Catalyst layer and solid polymer fuel cell
The catalyst layer with controlled tungsten oxide and optional metal compounds uniformly disperses within the polymer electrolyte, addressing the issue of hydroxyl radical-induced deterioration, improving the durability and performance of polymer electrolyte fuel cells.
Patent Information
- Application Number
- JP2023050198
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
AI Technical Summary
Existing catalyst layers in polymer electrolyte fuel cells are susceptible to deterioration due to hydroxyl radicals, leading to increased resistance and reduced lifespan, with existing inhibitors often failing to provide a sufficient effect due to uneven distribution or inappropriate amounts and types of additives.
A catalyst layer containing tungsten oxide dispersed within a solid polymer electrolyte, with a controlled ratio of tungsten oxide to acid groups (W'/A) between 0.0001 and 5.0, and optionally incorporating metal compounds or ions, to uniformly disperse tungsten oxide and suppress deterioration.
The catalyst layer effectively suppresses deterioration by uniformly distributing tungsten oxide, preventing aggregation and maintaining membrane integrity, even with higher tungsten oxide amounts, thereby enhancing the durability and performance of the fuel cell.
Smart Images

Figure 2024139315000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a catalyst layer and a polymer electrolyte fuel cell, and more particularly to a catalyst layer containing an additive that has the effect of suppressing deterioration of a solid polymer electrolyte, and a polymer electrolyte fuel cell using the same. [Background technology]
[0002] Membrane electrode assemblies (MEAs) are used in the areas where electrochemical reactions occur in soda electrolysis devices, water electrolysis devices, fuel cells, etc. It is said that MEAs are deteriorated when the electrolyte is attacked by radicals generated directly by the direct reaction of oxygen and hydrogen, or by electrochemical reactions, or by radicals generated via hydrogen peroxide. For example, in fuel cells, radical attack is known to increase the resistance of the electrolyte membrane, increase cross leakage, and shorten the lifespan due to thinning. Furthermore, degradation products generated by radical attack may cause catalyst poisoning, which may result in a decrease in electrolytic performance and cell performance.
[0003] In order to solve this problem, various proposals have been made in the past. For example, Patent Document 1 states: (a) A catalyst ink containing 0.25 times the molar amount of H2WO4 and 0.05 times the molar amount of Ce(NO3)3 relative to the molar amount of sulfonic acid groups in Nafion (registered trademark), or (b) Catalyst ink containing 0.25 times the molar amount of H2WO4 and 0.05 times the molar amount of Mn(NO3)3 relative to the molar number of sulfonic acid groups in Nafion (registered trademark) MEAs fabricated using the method are disclosed. The document states that an MEA made using a catalyst ink containing degradation inhibitors (H2WO4, Ce(NO3)3, Mn(NO3)3) has a higher molecular weight retention rate of the solid polymer electrolyte than an MEA made using a catalyst ink that does not contain degradation inhibitors.
[0004] Patent Document 2 discloses a polymer electrolyte membrane containing a perfluorosulfonic acid resin and zirconia having a primary particle diameter of 10 nm, in which the ratio of the mass (A) of the perfluorosulfonic acid resin to the mass (B) of the zirconia (=A / B ratio) is 99 / 1. The same document states: (A) In the case where zirconia, which catalytically decomposes hydrogen peroxide, is added to a perfluorosulfonic acid resin, adjusting the primary particle size of the zirconia to 1 nm to 50 nm increases the specific surface area of the zirconia, and the number of hydrogen peroxide decomposition reaction sites increases dramatically; and (B) This suppresses the deterioration of the polymer electrolyte membrane. is stated.
[0005] Furthermore, Patent Document 3 states: (a) An electrolyte membrane made of Nafion (registered trademark) is immersed in a 0.1 M aqueous solution of sodium tungstate at 90° C. for 30 minutes. (b) The electrolyte membrane is then removed from the aqueous solution and washed with water; (c) The electrolyte membrane is then immersed in 0.5 M sulfuric acid at 90° C. for 30 minutes. The present invention discloses a transition metal oxide-containing solid polymer electrolyte membrane obtained by the above process. The same document states: (A) By such a method, a transition metal oxide-containing solid polymer electrolyte membrane containing 2 wt % tungsten oxide hydrate can be obtained; and (B) The electrolyte membrane containing tungsten oxide hydrate has a lower fluorine dissolution rate than the electrolyte membrane not containing tungsten oxide hydrate. is stated.
[0006] As described in Patent Documents 1 to 3, the durability of a solid polymer electrolyte is improved by adding a certain type of deterioration inhibitor to the solid polymer electrolyte. In general, the greater the amount of deterioration inhibitor added, the more the durability of the solid polymer electrolyte is improved. However, when a solid degradation inhibitor is added to a solid polymer electrolyte, if the type, average particle size, and / or amount of the degradation inhibitor is inappropriate, a sufficient degradation inhibitor effect may not be obtained, which is believed to be due to oxidation or aggregation of the degradation inhibitor.
[0007] In addition, the addition of Ce ions, which have the effect of scavenging hydroxyl radicals that accelerate degradation, is said to be effective in suppressing degradation of the electrolyte membrane. However, when only Ce ions are added, the Ce ions move within the electrolyte membrane during fuel cell operation and become unevenly distributed, which can result in insufficient degradation suppression effects. Furthermore, in Patent Document 1, a poorly soluble W compound is used as a deterioration inhibitor, but the addition of a salt of a transition metal other than W is an essential requirement. Even if a salt of a transition metal other than W is not added, the conditions required to obtain a sufficient deterioration inhibitory effect are not clarified. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Patent No. 5194448 [Patent Document 2] Patent No. 5354935 [Patent Document 3] Patent No. 4326271 Summary of the Invention [Problem to be solved by the invention]
[0009] An object of the present invention is to provide a catalyst layer capable of suppressing deterioration caused by hydroxyl radicals. Another object of the present invention is to provide a polymer electrolyte fuel cell having such a catalyst layer. [Means for solving the problem]
[0010] In order to solve the above problems, the catalyst layer according to the present invention comprises: A solid polymer electrolyte; an electrode catalyst dispersed in the solid polymer electrolyte; Tungsten oxide dispersed in the solid polymer electrolyte; Equipped with The tungsten oxide is WO x nH2O (wherein 2≦x≦3, 0≦n<3, and x and n each include a non-integer), The following formula (1) is satisfied. 0.0001 <W' / A≦5.0 …(1) Here, W' / A is the ratio of the number of moles of tungsten (W') contained in the tungsten oxide to the number of moles of acid groups (A) contained in the solid polymer electrolyte.
[0011] The polymer electrolyte fuel cell according to the present invention comprises: an electrolyte membrane containing a solid polymer electrolyte B; an anode catalyst layer bonded to one surface of the electrolyte membrane; a cathode catalyst layer bonded to the other surface of the electrolyte membrane; an anode gas diffusion layer disposed on the outer side of the anode catalyst layer; a cathode gas diffusion layer disposed on the outer side of the cathode catalyst layer; Equipped with The anode catalyst layer and / or the cathode catalyst layer comprises the catalyst layer according to the present invention. Effect of the Invention
[0012] When tungsten oxide is added to the electrolyte membrane, if the amount of tungsten oxide added is relatively excessive (i.e., when W' / A is large), the deterioration of the electrolyte membrane may be accelerated. This is because (a) Tungsten oxide aggregates in the electrolyte membrane, causing deterioration in areas with low tungsten oxide concentrations, or (b) The aggregation of tungsten oxide caused the electrolyte membrane to swell unevenly, making it more susceptible to cracking. It is thought that.
[0013] In contrast, when tungsten oxide is added to the catalyst layer, deterioration of the catalyst layer is suppressed even when the W' / A in the catalyst layer is larger than that in the electrolyte membrane. This is thought to be because the electrode catalyst contained in the catalyst layer suppresses the aggregation of tungsten oxide, making it easier for tungsten oxide to be uniformly dispersed in the catalyst layer even when the amount of tungsten oxide added is relatively large. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a graph showing the relationship between W′ / A and normalized total F-elution amount. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] An embodiment of the present invention will be described in detail below. [1. Catalyst layer] The catalyst layer according to the present invention has the following configuration.
[0016] [Configuration 1] A solid polymer electrolyte; an electrode catalyst dispersed in the solid polymer electrolyte; Tungsten oxide dispersed in the solid polymer electrolyte; Equipped with The tungsten oxide is WO x nH2O (wherein 2≦x≦3, 0≦n<3, and x and n each include a non-integer), A catalyst layer that satisfies the following formula (1). 0.0001 <W' / A≦5.0 …(1) Here, W' / A is the ratio of the number of moles of tungsten (W') contained in the tungsten oxide to the number of moles of acid groups (A) contained in the solid polymer electrolyte.
[0017] [Configuration 2] The content of the tungsten oxide is 0.1 μg / cm 2 More than 50.0μg / cm 2 2. A catalyst layer according to claim 1, wherein:
[0018] [Configuration 3] 3. The catalyst layer according to claim 1, wherein the tungsten oxide has an average primary particle size of 10 nm or more and 500 nm or less.
[0019] [Configuration 4] (a) a compound containing a metal element (excluding tungsten oxide) dispersed in the solid polymer electrolyte; (b) ions of the metal element that are ion-exchanged with protons of acid groups contained in the solid polymer electrolyte, and / or (c) Ions containing the metal element that are ion-exchanged with protons of acid groups contained in the solid polymer electrolyte 4. The catalyst layer of any one of configurations 1 to 3, further comprising:
[0020] [Configuration 5] The catalyst layer according to embodiment 4, which satisfies the following formula (2): 0.0005≦M / A≦0.15 …(2) Here, M / A is the ratio of the number of moles of the metal element (M) to the number of moles of the acid group (A).
[0021] [1.1. Solid polymer electrolyte] The catalyst layer includes a solid polymer electrolyte (catalyst layer ionomer). In the present invention, the material of the solid polymer electrolyte is not particularly limited. The solid polymer electrolyte may be either a fluorine-based electrolyte or a hydrocarbon-based electrolyte. The catalyst layer may include any one of these solid polymer electrolytes, or may include two or more of them. The type of acid group of the solid polymer electrolyte is not particularly limited. Examples of the acid group include a sulfonic acid group, a carboxylic acid group, a phosphonic acid group, and a sulfonimide group. The solid polymer electrolyte may contain only one of these acid groups, or may contain two or more of them.
[0022] Examples of fluorine-based electrolytes include Nafion (registered trademark), Flemion (registered trademark), Aquivion (registered trademark), and Aciplex (registered trademark). The fluorine-based electrolyte includes not only fully fluorinated electrolytes that do not contain C—H bonds in the polymer structure, but also partially fluorinated electrolytes that contain C—H bonds and C—F bonds in the polymer structure.
[0023] Examples of the hydrocarbon electrolyte include: (a) A wholly aromatic hydrocarbon-based electrolyte comprising polyether ether ketone, polysulfone, polyether sulfone, polyimide, polyphenylene, polyamide, polyamide imide, or a derivative thereof, into which an acid group such as a sulfonic acid group has been introduced; (b) partially aromatic hydrocarbon electrolytes having an aromatic ring in a part of the polymer chain of an aliphatic hydrocarbon electrolyte; etc.
[0024] [1.2. Electrocatalyst] The catalyst layer includes an electrode catalyst, which may consist of catalyst particles alone, or may be a catalyst particle supported on the surface of a carrier.
[0025] [1.2.1. Catalyst particles] [A. Materials] In the present invention, the material of the catalyst particles is not particularly limited. (a) Precious metals (Pt, Au, Ag, Pd, Rh, Ir, Ru, Os), (b) An alloy containing two or more precious metal elements; (c) Alloys containing one or more precious metal elements and one or more base metal elements (e.g., Fe, Co, Ni, Cr, V, Ti, etc.); etc.
[0026] Among these, the catalyst particles are preferably made of Pt or a Pt alloy, since they have high activity in the electrode reaction of the fuel cell. Examples of Pt alloys include Pt-Fe alloys, Pt-Co alloys, Pt-Ni alloys, Pt-Pd alloys, Pt-Cr alloys, Pt-V alloys, Pt-Ti alloys, Pt-Ru alloys, and Pt-Ir alloys.
[0027] [B. Particle size] The particle size of the catalyst particles is not particularly limited, and the most suitable particle size can be selected according to the purpose. In general, if the particle size of the catalyst particles is too small, the catalyst particles tend to dissolve. Therefore, the particle size of the catalyst particles is preferably 1 nm or more. On the other hand, if the particle size of the catalyst particles is too large, the mass activity decreases. Therefore, the particle size of the catalyst particles is preferably 20 nm or less. The particle size of the catalyst particles is preferably 10 nm or less, and more preferably 5 nm or less.
[0028] 1.2.2. Carrier [A. Materials] The catalyst particles may be used as they are for various applications, or may be used in a state where they are supported on the surface of a carrier. When the catalyst particles are supported on the surface of a carrier, the fine catalyst particles can be stably dispersed, and therefore the amount of catalyst used can be reduced. The material of the support is not particularly limited, but a carbon support is preferable, for example, carbon black, carbon nanotubes, carbon nanohorns, activated carbon, natural graphite, mesocarbon microbeads, glassy carbon powder, etc.
[0029] [B. Catalyst loading] When the catalyst particles are supported on the surface of the carrier, the amount of catalyst supported is not particularly limited, and the optimal amount can be selected according to the purpose. In general, if the amount of catalyst supported is too small, sufficient activity cannot be obtained. On the other hand, even if the amount of catalyst supported is more than necessary, there is no difference in effect and there is no practical benefit. For example, when catalyst particles made of Pt or a Pt alloy are supported on the surface of a carbon support, the amount of the supported catalyst is preferably 5 wt % to 70 wt %.
[0030] [1.2.3. Electrode catalyst content] The content of the electrode catalyst contained in the catalyst layer is not particularly limited, and an optimal content can be selected depending on the purpose. For example, when the electrode catalyst is one in which catalyst particles are supported on the surface of a carbon support, the ratio (=I / C) of the solid polymer electrolyte (I) to the mass (C) of the carbon support is preferably 0.5 to 1.5.
[0031] [1.3. Tungsten oxide] [1.3.1. Materials] The catalyst layer contains tungsten oxide. In the present invention, "tungsten oxide" means WO x x ≦3, 0 ≦n<3, and x and n each include a non-integer. The catalyst layer may contain any one of these tungsten oxides, or may contain two or more of them. Tungsten oxide mainly acts to decompose hydrogen peroxide to render it harmless, and therefore, by adding an appropriate amount of tungsten oxide to the catalyst layer, deterioration of the catalyst layer or the solid polymer electrolyte contained in the electrolyte membrane adjacent thereto can be suppressed.
[0032] [1.3.2. W' / A] The catalyst layer according to the present invention satisfies the following formula (1). 0.0001 <W' / A≦5.0 …(1) Here, W' / A is the ratio of the number of moles of tungsten (W') contained in the tungsten oxide to the number of moles of acid groups (A) contained in the solid polymer electrolyte.
[0033] Formula (1) represents the range of the W' / A ratio. If the W' / A ratio is too small, the effect of suppressing degradation of the solid polymer electrolyte is reduced. Therefore, the W' / A ratio must be 0.0001 or more. The W' / A ratio is preferably 0.001 or more, 0.01 or more, 0.10 or more, or more than 0.25.
[0034] When tungsten oxide is added to the catalyst layer, a relatively high deterioration suppression effect can be obtained even if the amount of tungsten oxide added is relatively large, unlike when tungsten oxide is added to the electrolyte membrane. However, if the amount of tungsten oxide added is larger than necessary, the mass transfer in the catalyst layer may be hindered. Therefore, W' / A needs to be 5.0 or less. W' / A is preferably 4.0 or less, 3.0 or less, or 2.0 or less.
[0035] [1.3.3. Average primary particle size] The term "average primary particle size" refers to the average value of the primary particle size measured for 100 or more primary particles randomly selected under a microscope. The term "primary particle diameter" refers to the length in the direction in which the length of a primary particle is at its maximum (long diameter).
[0036] In general, the smaller the average primary particle size of tungsten oxide, the higher the hydrogen peroxide decomposition effect can be obtained with a small amount of addition. However, if the average primary particle size of tungsten oxide is too small, the electrolyte creates an acidic atmosphere in the catalyst layer, making the tungsten oxide more likely to dissolve. Therefore, the average primary particle size of tungsten oxide is preferably 10 nm or more. The average primary particle size is more preferably 20 nm or more, 50 nm or more, 70 nm or more, 100 nm or more, or 150 nm or more.
[0037] On the other hand, if the average primary particle size of tungsten oxide is too large, the mass transfer in the catalyst layer may be hindered. Therefore, the average primary particle size of tungsten oxide is preferably 500 nm or less. The average primary particle size is more preferably 400 nm or less, 300 nm or less, or 200 nm or less.
[0038] [1.3.4. Tungsten oxide content] "Tungsten oxide content (μg / cm 2 )" refers to the catalyst layer of 1 cm 2 This refers to the mass of tungsten oxide per unit.
[0039] In general, the higher the content of tungsten oxide, the more the deterioration of the solid polymer electrolyte contained in the catalyst layer or the electrolyte membrane adjacent thereto is suppressed. To obtain such an effect, the content of tungsten oxide is 0.1 μg / cm 2 More preferably, the content is 0.5 μg / cm 2 More than 1.0μg / cm 2 More than 5.0μg / cm 2 or more than 10.0μg / cm 2 That's all. On the other hand, if the content of tungsten oxide is made higher than necessary, the mass transfer in the catalyst layer may be hindered. Therefore, the content of tungsten oxide is set to 50.0 μg / cm 2 The content is preferably 40.0 μg / cm or less. 2 Less than or equal to 30.0 μg / cm 2 The following is the result.
[0040] [1.4. Compounds or ions containing metallic elements] [1.4.1. Materials] The catalyst layer may consist of only a solid polymer electrolyte, an electrode catalyst, and a tungsten oxide, or may further contain a compound or ions containing a metal element in addition to these.
[0041] Here, the term "compound or ion containing a metal element" refers to (a) A compound containing a metal element (excluding tungsten oxide) dispersed in a solid polymer electrolyte; (b) an ion of a metal element that is in ion exchange with a proton of an acid group contained in a solid polymer electrolyte, or (c) Ions containing metal elements that are in ion exchange with protons of acid groups contained in the solid polymer electrolyte This refers to.
[0042] The term "ion of a metal element" refers to an ion consisting of only a metal element. "Ions containing a metal element" refers to ions containing a metal element and a nonmetal element. Examples of ions containing a metal element include Ce(CH3COO)3 + , Ce(CF3COCOOCH3)3 + , WO2 2+ , WO2(OH) + etc.
[0043] Compounds and ions containing certain metal elements mainly have the effect of scavenging radicals, and therefore, by adding an appropriate amount of a compound containing a metal element (hereinafter also referred to as a "metal compound"), an ion of a metal element, and / or an ion containing a metal element to the catalyst layer, deterioration of the solid polymer electrolyte can be suppressed. The catalyst layer may contain any one of these compounds or ions, or may contain two or more of them.
[0044] Examples of metal elements include Ce, Ag, W, Cs, Sn, Mn, Ti, Co, Ni, Zn, Zr, Ru, Rh, Pd, Pt, Pr, etc. The catalyst layer may contain any one of these metal elements, or may contain two or more of them. The metal element is preferably at least one element selected from the group consisting of Ce, Ag, Cs, Sn, Mn, and W. This is because these elements all have a strong effect of suppressing the generation of radicals or scavenging radicals.
[0045] The metal compound may be a water-soluble compound or a poorly soluble compound. When a water-soluble metal compound is used, the metal compound dissociates in the catalyst layer, and some of the protons of the acid groups of the solid polymer electrolyte are replaced with ions of the metal element or ions containing the metal element. On the other hand, when a poorly soluble metal compound is used, the metal compound is in a dispersed state in the catalyst layer. Examples of metal compounds include nitrates, sulfates, oxides, carbonates, formates, acetates, citrates, perchlorates, phosphates, chlorides, fluorides, hydroxides, and acetylacetonate compounds.
[0046] [1.4.2. M / A] The catalyst layer preferably satisfies the following formula (2). 0.0005≦M / A≦0.15 …(2) Here, M / A is the ratio of the number of moles of the metal element (M) to the number of moles of the acid group (A).
[0047] Even when only tungsten oxide is added to the catalyst layer, the deterioration of the solid polymer electrolyte can be effectively suppressed. However, when a certain metal compound, ions of a metal element, and / or ions containing a metal element are further added to the catalyst layer in addition to tungsten oxide, the deterioration of the solid polymer electrolyte is further suppressed due to the synergistic effect of these. In order to obtain such an effect, the M / A ratio is preferably 0.0005 or more. The M / A ratio is more preferably 0.001 or more, and even more preferably 0.005 or more.
[0048] On the other hand, if the M / A ratio is too large, the conductivity of the solid polymer electrolyte may decrease. Therefore, the M / A ratio is preferably 0.15 or less. The M / A ratio is more preferably 0.10 or less, more preferably 0.05 or less, more preferably 0.04 or less, and even more preferably 0.03 or less.
[0049] [2. Manufacturing method of catalyst layer] The catalyst layer according to the present invention is (a) preparing a catalyst ink containing a solid polymer electrolyte, an electrode catalyst, and tungsten oxide, and, if necessary, a metal compound, an ion of a metal element, and / or a metal element; (b) The catalyst ink is applied to a suitable substrate surface and the solvent is removed. It can be produced by the above method. Alternatively, the catalyst layer may be formed by coating or spraying a catalyst ink on the surface of the electrolyte membrane and then removing the solvent.
[0050] [3. Polymer electrolyte fuel cell] The polymer electrolyte fuel cell according to the present invention has the following configuration.
[0051] [Configuration 6] an electrolyte membrane containing a solid polymer electrolyte B; an anode catalyst layer bonded to one surface of the electrolyte membrane; a cathode catalyst layer bonded to the other surface of the electrolyte membrane; an anode gas diffusion layer disposed on the outer side of the anode catalyst layer; a cathode gas diffusion layer disposed on the outer side of the cathode catalyst layer; Equipped with 6. A polymer electrolyte fuel cell comprising the anode catalyst layer and / or the cathode catalyst layer, the catalyst layer being formed from the catalyst layer according to any one of configurations 1 to 5.
[0052] [Configuration 7] (a) Ce ions added to the electrolyte membrane; (b) a Ce compound A added to the electrolyte membrane; (c) a Ce compound B added to the water-repellent layer of the anode gas diffusion layer; and (d) Ce compound C added to the water-repellent layer of the cathode gas diffusion layer 7. The polymer electrolyte fuel cell according to claim 6, further comprising at least one selected from the group consisting of:
[0053] [Configuration 8] the anode catalyst layer comprises the catalyst layer according to any one of configurations 1 to 5; 8. The polymer electrolyte fuel cell according to claim 7, further comprising at least one selected from the group consisting of the Ce ions, the Ce compound A, and the Ce compound B.
[0054] [Configuration 9] The cathode catalyst layer comprises the catalyst layer according to any one of configurations 1 to 5; 9. The polymer electrolyte fuel cell according to aspect 7 or 8, further comprising at least one selected from the group consisting of the Ce ions, the Ce compound A, and the Ce compound C.
[0055] [Configuration 10] the electrolyte membrane contains the Ce ions and / or the Ce compound A, The ratio (=C / S) of the number of moles of Ce (C) to the number of moles of acid groups (S) in the solid polymer electrolyte B is 0.0005 or more and 0.15 or less. 10. A polymer electrolyte fuel cell according to any one of configurations 7 to 9.
[0056] [Configuration 11] the water-repellent layer of the anode gas diffusion layer contains the Ce compound B, The content of the Ce compound B is 0.1 μg / cm 2 More than 100.0μg / cm 2 is less than or equal to 11. A polymer electrolyte fuel cell according to any one of configurations 7 to 10.
[0057] [Configuration 12] the water-repellent layer of the cathode gas diffusion layer contains the Ce compound C, The content of the Ce compound C is 0.1 μg / cm 2 More than 100.0μg / cm 2 is less than or equal to 12. A polymer electrolyte fuel cell according to any one of configurations 7 to 11.
[0058] [3.1. Electrolyte membrane] The electrolyte membrane contains a solid polymer electrolyte B. In the present invention, the type of solid polymer electrolyte B contained in the electrolyte membrane is not particularly limited. The solid polymer electrolyte B may be, for example, (a) Fluorine-based electrolytes such as Nafion®, Flemion®, Aquivion®, and Aciplex®; (b) Polyetheretherketone, polysulfone, polyethersulfone, polyimide, polyphenylene, polyamide, polyamideimide, or a wholly aromatic hydrocarbon-based electrolyte comprising a derivative thereof, into which an acid group such as a sulfonic acid group has been introduced; (c) partially aromatic hydrocarbon electrolytes having an aromatic ring in a part of the polymer chain of an aliphatic hydrocarbon electrolyte; etc.
[0059] The electrolyte membrane may contain only the solid polymer electrolyte B, or may be a composite of the solid polymer electrolyte B and a reinforcing material. Examples of reinforcing materials include: (a) Porous membranes and nonwoven fabrics of fluororesins such as polytetrafluoroethylene (PTFE), perfluoroalkoxyalkane (PFA), perfluoroethylenepropene copolymer (FEP), and ethylenetetrafluoroethylene copolymer (ETFE); (b) Porous membranes and nonwoven fabrics of hydrocarbon resins such as polyethylene (PE) and polypropylene (PP), etc.
[0060] [3.2. Anode catalyst layer, cathode catalyst layer] An anode catalyst layer is bonded to one surface of the electrolyte membrane. A cathode catalyst layer is bonded to the other surface of the electrolyte membrane. In the present invention, at least one of the anode catalyst layer and the cathode catalyst layer is made of the catalyst layer according to the present invention. When only one of the anode catalyst layer and the cathode catalyst layer is the catalyst layer according to the present invention, the configuration of the other catalyst layer is not particularly limited, and an optimal one can be selected depending on the purpose. Details of the catalyst layer according to the present invention are as described above, so explanation will be omitted.
[0061] [3.3. Anode gas diffusion layer, cathode gas diffusion layer] An anode gas diffusion layer and a cathode gas diffusion layer are disposed on both sides of the MEA. In the present invention, the structure of the gas diffusion layer is not particularly limited, and an optimal structure can be selected depending on the purpose. A gas diffusion layer usually comprises a substrate made of carbon paper or the like and a water-repellent layer (microporous layer) formed on the surface of the substrate. The water-repellent layer usually comprises a composite of conductive particles such as carbon and a water-repellent resin such as polytetrafluoroethylene.
[0062] [3.4. Ce ions and Ce compounds A-C] In addition to the tungsten compound contained in the catalyst layer, the solid polymer electrolyte fuel cell according to the present invention further comprises: (a) Ce ions added to the electrolyte membrane; (b) a Ce compound A added to the electrolyte membrane; (c) a Ce compound B added to the water-repellent layer of the anode gas diffusion layer; and (d) Ce compound C added to the water-repellent layer of the cathode gas diffusion layer The present invention further includes any one or more selected from the group consisting of:
[0063] [3.4.1. Composition of Ce compounds] Both Ce ions and Ce compounds have the ability to scavenge OH radicals. Therefore, when these are added to the electrolyte membrane and / or water-repellent layer, even if OH radicals are generated from hydrogen peroxide that was not completely decomposed by the tungsten compound in the catalyst layer, the OH radicals can be scavenged by the Ce ions or Ce compounds.
[0064] The Ce compound may be a water-soluble compound or a poorly soluble compound. When a water-soluble Ce compound is used, the Ce compound dissociates and some of the protons of the acid groups of the solid polymer electrolyte are replaced with Ce ions. On the other hand, when a poorly soluble Ce compound is used, the Ce compound is dispersed in the electrolyte membrane or the water-repellent layer, and the Ce ions are gradually eluted from the Ce compound. Examples of Ce compounds include nitrates, sulfates, carbonates, formates, acetates, oxalates, citrates, perchlorates, phosphates, chlorides, fluorides, oxides, hydroxides, acetylacetonate compounds, and cerium alkoxides.
[0065] When the Ce compound A is added to the electrolyte membrane, the electrolyte membrane may contain one type of Ce compound A, or may contain two or more types of Ce compounds A. Similarly, when a Ce compound B is added to the water-repellent layer of the anode gas diffusion layer, the water-repellent layer may contain one type of Ce compound B, or may contain two or more types of Ce compound B. Similarly, when a Ce compound C is added to the water-repellent layer of the cathode gas diffusion layer, the water-repellent layer may contain one type of Ce compound C, or may contain two or more types of Ce compound C. Furthermore, when the solid polymer fuel cell contains two or more of the Ce compounds A to C, these may be compounds having the same composition, or may be compounds having different compositions.
[0066] [3.4.2. Components to which Ce ions and Ce compounds A to C are added] The member to which the Ce ions and Ce compounds are added is not particularly limited, but is preferably a water-repellent layer of an electrolyte membrane and / or a gas diffusion layer. For example, when a tungsten compound is added to the anode catalyst layer, (a) Ce ions are added to the electrolyte membrane. (b) adding Ce compound A to the electrolyte membrane, and / or (c) Add Ce compound B to the water-repellent layer of the anode gas diffusion layer. It is preferable. Alternatively, when a tungsten compound is added to the cathode catalyst layer, (a) Ce ions are added to the electrolyte membrane. (b) adding Ce compound A to the electrolyte membrane, and / or (c) Add Ce compound C to the water-repellent layer of the cathode gas diffusion layer It is preferable.
[0067] When Ce ions or Ce compounds A to C are added to a member different from the member to which the tungsten compound is added, degradation of the solid polymer electrolyte may be suppressed more than when both are added to the same member (e.g., electrolyte membrane). This is thought to be because, in addition to functioning as a degradation inhibitor in each member, Ce ions diffuse into the catalyst layer and exert a degradation suppression effect due to a synergistic effect with the tungsten compound in the catalyst layer.
[0068] [3.4.3. Content of Ce ions or Ce compounds A to C] [A. C / S ratio] The "C / S ratio" is an index representing the content of Ce ions or Ce compound A contained in the electrolyte membrane, and refers to the ratio of the number of moles (C) of all Ce contained in the electrolyte membrane to the number of moles (S) of acid groups of solid polymer electrolyte B contained in the electrolyte membrane.
[0069] When the electrolyte membrane contains Ce ions and / or Ce compound A, the C / S ratio is not particularly limited and can be selected as an optimal value according to the purpose. In general, if the C / S ratio is too small, sufficient deterioration suppression effect may not be obtained. Therefore, the C / S ratio is preferably 0.0005 or more. The C / S ratio is more preferably 0.001 or more, and more preferably 0.005 or more.
[0070] On the other hand, if the C / S ratio is too large, the battery performance may be deteriorated. Therefore, the C / S ratio is preferably 0.15 or less. The C / S ratio is more preferably 0.10 or less, and even more preferably 0.05 or less.
[0071] [B. Content of Ce compound B] "Ce compound B content (μg / cm 2 )" refers to the mass of Ce compound B per unit area of the water-repellent layer formed on the MEA side surface of the anode gas diffusion layer.
[0072] In the present invention, the content of the Ce compound B is not particularly limited, and an optimal content can be selected depending on the purpose. In general, if the content of the Ce compound B is too small, a sufficient deterioration suppression effect may not be obtained. Therefore, the content of the Ce compound B is set to 0.1 μg / cm 2 More preferably, the content is 0.5 μg / cm 2 More preferably, 1.0 μg / cm 2 That's all.
[0073] On the other hand, if the content of Ce compound B is excessive, the battery performance may be deteriorated. Therefore, the content of Ce compound B is set to 100.0 μg / cm 2 The content is preferably 50.0 μg / cm or less. 2 More preferably, 25.0 μg / cm 2 The following is the result.
[0074] [C. Content of Ce compound C] "Ce compound C content (μg / cm 2 )" refers to the mass of Ce compound C per unit area of the water-repellent layer formed on the MEA side surface of the cathode gas diffusion layer.
[0075] In the present invention, the content of the Ce compound C is not particularly limited, and an optimal content can be selected depending on the purpose. In general, if the content of the Ce compound C is too small, a sufficient deterioration suppression effect may not be obtained. Therefore, the content of the Ce compound C is set to 0.1 μg / cm 2 More preferably, the content is 0.5 μg / cm 2 More preferably, 1.0 μg / cm 2 That's all.
[0076] On the other hand, if the content of the Ce compound C is excessive, the battery performance may be deteriorated. Therefore, the content of the Ce compound C is set to 100.0 μg / cm 2 The content is preferably 50.0 μg / cm or less. 2More preferably, 25.0 μg / cm 2 The following is the result.
[0077] [4. Manufacturing method of polymer electrolyte fuel cells] The polymer electrolyte fuel cell according to the present invention can be produced by various methods. For example, a catalyst layer containing a tungsten compound may be (a) preparing a dispersion in which a solid polymer electrolyte, an electrode catalyst, and a tungsten compound are dissolved or dispersed in a solvent; (b) The dispersion is applied to the surface of the substrate, and the solvent is evaporated. It can be produced by the above method.
[0078] For example, an electrolyte membrane containing Ce ions and / or Ce compound A is (a) preparing a dispersion in which a solid polymer electrolyte B and a water-soluble or poorly soluble Ce compound A are dissolved or dispersed in a solvent; (b) The dispersion is applied to the surface of the substrate, or the dispersion is impregnated into the pores of the reinforcing material, and the solvent is volatilized. It can be produced by the above method.
[0079] For example, the water-repellent layer containing the Ce compound B or the Ce compound C is (a) preparing a dispersion in which a water-repellent resin, conductive particles, and Ce compound B or Ce compound C are dissolved or dispersed in a solvent; (b) The dispersion liquid is applied to the surface of the gas diffusion layer substrate and then fired. It can be produced by the above method.
[0080] A membrane electrode assembly (MEA) is obtained by bonding catalyst layers to both sides of the obtained electrolyte membrane. A membrane-electrode-gas diffusion layer assembly (MEGA) is obtained by disposing gas diffusion layers on both sides of the MEA. A polymer electrolyte fuel cell according to the present invention is obtained by disposing separators with gas flow paths on both sides of the MEGA.
[0081] [5. Effect] When tungsten oxide is added to the electrolyte membrane, if the amount of tungsten oxide added is relatively excessive (i.e., when W' / A is large), the deterioration of the electrolyte membrane may be accelerated. This is because (a) Tungsten oxide aggregates in the electrolyte membrane, causing deterioration in areas with low tungsten oxide concentrations, or (b) The aggregation of tungsten oxide caused the electrolyte membrane to swell unevenly, making it more susceptible to cracking. It is thought that.
[0082] In contrast, when tungsten oxide is added to the catalyst layer, deterioration of the catalyst layer is suppressed even when the W' / A in the catalyst layer is larger than that in the electrolyte membrane. This is thought to be because the electrode catalyst contained in the catalyst layer suppresses the aggregation of tungsten oxide, making it easier for tungsten oxide to be uniformly dispersed in the catalyst layer even when the amount of tungsten oxide added is relatively large. EXAMPLES
[0083] (Examples 1 to 4, Comparative Examples 1 to 3) [1. Sample preparation] [1.1. Example 1 (WO3·H2O 10.0 μg / cm 2 Anode catalyst layer containing An electrolyte solution (D2020, Nafion (registered trademark) dispersion, 1000EW, manufactured by Chemours), Pt-supported carbon, and WO3·H2O (manufactured by EM Japan, estimated average particle size: 0.05 μm) were mixed in a predetermined ratio to obtain a first catalyst ink. The obtained first catalyst ink was applied to the surface of the substrate to obtain an anode catalyst layer. The content of tungsten oxide in the anode catalyst layer was 10.0 μg / cm 2 In addition, the W' / A of the anode catalyst layer was 0.29.
[0084] The second catalyst ink was prepared in the same manner as the first catalyst ink, except that WO3·H2O was not added. The second catalyst ink was applied to the surface of the substrate to obtain a cathode catalyst layer. The electrolyte membrane contains Fe as a degradation promoter. 2+ Ions at 2μg / cm 2 A Nafion (registered trademark) membrane (NR211) containing the electrolyte membrane was used. An anode catalyst layer and a cathode catalyst layer were transferred onto both sides of the electrolyte membrane, respectively, to obtain a membrane electrode assembly.
[0085] [1.2. Example 2 (WO3·H2O 50.0 μg / cm 2 Anode catalyst layer containing The tungsten oxide content in the anode catalyst layer is 50.0 μg / cm 2 An anode catalyst layer was obtained in the same manner as in Example 1, except that the amount of WO3·H2O added to the first catalyst ink was changed so that the W' / A ratio of the anode catalyst layer was 1.4. A membrane electrode assembly was then produced in the same manner as in Example 1.
[0086] [1.3. Example 3 (WO3·H2O 10.0 μg / cm 2 Cathode catalyst layer containing A first catalyst ink containing WO3·H2O was prepared in the same manner as in Example 1. The obtained first catalyst ink was applied to the surface of a substrate to obtain a cathode catalyst layer. The content of tungsten oxide in the cathode catalyst layer was 10.0 μg / cm 2 In addition, the W' / A of the cathode catalyst layer was 0.11. Next, a second catalyst ink not containing WO3·H2O was prepared in the same manner as in Example 1. The obtained second catalyst ink was applied to the surface of the substrate to obtain an anode catalyst layer. Thereafter, a membrane electrode assembly was prepared in the same manner as in Example 1.
[0087] [1.4. Example 4 (WO3·H2O 50.0 μg / cm 2 Cathode catalyst layer containing The tungsten oxide content in the cathode catalyst layer is 50.0 μg / cm 2 A cathode catalyst layer was obtained in the same manner as in Example 3, except that the amount of WO3·H2O added to the first catalyst ink was changed so that the W' / A ratio of the cathode catalyst layer was 0.53. A membrane electrode assembly was then produced in the same manner as in Example 3.
[0088] [1.5. Comparative Example 1 (Catalyst layer without WO3·H2O added] Except for not adding WO3·H2O to the first catalyst ink, the first catalyst ink was prepared in the same manner as in Example 1. Thereafter, in the same manner as in Example 1, a membrane electrode assembly was obtained in which neither the anode catalyst layer nor the cathode catalyst layer contained WO3·H2O.
[0089] 2. Test Method A constant current durability test was carried out using the membrane electrode assembly thus prepared. The test conditions for the constant current durability test were: current density: 0.05 A / cm 2 The test conditions were: temperature: 90°C, relative humidity: 40%RH, anode gas / cathode gas: H2 / Air, and test time: 100 hours. During the durability test, the water discharged from the membrane electrode assembly was collected, and the amount of fluoride ions contained in the collected water was measured. - The amount of elution was calculated. In addition, the total F of each sample was - The amount of elution was normalized by dividing it by that of Comparative Example 1, and the normalized total F - The amount of elution was calculated.
[0090] [3. Results] Figure 1 shows the relationship between W' / A and the normalized total F - The relationship between the amount of elution and the amount of elution is shown in FIG. (1) When WO3·H2O was added to the anode or cathode catalyst layer, the normalized total F - The amount of elution was significantly reduced. (2) Example 2 has a smaller normalized total F than Example 1. - The amount of elution increased slightly. This is thought to be because the amount of WO3·H2O added in Example 2 was greater than that in Comparative Example 1, which caused some aggregation of WO3·H2O in the catalyst layer and resulted in segregation.
[0091] Although the embodiment of the present invention has been described in detail above, the present invention is not limited to the above embodiment, and various modifications are possible without departing from the gist of the present invention. [Industrial Applicability]
[0092] The catalyst layer according to the present invention can be used as a catalyst layer for a polymer electrolyte fuel cell or a polymer electrolyte water electrolysis device.
Claims
1. A solid polymer electrolyte; an electrode catalyst dispersed in the solid polymer electrolyte; Tungsten oxide dispersed in the solid polymer electrolyte; Equipped with The tungsten oxide is WO x ・nH 2 O (2≦x≦3, 0≦n<3, x and n each include a non-integer), A catalyst layer that satisfies the following formula (1): 0.0001<W' / A≦5.0...(1) Here, W' / A is the ratio of the number of moles of tungsten (W') contained in the tungsten oxide to the number of moles of acid groups (A) contained in the solid polymer electrolyte.
2. The content of the tungsten oxide is 0.1 μg / cm 2 50.0 μg / cm or more 2 2. The catalyst layer according to claim 1, wherein:
3. 2. The catalyst layer according to claim 1, wherein the tungsten oxide has an average primary particle size of 10 nm or more and 500 nm or less.
4. (a) a compound containing a metal element (excluding tungsten oxide) dispersed in the solid polymer electrolyte; (b) ions of the metal element that are ion-exchanged with protons of acid groups contained in the solid polymer electrolyte, and / or (c) ions containing the metal element that are ion-exchanged with protons of acid groups contained in the solid polymer electrolyte; The catalyst layer of claim 1 further comprising:
5. The catalyst layer according to claim 4, which satisfies the following formula (2): 0.0005≦M / A≦0.15 ... (2) Here, M / A is the ratio of the number of moles of the metal element (M) to the number of moles of the acid group (A).
6. an electrolyte membrane containing a solid polymer electrolyte B; an anode catalyst layer bonded to one surface of the electrolyte membrane; a cathode catalyst layer bonded to the other surface of the electrolyte membrane; an anode gas diffusion layer disposed on the outer side of the anode catalyst layer; a cathode gas diffusion layer disposed on the outer side of the cathode catalyst layer; Equipped with A polymer electrolyte fuel cell, wherein the anode catalyst layer and / or the cathode catalyst layer comprises the catalyst layer according to claim 1 .
7. (a) Ce ions added to the electrolyte membrane; (b) a Ce compound A added to the electrolyte membrane; (c) a Ce compound B added to the water-repellent layer of the anode gas diffusion layer; and (d) Ce compound C added to the water-repellent layer of the cathode gas diffusion layer The polymer electrolyte fuel cell according to claim 6, further comprising at least one selected from the group consisting of:
8. The anode catalyst layer comprises the catalyst layer according to claim 1 , 8. The polymer electrolyte fuel cell according to claim 7, further comprising at least one selected from the group consisting of the Ce ions, the Ce compound A, and the Ce compound B.
9. The cathode catalyst layer comprises the catalyst layer according to claim 1 , 8. The polymer electrolyte fuel cell according to claim 7, further comprising at least one selected from the group consisting of the Ce ions, the Ce compound A, and the Ce compound C.
10. the electrolyte membrane contains the Ce ions and / or the Ce compound A, The ratio (=C / S) of the number of moles of Ce (C) to the number of moles of acid groups (S) in the solid polymer electrolyte B is 0.0005 or more and 0.15 or less. The polymer electrolyte fuel cell according to claim 7.
11. the water-repellent layer of the anode gas diffusion layer contains the Ce compound B, The content of the Ce compound B is 0.1 μg / cm 2 100.0 μg / cm or more 2 Is less than or equal to The polymer electrolyte fuel cell according to claim 7.
12. the water-repellent layer of the cathode gas diffusion layer contains the Ce compound C, The content of the Ce compound C is 0.1 μg / cm 2 100.0 μg / cm or more 2 Is less than or equal to The polymer electrolyte fuel cell according to claim 7.
Citation Information
Patent Citations
Yosetsuyokaabudochitsupu
JP1976094448A
Information converting device
JP1978054935A
Solid polymer electrolyte containing transition metal oxide
JP4326271B2