Thermoelectric conversion module
The thermoelectric conversion module addresses low efficiency in conventional elements by using P-type and N-type elements with distinct Seebeck coefficients and resistivities in a parallel circuit, enhancing power generation performance and enabling operation at higher temperatures.
Patent Information
- Application Number
- JP2024031691
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-01
- Publication Date
- 2024-10-09
AI Technical Summary
Conventional thermoelectric elements and modules suffer from low thermoelectric conversion efficiency, as indicated by a low ZT value and power factor, making it difficult to achieve high power generation performance, especially when operating at temperatures above 200°C and when multiple elements are connected in series.
The thermoelectric conversion module employs a configuration where P-type and N-type thermoelectric elements with different Seebeck coefficients and resistivities are connected via electrodes, forming a parallel circuit to enhance thermoelectric conversion efficiency, with a high Seebeck coefficient and high resistivity in one element and a low resistivity in the other, and optionally includes an insulating layer to prevent direct contact and reduce thermal conductivity.
This configuration achieves high thermoelectric conversion efficiency and a high ZT value, enabling effective power generation even with small temperature differences, and allows for the use of thermoelectric materials at higher temperatures.
Smart Images

Figure 2024139716000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermoelectric conversion module capable of obtaining high thermoelectric conversion efficiency. [Background technology]
[0002] 2. Description of the Related Art So-called segment-type thermoelectric elements in which a plurality of materials having different compositions are joined together are conventionally known. For example, Patent Document 1 describes a thermoelectric element in which a first electrode, a second electrode, a P-type semiconductor thin film made of a thermoelectric material, and an N-type semiconductor thin film made of a thermoelectric material are formed on a substrate, the P-type semiconductor thin film being connected to the first electrode and the N-type semiconductor thin film being connected to the second electrode, the P-type semiconductor thin film and the N-type semiconductor thin film being overlapped and bonded together, and the bonded surface being present over substantially the entire surface of the substrate.
[0003] Patent Documents 2 and 3 also describe a thermoelectric element in which a first thermoelectric material and a second thermoelectric material made of different materials are joined together, one of a pair of electrodes is connected to the first thermoelectric material, and the other of the pair of electrodes is connected to the second thermoelectric material. That is, in these conventional thermoelectric elements, electrodes are provided on the joined first thermoelectric material and second thermoelectric material, respectively, and the first thermoelectric material and the second thermoelectric material are electrically connected in series.
[0004] Furthermore, Patent Document 4 describes a thermoelectric conversion module in which N-type and P-type thermoelectric conversion elements are sandwiched between a low-temperature insulating substrate and a high-temperature insulating substrate in a structure called a π-type structure, and are joined to each insulating substrate via electrodes. In such a thermoelectric conversion module, the N-type and P-type thermoelectric conversion elements are connected in series to form a PN junction pair. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 10-303471 [Patent Document 2] JP 2009-32960 A [Patent Document 3] JP 2018-152464 A [Patent Document 4] JP 2012-248819 A Summary of the Invention [Problem to be solved by the invention]
[0006] The above conventional techniques still have the following problems. That is, the performance of thermoelectric elements required for practical thermoelectric power generation requires that the ZT value, which is an index expressing the energy conversion performance of a thermoelectric conversion material (dimensionless figure of merit ZT (=S2T / ρκ): where S, T, ρ, and κ are the Seebeck coefficient (thermoelectromotive force; electromotive force generated per 1 K temperature difference), absolute temperature, electrical resistivity, and thermal conductivity κ, respectively), be 1 or greater. However, with the above-mentioned conventional segment-type thermoelectric elements, the thermoelectric conversion efficiency was insufficient, making it difficult to increase the ZT value. In order to increase both the voltage output and the amount of electricity generated (= voltage x current) through thermoelectric conversion, the material must have P-type and N-type characteristics, an absolute value of the Seebeck coefficient of 100 μV / K or more, and a power factor (PW=S 2 / ρ) is 1×10 -3 W / mK 2 It is required to have a performance higher than that. To date, research and development has been conducted on various material systems with the aim of increasing the ZT value using a single material, but the only materials in practical use with a ZT value of approximately 1 at temperatures near room temperature are Bi-Te-based materials. However, Bi-Te-based materials have low heat resistance, limiting their use to temperatures below approximately 200°C, and have low thermoelectric conversion efficiency, making the practical use of thermoelectrics difficult. On the other hand, when the above-mentioned conventional segmented thermoelectric element is used, a thermoelectric material with a heat resistance of 200°C or more can be placed on the high-temperature side. However, since the ZT value of each thermoelectric material constituting the segmented thermoelectric element is small and multiple thermoelectric elements form an electrical and thermal series circuit, the ZT value of the element as a whole is small, making it difficult to increase the thermoelectric conversion efficiency. Furthermore, even in thermoelectric conversion modules in which multiple thermoelectric elements are electrically connected in series on a substrate, there is a demand for those with high power generation performance using thermoelectric elements with high thermoelectric conversion efficiency and high ZT values. Thermoelectric conversion modules come in a variety of structures, such as a π-type structure (a structure in which P-type thermoelectric elements and N-type thermoelectric elements are electrically connected in series alternately) and a unileg-type structure (a structure consisting of only P-type thermoelectric elements or only N-type thermoelectric elements, and the thermoelectric element on the high temperature side and the thermoelectric element on the low temperature side are electrically connected using a material with high electrical conductivity such as metal), but in all cases, there is a demand for those with high power generation performance using thermoelectric elements with high thermoelectric conversion efficiency and high ZT values.
[0007] The present invention has been made in consideration of the above-mentioned problems, and aims to provide a thermoelectric conversion module having high power generation performance by using a thermoelectric element having high thermoelectric conversion efficiency and a high ZT value. [Means for solving the problem]
[0008] The present invention employs the following configuration to solve the above problems. That is, a thermoelectric conversion module according to a first invention includes a plurality of thermoelectric element units which are P-type thermoelectric element units or N-type thermoelectric element units, the thermoelectric element units include a first thermoelectric material unit having one end and the other end, a second thermoelectric material unit joined to the first thermoelectric material unit directly or via a conductor, and a pair of electrodes connected to the first thermoelectric material unit, the pair of electrodes are connected to the one end side and the other end side of the first thermoelectric material unit while being spaced apart from each other, the first thermoelectric material unit and the second thermoelectric material unit joined to each other of the thermoelectric element units form a joint, the plurality of thermoelectric element units are electrically connected to each other via the electrodes, and the first thermoelectric material unit has a higher absolute value of the Seebeck coefficient and a higher electrical resistivity than the second thermoelectric material unit to which it is joined.
[0009] In this thermoelectric conversion module, a pair of electrodes are connected to one end and the other end of the first thermoelectric material section at a distance from each other, the first thermoelectric material section and the second thermoelectric material section which are joined to each other of the thermoelectric element section form a joint, and the multiple thermoelectric element sections are electrically connected via the electrodes, so that the multiple electrically connected thermoelectric element sections can form a Seebeck element, thermopile, or the like having good performance.
[0010] In addition, in this thermoelectric conversion module, in the thermoelectric element section, the first thermoelectric material section has a higher absolute value of the Seebeck coefficient and a higher electrical resistivity than the second thermoelectric material section, and a pair of electrodes are connected to one end side and the other end side of the first thermoelectric material section at a distance from each other, so that the first thermoelectric material section and the second thermoelectric material section form an electrical and thermal parallel circuit, and when a temperature difference occurs between the one end side and the other end side (heat flow occurs), a thermoelectromotive force is generated with high thermoelectric conversion efficiency. That is, the first thermoelectric material section, which is connected to the pair of electrodes and has a high Seebeck coefficient (absolute value) and a high electrical resistance, forms an electromotive voltage path that mainly follows the Seebeck effect, and the second thermoelectric material section, which is joined to and in contact with the first thermoelectric material section and has a low electrical resistance, forms a current path. It is desirable that the current value flowing in the second thermoelectric material section follows Ohm's law. In this way, by configuring a parallel circuit of the electromotive voltage path and the current path, a current path that serves as a current path separate from the electromotive voltage path is formed, thereby increasing the electrical conductivity flowing between the pair of electrodes while maintaining the high Seebeck coefficient (absolute value) of the first thermoelectric material section, and making it possible to obtain high thermoelectric conversion efficiency and ZT value.In the thermoelectric conversion module, it is possible to achieve high thermoelectric conversion efficiency even with a small temperature difference. The second thermoelectric material section and the pair of electrodes are not directly joined, but are in electrical contact via the first thermoelectric material section. The present invention has a structure in which a thermoelectric element section is made by joining together a number of materials with different compositions, but is characterized in that a pair of electrodes (two electrodes) are connected to the first thermoelectric material section. (Segment-type thermoelectric elements also have a structure in which a number of materials with different compositions are joined together, but the pair of electrodes are connected to different thermoelectric materials, and an electrode connection method different from that of the present invention is used.)
[0011] The thermoelectric conversion module of the second invention is characterized in that, in the first invention, the thermoelectric element section includes both the P-type thermoelectric element section and the N-type thermoelectric element section, the first thermoelectric material section and the second thermoelectric material section joined to each other of the P-type thermoelectric element section form a P-type junction, the first thermoelectric material section and the second thermoelectric material section joined to each other of the N-type thermoelectric element section form an N-type junction, and the electrode on the one end side of the P-type thermoelectric element section and the electrode on the one end side of the N-type thermoelectric element section are electrically connected. That is, in this thermoelectric conversion module, the first thermoelectric material part and the second thermoelectric material part joined to each other of the P-type thermoelectric element part form a P-type junction, and the first thermoelectric material part and the second thermoelectric material part joined to each other of the N-type thermoelectric element part form an N-type junction, and an electrode on one end side of the P-type thermoelectric element part and an electrode on one end side of the N-type thermoelectric element part are electrically connected, so that the P-type thermoelectric element part and the N-type thermoelectric element part connected in a π shape can form a Seebeck element or thermopile, etc., having good performance.
[0012] The thermoelectric conversion module of the third invention is characterized in that, in the first invention, the multiple thermoelectric element parts are composed only of the P-type thermoelectric element parts or only of the N-type thermoelectric element parts, and the electrode on the one end side of one of the thermoelectric element parts adjacent to each other is electrically connected to the electrode on the other end side of the other thermoelectric element part. That is, in this thermoelectric conversion module, the multiple thermoelectric element sections are composed of only P-type thermoelectric element sections or only N-type thermoelectric element sections, and the electrode on one end side of one of the adjacent thermoelectric element sections is electrically connected to the electrode on the other end side of the other thermoelectric element section, so that a Seebeck element or thermopile with good performance can be formed by multiple thermoelectric element sections of the same type, only P-type or only N-type, connected in a unileg type.
[0013] The thermoelectric conversion module according to a fourth invention is characterized in that, in any of the first to third inventions, an insulating layer is provided between the multiple thermoelectric element parts arranged in parallel. That is, in this thermoelectric conversion module, since an insulating layer is provided between a plurality of thermoelectric element sections arranged in parallel, the insulating layer can prevent the plurality of thermoelectric element sections from coming into direct contact with each other. It is preferable that the thermal conductivity of this insulating layer has insulating performance equal to or lower than the thermal conductivity of the thermoelectric element portion, and by suppressing the thermal conduction between the thermoelectric element portions, high thermoelectric conversion efficiency can be obtained without heat diffusion in a direction perpendicular to the heat flow direction (temperature difference application direction) applied to the thermoelectric conversion module.
[0014] The thermoelectric conversion module according to a fifth invention is characterized in that, in any one of the first to fourth inventions, the joint body has a pair of insulating material parts formed on an end face on the one end side and an end face on the other end side, covering at least the second thermoelectric material part. That is, in this thermoelectric conversion module, the junction has a pair of insulating material parts formed on the end face on one end side and the end face on the other end side, covering at least the second thermoelectric material parts, so that the insulating material parts can prevent the pair of electrodes from contacting the second thermoelectric material parts.
[0015] The thermoelectric conversion module of the sixth invention is characterized in that, in the second invention, the P-type thermoelectric element portion and the N-type thermoelectric element portion extend parallel to each other, and the module comprises a one-end side substrate installed at one end of the P-type thermoelectric element portion and the N-type thermoelectric element portion, and an other-end side substrate installed at the other end of the P-type thermoelectric element portion and the N-type thermoelectric element portion, and the one-end side substrate has a connection electrode portion that electrically connects the electrode on the one end side of the P-type thermoelectric element portion and the electrode on the one end side of the N-type thermoelectric element portion. That is, in this thermoelectric conversion module, the one-end side substrate has a connection electrode portion that electrically connects the electrode on one end side of the P-type thermoelectric element portion and the electrode on one end side of the N-type thermoelectric element portion, so that the electrodes on one end side of the P-type thermoelectric element portion and the N-type thermoelectric element portion can be easily connected to form a π-type module.
[0016] The thermoelectric conversion module of the seventh invention is characterized in that, in the third invention, the multiple thermoelectric element parts extend parallel to each other, and the module comprises a one-end side substrate installed at one end of the multiple thermoelectric element parts, an other-end side substrate installed at the other end of the multiple thermoelectric element parts, and a connecting electrode member that electrically connects the electrode on the one-end side of one of the adjacent thermoelectric element parts and the electrode on the other end side of the other thermoelectric element part. In other words, this thermoelectric conversion module is provided with a connecting electrode member that electrically connects the electrode on one end side of one adjacent thermoelectric element unit to the electrode on the other end side of the other thermoelectric element unit, so that the electrodes of one thermoelectric element unit and the other thermoelectric element unit that are adjacent to each other can be easily connected to form a uni-leg type module.
[0017] The thermoelectric conversion module of the eighth invention is characterized in that, in the sixth or seventh invention, the multiple thermoelectric element parts are formed in a chip shape, the one-end side substrate is installed on an end surface of the one end side of the multiple thermoelectric element parts, and the other-end side substrate is installed on an end surface of the other end side of the multiple thermoelectric element parts. That is, in this thermoelectric conversion module, a one-end side substrate is installed on an end face on one end side of the multiple thermoelectric element units, and the other-end side substrate is installed on an end face on the other end side of the multiple thermoelectric element units, and a π-type or uni-leg type module can be formed with multiple chip-shaped thermoelectric element units sandwiched between the one-end side substrate and the other-end side substrate.
[0018] The thermoelectric conversion module according to a ninth invention is characterized in that, in any of the first to eighth inventions, the first thermoelectric material part has a Seebeck coefficient that is 50 μV / K or more higher in absolute value than the second thermoelectric material part, and an electrical resistivity that is 10 times or more higher. That is, in this thermoelectric conversion module, the first thermoelectric material section has a Seebeck coefficient that is 50 μV / K or more higher in absolute value than the second thermoelectric material section, and has an electrical resistivity that is 10 times higher. Therefore, by forming both an electromotive voltage path with a sufficiently high Seebeck effect and a current path with sufficiently high electrical conductivity, the electromotive voltage value and current value output from between the pair of electrodes are both large, and a higher thermoelectric conversion efficiency and ZT value can be obtained.
[0019] A thermoelectric conversion module according to a tenth aspect of the present invention is any one of the first to ninth aspects of the present invention, wherein the first thermoelectric material section and the second thermoelectric material section are both A 2+δ It is characterized in that it is formed of M (wherein A is at least one of Ag and Cu, and M is at least one of S, Se and Te). In addition, the 1st Thermoelectric Materials Department A 2+δ M is the second thermoelectric material part A 2+δ It is possible to obtain a large ZT value by designing the composition of the material so that the absolute value of the Seebeck coefficient is 50 μV / K or more larger than M and the electrical resistivity is 10 times larger.
[0020] The thermoelectric conversion module of an eleventh invention is characterized in that, in the tenth invention, the first thermoelectric material part is formed of Ag—S, and the second thermoelectric material part is formed of Ag—Se or Ag—S—Se. That is, in this thermoelectric conversion module, for example, by forming the first thermoelectric material section from Ag2S and the second thermoelectric material section from Ag2Se, it becomes possible to obtain a ZT value of 1 or more at least at room temperature.
[0021] The thermoelectric conversion module of the 12th invention is characterized in that, in the 10th invention, the first thermoelectric material part is formed of Cu-S, and the second thermoelectric material part is formed of Cu-Se. That is, in this thermoelectric conversion module, for example, by forming the first thermoelectric material section from Cu2S and the second thermoelectric material section from Cu2Se, it becomes possible to obtain a ZT value of 1 or more at least at room temperature.
[0022] A thermoelectric conversion module according to a thirteenth aspect of the present invention is any one of the first to twelfth aspects of the present invention, characterized in that the first thermoelectric material portion is formed of a material containing at least Bi and Te. That is, in this thermoelectric conversion module, the first thermoelectric material part is made of a material containing at least Bi and Te, such as Bi-Te or Bi-Sb-Te. For example, the first thermoelectric material part is made of Bi2Te3, and the second thermoelectric material part is made of Cu. 0.55 Ni 0.45 (constantan), it is possible to obtain a power factor at least twice that of Bi2Te3 alone. Furthermore, if the first thermoelectric material part has a higher absolute value of the Seebeck coefficient and a higher electrical resistivity than the second thermoelectric material part to which it is joined, the thermoelectric properties will be improved compared to the first thermoelectric material part alone, regardless of the composition of the second thermoelectric material part. Effect of the Invention
[0023] According to the present invention, the following effects are obtained. That is, according to the thermoelectric conversion module of the present invention, a pair of electrodes are connected to one end side and the other end side of the first thermoelectric material part at a distance from each other, the first thermoelectric material part and the second thermoelectric material part which are joined to each other of the thermoelectric element parts form a joint, the multiple thermoelectric element parts are electrically connected via the electrodes, and the first thermoelectric material part has a higher absolute value of the Seebeck coefficient and a higher electrical resistivity than the second thermoelectric material part to which it is joined, so that a Seebeck element or thermopile or the like having high thermoelectric conversion efficiency and ZT value and good performance due to the multiple thermoelectric element parts connected in a π type or unileg type can be obtained. Therefore, since the thermoelectric conversion module according to the present invention has high thermoelectric conversion efficiency and ZT value, it becomes possible to put into practical use environmental power generation that extracts electricity with high efficiency by utilizing temperature difference. [Brief description of the drawings]
[0024] [Figure 1] 1 is a perspective view showing a first embodiment of a thermoelectric conversion module according to the present invention. [Diagram 2]FIG. 2 is a conceptual diagram for explaining the principle of a thermoelectric element in the first embodiment. [Diagram 3] FIG. 4 is a perspective view showing a second embodiment of a thermoelectric conversion module according to the present invention. [Figure 4] FIG. 4 is a cross-sectional view showing a third embodiment of a thermoelectric conversion module according to the present invention. [Diagram 5] FIG. 11 is a cross-sectional view showing a fourth embodiment of a thermoelectric conversion module according to the present invention. [Figure 6] FIG. 11 is a perspective view showing a fifth embodiment of a thermoelectric conversion module according to the present invention. [Figure 7] FIG. 13 is a plan view showing a thermoelectric conversion module installed between substrates in a fifth embodiment. [Figure 8] FIG. 2 is a cross-sectional view showing an example of a thermoelectric element unit of the present invention that was produced in order to demonstrate the principle of the thermoelectric element unit of the present invention. [Figure 9] FIG. 11 is a perspective view showing a sixth embodiment of a thermoelectric conversion module according to the present invention. [Figure 10] FIG. 11 is a cross-sectional view showing a seventh embodiment of a thermoelectric conversion module according to the present invention. [Figure 11] FIG. 13 is a perspective view showing an eighth embodiment of a thermoelectric conversion module according to the present invention. [Figure 12] 4 is a graph showing the results of evaluating the power generation characteristics of a thermoelectric element in an example of a thermoelectric conversion module according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] A first embodiment of a thermoelectric conversion module according to the present invention will be described below with reference to Fig. 1 and Fig. 2. In the drawings used in the following description, the scale is appropriately changed as necessary to make each part recognizable or easily recognizable.
[0026] As shown in FIGS. 1 and 2, a thermoelectric conversion module 10 of this embodiment includes a plurality of thermoelectric element units, which are P-type thermoelectric element units 11P or N-type thermoelectric element units 11N. The thermoelectric conversion module 10 of this embodiment includes both a P-type thermoelectric element portion 11P and an N-type thermoelectric element portion 11N as thermoelectric element portions. The P-type thermoelectric element part 11P and the N-type thermoelectric element part 11N each include a first thermoelectric material part 1 having one end part 1a and the other end part 1b, a second thermoelectric material part 2 joined to the first thermoelectric material part 1 directly or via a conductor 2a, and a pair of electrodes 3 connected to the first thermoelectric material part 1. When the first thermoelectric material part 1 and the second thermoelectric material part 2 are joined via the conductor 2a, the conductor 2a also functions as an intermediate layer. The conductor 2a is, for example, a conductive bonding material such as solder or In.
[0027] The pair of electrodes 3 are connected to one end 1a and the other end 1b of the first thermoelectric material part 1 at a distance from each other. Furthermore, the pair of electrodes 3 are not in contact with the second thermoelectric material part 2 and are disposed apart from the second thermoelectric material part 2 . The first thermoelectric material part 1 and the second thermoelectric material part 2 of the thermoelectric element part joined to each other form a joint body. That is, the first thermoelectric material part 1 and the second thermoelectric material part 2 joined to each other of the P-type thermoelectric element part 11P constitute a P-type junction body 14P, and the first thermoelectric material part 1 and the second thermoelectric material part 2 joined to each other of the N-type thermoelectric element part 11N constitute an N-type junction body 14N.
[0028] The P-type junction 14P is a junction exhibiting P-type characteristics. That is, the P-type junction 14P, which is a combination of the first thermoelectric material section 1 and the second thermoelectric material section 2, functions as a thermoelectric conversion material having P-type polarity as a whole. The N-type junction body 14N is a junction body exhibiting N-type characteristics. That is, the N-type junction body 14N, which is a combination of the first thermoelectric material part 1 and the second thermoelectric material part 2, functions as a thermoelectric conversion material having N-type polarity as a whole. The plurality of thermoelectric element parts are electrically connected via the electrode 3. That is, the electrode 3 on one end 1a side of the P-type thermoelectric element part 11P and the electrode 3 on one end 1a side of the N-type thermoelectric element part 11N are electrically connected.
[0029] The first thermoelectric material part 1 has a higher absolute value of the Seebeck coefficient and a higher electrical resistivity than the second thermoelectric material part 2 to which it is joined. That is, the first thermoelectric material part 1 of the P-type thermoelectric element part 11P has a higher absolute value of the Seebeck coefficient and a higher electrical resistivity than the second thermoelectric material part 2 of the P-type thermoelectric element part 11P, and the first thermoelectric material part 1 of the N-type thermoelectric element part 11N has a higher absolute value of the Seebeck coefficient and a higher electrical resistivity than the second thermoelectric material part 2 of the N-type thermoelectric element part 11N. The P-type or N-type of the thermoelectric element part is determined from the sign of the measured Seebeck coefficient. When joining the first thermoelectric material part 1 and the second thermoelectric material part 2, it is desirable to align the P-type / N-type polarities, i.e., to join P-type with P-type or N-type with N-type, but it is also possible to join parts with different polarities, i.e., P-type with N-type. Even in such a case, the first thermoelectric material part 1 has a higher absolute value of the Seebeck coefficient and a higher electrical resistivity than the second thermoelectric material part 2.
[0030] In addition, the thermoelectric conversion module 10 of this embodiment has the P-type thermoelectric element portion 11P and the N-type thermoelectric element portion 11N extending parallel to each other, and is provided with a one-end side substrate 14a installed at one end 1a of the P-type thermoelectric element portion 11P and the N-type thermoelectric element portion 11M, and an other-end side substrate 14b installed at the other end 1b of the P-type thermoelectric element portion 11P and the N-type thermoelectric element portion 11N. The one-end side substrate 14a has, on an insulating base material, a connection electrode portion 14c that electrically connects the electrode 3 on one end 1a side of the P-type thermoelectric element portion 11P and the electrode 3 on one end 1a side of the N-type thermoelectric element portion 11N. The other end side substrate 14b is provided on an insulating base material with a pair of terminal electrode portions 14d connected to the electrodes 3 on the other end 1b side of the P-type thermoelectric element portion 11P and the N-type thermoelectric element portion 11N. In the thermoelectric conversion module 10 of this embodiment, for example, one end 1a side is arranged on the high temperature side, and the other end 1b side is arranged on the low temperature side.
[0031] It is preferable that the first thermoelectric material section 1 has a Seebeck coefficient that is at least 50 μV / K larger in absolute value than the second thermoelectric material section 2, and an electrical resistivity that is at least 10 times larger. The electrical resistivity of the first thermoelectric material unit 1 at room temperature is 10 -5 Ωcm or less is preferable. For example, the first thermoelectric material unit 1 and the second thermoelectric material unit 2 are both A 2+δ M (wherein A is at least one of Ag and Cu, and M is at least one of S, Se and Te). The range of δ is preferably -0.5≦δ≦+0.5, and more preferably -0.05 to +0.02.
[0032] In the present invention, the thermoelectric material is defined as a material having a Seebeck coefficient with an absolute value of 0.1 μV / K or more. That is, the absolute value of the Seebeck coefficient of the second thermoelectric material section 2 is 0.1 μV / K or more. Furthermore, the absolute value of the Seebeck coefficient of the first thermoelectric material portion 1 is preferably 10 mV / K or less. Furthermore, when the electrical resistivity of the first thermoelectric material part 1 at room temperature is 10 mΩcm or less, it is preferable that the first thermoelectric material part 1 is thinner than the second thermoelectric material part 2. Furthermore, when the electrical resistivity of the first thermoelectric material part 1 at room temperature is 10 mΩcm or less, and the electrical resistivity of the second thermoelectric material part 2 at room temperature is 1 mΩcm or less and the thermal conductivity is 10 W / mK or more, it is preferable that the thickness of the first thermoelectric material part 1 is thicker than the thickness of the second thermoelectric material part 2.
[0033] A 2+δ In the case of an N-type thermoelectric element, for example, a configuration in which the first thermoelectric material part 1 is made of Ag-S and the second thermoelectric material part 2 is made of Ag-Se or Ag-S-Se can be used as M. In the case of a P-type thermoelectric element, for example, a configuration in which the first thermoelectric material part 1 is made of Cu-S and the second thermoelectric material part 2 is made of Cu-Se can be used. For example, the first thermoelectric material section 1 can be made of Ag2S, and the second thermoelectric material section 2 can be made of Ag2Se. Ag2S has a Seebeck coefficient that is 50 μV / K or more higher in absolute value than Ag2Se, and an electrical resistivity that is 10 times or more higher. Alternatively, the first thermoelectric material portion 1 may be made of Cu2S, and the second thermoelectric material portion 2 may be made of Cu2Se. Cu2S has a Seebeck coefficient that is 50 μV / K or more higher in absolute value than Cu2Se, and an electrical resistivity that is 10 times higher.
[0034] The first thermoelectric material portion 1 may be made of a material containing at least Bi and Te, such as Bi-Te or Bi-Sb-Te. For example, the first thermoelectric material portion 1 may be made of Bi2Te3 or (Bi 0.7 Sb 0.3 ) Te3, and the second thermoelectric material portion 2 is formed of Cu 0.55 Ni 0.45 (Constantan). Bi2Te3 and (Bi 0.7 Sb 0.3 ) Te3 is Cu 0.55 Ni 0.45 The absolute value of the Seebeck coefficient is 50 μV / K or more higher and the electrical resistivity is 10 times higher than that of the It is also possible to employ the first thermoelectric material portion 1 in which impurities such as Ru or Cu are added to the material containing Bi and Te.
[0035] In this manner, the first thermoelectric material part 1 is made of a semiconductor material or insulating material with high electrical resistance, such as a low thermal conductive chalcogenide material, and the second thermoelectric material part 2 is made of a conductive material with low electrical resistance, such as a semiconductor material or an alloy. Furthermore, in order to increase the temperature difference applied between the P-type thermoelectric element unit 11P and the N-type thermoelectric element unit 11N, it is preferable that both the first thermoelectric material unit 1 and the second thermoelectric material unit 2 have low thermal conductivity. In particular, it is preferable that the first thermoelectric material unit 1 has a thermal conductivity of 10 W / mK or less in order to obtain a high thermoelectromotive force by the Seebeck effect. The thermal conductivity of the first thermoelectric material part is preferably 0.02 W / mK or more.
[0036] The first thermoelectric material part 1 may be a thin film, but the second thermoelectric material part 2 is preferably a conductor bulk thicker than the first thermoelectric material part 1 . The thickness of the first thermoelectric material part 1 (i.e., the thickness in the stacking direction of the first thermoelectric material part 1 and the second thermoelectric material part 2) is preferably 100 nm to 10 mm, and may be 1 μm to 3 mm. The thickness of the second thermoelectric material part 2 is preferably 0.1 mm to 10 mm, and may be 0.5 mm to 3 mm. When the first thermoelectric material part 1 and the second thermoelectric material part 2 are joined via the conductor 2a, a conductive joining material such as solder or In can be used as the conductor 2a. Note that the electrical resistivity of the conductor 2a used in this joining part is preferably approximately the same as the electrical resistivity of the second thermoelectric material part 2. In many cases, the electrical resistivity of alloy materials and solder materials is similar (10 -4 For example, Cu as an alloy material 0.55 Ni 0.45 When constantan is used, the electrical resistivities of the second thermoelectric material part 2 and the solder are approximately the same, so that for the first thermoelectric material part 1, the solder can essentially be regarded as part of the second thermoelectric material part 2 from the standpoint of electrical conductivity, thereby increasing the freedom in designing the thermoelectric element. The pair of electrodes 3 may be made of, for example, Ag paste or Ag solder. The material of the pair of electrodes 3 has an electrical resistivity of 10 -4 Ωm or less is adopted.
[0037] A method for manufacturing the P-type thermoelectric element part 11P and the N-type thermoelectric element part 11N of this embodiment includes a joining process for joining the second thermoelectric material part 2 and the first thermoelectric material part 1, and an electrode formation process for forming a pair of electrodes 3 on the first thermoelectric material part 1. For example, in the joining step, the second thermoelectric material part 2 and the first thermoelectric material part 1 are joined together with a conductive joining material such as solder. In addition, in the above bonding process, various thin film growth methods (vapor phase growth methods such as PVD, sputtering, and CVD) are adopted. When a chalcogenide material is used for the first thermoelectric material part 1, it is preferable to form the first thermoelectric material part 1 as a film on the second thermoelectric material part 2 by the MBD method (molecular beam deposition method).
[0038] In the above bonding step, the first thermoelectric material part 1 may be formed as a film on the second thermoelectric material part 2 by a sol-gel method. In addition, in the above-mentioned joining process, a hot pressing method may be used in which, in a state in which the powder that will become the first thermoelectric material part 1 and the powder that will become the second thermoelectric material part 2 are stacked, the first thermoelectric material part 1 and the second thermoelectric material part 2 are sintered, and the first thermoelectric material part 1 and the second thermoelectric material part 2 are joined together at the same time.
[0039] As described above, in the thermoelectric conversion module 10 of the present embodiment, a pair of electrodes 3 are connected to one end 1a and the other end 1b of the first thermoelectric material part 1 with a space between them, the first thermoelectric material part 1 and the second thermoelectric material part 2 which are joined to each other of the thermoelectric element parts form a joint, and the multiple thermoelectric element parts are electrically connected via the electrodes 3, so that the multiple electrically connected thermoelectric element parts can form a Seebeck element, thermopile, or the like having good performance. In particular, in this embodiment, the first thermoelectric material part 1 and the second thermoelectric material part 2 joined to each other of the P-type thermoelectric element part 11P form a P-type junction 14P, and the first thermoelectric material part 1 and the second thermoelectric material part 2 joined to each other of the N-type thermoelectric element part 11N form an N-type junction 14N, and the electrode 3 on one end 1a of the P-type thermoelectric element part 11P and the electrode 3 on one end 1a of the N-type thermoelectric element part 11N are electrically connected, so that the P-type thermoelectric element part 11P and the N-type thermoelectric element part 11N connected in a π shape can form a Seebeck element or thermopile, etc., having good performance.
[0040] Furthermore, in this thermoelectric conversion module 10, in each of the P-type thermoelectric element section 11P and the N-type thermoelectric element section 11N, the first thermoelectric material section 1 has a higher absolute value of Seebeck coefficient and a higher electrical resistivity than the second thermoelectric material section 2 to which it is joined, and a pair of electrodes 3 are connected to one end 1a side and the other end 1b side of the first thermoelectric material section 1 at a distance from each other, so that the first thermoelectric material section 1 and the second thermoelectric material section 2 form an electrical and thermal parallel circuit, and when a temperature difference occurs between the one end 1a side and the other end 1b side (heat flow occurs), a thermoelectromotive force is generated with high thermoelectric conversion efficiency.
[0041] That is, as shown in FIG. 2, the first thermoelectric material part 1, which is connected to a pair of electrodes 3 and has a high Seebeck coefficient (absolute value) and a high electrical resistance, forms an electromotive voltage path R1 that mainly follows the Seebeck effect, and the second thermoelectric material part 2, which is joined to and in contact with the first thermoelectric material part 1 and has a low electrical resistance, forms a current path R2. It is desirable that the current value flowing in the second thermoelectric material part 2 follows Ohm's law. In this way, by forming a parallel circuit of the electromotive voltage path R1 and the current path R2, the current path R2, which is a current path separate from the electromotive voltage path R1, is formed, and the electrical conductivity flowing between the pair of electrodes 3 increases while maintaining the high Seebeck coefficient (absolute value) of the first thermoelectric material part 1, and a high thermoelectric conversion efficiency and ZT value can be obtained. Note that the arrow Y in FIG. 2 indicates the heat flow direction (the direction in which the heat flux flows, the direction in which a temperature difference occurs).
[0042] Furthermore, since the first thermoelectric material part 1 has a Seebeck coefficient whose absolute value is 50 μV / K or more higher than that of the second thermoelectric material part 2 and whose electrical resistivity is 10 times higher, the electromotive voltage path R1 having a sufficiently high Seebeck effect and the current path R2 having a sufficiently high electrical conductivity are both configured, and therefore the electromotive voltage value and current value output between the pair of electrodes 3 become large, and a higher thermoelectric conversion efficiency and a higher ZT value can be obtained. The absolute value of the Seebeck coefficient of the first thermoelectric material part 1 may be 100 μV / K or more greater than the absolute value of the Seebeck coefficient of the joined second thermoelectric material part 2. The greater the difference between the absolute value of the Seebeck coefficient of the first thermoelectric material part 1 and the absolute value of the Seebeck coefficient of the joined second thermoelectric material part 2, the more desirable it is, and although there is no particular upper limit, it may be 10,000 μV / K.
[0043] Furthermore, since the one-end side substrate 14a has a connection electrode portion 14c that electrically connects the electrode 3 on one end 1a side of the P-type thermoelectric element portion 11P and the electrode 3 on one end 1a side of the N-type thermoelectric element portion 11N, the electrode 3 on one end 1a side of the P-type thermoelectric element portion 11P and the N-type thermoelectric element portion 11N can be easily connected to form a π-type module.
[0044] Furthermore, since the first thermoelectric material part 1 has a Seebeck coefficient whose absolute value is 50 μV / K or more higher than that of the second thermoelectric material part 2 and whose electrical resistivity is 10 times higher, the electromotive voltage path R1 having a sufficiently high Seebeck effect and the current path R2 having a sufficiently high electrical conductivity are both configured, and therefore the electromotive voltage value and current value output between the pair of electrodes 3 become large, and a higher thermoelectric conversion efficiency and a higher ZT value can be obtained.
[0045] In addition, by forming the first thermoelectric material portion 1 from Ag2S and the second thermoelectric material portion 2 from Ag2Se, the output factor (PW=S 2 / ρ) becomes large, making it possible to obtain an N-type thermoelectric element with a ZT value of 1 or more at least at room temperature. In addition, by forming the first thermoelectric material portion 1 from Cu2S and the second thermoelectric material portion 2 from Cu2Se, the output factor (PW=S 2 / ρ) becomes large, making it possible to obtain a P-type thermoelectric element with a ZT value of 1 or more at least at room temperature. The first thermoelectric material portion 1 is made of Bi2Te3, and the second thermoelectric material portion 2 is made of Cu. 0.55 Ni 0.45By forming it from Bi2Te3 (constantan), it is possible to obtain an N-type thermoelectric element having a power factor at least twice that of a single substance of Bi2Te3. The first thermoelectric material portion 1 is made of (Bi 0.7 Sb 0.3 )2Te3, and the second thermoelectric material part 2 is formed of Cu 0.55 Ni 0.45 (Constantan) to form at least (Bi 0.7 Sb 0.3 It is now possible to obtain a P-type thermoelectric element with a power factor approximately twice that of a single element of 2Te3.
[0046] Next, second to eighth embodiments of the thermoelectric conversion module according to the present invention will be described below with reference to Figures 3 to 7 and 9 to 11. In the following description of each embodiment, the same components as those described in the above embodiments are denoted by the same reference numerals, and the description thereof will be omitted.
[0047] The difference between the second embodiment and the first embodiment is that in the first embodiment, the first thermoelectric material parts 1 of the P-type thermoelectric element part 11P and the N-type thermoelectric element part 11N are arranged at the bottom (substrate side), whereas in the thermoelectric conversion module 20 of the second embodiment, the first thermoelectric material parts 1 of the P-type thermoelectric element part 21P and the N-type thermoelectric element part 21N are arranged at the top, as shown in FIG. 3. The second embodiment also differs from the first embodiment in that the P-type junction body 24P and the N-type junction body 24N are provided with a pair of insulating material parts 25 formed to cover at least the second thermoelectric material part 2 on the end face on the one end 1a side and the end face on the other end 1b side.
[0048] In the second embodiment, the pair of electrodes 23 cover the pair of insulating material parts 25 . That is, the electrode 23 covers the end faces of the insulating material parts 25 formed on the end faces of the P-type junction body 24P and the N-type junction body 24N, and is connected to the first thermoelectric material part 1 in a state where it also covers the upper surface of the insulating material part 25. Furthermore, the pair of electrodes 23 on one end 1a side are connected to connection electrode portion 14c of one end side substrate 14a, and the electrode 23 on the other end 1b side is connected to terminal electrode portion 14d of the other end side substrate 14b. The insulating material portion 25 is made of an insulating material such as SiO2 or Si3N4. As described above, in the thermoelectric conversion module 20 of the second embodiment, the P-type junction body 24P and the N-type junction body 24N are provided with a pair of insulating material parts 25 formed to cover at least the second thermoelectric material part 2 on the end face on the one end 1a side and the end face on the other end 1b side, so that the insulating material parts 25 can prevent the pair of electrodes 23 from contacting the second thermoelectric material part 2.
[0049] Next, the difference between the third embodiment and the first embodiment is that in the first embodiment, the P-type thermoelectric element portion 1P and the N-type thermoelectric element portion 1N are rod-shaped extending long from one end 1a to the other end 1b, whereas in the thermoelectric conversion module 30 of the third embodiment, the P-type thermoelectric element portion 31P and the N-type thermoelectric element portion 31N are formed in a chip shape, as shown in FIG. 4. That is, in the third embodiment, the P-type thermoelectric element portion 31P and the N-type thermoelectric element portion 31N are formed in a rectangular parallelepiped shape, and one end portion 1a and the other end portion 1b of the first thermoelectric material portion 1 are disposed on both end faces thereof.
[0050] Another difference between the third embodiment and the first embodiment is that the one-end side substrate 34a is installed on the end surface on the one end 1a side of the P-type thermoelectric element portion 31P and the N-type thermoelectric element portion 31N, and the other-end side substrate 34b is installed on the end surface on the other end 1b side of the P-type thermoelectric element portion 31P and the N-type thermoelectric element portion 31N. The one end side substrate 34a includes a connection electrode portion 34c that connects the electrode 33 on the one end 1a side of the P-type thermoelectric element portion 31P and the electrode 33 on the one end 1a side of the N-type thermoelectric element portion 31N. That is, the P-type thermoelectric element unit 31P and the N-type thermoelectric element unit 31N are arranged side by side with the first thermoelectric material units 1 formed on one side of the second thermoelectric material unit 2 facing each other, and the electrodes 33 on one end 1a side of the P-type thermoelectric element units 31P facing each other are electrically connected to each other by the connection electrode unit 34c.
[0051] Thus, in the thermoelectric conversion module 30 of the third embodiment, the one-end side substrate 34a is installed on the end surface on the one end 1a side of the P-type thermoelectric element portion 31P and the N-type thermoelectric element portion 31N, and the other-end side substrate 34b is installed on the end surface on the other end side of the P-type thermoelectric element portion 31P and the N-type thermoelectric element portion 31N, so that a π-type module can be formed with the chip-shaped P-type thermoelectric element portion 31P and N-type thermoelectric element portion 31N sandwiched between the one-end side substrate 34a and the other-end side substrate 34b.
[0052] Next, the fourth embodiment differs from the third embodiment in that, whereas in the third embodiment, the first thermoelectric material part 1 is connected to one side of the second thermoelectric material part 2, in the thermoelectric conversion module 40 of the fourth embodiment, the first thermoelectric material part 1 is joined to both opposite side surfaces of the second thermoelectric material part 2, as shown in FIG. 5. In the fourth embodiment, electrodes 43 are formed on one end 1a and the other end 1b of a pair of first thermoelectric material parts 1 joined to both side surfaces of the second thermoelectric material part 2, respectively.
[0053] Furthermore, in the fourth embodiment, similarly to the second embodiment, a pair of insulating material parts 45 is provided which are formed by covering at least the second thermoelectric material part 2 on an end face on one end 1a side and an end face on the other end 1b side of the joint 44 between the first thermoelectric material part 1 and the second thermoelectric material part 2. The connection electrode portion 44c patterned on the one end side substrate 44a using a metal film such as Cu foil is connected to each electrode 43 formed on one end 1a of the first thermoelectric material portion 1 on both side surfaces. A pair of terminal electrode portions 44d patterned with a metal film such as Cu foil on the other end side substrate 44b are connected to the electrodes 43 of the corresponding P-type thermoelectric element portion 41P and N-type thermoelectric element portion 41N.
[0054] As described above, in the thermoelectric conversion module 40 of the fourth embodiment, the first thermoelectric material part 1 is joined to both side surfaces of the second thermoelectric material part, so that an electromotive voltage path is formed on both side surfaces, thereby achieving higher thermoelectric conversion efficiency.
[0055] Next, the difference between the fifth embodiment and the third embodiment is that in the third embodiment, the P-type thermoelectric element unit 31P and the N-type thermoelectric element unit 31N are arranged side by side with their first thermoelectric material units 1 facing each other and there is no space between them, whereas in the thermoelectric conversion module 50 of the fifth embodiment, as shown in Figures 6 and 7, the chip-shaped P-type thermoelectric element unit 51P and the N-type thermoelectric element unit 51N are arranged in parallel with their first thermoelectric material units 1 on their upper surfaces, and an insulating layer 56 is provided between the P-type thermoelectric element unit 51P and the N-type thermoelectric element unit 51N.
[0056] In addition, in the fifth embodiment, the connection electrode portion 54c, which is the electrode on the other end portion 1b side, is formed to bridge from above the first thermoelectric material portion 1 of the P-type thermoelectric element portion 51P to above the first thermoelectric material portion 1 of the N-type thermoelectric element portion 51N, via the insulating layer 56. That is, as shown in FIG. 7, when one end side substrate 54a and the other end side substrate 45b are installed on both end surfaces of P-type thermoelectric element portion 51P and N-type thermoelectric element portion 51N, no connection electrode portions are formed on one end side substrate 54a and the other end side substrate 45b. In addition, a terminal electrode portion 54d, which serves as the electrode on the one end portion 1a side, is formed and connected to the first thermoelectric material portion 1 of the P-type thermoelectric element portion 51P and the first thermoelectric material portion 1 of the N-type thermoelectric element portion 51N, respectively. The insulating layer 56 is made of an insulating material such as SiO2 or Si3N4. The terminal electrode portion 54d and the connection electrode portion 54c are formed of a metal such as a Cu plate, and are bonded to the corresponding insulating layer 56 and first thermoelectric material portion 1 by soldering or the like.
[0057] In this way, in the thermoelectric conversion module 50 of the fifth embodiment, an insulating layer 56 is provided between the P-type thermoelectric element section 51P and the N-type thermoelectric element section 51N arranged in parallel, so that the insulating layer 56 can prevent the P-type thermoelectric element section 51P and the N-type thermoelectric element section 51N from coming into direct contact with each other.
[0058] Next, the difference between the sixth embodiment and the second embodiment is that the second embodiment is a so-called π-type thermoelectric conversion module that uses both P-type thermoelectric element section 21P and N-type thermoelectric element section 21N, whereas the thermoelectric conversion module 60 of the sixth embodiment is a uni-leg type thermoelectric conversion module that uses only one of the P-type thermoelectric element section 21P or the N-type thermoelectric element section 21N, as shown in FIG. 9.
[0059] That is, the thermoelectric conversion module 60 of the sixth embodiment has, for example, a pair of N-type thermoelectric element parts 21N extending parallel to each other, and includes a one-end side substrate 64a installed on one end 1a of each N-type thermoelectric element part 21N, and an other-end side substrate 64b installed on the other end 1b of each N-type thermoelectric element part 21N. The one end side substrate 64a is provided, on an insulating base material, with a pair of connection electrode portions 64c that are connected to the electrodes 23 on the one end 1a side of the N-type thermoelectric element portion 21N. The other end side substrate 64b is provided, on an insulating base material, with a connection electrode portion 64e connected to the electrode 23 on the other end 1b side of the N-type thermoelectric element portion 21N, and a pair of terminal electrodes 64d.
[0060] Furthermore, the thermoelectric conversion module 60 is provided with a connecting electrode member 64f that electrically connects the electrode 23 on one end 1a side of one adjacent N-type thermoelectric element unit 21N to the electrode 23 on the other end 1b side of the other N-type thermoelectric element unit 21N. That is, the connecting electrode member 64f arranged between a pair of adjacent N-type thermoelectric element units 21N has one end electrically connected to the electrode 23 on one end 1a of one N-type thermoelectric element unit 21N via a connecting electrode portion 64c, and the other end electrically connected to the electrode 23 on the other end 1b of the other N-type thermoelectric element unit 21N via a connecting electrode portion 64e. The connecting electrode members 64f are disposed at a distance from the pair of N-type thermoelectric element portions 21N so as not to come into direct contact with the pair of N-type thermoelectric element portions 21N. As a result, the pair of N-type thermoelectric element portions 21N are electrically connected in series in a uni-leg configuration by the connecting electrode member 64f.
[0061] In addition, the thermoelectric conversion module 60 is provided with a terminal electrode member 64g that electrically connects a connection electrode portion 64c connected to the electrode 23 on one end 1a side of the adjacent N-type thermoelectric element portion 21N and a terminal electrode portion 64d of the other end side substrate 64b. The terminal electrode member 64g is disposed at a distance from the N-type thermoelectric element portion 21N so as not to come into direct contact with the N-type thermoelectric element portion 21N. The connecting electrode member 64f and the terminal electrode member 64g are formed of a metal plate such as a Cu plate extending along the N-type thermoelectric element portion 21N, and their ends are bonded and connected to the corresponding connection electrode portions 64c, 64e and terminal electrode portion 64d by solder or the like.
[0062] In this way, the thermoelectric conversion module 60 of the sixth embodiment is provided with a connecting electrode member 64f that electrically connects the electrode 23 on one end 1a side of one adjacent thermoelectric element unit (the N-type thermoelectric element unit 21N at the back of Figure 9) to the electrode 23 on the other end 1b side of the other adjacent thermoelectric element unit (the N-type thermoelectric element unit 21N at the front of Figure 9), so that the electrodes 23 of one thermoelectric element unit and the other thermoelectric element unit that are adjacent to each other can be easily connected to form a uni-leg type module. In the sixth embodiment, the N-type thermoelectric element units 21N, all of which are the same N-type, are used as the plurality of thermoelectric element units. However, the P-type thermoelectric element units 21P, all of which are the same P-type, may be used as the plurality of thermoelectric element units.
[0063] Next, the difference between the seventh embodiment and the fourth embodiment is that in the thermoelectric conversion module 40 of the fourth embodiment, the connection electrode portion 44c formed on the one end side substrate 44a is a π type connected to each electrode 43 formed on one end 1a of the first thermoelectric material portion 1 on both side surfaces of the adjacent P-type thermoelectric element portion 41P and N-type thermoelectric element portion 41N, whereas the thermoelectric conversion module 70 of the seventh embodiment is a uni-leg type thermoelectric conversion module that has a connecting electrode member 74f and uses only one of the P-type thermoelectric element portion 21P or the N-type thermoelectric element portion 21N, as shown in Figure 10.
[0064] That is, the thermoelectric conversion module 70 of the seventh embodiment has, for example, a pair of chip-shaped N-type thermoelectric element parts 41N arranged upright with a gap between them, and includes a one-end side substrate 74a installed at one end 1a of each N-type thermoelectric element part 41N, and an other-end side substrate 74b installed at the other end 1b of each N-type thermoelectric element part 41N. The one end side substrate 74a is provided on an insulating base material with a pair of connection electrode parts 74c which are connected to the electrodes 43 on the one end 1a side of the N-type thermoelectric element part 41N and which are patterned with a metal film such as Cu foil. The other end side substrate 74b is provided with a connection electrode portion 74e and a pair of terminal electrodes 74d which are patterned on an insulating base material using a metal film such as Cu foil. The connection electrode portion 74e is connected to the electrode 43 on the other end portion 1b side of the other N-type thermoelectric element portion 41N.
[0065] Furthermore, the thermoelectric conversion module 70 is provided with a connecting electrode member 74f that electrically connects the electrode 43 on one end 1a side of one adjacent N-type thermoelectric element unit 41N to the electrode 43 on the other end 1b side of the other N-type thermoelectric element unit 41N. That is, the connecting electrode member 74f arranged between a pair of adjacent N-type thermoelectric element units 41N has one end electrically connected to the electrode 43 on one end 1a of one N-type thermoelectric element unit 41N via the connecting electrode portion 74c, and the other end electrically connected to the electrode 43 on the other end 1b of the other N-type thermoelectric element unit 41N via the connecting electrode portion 74e. The connecting electrode member 74f is disposed at a distance from the N-type thermoelectric element portion 21N so as not to come into direct contact with the pair of N-type thermoelectric element portions 21N. As a result, the pair of N-type thermoelectric element portions 41N are electrically connected in series in a uni-leg configuration by the connecting electrode member 74f.
[0066] In addition, the thermoelectric conversion module 70 is provided with a terminal electrode member 74g that electrically connects a connection electrode portion 74c connected to the electrode 43 on one end 1a side of the adjacent N-type thermoelectric element portion 41N and a terminal electrode portion 74d of the other end side substrate 74b. The terminal electrode member 74g is disposed at a distance from the N-type thermoelectric element portion 21N so as not to come into direct contact with the N-type thermoelectric element portion 21N. The connecting electrode member 74f and the terminal electrode member 74g are formed of a metal plate such as a Cu plate or a leaf spring extending along the N-type thermoelectric element portion 41N, and their ends are bonded to the corresponding connecting electrode portions 74c, 74e and terminal electrode portion 74d by solder or the like.
[0067] In this way, the thermoelectric conversion module 70 of the seventh embodiment is provided with a connecting electrode member 74f that electrically connects the electrode 43 on one end 1a of one adjacent thermoelectric element unit (N-type thermoelectric element unit 41N on the right side of Figure 10) to the electrode 43 on the other end 1b of the other adjacent thermoelectric element unit (N-type thermoelectric element unit 41N on the left side of Figure 10), so that the electrodes 43 of one thermoelectric element unit and the other thermoelectric element unit that are adjacent to each other can be easily connected to form a uni-leg type module. In the seventh embodiment, the N-type thermoelectric element units 41N, all of which are the same N-type, are used as the plurality of thermoelectric element units. However, the P-type thermoelectric element units 41P, all of which are the same P-type, may be used as the plurality of thermoelectric element units.
[0068] Next, the difference between the eighth embodiment and the fifth embodiment is that in the thermoelectric conversion module 50 of the fifth embodiment, the connection electrode portion 54c is formed to span from above the first thermoelectric material portion 1 of the P-type thermoelectric element portion 51P to above the first thermoelectric material portion 1 of the N-type thermoelectric element portion 51N via the insulating layer 56, forming a π-type, whereas the thermoelectric conversion module 80 of the eighth embodiment is a uni-leg type thermoelectric conversion module that includes a connecting electrode member 84f and uses only one of the P-type thermoelectric element portion 51P or the N-type thermoelectric element portion 51N, as shown in FIG. 11.
[0069] That is, the thermoelectric conversion module 80 of the eighth embodiment is provided with a connecting electrode member 84f, for example, on an insulating layer 56a arranged between a pair of N-type thermoelectric element units 51N, which electrically connects the electrode 53 on one end 1a side of one adjacent N-type thermoelectric element unit 51N to the electrode 53 on the other end 1b side of the other N-type thermoelectric element unit 51N. As a result, the pair of N-type thermoelectric element portions 51N are electrically connected in series in a uni-leg configuration by the connecting electrode member 84f.
[0070] In addition, in the thermoelectric conversion module 80 of the eighth embodiment, an insulating layer 56b is also joined to the side surface of the N-type thermoelectric element portion 51N, which is one of the above-mentioned portions, opposite to the insulating layer 56a side. The insulating layer 56b is provided on its upper surface with a connection electrode portion 84c having one end connected to the electrode 53 on the other end portion 1b side formed on the first thermoelectric material portion 1 of one of the N-type thermoelectric element portions 51N, and a terminal electrode portion 84d connected to the other end of the connection electrode portion 84c.
[0071] Furthermore, a terminal electrode portion 84d, which is also an electrode on the one end portion 1a side, is connected to the first thermoelectric material portion 1 of the other N-type thermoelectric element portion 51N. That is, the terminal electrode portion 84d is connected to the insulating layer 56b and to the first thermoelectric material portion 1 of the other N-type thermoelectric element portion 51N. The terminal electrode portion 84d, the connection electrode portion 84c, the electrode 53 and the linking electrode member 84f are formed of metal such as a Cu plate, and are bonded to the corresponding insulating layers 56a, 56b and the first thermoelectric material portion 1 by soldering or the like.
[0072] In this way, the thermoelectric conversion module 80 of the eighth embodiment is provided with a connecting electrode member 84f that electrically connects the electrode 53 on one end 1a side of one adjacent thermoelectric element unit (the N-type thermoelectric element unit 51N at the back of Figure 11) to the electrode 53 on the other end 1b side of the other adjacent thermoelectric element unit (the N-type thermoelectric element unit 51N at the front of Figure 11), so that the electrodes 53 of one thermoelectric element unit and the other thermoelectric element unit that are adjacent to each other can be easily connected to form a uni-leg type module. In the eighth embodiment, the N-type thermoelectric element units 51N, all of which are the same N-type, are used as the plurality of thermoelectric element units. However, the P-type thermoelectric element units 51P, all of which are the same P-type, may be used as the plurality of thermoelectric element units. EXAMPLES
[0073] In order to verify the principles of thermoelectric properties for the P-type thermoelectric element portion and the N-type thermoelectric element portion in the thermoelectric conversion module of the present invention, a sample of a thermoelectric element as shown in FIG. 8 was fabricated as an example, and the evaluation results are shown in Tables 1 and 2. In the examples of the present invention, the first thermoelectric material part and the second thermoelectric material part were fabricated using the materials and manufacturing methods described in the above embodiment, and their thermoelectric properties (conductivity type determination (P / N type determination), Seebeck coefficient, electrical resistivity, and power factor) at room temperature (300 K) were investigated. As a comparative example of the present invention, a thermoelectric element made of a single thermoelectric material was evaluated in the same manner as in the examples of the present invention. Each example was produced as follows. In the examples of the present invention, for evaluation purposes, the first thermoelectric material part 1 is joined to the upper surface of the second thermoelectric material part 2, and a pair of electrodes 3 is formed on the upper surface of the first thermoelectric material part 1.
[0074] <Examples 1 and 2> <Examples 9 to 12> (Solder joint) First, a Bi-Te bulk sintered body (or a Bi-Sb-Te bulk sintered body) to become the first thermoelectric material part and a Cu-Ni alloy plate or a Cu plate to become the second thermoelectric material part were prepared, cut to a specified size, and the joining surfaces were polished. Thereafter, a solder foil was placed on the bonding surface between the Bi-Te bulk sintered body and the Cu-Ni alloy plate or Cu plate, and the Bi-Te bulk sintered body was joined to the Cu-Ni alloy plate or Cu plate by using a hot press machine and utilizing solder melting. That is, the second thermoelectric material part was joined to the first thermoelectric material part through an intermediate layer of solder as a conductor. The above joining conditions were a pressure of 100 MPa, a joining temperature of 250 °C, and a holding time of about 5 minutes. After visually confirming the melting of the solder, a cooling process and a process of reducing the pressure were performed. Thereafter, two pairs of electrodes were formed on the first thermoelectric material part side (Bi-Te side) using an Ag paste or the like to obtain Examples 1 and 2.
[0075] <Example 3> (MBD film formation) First, an Ag2S thin film serving as the first thermoelectric material part was formed on an Ag2Se bulk sintered body serving as the second thermoelectric material part using an MBD (molecular beam epitaxy) apparatus. The Ag2Se bulk sintered body was formed by the SHS (self-propagating high-temperature synthesis) method. In the film formation by the above MBD method, the substrate temperature was set at room temperature, and a cell containing Ag and S as raw materials was heated to an appropriate temperature with a heater to perform film formation, thereby obtaining a single-phase thin film of Ag2S serving as the first thermoelectric material part. In addition, it has been confirmed by X-ray diffraction experiments that the Ag2S thin film and the Ag2Se bulk sintered body are crystalline materials. Ag2S 1-x Se x In the Ag2S-Se system, in the low-temperature phase near room temperature below the phase transition temperature, when x ≤ 0.6, it has the same crystal structure as Ag2S (monoclinic, space group P21 / c), and when x ≥ 0.7, it has the same crystal structure as Ag2Se (orthorhombic, space group P212121). (In the composition range of 0.6 < x < 0.7, depending on the film formation conditions, a mixed phase or a different crystal structure is obtained.) The production of the electrodes is the same as in Examples 1 and 2.
[0076] <Examples 4 to 8><Examples 13 to 17> (Hot press) First, the raw material powders (e.g., Ag, S, Cu, etc.) for the first thermoelectric material part and the second thermoelectric material part are weighed out to a predetermined stoichiometric ratio, mixed, molded using a press, and then heat-treated at a predetermined temperature to obtain, for example, a sintered body of a single phase of AgS. When a chalcogenide containing S, Se, or Te is used, a single-phase sintered body can be obtained even by using the self-heating reaction method. If an unreacted phase is confirmed by the X-ray diffraction experiment, the sintered body is crushed into powder and the above process is repeated. Since the X-ray diffraction experiment shows that a single-phase sintered body is obtained, this process is repeated.
[0077] After the single-phase sintered body is obtained, the sintered body is pulverized in a mortar or the like to obtain, for example, Ag2S, Ag2Se, Cu, etc. 2-δ S, Cu 2-δ Obtain Se powder. These powders are heated and pressurized in a hot press to produce bulk bodies of the first and second thermoelectric material parts, and at the same time, a joint body of the first and second thermoelectric material parts is produced. Note that, during the hot press, Ag2S, Ag2Se, Cu, etc. are used in consideration of density. 2-δ S, Cu 2-δ The Se is weighed out to achieve the desired thickness, and the raw materials are added in order and molded.
[0078] In addition, the bonding conditions using the hot press are a pressure of 100 MPa, a predetermined holding temperature, and a holding time of 20 minutes to form a bonded body. Thereafter, the bonded body is cut using a wire saw or the like to obtain a chip-shaped bonded body of, for example, 17 mm×3 mm×2 mmt. The electrodes were prepared in the same manner as in Examples 1 and 2.
[0079] <Method of evaluating thermoelectric elements> When a temperature difference ΔT is applied to a thermoelectric element, a voltage ΔV proportional to the temperature difference is generated. This phenomenon is called the Seebeck effect, and the generated voltage is called thermoelectromotive force, with the proportionality coefficient S = ΔV / ΔT defined as the Seebeck coefficient S. In other words, to measure the Seebeck coefficient, it is necessary to measure both the potential difference (thermoelectromotive force) between two terminals and the temperature difference. The Seebeck coefficient was measured using two commercially available Peltier elements, one of which was cooled and the other was wired to be heated so as to create a temperature difference between the two Peltier elements, with a temperature difference of 0.1 to 5°C. The thermocouple used for the measurements was a T-type thermocouple (Cu-Constantan). An extremely thin type, about 20 microns, was selected for this thermocouple, and a rubber material with high electrical insulation and heat insulation was used to apply a load, achieving good thermal and electrical contact between the material and the thermocouple. In addition, a two-terminal method called the thermoelectric probe method was adopted, and the potential difference (thermoelectromotive force) between the two terminals was measured using the Cu wiring of two T-type thermocouples. The relationship between the thermoelectromotive force ΔV and the temperature difference ΔT was plotted, and the Seebeck coefficient was evaluated from the linear relationship near the zero temperature difference (near the origin of ΔV / ΔT). The P type and N type (conductivity type) were determined from the sign of the measured Seebeck coefficient. When joining the first thermoelectric material part and the second thermoelectric material part, it is desirable to align the P type / N type polarity to be the same, i.e., to join P types together or N types together, but it is also possible to join opposite polarities, i.e., P type and N type together. Even in such a case, the first thermoelectric material part has a higher absolute value of the Seebeck coefficient and a higher electrical resistivity than the second thermoelectric material part to which it is joined.
[0080] The electrical resistivity (electrical conductivity) was measured by the four-terminal method. In this measurement, a terminal for measuring a current and a terminal for measuring a voltage were both connected to the electrode terminal. In addition, when calculating the electrical resistivity from the electrical resistance value, the thickness was determined as the sum of the thicknesses of the multiple materials. For example, when determining the electrical resistivity of a joint of 0.1 mm Ag2S (first thermoelectric material portion) and 2 mm Ag2Se (second thermoelectric material portion) in Example 4, the thickness was determined as 2.1 mm, which is the sum of the thicknesses of the two materials. The output factor is expressed as the product of the square of the Seebeck coefficient and the reciprocal of the electrical resistivity (=electrical conductivity), and was calculated from the measured Seebeck coefficient and electrical resistivity.
[0081] [Table 1]
[0082] As can be seen from the above evaluation results, the examples of the present invention all have significantly improved output factors compared to the comparative examples in which the first thermoelectric material section or the second thermoelectric material section is made of a single material. The absolute values of the Seebeck coefficients of the Bi-Te-based materials of Comparative Examples 1 and 2 are 50 μV / K or more larger than the absolute value of the Seebeck coefficient of the Cu-Ni material of Comparative Example 3, and the electrical resistivity of the Bi-Te-based materials of Comparative Examples 1 and 2 is 10 times or more larger than the electrical resistivity of the Cu-Ni material of Comparative Example 3. Therefore, in Examples 1 and 2 in which the first thermoelectric material section is made of a Bi-Te-based material and the second thermoelectric material section is made of Cu-Ni, both an electromotive voltage path with a sufficiently high Seebeck effect and a current path with a sufficiently high electrical conductivity are configured, so that both the electromotive voltage value and the current value outputted between the pair of electrodes become large, and the output factor is significantly improved. N-type characteristics are obtained in Example 1, and P-type characteristics are obtained in Example 2.
[0083] The absolute value of the Seebeck coefficient of Ag2S in Comparative Example 4 is at least 50 μV / K greater than the absolute value of the Seebeck coefficient of Ag2Se in Comparative Example 5, and the electrical resistivity of Ag2S in Comparative Example 4 is at least 10 times greater than the electrical resistivity of Ag2Se in Comparative Example 5. For this reason, in Examples 3 to 6 in which the first thermoelectric material section is made of an Ag2S-based material and the second thermoelectric material section is made of Ag2Se, both an electromotive voltage path with a sufficiently high Seebeck effect and a current path with sufficiently high electrical conductivity are configured, and as a result, both the electromotive voltage value and the current value output from between the pair of electrodes become large, and the output factor is significantly improved. It should be noted that Example 5 exhibits N-type characteristics, whereas Example 4 exhibits P-type characteristics. However, since this material normally exhibits N-type characteristics, it is believed that the P-type characteristics in Example 4 are due to impurities, crystal defects, etc.
[0084] In addition, the absolute value of the Seebeck coefficient of Cu2S in Comparative Example 6 is 50 μV / K or more higher than the absolute value of the Seebeck coefficient of Cu2Se in Comparative Example 7, and the electrical resistivity of Cu2S in Comparative Example 6 is 10 times or more higher than the electrical resistivity of Cu2Se in Comparative Example 7. 2-δ The second thermoelectric material is Cu. 2-δ In Examples 7, 8, and 13 to 17 in which Se was used, both an electromotive voltage path with a sufficiently high Seebeck effect and a current path with sufficiently high electrical conductivity were configured, so that the electromotive voltage value and current value outputted between the pair of electrodes were both large, and the output factor was significantly improved.
[0085] Furthermore, the absolute values of the Seebeck coefficients of the Bi-Te based materials of Comparative Examples 1 and 2 are at least 50 μV / K greater than the absolute value of the Seebeck coefficient of Cu of Comparative Example 8, and the electrical resistivity of the Bi-Te based materials of Comparative Examples 1 and 2 is at least 10 times greater than the electrical resistivity of Cu of Comparative Example 8. For this reason, in Examples 9 to 12 in which the first thermoelectric material section is made of a Bi-Te based material and the second thermoelectric material section is made of Cu, both an electromotive voltage path with a sufficiently high Seebeck effect and a current path with sufficiently high electrical conductivity are configured, so that both the electromotive voltage value and the current value outputted between the pair of electrodes become large, and the output factor is significantly improved.
[0086] In examples where the first thermoelectric material portion is made of Ag2S and the second thermoelectric material portion is made of Ag2Se, it has been confirmed that Ag2S and Ag2Se have thermal conductivities of less than 1 W / mK at room temperature, and in example 4, for example, a ZT value of about 3 at room temperature is obtained, indicating high thermoelectric performance. In addition, a pi-type thermoelectric conversion module with four elements was fabricated using two each of the Bi-Te / Cu-Ni elements exhibiting N-type characteristics of Example 1 and the Bi-Sb-Te / Cu-Ni elements exhibiting P-type characteristics of Example 2, and the power generation performance was compared with that of a pi-type thermoelectric conversion module with four elements consisting only of Bi-Te (Comparative Example 1) and Bi-Sb-Te (Comparative Example 2). As a result, it was confirmed that the thermoelectric conversion module using the elements of the embodiment had a 38.4% improvement in power generation output when a temperature difference of 30 K was applied (the temperature on the low-temperature side was about 20° C. near room temperature).
[0087] <Examples 21 to 25> (Hot press) Examples 21 to 25 of the present invention were produced by the same manufacturing method as in Examples 4 to 6 above, and the temperature dependence of the thermoelectric properties of Examples 21 to 25 was evaluated. In Example 22, the second thermoelectric material part was joined to the first thermoelectric material part by hot pressing via an intermediate layer of Ag as a conductor, and in Example 23, the second thermoelectric material part was joined to the first thermoelectric material part by hot pressing via an intermediate layer of In as a conductor.
[0088] High temperature thermoelectric characterization In the evaluation method of Examples 1 to 17 above, the thermoelectric characteristics were measured at room temperature (25°C), but in Examples 21 to 25 of the present invention, the thermoelectric characteristics were measured at high temperatures of 88 to 95°C. In Examples 21 to 25, the first thermoelectric material portion was Ag2S and the second thermoelectric material portion was Ag2Se. The results are shown in Table 2. As can be seen from the evaluation results of Examples 21 to 25, even at measurement temperatures of 88 to 95° C., a high Seebeck coefficient (absolute value) is maintained, and the power factor is significantly improved. At a measurement temperature of 88 to 95°C, the power factor of Ag2S alone and Ag2Se alone is 2×10 -3W / mK 2 In Examples 21 to 25, extremely high thermoelectric conversion characteristics were obtained compared to a single element. The thermal conductivity of the thermoelectric elements of Examples 21 to 25 was 1.2 W / mK or less. In Examples 24 and 25, the ZT value (=S 2 T / ρκ): where S, T, ρ, and κ are the Seebeck coefficient, absolute temperature, electrical resistivity, and thermal conductivity, respectively. In Example 21, a ZT value of 5 or more was measured, indicating that extremely high thermoelectric conversion properties were obtained.
[0089] [Table 2]
[0090] -Evaluation of power generation characteristics Next, as Example 26, the first thermoelectric material part was made of Ag2S and the second thermoelectric material part was made of Ag2S 0.5 Se 0.5 The power generation characteristics of the thermoelectric element were evaluated. In addition, Ag2S and Ag2S 0.5 Se 0.5 Both show N-type characteristics. 0.5 Se 0.5 The bonding was performed by hot pressing at a temperature of 200° C. or less. In Example 26, no intermediate layer was used, and the element was directly bonded. The thickness of the element is 10 μm for the Ag2S of the first thermoelectric material and 10 μm for the Ag2S of the second thermoelectric material. 0.5 Se 0.5 The thickness of the element was 0.70 mm. The width of the element was 2.2 mm. Furthermore, the distance between the pair of electrodes was 2.91 mm. The electrodes were needle electrodes, which were touched to the first thermoelectric material part in a dotted line to evaluate the power generation characteristics.
[0091] FIG. 12 shows the Ag2S / Ag2S of Example 26 of the present invention. 0.5 Se 0.5 The results of evaluating the power generation characteristics of a thermoelectric element are shown below. To evaluate the power generation characteristics, a closed circuit was created consisting of a thermoelectric element, a variable resistance element (external load resistance element), and an ammeter, and a temperature difference was applied across both ends of the thermoelectric element to measure the voltage, current, and power output from the thermoelectric element. FIG. 12 shows the output voltage value (shown on the left axis) and the power generation output density (shown on the right axis) relative to the current. Since the thermoelectric element of Example 26 exhibits N-type characteristics, the voltage value is a negative value, but the voltage value shown on the left axis of Fig. 12 is expressed as an absolute value. The amount of power generation is represented as the product of the voltage value and the current value. The power generation output density is calculated by dividing the amount of power generation by the cross-sectional area of the element (the product of the thickness of the element and the width of the element). In Figure 12, actual measured values are displayed as plots, and values calculated based on those measured values are displayed as lines. The voltage value when the output current is zero is called the open circuit voltage. The current value when the output voltage is 0V is called the short circuit current. Figure 12 also shows the results of open circuit voltage evaluation when the low temperature side temperatures of the element are set to 50°C, 60°C, and 70°C, with a temperature difference of 3K.
[0092] As a result of evaluating the power generation characteristics of the thermoelectric element of Example 26, when the low-temperature side temperature of the element was 60°C, the open circuit voltage was 0.59 mV, the short circuit current was 191 μA, and the power generation output density was 1.7 μW cm ―2 It became. The absolute value of the Seebeck coefficient calculated from the open circuit voltage was 196 μV / K. Ag2S 0.5 Se 0.5 Since the absolute value of the Seebeck coefficient of the single element is 130 μV / K, it is clear that the output voltage of Example 26 is increased. Furthermore, the electrical resistivity of Ag2S alone is high, and the short circuit current value of Example 26 is more than 1000 times larger than that of Ag2S alone. Ag2S alone, Ag2S 0.5 Se 0.5 The power output density of each unit is 0.1 μWcm ―2 Less than 1.0μWcm ―2 In contrast, the Ag2S / Ag2S in Example 26 is calculated as follows: 0.5 Se 0.5 The power generation density of the thermoelectric element (= 1.7 μW cm―2 ) is large, and it is clear that extremely high thermoelectric conversion properties have been obtained compared to a single element.
[0093] The technical scope of the present invention is not limited to the above-described embodiment and examples, and various modifications can be made without departing from the spirit of the present invention. [Explanation of symbols]
[0094] 1...first thermoelectric material portion, 1a...one end portion, 1b...other end portion, 2...second thermoelectric material portion, 2a...conductor, 3,43,53...electrode, 10,20,30,40,50,60,70,80...thermoelectric conversion module, 11P,21P,31P,41P,51P...P-type thermoelectric element portion, 11N,21N,31N,41N,51N...N-type thermoelectric element portion, 14a, 44a, 54a, 64a, 74a... one end side substrate, 14b, 44b, 54b, 54b, 64b, 74b... other end side substrate, 14c, 34c, 44c, 54c, 64c, 74c, 84c... connection electrode portion, 14P, 24P... P-type junction, 14N, 24N... N-type junction, 25... insulating material portion, 44... junction, 56, 56a, 56b... insulating layer
Claims
1. A plurality of thermoelectric element units which are P-type thermoelectric element units or N-type thermoelectric element units are provided, the thermoelectric element portion includes a first thermoelectric material portion having one end and another end; a second thermoelectric material part joined to the first thermoelectric material part directly or via an electric conductor; a pair of electrodes connected to the first thermoelectric material portion; the pair of electrodes are connected to the one end side and the other end side of the first thermoelectric material part while being spaced apart from each other; the first thermoelectric material part and the second thermoelectric material part of the thermoelectric element part joined to each other form a joint body, The plurality of thermoelectric element units are electrically connected via the electrodes, A thermoelectric conversion module, wherein the first thermoelectric material section has a higher absolute value of Seebeck coefficient and a higher electrical resistivity than the second thermoelectric material section to which it is joined.
2. The thermoelectric conversion module according to claim 1 , The thermoelectric element unit includes both the P-type thermoelectric element unit and the N-type thermoelectric element unit, the first thermoelectric material part and the second thermoelectric material part of the P-type thermoelectric element part joined to each other constitute a P-type junction body, the first thermoelectric material part and the second thermoelectric material part of the N-type thermoelectric element part joined to each other constitute an N-type junction body, A thermoelectric conversion module, characterized in that the electrode on the one end side of the P-type thermoelectric element portion and the electrode on the one end side of the N-type thermoelectric element portion are electrically connected to each other.
3. The thermoelectric conversion module according to claim 1 , The plurality of thermoelectric element units are composed of only the P-type thermoelectric element units or only the N-type thermoelectric element units, A thermoelectric conversion module characterized in that the electrode on one end side of one of the thermoelectric element sections adjacent to each other is electrically connected to the electrode on the other end side of the other thermoelectric element section.
4. The thermoelectric conversion module according to claim 1 , A thermoelectric conversion module comprising: an insulating layer provided between the plurality of thermoelectric element portions arranged in parallel.
5. The thermoelectric conversion module according to claim 1 , A thermoelectric conversion module characterized in that the joint has a pair of insulating material parts formed on the end surface on the one end side and the end surface on the other end side, covering at least the second thermoelectric material part.
6. The thermoelectric conversion module according to claim 2, The P-type thermoelectric element portion and the N-type thermoelectric element portion extend parallel to each other, a one-end side substrate disposed at one end of the P-type thermoelectric element portion and the N-type thermoelectric element portion; a second end side substrate disposed at the second end of the P-type thermoelectric element portion and the N-type thermoelectric element portion, A thermoelectric conversion module characterized in that the one-end side substrate has a connection electrode portion that electrically connects the electrode on the one-end side of the P-type thermoelectric element portion and the electrode on the one-end side of the N-type thermoelectric element portion.
7. The thermoelectric conversion module according to claim 3 , The plurality of thermoelectric element portions extend parallel to each other, a one-end-side substrate disposed at one end of the plurality of thermoelectric element units; an other end side substrate disposed at the other end of the plurality of thermoelectric element units; A thermoelectric conversion module characterized by comprising a connecting electrode member that electrically connects the electrode on the one end side of one of the adjacent thermoelectric element sections and the electrode on the other end side of the other thermoelectric element section.
8. The thermoelectric conversion module according to claim 6 or 7, The plurality of thermoelectric element portions are formed in a chip shape, the one end side substrate is disposed on an end surface of the one end side of the plurality of thermoelectric element units, A thermoelectric conversion module, characterized in that the other end side substrate is installed on end faces of the other end side of the plurality of thermoelectric element portions.
9. The thermoelectric conversion module according to claim 1 , A thermoelectric conversion module, characterized in that the first thermoelectric material section has a Seebeck coefficient whose absolute value is 50 μV / K or more higher than that of the second thermoelectric material section, and an electrical resistivity which is 10 times or more higher.
10. The thermoelectric conversion module according to claim 1 , The first thermoelectric material unit and the second thermoelectric material unit are both A 2+δ A thermoelectric conversion module comprising: a first insulating layer and a second insulating layer; a second insulating layer and a third insulating layer; and a fourth insulating layer and a fourth insulating layer, wherein A is at least one of Ag and Cu, and M is at least one of S, Se and Te.
11. The thermoelectric conversion module according to claim 10, the first thermoelectric material portion is formed of Ag—S; A thermoelectric conversion module, characterized in that the second thermoelectric material portion is formed of Ag--Se or Ag--S--Se.
12. The thermoelectric conversion module according to claim 10, the first thermoelectric material portion is formed of Cu—S; A thermoelectric conversion module, characterized in that the second thermoelectric material portion is formed of Cu--Se.
13. The thermoelectric conversion module according to claim 1 , A thermoelectric conversion module, wherein the first thermoelectric material portion is formed of a material containing at least Bi and Te.
Citation Information
Patent Citations
Thermoelectric element and thermoelectric element module using the same
JP1998303471A
Segmented thermoelectric device, thermoelectric module, generator, and temperature-regulating device
JP2009032960A
Thermoelectric conversion element and manufacturing method thereof
JP2012248819A
Segment type thermoelectric power module
JP2018152464A