Radio wave shielding material and radio wave shielding sheet
The use of activated carbon supported with acid in radio wave shielding materials addresses the cost issue of carbon nanofiber sheets by enhancing shielding properties effectively.
Patent Information
- Application Number
- JP2023050054
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
AI Technical Summary
Existing radio wave shielding materials, such as those using carbon nanofiber sheets, are costly and require high material expenses.
A radio wave shielding material made of activated carbon supported with acid, specifically using acids like sulfuric acid, phosphoric acid, hydrochloric acid, nitric acid, or aromatic amino acids, to enhance radio wave shielding properties.
The use of activated carbon supported with acid provides a cost-effective solution with improved radio wave shielding properties, demonstrated by significant attenuation of radio waves across various frequency ranges.
Smart Images

Figure 2024139212000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a radio wave shielding material and a radio wave shielding sheet. [Background technology]
[0002] Radio wave shielding materials that attenuate radio wave energy by reflecting and absorbing radio waves or by multiple reflection are known. For example, an electromagnetic wave absorber using a carbon nanofiber sheet obtained by carbonizing and activating a nanofiber sheet formed by electrospinning on a substrate made of a carbon fiber precursor is known (see, for example, Patent Document 1). According to this electromagnetic wave absorber, by using a carbon nanofiber sheet that is thin and dense but also has sufficient voids to absorb electromagnetic waves, it is said that electromagnetic waves can easily pass through the sheet and can easily be converted into thermal energy by collision with the fibers, thereby improving the electromagnetic wave absorption characteristics. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2008-218859 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, the electromagnetic wave absorber in Patent Document 1 is expensive because it uses a carbon nanofiber sheet. Therefore, the main object of the present invention is to provide a new radio wave shielding material that contributes to improving radio wave shielding properties. [Means for solving the problem]
[0005] The present inventors have conducted extensive research to solve the above problems and have found that the above problems can be solved by using a radio wave shielding material made of activated carbon carrying an acid.
[0006] That is, the present invention provides the following aspects. Item 1. Radio wave shielding material made of activated carbon carrying acid. Item 2. The radio wave shielding material according to Item 1, wherein the acid is at least one selected from the group consisting of sulfuric acid, phosphoric acid, hydrochloric acid, nitric acid, and aromatic amino acids. Item 3. The specific surface area of the radio wave shielding material is 50 to 2000 m 2 Item 2. The radio wave shielding material according to Item 1, wherein the R 2 is 0.1 to 0.5. Item 4. The radio wave shielding material according to Item 1, wherein the activated carbon is fibrous activated carbon. Item 5. A radio wave shielding sheet comprising the radio wave shielding material according to any one of items 1 to 4. Item 6. The radio wave shielding sheet according to item 5, wherein the radio wave shielding sheet is in the form of a nonwoven fabric. Effect of the Invention
[0007] According to the radio wave shielding material of the present invention, since it is made of activated carbon carrying an acid, it is possible to provide a novel radio wave shielding material which contributes to improving radio wave shielding properties. [Brief description of the drawings]
[0008] [Figure 1] 1 is a graph showing the evaluation results of the radio wave shielding properties of the radio wave shielding sheets in the examples, in which the attenuation (dB) from 0.2 to 0.5 THz was measured. [Diagram 2] 1 is a graph showing the evaluation results of the radio wave shielding properties of the radio wave shielding sheets in the examples, in which the attenuation (dB) from 0.5 to 2.0 THz was measured. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] <Radio wave shielding material> The radio wave shielding material of the present invention is made of activated carbon carrying an acid.
[0010] In the radio wave shielding material of the present invention, the form of the activated carbon is not particularly limited, but examples thereof include granular activated carbon, powdered activated carbon, fibrous activated carbon, and the like. From the viewpoint of ease of processing in a sheet form described later, fibrous activated carbon is more preferable. The average fiber diameter of the fibrous activated carbon is preferably 30 μm or less, more preferably about 1 to 20 μm, and even more preferably about 10 to 20 μm. The average fiber diameter in the present invention is measured and calculated using a reflecting microscope in accordance with JIS K 1477:2007 7.3.1. The particle size of the granular activated carbon and powdered activated carbon includes an integrated volume percentage D50 of 0.01 to 5 mm measured by a laser diffraction / scattering method.
[0011] The raw material type and form of the activated carbon precursor are not particularly limited. Examples of the raw material type of the activated carbon precursor include infusible or carbonized organic materials, curable resins such as phenolic resins, and the like. Examples of the organic materials include polyacrylonitrile, pitch, polyvinyl alcohol, cellulose, and the like. In addition, examples of the raw material type of the activated carbon precursor include sawdust, wood chips, wood, peat, charcoal, coconut shells, coal, oil, carbonaceous materials (petroleum coke, coal coke, petroleum pitch, coal pitch, coal tar pitch, and composites thereof), synthetic resins (phenolic resins, polyacrylonitrile (PAN), polyimide, furan resin, and the like), cellulose-based fibers (paper, cotton fibers, and the like), and composites thereof (paper-phenolic resin laminates, and the like), fullerenes, and the like. Among these, in terms of theoretical carbonization yield during carbonization, pitch is preferable, and coal pitch is more preferable. Examples of the form of the activated carbon precursor include granular, powdery, fibrous, and the like.
[0012] The method for obtaining the activated carbon used in the radio wave shielding material of the present invention is not particularly limited, but examples thereof include a method in which the above-mentioned activated carbon precursor is treated using water vapor or carbon dioxide as an activation gas, and the specific surface area can be adjusted by adjusting the activation temperature and activation time.
[0013] In the radio wave shielding material of the present invention, the specific surface area of the activated carbon before the acid is supported is set to 500 to 3500 m from the viewpoint of improving the radio wave absorption efficiency. 2 / g is preferable, and 900 to 2500m 2 / g is more preferable, and 1200 to 2000m 2 The specific surface area of the activated carbon is a value determined by the BET method (single point method) described in JIS K1477.
[0014] The radio wave shielding material of the present invention is formed by supporting an acid on activated carbon. This allows the radio wave shielding material of the present invention to contribute to improving radio wave shielding properties. Although the mechanism by which the radio wave shielding material of the present invention has excellent radio wave shielding properties due to the acid being supported on activated carbon is not entirely clear, it is presumed that the radio waves incident on the radio wave shielding material of the present invention are first attenuated by the acid, and then the attenuated radio waves are absorbed by the activated carbon, resulting in excellent radio wave shielding properties.
[0015] In the present invention, the term "acid supported" refers to a radio wave shielding material whose acidity (mmol / g) measured by the following measurement method is a positive value (greater than 0). (Method for measuring the acidity of radio wave shielding materials) Dry 0.5 g of radio wave shielding material at 115°C for at least 1 hour and measure its weight. Place the weighed radio wave shielding material in 50 mL of 0.1 N sodium hydroxide solution, shake for 30 minutes at 25°C, and then leave to stand for at least 30 minutes. After that, filter the solution to remove the radio wave shielding material. Using a titrator, titrate 10 mL of the filtrate with 0.1 N hydrochloric acid solution. Titrate a blank solution in which the radio wave shielding material is not placed in the sodium hydroxide solution under the same conditions. Then calculate the acidity of the radio wave shielding material using the following formula. (Formula) Acidity of radio wave shielding material (mmol / g) = 0.1 x (BA) x (50 / 10) x (1 / dry weight) A: The titration volume of hydrochloric acid [mL] when the radio wave shielding material is placed in sodium hydroxide and the pH is 4.3 B: Titration volume of hydrochloric acid at blank pH = 4.3 [mL]
[0016] In the radio wave shielding material of the present invention, the acid may be an inorganic acid or an organic acid. The inorganic acid may be at least one selected from the group consisting of sulfuric acid, phosphoric acid, hydrochloric acid, and nitric acid, and among these, sulfuric acid is preferred. The organic acid may be, for example, oxalic acid, malic acid, malonic acid, citric acid, or an aromatic amino acid, and among these, aromatic amino acids are preferred. The aromatic amino acid may be o-aminobenzoic acid, m-aminobenzoic acid, p-aminobenzoic acid, 3-aminosalicylic acid, 4-aminosalicylic acid, 5-aminosalicylic acid, o-aminobenzenesulfonic acid, m-aminobenzenesulfonic acid, or p-aminobenzenesulfonic acid, and among these, o-aminobenzoic acid, m-aminobenzoic acid, or p-aminobenzoic acid is more preferred. In addition, inorganic acids and organic acids may be used in combination. A preferred combination when used in combination is a combination of sulfuric acid and / or phosphoric acid with an aromatic amino acid.
[0017] The acidity of the radio wave shielding material of the present invention is, for example, 1.0 mmol / g or more, preferably 1.0 to 10.0 mmol / g, and more preferably 1.0 to 5.0 mmol / g.
[0018] The radio wave shielding material of the present invention has a specific surface area of 50 to 2000 m from the viewpoint of improving the efficiency of radio wave absorption. 2 / g, and 200 to 1000m 2 / g is preferable, and 300 to 800m 2 In the present invention, the specific surface area of the radio wave shielding material is a value determined by the BET method (single point method) described in JIS K1477.
[0019] In the radio wave shielding material of the present invention, the ratio of the specific surface area of the radio wave shielding material to the specific surface area of the activated carbon before the acid is supported thereon (specific surface area of radio wave shielding material / specific surface area of activated carbon×100) is, for example, 5 to 60%, preferably 10 to 40%, and more preferably 30 to 40%.
[0020] <Method of manufacturing radio wave shielding material> The method for producing the radio wave shielding material of the present invention is not particularly limited, but examples thereof include the following method.
[0021] First, the activated carbon is prepared. The method for obtaining the activated carbon is as described above. Next, a treatment liquid containing an acid and water is prepared. The amount of the acid in the treatment liquid may be appropriately adjusted, but for example, it may be about 10 to 90 parts by mass with respect to 100 parts by mass of the activated carbon to be immersed later.
[0022] Next, the prepared activated carbon is immersed in the treatment liquid to support the acid. For example, the activated carbon is uniformly dispersed in the treatment liquid, and then the dispersion is left to stand for a sufficient period of time. The time for immersing the activated carbon in the treatment liquid is, for example, about 1 hour or more. The ratio of the mass of the activated carbon to the volume of the treatment liquid is, for example, within the range of 5 to 50 g / L.
[0023] The activated carbon is then removed from the treatment liquid and dried. For example, natural drying, ventilation drying, hot air drying, microwave heating drying, indirect heating drying, etc. can be used for this drying. Drying is carried out while maintaining the atmospheric temperature at, for example, 70 to 130°C, preferably 80 to 115°C. In this manner, the radio wave shielding material of the present invention can be produced.
[0024] <Radio wave shielding sheet> The radio wave shielding sheet of the present invention uses the radio wave shielding material of the present invention and includes the radio wave shielding material of the present invention. Specifically, the radio wave shielding sheet of the present invention is, for example, the radio wave shielding material formed into a sheet. The form of the radio wave shielding sheet is not particularly limited, but a nonwoven fabric is preferred. The form of the nonwoven fabric is not particularly limited, but for example, a wet nonwoven fabric such as a wet papermaking nonwoven fabric, and a dry nonwoven fabric such as a needle punch nonwoven fabric are included. The radio wave shielding sheet of the present invention may contain a binder as necessary for the purpose of forming the radio wave shielding material into a sheet. The binder is not particularly limited as long as it can bond the activated carbon constituting the radio wave shielding material to each other, and for example, a fibrous binder is included, and a commercially available fibrous binder such as Melty manufactured by Unitika Ltd. can be used.
[0025] When the radio wave shielding sheet of the present invention contains a binder, the mass ratio of the binder to the radio wave shielding material of the present invention (binder / radio wave shielding material) is preferably about 5 / 95 to 50 / 50, and more preferably about 10 / 90 to 30 / 70. 2 ) the content (g / m) of the radio wave shielding material of the present invention 2 The ratio of the mass (g / m2) of the radio wave shielding sheet of the present invention (content of radio wave shielding material / mass of radio wave shielding sheet×100) is 40 to 90 mass%, and preferably 50 to 90 mass%. 2 ) vs. binder content (g / m 2 The proportion of the binder (content of binder / mass of radio wave shielding sheet×100) is 5 to 30% by mass, and preferably 10 to 30% by mass.
[0026] The radio wave shielding sheet of the present invention may contain activated carbon that does not support an acid. The form of activated carbon that does not support an acid is not particularly limited, but examples thereof include granular activated carbon, powdered activated carbon, and fibrous activated carbon. From the viewpoint of ease of processing in a sheet form, fibrous activated carbon is more preferable. The average fiber diameter of the fibrous activated carbon is preferably 30 μm or less, more preferably about 1 to 20 μm. The acidity of activated carbon that does not support an acid is more preferably 0.0 mmol / g.
[0027] In the radio wave shielding sheet of the present invention, the raw material type and form of the activated carbon precursor of the activated carbon not carrying the acid are not particularly limited. Examples of raw material types of the activated carbon precursor include infusible or carbonized organic materials, curable resins such as phenolic resins, and the like, and examples of the organic materials include polyacrylonitrile, pitch, polyvinyl alcohol, cellulose, and the like. In addition, examples of the raw material types of the activated carbon precursor include sawdust, wood chips, wood, peat, charcoal, coconut shells, coal, oil, carbonaceous materials (petroleum coke, coal coke, petroleum pitch, coal pitch, coal tar pitch, and composites thereof), synthetic resins (phenolic resin, polyacrylonitrile (PAN), polyimide, furan resin, and the like), cellulose-based fibers (paper, cotton fibers, and the like), and composites thereof (paper-phenolic resin laminates, and the like), fullerenes, and the like. Among these, in terms of theoretical carbonization yield during carbonization, pitch is preferable, and coal pitch is more preferable. Examples of the form of the activated carbon precursor include granular, powdery, fibrous, and the like.
[0028] In the radio wave shielding sheet of the present invention, the method for obtaining activated carbon not carrying the acid is not particularly limited, but examples thereof include a method in which the activated carbon precursor is treated with water vapor or carbon dioxide as an activation gas, and the specific surface area is adjusted by adjusting the activation temperature and activation time.
[0029] In the radio wave shielding sheet of the present invention, the specific surface area of the activated carbon not carrying the acid is preferably 500 to 2000 m from the viewpoint of improving the efficiency of absorbing radio waves. 2 / g is preferable, and 500 to 1500m 2 / g is more preferable, and 500 to 1000m 2 / g is more preferred.
[0030] When the radio wave shielding sheet of the present invention contains the activated carbon not carrying an acid, the mass ratio to the radio wave shielding material of the present invention (activated carbon not carrying an acid / radio wave shielding material) is 10 / 90 to 40 / 60, and preferably 20 / 80 to 35 / 65. 2 ) of the activated carbon not carrying the acid (g / m 2 The proportion of the activated carbon not carrying an acid thereon (the content of the activated carbon not carrying an acid / the mass of the radio wave shielding sheet×100) is, for example, 10 to 30% by mass, and preferably 15 to 25% by mass.
[0031] The mass of the radio wave shielding sheet of the present invention is not particularly limited, but is, for example, 30 to 300 g / m 2 The above mass is the mass per unit area (g / m2) calculated in accordance with JIS L 1913:2010 6.2. 2 ) The thickness of the radio wave shielding sheet of the present invention is not particularly limited, but may be, for example, 0.2 to 3.0 mm, preferably 0.3 to 1.5 mm. The thickness is determined by averaging values measured at three arbitrary points using a Synex Gauge manufactured by Mitutoyo Corporation, and the average value is taken as the thickness (mm) of the sheet. The apparent density of the radio wave shielding sheet of the present invention, calculated from the mass and thickness, is, for example, 0.05 to 0.4 g / cm. 3 and 0.05 to 0.25 g / cm 3 are preferred.
[0032] The radio wave shielding sheet of the present invention can be manufactured by a known method. For example, when a needle-punched nonwoven fabric is to be produced from dry nonwoven fabrics, the components including the radio wave shielding material of the present invention and the binder are carded to form a thin web, the web is needle-punched, heat-treated at a temperature at which the binder can melt, and then cooled to obtain the radio wave shielding sheet of the present invention. When a wet-laid nonwoven fabric is to be produced, a solution including the radio wave shielding material of the present invention is mixed and sheared using a device such as a pulper, beater, or refiner to prepare a uniformly dispersed slurry, and the obtained slurry is poured onto a wire, dehydrated, and dried to obtain the radio wave shielding sheet of the present invention.
[0033] <Radio frequency range and radio shielding performance of radio shielding sheet> The frequency range of radio waves shielded by the radio wave shielding sheet of the present invention is not particularly limited, but may be, for example, 0.2 to 2.0 THz, such as 0.2 to 0.5 THz and / or 0.5 to 2.0 THz. In addition, the radio wave shielding performance of the radio wave shielding sheet of the present invention is preferably an average value of attenuation from 0.2 to 0.5 THz measured by the following measurement method of -60 to -20 dB, preferably -60 to -40 dB. In addition, the radio wave shielding performance of the radio wave shielding sheet of the present invention is preferably an average value of attenuation from 0.5 to 2.0 THz measured by the following measurement method of -60 to -15 dB, preferably -60 to -28 dB. <Measurement method> The radio wave shielding sheet is cut into a 2 cm x 2 cm square to be used as a measurement sample, and transmission measurements are performed using terahertz time-domain spectroscopy (Tera Prospector, a terahertz spectrometer manufactured by Nippo Precision Co., Ltd.) The sample chamber is purged with dry air, and the reference is a state without a sample (dry air). EXAMPLES
[0034] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to the examples.
[0035] [Evaluation method] (1) The specific surface area of the activated carbon before the acid is supported, the specific surface area of the radio wave shielding material, and the specific surface area of the activated carbon without the acid supported that is included in the radio wave shielding sheet (m 2 / g) It was determined by the BET method (one point method) described in JIS K1477.
[0036] (2) The average fiber diameter of the radio wave shielding material and the average fiber diameter (μm) of the activated carbon without acid contained in the radio wave shielding sheet Measurements and calculations were made using a reflecting microscope in accordance with JIS K 1477:2007 7.3.1.
[0037] (3) Acidity of radio wave shielding material (mmol / g) 0.5 g of radio wave shielding material was dried at 115°C for at least 1 hour and its weight was measured. The radio wave shielding material whose weight had been measured was placed in 50 mL of 0.1 N aqueous sodium hydroxide solution, shaken at 25°C for 30 minutes, and then left to stand for at least 30 minutes. The solution was then filtered to remove the radio wave shielding material. 10 mL of the filtrate was titrated with 0.1 N aqueous hydrochloric acid solution using a titrator. A blank sample was also titrated under the same conditions, except that the radio wave shielding material was not placed in the aqueous sodium hydroxide solution. The acidity of the radio wave shielding material was then calculated using the following formula. (Formula) Acidity of radio wave shielding material (mmol / g) = 0.1 x (BA) x (50 / 10) x (1 / dry weight) A: The titration volume of hydrochloric acid [mL] when the radio wave shielding material is placed in sodium hydroxide and the pH is 4.3 B: Titration volume of hydrochloric acid at blank pH = 4.3 [mL]
[0038] (4) Acidity (mmol / g) of the activated carbon that does not support acid contained in the radio wave shielding sheet 0.5g of activated carbon not carrying acid contained in the radio wave shielding sheet was dried at 115℃ for 1 hour or more, and the weight was measured. The activated carbon whose weight was measured was placed in 50mL of 0.1N sodium hydroxide solution, shaken at 25℃ for 30 minutes, and then left to stand for 30 minutes or more. The solution was then filtered to remove the activated carbon. 10mL of the filtrate was titrated with 0.1N hydrochloric acid solution using a titration device. A blank state in which the activated carbon was not placed in the sodium hydroxide solution was also titrated under the same conditions. The acidity of the activated carbon not carrying acid contained in the radio wave shielding sheet was calculated using the following formula. (Formula) Acidity of activated carbon not carrying acid contained in radio wave shielding sheet (mmol / g) = 0.1 x (BA) x (50 / 10) x (1 / dry weight) A: The titration volume of hydrochloric acid when the activated carbon is placed in sodium hydroxide at pH = 4.3 [mL] B: Titration volume of hydrochloric acid at blank pH = 4.3 [mL]
[0039] (5) Evaluation of the radio wave shielding properties of radio wave shielding sheets The radio wave shielding properties were evaluated using the radio wave shielding sheet obtained. Specifically, the radio wave shielding sheet was cut into a square of 2 cm x 2 cm to prepare a measurement sample. Transmission measurements were performed using terahertz time-domain spectroscopy (Tera Prospector, a terahertz spectrometer manufactured by Nippou Precision Co., Ltd.). The sample chamber was purged with dry air, and the reference was a state without a sample (dry air). The lower the attenuation value (the larger the absolute value of the negative value), the better the radio wave shielding properties.
[0040] (6) Mass of radio wave shielding sheet (g / m 2 ) and thickness (mm) The mass of the radio wave shielding sheet was determined in accordance with JIS L 1913:2010 6.2. The thickness of the radio wave shielding sheet was determined by averaging the values measured at three arbitrary points using a Synex Gauge manufactured by Mitutoyo Corporation, and the sheet thickness (mm) was determined as the average value.
[0041] [Test example A] Example 1 (1) Manufacturing of radio wave shielding materials (1-1) Preparation of activated carbon Granular coal pitch was fed to a melt extruder, melt mixed at a melting temperature of 320°C, and spun at a discharge rate of 20g / min to obtain pitch fiber. The obtained pitch fiber was heated in air from room temperature to 354°C at a rate of 1-30°C / min for 54 minutes to perform infusibilization treatment, and an activated carbon precursor, which is an infusibilized pitch fiber, was obtained. The obtained activated carbon precursor was activated by continuously introducing a gas with a H2O concentration of 100% by volume into an activation furnace and heat-treating it at an atmospheric temperature of 875°C for 50 minutes to obtain a fibrous activated carbon. The specific surface area of the activated carbon before the acid was supported was measured using the fibrous activated carbon.
[0042] (1-2) Preparation of the acid solution contained in the radio wave shielding material of the present invention A sulfuric acid aqueous solution containing sulfuric acid at a concentration of 75% by mass as an inorganic acid was prepared. This sulfuric acid aqueous solution was stirred at a temperature of 65°C, and p-aminobenzoic acid was added as an aromatic amine to the aqueous solution and completely dissolved, and then water was added so that the ratio of the mass of the activated carbon to the volume of the treatment liquid was 20 g / L to obtain a treatment liquid. The amounts of sulfuric acid and aromatic amine charged were 30.0 parts by mass per 100 parts by mass of activated carbon. The amount of sulfuric acid charged (parts by mass) indicates the amount (parts by mass) of only sulfuric acid in the sulfuric acid aqueous solution excluding pure water.
[0043] (1-3) Supporting the acid contained in the radio wave shielding material of the present invention on activated carbon Next, 100 parts by mass of the activated carbon obtained above was immersed in the prepared solution. The solution was then stirred for 10 minutes to uniformly disperse the activated carbon in the solution. The dispersion was then allowed to stand. After being allowed to stand for 1 hour or more, the activated carbon was removed from the solution and dried at 80°C for 3 hours using a dryer to obtain the radio wave shielding material of Example 1. The physical properties of the obtained radio wave shielding material are shown in Table 1.
[0044] (2) Manufacturing of radio wave shielding sheets The obtained radio wave shielding material was mixed with a core-sheath type binder fiber (LMF2 DENIER, manufactured by Huvis, with a core melting point of 265°C, a sheath melting point of 110°C, fineness of 2.2 dtex, average fiber length of 51 mm) in which the sheath was copolymerized with PET and the core was PET, in the mass ratio shown in Table 1, and a nonwoven web was formed by carding. A plurality of the obtained nonwoven webs were laminated to the mass shown in Table 1, the fibers were entangled by needle punching, and the nonwoven web was heated at a temperature of 110°C to melt the binder fiber and fuse the binder fiber to the radio wave shielding material, resulting in a mass of 150 g / m 2 , thickness 1.1 mm, apparent density 0.14 g / cm 3 The physical properties of the radio wave shielding sheet obtained are shown in Table 1.
[0045] (3) Evaluation of radio wave shielding The radio wave shielding properties were evaluated using the radio wave shielding sheet obtained. Specifically, the radio wave shielding sheet was cut into a square of 2 cm x 2 cm to prepare a measurement sample, and transmission measurements were performed using terahertz time-domain spectroscopy (Tera Prospector, a terahertz spectrometer manufactured by Nippo Precision Co., Ltd.). The sample chamber was purged with dry air, and the reference was a state without a sample (dry air). The results of the attenuation (unit: dB) from 0.2 to 0.5 THz are shown in Figure 1, and the average values of the attenuation at each frequency obtained are shown in Table 2. The lower the attenuation value (the larger the absolute negative value), the better the radio wave shielding properties.
[0046] Example 2 (1) Manufacturing of radio wave shielding materials The radio wave shielding material was prepared as in Example 1. The physical properties of the radio wave shielding material are shown in Table 1.
[0047] (2) Preparation of activated carbon without acid support Granular coal pitch was fed to a melt extruder, melt mixed at a melting temperature of 320°C, and spun at a discharge rate of 20 g / min to obtain pitch fiber. The obtained pitch fiber was subjected to infusible treatment by increasing the temperature in air from room temperature to 354°C at a rate of 1 to 30°C / min for 54 minutes, to obtain an activated carbon precursor, which is an infusible pitch fiber. The obtained activated carbon precursor was activated by continuously introducing a gas with a HO concentration of 100% by volume into an activation furnace and heat-treating it at an atmospheric temperature of 875°C for 30 minutes, to obtain a fibrous activated carbon not carrying acid. The specific surface area of the obtained fibrous activated carbon was 825 m 2 The physical properties of the activated carbon not carrying an acid are shown in Table 1.
[0048] (3) Manufacturing of radio wave shielding sheets The prepared radio wave shielding material, a core-sheath type binder fiber with copolymerized PET in the sheath and PET in the core (LMF 2 DENIER, manufactured by Huvis, with a core melting point of 265°C, sheath melting point of 110°C, fineness of 2.2 dtex, average fiber length of 51 mm), and the prepared acid-free fibrous activated carbon were mixed in the mass ratios shown in Table 1, and a nonwoven web was formed by carding. A plurality of the obtained nonwoven webs were laminated to the mass shown in Table 1, the fibers were entangled by needle punching, and the binder fiber was melted by heating at a temperature of 110°C, and the binder fiber was fused to the radio wave shielding material and the acid-free fibrous activated carbon to form a nonwoven web of mass 150 g / m 2 , thickness 1.1 mm, apparent density 0.14 g / cm 3 The physical properties of the radio wave shielding sheet obtained are shown in Table 1.
[0049] (4) Evaluation of radio wave shielding The radio wave shielding properties were evaluated using the radio wave shielding sheet obtained. Specifically, the radio wave shielding sheet was cut into a square of 2 cm x 2 cm to prepare a measurement sample. Transmission measurements were performed using terahertz time-domain spectroscopy (Tera Prospector, a terahertz spectrometer manufactured by Nippou Precision Co., Ltd.). The sample chamber was purged with dry air, and the reference was a state without a sample (dry air). Figure 1 shows the results of attenuation (unit: dB) from 0.2 to 0.5 THz, and Table 2 shows the average attenuation values obtained for each frequency.
[0050] Example 3 (1) Manufacturing of radio wave shielding materials The radio wave shielding material was prepared as in Example 1. The physical properties of the radio wave shielding material are shown in Table 1.
[0051] (2) Preparation of activated carbon without acid support Activated carbon not carrying an acid was prepared as in Example 2. The physical properties of the activated carbon not carrying an acid are shown in Table 1.
[0052] (3) Manufacturing of radio wave shielding sheets The prepared radio wave shielding material, a core-sheath type binder fiber with copolymerized PET in the sheath and PET in the core (LMF 2 DENIER, manufactured by Huvis, with a core melting point of 265°C, sheath melting point of 110°C, fineness of 2.2 dtex, average fiber length of 51 mm), and the prepared acid-free fibrous activated carbon were mixed in the mass ratios shown in Table 1, and a nonwoven web was formed by carding. A plurality of the obtained nonwoven webs were laminated to the mass shown in Table 1, the fibers were entangled by needle punching, and the binder fiber was melted by heating at a temperature of 110°C, and the binder fiber was fused to the radio wave shielding material and the acid-free fibrous activated carbon to form a nonwoven web of mass 60 g / m 2 , thickness 0.5mm, apparent density 0.12g / cm 3 The physical properties of the radio wave shielding sheet obtained are shown in Table 1.
[0053] (4) Evaluation of radio wave shielding The radio wave shielding properties were evaluated using the radio wave shielding sheet obtained. Specifically, the radio wave shielding sheet was cut into a square of 2 cm x 2 cm to prepare a measurement sample. Transmission measurements were performed using terahertz time-domain spectroscopy (Tera Prospector, a terahertz spectrometer manufactured by Nippou Precision Co., Ltd.). The sample chamber was purged with dry air, and the reference was a state without a sample (dry air). Figure 1 shows the results of attenuation (unit: dB) from 0.2 to 0.5 THz, and Table 2 shows the average attenuation values obtained for each frequency.
[0054] Example 4 (1) Manufacturing of radio wave shielding materials (1-1) Preparation of activated carbon Granular coal pitch was fed to a melt extruder, melt mixed at a melting temperature of 320°C, and spun at a discharge rate of 20g / min to obtain pitch fiber. The obtained pitch fiber was heated in air from room temperature to 354°C at a rate of 1-30°C / min for 54 minutes to perform infusibilization treatment, and an activated carbon precursor, which is an infusibilized pitch fiber, was obtained. The obtained activated carbon precursor was activated by continuously introducing a gas with a H2O concentration of 100% by volume into an activation furnace and heat-treating it at an atmospheric temperature of 875°C for 50 minutes to obtain a fibrous activated carbon. The specific surface area of the activated carbon before the acid was supported was measured using the fibrous activated carbon.
[0055] (1-2) Preparation of the acid solution contained in the radio wave shielding material of the present invention A phosphoric acid aqueous solution containing phosphoric acid at a concentration of 50% by mass was prepared as an inorganic acid. Water was added to the prepared phosphoric acid aqueous solution so that the ratio of the mass of activated carbon to the volume of the treatment liquid was 30 g / L, to obtain a treatment liquid.
[0056] (1-3) Supporting the acid contained in the radio wave shielding material of the present invention on activated carbon Next, 100 parts by mass of the activated carbon obtained above was immersed in the prepared solution. The solution was then stirred for 10 minutes to uniformly disperse the activated carbon in the solution. The dispersion was then allowed to stand. After being allowed to stand for 1 hour or more, the activated carbon was removed from the solution and dried at 80°C for 3 hours using a dryer to obtain the radio wave shielding material of Example 1. The physical properties of the obtained radio wave shielding material are shown in Table 1.
[0057] (2) Manufacturing of radio wave shielding sheets The obtained radio wave shielding material was mixed with a core-sheath type binder fiber (LMF 2 DENIER, manufactured by Huvis, with a core melting point of 265°C, a sheath melting point of 110°C, fineness of 2.2 dtex, average fiber length of 51 mm) in which the sheath was copolymerized with PET and the core was PET, in the mass ratio shown in Table 1, and a nonwoven web was formed by carding. A plurality of the obtained nonwoven webs were laminated to the mass shown in Table 1, the fibers were entangled by needle punching, and the nonwoven web was heated at a temperature of 110°C to melt the binder fiber and fuse the binder fiber to the radio wave shielding material, resulting in a mass of 84 g / m 2 , thickness 0.40mm, apparent density 0.21g / cm 3 The physical properties of the radio wave shielding sheet obtained are shown in Table 1.
[0058] (3) Evaluation of radio wave shielding The radio wave shielding properties were evaluated using the radio wave shielding sheet obtained. Specifically, the radio wave shielding sheet was cut into a 2 cm x 2 cm square to prepare a measurement sample, and transmission measurements were performed using terahertz time-domain spectroscopy (Tera Prospector, a terahertz spectrometer manufactured by Nippo Precision Co., Ltd.). The sample chamber was purged with dry air, and the reference was a state without a sample (dry air). Figure 1 shows the results of attenuation (unit: dB) from 0.2 to 0.5 THz, and Table 2 shows the average attenuation values obtained for each frequency.
[0059] Comparative Example 1 (1) Preparation of activated carbon without acid Granular coal pitch was fed to a melt extruder, melt mixed at a melting temperature of 320°C, and spun at a discharge rate of 20 g / min to obtain pitch fiber. The obtained pitch fiber was subjected to infusible treatment by increasing the temperature in air from room temperature to 354°C at a rate of 1 to 30°C / min for 54 minutes, to obtain an activated carbon precursor, which is an infusible pitch fiber. The obtained activated carbon precursor was activated by continuously introducing a gas with a HO concentration of 100% by volume into an activation furnace and heat-treating it at an atmospheric temperature of 875°C for 50 minutes, to obtain a fibrous activated carbon not carrying acid. The specific surface area of the obtained fibrous activated carbon was 1731 m 2 The physical properties of the activated carbon not carrying an acid are shown in Table 1.
[0060] (2) Manufacturing of radio wave shielding sheets A core-sheath type binder fiber (LMF 2 DENIER, manufactured by Huvis, with a core melting point of 265°C, a sheath melting point of 110°C, a fineness of 2.2 dtex, and an average fiber length of 51 mm) in which the sheath is made of copolymerized PET and the core is made of PET, and the prepared fibrous activated carbon not carrying any acid were mixed in the mass ratio shown in Table 1, and a nonwoven web was formed by carding. A plurality of the obtained nonwoven webs were laminated to the mass shown in Table 1, the fibers were entangled by needle punching, and the nonwoven web was heated at a temperature of 110°C to melt the binder fiber, and the binder fiber and the activated carbon not carrying any acid were fused together to form a nonwoven web having a mass of 60 g / m 2 , thickness 0.4mm, apparent density 0.15g / cm 3 The physical properties of the radio wave shielding sheet obtained are shown in Table 1.
[0061] (3) Evaluation of radio wave shielding The radio wave shielding properties were evaluated using the radio wave shielding sheet obtained. Specifically, the radio wave shielding sheet was cut into a 2 cm x 2 cm square to prepare a measurement sample, and transmission measurements were performed using terahertz time-domain spectroscopy (Tera Prospector, a terahertz spectrometer manufactured by Nippo Precision Co., Ltd.). The sample chamber was purged with dry air, and the reference was a state without a sample (dry air). Figure 1 shows the results of attenuation (unit: dB) from 0.2 to 0.5 THz, and Table 2 shows the average attenuation values obtained for each frequency.
[0062] [Table 1]
[0063] [Table 2]
[0064] It is clear from FIG. 1 and Table 2 that the radio wave shielding materials of Examples 1 to 4, which are made of activated carbon carrying acid, improve the radio wave shielding properties when made into a radio wave shielding sheet.
[0065] [Test Example B] The radio wave shielding properties were evaluated using the radio wave shielding sheets of Examples 1 to 4 obtained. Specifically, the radio wave shielding sheets were cut into squares of 2 cm x 2 cm to prepare measurement samples, and transmission measurements were performed using terahertz time domain spectroscopy (Tera Prospector, a terahertz spectrometer manufactured by Nippo Precision Co., Ltd.). The sample chamber was purged with dry air, and the reference was a state without a sample (dry air). The results of the attenuation (unit: dB) from 0.5 to 2.0 THz are shown in FIG. 2, and the average values of the attenuation at each frequency obtained are shown in Table 3.
[0066] [Table 3]
[0067] 2 and Table 3, the radio wave shielding materials and radio wave shielding sheets of Examples 1 to 4 were excellent in radio wave shielding properties even in the high frequency range of 0.5 to 2.0 THz.
Claims
1. A radio wave shielding material made of activated carbon carrying acid.
2. 2. The radio wave shielding material according to claim 1, wherein the acid is at least one selected from the group consisting of sulfuric acid, phosphoric acid, hydrochloric acid, nitric acid, and aromatic amino acids.
3. The specific surface area of the radio wave shielding material is 50 to 2000 m 2 The radio wave shielding material according to claim 1, wherein the molar ratio of the radio wave shielding material to the molar ratio of the
4. 2. The radio wave shielding material according to claim 1, wherein the activated carbon is fibrous activated carbon.
5. A radio wave shielding sheet comprising the radio wave shielding material according to any one of claims 1 to 4.
6. The radio wave shielding sheet according to claim 5 , wherein the radio wave shielding sheet is in the form of a nonwoven fabric.
Citation Information
Patent Citations
Electromagnetic wave absorber
JP2008218859A