP1987029222A