Carbon fiber sheet manufacturing method
By laminating and treating carbon fiber sheet precursors under inert conditions with controlled oxygen reduction methods, the method addresses oxidative wear and quality issues in carbon fiber sheet production, enhancing furnace longevity and product consistency.
Patent Information
- Application Number
- JP2023050852
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
AI Technical Summary
The existing methods for manufacturing carbon fiber sheets in fuel cells face challenges with increased oxygen concentration in heat treatment furnaces due to external oxygen ingress, leading to oxidative wear and tear of furnace materials and quality variations in the carbon fiber sheets.
A method involving laminating carbon fiber sheet precursors and treating them under an inert atmosphere, with oxygen reduction operations such as gap crushing, inert gas replacement, and pressing to minimize oxygen between layers, ensuring the heat treatment is conducted at controlled oxygen levels.
This approach reduces oxidative wear of the furnace, maintains consistent carbon fiber sheet quality, and decreases maintenance frequency by controlling oxygen concentration during the heat treatment process.
Smart Images

Figure 2024139909000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a carbon fiber sheet that is preferably used as a gas diffuser in a fuel cell. [Background technology]
[0002] As gas diffusers constituting the membrane electrode assembly in which the power generation reaction occurs in a fuel cell, carbon fiber sheets such as carbon paper in which short carbon fibers are bound with a resin carbide, carbon fiber nonwoven fabric formed by entangling carbon fibers, and carbon fiber fabrics are used. The manufacturing process of such carbon fiber sheets involves a step of heat treatment in a high-temperature heat treatment furnace, but increasing the number of heat treatment furnaces to increase production volume increases the costs of installing and operating the equipment, which directly leads to an increase in manufacturing costs.
[0003] In response to these problems, Patent Document 1 proposes a method of stacking multiple carbon fiber sheet precursors and joining their widthwise ends together, simultaneously heat-treating the multiple carbon fiber sheet precursors, cutting off the joined ends, and dividing the sheets into multiple sheets to produce a carbon fiber sheet.
[0004] Furthermore, Patent Document 2 proposes a method for producing a carbon fiber sheet by heat treating a carbon fiber sheet precursor in a state where multiple sheets are stacked without joining the width direction ends. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP2015-071508A published [Patent Document 2] Patent Publication No. 2020-133006 published Summary of the Invention [Problem to be solved by the invention]
[0006] However, when multiple carbon fiber sheets are stacked and transported through a heat treatment furnace as described in Patent Documents 1 and 2, a large amount of oxygen brought in from outside the furnace exists between the sheet layers, and continuous transportation brings oxygen into the heat treatment furnace, causing an increase in the oxygen concentration in the heat treatment furnace.
[0007] If the oxygen concentration inside the heat treatment furnace increases, the oxidation and wear of the furnace materials will accelerate, requiring more frequent maintenance of the heat treatment furnace. In addition, there will be areas where the oxidation reaction of the carbon fiber sheet will occur excessively locally, raising concerns about the impact on quality variation. [Means for solving the problem]
[0008] The present invention for solving the above problems is as follows. (1) A method for producing a carbon fiber sheet, comprising: a heat treatment step in which a plurality of stacked carbon fiber sheet precursors, each containing carbon fibers or carbon fiber precursor fibers, and a carbonizable resin binder, are continuously transported through a heat treatment furnace and heat-treated at 400°C or higher in an inert atmosphere to form a carbon fiber sheet; and an oxygen content reduction step in which an operation for reducing the amount of oxygen present between the layers of the stacked carbon fiber sheet precursors is performed prior to the heat treatment step. (2) The method for producing a carbon fiber sheet according to (1), wherein the oxygen content reducing step is carried out between a position 300 mm upstream from an inlet of the heat treatment furnace and a position where the temperature inside the heat treatment furnace becomes 400° C. (3) The method for producing a carbon fiber sheet according to (1) or (2), wherein the amount of oxygen in the heat treatment step is 120 ppm or less. (4) The method for producing a carbon fiber sheet according to any one of (1) to (3), wherein the operation for reducing the amount of oxygen includes an operation for squeezing gaps generated between layers of a plurality of carbon fiber sheet precursors to push out oxygen present between the layers from between the layers. (5) The method for producing a carbon fiber sheet according to (4), wherein the operation of squeezing gaps generated between the layers of the plurality of carbon fiber sheet precursors to push out oxygen present between the layers from between the layers includes at least one operation selected from the group consisting of an operation of placing a weight on an uppermost surface of the plurality of stacked carbon fiber sheet precursors, an operation of blowing an inert gas from one or both sides of the plurality of stacked carbon fiber sheet precursors to reduce gaps between the layers, and an operation of pressing a guide member from one or both sides of the plurality of stacked carbon fiber sheet precursors. (6) The method for producing a carbon fiber sheet according to any one of (1) to (5), wherein the operation for reducing the oxygen amount comprises replacing oxygen present between layers with an inert gas. (7) The method for producing a carbon fiber sheet according to (6), wherein the oxygen present between the layers is replaced with an inert gas by blowing an inert gas onto one side or an end in a width direction of the carbon fiber sheet precursor. (8) The method for producing a carbon fiber sheet according to (7), wherein in the oxygen content reduction step, an operation of sucking gas from a surface or end opposite to the surface or end on the side where the inert gas is blown is further performed. (9) The method for producing a carbon fiber sheet according to any one of (1) to (8), wherein the oxygen content is reduced by stacking a plurality of the carbon fiber sheets under an inert gas atmosphere. Effect of the Invention
[0009] According to the present invention, even when multiple stacked carbon fiber sheets are run continuously through a heat treatment furnace, it is possible to suppress an increase in the oxygen concentration inside the heat treatment furnace due to the oxygen present between the stacked layers, and by suppressing the oxidative wear of the furnace materials of the heat treatment furnace, the frequency of maintenance of the heat treatment furnace can be reduced. In addition, by preventing excessive oxidation reactions of the carbon fiber sheets, the impact on quality can be reduced. [Brief description of the drawings]
[0010] [Figure 1]FIG. 1 is a schematic cross-sectional view of a carbon fiber sheet production process in which a weight is placed on the uppermost surface of a carbon fiber sheet precursor. [Diagram 2] FIG. 1 is a schematic cross-sectional view of a carbon fiber sheet manufacturing process in which an oxygen-free gas is blown onto both sides of a carbon fiber sheet precursor to reduce interlayer gaps. [Diagram 3] 1 is a schematic cross-sectional view of a carbon fiber sheet production process in which a guide member is pressed against one side of a carbon fiber sheet precursor. [Figure 4] FIG. 1 is a top view schematic diagram of a carbon fiber sheet production process in which an inert gas is sprayed onto an end portion in the width direction of a carbon fiber sheet precursor. [Diagram 5] FIG. 2 is a schematic cross-sectional view of a carbon fiber sheet production process in which a plurality of carbon fiber sheet precursors are laminated under an inert gas atmosphere. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The method for producing a carbon fiber sheet of the present invention includes a heat treatment step of continuously heat treating a carbon fiber sheet precursor to form a carbon fiber sheet, and an oxygen amount reduction step prior to the heat treatment step.
[0012] First, the configuration of the carbon fiber sheet precursor used in the heat treatment step will be described. The carbon fiber sheet precursor used in the present invention contains carbon fibers or carbon fiber precursor fibers, and a carbonizable resin binder.
[0013] The carbon fiber precursor fiber in the present invention is a fiber that becomes a carbon fiber by heat treatment. The carbonizable resin binder is a resin component that can be carbonized by heat treatment, and is intended to bind carbon fibers together and to increase the electrical conductivity of the carbon fiber sheet.
[0014] The carbon fiber precursor fiber is not particularly limited as long as it is a fiber that can be turned into carbon fiber by heat treatment, and examples of the carbon fiber precursor fiber include polyacrylonitrile (PAN)-based fiber, pitch-based fiber, rayon-based fiber, phenol-based fiber, and flame-resistant fiber obtained by infusible treatment of these fibers, etc. Among these, PAN-based fiber or pitch-based fiber is preferred, since it can increase the bending strength and tensile strength of the resulting carbon fiber sheet, and PAN-based fiber is particularly preferred.
[0015] Examples of carbon fibers include fibers obtained by heat treating the above-mentioned carbon fiber precursor fibers, i.e., PAN-based carbon fibers, pitch-based carbon fibers, rayon-based carbon fibers, phenol-based carbon fibers, etc. Among these, PAN-based carbon fibers or pitch-based carbon fibers that can increase the bending strength and tensile strength of the obtained carbon fiber sheet are preferred, and PAN-based carbon fibers are particularly preferred.
[0016] The carbonizable resin binder is not particularly limited as long as it is a resin component that can be carbonized by heat treatment, and examples of the carbonizable resin binder include thermosetting resins such as epoxy resins, unsaturated polyester resins, phenol resins, polyimide resins, and melamine resins, and thermoplastic resins such as acrylic resins, polyvinylidene chloride resins, polytetrafluoroethylene resins, and polyvinyl alcohol resins. It is preferable to use a thermosetting resin that has excellent adhesion between fibers in the obtained carbon fiber sheet and excellent electrical conductivity, and generates a relatively small amount of decomposition gas during heat treatment, and therefore has a high carbonization yield, and among these, it is more preferable to use a phenol resin.
[0017] The ratio of carbon fiber contained in 100% by mass of the carbon fiber sheet is preferably 20 to 90% by mass, more preferably 40 to 80% by mass. If the ratio of carbon fiber is less than 20% by mass, the tensile strength of the obtained carbon fiber sheet may decrease, or the carbon fiber sheet may become brittle and easily breakable. If the ratio of carbon fiber exceeds 90% by mass, the obtained carbon fiber sheet may become bulky, and the tensile strength and compressive strength may decrease. When using a carbon fiber sheet precursor containing carbon fiber precursor fibers, the ratio is adjusted to the above range after the heat treatment step described below.
[0018] The form of the carbon fiber sheet precursor includes a fiber structure such as a woven fabric, a paper body, or a nonwoven fabric using carbon fiber or carbon fiber precursor fiber, and a carbonizable resin binder is contained therein. However, since the carbon fiber sheet has excellent characteristics of absorbing dimensional changes in the thickness direction, it is preferable to use a paper body of carbon fiber or carbon fiber precursor fiber as the fiber structure. When producing such a paper body, one of the preferred embodiments is to make a paper of carbon fiber or carbon fiber precursor fiber, immerse it in an aqueous dispersion containing a binder, and then dry it. This produces a fiber structure in which the fibers are dispersed and the shape is fixed by the binder. Other binders that can be used are styrene-butadiene rubber, epoxy resin, etc.
[0019] As a method for producing a carbon fiber sheet precursor by incorporating a carbonizable resin binder into the above-mentioned fiber structure, for example, a method can be mentioned in which the above-mentioned fiber structure is immersed in the above-mentioned carbonizable resin binder or a solution or dispersion thereof, and then the excess resin binder is squeezed out and the fiber structure is dried.
[0020] In one preferred embodiment, the carbon fiber sheet precursor produced as described above is heated and pressurized to semi-cure the resin binder while forming it to a predetermined thickness to make the thickness smooth. The forming method is not limited as long as the thickness can be made smooth, but examples of the forming method include forming by passing the sheet between heated calendar rolls, forming by pressing intermittently with a heated plate, and forming using a double belt press machine.
[0021] The method for producing a carbon fiber sheet of the present invention includes a heat treatment step of continuously running a plurality of the carbon fiber sheet precursors, in a stacked state, through a heat treatment furnace to perform a heat treatment.
[0022] The term "continuously running" means that the sheet-like material is transported from unwinding to winding within a predetermined speed range. During the continuous running, it is preferable that the sheet-like material is not broken or transport is not stopped from unwinding to winding.
[0023] The number of carbon fiber sheet precursors to be laminated is preferably 2 to 8, more preferably 2 to 6, in order to perform uniform heat treatment. The state of laminating multiple sheets means a state in which multiple carbon fiber sheet precursors overlap at least partially. In the state in which multiple carbon fiber sheet precursors are laminated, the multiple carbon fiber sheet precursors may or may not be fixed to each other at a part such as the width direction end, but it is preferable that they are not fixed because damage caused by distortion due to wrinkles or arches of the carbon fiber sheet precursor or carbon fiber sheet generated by heat treatment is less likely to occur.
[0024] In the heat treatment step of the present invention, the carbon fiber sheet precursor laminated in a plurality of sheets is heat treated at a temperature of 400°C or higher in a heat treatment furnace. That is, the portion in the heat treatment furnace where the temperature reaches 400°C or higher corresponds to the heat treatment step. The heat treatment is performed in an inert atmosphere to prevent the carbon fiber sheet precursor from being burned and to prevent the furnace material in the heat treatment furnace from being oxidized. As the inert gas, nitrogen, helium, argon, or other rare gases can be used, and among them, nitrogen, which is relatively low cost, is preferable.
[0025] In order to ensure the electrical conductivity and thermal conductivity required for a carbon fiber sheet for fuel cell applications, the maximum temperature of the heat treatment is preferably 1,600 to 3,000° C. If the maximum temperature is less than 1,600° C., the degree of graphitization of the carbon fiber sheet may be low, resulting in low electrical conductivity and thermal conductivity. If the heat treatment temperature exceeds 3,000° C., a lot of energy is required, and the wear of the furnace material may progress, resulting in increased costs for maintaining the heat treatment furnace.
[0026] In the method for producing a carbon fiber sheet of the present invention, it is sufficient to have one heat treatment step, but it is also a preferred embodiment to have two heat treatment steps by using a first heat treatment furnace for performing heat treatment at a relatively low temperature and a second heat treatment furnace for performing heat treatment at a relatively high temperature, that is, to heat treat the carbon fiber sheet precursor by continuously running it through the first heat treatment furnace and the second heat treatment furnace. In this case, the maximum temperature of the first heat treatment furnace is preferably 400°C to 700°C, and the maximum temperature of the second heat treatment furnace is preferably 1,600°C to 3,000°C. By having two heat treatment steps in this way, it is possible to separate the first heat treatment step, which generates a lot of decomposition gas and progresses shrinkage due to carbonization, from the second heat treatment step, which is necessary to maintain the performance as a cell when used as an electrode for a fuel cell, and it is possible to prevent the decomposition gas generated in the first heat treatment step from flowing into the furnace used in the second heat treatment step and solidifying and precipitating. In the case of having two heat treatment steps, the oxygen amount reduction step may be performed either before the first heat treatment step or before the second heat treatment step, but it is preferable to perform the oxygen amount reduction step before the second heat treatment step, which has a higher maximum temperature, because it is more effective in suppressing the oxidation loss of the furnace material of the heat treatment furnace and in suppressing the excessive oxidation reaction of the carbon fiber sheet. Also, it is one of the preferred embodiments to perform the oxygen amount reduction step either before the first heat treatment step or before the second heat treatment step.
[0027] The manufacturing method of the present invention has an oxygen amount reduction step in which an operation for reducing the amount of oxygen present between the layers of the laminated carbon fiber sheet precursor is performed before the heat treatment step. Here, before the heat treatment step refers to the upstream of the position where the temperature becomes 400 ° C. in the heat treatment furnace. As described above, the heat treatment step of the present invention is performed under an inert atmosphere, but when a plurality of carbon fiber sheet precursors are laminated and heat treated, oxygen outside the heat treatment furnace may be brought between the layers. This is because a gap is generated between the layers in front of the heat treatment furnace due to bending, fluttering, wrinkles, etc. that occur when the carbon fiber sheet precursor is run, and oxygen is brought into the heat treatment furnace in a form in which the oxygen is enclosed in the gap. The oxygen amount reduction step is a step for reducing the amount of oxygen brought in as described above, and is a step necessary for suppressing the oxidative wear of the furnace material of the heat treatment furnace and the quality variation due to the excessive oxidation of the carbon fiber sheet.
[0028] The oxygen amount reduction step is not particularly limited as long as it is an operation that reduces the oxygen brought into the heat treatment furnace by continuously transporting the base material, and examples of the oxygen amount reduction step include an operation of squeezing gaps generated between layers of a plurality of carbon fiber sheet precursors to push out the oxygen present between the layers, an operation of replacing the oxygen present between the layers with an inert gas, and an operation of stacking a plurality of carbon fiber sheets under an inert gas atmosphere so that no oxygen is present between the layers.
[0029] Examples of the operation of squeezing the gaps generated between the layers of a plurality of carbon fiber sheet precursors to push out the oxygen present between the layers from between the layers include an operation of placing a weight on the uppermost surface of the plurality of stacked carbon fiber sheet precursors, an operation of blowing an inert gas from one or both sides of the plurality of stacked carbon fiber sheet precursors to reduce the gaps between the layers, an operation of pressing a guide member from one or both sides of the plurality of stacked carbon fiber sheet precursors, etc. As the inert gas, nitrogen or a rare gas such as helium or argon can be used, and among them, nitrogen, which is relatively low cost, is preferable.
[0030] As an operation for replacing oxygen present between layers with an inert gas, for example, an operation for blowing an inert gas from one side or an end in the width direction of the carbon fiber sheet precursor can be mentioned. In this case, it is also one of the preferred embodiments to further perform an operation for sucking the gas from the side or end opposite to the side to which the inert gas is blown.
[0031] The above-mentioned operations given as examples of the oxygen amount reducing step may be carried out alone or in combination.
[0032] The oxygen amount reduction step is preferably carried out between a position 300 mm upstream of the entrance of the heat treatment furnace and a position where the temperature inside the heat treatment furnace becomes 400° C., and more preferably between a position 200 mm upstream of the entrance of the heat treatment furnace and a position where the temperature inside the heat treatment furnace becomes 300° C. If it is carried out upstream of a position 300 mm upstream of the entrance of the heat treatment furnace, oxygen may again penetrate between the layers after the oxygen amount reduction operation is performed, and the oxygen amount during heat treatment may not be reduced. If it is carried out downstream of the position where the temperature inside the heat treatment furnace becomes 400° C., the effect of the present application cannot be obtained, and an oxidation reaction with the furnace material in the heat treatment furnace or the carbon fiber sheet precursor may occur.
[0033] The amount of oxygen in the heat treatment step is preferably 120 ppm or less, more preferably 100 ppm or less, and even more preferably 80 ppm or less. The amount of oxygen in the heat treatment step is 120 ppm or less, which means that the amount of oxygen in the region in the heat treatment furnace where the temperature is 400 ° C or more is 120 ppm or less. In order to confirm whether the above condition is satisfied, it can be confirmed by measuring the amount of oxygen at a position in the heat treatment furnace where the temperature is 400 ° C or more, but it can also be confirmed by measuring at a position upstream of the region in the heat treatment furnace where the temperature is 400 ° C or more from the heat treatment furnace inlet where the temperature is less than 400 ° C. The amount of oxygen at the position from the heat treatment furnace inlet where the temperature is less than 400 ° C. is greater than the amount of oxygen in the region downstream where the temperature is 400 ° C. or more. Therefore, if the amount of oxygen at the position from the heat treatment furnace inlet where the temperature is less than 400 ° C. is 120 ppm or less, it can be indirectly confirmed that the amount of oxygen in the region downstream where the temperature is 400 ° C. or more is also 120 ppm or less. The measurement position is preferably set at a position within the heat treatment furnace that does not structurally become a drift of the gas flowing within the furnace. When measuring at multiple points, the maximum value is taken as the amount of oxygen within the heat treatment furnace.
[0034] The carbon fiber sheet produced by the carbon fiber sheet production method of the present invention can suppress local oxidation reactions by reducing the amount of oxygen, and in particular can suppress the variation in physical properties between the product immediately after production has started and the product immediately before production is completed.
[0035] For example, when measuring the basis weight of a carbon fiber sheet at multiple points, the difference between the average value and the maximum value, and the difference between the average value and the minimum value are preferably 10% or less of the average value. For measuring the basis weight, for example, 100 mm x 100 mm samples are taken at three points each at the most upstream and most downstream parts when continuously producing carbon fiber sheets, for a total of six points, and the mass of each sample is weighed using an electronic balance to calculate the basis weight, so that the average value of the six basis weights, the difference between the average value and the maximum value, and the difference between the average value and the minimum value can be measured.
[0036] Regarding the four-point bending stress of the carbon fiber sheet, it is preferable that the difference between the average value and the maximum value, and the difference between the average value and the minimum value when measuring multiple points are 20% or less of the average value. For example, a sample for measuring the four-point bending stress may be 20 mm x 50 mm. By collecting and measuring six points in total, three points each at the most upstream part and the most downstream part when the carbon fiber sheet is continuously produced and wound, the average value of the six points, the difference between the average value and the maximum value, and the difference between the average value and the minimum value can be measured. In this case, if a sample is obtained whose longitudinal direction coincides with the transport direction of the carbon fiber sheet, the four-point bending stress in the transport direction can be measured, and if a sample is obtained whose longitudinal direction coincides with the width direction of the carbon fiber sheet, the four-point bending stress in the width direction can be measured. The longitudinal direction of the sample refers to the long side direction of the sample.
[0037] Preferred embodiments of the present invention will be described below with reference to the drawings. However, the present invention is not limited to these embodiments. Furthermore, the descriptions of preferred materials, numerical ranges, etc. in the descriptions of individual embodiments can also be construed as descriptions of the manufacturing method of the present invention as a general concept.
[0038] 1 to 5 are diagrams that illustrate a carbon fiber sheet manufacturing apparatus that continuously heat-treats a carbon fiber sheet precursor, in order to explain the carbon fiber sheet manufacturing method of the present invention.
[0039] First, a preferred embodiment of the carbon fiber sheet manufacturing apparatus of the present invention will be described. As shown in Figures 1 to 5, a heat treatment furnace 100, which has a common structure among heat treatment furnaces, is a horizontal furnace capable of transporting carbon fiber sheet precursors 11 and 12 in a horizontal direction inside the heat treatment furnace.
[0040] In order to prevent oxidation of the carbon fiber sheet precursors 11, 12 and the heat treatment furnace 100 itself, it is preferable to supply an inert gas such as nitrogen or argon from the inert gas supply points 111 of the inlet seal portion 109 and the outlet seal portion 110 and fill the inside of the heat treatment furnace 100 with the gas.
[0041] The materials constituting the heat treatment furnace can be made of metal, carbon, or ceramic, but it is preferable to use carbon, especially graphite, for the parts that reach temperatures of 1,000°C or higher because of its high chemical stability.
[0042] The heat treatment furnace 100 heat-treats the carbon fiber sheet precursors 11, 12 by continuously running two stacked carbon fiber sheet precursors 11, 12 through the heat treatment furnace 101, carbonizing the carbonizable resin binder, and, if the carbon fiber precursor sheet contains carbon fiber precursor fibers, heat-treating the carbon fiber precursor fibers to form carbon fiber sheets 21, 22.
[0043] The heat treatment furnace 100 is provided with a heat treatment furnace interior 101 through which the carbon fiber sheet precursors 11 and 12 pass. One of the openings in the heat treatment furnace interior is an inlet (hereinafter, furnace inlet) 105 of the heat treatment furnace, and the other is an outlet (hereinafter, furnace outlet) 106 of the heat treatment furnace.
[0044] The carbon fiber sheet precursors 11, 12 enter the heat treatment furnace 101 from the furnace inlet 105, and move continuously within the heat treatment furnace 101 on a hearth 104 provided on the muffle lower wall 103 toward the furnace outlet 106, while being heat-treated to become a carbon fiber sheet.
[0045] The heat treatment furnace 100 is provided with an exhaust port 108 to prevent decomposition gas generated in the heat treatment furnace 101 from remaining in the heat treatment furnace 101 and solidifying and depositing or liquefying, and adhering to the muffle upper wall 102 or hearth 104 in the heat treatment furnace.
[0046] In Figures 1 to 5, only one heat treatment furnace 100 is used as the heat treatment furnace to heat treat the carbon fiber sheet precursors 11, 12 at a maximum temperature of 1,600°C to 3,000°C to produce the carbon fiber sheets 21, 22. However, as described above, two heat treatment furnaces may be used. In that case, it is preferable to heat the carbon fiber sheet precursors 11, 12 at a maximum temperature of 400°C to 1,000°C in the first heat treatment furnace and heat treat them at a maximum temperature of 1,600°C to 3,000°C in the second heat treatment furnace.
[0047] A first example of the method for producing a carbon fiber sheet of the present invention is shown in Fig. 1. In Fig. 1, a touch roll 202 is placed as a weight on the upper carbon fiber sheet precursor 12 of two laminated carbon fiber sheet precursors 11 and 12 in the oxygen content reduction step.
[0048] The weight is preferably in contact with the entire width of the overlapping portion of the multiple carbon fiber sheet precursors 11 and 12, but the width of the weight is not particularly limited as long as it is not extremely narrower than the width of the overlapping portion of the carbon fiber sheet precursors 11 and 12. The width is preferably 0.5 times or more, more preferably 1.0 times or more, of the width of the overlapping portion of the carbon fiber sheet precursors. If it is less than 0.5 times, the effect of reducing the amount of oxygen decreases.
[0049] The weight is preferably in the form of a roll like the touch roll 202 in order to reduce abrasion with the carbon fiber sheet precursors 11 and 12. The weight of the weight is not particularly limited, but is more preferably 0.05 to 5.00 kg / m per unit width relative to the width of the overlapping carbon fiber sheet precursors. If it is less than 0.05 kg / m, the effect of reducing the amount of oxygen may decrease. If it exceeds 5.00 kg / m, the bond between the carbon fibers or carbon fiber precursor fibers contained in the carbon fiber sheet precursor and the resin binder may be destroyed, and the tensile strength of the carbon fiber sheet after heat treatment may decrease.
[0050] The material of the weight is not particularly limited, but when the weight is placed in a heat treatment furnace, it is preferable to use metal, carbon, or ceramics in order to prevent oxidation and melting due to heat, and among these, carbon and ceramics are preferable in order to prevent the effects of thermal deformation.
[0051] The weight is fixed at a specific position so as to be in contact with the carbon fiber sheet precursor. The fixing method is not particularly limited and may be any method as long as it does not move significantly during continuous transport.
[0052] A second example of the method for producing a carbon fiber sheet of the present invention is shown in Fig. 2. In Fig. 2, as an oxygen amount reduction step, a blower 203 is provided on both sides of two laminated carbon fiber sheet precursors 11 and 12 to blow an inert gas thereon.
[0053] The inert gas blown by the blower 203 is preferably blown over the entire width of the overlapping portion of the carbon fiber sheet precursors 11 and 12, but is not particularly limited as long as it is not extremely narrower than the width of the overlapping portion of the carbon fiber sheet precursors 11 and 12. It is preferably 0.5 times or more, more preferably 1.0 times or more, of the width of the overlapping portion of the carbon fiber sheet precursors. If it is less than 0.5 times, the effect of reducing the amount of oxygen decreases.
[0054] The wind speed blown by the blower 203 is not particularly limited, but is preferably 1 to 5 m / s, and more preferably 1.5 to 3 m / s. If it is less than 1 m / s, the effect of reducing the amount of oxygen may be reduced, and if it exceeds 5 m / s, the flapping of the carbon fiber sheet precursor becomes large, which may cause breakage of the carbon fiber sheet or the carbon fiber sheet precursor during transportation, or meandering of the substrate.
[0055] A third example of the method for producing a carbon fiber sheet of the present invention is shown in Fig. 3. In Fig. 3, a guide member 204 is arranged on the running line of the carbon fiber sheet precursor as an oxygen content reduction step, and is pressed against the carbon fiber sheet precursor. The guide member 204 is composed of a part arranged in the width direction of the carbon fiber sheet precursor and a part arranged in the longitudinal direction outside both ends of the carbon fiber sheet precursor. The part arranged in the width direction of the guide member 204 crushes the gaps between the carbon fiber sheet precursors to reduce the amount of oxygen, and the part arranged in the longitudinal direction outside both ends of the carbon fiber sheet precursor can also regulate the meandering of the carbon fiber sheet precursor.
[0056] The material constituting the guide member 204 can be metal, oxygen, or ceramics, but carbon or ceramics is preferable in order to eliminate the influence of thermal deformation.
[0057] The shape of the guide member 204 is not particularly important as long as it can push out the oxygen between the layers of multiple carbon fiber sheet precursors, but it is preferable for the shape to prevent the carbon fiber sheet precursor from bending in the running direction, because this prevents cracks from occurring at the bonding points between the carbon fibers and the binder in the carbon fiber sheet and prevents damage such as wrinkles and breaks.
[0058] A fourth example of the method for producing a carbon fiber sheet of the present invention is shown in Fig. 4. In Fig. 4, as an oxygen amount reduction step, a blower 203 is arranged on one side of the carbon fiber sheet precursors 11 and 12, and an aspirator 205 is arranged on the opposite side. An inert gas is blown from the blower 203 toward the opposite side, and the aspirator 205 sucks in the oxygen present between the layers and the inert gas blown from the blower 203. With this configuration, it becomes easier to replace the oxygen between the layers with the inert gas.
[0059] The wind speed blown by the blower 203 and the wind speed sucked by the suction device 205 are not particularly limited, but are preferably 1 to 5 m / s, and more preferably 1.5 to 3 m / s. If it is less than 1 m / s, the effect of reducing the amount of oxygen may be reduced, and if it exceeds 5 m / s, the flapping of the carbon fiber sheet precursor becomes large, and the carbon fiber sheet precursor may break or the substrate may meander during transportation.
[0060] A fifth embodiment of the method for producing a carbon fiber sheet of the present invention is shown in Fig. 5. In Fig. 5, carbon fiber sheet precursors 11 and 12 are laminated under an inert gas atmosphere as an oxygen content reducing step. The inert gas atmosphere in Fig. 5 refers to the inside of the inlet of a heat treatment furnace.
[0061] In FIG. 5, a guide roll 206 is placed between the carbon fiber sheet precursors 11 and 12 before they run through the inert gas atmosphere to create a gap between the layers, and the amount of oxygen is reduced by laminating them under an inert gas atmosphere.
[0062] The distance between the layers of the carbon fiber sheet precursors 11 and 12 when they enter the inert gas atmosphere is not particularly limited, but is preferably 5 mm or more. If it is less than 5 mm, it may be insufficient to replace oxygen with the inert gas from between the layers. [Explanation of symbols]
[0063] 11 Carbon fiber sheet precursor 12 Carbon fiber sheet precursor 21 Carbon fiber sheet 22 Carbon fiber sheet 100 Heat treatment furnace 101 Heat treatment furnace 102 Muffle upper wall 103 Muffle lower wall 104 Hearth 105 Entrance of heat treatment furnace (furnace entrance) 106 Heat treatment furnace outlet (furnace outlet) 107 Heat source 108 Exhaust port 109 Inlet seal part 110 Exit seal part 111 Inert gas supply point 201 Freerolls 202 Touch roll 203 Blower 204 Guide member 205 Suction machine 206 Guide Roll [Industrial Applicability]
[0064] INDUSTRIAL APPLICABILITY The present invention can be used for a method for producing a carbon fiber sheet, particularly a carbon fiber sheet that is preferably used as a gas diffuser in a fuel cell.
Claims
1. A method for producing a carbon fiber sheet, comprising: a heat treatment step of continuously running a plurality of stacked carbon fiber sheet precursors, each containing carbon fibers or carbon fiber precursor fibers, and a carbonizable resin binder, through a heat treatment furnace to heat treat the precursors at 400°C or higher in an inert atmosphere to form a carbon fiber sheet; and an oxygen amount reduction step of performing an operation to reduce the amount of oxygen present between the layers of the stacked carbon fiber sheet precursors prior to the heat treatment step.
2. The method for producing a carbon fiber sheet according to claim 1 , wherein the oxygen content reducing step is carried out between a position 300 mm upstream from an inlet of the heat treatment furnace and a position where a temperature inside the heat treatment furnace reaches 400° C.
3. The method for producing a carbon fiber sheet according to claim 1, wherein the amount of oxygen in the heat treatment step is 120 ppm or less.
4. 2. The method for producing a carbon fiber sheet according to claim 1, wherein the operation of reducing the amount of oxygen comprises a step of squeezing gaps generated between layers of a plurality of carbon fiber sheet precursors to push out oxygen present between the layers.
5. 5. The method for producing a carbon fiber sheet according to claim 4, wherein the operation of squeezing gaps generated between the layers of the plurality of carbon fiber sheet precursors to push out oxygen present between the layers from between the layers includes at least one operation selected from the group consisting of an operation of placing a weight on an uppermost surface of the plurality of stacked carbon fiber sheet precursors, an operation of blowing an inert gas from one or both sides of the plurality of stacked carbon fiber sheet precursors to reduce gaps between the layers, and an operation of pressing a guide member from one or both sides of the plurality of stacked carbon fiber sheet precursors.
6. The method for producing a carbon fiber sheet according to claim 1 , wherein the oxygen content is reduced by replacing oxygen present between layers with an inert gas.
7. The method for producing a carbon fiber sheet according to claim 6, wherein the operation of replacing oxygen present between the layers with an inert gas comprises an operation of blowing an inert gas onto one surface or an end portion in a width direction of the carbon fiber sheet precursor.
8. The method for producing a carbon fiber sheet according to claim 7, wherein in the oxygen content reduction step, an operation of sucking gas from a surface or end opposite to the surface or end on the side where the inert gas is blown is further performed.
9. The method for producing a carbon fiber sheet according to claim 1 , wherein the oxygen content is reduced by stacking a plurality of the carbon fiber sheets under an inert gas atmosphere.
Citation Information
Patent Citations
For carbon fiber production furnace - gas diffusion of the annealer
JP1982116098U
Sealing apparatus for carbonization furnace for producing carbon fiber and method for producing carbon fiber
JP2001098428A
Sealing device of carbonization furnace for carbon fiber production
JP2010007209A
Method for producing carbon fiber sheet
JP2020133006A
Method of producing porous electrode substrate
JP2015071508A