Thermoelectric element
The thermoelectric element with a high Seebeck coefficient and resistivity parallel circuit configuration addresses efficiency and miniaturization challenges, achieving high conversion efficiency and ZT values for practical applications.
Patent Information
- Application Number
- JP2024031690
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-01
- Publication Date
- 2024-10-09
AI Technical Summary
Conventional thermoelectric elements face challenges in achieving high thermoelectric conversion efficiency, particularly due to low ZT values and limited miniaturization, making them unsuitable for practical applications at high temperatures and requiring improved voltage output and power generation.
A thermoelectric element design featuring a first thermoelectric material with a higher Seebeck coefficient and electrical resistivity than a second material, configured in a parallel circuit with non-contact electrodes, allowing for high thermoelectric conversion efficiency and miniaturization through a compact chip shape.
The design achieves high thermoelectric conversion efficiency and ZT values, enabling easy surface mounting and flexible installation, suitable for energy harvesting at high temperatures.
Smart Images

Figure 2024139715000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermoelectric element capable of obtaining high thermoelectric conversion efficiency. [Background technology]
[0002] 2. Description of the Related Art So-called segment-type thermoelectric elements in which a plurality of materials having different compositions are joined together are conventionally known. For example, Patent Document 1 describes a thermoelectric element in which a first electrode, a second electrode, a P-type semiconductor thin film made of a thermoelectric material, and an N-type semiconductor thin film made of a thermoelectric material are formed on a substrate, the P-type semiconductor thin film being connected to the first electrode and the N-type semiconductor thin film being connected to the second electrode, the P-type semiconductor thin film and the N-type semiconductor thin film being overlapped and bonded together, and the bonded surface being present over substantially the entire surface of the substrate.
[0003] Patent Documents 2 and 3 also describe a thermoelectric element in which a first thermoelectric material and a second thermoelectric material made of different materials are joined together, one of a pair of electrodes is connected to the first thermoelectric material, and the other of the pair of electrodes is connected to the second thermoelectric material. That is, in these conventional thermoelectric elements, electrodes are provided on the joined first thermoelectric material and second thermoelectric material, respectively, and the first thermoelectric material and the second thermoelectric material are electrically connected in series. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 10-303471 [Patent Document 2] JP 2009-32960 A [Patent Document 3] JP 2018-152464 A Summary of the Invention [Problem to be solved by the invention]
[0005] The above conventional techniques still have the following problems. In other words, the performance of a thermoelectric element required for practical thermoelectric power generation is the ZT value (dimensional figure of merit ZT (= S 2 T / ρκ): However, S, T, ρ, and κ are required to have a Seebeck coefficient (thermoelectromotive force; electromotive force generated per 1K temperature difference), absolute temperature, electrical resistivity, and thermal conductivity κ of 1 or more. In order to increase both the voltage output and power generation amount (= voltage x current) obtained by thermoelectric conversion, the material must have P-type and N-type characteristics, the absolute value of the Seebeck coefficient must be 100μV / K or more, and the power factor (Power factor PW=S 2 / ρ) is 1×10 -3 W / mK 2 It is required to have a performance higher than that. To date, research and development has been conducted on various material systems with the aim of increasing the ZT value using a single material, but the only materials in practical use with a ZT value of approximately 1 at temperatures near room temperature are Bi-Te-based materials. However, Bi-Te-based materials have low heat resistance, limiting their use to temperatures below approximately 200°C, and have low thermoelectric conversion efficiency, making the practical use of thermoelectrics difficult. On the other hand, when the above-mentioned conventional segmented thermoelectric element is used, a thermoelectric material with a heat resistance of 200°C or more can be arranged on the high temperature side, but the ZT value of each thermoelectric material constituting the segmented thermoelectric element is small, and since multiple thermoelectric elements form an electrical and thermal series circuit, the ZT value of the element as a whole is small, making it difficult to increase the thermoelectric conversion efficiency. Furthermore, there is a demand for a thermoelectric element that can be surface mounted and miniaturized.
[0006] The present invention has been made in consideration of the above-mentioned problems, and aims to provide a thermoelectric element that has high thermoelectric conversion efficiency, is capable of obtaining a high ZT value, and can be surface-mounted and miniaturized. [Means for solving the problem]
[0007] The present invention employs the following configuration to solve the above problems. That is, a thermoelectric element according to a first invention includes a first thermoelectric material part having one end and the other end, a second thermoelectric material part joined to the first thermoelectric material part directly or via a conductor, and a pair of electrodes connected to the first thermoelectric material part, the first thermoelectric material part has a higher absolute value of Seebeck coefficient and a higher electrical resistivity than the second thermoelectric material part, a joint between the first thermoelectric material part and the second thermoelectric material part has end faces on the one end side and the other end side, and the pair of electrodes are in contact with the first thermoelectric material part without contacting the second thermoelectric material part, and are formed on the end face on the one end side and the end face on the other end side of the joint.
[0008] In this thermoelectric element, the joint between the first thermoelectric material part and the second thermoelectric material part has end faces on one end side and the other end side, and a pair of electrodes are in contact with the first thermoelectric material part without contacting the second thermoelectric material part, and are formed on the end face on the one end side and the end face on the other end side of the joint.This makes it possible to surface mount and reduce the size, and to realize an element with high thermoelectric conversion efficiency and ZT value. That is, the thermoelectric element of the present invention is entirely chipped, and has electrodes formed on both end faces, which facilitates surface mounting by soldering or the like, and has a compact shape, allowing for a high degree of freedom in where it can be installed. For example, in an existing pi-shaped thermoelectric module, multiple thermoelectric elements with electrodes are electrically connected in series on a substrate, but it is possible to install the chipped thermoelectric element of the present invention without changing the structure of the thermoelectric module.
[0009] In this thermoelectric element, the first thermoelectric material section has a higher absolute value of the Seebeck coefficient and a higher electrical resistivity than the second thermoelectric material section, and a pair of electrodes are connected to one end side and the other end side of the first thermoelectric material section at a distance from each other, so that the first thermoelectric material section and the second thermoelectric material section form an electrical and thermal parallel circuit, and when a temperature difference occurs between the one end side and the other end side (heat flow occurs), an electromotive force is generated with high thermoelectric conversion efficiency. That is, the first thermoelectric material section, which has a high Seebeck coefficient (absolute value) and a high electrical resistance value and to which the pair of electrodes are connected, forms an electromotive voltage path that mainly follows the Seebeck effect, and the second thermoelectric material section, which is joined to and in contact with the first thermoelectric material section and has a low electrical resistance value, forms a current path. It is desirable that the current value flowing in the second thermoelectric material section follows Ohm's law. In this way, by configuring a parallel circuit of the electromotive voltage path and the current path, a current path that serves as a current path separate from the electromotive voltage path is formed, so that the electrical conductivity increases while maintaining the high Seebeck coefficient (absolute value) of the first thermoelectric material part, and high thermoelectric conversion efficiency and ZT value can be obtained. The second thermoelectric material section and the pair of electrodes are not directly joined, but are in electrical contact via the first thermoelectric material section. The present invention has a structure of a thermoelectric element in which multiple materials with different compositions are joined, but is characterized in that a pair of electrodes (two electrodes) are connected to the first thermoelectric material section. (Segment-type thermoelectric elements also have a structure in which multiple materials with different compositions are joined, but the pair of electrodes are connected to different thermoelectric materials, and an electrode connection method different from that of the present invention is used.)
[0010] The thermoelectric element according to the second invention is characterized in that, in the first invention, it has a pair of insulating material parts formed by covering at least the second thermoelectric material part with an end face on the one end side and an end face on the other end side of the joint body. In other words, this thermoelectric element has a pair of insulating material parts formed to cover at least the second thermoelectric material parts on the end faces on one end side and the other end side of the junction, so that the insulating material parts can prevent the pair of electrodes from contacting the second thermoelectric material parts on the end faces of the junction.
[0011] The thermoelectric element of the third invention is characterized in that, in the first or second invention, the first thermoelectric material part is joined to the upper and lower surfaces of the second thermoelectric material part, respectively, and the pair of electrodes is connected to each of the first thermoelectric material parts on the upper and lower surfaces. That is, in this thermoelectric element, the first thermoelectric material part is laminated on the upper and lower surfaces of the second thermoelectric material part, and a pair of electrodes is connected to each of the first thermoelectric material parts on the upper and lower surfaces, so that an electromotive force path is formed on the top and bottom, respectively, and higher thermoelectric conversion efficiency can be obtained.
[0012] The thermoelectric element of the fourth invention is characterized in that, in the third invention, the first thermoelectric material part is also joined to both side surfaces of the second thermoelectric material part, and the pair of electrodes are also connected to each of the first thermoelectric material parts on both side surfaces. That is, in this thermoelectric element, the first thermoelectric material part is joined to both side surfaces of the second thermoelectric material part, and a pair of electrodes is connected to each of the first thermoelectric material parts on both side surfaces, so that an electromotive force path is formed not only on the top and bottom surfaces but also on both side surfaces, thereby achieving even higher thermoelectric conversion efficiency.
[0013] The thermoelectric element of the fifth invention is characterized in that, in the first invention, the first thermoelectric material part is also joined to both end faces of the second thermoelectric material part, and the pair of electrodes are formed on the first thermoelectric material part on both end faces. That is, in this thermoelectric element, the first thermoelectric material part is also joined to both end faces of the second thermoelectric material part, and a pair of electrodes is formed on the first thermoelectric material part on both end faces, so that an electromotive voltage path is formed from the pair of electrodes to at least the first thermoelectric material part on the outer circumferential surface via the first thermoelectric material part on both end faces, thereby achieving higher thermoelectric conversion efficiency. Also, there is no need to form insulating material parts on both end faces of the second thermoelectric material part, which reduces the manufacturing process.
[0014] The thermoelectric element according to a sixth aspect of the present invention is characterized in that, in the first or second aspect of the present invention, the first thermoelectric material part has a Seebeck coefficient that is 50 μV / K or more higher in absolute value than the second thermoelectric material part, and has an electrical resistivity that is 10 times or more higher. That is, in this thermoelectric element, the first thermoelectric material section has a Seebeck coefficient that is 50 μV / K or more higher in absolute value than the second thermoelectric material section, and has an electrical resistivity that is 10 times higher. Therefore, by forming an electromotive voltage path with a sufficiently high Seebeck effect and a current path with sufficiently high electrical conductivity, it is possible to obtain a higher thermoelectric conversion efficiency and ZT value.
[0015] A thermoelectric element according to a seventh aspect of the present invention is the thermoelectric element according to the first or second aspect of the present invention, 2+δ It is characterized in that it is formed of M (wherein A is at least one of Ag and Cu, and M is at least one of S, Se and Te). In addition, the 1st Thermoelectric Materials Department A 2+δ M is the second thermoelectric material part A 2+δ It is possible to obtain a large ZT value by designing the composition of the material so that the absolute value of the Seebeck coefficient is 50 μV / K or more larger than M and the electrical resistivity is 10 times larger.
[0016] The thermoelectric element of the eighth invention is characterized in that, in the seventh invention, the first thermoelectric material part is formed of Ag—S, and the second thermoelectric material part is formed of Ag—Se or Ag—S—Se. That is, in this thermoelectric element, for example, by forming the first thermoelectric material section from Ag2S and the second thermoelectric material section from Ag2Se, it becomes possible to obtain a ZT value of 1 or more at least at room temperature.
[0017] A thermoelectric element according to a ninth invention is characterized in that, in the seventh invention, the first thermoelectric material part is formed of Cu-S, and the second thermoelectric material part is formed of Cu-Se. That is, in this thermoelectric element, for example, by forming the first thermoelectric material section from Cu2S and the second thermoelectric material section from Cu2Se, it becomes possible to obtain a ZT value of 1 or more at least at room temperature.
[0018] A thermoelectric element according to a tenth aspect of the present invention is the thermoelectric element according to any one of the first to sixth aspects of the present invention, characterized in that the first thermoelectric material portion is formed of a material containing at least Bi and Te. That is, in this thermoelectric element, the first thermoelectric material portion is made of a material containing at least Bi and Te, such as Bi-Te or Bi-Sb-Te. For example, the first thermoelectric material portion is made of Bi2Te3, and the second thermoelectric material portion is made of Cu. 0.55 Ni 0.45 (constantan), it is possible to obtain a power factor at least twice that of Bi2Te3 alone. If the first thermoelectric material section has a higher absolute value of the Seebeck coefficient and a higher electrical resistivity than the second thermoelectric material section, the thermoelectric properties will be improved compared to the first thermoelectric material section alone, regardless of the composition of the second thermoelectric material section. Effect of the Invention
[0019] According to the present invention, the following effects are obtained. That is, in the thermoelectric element according to the present invention, the joint between the first thermoelectric material part and the second thermoelectric material part has end faces on one end side and the other end side, and a pair of electrodes are in contact with the first thermoelectric material part without contacting the second thermoelectric material part, and are formed on the end face on the one end side and the end face on the other end side of the joint. Therefore, surface mounting and miniaturization are possible, and an element having high thermoelectric conversion efficiency and ZT value can be realized. Therefore, the thermoelectric element of the present invention has a high degree of freedom in installation and can be easily implemented in a circuit or module, and since it achieves high thermoelectric conversion efficiency and ZT value, it becomes possible to commercialize environmental power generation that extracts electricity highly efficiently by using temperature differences. [Brief description of the drawings]
[0020] [Figure 1]1 is a cross-sectional view showing a thermoelectric element according to a first embodiment of the thermoelectric element according to the present invention. [Diagram 2] FIG. 2 is a conceptual diagram for explaining the principle of a thermoelectric element in the first embodiment. [Diagram 3] 1 is a cross-sectional view perpendicular to an axial direction (direction from one end to the other end) showing a thermoelectric element according to a second embodiment of the present invention. FIG. [Figure 4] FIG. 11 is a perspective view showing a thermoelectric element in a second embodiment. [Diagram 5] FIG. 11 is a cross-sectional view showing a thermoelectric element in an axial direction (direction from one end to the other end) in a third embodiment of the thermoelectric element according to the present invention. [Figure 6] FIG. 2 is a cross-sectional view showing an example of a thermoelectric element of the present invention produced in order to demonstrate the principle of the thermoelectric element of the present invention. [Figure 7] 4 is a graph showing the results of evaluating the power generation characteristics of a thermoelectric element in an example of a thermoelectric element according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] A first embodiment of a thermoelectric element according to the present invention will be described below with reference to Figures 1 and 2. In the drawings used in the following description, the scale is appropriately changed as necessary to make each part recognizable or easily recognizable.
[0022] As shown in Figures 1 and 2, the thermoelectric element 10 of this embodiment comprises a first thermoelectric material part 1 having one end 1a and the other end 1b, a second thermoelectric material part 2 joined to the first thermoelectric material part 1 directly or via a conductor 2a, and a pair of electrodes 3 connected to the first thermoelectric material part 1. When the first thermoelectric material part 1 and the second thermoelectric material part 2 are joined via the conductor 2a, the conductor 2a also functions as an intermediate layer. The conductor 2a is, for example, a conductive bonding material such as solder or In. The first thermoelectric material section 1 has a higher Seebeck coefficient and a higher electrical resistivity than the second thermoelectric material section 2 . The joint 4 of the first thermoelectric material part 1 and the second thermoelectric material part 2 is formed in a chip shape having end faces on one end side and the other end side. That is, the joint 4 is in a plate or rectangular parallelepiped shape, and one end 1a and the other end 1b of the first thermoelectric material part 1 are disposed on both end faces. The thickness of the first thermoelectric material part 1 (i.e., the thickness in the stacking direction of the first thermoelectric material part 1 and the second thermoelectric material part 2) is preferably 100 nm to 10 mm, and may be 1 μm to 3 mm. The thickness of the second thermoelectric material part 2 is preferably 0.1 mm to 10 mm, and may be 0.5 mm to 3 mm.
[0023] The pair of electrodes 3 are in contact with the first thermoelectric material part 1 without being in contact with the second thermoelectric material part 2 . That is, the thermoelectric element 10 of this embodiment has a pair of insulating material parts 5 formed by covering at least the second thermoelectric material part 2 with the end face on one end 1a side and the end face on the other end 1b side of the above-mentioned joint body 4. The pair of electrodes 3 are formed on an end surface of the bonded body 4 at one end 1a and an end surface of the bonded body 4 at the other end 1b. That is, the pair of electrodes 3 are connected to one end 1a and the other end 1b of the first thermoelectric material part 1 at a distance from each other. Furthermore, the pair of electrodes 3 are not in contact with the second thermoelectric material part 2 and are disposed apart from the second thermoelectric material part 2 . Moreover, the end face of the joined body 4 on the one end 1a side and the end face on the other end 1b side are disposed opposite to each other.
[0024] The first thermoelectric material part 1 is joined to the top and bottom surfaces of the second thermoelectric material part 2, respectively. Further, a pair of electrodes 3 are connected to the first thermoelectric material parts 1 on the upper and lower surfaces, respectively. That is, the pair of electrodes 3 are connected to the surfaces of the first thermoelectric material part 1 and are formed on both end surfaces of the joined body 4, covering the pair of insulating material parts 5. The pair of electrodes 3 extend beyond the pair of insulating material parts 5 to reach the upper and lower surfaces of the joined body 4 (the first thermoelectric material part 1). In this manner, the pair of electrodes 3 are in contact with and connected to only the first thermoelectric material portion 1 , and are not in contact with the second thermoelectric material portion 2 due to the pair of insulating material portions 5 .
[0025] It is preferable that the first thermoelectric material section 1 has a Seebeck coefficient that is at least 50 μV / K larger in absolute value than the second thermoelectric material section 2, and an electrical resistivity that is at least 10 times larger. The electrical resistivity of the first thermoelectric material unit 1 at room temperature is 10 -5 Ωcm or less is preferable. For example, the first thermoelectric material unit 1 and the second thermoelectric material unit 2 are both A 2+δ M (wherein A is at least one of Ag and Cu, and M is at least one of S, Se and Te). The range of δ is preferably -0.5≦δ≦+0.5, and more preferably -0.05 to +0.02.
[0026] In the present invention, the thermoelectric material is defined as a material having a Seebeck coefficient with an absolute value of 0.1 μV / K or more. That is, the absolute value of the Seebeck coefficient of the second thermoelectric material section 2 is 0.1 μV / K or more. Furthermore, the absolute value of the Seebeck coefficient of the first thermoelectric material portion 1 is preferably 10 mV / K or less. Furthermore, when the electrical resistivity of the first thermoelectric material part 1 at room temperature is 10 mΩcm or less, it is preferable that the first thermoelectric material part 1 is thinner than the second thermoelectric material part 2. Furthermore, when the electrical resistivity of the first thermoelectric material part 1 at room temperature is 10 mΩcm or less, and the electrical resistivity of the second thermoelectric material part 2 at room temperature is 1 mΩcm or less and the thermal conductivity is 10 W / mK or more, it is preferable that the thickness of the first thermoelectric material part 1 is thicker than the thickness of the second thermoelectric material part 2.
[0027] A 2+δIn the case of an N-type thermoelectric element, for example, a configuration in which the first thermoelectric material part 1 is made of Ag-S and the second thermoelectric material part 2 is made of Ag-Se or Ag-S-Se can be used as M. In the case of a P-type thermoelectric element, for example, a configuration in which the first thermoelectric material part 1 is made of Cu-S and the second thermoelectric material part 2 is made of Cu-Se can be used. For example, the first thermoelectric material section 1 can be made of Ag2S, and the second thermoelectric material section 2 can be made of Ag2Se. Ag2S has a Seebeck coefficient that is 50 μV / K or more higher in absolute value than Ag2Se, and an electrical resistivity that is 10 times or more higher. Alternatively, the first thermoelectric material portion 1 may be made of Cu2S, and the second thermoelectric material portion 2 may be made of Cu2Se. Cu2S has a Seebeck coefficient that is 50 μV / K or more higher in absolute value than Cu2Se, and an electrical resistivity that is 10 times higher. The first thermoelectric material portion 1 may be made of a material containing at least Bi and Te, such as Bi-Te or Bi-Sb-Te. For example, the first thermoelectric material portion 1 may be made of Bi2Te3 or (Bi 0.7 Sb 0.3 ) Te3, and the second thermoelectric material portion 2 is formed of Cu 0.55 Ni 0.45 (Constantan). Bi2Te3 and (Bi 0.7 Sb 0.3 ) Te3 is Cu 0.55 Ni 0.45 The absolute value of the Seebeck coefficient is 50 μV / K or more higher and the electrical resistivity is 10 times higher than that of the It is also possible to employ the first thermoelectric material portion 1 in which impurities such as Ru or Cu are added to the material containing Bi and Te.
[0028] In this manner, the first thermoelectric material part 1 is made of a semiconductor material or insulating material with high electrical resistance, such as a low thermal conductive chalcogenide material, and the second thermoelectric material part 2 is made of a conductive material with low electrical resistance, such as a semiconductor material or an alloy. Moreover, it is preferable that both the first thermoelectric material part 1 and the second thermoelectric material part 2 have low thermal conductivity in order to increase the temperature difference applied to the thermoelectric element 10. In particular, it is preferable that the first thermoelectric material part 1 has a thermal conductivity of 10 W / mK or less in order to obtain a high thermoelectromotive force by the Seebeck effect. The thermal conductivity of the first thermoelectric material part is preferably 0.02 W / mK or more.
[0029] The first thermoelectric material part 1 may be a thin film, but the second thermoelectric material part 2 is preferably a conductor bulk thicker than the first thermoelectric material part 1 . The thickness of the first thermoelectric material part 1 (i.e., the thickness in the stacking direction of the first thermoelectric material part 1 and the second thermoelectric material part 2) is preferably 100 nm to 10 mm, and may be 1 μm to 3 mm. The thickness of the second thermoelectric material part 2 is preferably 0.1 mm to 10 mm, and may be 0.5 mm to 3 mm. When the first thermoelectric material part 1 and the second thermoelectric material part 2 are joined via the conductor 2a, a conductive joining material such as solder or In can be used as the conductor 2a. Note that the electrical resistivity of the conductor 2a used in this joining part is preferably approximately the same as the electrical resistivity of the second thermoelectric material part 2. In many cases, the electrical resistivity of alloy materials and solder materials is similar (10 -4 For example, Cu as an alloy material 0.55 Ni 0.45 When constantan is used, the electrical resistivities of the second thermoelectric material part 2 and the solder are approximately the same, so that for the first thermoelectric material part 1, the solder can essentially be regarded as part of the second thermoelectric material part 2 from the standpoint of electrical conductivity, thereby increasing the freedom in designing the thermoelectric element. The pair of electrodes 3 may be made of, for example, Ag paste or Ag solder, and are formed on both end surfaces of the bonding body 4 by dipping or the like. The material of the pair of electrodes 3 has an electrical resistivity of 10 -4 Ωm or less is adopted. The insulating material portion 5 is made of, for example, alumina, SiO2, or the like.
[0030] The method for manufacturing the thermoelectric element 10 of this embodiment includes a joining process for joining the second thermoelectric material part 2 and the first thermoelectric material part 1, and an electrode formation process for forming a pair of electrodes 3 on the first thermoelectric material part 1. For example, in the joining step, the second thermoelectric material part 2 and the first thermoelectric material part 1 are joined together with a conductive joining material such as solder. In addition, in the above bonding process, various thin film growth methods (vapor phase growth methods such as PVD, sputtering, and CVD) are adopted. When a chalcogenide material is used for the first thermoelectric material part 1, it is preferable to form the first thermoelectric material part 1 as a film on the second thermoelectric material part 2 by the MBD method (molecular beam deposition method).
[0031] In the above bonding step, the first thermoelectric material part 1 may be formed as a film on the second thermoelectric material part 2 by a sol-gel method. In addition, in the above-mentioned joining process, a hot pressing method may be used in which, in a state in which the powder that will become the first thermoelectric material part 1 and the powder that will become the second thermoelectric material part 2 are stacked, the first thermoelectric material part 1 and the second thermoelectric material part 2 are sintered, and the first thermoelectric material part 1 and the second thermoelectric material part 2 are joined together at the same time.
[0032] As described above, in the thermoelectric element 10 of the present embodiment, the joint 4 of the first thermoelectric material part 1 and the second thermoelectric material part 2 has end faces on one end side and the other end side, and the pair of electrodes 3 are in contact with the first thermoelectric material part 1 without contacting the second thermoelectric material part 2, and are formed on the end face on one end 1a side and the end face on the other end 1b side of the joint 4, so that surface mounting and miniaturization are possible, and an element having high thermoelectric conversion efficiency and ZT value can be realized. That is, the thermoelectric element 10 of the present embodiment is formed as a chip entirely, and the electrodes 3 are formed on both end faces, so that surface mounting by solder or the like is easy, and the compact shape provides a high degree of freedom in the installation location.
[0033] In this thermoelectric element 10, the first thermoelectric material part 1 has a higher Seebeck coefficient and higher electrical resistivity than the second thermoelectric material part 2, and a pair of electrodes 3 are connected to one end 1a and the other end 1b of the first thermoelectric material part 1 at a distance from each other. Therefore, the first thermoelectric material part 1 and the second thermoelectric material part 2 form a parallel circuit, and when a temperature difference occurs between the one end 1a and the other end 1b (heat flow occurs), an electromotive force is generated with high thermoelectric conversion efficiency.
[0034] That is, as shown in FIG. 2, the first thermoelectric material part 1, which is connected to a pair of electrodes 3 and has a high Seebeck coefficient (absolute value) and a high electrical resistance, forms an electromotive voltage path R1 that mainly follows the Seebeck effect, and the second thermoelectric material part 2, which is joined to and in contact with the first thermoelectric material part 1 and has a low electrical resistance, forms a current path R2. It is desirable that the current value flowing in the second thermoelectric material part 2 follows Ohm's law. In this way, by forming a parallel circuit of the electromotive voltage path R1 and the current path R2, the current path R2, which is a current path separate from the electromotive voltage path R1, is formed, and the electrical conductivity flowing between the pair of electrodes 3 increases while maintaining the high Seebeck coefficient (absolute value) of the first thermoelectric material part 1, and a high thermoelectric conversion efficiency and ZT value can be obtained. Note that the arrow Y in FIG. 2 indicates the heat flow direction (the direction in which the heat flux flows, the direction in which a temperature difference occurs).
[0035] In addition, the joint body 4 has a pair of insulating material parts 5 formed to cover at least the second thermoelectric material parts 2 on the end face on one end 1a side and the end face on the other end 1b side. Therefore, the insulating material parts 5 can prevent the pair of electrodes 3 from contacting the second thermoelectric material parts 2 on the end faces of the joint body 4. Furthermore, the first thermoelectric material part 1 is stacked on the upper and lower surfaces of the second thermoelectric material part 2, respectively, and a pair of electrodes 3 is connected to the first thermoelectric material parts 1 on the upper and lower surfaces, respectively, so that an electromotive force path R1 is formed on the upper and lower surfaces, respectively, and higher thermoelectric conversion efficiency can be obtained.
[0036] Furthermore, since the first thermoelectric material part 1 has a Seebeck coefficient whose absolute value is 50 μV / K or more higher than that of the second thermoelectric material part 2 and whose electrical resistivity is 10 times higher, an electromotive voltage path R1 with a sufficiently high Seebeck effect and a current path R2 with sufficiently high electrical conductivity are formed, thereby making it possible to obtain higher thermoelectric conversion efficiency and ZT value. The absolute value of the Seebeck coefficient of the first thermoelectric material part 1 may be 100 μV / K or more greater than the absolute value of the Seebeck coefficient of the second thermoelectric material part 2. The greater the difference between the absolute value of the Seebeck coefficient of the first thermoelectric material part 1 and the absolute value of the Seebeck coefficient of the second thermoelectric material part 2, the more desirable it is, and although there is no particular upper limit, it may be 10,000 μV / K.
[0037] In addition, by forming the first thermoelectric material portion 1 from Ag2S and the second thermoelectric material portion 2 from Ag2Se, the output factor (PW=S 2 / ρ) becomes large, making it possible to obtain an N-type thermoelectric element with a ZT value of 1 or more at least at room temperature. In addition, by forming the first thermoelectric material portion 1 from Cu2S and the second thermoelectric material portion 2 from Cu2Se, the output factor (PW=S 2 / ρ) becomes large, making it possible to obtain a P-type thermoelectric element with a ZT value of 1 or more at least at room temperature. The first thermoelectric material portion 1 is made of Bi2Te3, and the second thermoelectric material portion 2 is made of Cu. 0.55 Ni 0.45 By forming it from Bi2Te3 (constantan), it is possible to obtain an N-type thermoelectric element having a power factor at least twice that of a single substance of Bi2Te3. The first thermoelectric material portion 1 is made of (Bi 0.7 Sb 0.3 )2Te3, and the second thermoelectric material part 2 is formed of Cu 0.55 Ni 0.45 (Constantan) to form at least (Bi 0.7 Sb 0.3 It is now possible to obtain a P-type thermoelectric element with a power factor approximately twice that of a single element of 2Te3.
[0038] Next, second and third embodiments of the thermoelectric element according to the present invention will be described below with reference to Fig. 3 to Fig. 6. In the following description of each embodiment, the same components as those described in the above embodiments are denoted by the same reference numerals, and the description thereof will be omitted.
[0039] The second embodiment differs from the first embodiment in that, in the first embodiment, the first thermoelectric material part 1 is joined to the top and bottom surfaces of the second thermoelectric material part 2, respectively, and a pair of electrodes 3 is connected to each of the first thermoelectric material parts 1 on the top and bottom surfaces, whereas in the thermoelectric element 20 of the second embodiment, as shown in Figures 3 and 4, the first thermoelectric material part 1 is joined to both side surfaces of the second thermoelectric material part 2, respectively, and a pair of electrodes 3 is also connected to each of the first thermoelectric material parts 1 on both side surfaces. The joint body 4 is formed in a plate-like or rectangular parallelepiped chip shape, and the top and bottom surfaces of the second thermoelectric material part 2 are perpendicular to both side surfaces of the second thermoelectric material part 2 .
[0040] That is, in the second embodiment, the first thermoelectric material part 1 covers the entire outer peripheral surface of the second thermoelectric material part 2 , and the first thermoelectric material part 1 is joined to all four outer peripheral surfaces of the second thermoelectric material part 2 . As described above, in the thermoelectric element 20 of the second embodiment, the first thermoelectric material part 1 is joined to both side surfaces of the second thermoelectric material part 2, and a pair of electrodes 3 is connected to each of the first thermoelectric material parts 1 on both side surfaces. As a result, an electromotive force path R1 is formed not only on the top and bottom surfaces but also on both side surfaces, and an even higher thermoelectric conversion efficiency can be obtained.
[0041] Next, the third embodiment differs from the second embodiment in that, while in the second embodiment, the first thermoelectric material part 1 is joined to the top and bottom surfaces and both side surfaces of the second thermoelectric material part 2, in the thermoelectric element 30 of the third embodiment, as shown in FIG. 5, the first thermoelectric material part 1 is joined to both end surfaces of the second thermoelectric material part 2, and a pair of electrodes 3 are formed on the first thermoelectric material part 1 on both end surfaces.
[0042] That is, in the third embodiment, the entire surface of the chip-like second thermoelectric material section 2 is covered with the first thermoelectric material section 1 . As described above, in the thermoelectric element 30 of the third embodiment, the first thermoelectric material part 1 is joined to both end faces of the second thermoelectric material part 2, and a pair of electrodes 3 is formed on the first thermoelectric material parts 1 on both end faces, so that an electromotive voltage path R1 is formed from the pair of electrodes 3 to each first thermoelectric material part 1 on the outer circumferential surface via the first thermoelectric material parts 1 on both end faces, thereby achieving higher thermoelectric conversion efficiency. Also, there is no need to form insulating material parts on both end faces of the second thermoelectric material part 2, which reduces the manufacturing process. EXAMPLES
[0043] In order to demonstrate the principle of the thermoelectric properties of the present invention, a sample as shown in FIG. 6 was produced as an example, and the evaluation results are shown in Tables 1 and 2. In the examples of the present invention, the first thermoelectric material part and the second thermoelectric material part were fabricated using the materials and manufacturing methods described in the above embodiment, and their thermoelectric properties (conductivity type determination (P / N type determination), Seebeck coefficient, electrical resistivity, and power factor) at room temperature (300 K) were investigated. As a comparative example of the present invention, a thermoelectric element made of a single thermoelectric material was evaluated in the same manner as in the examples of the present invention. Each example was produced as follows. In this embodiment of the present invention, for evaluation purposes, the first thermoelectric material part 1 is joined only to the top surface of the second thermoelectric material part 2. In addition, a pair of electrodes 3 are formed on the top surface of the first thermoelectric material part 1.
[0044] <Examples 1 and 2> <Examples 9 to 12> (Solder joint) First, a Bi-Te bulk sintered body (or a Bi-Sb-Te bulk sintered body) to become the first thermoelectric material part and a Cu-Ni alloy plate or a Cu plate to become the second thermoelectric material part were prepared, cut to a specified size, and the joining surfaces were polished. After that, a solder foil was placed on the bonding surface between the Bi-Te bulk sintered body and the Cu-Ni alloy plate or Cu plate, and the Bi-Te bulk sintered body was bonded to the Cu-Ni alloy plate or Cu plate by using a hot press machine and utilizing solder melting. That is, the second thermoelectric material part was bonded to the first thermoelectric material part through an intermediate layer of solder as a conductor. The above bonding conditions were a pressure of 100 MPa, a bonding temperature of 250 degrees, and a holding time of about 5 minutes. After visually confirming the melting of the solder, a cooling process and a process of reducing the pressure were carried out. After that, two pairs of electrodes were formed on the first thermoelectric material part side (Bi-Te side) using an Ag paste or the like to obtain Examples 1 and 2.
[0045] <Example 3> (MBD film formation) First, an Ag2S thin film serving as the first thermoelectric material part was formed on an Ag2Se bulk sintered body serving as the second thermoelectric material part using an MBD (molecular beam epitaxy) apparatus. The Ag2Se bulk sintered body was formed by the SHS (self-propagating high-temperature synthesis) method. In the film formation by the above MBD method, the substrate temperature was set at room temperature, and a cell containing Ag and S as raw materials was heated to an appropriate temperature with a heater to perform film formation, thereby obtaining a single-phase thin film of Ag2S serving as the first thermoelectric material part. In addition, it has been confirmed by X-ray diffraction experiments that the Ag2S thin film and the Ag2Se bulk sintered body are crystalline materials. Ag2S 1-x Se x In the system, in the low-temperature phase near room temperature below the phase transition temperature, when x ≤ 0.6, it has the same crystal structure as Ag2S (monoclinic, space group P21 / c), and when x ≥ 0.7, it has the same crystal structure as Ag2Se (orthorhombic, space group P212121). (In the composition range of 0.6 < x < 0.7, depending on the film formation conditions, a mixed phase or a different crystal structure is taken.) The production of the electrodes is the same as in Examples 1 and 2.
[0046] <Examples 4 to 8> <Examples 13 to 17> (Hot press) First, the raw material powders (e.g., Ag, S, Cu, etc.) for the first thermoelectric material part and the second thermoelectric material part are weighed out to a predetermined stoichiometric ratio, mixed, molded using a press, and then heat-treated at a predetermined temperature to obtain, for example, a sintered body of a single phase of AgS. When a chalcogenide containing S, Se, or Te is used, a single-phase sintered body can be obtained even by using the self-heating reaction method. If an unreacted phase is confirmed by the X-ray diffraction experiment, the sintered body is crushed into powder and the above process is repeated. Since the X-ray diffraction experiment shows that a single-phase sintered body is obtained, this process is repeated.
[0047] After the single-phase sintered body is obtained, the sintered body is pulverized in a mortar or the like to obtain, for example, Ag2S, Ag2Se, Cu, etc. 2-δ S, Cu 2-δ Obtain Se powder. These powders are heated and pressurized in a hot press to produce bulk bodies of the first and second thermoelectric material parts, and at the same time, a joint body of the first and second thermoelectric material parts is produced. Note that, during the hot press, Ag2S, Ag2Se, Cu, etc. are used in consideration of density. 2-δ S, Cu 2-δ The Se is weighed out to achieve the desired thickness, and the raw materials are added in order and molded.
[0048] In addition, the bonding conditions using the hot press are a pressure of 100 MPa, a predetermined holding temperature, and a holding time of 20 minutes to form a bonded body. Thereafter, the bonded body is cut using a wire saw or the like to obtain a chip-shaped bonded body of, for example, 17 mm×3 mm×2 mmt. The electrodes were prepared in the same manner as in Examples 1 and 2.
[0049] <Method of evaluating thermoelectric elements> When a temperature difference ΔT is applied to a thermoelectric element, a voltage ΔV proportional to the temperature difference is generated. This phenomenon is called the Seebeck effect, and the generated voltage is called thermoelectromotive force, with the proportionality coefficient S = ΔV / ΔT defined as the Seebeck coefficient S. In other words, to measure the Seebeck coefficient, it is necessary to measure both the potential difference (thermoelectromotive force) between two terminals and the temperature difference. The Seebeck coefficient was measured using two commercially available Peltier elements, one of which was cooled and the other was wired to be heated so as to create a temperature difference between the two Peltier elements, with a temperature difference of 0.1 to 5°C. The thermocouple used for the measurements was a T-type thermocouple (Cu-Constantan). An extremely thin type, about 20 microns, was selected for this thermocouple, and a rubber material with high electrical insulation and heat insulation was used to apply a load, achieving good thermal and electrical contact between the material and the thermocouple. In addition, a two-terminal method called the thermoelectric probe method was adopted, and the potential difference (thermoelectromotive force) between the two terminals was measured using the Cu wiring of two T-type thermocouples. The relationship between the thermoelectromotive force ΔV and the temperature difference ΔT was plotted, and the Seebeck coefficient was evaluated from the linear relationship near the zero temperature difference (near the origin of ΔV / ΔT). The P type and N type (conductivity type) were determined from the sign of the measured Seebeck coefficient. When joining the first thermoelectric material part and the second thermoelectric material part, it is desirable to align the P type / N type polarity to be the same, i.e., to join P types together or N types together, but it is also possible to join opposite polarities, i.e., P type and N type together. Even in such a case, the first thermoelectric material part has a higher absolute value of the Seebeck coefficient and a higher electrical resistivity than the second thermoelectric material part to which it is joined.
[0050] The electrical resistivity (electrical conductivity) was measured by the four-terminal method. In this measurement, a terminal for measuring a current and a terminal for measuring a voltage were both connected to the electrode terminal. In addition, when calculating the electrical resistivity from the electrical resistance value, the thickness was determined as the sum of the thicknesses of the multiple materials. For example, when determining the electrical resistivity of a joint of 0.1 mm Ag2S (first thermoelectric material portion) and 2 mm Ag2Se (second thermoelectric material portion) in Example 4, the thickness was determined as the sum of the thicknesses of the two materials, that is, 2.1 mm. The output factor is expressed as the product of the square of the Seebeck coefficient and the reciprocal of the electrical resistivity (=electrical conductivity), and was calculated from the measured Seebeck coefficient and electrical resistivity.
[0051] [Table 1]
[0052] As can be seen from the above evaluation results, the examples of the present invention all have significantly improved output factors compared to the comparative examples in which the first thermoelectric material section or the second thermoelectric material section is made of a single material. The absolute values of the Seebeck coefficients of the Bi-Te-based materials of Comparative Examples 1 and 2 are 50 μV / K or more larger than the absolute value of the Seebeck coefficient of the Cu-Ni material of Comparative Example 3, and the electrical resistivity of the Bi-Te-based materials of Comparative Examples 1 and 2 is 10 times or more larger than the electrical resistivity of the Cu-Ni material of Comparative Example 3. Therefore, in Examples 1 and 2 in which the first thermoelectric material section is made of a Bi-Te-based material and the second thermoelectric material section is made of Cu-Ni, both an electromotive voltage path with a sufficiently high Seebeck effect and a current path with a sufficiently high electrical conductivity are configured, so that both the electromotive voltage value and the current value outputted between the pair of electrodes become large, and the output factor is significantly improved. N-type characteristics are obtained in Example 1, and P-type characteristics are obtained in Example 2.
[0053] The absolute value of the Seebeck coefficient of Ag2S in Comparative Example 4 is at least 50 μV / K greater than the absolute value of the Seebeck coefficient of Ag2Se in Comparative Example 5, and the electrical resistivity of Ag2S in Comparative Example 4 is at least 10 times greater than the electrical resistivity of Ag2Se in Comparative Example 5. For this reason, in Examples 3 to 6 in which the first thermoelectric material section is made of an Ag2S-based material and the second thermoelectric material section is made of Ag2Se, both an electromotive voltage path with a sufficiently high Seebeck effect and a current path with sufficiently high electrical conductivity are configured, and as a result, both the electromotive voltage value and the current value output from between the pair of electrodes become large, and the output factor is significantly improved. It should be noted that Example 5 exhibits N-type characteristics, whereas Example 4 exhibits P-type characteristics. However, since this material normally exhibits N-type characteristics, it is believed that the P-type characteristics in Example 4 are due to impurities, crystal defects, etc.
[0054] In addition, the absolute value of the Seebeck coefficient of Cu2S in Comparative Example 6 is 50 μV / K or more higher than the absolute value of the Seebeck coefficient of Cu2Se in Comparative Example 7, and the electrical resistivity of Cu2S in Comparative Example 6 is 10 times or more higher than the electrical resistivity of Cu2Se in Comparative Example 7. 2-δ The second thermoelectric material is Cu. 2-δ In Examples 7, 8, and 13 to 17 in which Se was used, both an electromotive voltage path with a sufficiently high Seebeck effect and a current path with sufficiently high electrical conductivity were configured, so that the electromotive voltage value and current value outputted between the pair of electrodes were both large, and the output factor was significantly improved.
[0055] Furthermore, the absolute values of the Seebeck coefficients of the Bi-Te based materials of Comparative Examples 1 and 2 are at least 50 μV / K greater than the absolute value of the Seebeck coefficient of Cu of Comparative Example 8, and the electrical resistivity of the Bi-Te based materials of Comparative Examples 1 and 2 is at least 10 times greater than the electrical resistivity of Cu of Comparative Example 8. For this reason, in Examples 9 to 12 in which the first thermoelectric material section is made of a Bi-Te based material and the second thermoelectric material section is made of Cu, both an electromotive voltage path with a sufficiently high Seebeck effect and a current path with sufficiently high electrical conductivity are configured, so that both the electromotive voltage value and the current value outputted between the pair of electrodes become large, and the output factor is significantly improved.
[0056] In examples where the first thermoelectric material portion is made of Ag2S and the second thermoelectric material portion is made of Ag2Se, it has been confirmed that Ag2S and Ag2Se have thermal conductivities of less than 1 W / mK at room temperature, and in example 4, for example, a ZT value of about 3 at room temperature is obtained, indicating high thermoelectric performance. In addition, a pi-type thermoelectric conversion module with four elements was fabricated using two each of the Bi-Te / Cu-Ni elements exhibiting N-type characteristics of Example 1 and the Bi-Sb-Te / Cu-Ni elements exhibiting P-type characteristics of Example 2, and the power generation performance was compared with that of a pi-type thermoelectric conversion module with four elements consisting only of Bi-Te (Comparative Example 1) and Bi-Sb-Te (Comparative Example 2). As a result, it was confirmed that the thermoelectric conversion module using the elements of the embodiment had a 38.4% improvement in power generation output when a temperature difference of 30 K was applied (the temperature on the low-temperature side was about 20° C. near room temperature).
[0057] <Examples 21 to 25> (Hot press) Examples 21 to 25 of the present invention were produced by the same manufacturing method as in Examples 4 to 6 above, and the temperature dependence of the thermoelectric properties of Examples 21 to 25 was evaluated. In Example 22, the second thermoelectric material part was joined to the first thermoelectric material part by hot pressing via an intermediate layer of Ag as a conductor, and in Example 23, the second thermoelectric material part was joined to the first thermoelectric material part by hot pressing via an intermediate layer of In as a conductor.
[0058] High temperature thermoelectric characterization In the evaluation method of Examples 1 to 17 above, the thermoelectric characteristics were measured at room temperature (25°C), but in Examples 21 to 25 of the present invention, the thermoelectric characteristics were measured at high temperatures of 88 to 95°C. In Examples 21 to 25, the first thermoelectric material portion was Ag2S and the second thermoelectric material portion was Ag2Se. The results are shown in Table 2. As can be seen from the evaluation results of Examples 21 to 25, even at measurement temperatures of 88 to 95° C., a high Seebeck coefficient (absolute value) is maintained, and the power factor is significantly improved. At a measurement temperature of 88 to 95°C, the power factor of Ag2S alone and Ag2Se alone is 2×10 -3W / mK 2 In Examples 21 to 25, extremely high thermoelectric conversion characteristics were obtained compared to a single element. The thermal conductivity of the thermoelectric elements of Examples 21 to 25 was 1.2 W / mK or less. In Examples 24 and 25, the ZT value (=S 2 T / ρκ): where S, T, ρ, and κ are the Seebeck coefficient, absolute temperature, electrical resistivity, and thermal conductivity, respectively. In Example 21, a ZT value of 5 or more was measured, indicating that extremely high thermoelectric conversion properties were obtained.
[0059] [Table 2]
[0060] -Evaluation of power generation characteristics Next, as Example 26, the first thermoelectric material part was made of Ag2S and the second thermoelectric material part was made of Ag2S 0.5 Se 0.5 The power generation characteristics of the thermoelectric element were evaluated. In addition, Ag2S and Ag2S 0.5 Se 0.5 Both show N-type characteristics. 0.5 Se 0.5 The bonding was performed by hot pressing at a temperature of 200° C. or less. In Example 26, no intermediate layer was used, and the element was directly bonded. The thickness of the element is 10 μm for the Ag2S of the first thermoelectric material and 10 μm for the Ag2S of the second thermoelectric material. 0.5 Se 0.5 The thickness of the element was 0.70 mm. The width of the element was 2.2 mm. Furthermore, the distance between the pair of electrodes was 2.91 mm. The electrodes were needle electrodes, which were touched to the first thermoelectric material part in a dotted line to evaluate the power generation characteristics.
[0061] FIG. 7 shows the Ag2S / Ag2S of Example 26 of the present invention. 0.5 Se 0.5 The results of evaluating the power generation characteristics of a thermoelectric element are shown below. To evaluate the power generation characteristics, a closed circuit was created consisting of a thermoelectric element, a variable resistance element (external load resistance element), and an ammeter, and a temperature difference was applied across both ends of the thermoelectric element to measure the voltage, current, and power output from the thermoelectric element. FIG. 7 shows the output voltage value (shown on the left axis) and the power generation output density (shown on the right axis) versus current. Since the thermoelectric element of Example 26 exhibits N-type characteristics, the voltage value is a negative value, but the voltage value shown on the left axis of Fig. 7 is expressed as an absolute value. The amount of power generation is represented as the product of the voltage value and the current value. The power generation output density is calculated by dividing the amount of power generation by the cross-sectional area of the element (the product of the thickness of the element and the width of the element). In Figure 7, actual measured values are displayed as plots, and values calculated based on those measured values are displayed as lines. The voltage value when the output current is zero is called the open circuit voltage. The current value when the output voltage is 0V is called the short circuit current. Figure 7 also shows the results of open circuit voltage evaluation when the low temperature side temperatures of the element are set to 50°C, 60°C, and 70°C, with a temperature difference of 3K.
[0062] As a result of evaluating the power generation characteristics of the thermoelectric element of Example 26, when the low-temperature side temperature of the element was 60°C, the open circuit voltage was 0.59 mV, the short circuit current was 191 μA, and the power generation output density was 1.7 μW cm ―2 It became. The absolute value of the Seebeck coefficient calculated from the open circuit voltage was 196 μV / K. Ag2S 0.5 Se 0.5 Since the absolute value of the Seebeck coefficient of the single element is 130 μV / K, it is clear that the output voltage of Example 26 is increased. Furthermore, the electrical resistivity of Ag2S alone is high, and the short circuit current value of Example 26 is more than 1000 times larger than that of Ag2S alone. Ag2S alone, Ag2S 0.5 Se 0.5 The power output density of each unit is 0.1 μWcm ―2 Less than 1.0μWcm ―2 In contrast, the Ag2S / Ag2S in Example 26 is calculated as follows: 0.5 Se 0.5 The power generation density of the thermoelectric element (= 1.7 μW cm―2 ) is large, and it is clear that extremely high thermoelectric conversion properties have been obtained compared to a single element.
[0063] The technical scope of the present invention is not limited to the above-described embodiment and examples, and various modifications can be made without departing from the spirit of the present invention. For example, in the above embodiment, the thermoelectric element of the present invention is described as being used for power generation, but the thermoelectric element of the present invention may also be used for Peltier cooling, Peltier temperature control, or the like. Although the shape of the rectangular column is shown in FIG. 3, the shape may be a cylinder (a combination of a cylindrical first thermoelectric material part and a cylindrical second thermoelectric material part) or a polygonal column. [Explanation of symbols]
[0064] Reference Signs List 1: first thermoelectric material portion, 1a: one end portion, 1b: other end portion, 2: second thermoelectric material portion, 2a: conductor, 3: electrode, 4: joint body, 5: insulating material portion, 10, 20, 30: thermoelectric element
Claims
1. a first thermoelectric material portion having one end and another end; a second thermoelectric material part joined to the first thermoelectric material part directly or via an electric conductor; a pair of electrodes connected to the first thermoelectric material portion; the first thermoelectric material portion has a higher absolute value of a Seebeck coefficient and a higher electrical resistivity than the second thermoelectric material portion; a joint body of the first thermoelectric material part and the second thermoelectric material part has end faces on the one end side and the other end side, A thermoelectric element characterized in that the pair of electrodes are in contact with the first thermoelectric material part without contacting the second thermoelectric material part, and are formed on an end face on the one end side and an end face on the other end side of the joint body.
2. 2. The thermoelectric element according to claim 1, A thermoelectric element comprising a pair of insulating material parts formed to cover at least the second thermoelectric material part at an end face on the one end side and an end face on the other end side of the joint body.
3. The thermoelectric element according to claim 1 or 2, the first thermoelectric material part is joined to an upper surface and a lower surface of the second thermoelectric material part, A thermoelectric element, characterized in that the pair of electrodes are connected to the first thermoelectric material portions on the upper and lower surfaces, respectively.
4. The thermoelectric element according to claim 3, the first thermoelectric material part is also joined to both side surfaces of the second thermoelectric material part, A thermoelectric element, characterized in that the pair of electrodes are also connected to each of the first thermoelectric material portions on both side surfaces.
5. The thermoelectric element according to claim 3, the first thermoelectric material part is also joined to both end surfaces of the second thermoelectric material part, A thermoelectric element, characterized in that the pair of electrodes are formed on the first thermoelectric material portion on both end surfaces.
6. The thermoelectric element according to claim 1 or 2, A thermoelectric element, characterized in that the first thermoelectric material section has a Seebeck coefficient whose absolute value is 50 μV / K or more higher than that of the second thermoelectric material section, and an electrical resistivity which is 10 times or more higher.
7. The thermoelectric element according to claim 1 or 2, The first thermoelectric material unit and the second thermoelectric material unit are both A 2+δ A thermoelectric element comprising: a first insulating layer and a second insulating layer, the second insulating layer being formed of at least one of Ag and Cu, and at least one of S, Se and Te.
8. The thermoelectric element according to claim 7, the first thermoelectric material portion is formed of Ag—S; A thermoelectric element, characterized in that the second thermoelectric material portion is formed of Ag--Se or Ag--S--Se.
9. The thermoelectric element according to claim 7, the first thermoelectric material portion is formed of Cu—S; A thermoelectric element, characterized in that the second thermoelectric material portion is formed of Cu--Se.
10. The thermoelectric element according to claim 1 or 2, A thermoelectric element, characterized in that the first thermoelectric material portion is formed of a material containing at least Bi and Te.
Citation Information
Patent Citations
Thermoelectric element and thermoelectric element module using the same
JP1998303471A
Segmented thermoelectric device, thermoelectric module, generator, and temperature-regulating device
JP2009032960A
Segment type thermoelectric power module
JP2018152464A