Thermoelectric element

The thermoelectric element with a high Seebeck coefficient and resistivity chip design addresses efficiency and miniaturization challenges, achieving enhanced thermoelectric conversion and power generation through a parallel circuit configuration.

JP2024139717APending Publication Date: 2024-10-09MITSUBISHI MATERIALS CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024031692
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2024-03-01
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Conventional thermoelectric elements face challenges in achieving high thermoelectric conversion efficiency, particularly due to low ZT values and limitations in miniaturization and surface mounting, with existing materials having low heat resistance and limited thermoelectric conversion efficiency, especially at higher temperatures.

Method used

A thermoelectric element design featuring a first thermoelectric material with a higher Seebeck coefficient and electrical resistivity, formed in a chip shape, and a second thermoelectric material in a parallel circuit configuration, with electrodes on one end and the second material on the outer peripheral surface, allowing for high thermoelectric conversion efficiency and miniaturization.

Benefits of technology

The design achieves high thermoelectric conversion efficiency and ZT values, enabling easy surface mounting and installation, with improved power generation output and reduced electrical resistance, suitable for energy harvesting applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139717000001_ABST
    Figure 2024139717000001_ABST
Patent Text Reader

Abstract

To provide a thermoelectric element that has high thermoelectric conversion efficiency, can obtain a high ZT value, is surface mountable, and can be reduced in size.SOLUTION: A thermoelectric element comprises: a first thermoelectric material part 1 having one end 1a and the other end 1b; a second thermoelectric material part 2 joined to the first thermoelectric material part directly or with a conductor 2a therebetween; and a pair of electrodes 3 connected to the first thermoelectric material part. The first thermoelectric material part has a higher Seebeck coefficient and a higher electric resistivity than the second thermoelectric material part. The first thermoelectric material part is formed into a chip shape. The pair of electrodes are provided on a one-end-side face and the-other-end-side face of the first thermoelectric material part. The second thermoelectric material part is formed on an outer peripheral surface of the first thermoelectric material part in a non-contact state with the pair of electrodes.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermoelectric element capable of obtaining high thermoelectric conversion efficiency. [Background technology]

[0002] 2. Description of the Related Art So-called segment-type thermoelectric elements in which a plurality of materials having different compositions are joined together are conventionally known. For example, Patent Document 1 describes a thermoelectric element in which a first electrode, a second electrode, a P-type semiconductor thin film made of a thermoelectric material, and an N-type semiconductor thin film made of a thermoelectric material are formed on a substrate, the P-type semiconductor thin film being connected to the first electrode and the N-type semiconductor thin film being connected to the second electrode, the P-type semiconductor thin film and the N-type semiconductor thin film being overlapped and bonded together, and the bonded surface being present over substantially the entire surface of the substrate.

[0003] Patent Documents 2 and 3 also describe a thermoelectric element in which a first thermoelectric material and a second thermoelectric material made of different materials are joined together, one of a pair of electrodes is connected to the first thermoelectric material, and the other of the pair of electrodes is connected to the second thermoelectric material. That is, in these conventional thermoelectric elements, electrodes are provided on the joined first thermoelectric material and second thermoelectric material, respectively, and the first thermoelectric material and the second thermoelectric material are electrically connected in series. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 10-303471 [Patent Document 2] JP 2009-32960 A [Patent Document 3] JP 2018-152464 A Summary of the Invention [Problem to be solved by the invention]

[0005] The above conventional techniques still have the following problems. That is, the performance of thermoelectric elements required for practical thermoelectric power generation requires that the ZT value (dimensionless figure of merit ZT (=S2T / ρκ): where S, T, ρ, and κ are the Seebeck coefficient (thermoelectromotive force; electromotive force generated per 1K temperature difference), absolute temperature, electrical resistivity, and thermal conductivity κ), which is an index showing the energy conversion performance of thermoelectric conversion materials, must be 1 or more. In addition, to increase both the voltage output and the amount of power generated (= voltage x current) obtained by thermoelectric conversion, the thermoelectric element must have P-type and N-type characteristics, the absolute value of the Seebeck coefficient must be 100μV / K or more, and the power factor (Power factor PW=S 2 / ρ) is 1×10 -3 W / mK 2 It is required to have a performance higher than that. To date, research and development has been conducted on various material systems with the aim of increasing the ZT value using a single material, but the only materials in practical use with a ZT value of approximately 1 at temperatures near room temperature are Bi-Te-based materials. However, Bi-Te-based materials have low heat resistance, limiting their use to temperatures below approximately 200°C, and have low thermoelectric conversion efficiency, making the practical use of thermoelectrics difficult. On the other hand, when the above-mentioned conventional segmented thermoelectric element is used, a thermoelectric material with a heat resistance of 200°C or more can be arranged on the high temperature side, but the ZT value of each thermoelectric material constituting the segmented thermoelectric element is small, and since multiple thermoelectric elements form an electrical and thermal series circuit, the ZT value of the element as a whole is small, making it difficult to increase the thermoelectric conversion efficiency. Furthermore, there is a demand for a thermoelectric element that can be surface mounted and miniaturized.

[0006] The present invention has been made in consideration of the above-mentioned problems, and aims to provide a thermoelectric element that has high thermoelectric conversion efficiency, is capable of obtaining a high ZT value, and can be surface-mounted and miniaturized. [Means for solving the problem]

[0007] The present invention employs the following configuration to solve the above problems. That is, a thermoelectric element according to a first invention includes a first thermoelectric material part having one end and the other end, a second thermoelectric material part joined to the first thermoelectric material part directly or via a conductor, and a pair of electrodes connected to the first thermoelectric material part, the first thermoelectric material part has a higher absolute value of Seebeck coefficient and a higher electrical resistivity than the second thermoelectric material part, the first thermoelectric material part is formed in a chip shape, the pair of electrodes are provided on an end face on the one end side and an end face on the other end side of the first thermoelectric material part, and the second thermoelectric material part is formed on an outer circumferential surface of the first thermoelectric material part in a state of not contacting the pair of electrodes.

[0008] In this thermoelectric element, the first thermoelectric material part is formed in a chip shape, a pair of electrodes is provided on one end face and the other end face of the first thermoelectric material part, and the second thermoelectric material part is formed on the outer peripheral surface of the first thermoelectric material part without contacting the pair of electrodes. This enables surface mounting and miniaturization, and makes it possible to realize an element with high thermoelectric conversion efficiency and ZT value. That is, the thermoelectric element of the present invention is entirely chipped, and has electrodes formed on both end faces, which facilitates surface mounting by soldering or the like, and has a compact shape, allowing for a high degree of freedom in where it can be installed. For example, in an existing pi-shaped thermoelectric module, multiple thermoelectric elements with electrodes are electrically connected in series on a substrate, but it is possible to install the chipped thermoelectric element of the present invention without changing the structure of the thermoelectric module. In addition, since the element structure makes it easy to increase the contact area between the first thermoelectric material part and the electrode, it is easy to reduce the electrical resistance of the entire element, making it possible to increase the thermoelectric power generation output when a temperature difference is applied.

[0009] In this thermoelectric element, the first thermoelectric material section has a higher absolute value of the Seebeck coefficient and a higher electrical resistivity than the second thermoelectric material section, and a pair of electrodes are connected to one end side and the other end side of the first thermoelectric material section at a distance from each other, so that the first thermoelectric material section and the second thermoelectric material section form an electrical and thermal parallel circuit, and when a temperature difference occurs between the one end side and the other end side (heat flow occurs), a thermoelectromotive force is generated with high thermoelectric conversion efficiency. That is, the first thermoelectric material section, which has a high Seebeck coefficient (absolute value) and a high electrical resistance value and to which the pair of electrodes are connected, forms an electromotive voltage path that mainly follows the Seebeck effect, and the second thermoelectric material section, which has a low electrical resistance value and is joined and in contact with the first thermoelectric material section, forms a current path. It is desirable that the current value flowing in the second thermoelectric material section follows Ohm's law. In this way, by configuring a parallel circuit of an electromotive voltage path and a current path, a current path that serves as a current path separate from the electromotive voltage path is formed, so that the electrical conductivity flowing between the pair of electrodes increases while maintaining the high Seebeck coefficient (absolute value) of the first thermoelectric material part, and high thermoelectric conversion efficiency and ZT value can be obtained. The second thermoelectric material section and the pair of electrodes are not directly joined, but are in electrical contact via the first thermoelectric material section. The present invention has a structure of a thermoelectric element in which multiple materials with different compositions are joined, but is characterized in that a pair of electrodes (two electrodes) are connected to the first thermoelectric material section. (Segment-type thermoelectric elements also have a structure in which multiple materials with different compositions are joined, but the pair of electrodes are connected to different thermoelectric materials, and an electrode connection method different from that of the present invention is used.)

[0010] The thermoelectric element of the second invention is characterized in that, in the first invention, it has an insulating material part formed on the surface of the first thermoelectric material part, between the electrode and the first thermoelectric material part. In other words, this thermoelectric element has an insulating material part formed on the surface of the first thermoelectric material part between the electrodes and the first thermoelectric material part, so that the insulating material part can prevent the pair of electrodes from contacting the second thermoelectric material part.

[0011] A thermoelectric element according to a third invention is the thermoelectric element according to the first or second invention, characterized in that the second thermoelectric material part is joined to the top and bottom surfaces of the first thermoelectric material part, respectively. That is, in this thermoelectric element, the second thermoelectric material section is joined to the top and bottom surfaces of the first thermoelectric material section, respectively, so that current paths are formed above and below, respectively, and higher thermoelectric conversion efficiency can be obtained.

[0012] A thermoelectric element according to a fourth invention is the third invention, characterized in that the second thermoelectric material part is also joined to both side surfaces of the first thermoelectric material part. In other words, in this thermoelectric element, the second thermoelectric material part is joined to both side surfaces of the first thermoelectric material part, so that current paths are formed not only on the top and bottom surfaces but also on both side surfaces, thereby achieving even higher thermoelectric conversion efficiency.

[0013] A thermoelectric element according to a fifth invention is any of the first to fourth inventions, characterized in that the first thermoelectric material part has a Seebeck coefficient that is 50 μV / K or more higher in absolute value than the second thermoelectric material part, and an electrical resistivity that is 10 times or more higher. That is, in this thermoelectric element, the first thermoelectric material section has a Seebeck coefficient that is 50 μV / K or more higher than that of the second thermoelectric material section, and an electrical resistivity that is 10 times higher. Therefore, by forming an electromotive voltage path with a sufficiently high Seebeck effect (absolute value) and a current path with sufficiently high electrical conductivity, it is possible to obtain a higher thermoelectric conversion efficiency and ZT value.

[0014] A thermoelectric element according to a sixth aspect of the present invention is any one of the first to fifth aspects of the present invention, wherein the first thermoelectric material section and the second thermoelectric material section are both A 2+δ It is characterized in that it is formed of M (wherein A is at least one of Ag and Cu, and M is at least one of S, Se and Te). In addition, the 1st Thermoelectric Materials Department A 2+δ M is the second thermoelectric material part A 2+δIt is possible to obtain a large ZT value by designing the composition of the material so that the absolute value of the Seebeck coefficient is 50 μV / K or more larger than M and the electrical resistivity is 10 times larger.

[0015] The thermoelectric element of the seventh invention is characterized in that, in the sixth invention, the first thermoelectric material part is formed of Ag—S, and the second thermoelectric material part is formed of Ag—Se or Ag—S—Se. That is, in this thermoelectric element, for example, by forming the first thermoelectric material section from Ag2S and the second thermoelectric material section from Ag2Se, it becomes possible to obtain a ZT value of 1 or more at least at room temperature.

[0016] The thermoelectric element according to an eighth invention is characterized in that, in the sixth invention, the first thermoelectric material part is formed of Cu-S, and the second thermoelectric material part is formed of Cu-Se. That is, in this thermoelectric element, for example, by forming the first thermoelectric material section from Cu2S and the second thermoelectric material section from Cu2Se, it becomes possible to obtain a ZT value of 1 or more at least at room temperature.

[0017] A thermoelectric element according to a ninth invention is any one of the first to fifth inventions, characterized in that the first thermoelectric material portion is formed of a material containing at least Bi and Te. That is, in this thermoelectric element, the first thermoelectric material portion is made of a material containing at least Bi and Te, such as Bi-Te or Bi-Sb-Te. For example, the first thermoelectric material portion is made of Bi2Te3, and the second thermoelectric material portion is made of Cu. 0.55 Ni 0.45 (constantan), it is possible to obtain a power factor at least twice that of Bi2Te3 alone. If the first thermoelectric material section has a higher absolute value of the Seebeck coefficient and a higher electrical resistivity than the second thermoelectric material section, the thermoelectric properties will be improved compared to the first thermoelectric material section alone, regardless of the composition of the second thermoelectric material section.

[0018] A thermoelectric element according to a tenth invention is any of the first to ninth inventions, characterized in that the pair of electrodes are partially embedded in the first thermoelectric material part. That is, in this thermoelectric element, the pair of electrodes are partially embedded in the first thermoelectric material part, so that the electrodes are firmly fixed to the first thermoelectric material part, and stable conduction can be achieved. Effect of the Invention

[0019] According to the present invention, the following effects are obtained. That is, in the thermoelectric element according to the present invention, the first thermoelectric material part is formed in a chip shape, a pair of electrodes is provided on one end face and the other end face of the first thermoelectric material part, and the second thermoelectric material part is formed on the outer peripheral surface of the first thermoelectric material part in a state of not contacting the pair of electrodes. Therefore, it is possible to realize an element that can be surface mounted and miniaturized, and that has high thermoelectric conversion efficiency and ZT value. Therefore, the thermoelectric element of the present invention has a high degree of freedom in installation and can be easily implemented in a circuit or module, and since it achieves high thermoelectric conversion efficiency and ZT value, it becomes possible to commercialize environmental power generation that extracts electricity highly efficiently by using temperature differences. [Brief description of the drawings]

[0020] [Figure 1] 1 is a cross-sectional view showing a thermoelectric element according to a first embodiment of the thermoelectric element according to the present invention. [Diagram 2] FIG. 2 is a conceptual diagram for explaining the principle of a thermoelectric element in the first embodiment. [Diagram 3] 1 is a cross-sectional view perpendicular to an axial direction (direction from one end to the other end) showing a thermoelectric element according to a second embodiment of the present invention. FIG. [Figure 4] FIG. 2 is a cross-sectional view showing an example of a thermoelectric element of the present invention produced in order to demonstrate the principle of the thermoelectric element of the present invention. [Diagram 5] FIG. 11 is a cross-sectional view showing a thermoelectric element according to a third embodiment of the thermoelectric element according to the present invention. [Figure 6]10A to 10C are perspective views showing the manufacturing process of a thermoelectric element in the third embodiment in the order of steps. [Figure 7] FIG. 3 is a cross-sectional view showing a thermoelectric element in another example of the first embodiment of the thermoelectric element according to the present invention. [Figure 8] 4 is a graph showing the results of evaluating the power generation characteristics of a thermoelectric element in an example of a thermoelectric element according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] A first embodiment of a thermoelectric element according to the present invention will be described below with reference to Figures 1 and 2. In the drawings used in the following description, the scale is appropriately changed as necessary to make each part recognizable or easily recognizable.

[0022] As shown in Figures 1 and 2, the thermoelectric element 10 of this embodiment comprises a first thermoelectric material part 1 having one end 1a and the other end 1b, a second thermoelectric material part 2 joined to the first thermoelectric material part 1 directly or via a conductor 2a, and a pair of electrodes 3 connected to the first thermoelectric material part 1. When the first thermoelectric material part 1 and the second thermoelectric material part 2 are joined via the conductor 2a, the conductor 2a also functions as an intermediate layer. The conductor 2a is, for example, a conductive bonding material such as solder or In. The first thermoelectric material section 1 has a higher absolute value of the Seebeck coefficient and a higher electrical resistivity than the second thermoelectric material section 2 . The first thermoelectric material part 1 is formed in a chip shape. That is, the first thermoelectric material part 1 has a rectangular parallelepiped shape, and both end faces thereof are one end part 1a and the other end part 1b.

[0023] The pair of electrodes 3 are formed on an end surface of the first thermoelectric material part 1 on the one end 1a side and an end surface of the first thermoelectric material part 1 on the other end 1b side. The second thermoelectric material part 2 is formed on the outer circumferential surface of the first thermoelectric material part 1 in a state of not being in contact with the pair of electrodes 3 . That is, the pair of electrodes 3 and the second thermoelectric material part 2 are spaced apart from each other, and the pair of electrodes 3 are in contact with the first thermoelectric material part 1 without being in contact with the second thermoelectric material part 2.

[0024] Moreover, the thermoelectric element 10 of this embodiment includes an insulating material portion 5 formed on the surface of the first thermoelectric material portion 1 between the electrode 3 and the first thermoelectric material portion 1 . The second thermoelectric material part 2 is joined to the top and bottom surfaces of the first thermoelectric material part 1, respectively. That is, the second thermoelectric material part 2 is formed on the upper and lower surfaces of the first thermoelectric material part 1 and spaced apart from the pair of electrodes 3 formed on both end surfaces of the first thermoelectric material part 1 by, for example, about 1 mm. Moreover, the insulating material portion 5 is formed on the upper and lower surfaces of the first thermoelectric material portion 1 from the end portion of the second thermoelectric material portion 2 to the nearby electrode 3 . In this manner, the pair of electrodes 3 are connected in contact with only the first thermoelectric material portion 1 , and are not in contact with the second thermoelectric material portion 2 due to the insulating material portion 5 .

[0025] It is preferable that the first thermoelectric material section 1 has a Seebeck coefficient that is at least 50 μV / K larger in absolute value than the second thermoelectric material section 2, and an electrical resistivity that is at least 10 times larger. The electrical resistivity of the first thermoelectric material unit 1 at room temperature is 10 -5 Ωcm or less is preferable. For example, the first thermoelectric material unit 1 and the second thermoelectric material unit 2 are both A 2+δ M (wherein A is at least one of Ag and Cu, and M is at least one of S, Se and Te). The range of δ is preferably -0.5≦δ≦+0.5, and more preferably -0.05 to +0.02.

[0026] In the present invention, the thermoelectric material is defined as a material having a Seebeck coefficient with an absolute value of 0.1 μV / K or more. That is, the absolute value of the Seebeck coefficient of the second thermoelectric material section 2 is 0.1 μV / K or more. Furthermore, the absolute value of the Seebeck coefficient of the first thermoelectric material portion 1 is preferably 10 mV / K or less. Furthermore, when the electrical resistivity of the first thermoelectric material part 1 at room temperature is 10 mΩcm or less, it is preferable that the first thermoelectric material part 1 is thinner than the second thermoelectric material part 2. Furthermore, when the electrical resistivity of the first thermoelectric material part 1 at room temperature is 10 mΩcm or less, and the electrical resistivity of the second thermoelectric material part 2 at room temperature is 1 mΩcm or less and the thermal conductivity is 10 W / mK or more, it is preferable that the thickness of the first thermoelectric material part 1 is thicker than the thickness of the second thermoelectric material part 2.

[0027] A 2+δ In the case of an N-type thermoelectric element, for example, a configuration in which the first thermoelectric material part 1 is made of Ag-S and the second thermoelectric material part 2 is made of Ag-Se or Ag-S-Se can be used as M. In the case of a P-type thermoelectric element, for example, a configuration in which the first thermoelectric material part 1 is made of Cu-S and the second thermoelectric material part 2 is made of Cu-Se can be used. For example, the first thermoelectric material section 1 can be made of Ag2S, and the second thermoelectric material section 2 can be made of Ag2Se. Ag2S has a Seebeck coefficient that is 50 μV / K or more higher in absolute value than Ag2Se, and an electrical resistivity that is 10 times or more higher. Alternatively, the first thermoelectric material portion 1 may be made of Cu2S, and the second thermoelectric material portion 2 may be made of Cu2Se. Cu2S has a Seebeck coefficient that is 50 μV / K or more higher in absolute value than Cu2Se, and an electrical resistivity that is 10 times higher. The first thermoelectric material portion 1 may be made of a material containing at least Bi and Te, such as Bi-Te or Bi-Sb-Te. For example, the first thermoelectric material portion 1 may be made of Bi2Te3 or (Bi 0.7 Sb 0.3 ) Te3, and the second thermoelectric material portion 2 is formed of Cu 0.55 Ni 0.45 (Constantan). Bi2Te3 and (Bi 0.7 Sb 0.3 ) Te3 is Cu 0.55 Ni 0.45 The absolute value of the Seebeck coefficient is 50 μV / K or more higher and the electrical resistivity is 10 times higher than that of the It is also possible to employ the first thermoelectric material portion 1 in which impurities such as Ru or Cu are added to the material containing Bi and Te. The insulating material portion 5 is formed of, for example, alumina, SiO2, an organic material (resin), or the like.

[0028] In this manner, the first thermoelectric material section 1 is made of a high resistance semiconductor material or insulating material such as a low thermal conductive chalcogenide material, and the second thermoelectric material section 2 is made of a low resistance conductive material such as a semiconductor material or alloy. It is preferable that both the first thermoelectric material part 1 and the second thermoelectric material part 2 have low thermal conductivity. Note that, in order to obtain a high thermoelectromotive force, the first thermoelectric material part 1 preferably has a thermal conductivity of 10 W / mK or less. The thermal conductivity of the first thermoelectric material portion 1 is preferably 0.02 W / mK or more.

[0029] When the first thermoelectric material part 1 and the second thermoelectric material part 2 are joined via the conductor 2a, solder, In, etc. can be used as the conductor 2a. Note that the electrical resistivity of this conductor 2a is preferably approximately the same as that of the second thermoelectric material part. The pair of electrodes 3 may be made of, for example, Ag paste or Ag solder, and are formed on both end faces of the first thermoelectric material part 1 by dipping or the like. The material of the pair of electrodes 3 has an electrical resistivity of 10 -4 Ωm or less is adopted.

[0030] The method for manufacturing the thermoelectric element 10 of this embodiment includes a joining process for joining the second thermoelectric material part 2 and the first thermoelectric material part 1, and an electrode formation process for forming a pair of electrodes 3 on the first thermoelectric material part 1. For example, in the joining step, the second thermoelectric material part 2 and the first thermoelectric material part 1 are joined together with a conductive joining material such as solder. In addition, in the above bonding process, various thin film growth methods (vapor phase growth methods such as PVD, sputtering, and CVD) are adopted. When a chalcogenide material is used for the first thermoelectric material part 1, it is preferable to form the first thermoelectric material part 1 as a film on the second thermoelectric material part 2 by the MBD method (molecular beam deposition method).

[0031] In the above bonding step, the first thermoelectric material part 1 may be formed as a film on the second thermoelectric material part 2 by a sol-gel method. In addition, in the above-mentioned joining process, a hot pressing method may be used in which, in a state in which the powder that will become the first thermoelectric material part 1 and the powder that will become the second thermoelectric material part 2 are stacked, the first thermoelectric material part 1 and the second thermoelectric material part 2 are sintered, and the first thermoelectric material part 1 and the second thermoelectric material part 2 are joined together at the same time.

[0032] As described above, in the thermoelectric element 10 of the present embodiment, the first thermoelectric material part 1 is formed in a chip shape, a pair of electrodes 3 are provided on an end face on one end 1a side and an end face on the other end 1b side of the first thermoelectric material part 1, and the second thermoelectric material part 2 is formed on the outer peripheral surface of the first thermoelectric material part 1 in a state of not contacting the pair of electrodes 3. Therefore, it is possible to realize an element that can be surface mounted and miniaturized, and that has high thermoelectric conversion efficiency and ZT value. In other words, the thermoelectric element 10 of the present invention is formed as a chip in its entirety, and since electrodes 3 are formed on both end surfaces, it is easy to surface mount using solder or the like, and since it has a compact shape, there is a high degree of freedom in where it can be installed.

[0033] In this thermoelectric element 10, the first thermoelectric material part 1 has a higher Seebeck coefficient (absolute value) and higher electrical resistivity than the second thermoelectric material part 2, and a pair of electrodes 3 are connected to one end 1a and the other end 1b of the first thermoelectric material part 1 at a distance from each other. Therefore, the first thermoelectric material part 1 and the second thermoelectric material part 2 form a parallel circuit, and when a temperature difference occurs between the one end 1a and the other end 1b (heat flow occurs), an electromotive force is generated with high thermoelectric conversion efficiency.

[0034] That is, as shown in FIG. 2, the first thermoelectric material part 1, which is connected to a pair of electrodes 3 and has a high Seebeck coefficient (absolute value) and a high electrical resistance, forms an electromotive voltage path R1 that mainly follows the Seebeck effect, and the second thermoelectric material part 2, which is joined to and in contact with the first thermoelectric material part 1 and has a low electrical resistance, forms a current path R2. It is desirable that the current value flowing in the second thermoelectric material part 2 follows Ohm's law. In this way, by forming a parallel circuit of the electromotive voltage path R1 and the current path R2, the current path R2, which is a current path separate from the electromotive voltage path R1, is formed, and the electrical conductivity flowing between the pair of electrodes 3 increases while maintaining the high Seebeck coefficient (absolute value) of the first thermoelectric material part 1, and a high thermoelectric conversion efficiency and ZT value can be obtained. Note that the arrow Y in FIG. 2 indicates the heat flow direction (the direction in which the heat flux flows, the direction in which a temperature difference occurs).

[0035] In addition, since the insulating material part 5 is formed on the surface of the first thermoelectric material part 1 between the electrode 3 and the first thermoelectric material part 1, the insulating material part 5 can prevent the pair of electrodes 3 from contacting the second thermoelectric material part 2. Furthermore, since the second thermoelectric material part 2 is joined to the top and bottom surfaces of the first thermoelectric material part 1, current paths R2 are formed on the top and bottom, respectively, and higher thermoelectric conversion efficiency can be obtained.

[0036] Furthermore, since the first thermoelectric material part 1 has a Seebeck coefficient whose absolute value is 50 μV / K or more higher than that of the second thermoelectric material part 2 and whose electrical resistivity is 10 times higher, an electromotive voltage path R1 with a sufficiently high Seebeck effect and a current path R2 with sufficiently high electrical conductivity are formed, thereby making it possible to obtain higher thermoelectric conversion efficiency and ZT value. The absolute value of the Seebeck coefficient of the first thermoelectric material part 1 may be 100 μV / K or more greater than the absolute value of the Seebeck coefficient of the second thermoelectric material part 2. The greater the difference between the absolute value of the Seebeck coefficient of the first thermoelectric material part 1 and the absolute value of the Seebeck coefficient of the second thermoelectric material part 2, the more desirable it is, and although there is no particular upper limit, it may be 10,000 μV / K.

[0037] In addition, by forming the first thermoelectric material portion 1 from Ag2S and the second thermoelectric material portion 2 from Ag2Se, the output factor (PW=S 2 / ρ) becomes large, making it possible to obtain an N-type thermoelectric element with a ZT value of 1 or more at least at room temperature. In addition, by forming the first thermoelectric material portion 1 from Cu2S and the second thermoelectric material portion 2 from Cu2Se, the output factor (PW=S 2 / ρ) becomes large, making it possible to obtain a P-type thermoelectric element with a ZT value of 1 or more at least at room temperature. The first thermoelectric material portion 1 is made of Bi2Te3, and the second thermoelectric material portion 2 is made of Cu. 0.55 Ni 0.45 By forming it from Bi2Te3 (constantan), it is possible to obtain an N-type thermoelectric element having a power factor at least twice that of a single substance of Bi2Te3. The first thermoelectric material portion 1 is made of (Bi 0.7 Sb 0.3 )2Te3, and the second thermoelectric material part 2 is formed of Cu 0.55 Ni 0.45 (Constantan) to form at least (Bi 0.7 Sb 0.3 It is now possible to obtain a P-type thermoelectric element with a power factor approximately twice that of a single element of 2Te3.

[0038] Next, second and third embodiments of the thermoelectric element according to the present invention will be described below with reference to Fig. 3 to Fig. 6. In the following description of each embodiment, the same components as those described in the above embodiments are denoted by the same reference numerals, and the description thereof will be omitted.

[0039] The second embodiment differs from the first embodiment in that, while in the first embodiment, the second thermoelectric material part 2 is joined to the top and bottom surfaces of the first thermoelectric material part 1, in the thermoelectric element 20 of the second embodiment, the second thermoelectric material part 2 is joined to both side surfaces of the first thermoelectric material part 1 as well, as shown in FIG. 3.

[0040] That is, in the second embodiment, the second thermoelectric material part 2 covers the entire outer peripheral surface of the first thermoelectric material part 1 , and the second thermoelectric material part 2 is joined to all four outer peripheral surfaces of the first thermoelectric material part 1 . As described above, in the thermoelectric element 20 of the second embodiment, the second thermoelectric material part 2 is joined to both side surfaces of the first thermoelectric material part 1, so that a current path R2 is formed not only on the top and bottom surfaces but also on both side surfaces, thereby achieving even higher thermoelectric conversion efficiency.

[0041] Next, the third embodiment differs from the first embodiment in that, in the first embodiment, a pair of electrodes 3 are formed on the end face on one end 1a side and the end face on the other end 1b side of the first thermoelectric material part 1, whereas in the thermoelectric element 30 of the third embodiment, as shown in Figures 5 and 6, a pair of electrodes 33 protrude outward from the end face on one end 1a side and the end face on the other end 1b side of the first thermoelectric material part 31, and a portion of the base end side is embedded in the first thermoelectric material part 31.

[0042] That is, the pair of electrodes 3 in the first embodiment are formed on both end faces of the first thermoelectric material part 1 by dipping or the like with a conductive material such as Ag paste or Ag solder, whereas in the third embodiment, the pair of electrodes 33 are formed from a metal plate such as a Cu plate, and are formed with tip portions protruding outward from the end face on one end 1a side and the end face on the other end 1b side of the first thermoelectric material part 31, and with the base end side embedded within the first thermoelectric material part 31.

[0043] In a manufacturing method of the thermoelectric element 30 of the third embodiment, for example, as shown in (a) of Fig. 6, first, a first thermoelectric material lower part 31a which becomes the lower first thermoelectric material part 31 is placed on the second thermoelectric material part 2, and then, as shown in (b) of Fig. 6, a pair of electrodes 33 is placed on the first thermoelectric material lower part 31a with an intermediate insulating material 35 such as a glass plate disposed therebetween. At this time, the tips of the pair of electrodes 33 are arranged to protrude from both end faces of the first thermoelectric material lower part 31a. The intermediate insulating material 35 may be made of any material having a higher resistance than the first thermoelectric material portion 31 . Furthermore, as shown in FIG. 6(c), the first thermoelectric material upper part 31b, which will become the upper first thermoelectric material part 31, and the second thermoelectric material part 2 are placed on the pair of electrodes 33 and the intermediate insulating material 35, and the above-mentioned laminated parts are joined by hot pressing, spark plasma sintering, or the like.

[0044] As a result, a pair of electrodes 33 are sandwiched and joined between the first thermoelectric material lower part 31a and the second thermoelectric material upper part 31b, and the tip parts are provided protruding outward from both end faces of the first thermoelectric material part 31 with the base parts embedded in the chip-shaped first thermoelectric material part 31 consisting of the first thermoelectric material lower part 31a and the second thermoelectric material upper part 31b. As described above, in the thermoelectric element 30 of the third embodiment, a pair of electrodes 33 are partially embedded within the first thermoelectric material part 31, so that the electrodes 33 are firmly fixed to the first thermoelectric material part 31, thereby ensuring stable electrical conduction. EXAMPLES

[0045] In order to demonstrate the principle of the thermoelectric properties of the present invention, a sample as shown in FIG. 4 was produced as an example, and the evaluation results are shown in Tables 1 and 2. In the examples of the present invention, the first thermoelectric material part and the second thermoelectric material part were fabricated using the materials and manufacturing methods described in the above embodiment, and their thermoelectric properties (conductivity type determination (P / N type determination), Seebeck coefficient, electrical resistivity, and power factor) at room temperature (300 K) were investigated. As a comparative example of the present invention, a thermoelectric element made of a single thermoelectric material was evaluated in the same manner as in the examples of the present invention. Each example was produced as follows. In the examples of the present invention, for evaluation purposes, the first thermoelectric material part 1 is joined to the upper surface of the second thermoelectric material part 2, and a pair of electrodes 3 is formed on the upper surface of the first thermoelectric material part 1.

[0046] <Examples 1 and 2> <Examples 9 to 12> (Solder joint) First, a Bi-Te bulk sintered body (or Bi-Sb-Te bulk sintered body) serving as the first thermoelectric material part and a Cu-Ni alloy plate or a Cu plate serving as the second thermoelectric material part were prepared, cut into a predetermined size, and the bonding surfaces were polished. After that, a solder foil was placed on the bonding surface between the Bi-Te bulk sintered body and the Cu-Ni alloy plate or the Cu plate, and using a hot press machine, the Bi-Te bulk sintered body and the Cu-Ni alloy plate or the Cu plate were joined by utilizing solder melting. That is, the second thermoelectric material part was joined to the first thermoelectric material part through an intermediate layer of solder as a conductor. The above joining conditions were a pressure of 100 MPa, a joining temperature of 250 degrees, and a holding time of about 5 minutes. After visually confirming the melting of the solder, a cooling process and a process of reducing the pressure were performed. Thereafter, using an Ag paste or the like, two pairs of electrodes were formed on the first thermoelectric material part side (Bi-Te side) to obtain Examples 1 and 2.

[0047] <Example 3> (MBD Film Deposition) First, using an MBD (molecular beam epitaxy) apparatus, an Ag2S thin film serving as the first thermoelectric material part was deposited on an Ag2Se bulk sintered body serving as the second thermoelectric material part. The Ag2Se bulk sintered body was formed by the SHS (self-propagating high-temperature synthesis) method. In the film deposition by the above MBD method, the substrate temperature was set at room temperature, and a cell containing Ag and S as raw materials was heated to an appropriate temperature with a heater to perform film deposition, thereby obtaining a single-phase thin film of Ag2S serving as the first thermoelectric material part. Note that through an X-ray diffraction experiment, it has been confirmed that the Ag2S thin film and the Ag2Se bulk sintered body are crystalline materials. Ag2S 1-x Se x In the Ag2S The production of the electrodes is the same as in Examples 1 and 2.

[0048] <Examples 4 to 8> <Examples 13 to 17> (Hot press) First, the raw material powders (e.g., Ag, S, Cu, etc.) for the first thermoelectric material part and the second thermoelectric material part are weighed out to a predetermined stoichiometric ratio, mixed, molded using a press, and then heat-treated at a predetermined temperature to obtain, for example, a sintered body of a single phase of AgS. When a chalcogenide containing S, Se, or Te is used, a single-phase sintered body can be obtained even by using the self-heating reaction method. If an unreacted phase is confirmed by the X-ray diffraction experiment, the sintered body is crushed into powder and the above process is repeated. Since the X-ray diffraction experiment shows that a single-phase sintered body is obtained, this process is repeated.

[0049] After the single-phase sintered body is obtained, the sintered body is pulverized in a mortar or the like to obtain, for example, Ag2S, Ag2Se, Cu, etc. 2-δ S, Cu 2-δ Obtain Se powder. These powders are heated and pressurized in a hot press to produce bulk bodies of the first and second thermoelectric material parts, and at the same time, a joint body of the first and second thermoelectric material parts is produced. Note that, during the hot press, Ag2S, Ag2Se, Cu, etc. are used in consideration of density. 2-δ S, Cu 2-δ The Se is weighed out to achieve the desired thickness, and the raw materials are added in order and molded.

[0050] In addition, the bonding conditions using the hot press are a pressure of 100 MPa, a predetermined holding temperature, and a holding time of 20 minutes to form a bonded body. Thereafter, the bonded body is cut using a wire saw or the like to obtain a chip-shaped bonded body of, for example, 17 mm×3 mm×2 mmt. The electrodes were prepared in the same manner as in Examples 1 and 2.

[0051] <Method of evaluating thermoelectric elements> When a temperature difference ΔT is applied to a thermoelectric element, a voltage ΔV proportional to the temperature difference is generated. This phenomenon is called the Seebeck effect, and the generated voltage is called thermoelectromotive force, with the proportionality coefficient S = ΔV / ΔT defined as the Seebeck coefficient S. In other words, to measure the Seebeck coefficient, it is necessary to measure both the potential difference (thermoelectromotive force) between two terminals and the temperature difference. The Seebeck coefficient was measured using two commercially available Peltier elements, one of which was cooled and the other was wired to be heated so as to create a temperature difference between the two Peltier elements, with a temperature difference of 0.1 to 5°C. The thermocouple used for the measurements was a T-type thermocouple (Cu-Constantan). An extremely thin type, about 20 microns, was selected for this thermocouple, and a rubber material with high electrical insulation and heat insulation was used to apply a load, achieving good thermal and electrical contact between the material and the thermocouple. In addition, a two-terminal method called the thermoelectric probe method was adopted, and the potential difference (thermoelectromotive force) between the two terminals was measured using the Cu wiring of two T-type thermocouples. The relationship between the thermoelectromotive force ΔV and the temperature difference ΔT was plotted, and the Seebeck coefficient was evaluated from the linear relationship near the zero temperature difference (near the origin of ΔV / ΔT). The P type and N type (conductivity type) were determined from the sign of the measured Seebeck coefficient. When joining the first thermoelectric material part and the second thermoelectric material part, it is desirable to align the P type / N type polarity to be the same, i.e., to join P types together or N types together, but it is also possible to join opposite polarities, i.e., P type and N type together. Even in such a case, the first thermoelectric material part has a higher absolute value of the Seebeck coefficient and a higher electrical resistivity than the second thermoelectric material part to which it is joined.

[0052] The electrical resistivity (electrical conductivity) was measured by the four-terminal method. In this measurement, a terminal for measuring a current and a terminal for measuring a voltage were both connected to the electrode terminal. In addition, when calculating the electrical resistivity from the electrical resistance value, the thickness was determined as the sum of the thicknesses of the multiple materials. For example, when determining the electrical resistivity of a joint of 0.1 mm Ag2S (first thermoelectric material portion) and 2 mm Ag2Se (second thermoelectric material portion) in Example 4, the thickness was determined as the sum of the thicknesses of the two materials, that is, 2.1 mm. The output factor is expressed as the product of the square of the Seebeck coefficient and the reciprocal of the electrical resistivity (=electrical conductivity), and was calculated from the measured Seebeck coefficient and electrical resistivity.

[0053] [Table 1]

[0054] As can be seen from the above evaluation results, the examples of the present invention all have significantly improved output factors compared to the comparative examples in which the first thermoelectric material section or the second thermoelectric material section is made of a single material. The absolute values ​​of the Seebeck coefficients of the Bi-Te-based materials of Comparative Examples 1 and 2 are 50 μV / K or more larger than the absolute value of the Seebeck coefficient of the Cu-Ni material of Comparative Example 3, and the electrical resistivity of the Bi-Te-based materials of Comparative Examples 1 and 2 is 10 times or more larger than the electrical resistivity of the Cu-Ni material of Comparative Example 3. Therefore, in Examples 1 and 2 in which the first thermoelectric material section is made of a Bi-Te-based material and the second thermoelectric material section is made of Cu-Ni, both an electromotive voltage path with a sufficiently high Seebeck effect and a current path with a sufficiently high electrical conductivity are configured, so that both the electromotive voltage value and the current value outputted between the pair of electrodes become large, and the output factor is significantly improved. N-type characteristics are obtained in Example 1, and P-type characteristics are obtained in Example 2.

[0055] The absolute value of the Seebeck coefficient of Ag2S in Comparative Example 4 is at least 50 μV / K greater than the absolute value of the Seebeck coefficient of Ag2Se in Comparative Example 5, and the electrical resistivity of Ag2S in Comparative Example 4 is at least 10 times greater than the electrical resistivity of Ag2Se in Comparative Example 5. For this reason, in Examples 3 to 6 in which the first thermoelectric material section is made of an Ag2S-based material and the second thermoelectric material section is made of Ag2Se, both an electromotive voltage path with a sufficiently high Seebeck effect and a current path with sufficiently high electrical conductivity are configured, and as a result, both the electromotive voltage value and the current value output from between the pair of electrodes become large, and the output factor is significantly improved. It should be noted that Example 5 exhibits N-type characteristics, whereas Example 4 exhibits P-type characteristics. However, since this material normally exhibits N-type characteristics, it is believed that the P-type characteristics in Example 4 are due to impurities, crystal defects, etc.

[0056] In addition, the absolute value of the Seebeck coefficient of Cu2S in Comparative Example 6 is 50 μV / K or more higher than the absolute value of the Seebeck coefficient of Cu2Se in Comparative Example 7, and the electrical resistivity of Cu2S in Comparative Example 6 is 10 times or more higher than the electrical resistivity of Cu2Se in Comparative Example 7. 2-δ The second thermoelectric material is Cu. 2-δ In Examples 7, 8, and 13 to 17 in which Se was used, both an electromotive voltage path with a sufficiently high Seebeck effect and a current path with sufficiently high electrical conductivity were configured, so that the electromotive voltage value and current value outputted between the pair of electrodes were both large, and the output factor was significantly improved.

[0057] Furthermore, the absolute values ​​of the Seebeck coefficients of the Bi-Te based materials of Comparative Examples 1 and 2 are at least 50 μV / K greater than the absolute value of the Seebeck coefficient of Cu of Comparative Example 8, and the electrical resistivity of the Bi-Te based materials of Comparative Examples 1 and 2 is at least 10 times greater than the electrical resistivity of Cu of Comparative Example 8. For this reason, in Examples 9 to 12 in which the first thermoelectric material section is made of a Bi-Te based material and the second thermoelectric material section is made of Cu, both an electromotive voltage path with a sufficiently high Seebeck effect and a current path with sufficiently high electrical conductivity are configured, so that both the electromotive voltage value and the current value outputted between the pair of electrodes become large, and the output factor is significantly improved.

[0058] In examples where the first thermoelectric material portion is made of Ag2S and the second thermoelectric material portion is made of Ag2Se, it has been confirmed that Ag2S and Ag2Se have thermal conductivities of less than 1 W / mK at room temperature, and in example 4, for example, a ZT value of about 3 at room temperature is obtained, indicating high thermoelectric performance. In addition, a pi-type thermoelectric conversion module with four elements was fabricated using two each of the Bi-Te / Cu-Ni elements exhibiting N-type characteristics of Example 1 and the Bi-Sb-Te / Cu-Ni elements exhibiting P-type characteristics of Example 2, and the power generation performance was compared with that of a pi-type thermoelectric conversion module with four elements consisting only of Bi-Te (Comparative Example 1) and Bi-Sb-Te (Comparative Example 2). As a result, it was confirmed that the thermoelectric conversion module using the elements of the embodiment had a 38.4% improvement in power generation output when a temperature difference of 30 K was applied (the temperature on the low-temperature side was about 20° C. near room temperature).

[0059] <Examples 21 to 25> (Hot press) Examples 21 to 25 of the present invention were produced by the same manufacturing method as in Examples 4 to 6 above, and the temperature dependence of the thermoelectric properties of Examples 21 to 25 was evaluated. In Example 22, the second thermoelectric material part was joined to the first thermoelectric material part by hot pressing via an intermediate layer of Ag as a conductor, and in Example 23, the second thermoelectric material part was joined to the first thermoelectric material part by hot pressing via an intermediate layer of In as a conductor.

[0060] High temperature thermoelectric characterization In the evaluation method of Examples 1 to 17 above, the thermoelectric characteristics were measured at room temperature (25°C), but in Examples 21 to 25 of the present invention, the thermoelectric characteristics were measured at high temperatures of 88 to 95°C. In Examples 21 to 25, the first thermoelectric material portion was Ag2S and the second thermoelectric material portion was Ag2Se. The results are shown in Table 2. As can be seen from the evaluation results of Examples 21 to 25, even at measurement temperatures of 88 to 95° C., a high Seebeck coefficient (absolute value) is maintained, and the power factor is significantly improved. At a measurement temperature of 88 to 95°C, the power factor of Ag2S alone and Ag2Se alone is 2×10 -3W / mK 2 In Examples 21 to 25, extremely high thermoelectric conversion characteristics were obtained compared to a single element. The thermal conductivity of the thermoelectric elements of Examples 21 to 25 was 1.2 W / mK or less. In Examples 24 and 25, the ZT value (=S 2 T / ρκ): where S, T, ρ, and κ are the Seebeck coefficient, absolute temperature, electrical resistivity, and thermal conductivity, respectively. In Example 21, a ZT value of 5 or more was measured, indicating that extremely high thermoelectric conversion properties were obtained.

[0061] [Table 2]

[0062] -Evaluation of power generation characteristics Next, as Example 26, the first thermoelectric material part was made of Ag2S and the second thermoelectric material part was made of Ag2S 0.5 Se 0.5 The power generation characteristics of the thermoelectric element were evaluated. In addition, Ag2S and Ag2S 0.5 Se 0.5 Both show N-type characteristics. 0.5 Se 0.5 The bonding was performed by hot pressing at a temperature of 200° C. or less. In Example 26, no intermediate layer was used, and the element was directly bonded. The thickness of the element is 10 μm for the Ag2S of the first thermoelectric material and 10 μm for the Ag2S of the second thermoelectric material. 0.5 Se 0.5 The thickness of the element was 0.70 mm. The width of the element was 2.2 mm. Furthermore, the distance between the pair of electrodes was 2.91 mm. The electrodes were needle electrodes, which were touched to the first thermoelectric material part in a dotted line to evaluate the power generation characteristics.

[0063] FIG. 8 shows the Ag2S / Ag2S of Example 26 of the present invention. 0.5 Se 0.5 The results of evaluating the power generation characteristics of a thermoelectric element are shown below. To evaluate the power generation characteristics, a closed circuit was created consisting of a thermoelectric element, a variable resistance element (external load resistance element), and an ammeter, and a temperature difference was applied across both ends of the thermoelectric element to measure the voltage, current, and power output from the thermoelectric element. FIG. 8 shows the output voltage value (shown on the left axis) and the power generation output density (shown on the right axis) versus current. Since the thermoelectric element of Example 26 exhibits N-type characteristics, the voltage value is a negative value, but the voltage value shown on the left axis of Fig. 8 is expressed as an absolute value. The amount of power generation is represented as the product of the voltage value and the current value. The power generation output density is calculated by dividing the amount of power generation by the cross-sectional area of ​​the element (the product of the thickness of the element and the width of the element). In Figure 8, actual measured values ​​are displayed as plots, and values ​​calculated based on those measured values ​​are displayed as lines. The voltage value when the output current is zero is called the open circuit voltage. The current value when the output voltage is 0V is called the short circuit current. Figure 8 also shows the results of open circuit voltage evaluation when the low temperature side temperatures of the element are set to 50°C, 60°C, and 70°C, with a temperature difference of 3K.

[0064] As a result of evaluating the power generation characteristics of the thermoelectric element of Example 26, when the low-temperature side temperature of the element was 60°C, the open circuit voltage was 0.59 mV, the short circuit current was 191 μA, and the power generation output density was 1.7 μW cm ―2 It became. The absolute value of the Seebeck coefficient calculated from the open circuit voltage was 196 μV / K. Ag2S 0.5 Se 0.5 Since the absolute value of the Seebeck coefficient of the single element is 130 μV / K, it is clear that the output voltage of Example 26 is increased. Furthermore, the electrical resistivity of Ag2S alone is high, and the short circuit current value of Example 26 is more than 1000 times larger than that of Ag2S alone. Ag2S alone, Ag2S 0.5 Se 0.5 The power output density of each unit is 0.1 μWcm ―2 Less than 1.0μWcm ―2 In contrast, the Ag2S / Ag2S in Example 26 is calculated as follows: 0.5 Se 0.5 The power generation density of the thermoelectric element (= 1.7 μW cm―2 ) is large, and it is clear that extremely high thermoelectric conversion properties have been obtained compared to a single element.

[0065] The technical scope of the present invention is not limited to the above-described embodiment and examples, and various modifications can be made without departing from the spirit of the present invention. For example, in the above embodiment, the thermoelectric element of the present invention is described as being used for power generation, but the thermoelectric element of the present invention may also be used for Peltier cooling, Peltier temperature control, or the like. Furthermore, like the thermoelectric element of the first embodiment described above, it is preferable to have an insulating material part formed on the surface of the first thermoelectric material part between the electrode and the first thermoelectric material part, but a thermoelectric element 10A that does not have an insulating material part may also be used, as shown in Figure 7. [Explanation of symbols]

[0066] Reference Signs List 1, 31...first thermoelectric material portion, 1a...one end portion, 1b...other end portion, 2...second thermoelectric material portion, 2a...conductor, 3, 33...electrode, 5...insulating material portion, 10, 20, 30...thermoelectric element

Claims

1. a first thermoelectric material portion having one end and another end; a second thermoelectric material part joined to the first thermoelectric material part directly or via an electric conductor; a pair of electrodes connected to the first thermoelectric material portion; the first thermoelectric material portion has a higher absolute value of a Seebeck coefficient and a higher electrical resistivity than the second thermoelectric material portion; The first thermoelectric material portion is formed in a chip shape, the pair of electrodes are provided on an end surface on the one end side and an end surface on the other end side of the first thermoelectric material part, A thermoelectric element, characterized in that the second thermoelectric material part is formed on an outer peripheral surface of the first thermoelectric material part in a state of not contacting the pair of electrodes.

2. 2. The thermoelectric element according to claim 1, A thermoelectric element comprising an insulating material portion formed on a surface of the first thermoelectric material portion between the electrode and the first thermoelectric material portion.

3. The thermoelectric element according to claim 1 or 2, A thermoelectric element, characterized in that the second thermoelectric material portion is joined to an upper and lower surface of the first thermoelectric material portion, respectively.

4. The thermoelectric element according to claim 3, A thermoelectric element, characterized in that the second thermoelectric material portion is also joined to both side surfaces of the first thermoelectric material portion.

5. The thermoelectric element according to claim 1 or 2, A thermoelectric element, characterized in that the first thermoelectric material section has a Seebeck coefficient whose absolute value is 50 μV / K or more higher than that of the second thermoelectric material section, and an electrical resistivity which is 10 times or more higher.

6. The thermoelectric element according to claim 1 or 2, The first thermoelectric material unit and the second thermoelectric material unit are both A 2+δA thermoelectric element comprising: a first insulating layer and a second insulating layer, the second insulating layer being formed of at least one of Ag and Cu, and at least one of S, Se and Te.

7. 7. The thermoelectric element according to claim 6, the first thermoelectric material portion is formed of Ag—S; A thermoelectric element, characterized in that the second thermoelectric material portion is formed of Ag--Se or Ag--S--Se.

8. 7. The thermoelectric element according to claim 6, the first thermoelectric material portion is formed of Cu—S; A thermoelectric element, characterized in that the second thermoelectric material portion is formed of Cu--Se.

9. The thermoelectric element according to claim 1 or 2, A thermoelectric element, characterized in that the first thermoelectric material portion is formed of a material containing at least Bi and Te.

10. The thermoelectric element according to claim 1 or 2, A thermoelectric element, characterized in that the pair of electrodes are partially embedded in the first thermoelectric material portion.

Citation Information

Patent Citations

  • Thermoelectric element and thermoelectric element module using the same

    JP1998303471A

  • Segmented thermoelectric device, thermoelectric module, generator, and temperature-regulating device

    JP2009032960A

  • Segment type thermoelectric power module

    JP2018152464A